Acoustic emission multi-parameter fusion asphalt mixture fatigue life prediction method
By using a multi-parameter fusion method of acoustic emission, the characteristics such as event density and b-value reverse damage are calculated and combined with macroscopic mechanical damage, which solves the problems of insufficient sensitivity and long-term testing in the fatigue life evaluation of asphalt mixtures in the existing technology, and realizes rapid and accurate fatigue life prediction.
Patent Information
- Application Number
- CN202611594682.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-15
- Publication Date
- 2026-11-24
AI Technical Summary
Existing technologies for evaluating the fatigue life of asphalt mixtures in roads rely on long-term testing and are not sensitive enough to early microcracks, interfacial debonding, and shear slip, thus failing to effectively predict the remaining life.
By using a multi-parameter acoustic emission fusion method, the event density, b-value reverse damage amount, S-value, and the proportion of shear and tensile events are calculated to form acoustic emission window characteristics. These characteristics are then fused with macroscopic mechanical damage amounts to directly calculate and predict the remaining lifetime and total lifetime.
It enables rapid and accurate prediction of fatigue life of asphalt mixtures, improves the sensitivity and prediction accuracy of early damage, and reduces the test time requirement.
Smart Images

Figure QLYQS_2 
Figure QLYQS_3 
Figure QLYQS_4
Abstract
Description
Technical Field
[0001] This application relates to the field of asphalt mixture life prediction technology, and in particular to a method for predicting the fatigue life of asphalt mixtures by acoustic emission multi-parameter fusion. Background Technology
[0002] The fatigue life evaluation of road asphalt mixtures typically relies on four-point bending, three-point bending, indirect tensile, or semi-circular bending fatigue tests. The fatigue performance of the material is determined through cyclic stiffness decay, dynamic modulus changes, hysteretic dissipation energy, fatigue equations, or a specified number of failure cycles. While this method provides a clear evaluation scope, it requires a relatively long loading process during testing and lacks sensitivity to early microcracks, interfacial debonding, and shear slip.
[0003] Acoustic emission (AE) technology can monitor microscopic changes within materials and capture transient elastic waves formed by localized energy release during asphalt mixture fatigue. It is currently used in road fatigue analysis. Existing AE fatigue analyses primarily focus on statistical analysis of collected parameters such as amplitude, energy, ring count, event count, and duration. For example, patent CN119269285A obtains four parameters—ring count, energy, duration, and amplitude—through AE tests. After normalization, these parameters are weighted and fused using a fuzzy comprehensive evaluation method to form a comprehensive evaluation parameter C. A dynamic threshold is determined based on kernel density estimation, and a multi-parameter joint distribution model is established to achieve a four-level early warning system for fatigue conditions. However, this approach only processes the four key parameters—ring count, energy, duration, and amplitude—and focuses solely on AE parameters without converting them into damage quantities with clear mechanical and physical meaning. It only outputs comprehensive evaluation results and multi-level early warning levels, failing to predict the remaining life of the asphalt road.
[0004] Therefore, there is a need to provide an improved technical solution that addresses the shortcomings of the existing technology. Summary of the Invention
[0005] The purpose of this application is to provide a method for predicting the fatigue life of asphalt mixtures by integrating multiple acoustic emission parameters. This method calculates event density, b-value reverse damage amount, S-value, and the proportion of shear-type and tensile-type events to form five types of acoustic emission window features. The weights are determined based on the correlation between each normalized feature and the macroscopic mechanical damage amount to form an acoustic emission damage factor. This factor is then integrated with the macroscopic mechanical damage amount, which consists of dynamic stiffness, force amplitude, displacement amplitude, and dissipated energy. Based on the current comprehensive damage index, growth rate, and calibration critical value, the predicted remaining life and predicted total life are directly calculated.
[0006] To achieve the above objectives, this application provides the following technical solution: A method for predicting the fatigue life of asphalt mixtures by integrating multiple acoustic emission parameters includes the following steps: S1. Conduct full-life fatigue loading on the calibration specimens of asphalt mixture with the same mix proportion for the surface layer of the road to be tested, and simultaneously collect acoustic emission data and loading data during the fatigue loading process; use the running time in the loading data and the occurrence time in the acoustic emission data as a unified time reference to divide the test process into continuous time windows; S2. Calculate stiffness damage, force amplitude damage, displacement amplitude damage, and dissipated energy damage based on the loading data, and then weight and fuse these four factors to construct the first... Macroscopic mechanical damage quantity per observation window ; S3. Calculate the event density, b-value, reverse damage amount, S-value, proportion of shear-type events, and proportion of tensile events based on the acoustic emission data. After normalization, calculate the macroscopic mechanical damage amount. The acoustic emission damage factor is obtained by fusing the correlation weights. ; S4. Set the acoustic emission damage factor for the current observation window. Compared with macroscopic mechanical damage By fusion coefficient By combining the results, a comprehensive damage index is obtained. : ; Among them, the fusion coefficient This represents the contribution ratio of acoustic emission damage factor to the overall damage index, determined based on the principle of minimizing the mean square error of the standardized life of the calibrated specimen. ; S5. Using the current observation window of the target specimen as the endpoint, select the current observation window and the nearest previous one. One observation window is used to calculate the overall damage growth rate: ; In the formula, represents the comprehensive damage growth rate corresponding to the kth observation window; j is the sequence number of the fitted observation window. For the first The cumulative number of cycles corresponding to each observation window; The comprehensive damage index for the j-th observation window; and These represent the average number of cycles and the comprehensive damage index within the selected observation window, respectively. , m is the number of observation windows for fitting; S6. Drill representative core samples from the road surface to be tested as target specimens. Perform fatigue loading and acoustic emission monitoring under the same conditions as the calibration specimens, and analyze the comprehensive damage index. Predicting remaining lifespan and predicted total lifespan : ; ; in, The critical fusion damage value is determined by full-life calibration specimens under the same conditions; This is the current observation window number; This represents the current overall damage growth rate; For the first The cumulative number of fatigue loading cycles corresponding to each observation window.
[0007] Furthermore, the acoustic emission data includes the amplitude, rise time, duration, ring count, energy, and occurrence time of the acoustic emission event; the loading data includes the cycle number, axial displacement, axial force, and running time for each sampling point.
[0008] Furthermore, in S3, the S value is calculated based on the number of events, event energy levels, and maximum energy level for each observation window: ; in, For the first The number of events per observation window; , To output energy to acoustic emission devices; For the first The maximum logarithmic energy level within each observation window.
[0009] Furthermore, in S3, the event density, b-value, reverse damage amount, S-value, proportion of shear-type events, and proportion of tensile-type events are denoted as the [missing information]. acoustic emission characteristics ,in =1, 2, 3, 4, 5; Normalized values for each acoustic emission characteristic are: ; in, For the first Within the observation window, the first Normalized values of class features; , These are the lower and upper bounds of the normalization boundary, determined based on the calibration specimens. Pearson correlation coefficient between the original values of each acoustic emission characteristic and the macroscopic mechanical damage amount; When the acoustic emission characteristic type is event density, b-value, reverse damage amount, and S-value... , The baseline value and the 95th percentile critical value of the fatigue loading stabilization stage of the calibrated specimen were used respectively; when the acoustic emission characteristic type was shear-type event proportion and tensile event proportion... , The 5th percentile and 95th percentile values of this characteristic data were used respectively during the entire lifespan of the calibrated specimen.
[0010] Furthermore, in S3, the acoustic emission damage factor The formula is: ; in, For the first Within the observation window, the first Normalized values of class features =1,2,3,4,5, corresponding to event density, b-value reverse damage amount, S-value, proportion of shear-type events and proportion of tensile-type events, respectively; Correlation weights for various features; correlation weights for: ; in, This represents the Pearson correlation coefficient; For calibration specimen number Normalized value sequence of acoustic emission features; To calibrate the sequence of macroscopic mechanical damage quantities of the specimen; For summation index variables; For calibration specimen number Normalized values of acoustic emission characteristics; .
[0011] Furthermore, in S3, when the number of events in the observation window is less than the minimum number of events required for stable fitting of the b-value, linear interpolation is performed using the b-values of adjacent effective observation windows. The b-value interpolation is only used to maintain the continuity of the amplitude distribution characteristic sequence and does not change the actual number of events and crack mode count in that window. When there are no effective acoustic emission events in the observation window, the proportion of shear-type events and the proportion of tensile-type events are set to 0, and the no-event window mark is retained. When the number of valid acoustic emission events within the observation window meets the following conditions In this case, the observation window is defined as an event sparse window. The b-value of this window is obtained by linear interpolation of adjacent valid observation windows, while the event density, S-value, proportion of sheared events, and proportion of stretched events are still calculated based on the actual valid events. ; ; In the formula, The number of valid acoustic emission events within the k-th observation window; The minimum number of events required to stably calculate the value of b; and These represent the number of shear-type and stretch-type events, respectively. and These represent the proportions of shear-type and stretch-type events, respectively.
[0012] when At that time, the event density, S-value, proportion of shearing events and proportion of stretching events are all set to 0, and the no-event window marker is retained, and no proportion division calculation is performed.
[0013] Furthermore, in S5, the overall damage growth rate for: ; In the formula, represents the comprehensive damage growth rate corresponding to the kth observation window; j is the sequence number of the fitted observation window. For the first The cumulative number of cycles corresponding to each observation window; The comprehensive damage index for the j-th observation window; and These represent the average number of cycles and the comprehensive damage index within the selected observation window, respectively. , m represents the number of observation windows used for fitting.
[0014] The technical solution of this application has the following beneficial effects: This method synchronously acquires acoustic emission data and loading data throughout the entire fatigue loading process, dividing the experimental process into continuous observation windows with a unified time reference. This achieves temporal alignment and deep fusion of acoustic emission micro-damage information and macroscopic mechanical response. The method uses five types of acoustic emission characteristics to form an acoustic emission damage factor, which, together with the macroscopic mechanical damage quantity, forms a comprehensive damage index. This index is then used to directly calculate the predicted remaining life and predicted total fatigue life at that moment.
[0015] In the acoustic emission dimension, this method uses event density, b-value reverse damage amount, S-value, shear event ratio, and tensile event ratio as five types of acoustic emission features, corresponding to damage activity frequency, amplitude distribution variation, comprehensive energy level activity, and crack mode composition, respectively. This significantly expands the physical dimension of acoustic emission damage information compared to a single parameter. After determining the weights of these five types of acoustic emission features through correlation analysis with macroscopic mechanical damage amount, they are fused into an acoustic emission damage factor. This allows the shear and tensile event ratios to participate in lifetime prediction according to their actual correlation contribution, effectively reduces the influence of weakly correlated features, and improves the interpretability of multi-parameter fusion.
[0016] In the macroscopic mechanical dimension, this method calculates and weights dynamic stiffness, force amplitude, displacement amplitude, and dissipated energy cyclically to form a macroscopic mechanical damage quantity. This allows for the identification of progressive degradation and fatigue acceleration stages of load-bearing performance, making full use of complete loading data. Ultimately, the acoustic emission damage factor and the macroscopic mechanical damage quantity jointly determine the comprehensive damage index, and the remaining life is calculated from the difference between this index and the critical value, along with its growth rate. Detailed Implementation
[0017] The present application will now be described in detail with reference to embodiments. The various examples are provided by way of explanation and not for limitation of the present application.
[0018] This method is applicable to fatigue life prediction of asphalt mixtures with the same mix proportion, specimen size, acoustic emission threshold, and loading conditions. It mainly consists of two stages: The first stage (steps S1-S5) involves subjecting several calibrated specimens to full-life fatigue loading to determine the RA value, average frequency discrimination threshold, normalized boundaries of each acoustic emission characteristic, correlation weights, macroscopic mechanical damage combination coefficient, fusion coefficient, and critical fusion damage value, in order to establish a model. The second stage (step S6) involves rapid prediction using a target specimen. The target specimen is a representative core sample drilled from the pavement to be tested, or it can be an indoor molded specimen with a material condition comparable to the pavement to be tested.
[0019] Calibration specimens and target specimens should have the same or equivalent asphalt mixture mix proportions, specimen dimensions, aging and environmental conditions, loading methods, loading levels, test temperatures, acoustic emission thresholds, and sensor arrangements. The first stage of calibration work can establish a parameter database in advance. When the material type and test conditions are within the existing calibration range, it is not necessary to conduct full-life calibration tests for each pavement to be tested. Only when applicable calibration data is lacking should full-life calibration tests under the corresponding conditions be conducted. Target specimens only need to undergo short-term fatigue loading, with acoustic emission and mechanical data collected simultaneously.
[0020] A method for predicting the fatigue life of asphalt mixtures by integrating multiple acoustic emission parameters includes the following steps: S1. Establish calibration samples. Conduct full-life fatigue loading on calibration specimens of asphalt mixture with the same mix proportion for the surface layer of the road to be tested, and simultaneously collect acoustic emission data and loading data during the fatigue loading process, so as to determine characteristic reference values, characteristic critical values and life prediction parameters based on the complete failure process of the calibration specimens; The acoustic emission data includes the amplitude, rise time, duration, ring count, energy, and occurrence time of the acoustic emission event; the loading data includes the cycle number, axial displacement, axial force, and running time for each sampling point.
[0021] S1.1 Determine the time observation window; using the running time and acoustic emission event occurrence time in the loaded data as a unified time reference, divide the experimental process into continuous time windows, with a window length generally ranging from 3s to 60s.
[0022] S2. Calculate stiffness damage, force amplitude damage, displacement amplitude damage, and dissipated energy damage based on the loading data, and then weight and fuse these four factors to construct the first... Macroscopic mechanical damage quantity per observation window Specifically, it includes the following steps: S2.1 Calculate the cycle-by-cycle mechanical characteristics. During the fatigue loading process of the calibration specimen... The axial force and axial displacement time history calculation force amplitude for each cycle Displacement amplitude Dynamic stiffness Hysteresis dissipation energy ; ; ; ; ; in, The force amplitude in the j-th cycle; Let be the displacement amplitude of the j-th cycle; and These are the maximum and minimum values of the axial force, respectively. and These are the maximum and minimum values of the axial displacement, respectively. For dynamic stiffness; The area enclosed by the hysteresis curves of axial force and axial displacement; To prevent positive numbers with a denominator of zero.
[0023] The median of the calculation results for each cycle within the k-th observation window is taken to obtain the dynamic stiffness of that observation window. Amplitude Displacement amplitude and dissipated energy .
[0024] S2.2 Constructing Macroscopic Mechanical Damage. Based on the dynamic stiffness, force amplitude, displacement amplitude, and dissipated energy during the stable loading phase, stiffness damage is constructed respectively. Force amplitude damage Displacement amplitude damage and dissipated energy damage And by weighting and integrating the four elements, the first... Macroscopic mechanical damage quantity per observation window ; ; ; ; ; ; Where T is the interval constraint function, This indicates stiffness damage. Force amplitude damage Displacement amplitude damage and dissipated energy damage All values are limited to the range of 0 to 1; values less than 0 are taken as 0, and values greater than 1 are taken as 1. , , and These represent the stiffness damage, force amplitude damage, displacement amplitude damage, and dissipated energy damage for the kth observation window, respectively. , , and These are the reference values for the corresponding mechanical parameters (dynamic stiffness, force amplitude, displacement amplitude, and dissipated energy) during the stable loading stage of the calibration specimen. and These represent the displacement amplitude and dissipated energy at which the calibration specimen reaches the fatigue failure criterion, respectively. When multiple calibration specimens are available, the median of the calculated results for each reference value and critical value is taken. In the macroscopic mechanical damage formula... , , , As weight, and , Under the above constraints, candidate weight combinations are set with a step size of 0.05, and the predicted fatigue life of the calibrated specimens is calculated respectively. The weight combination with the smallest standard life mean square error is taken as the final value.
[0025] S3. Calculate the event density, b-value, reverse damage amount, S-value, proportion of shear-type events, and proportion of tensile events based on the acoustic emission data. After normalization, calculate the macroscopic mechanical damage amount. The acoustic emission damage factor is obtained by fusing the correlation weights. The steps include: S3.1 Calculate the acoustic emission event density. Statistical analysis of the... Number of valid acoustic emission events within each observation window Divide by the actual effective duration of the window. .
[0026] ; In the formula, For the first Acoustic emission event density for each observation window. A significant increase in event density indicates enhanced local damage activity per unit time.
[0027] S3.2 Calculate the b-value and its reverse damage amount. Using 2dB amplitude intervals, count the cumulative number of events with amplitudes not less than each threshold, and perform least-squares fitting on the common logarithm of the cumulative frequency and the variable obtained by dividing the amplitude threshold by 20. ; In the formula, This indicates that the amplitude is not less than the threshold. The cumulative number of acoustic emission events; , The first Intercept and b-value of each observation window; For the observation window number, This is the amplitude threshold number; A decrease in the b-value indicates an increase in the proportion of large-value events; to unify the damage direction of various features, the b-value is converted into a reverse damage quantity: ; In the formula, It increases as the value of b decreases; For the first The b-value for each observation window; , These represent the minimum and maximum values of b during the full-life fatigue loading process of the calibration specimen, respectively. When the number of events in the observation window is less than the minimum number of events required for stable fitting of the b-value, linear interpolation is performed using the b-values of adjacent effective observation windows. The b-value interpolation is only used to maintain the continuity of the amplitude distribution characteristic sequence and does not change the actual number of events and crack mode count in the window. When there are no effective acoustic emission events in the observation window, the proportion of shear-type events and the proportion of tensile-type events are set to 0, and the no-event window mark is retained. An observation window with fewer events than the minimum number of events required for stable fitting of the b-value and no valid acoustic emission events is called an event sparse window; the event density, S-value, and shearing event ratio of the event sparse window are still calculated based on the actual number of events and the effective duration.
[0028] S3.3 Calculate the S-value activity. The S-value is calculated based on the number of events, event energy levels, and maximum energy level for each observation window. The S-value describes the overall intensity of acoustic emission activity within that window. ; in, For the first The number of events per observation window; , To output energy to acoustic emission devices; For the first The maximum logarithmic energy level within each observation window; When the acoustic emission device outputs energy count When this is done, it is converted into a logarithmic energy level. , ,make It also reflects the frequency of events, the average energy level effect, and the maximum energy level within the window.
[0029] S3.4 The calculation steps for the proportion of shear-type events and the proportion of stretch-type events are as follows: S3.4.1 Calculate the RA value, average frequency, and classify the event types. For the first... Individual acoustic emission events, with rise time With amplitude The ratio is used to calculate the RA value, based on the ring count. With duration The ratio is used to calculate the average frequency. .
[0030] ; ; in, and For calibration thresholds under the same material, sensor arrangement, acquisition threshold, and loading conditions, S, T, and M represent shear-type, tensile-type, and mixed-type events, respectively. When independent crack type markers are available, the thresholds can be determined by classification accuracy or cross-validation; when independent markers are lacking, a two-dimensional partition can be formed using the RA value of the calibration events and the median of the average frequency. Events that do not simultaneously meet the shear-type or tensile-type conditions are classified as mixed-type to reduce misclassification of boundary events.
[0031] S3.4.2 Calculate the proportion of shearing events and the proportion of stretching events Statistics of the first Number of shearing events within each observation window Stretch-type event count and the total number of valid events Mixed events are counted. It is not used as a fusion feature on its own.
[0032] ; S3.4.3. Determine the normalization boundary based on the calibrated specimens and calculate each normalization characteristic. The event density, b-value, reverse damage amount, S-value, proportion of shear-type events, and proportion of tensile-type events are denoted as the [missing value]. acoustic emission characteristics ,in =1, 2, 3, 4, 5; Normalized values for each acoustic emission characteristic are: ; in, For the first Within the observation window, the first Normalized values of class features; , These are the lower and upper bounds of the normalization boundary, determined based on the calibration specimens. Let Pearson's correlation coefficient be the original value of each acoustic emission characteristic and the amount of macroscopic mechanical damage. Then, reverse normalization is used to make all All increase with increasing macroscopic damage; ; In the formula, For the first Pearson correlation coefficient between acoustic emission characteristics and macroscopic mechanical damage; To determine the number of effective observation windows for the specimen; and These are the normalized value of the acoustic emission characteristic of type q and the amount of macroscopic mechanical damage within the k-th observation window, respectively. and These are the average values of the corresponding sequences.
[0033] When the acoustic emission characteristic type is event density, b-value, reverse damage amount, and S-value... , The baseline value and the 95th percentile critical value of the fatigue loading stabilization stage of the calibrated specimen were used respectively; when the acoustic emission characteristic type was shear-type event proportion and tensile event proportion... , The 5th percentile and 95th percentile values of this characteristic data were used respectively during the entire lifespan of the calibrated specimen.
[0034] S3.4.4 Calculate the correlation coefficients and correlation weights between each normalized characteristic and the amount of macroscopic mechanical damage. for: ; in, This represents the Pearson correlation coefficient; For calibration specimen number Normalized value sequence of acoustic emission features; To calibrate the sequence of macroscopic mechanical damage quantities of the specimen; For summation index variables; For calibration specimen number Normalized values of acoustic emission characteristics; ; Relevance weight This approach assigns higher weights to acoustic emission characteristics that are strongly correlated with the evolution of macroscopic mechanical damage, and allows the proportion of shear-tension events to participate in the fusion process based on their actual data contributions.
[0035] S3.5. The normalized event density, b-value inverse damage, S-value, proportion of shear-type events, and proportion of stretch-type events are fused according to their correlation weights to construct the acoustic emission damage factor. : ; in, For the first Within the observation window, the first Normalized values of class features =1,2,3,4,5, corresponding to event density, b-value reverse damage amount, S-value, proportion of shear-type events and proportion of tensile-type events, respectively; Correlation weights for various features. Acoustic emission damage factor. The damage degree is comprehensively represented by acoustic emission activity frequency, amplitude distribution, energy level activity, and shear crack mode.
[0036] S4. Construct a comprehensive damage index. This involves using the acoustic emission damage factor of the current observation window. Compared with macroscopic mechanical damage By fusion coefficient By combining the results, a comprehensive damage index is obtained. : ; Among them, the fusion coefficient This indicates the proportion of acoustic emission damage factor in the overall damage index. ; The fusion weight represents the amount of macroscopic mechanical damage; the fusion coefficient. The candidate value is determined based on the minimum mean square error of the standardized lifetime of the calibration sample, and remains unchanged during the window-by-window prediction process of the target sample after determination. S5. Calculate the current comprehensive damage growth rate of the target specimen. Using the current observation window of the target specimen as the endpoint, select the current observation window and the nearest preceding window. There are 1 observation window, totaling One observation window is used to calculate the overall damage growth rate: ; ; ; In the formula, represents the comprehensive damage growth rate corresponding to the kth observation window; j is the sequence number of the fitted observation window. For the first The cumulative number of cycles corresponding to each observation window; The comprehensive damage index for the j-th observation window; and , which represent the number of cycles and the average value of the comprehensive damage index within the selected observation window, respectively; m is the number of fitted observation windows.
[0037] In this embodiment, m=3. After completing at least three consecutive observation windows, the growth rate can be recalculated after each update of the current observation window; If the current comprehensive damage growth rate is less than or equal to 0, the most recent effective positive growth rate will be used, or the fitting window will be expanded and the calculation will be recalculated to reduce the impact of short-term acoustic emission discrete fluctuations.
[0038] S6. Drill representative core samples from the road surface to be tested as target specimens. Perform fatigue loading and acoustic emission monitoring under the same conditions as the calibration specimens, and analyze the comprehensive damage index. Predicting remaining lifespan and predicted total lifespan : ; ;; in, The critical comprehensive damage value is determined by full-life calibration specimens with the same mix proportion and test conditions; This is the current observation window number; This represents the current overall damage growth rate; For the first The cumulative number of fatigue loading cycles corresponding to each observation window; comprehensive damage index Overall damage growth rate and cumulative number of cycles All samples were obtained from the target sample in step S5. After at least three consecutive observation windows have been completed for the target specimen, calculations can be performed in any current observation window without loading the specimen to fatigue failure. Assuming each observation window is 20 seconds, the minimum effective data acquisition time is 60 seconds, which also includes pre-loading and stabilization loading times.
[0039] Through the above steps, for each current observation window that meets the minimum data length requirement, an acoustic emission damage factor can be formed from five types of acoustic emission characteristics, and together with the macroscopic mechanical damage quantity, a comprehensive damage index can be formed, which can then be used to directly calculate the predicted remaining life and predicted total fatigue life at that moment.
[0040] Furthermore, in step S4, the fusion coefficient The following steps are followed to determine the candidate values: Set candidate values in the interval [0,1] with a step size of 0.05; calculate the comprehensive damage index corresponding to each candidate value, and perform fatigue life back-calculation using calibrated specimens; calculate the average relative error between the predicted life and the actual fatigue life. ; In the formula, Take the fusion coefficient as The average relative error over time; The total number of prediction results involved in the error calculation; The prediction result number; To use the fusion coefficient The obtained number One predicted fatigue life; For the first The actual fatigue life corresponding to each calibration specimen or observation point; The candidate value corresponding to the minimum normalized lifetime mean square error is determined as the fusion coefficient: ; In the formula, This is the final determined fusion coefficient.
[0041] Furthermore, in step S6, the comprehensive damage index at which the calibration specimen reaches the fatigue failure cycle number is defined as the critical comprehensive damage value of the specimen. When there are multiple calibration specimens, the median of the critical comprehensive damage values of all calibration specimens is taken. ; In the formula, This is the critical comprehensive damage value; Let R be the comprehensive damage index at which the r-th calibration specimen reaches fatigue failure; R is the number of calibration specimens. When predicting the life of the target specimen, the values obtained from calibration are directly used. There is no need to wait for the target specimen to fail.
[0042] In the above text, the fatigue failure cycle count refers to the number of cycles required to reduce the dynamic stiffness to 50% of the initial dynamic stiffness for the r-th full-life calibration specimen. ; In the formula, Let r be the number of fatigue failure cycles for the r-th calibration specimen; The dynamic stiffness at the number of cycles n; This is the initial dynamic stiffness. If the specimen completely fractures before reaching the above conditions, the number of cycles at which complete fracture occurs is taken as the initial dynamic stiffness. .
[0043] Furthermore, the method for predicting the fatigue life of asphalt mixtures by fusion of multiple acoustic emission parameters also includes step S7: When it is necessary to convert the remaining fatigue cycle count of the target specimen into the remaining equivalent standard axle load count of the road surface to be tested, the equivalent load conversion factor is used: ; ; ; In the formula, This is the conversion factor between indoor loading cycles and the number of standard axle load applications on the road surface; The key stress or strain amplitude for indoor fatigue testing; The key stress or strain amplitude at the corresponding location of the road surface under standard axle load; The fatigue sensitivity index is obtained by fitting fatigue tests at different loading levels; The predicted number of remaining fatigue cycles for the target specimen; The remaining equivalent standard axle load application count for the road surface under test; The number of equivalent standard axle loads applied to the road surface under test is the annual average number of times. To predict the remaining service life.
[0044] Example This embodiment uses AC-16 graded asphalt mixture, which is sheared and compacted to prepare test slabs. After cooling, these slabs are cut into small beam specimens with a length of 380 mm, a width of 63.5 mm, and a height of 50 mm. Fatigue loading is performed using a four-point bending method at a test temperature of 20℃ and a loading frequency set to 10 Hz according to the test conditions. The acoustic emission equipment used is the German Vallen AMSY-6 acoustic emission equipment; domestic equipment can also be used as long as it meets the parameter acquisition requirements. The acquisition threshold is set to 40 dB. The event occurrence time, amplitude, rise time, duration, ring count, and energy are recorded. Simultaneously, the load, displacement, and cumulative number of cycles during the loading process are also acquired.
[0045] The calibration specimen and the target specimen used the same mix ratio, molding method, dimensions, loading level, temperature, and acoustic emission acquisition conditions. Complete fatigue loading records from both sets of specimens were used for parameter calibration. A separate set of specimens not included in this parameter calibration was selected as the target specimen. The calibration specimens were numbered B1 and B2, and the target specimen was numbered T1.
[0046] A method for predicting the fatigue life of asphalt mixtures using acoustic emission multi-parameter fusion includes the following steps: S1. Establish calibration samples; Full-life four-point bending fatigue loading was carried out on calibration specimens B1 and B2, and acoustic emission data and loading data were collected simultaneously during the fatigue loading process. S1.1 Determine the time observation window; using the loading operation time and the time of acoustic emission event occurrence as a unified time reference, the test process is divided into continuous time observation windows; in this embodiment, the window length is 20s, and under the 10Hz loading condition, a single observation window corresponds to approximately 200 loading cycles, and the actual number of cycles within the window is based on the original loading record.
[0047] The loading records of the calibration specimens were processed cyclically to extract dynamic stiffness, force amplitude, displacement amplitude, and dissipated energy. The median dynamic stiffness from the 50th to the 150th cycle was taken as the reference stiffness, and the fatigue failure criterion was the first time the dynamic stiffness decreased to 50% of the reference stiffness. The reference stiffnesses of calibration specimens B1 and B2 were 5.90 kN / mm and 5.70 kN / mm, respectively, with corresponding failure stiffness thresholds of 2.95 kN / mm and 2.85 kN / mm, respectively. The measured fatigue failure lives were 2220 and 2254 cycles, respectively. The specific results are shown in Table 1.
[0048] Table 1. Reference stiffness and failure life of calibration specimens B1 and B2
[0049] S2. Calculate stiffness damage, force amplitude damage, displacement amplitude damage, and dissipated energy damage based on the loading data, and then weight and fuse these four factors to construct the first... Macroscopic mechanical damage quantity per observation window ; S2.1 Calculate the cycle-by-cycle mechanical characteristics; perform window division and feature extraction on the records of calibration samples B1 and B2. The upper limit of the window displacement amplitude used for the target sample calculation is 0.066614128 mm, and the upper limit of the window dissipation energy is 0.017064960 kN·mm.
[0050] S2.2 Construct macroscopic mechanical damage quantities; Based on the mechanical parameters during the stable loading stage, stiffness damage, force amplitude damage, displacement amplitude damage, and dissipated energy damage are constructed respectively. After being constrained to the range of 0 to 1 by an interval constraint function, the macroscopic mechanical damage is obtained by weighted fusion. ; In this embodiment, four non-negative damage parameters with a total weight of 1 are used as constraints. The weight search step size is 0.05, resulting in 1771 combinations of mechanical coefficients. The fusion coefficient is set with 21 candidate values with a step size of 0.05, and a total of 37191 joint candidate parameters are calculated.
[0051] Parameter selection was performed using two sets of calibration samples, which were alternately used. In the first round, parameters were determined using B2 and the predicted lifetime was calculated against B1. In the second round, parameters were determined using B1 and the predicted lifetime was calculated against B2. Each round contained eight evaluation windows.
[0052] Within the above candidate range, the parameter combinations with the smallest standardized lifetime mean square error are shown in Table 2: Table 2 Macroscopic mechanical damage coefficient and fusion coefficient
[0053] In this embodiment, the mechanical coefficient is set to 0, therefore, force amplitude damage and energy dissipation damage do not directly participate in the macroscopic mechanical damage weighting of the selected combination. The mean square errors of the standardized lifetimes of the two wheels are 0.148116616 and 0.150458169, respectively, with an average value of 0.149287392.
[0054] S3. Calculate the event density, b-value, reverse damage amount, S-value, proportion of shear-type events, and proportion of tensile events based on the acoustic emission data. After normalization, calculate the macroscopic mechanical damage amount. The acoustic emission damage factor is obtained by fusing the correlation weights. ; The event density is obtained by counting the number of valid acoustic emission events within the k-th observation window and dividing it by the actual effective duration of the window. The cumulative number of events is counted with an amplitude interval of 2dB, and the b value of each observation window is obtained by least squares fitting; a decrease in the b value indicates an increase in the proportion of large-amplitude events, and the b value is mapped to the reverse damage amount.
[0055] The lower bound of the effective b-values in the calibration data is 0.946954494, the upper bound is 2.807670301, and the median is 1.557987152. For windows where the b-values cannot be effectively fitted, the most recent effective b-value is used; before obtaining the first effective b-value, the aforementioned calibration median is used.
[0056] Based on the calculation results of the original fields of the calibrated events, the RA threshold for the event partition was determined to be 0.212809917 μs / dB, and the average frequency characteristic threshold was determined to be 0.044876589 counts / μs. According to this partitioning rule, the events were divided into shear-type, stretch-type, and mixed-type events, with mixed-type events included in the total number of events.
[0057] The upper and lower bounds and normalization directions of the five types of acoustic emission characteristics were determined, and the normalized acoustic emission characteristics were calculated; the normalization parameters in this embodiment are shown in Table 3.
[0058] Table 3 Normalized parameters of acoustic emission characteristics in the embodiments
[0059] Normalization results are limited to the range of 0 to 1. S-values without an event window are retained as missing values and are not recorded as measured zero values. The above values are the final parameters recalculated using two sets of calibration samples after selecting the parameter combination; in each training round of parameter search, the parameters for that round are determined only using the corresponding training samples.
[0060] Using the mechanical coefficients selected in Table 2, the macroscopic mechanical damage of the two sets of calibration samples was recalculated, and the correlation coefficients between the five types of normalized acoustic emission characteristics and the macroscopic mechanical damage were calculated. The sum of the absolute values of the five correlation coefficients was 0.624678844, and the weights were obtained after normalization as shown in Table 4.
[0061] Table 4. Correlation coefficients and weights of acoustic emission characteristics in this embodiment
[0062] The normalized five types of acoustic emission features are multiplied by their corresponding correlation weights and summed to obtain the acoustic emission damage factor for the k-th observation window. Substituting the relevance weights into Table 3, we obtain the following formula: ; In the above formula, , , , , The respective The normalized values of five features for each observation window correspond to event density, b-value reverse damage amount, S-value, proportion of shearing events, and proportion of stretching events, respectively. S4, Structural Comprehensive Damage Index ; Acoustic emission damage factor in the current observation window Compared with macroscopic mechanical damage By fusion coefficient Combined to obtain comprehensive damage index ; The candidate fusion coefficients are traversed in the interval [0,1] with a step size of 0.05, and the optimal fusion coefficient is determined by minimizing the average relative error of the calibrated specimen lifetime prediction. The fusion coefficient in this embodiment =0.10, that is, the acoustic emission damage factor weight is 0.10, and the macroscopic mechanical damage amount weight is 0.90.
[0063] The comprehensive damage value at the failure time of the calibration specimen was determined. Interpolation of the comprehensive damage index for adjacent windows was performed at the failure cycle. The comprehensive damage value at failure B1 was 0.392448065, and the comprehensive damage value at failure B2 was 0.241775438. The median was taken to obtain the fixed critical comprehensive damage value of 0.317111752 for the target specimen. The critical comprehensive damage values of the calibration specimens are shown in Table 5.
[0064] Table 5 Critical comprehensive damage values of calibrated specimens
[0065] S5. Calculate the current comprehensive damage growth rate of the target specimen; Selecting the current observation window and the three most recent observation windows, the comprehensive damage index and the cumulative number of cycles are fitted using the least squares method to obtain the current comprehensive damage growth rate. If the fitted growth rate is ≤0, the most recent effective positive growth rate is used to eliminate the influence of short-term fluctuations in acoustic emission. S6. Calculate the acoustic emission and mechanical damage state of the target specimen in the current window, calculate the damage growth rate, and output the fatigue life of the target specimen.
[0066] After fixing the above calibration parameters, window-by-window calculations are performed according to the time sequence of the target sample T1 records. Each prediction time point uses only the target sample records from that time point and earlier.
[0067] Taking the cumulative loading of 3000 times as an example, the current time is the 15th complete observation window, with a time range of 280 to 300 seconds, corresponding to the 2801st to 3000th cycles.
[0068] The reference values for the stable stage of the target specimen are: dynamic stiffness 5.847646479 kN / mm, force amplitude 0.373573792 kN, displacement amplitude 0.063622021 mm, and dissipated energy 0.002281878 kN·mm.
[0069] The mechanical characteristics and damage components of the current window are shown in Table 6.
[0070] Table 6 Mechanical characteristics and damage components of the target specimen in the current window
[0071] After weighting with calibration coefficients, the contributions of stiffness damage and displacement amplitude damage are 0.156451124 and 0.053667030, respectively, resulting in a current macroscopic mechanical damage amount of 0.210118154.
[0072] The current window contains 95 valid acoustic emission events, including 18 shear-type, 32 stretch-type, and 45 mixed-type events. The event density is 4.75 s. -1 The proportion of shear events was 0.189473684, and the proportion of stretch events was 0.336842105.
[0073] The current window value b is 1.577197129, and its reverse damage is 0.661290224. The maximum acoustic emission amplitude is 59.6 dB, and the mean of the amplitude exponent is 4237.536350786. The calculated results of the three components of the S value are 0.231925734, 0.105186290, and 0.044700000, respectively, resulting in an S value of 0.381812024.
[0074] Normalization was performed using a fixed calibration boundary, and the results are shown in Table 7.
[0075] Table 7 Acoustic emission characteristics and weighted contributions of the target sample in the current window
[0076] The current b-value indicates that the reverse damage amount is below the calibration lower bound, so it is normalized to 0. After weighting the five features, the acoustic emission damage factor is obtained as 0.597598867.
[0077] Further calculations based on the fixed fusion coefficient yielded a current comprehensive damage index of 0.248866226.
[0078] The damage indices of the four windows at the end of the target sample are shown in Table 8.
[0079] Table 8 Damage index of the final window of the target sample
[0080] Fitting the data using three windows corresponding to 2600, 2800, and 3000 cycles, we obtained the current original damage growth rate as −0.000351963085 per cycle.
[0081] According to the established processing rules in this example, when the initial growth rate is not positive, the most recent effective positive growth rate is used. Therefore, the current lifetime is calculated using the effective positive growth rate of 0.000108985886 per cycle at 2800 cycles. This rate is determined by three windows corresponding to 2400, 2600, and 2800 cycles.
[0082] The difference between the current comprehensive damage index and the calibrated critical value is 0.068245526. Based on this damage difference and the selected growth rate, the predicted remaining lifetime of the target sample is 626.186820 cycles, and the predicted total lifetime is 3626.186820 cycles. The current prediction output of this embodiment is shown in Table 9.
[0083] Table 9 Current prediction results for the target sample
[0084] A post-test verification of the complete loading record of the target specimen revealed a 50% reference stiffness threshold of 2.923823239 kN / mm, with 3417 cycles required to first reach this threshold. Therefore, the measured fatigue failure life of the target specimen was 3417 cycles. The predicted total life was 3626.19 cycles, with an absolute error of 209.19 cycles and a relative error of 6.12% compared to the measured failure life.
[0085] Note that the calibration specimen is used to determine the feature normalization boundary, transformation direction, correlation weight, fusion coefficient, and critical comprehensive damage value. Once these parameters are determined, they remain fixed during the window-by-window prediction process for the target specimen. Each prediction time point uses only the target specimen monitoring data obtained at that time point and previously; records of subsequent loading of the target specimen to failure are used for post-event verification of the prediction results and are not involved in the parameter determination for previous prediction time points. This embodiment ultimately predicts the fatigue life of the target specimen (indoor beam specimen). When the target specimen is a pavement core sample, its remaining fatigue cycle count needs to be converted into the remaining equivalent standard axle load count of the pavement to be tested using step S7 above.
[0086] The above description is merely a preferred embodiment of this application and is not intended to limit this application. Various modifications and variations can be made to this application by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the protection scope of this application.
Claims
1. A method for predicting the fatigue life of asphalt mixtures by integrating multiple acoustic emission parameters, characterized in that, Includes the following steps: S1. Conduct full-life fatigue loading on the calibration specimens of asphalt mixture with the same mix proportion for the surface layer of the road to be tested, and simultaneously collect acoustic emission data and loading data during the fatigue loading process; divide the test process into continuous time windows with a unified time reference; S2. Calculate stiffness damage, force amplitude damage, displacement amplitude damage, and dissipated energy damage based on the loading data, and then weight and fuse these four factors to construct the first... Macroscopic mechanical damage quantity per observation window ; S3. Calculate the event density, b-value, reverse damage amount, S-value, proportion of shear-type events, and proportion of tensile events based on the acoustic emission data. After normalization, calculate the macroscopic mechanical damage amount. The acoustic emission damage factor is obtained by fusing the correlation weights. ; S4. Set the acoustic emission damage factor for the current observation window. Compared with macroscopic mechanical damage By fusion coefficient By combining the results, a comprehensive damage index is obtained. : ; Among them, the fusion coefficient This represents the contribution ratio of acoustic emission damage factor to the overall damage index, determined based on the principle of minimizing the mean square error of the standardized life of the calibrated specimen. ; S5. Using the current observation window of the target specimen as the endpoint, select the current observation window and the nearest previous one. One observation window is used to calculate the overall damage growth rate. ; S6. Drill representative core samples from the road surface to be tested as target specimens. Perform fatigue loading and acoustic emission monitoring under the same conditions as the calibration specimens, and analyze the comprehensive damage index. Predicting remaining lifespan and predicted total lifespan : ; ; in, The critical fusion damage value is determined by full-life calibration specimens under the same conditions; This is the current observation window number; This represents the current overall damage growth rate; For the first The cumulative number of fatigue loading cycles corresponding to each observation window.
2. The method for predicting the fatigue life of asphalt mixtures by acoustic emission multi-parameter fusion according to claim 1, characterized in that, The acoustic emission data includes the amplitude, rise time, duration, ring count, energy, and occurrence time of the acoustic emission event; the loading data includes the cycle number, axial displacement, axial force, and running time for each sampling point.
3. The method for predicting the fatigue life of asphalt mixtures by acoustic emission multi-parameter fusion according to claim 1, characterized in that, In S2, the macroscopic mechanical damage quantity The calculation formula is: ; in, For stiffness damage, For force amplitude damage, For displacement amplitude damage, Damage caused by dissipated energy; , , , As weight, and , Under the above constraints, candidate weight combinations are set with a step size of 0.05, and the predicted fatigue life of the calibration specimens is calculated for each combination. The weight combination with the smallest normalized life mean square error is then selected as the predicted fatigue life. , , , The final value of .
4. The method for predicting the fatigue life of asphalt mixtures by acoustic emission multi-parameter fusion according to claim 1, characterized in that, In S3, the S value is calculated based on the number of events, event energy levels, and maximum energy level for each observation window: ; in, For the first The number of events per observation window; , To output energy to acoustic emission devices; For the first The maximum logarithmic energy level within each observation window.
5. The method for predicting the fatigue life of asphalt mixtures by acoustic emission multi-parameter fusion according to claim 1, characterized in that, In S3, the event density, b-value, reverse damage amount, S-value, proportion of shear-type events, and proportion of tensile events are denoted as the [number missing]. acoustic emission characteristics ,in =1, 2, 3, 4, 5; Normalized values for each acoustic emission characteristic are: ; in, For the first Within the observation window, the first Normalized values of class features; , These are the lower and upper bounds of the normalization boundary, determined based on the calibration specimens. Pearson correlation coefficients are the original values of each acoustic emission characteristic and the amount of macroscopic mechanical damage.
6. The method for predicting the fatigue life of asphalt mixtures by acoustic emission multi-parameter fusion according to claim 5, characterized in that, When the acoustic emission characteristic type is event density, b-value, reverse damage amount, and S-value... , The baseline value and the 95th percentile critical value of the fatigue loading stabilization stage of the calibrated specimen were used respectively; when the acoustic emission characteristic type was shear-type event proportion and tensile event proportion... , The 5th percentile and 95th percentile values of this characteristic data were used respectively during the entire lifespan of the calibrated specimen.
7. The method for predicting the fatigue life of asphalt mixtures by acoustic emission multi-parameter fusion according to claim 1, characterized in that, In S3, acoustic emission damage factor The formula is: ; in, For the first Within the observation window, the first Normalized values of class features =1,2,3,4,5, corresponding to event density, b-value reverse damage amount, S-value, proportion of shear-type events and proportion of tensile-type events, respectively; The relevance weights for various features.
8. The method for predicting the fatigue life of asphalt mixtures by acoustic emission multi-parameter fusion according to claim 7, characterized in that, Relevance weight for: ; in, This represents the Pearson correlation coefficient; For calibration specimen number Normalized value sequence of acoustic emission features; To calibrate the sequence of macroscopic mechanical damage quantities of the specimen; For summation index variables; For calibration specimen number Normalized values of acoustic emission characteristics; .
9. The method for predicting the fatigue life of asphalt mixtures by acoustic emission multi-parameter fusion according to claim 1, characterized in that, In S3, when the number of events in the observation window is less than the minimum number of events required for stable fitting of the b value, linear interpolation is performed using the b value of adjacent effective observation windows. The b value interpolation is only used to maintain the continuity of the amplitude distribution characteristic sequence and does not change the actual number of events and crack mode count in the window. When there are no valid acoustic emission events in the observation window, the proportion of shear-type events and the proportion of stretch-type events are set to 0, and the no-event window mark is retained; When the number of valid acoustic emission events within the observation window meets the following conditions In this case, the observation window is defined as an event sparse window. The b-value of this window is obtained by linear interpolation of adjacent valid observation windows, while the event density, S-value, proportion of sheared events, and proportion of stretched events are still calculated based on the actual valid events. ; ; In the formula, The number of valid acoustic emission events within the k-th observation window; The minimum number of events required to stably calculate the value of b; and These represent the number of shear-type and stretch-type events, respectively. and The proportions of shear-type and stretch-type events are respectively; when At that time, the event density, S-value, proportion of shearing events and proportion of stretching events are all set to 0, and the no-event window marker is retained, and no proportion division calculation is performed.
10. The method for predicting the fatigue life of asphalt mixtures by acoustic emission multi-parameter fusion according to claim 1, characterized in that, In S5, the overall damage growth rate for: ; In the formula, represents the comprehensive damage growth rate corresponding to the kth observation window; j is the sequence number of the fitted observation window. For the first The cumulative number of cycles corresponding to each observation window; The comprehensive damage index for the j-th observation window; and These represent the average number of cycles and the comprehensive damage index within the selected observation window, respectively. , m represents the number of observation windows used for fitting.
Citation Information
Patent Citations
Asphalt mixture fatigue state sound emission early warning method based on multi-parameter fusion
CN119269285A