Long-lasting stable inverse opal photonic crystal thin film, preparation method and application thereof
By using a rigid polymethyl methacrylate framework and a chiral copper (I) cluster in an inverse opal photonic crystal thin film, the problems of polymer inverse opal framework collapse and limited optical function were solved, achieving structural stability and multifunctional integration, simplifying the fabrication process, and providing multi-level information encryption capabilities.
Patent Information
- Application Number
- CN202611657957.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-26
- Publication Date
- 2026-11-24
AI Technical Summary
The polymer inverse opal framework is prone to collapse during long-term storage, and the structural color decays irreversibly. Existing systems have limited optical functions, making it difficult to integrate solvent response and chiral luminescence. Stabilization processes are complex and costly.
A rigid polymethyl methacrylate three-dimensional ordered porous inverse opal framework and chiral copper (I) cluster luminescent units loaded in the pores were used to prepare a long-lasting and stable inverse opal photonic crystal thin film by combining colloidal crystal template method and solution casting process. The film has intrinsic structural color, reversible solvent-responsive optical properties and photoactivated circular polarization luminescence properties.
It achieves long-term structural stability of inverse opal photonic crystal thin films at room temperature, possesses multi-dimensional optical function output, simplifies the preparation process, reduces costs, and provides multi-level information encryption and dynamic anti-counterfeiting capabilities.
Smart Images

Figure CN123156338A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of functional photonic materials and structural color materials, and in particular to a long-lasting and stable inverse opal photonic crystal thin film, its preparation method, and its applications. Background Technology
[0002] Structural colors originate from the Bragg reflection of visible light through micro- and nano-periodic structures, exhibiting characteristics such as high saturation, resistance to light fading, and angle-dependent iridescence. Inverse opal structures, as a type of three-dimensional ordered porous photonic crystal, offer tunable pore structure and flexible optical control, making them a research hotspot in structural color materials.
[0003] Inverse opal systems based on flexible polymers such as polyurethane and polyacrylamide are prone to chain segment rearrangement during long-term storage at room temperature. This leads to pore wall shrinkage, collapse of the three-dimensional periodic structure, and irreversible decay of the structural color, making them unsuitable for long-term service or recycling. This problem is a major obstacle to the application of polymer inverse opal.
[0004] At the same time, most existing systems only have a single structural color response, making it difficult to integrate multi-dimensional optical signals such as solvent response and chiral luminescence in the same material. This limits the information dimensions that can be used for encoding, making it difficult to further improve the anti-counterfeiting security level.
[0005] Existing stabilization methods, such as using inorganic oxide frameworks or multilayer composite structures, generally require high-temperature sintering and vapor deposition processes, which are complex, costly, and difficult to integrate with subsequent functions. Conversely, systems pursuing multifunctional integration often sacrifice structural stability. Therefore, the trade-off between structural durability and functional diversity in structural color materials remains unresolved. Summary of the Invention
[0006] Therefore, there is a need to provide a long-lasting and stable inverse opal photonic crystal thin film, its preparation method and application, to solve the following problems: 1. During long-term storage, the polymer inverse opal framework suffers from the collapse of its three-dimensional periodic structure and irreversible decay of its structural color due to chain segment rearrangement; 2. Existing systems have limited optical functions and it is difficult to integrate solvent response and chiral luminescence in the same material; Existing stabilization routes are complex and costly.
[0007] To achieve the above objectives, the present invention provides a long-lasting and stable inverse opal photonic crystal thin film, comprising a rigid polymethyl methacrylate three-dimensional ordered porous inverse opal framework, and chiral copper (I) cluster light-emitting units loaded in the pores of the rigid polymethyl methacrylate three-dimensional ordered porous inverse opal framework; the inverse opal photonic crystal thin film simultaneously possesses intrinsic structural color, reversible solvent-responsive optical properties, and photoactivated circularly polarized light emission properties.
[0008] The rigid polymethyl methacrylate (PMMA) framework has a high glass transition temperature of 68-72°C, remaining in a glassy state at room temperature. This inhibits polymer chain rearrangement, thus contributing to the stability of the three-dimensional ordered macroporous structure of the inverse opal photonic crystal film during long-term storage. The chiral copper (I) clusters loaded within the three-dimensional interconnected channels impart circularly polarized luminescence properties to the inverse opal photonic crystal film. The synergistic effect of the rigid framework and the chiral copper (I) clusters enables the inverse opal photonic crystal film to simultaneously possess intrinsic structural color, reversible solvent-responsive optical properties, and photoactivated circularly polarized luminescence properties.
[0009] In this invention, the photoactivated circularly polarized luminescence refers to luminescence with a power density of 700 mW·cm⁻¹. -2 Under continuous irradiation with 365 nm ultraviolet light, the circularly polarized luminescence intensity of the thin film increases to more than 100 times the initial value within the first minute of irradiation and changes by no more than ±10% within the following 3 minutes, while the luminescence asymmetry factor |glum| remains in the range of 0 to 0.024, exhibiting circularly polarized luminescence behavior.
[0010] Furthermore, the pore size of the inverse opal framework is 200–700 nm, which covers the periodic scale required for Bragg reflection in the visible light band, facilitating the tuning of structural color through the particle size of the silica gel template microspheres. The loading amount of the chiral copper (I) cluster is 0.1–3 wt%, based on the mass of the rigid polymethyl methacrylate three-dimensional ordered porous inverse opal framework. This loading range ensures that the number of luminescent units is sufficient to output a detectable circularly polarized emission signal while avoiding fluorescence degradation caused by excessive loading.
[0011] Furthermore, the chiral copper (I) cluster is an R-configuration or S-configuration chiral copper (I) complex, prepared by a coordination reaction between copper hexafluorophosphate tetraacetonitrile and 4-ethynylpyridine, and one of R-binaphthyldiphenylphosphine or S-binaphthyldiphenylphosphine. Using both R-configuration and S-configuration enantiomers, mirror-symmetric circularly polarized emission signals can be obtained, providing a chiral dimension for information encoding.
[0012] Furthermore, after being stored at room temperature in the dark for 10 months, the film still maintains a regularly arranged porous structure on its surface. This characteristic reflects the ability of the inverse opal framework to suppress chain rearrangement, which is beneficial for the long-term service of the inverse opal photonic crystal film.
[0013] This invention also discloses a method for preparing the long-lasting and stable inverse opal photonic crystal thin film, which includes the following steps:
[0014] Step 1: Monodisperse silica microspheres were prepared using the modified Stöber process. Tetraethyl orthosilicate was used as the silica source, anhydrous ethanol and deionized water were used as solvents, and ammonia was used as a catalyst. The particle size of the microspheres was controlled by adjusting the concentration of ammonia. After the reaction, the microspheres were obtained by centrifugation and ethanol washing. In this step, the concentration of ammonia was the only control variable. The particle size of the monodisperse silica microspheres increased with the increase of the amount of ammonia, thus obtaining templates for different structural colors.
[0015] Step 2: The monodisperse silica microspheres are dispersed in anhydrous ethanol to prepare a colloidal suspension, and silica crystalline templates are prepared on a hydrophilic substrate by coating-evaporation induced self-assembly method;
[0016] Step 3: Cast the polymethyl methacrylate solution containing chiral copper (I) clusters onto the silica gel crystal template. After the solvent evaporates, a composite opal film is obtained. The chiral copper (I) clusters are blended with polymethyl methacrylate during the casting process, so that the light-emitting units fill the template pores along with the substrate. The copper clusters are distributed in the channels formed later, eliminating the need for additional impregnation and loading after etching, thus simplifying the process.
[0017] Step 4: The silica gel bulk crystal template is removed by etching with hydrofluoric acid solution. After washing and drying, the inverse opal photonic crystal film is obtained. Hydrofluoric acid has good selectivity for silica, removing the template without damaging the chemical structure of the polymethyl methacrylate backbone.
[0018] Furthermore, step 1 specifically includes:
[0019] Material mixing: First, mix tetraethyl orthosilicate, deionized water, and the first part of anhydrous ethanol, stir to dissolve, then add a mixture of ammonia and the second part of anhydrous ethanol, stir evenly to obtain a reaction solution, wherein the volume fraction of ammonia in the reaction solution is 9%~22%;
[0020] Hydrolysis stage: The reaction solution is hydrolyzed for 10-30 minutes at 15-25℃ and 800-1200 rpm to generate silanol from tetraethyl orthosilicate.
[0021] Growth stage: Reduce the stirring speed to 200-400 rpm, maintain 15-25℃ and continue the reaction for 4-8 hours;
[0022] Post-processing: After the reaction was completed, the solid was separated by centrifugation and washed 2-4 times with anhydrous ethanol to obtain monodisperse silica microspheres.
[0023] Step 1 uses a higher stirring speed during the hydrolysis stage and a lower stirring speed during the growth stage, which is beneficial for obtaining microspheres with good monodispersity.
[0024] Furthermore, the polymethyl methacrylate solution containing chiral copper (I) clusters is obtained by mixing a dichloromethane solution of a polymethyl methacrylate monolayer with a dimethyl sulfoxide solution of chiral copper (I) clusters. After casting, it is first left to stand at room temperature in the dark, and then dried at a constant temperature of 35-45°C.
[0025] Further, the preparation method of the chiral copper (I) cluster is as follows: copper hexafluorophosphate tetraacetonitrile and 4-ethynylpyridine, and one of R-binaphthyldiphenylphosphine or S-binaphthyldiphenylphosphine, are dissolved in a mixed solvent of dichloromethane and methanol at a molar ratio of 1:1:1. After stirring at room temperature until the solid is completely dissolved, triethylamine is added to catalyze the reaction. After filtration, the filtrate is allowed to stand at room temperature in the dark to evaporate, thereby obtaining chiral copper (I) cluster crystals.
[0026] Further, step 2 includes: dispersing the monodisperse silica microspheres in anhydrous ethanol to prepare a colloidal suspension with a mass fraction of 2%-6%, ultrasonically dispersing the suspension, and then dropping 40-60 μL onto one end of a hydrophilic glass slide. The slide is then coated using an automatic coating machine at a speed of 5-15 mm / s. -1 Apply the coating using a scraping method at a specific speed.
[0027] In step 4, the hydrofluoric acid solution has a mass fraction of 5%–15%, the total etching time is 8–16 hours, and the etching is performed with oscillation for 3–5 minutes every 1–3 hours during the etching process. The oscillation refreshes the etching solution within the template pores, which is beneficial for the complete removal of the template.
[0028] This invention also discloses the application of the long-lasting and stable inverse opal photonic crystal film, which is used to prepare optical anti-counterfeiting labels, multi-level information encryption devices, or dynamic optical display devices.
[0029] Compared with the prior art, the present invention has the following technical effects:
[0030] 1. To address the issue of polymer inverse opal frameworks collapsing easily during long-term storage, this invention uses rigid polymethyl methacrylate (PMMA) as the framework material, leveraging its high glass transition temperature to suppress chain rearrangement. Tests show that after 10 months of storage at room temperature in the dark, the inverse opal photonic crystal film still maintains a regularly arranged porous structure on its surface.
[0031] 2. To address the issue of limited optical functionality in existing inverse opal photonic crystal films, this invention loads chiral copper (I) clusters within the three-dimensional interconnected channels. The inverse opal photonic crystal film exhibits both static structural color and reversible solvent response shift in the same reflection channel, and displays ultraviolet-activated circularly polarized luminescence in the emission channel, forming a dual-channel (reflection / emission) optical carrier with a triple stimulus response. Circularly polarized emission spectroscopy tests show that the circularly polarized emission signals of the R-configuration and S-configuration samples are mirror-symmetric, with the highest value of the circularly polarized emission asymmetry factor |glum| being 2.4 × 10⁻⁶. -2 Since the outputs of the three types of optical functions are distinguishable on a time scale (solvent response is on the order of seconds, and circularly polarized luminescence activation is on the order of minutes), this invention can form three levels of interpretation based on reflected color, circularly polarized chirality, and irradiation duration, which can be used for multi-level information encryption and dynamic anti-counterfeiting.
[0032] 3. In view of the problem of the complexity of existing stabilization processes, this invention adopts the colloidal crystal template method and solution casting process. The chiral copper (I) cluster is introduced along with the matrix during the casting process, without the need for high-temperature sintering, vapor deposition or etching and impregnation processes. Casting and etching are both carried out under normal pressure.
[0033] 4. To address the trade-off between structural durability and functional diversity, the rigid polymethyl methacrylate framework responsible for structural stability and the chiral copper (I) cluster responsible for light emission belong to different structural levels in this invention. The former constitutes a three-dimensional ordered porous framework, while the latter is loaded in the pores. The two are spatially separated, which helps to alleviate the mutual constraints between long-term structural maintenance and multimodal optical output. Attached Figure Description
[0034] Figure 1 Differential scanning calorimetry (DSC) curves of the polymethyl methacrylate film and the blue, green, and red inverse opal photonic crystal films obtained in Examples 1-3, respectively, before and after etching; wherein... Figure 1 (a) DSC images of the pure polymethyl methacrylate film prepared in step 3 of Example 1 before and after etching; Figure 1 (b) is a DSC comparison diagram of the composite opal film before etching prepared by steps 1 to 5 of Example 1 and the final prepared blue inverse opal crystal film. Figure 1 (c) is a DSC comparison diagram of the composite opal film before etching prepared by steps 1 to 5 of Example 2 and the finally prepared green inverse opal crystal film. Figure 1 (d) is a DSC comparison diagram of the composite opal film before etching prepared by steps 1 to 5 of Example 3 and the finally prepared red inverse opal crystal film.
[0035] Figure 2Thermogravimetric analysis (TG) curves of polymethyl methacrylate film before and after etching.
[0036] Figure 3 The thermogravimetric analysis (TG) curves of the blue, green, and red inverse opal photonic crystal thin films before and after etching are shown in Examples 1-3, respectively; where, Figure 3 (a) is a TG comparison diagram of the composite opal film before etching prepared in steps 1 to 5 of Example 1 and the final prepared blue inverse opal crystal film. Figure 3 (b) is a TG comparison diagram of the composite opal film before etching prepared in steps 1 to 5 of Example 2 and the finally prepared green inverse opal crystal film. Figure 3 (c) is a TG comparison diagram of the composite opal film before etching prepared in steps 1 to 5 of Example 3 and the final prepared red inverse opal crystal film.
[0037] Figure 4 The images show the microstructure of the silica gel crystalline template as scanned by field emission scanning electron microscopy, along with images showing further processing. Figure 4 (a) is a microscopic morphology image of a silica gel crystalline template obtained by field emission scanning electron microscopy; Figure 4 (b) is the spatial frequency distribution map after the micromorphology map is processed by two-dimensional Fourier fast transform;
[0038] Figure 5 The microstructure images and further processing images of the inverse opal photonic crystal thin film prepared in Example 1 are obtained by field emission scanning electron microscopy. Figure 5 (a) Microscopic morphology of the inverse opal photonic crystal thin film prepared in Example 1, as scanned by field emission scanning electron microscopy; Figure 5 (b) is the spatial frequency distribution map of the micro-morphology image after processing by two-dimensional Fourier fast transform;
[0039] Figure 6 The image shows the cross-sectional structure of the inverse opal photonic crystal thin film prepared in Example 1, obtained by field emission scanning electron microscopy.
[0040] Figure 7 Microscopic morphology image of the inverse opal photonic crystal thin film prepared in Example 1 after being stored at room temperature in the dark for 10 months, scanned by field emission scanning electron microscopy.
[0041] Figure 8 Microscopic morphology of the polyurethane-based blue inverse opal photonic crystal thin film prepared for Comparative Example 4 after being stored at room temperature in the dark for 1 month, as scanned by field emission scanning electron microscopy.
[0042] Figure 9Comparison of the microstructure of the inverse opal photonic crystal thin film prepared in Example 1 after treatment at different temperatures and then scanned by field emission scanning electron microscopy.
[0043] Figure 10 The reflection spectra of the inverse opal photonic crystal thin film obtained in Example 1 in different media;
[0044] Figure 11 The solvent response reflection spectra and cycle stability curves of the inverse opal photonic crystal thin films obtained in Examples 1-3 in ethanol are shown.
[0045] Figure 12 The graphs show the solvent response reflection spectra and cycle stability curves of the inverse opal photonic crystal thin films obtained in Examples 1-3 in water.
[0046] Figure 13 The images show fluorescence intensity diagrams of inverse opal photonic crystal films with different chiral copper (I) cluster loadings in Examples 1 and 4-12; wherein, Figure 13 (a) Fluorescence intensity diagrams of R-configuration chiral copper (I) cluster-doped films with different chiral copper (I) cluster loadings prepared in Examples 1 and 4-7; Figure 13 (b) Fluorescence intensity diagrams of S-configuration chiral copper (I) cluster-doped films with different chiral copper (I) cluster loadings prepared in Examples 8-12;
[0047] Figure 14 Comparison of the changes in luminescence intensity of the inverse opal photonic crystal thin films prepared in Examples 1-3 with the extension of irradiation time;
[0048] Figure 15 Comparison of circularly polarized luminescence of the inverse opal photonic crystal thin films prepared in Examples 1 and 10;
[0049] Figure 16 Comparison of circular dichroic signals of the inverse opal photonic crystal thin films prepared in Examples 1 and 10. Detailed Implementation
[0050] To explain in detail the technical content, structural features, objectives, and effects of the technical solution, the following description is provided in conjunction with specific embodiments and accompanying drawings.
[0051] Example 1: Blue inverse opal photonic crystal thin film loaded with R-configuration chiral copper (I) clusters
[0052] In this embodiment, the silica gel crystalline template microspheres have a particle size of approximately 360 nm, the inverse opal photonic crystal film exhibits a blue structural color, the chiral copper (I) cluster has an R configuration, and the loading amount is 1 wt%.
[0053] 1) Preparation of monodisperse silica microspheres: 3 mL of tetraethyl orthosilicate, 50 mL of anhydrous ethanol, and 2 mL of deionized water were added to a three-necked flask and stirred at 600 rpm at 20°C until the raw materials were uniformly mixed. 9 mL of premixed ammonia (28 wt%) and 25 mL of ethanol solution were added to the system at once, with the volume fraction of concentrated ammonia in the reaction solution being approximately 10%. The stirring speed was increased to 1000 rpm for 10 min to initiate hydrolysis. The stirring speed was then reduced to 300 rpm, and the reaction was maintained at 20°C for 6 h. After the reaction, the microspheres were centrifuged and washed three times at 9000 rpm at 4°C to obtain monodisperse silica microspheres with a particle size of approximately 360 nm, which were then redispersed in anhydrous ethanol for later use. Note that 600 rpm was the stirring speed during the premixing stage, while the stirring speeds during the hydrolysis and growth stages were 1000 rpm and 300 rpm, respectively.
[0054] 2) Photonic crystal template assembly: Prepare a 2 wt% silica-ethanol suspension, sonicate for 1 min and vortex for 1 min to ensure uniform dispersion; use an automatic coating machine to coat the silica-ethanol onto a hydrophilic glass slide at a coating speed of 10 mm / s. -1 The volume of liquid used for each coating was 50 μL, and the coating was applied 15 times on the same glass slide. After coating, the slide was allowed to dry horizontally at room temperature to obtain a blue silica gel crystal template.
[0055] 3) Synthesis of polymethyl methacrylate (PMMA) monolayer: MMA monomer was washed with 5 wt% sodium hydroxide aqueous solution, then with deionized water until neutral, dried over anhydrous magnesium sulfate, and purified by vacuum distillation. 40 g of the purified PMMA monomer was weighed and 0.08 g of benzoyl peroxide (0.2 wt% of monomer mass) was added as initiator. The mixture was stirred until completely dissolved and transferred to a three-necked flask. High-purity nitrogen was purged for 10 min to remove oxygen. The flask was then sealed and placed in an 80℃ constant-temperature water bath for prepolymerization at 300 rpm. After approximately 45 min of reaction, when the viscosity of the system reached a glycerol-like state, the reaction solution was transferred to a polytetrafluoroethylene (PTFE) template. Heating was continued at 60℃ for 24 h until the surface was dry and cured. The temperature was then raised to 100℃ and maintained at this high temperature for 4 h, followed by gradual cooling to room temperature to ensure complete polymerization of all remaining monomers, yielding a PMMA monolayer.
[0056] 4) Synthesis of chiral copper (I) clusters: Weigh 15 mg (0.04 mmol) copper hexafluorophosphate tetraacetonitrile, 25 mg (0.04 mmol) R-binaphthyl diphenylphosphine, and 4 mg (0.04 mmol) 4-ethynylpyridine and add them to a reaction beaker; add 2 mL of a mixed solvent of dichloromethane and 2 mL of anhydrous methanol, and stir at room temperature in the dark for 5 min until the solid is completely dissolved, obtaining a clear yellow solution; add 1 drop of triethylamine to the solution and continue stirring in the dark for 10 min; filter the reaction solution with filter paper, collect the filtrate in a light-protected sample bottle, seal and allow it to stand at room temperature for 12 h to evaporate; after the solvent slowly evaporates, yellow rod-shaped crystals precipitate, wash three times with cold methanol, and dry under vacuum to obtain the R-configuration chiral copper (I) cluster (denoted as R-Cu), which is stored in the dark and refrigerated. The S-configuration chiral copper (I) cluster is prepared using the same method, with S-binaphthyl diphenylphosphine as the chiral ligand (denoted as S-Cu).
[0057] 5) Preparation of composite membrane by blending and casting: Weigh 200 mg of polymethyl methacrylate obtained in step 3), dissolve it in 2 mL of dichloromethane, and stir until completely dissolved; weigh 2 mg of R-configuration chiral copper (I) clusters (R-Cu) obtained in step 4), dissolve them in 1 mL of dimethyl sulfoxide (DMSO) to prepare a 2 mg / mL R-Cu / DMSO stock solution; add 1000 μL of the above stock solution (containing 2.0 mg R-Cu) to the polymethyl methacrylate solution, corresponding to a copper cluster loading of 1 wt% (relative to the mass of polymethyl methacrylate); stir at room temperature in the dark for 5 min to obtain a uniform and transparent yellow blend solution. Slowly cast the blend solution onto the blue silica gel crystal template obtained in step 2), let it stand at room temperature in the dark for 2 h, and after most of the solvent has evaporated, transfer it to a 40℃ constant temperature hot plate to continue drying for 1 h; after cooling to room temperature, demold to obtain a composite opal membrane loaded with 1 wt% R-configuration chiral copper (I) clusters.
[0058] 6) Etching to obtain an inverse opal film: Immerse the composite opal film in a 10% hydrofluoric acid aqueous solution and gently agitate for 3 minutes every 2 hours. Repeat this process 6 times to ensure complete etching of the silica template. After removal, wash the film repeatedly with deionized water and anhydrous ethanol to remove residual hydrofluoric acid. After drying, a blue inverse opal photonic crystal film is obtained.
[0059] Example 2: Green inverse opal photonic crystal thin film loaded with R-configuration chiral copper (I) clusters
[0060] The preparation method of this embodiment is the same as that of Example 1, except that: in step 1), the amount of ammonia water is adjusted to 15 mL, the amount of ethanol is adjusted to 19 mL, the volume fraction of concentrated ammonia water in the reaction solution is about 17%, and monodisperse silica microspheres with a particle size of about 484 nm are obtained; in step 2), a green silica gel bulk crystal template is obtained; and finally, a green inverse opal photonic crystal film is obtained.
[0061] Example 3: Red inverse opal photonic crystal thin film loaded with R-configuration chiral copper (I) clusters
[0062] The preparation method of this embodiment is the same as that of Example 1, except that: in step 1), the amount of ammonia water is adjusted to 19 mL, the amount of ethanol is adjusted to 15 mL, the volume fraction of concentrated ammonia water in the reaction solution is about 21%, and monodisperse silica microspheres with a particle size of about 622 nm are obtained; in step 2), a red silica gel crystalline template is obtained; and finally, a red inverse opal photonic crystal film is obtained.
[0063] Examples 4-7 Blue inverse opal photonic crystal thin films of chiral copper (I) clusters with different loading amounts and R configurations
[0064] The preparation method of this embodiment is the same as that of Example 1, except that the amount of chiral copper (I) clusters is adjusted so that the loading amounts are 0.1 wt%, 0.5 wt%, 2 wt%, and 3 wt% respectively, to obtain samples with different loading amounts.
[0065] Example 8: Blue inverse opal photonic crystal thin film loaded with S-configuration chiral copper (I) clusters
[0066] In this embodiment, the silica gel crystalline template microspheres have a particle size of approximately 360 nm, the inverse opal photonic crystal film exhibits a blue structural color, the chiral copper (I) cluster has an S configuration, and the loading amount is 0.1 wt%.
[0067] 1) Preparation of monodisperse silica microspheres: 3 mL of tetraethyl orthosilicate, 50 mL of anhydrous ethanol and 2 mL of deionized water were added to a three-necked flask and stirred at 600 rpm at 15°C to mix the raw materials evenly; 9 mL of premixed ammonia water (28 wt%) and 25 mL of ethanol solution were added to the system at one time. The volume fraction of concentrated ammonia water in the reaction solution was about 10%. The stirring speed was increased to 800 rpm and stirred for 30 min to initiate hydrolysis; then the stirring speed was reduced to 200 rpm and the reaction was kept at 25°C for 4 h; after the reaction was completed, the microspheres were centrifuged and washed 3 times at 4°C and 9000 rpm to obtain monodisperse silica microspheres with a particle size of about 360 nm, which were then redispersed in anhydrous ethanol for later use.
[0068] 2) Photonic crystal template assembly: Prepare a 4 wt% silica-ethanol suspension, sonicate for 1 min and vortex for 1 min to ensure uniform dispersion; use an automatic coating machine to coat the silica-ethanol onto a hydrophilic glass slide at a coating speed of 5 mm / s. -1 The volume of liquid for each coating was 50 μL, and the coating was applied 13 times on the same glass slide. After coating, the slide was allowed to dry horizontally at room temperature to obtain a blue silica gel crystal template.
[0069] 3) Synthesis of polymethyl methacrylate (PMMA) monolayer: MMA monomer was washed with 5 wt% sodium hydroxide aqueous solution, then with deionized water until neutral, dried over anhydrous magnesium sulfate, and purified by vacuum distillation. 40 g of the purified PMMA monomer was weighed and 0.08 g of benzoyl peroxide (0.2 wt% of monomer mass) was added as initiator. The mixture was stirred until completely dissolved and transferred to a three-necked flask. High-purity nitrogen was purged for 10 min to remove oxygen. The flask was then sealed and placed in an 80℃ constant-temperature water bath for prepolymerization at 300 rpm. After approximately 45 min of reaction, when the viscosity of the system reached a glycerol-like state, the reaction solution was transferred to a polytetrafluoroethylene (PTFE) template. Heating was continued at 60℃ for 24 h until the surface was dry and cured. The temperature was then raised to 100℃ and maintained at this high temperature for 4 h, followed by gradual cooling to room temperature to ensure complete polymerization of all remaining monomers, yielding a PMMA monolayer.
[0070] 4) Synthesis of chiral copper (I) clusters: Weigh 15 mg (0.04 mmol) copper hexafluorophosphate tetraacetonitrile, 25 mg (0.04 mmol) S-binaphthyl diphenylphosphine, and 4 mg (0.04 mmol) 4-ethynylpyridine and add them to a reaction beaker; add 2 mL of a mixed solvent of dichloromethane and 2 mL of anhydrous methanol, and stir at room temperature in the dark for 5 min until the solid is completely dissolved to obtain a clear yellow solution; add 1 drop of triethylamine to the solution and continue stirring in the dark for 10 min; filter the reaction solution with filter paper, collect the filtrate in a light-protected sample bottle, seal and let it stand at room temperature for 12 h to evaporate; after the solvent slowly evaporates, yellow rod-shaped crystals precipitate, wash 3 times with cold methanol, and dry under vacuum to obtain the S-configuration chiral copper (I) cluster (denoted as S-Cu), and store it in the dark and cold.
[0071] 5) Preparation of composite membrane by blending and casting: Weigh 200 mg of polymethyl methacrylate obtained in step 3), dissolve it in 2 mL of dichloromethane, and stir until completely dissolved; weigh 2 mg of S-configuration chiral copper (I) cluster (S-Cu) obtained in step 4), dissolve it in 1 mL of dimethyl sulfoxide (DMSO) to prepare a 2 mg / mL S-Cu / DMSO stock solution; add 100 μL of the above stock solution (containing 0.2 mg S-Cu) to the polymethyl methacrylate solution, corresponding to a copper cluster loading of 0.1 wt% (relative to the mass of polymethyl methacrylate); stir at room temperature in the dark for 5 min to obtain a uniform and transparent yellow blend solution. The blended solution was slowly poured onto the blue silica gel crystal template obtained in step 2), and left to stand at room temperature in the dark for 2 h. After most of the solvent evaporated, it was transferred to a constant temperature hot plate at 35℃ and dried for another 1 h. After cooling to room temperature, it was demolded to obtain a composite opal film loaded with 0.1 wt% S-configuration chiral copper (I) clusters.
[0072] 6) Etching to obtain an inverse opal film: Immerse the composite opal film in a 5% hydrofluoric acid aqueous solution and gently agitate for 5 minutes every 3 hours. Repeat this process 3 times to ensure complete etching of the silica template. After removal, wash the film repeatedly with deionized water and anhydrous ethanol to remove residual hydrofluoric acid. After drying, a blue inverse opal photonic crystal film is obtained.
[0073] Example 9: Blue inverse opal photonic crystal thin film loaded with S-configuration chiral copper (I) clusters
[0074] In this embodiment, the silica gel crystalline template microspheres have a particle size of approximately 360 nm, the inverse opal photonic crystal film exhibits a blue structural color, the chiral copper (I) cluster has an S configuration, and the loading amount is 0.5 wt%.
[0075] 1) Preparation of monodisperse silica microspheres: 3 mL of tetraethyl orthosilicate, 50 mL of anhydrous ethanol and 2 mL of deionized water were added to a three-necked flask and stirred at 600 rpm at 25 °C to mix the raw materials evenly; 9 mL of premixed ammonia water (28 wt%) and 25 mL of ethanol solution were added to the system at one time. The volume fraction of concentrated ammonia water in the reaction solution was about 10%. The stirring speed was increased to 1200 rpm and stirred for 10 min to initiate hydrolysis; then the speed was reduced to 400 rpm and the reaction was kept at 15 °C for 8 h; after the reaction was completed, the microspheres were centrifuged and washed 3 times at 4 °C and 9000 rpm to obtain monodisperse silica microspheres with a particle size of about 360 nm, which were then redispersed in anhydrous ethanol for later use.
[0076] 2) Photonic crystal template assembly: Prepare a 6 wt% silica-ethanol suspension, sonicate for 1 min and vortex for 1 min to ensure uniform dispersion; use an automatic coating machine to coat the silica-ethanol onto a hydrophilic glass slide at a coating speed of 15 mm / s. -1 The volume of liquid for each coating was 50 μL, and the coating was applied 10 times on the same glass slide. After coating, the slide was allowed to dry horizontally at room temperature to obtain a blue silica gel crystal template.
[0077] 3) Synthesis of polymethyl methacrylate (PMMA) monolayer: MMA monomer was washed with 5 wt% sodium hydroxide aqueous solution, then with deionized water until neutral, dried over anhydrous magnesium sulfate, and purified by vacuum distillation. 40 g of the purified PMMA monomer was weighed and 0.08 g of benzoyl peroxide (0.2 wt% of monomer mass) was added as initiator. The mixture was stirred until completely dissolved and transferred to a three-necked flask. High-purity nitrogen was purged for 10 min to remove oxygen. The flask was then sealed and placed in an 80℃ constant-temperature water bath for prepolymerization at 300 rpm. After approximately 45 min of reaction, when the viscosity of the system reached a glycerol-like state, the reaction solution was transferred to a polytetrafluoroethylene (PTFE) template. Heating was continued at 60℃ for 24 h until the surface was dry and cured. The temperature was then raised to 100℃ and maintained at this high temperature for 4 h, followed by gradual cooling to room temperature to ensure complete polymerization of all remaining monomers, yielding a PMMA monolayer.
[0078] 4) Synthesis of chiral copper (I) clusters: Weigh 15 mg (0.04 mmol) copper hexafluorophosphate tetraacetonitrile, 25 mg (0.04 mmol) S-binaphthyl diphenylphosphine, and 4 mg (0.04 mmol) 4-ethynylpyridine and add them to a reaction beaker; add 2 mL of a mixed solvent of dichloromethane and 2 mL of anhydrous methanol, and stir at room temperature in the dark for 5 min until the solid is completely dissolved to obtain a clear yellow solution; add 1 drop of triethylamine to the solution and continue stirring in the dark for 10 min; filter the reaction solution with filter paper, collect the filtrate in a light-protected sample bottle, seal and let it stand at room temperature for 12 h to evaporate; after the solvent slowly evaporates, yellow rod-shaped crystals precipitate, wash 3 times with cold methanol, and dry under vacuum to obtain the S-configuration chiral copper (I) cluster (denoted as S-Cu), and store it in the dark and cold.
[0079] 5) Preparation of composite membrane by blending and casting: Weigh 200 mg of polymethyl methacrylate obtained in step 3), dissolve it in 2 mL of dichloromethane, and stir until completely dissolved; weigh 2 mg of S-configuration chiral copper (I) cluster (S-Cu) obtained in step 4), dissolve it in 1 mL of dimethyl sulfoxide (DMSO) to prepare a 2 mg / mL S-Cu / DMSO stock solution; add 500 μL of the above stock solution (containing 1.0 mg S-Cu) to the polymethyl methacrylate solution, corresponding to a copper cluster loading of 0.5 wt% (relative to the mass of polymethyl methacrylate); stir at room temperature in the dark for 5 min to obtain a uniform and transparent yellow blend solution. The blended solution was slowly poured onto the blue silica gel crystal template obtained in step 2), and left to stand at room temperature in the dark for 2 h. After most of the solvent evaporated, it was transferred to a 45°C constant temperature hot plate to continue drying for 1 h. After cooling to room temperature, it was demolded to obtain a composite opal film loaded with 0.5 wt% S-configuration chiral copper (I) clusters.
[0080] 6) Etching to obtain an inverse opal film: Immerse the composite opal film in a 15% hydrofluoric acid aqueous solution and gently agitate for 3 minutes every 2 hours. Repeat this process 6 times to ensure complete etching of the silica template. After removal, wash the film repeatedly with deionized water and anhydrous ethanol to remove residual hydrofluoric acid. After drying, a blue inverse opal photonic crystal film is obtained.
[0081] Examples 10-12 Blue inverse opal photonic crystal thin films of chiral copper (I) clusters with different loading amounts and S-configurations
[0082] The preparation methods of this series of examples are the same as those of Example 1, except that the amount of chiral copper (I) clusters fed is adjusted so that the loading amounts are 1 wt% (Example 10), 2 wt% (Example 11), and 3 wt% (Example 12) to obtain samples with different loading amounts.
[0083] Meanwhile, R-binaphthylphosphine in step 4) is replaced with S-binaphthylphosphine, while the other steps remain unchanged, to obtain blue inverse opal photonic crystal films of S-configuration chiral copper (I) clusters with different loading amounts. Their circularly polarized emission signals are mirror-symmetric to those of the R-configuration samples.
[0084] Comparative Examples 1-3: Polymethyl methacrylate inverse opal films without chiral copper (I) clusters
[0085] Comparative Examples 1-3 were performed according to steps 1) to 3), 5), and 6) of Examples 1-3, except that step 4) preparation of chiral copper (I) clusters was omitted. Therefore, the blend solution in step 5) did not contain chiral copper (I) clusters, resulting in polymethyl methacrylate inverse opal films (denoted as IOPMMA) without chiral copper (I) clusters. Using silica microspheres with a particle size of approximately 360 nm from Example 1, approximately 484 nm from Example 2, and approximately 622 nm from Example 3 as templates, blue (Comparative Example 1), green (Comparative Example 2), and red (Comparative Example 3) polymethyl methacrylate inverse opal films were finally obtained, respectively.
[0086] Comparative Example 4: Polyurethane-based blue inverse opal photonic crystal thin film
[0087] Commercially available thermoplastic polyurethane (molecular weight 80,000) was used to replace polymethyl methacrylate, and a polyurethane casting solution with a mass fraction of 12 wt% was prepared. Polyurethane inverse opal films were prepared according to the same template casting and etching process as in Example 1.
[0088] Experimental Example 1: Characterization of Thermal Properties and Structural Stability
[0089] Test samples: polymethyl methacrylate monolayer (prepared from step 3 of Example 1, before and after hydrofluoric acid etching), composite opal films prepared in Examples 1-3 (before etching, i.e., composite opal films containing silica gel crystal templates prepared in steps 1 to 5), and the finally prepared inverse opal photonic crystal film (after etching).
[0090] Test methods: The glass transition temperature was tested using a differential scanning calorimeter (Q 25) at a heating rate of 10 ℃ / min, and the test atmosphere was nitrogen; the thermogravimetric analysis (TA 55) was used to test the thermogravimetric behavior, with a heating range from room temperature to 600℃, and the test atmosphere was nitrogen.
[0091] Results and Analysis:
[0092] (1) Figure 1 Differential scanning calorimetry (DSC) curves of the polymethyl methacrylate film and the blue, green, and red inverse opal photonic crystal films obtained in Examples 1-3, respectively, before and after etching. Figure 1 (a) DSC images of the pure polymethyl methacrylate film prepared in step 3 of Example 1 before and after etching. Figure 1As shown in (a), the glass transition temperature of the pure polymethyl methacrylate film prepared in step 3 of Example 1 before etching is approximately 69.5°C, and the glass transition temperature after etching is approximately 69.6°C, which are essentially the same. This result demonstrates that hydrofluoric acid etching does not significantly alter the molecular chain structure and aggregation state of polymethyl methacrylate, and the etching process exhibits good selectivity for the polymer matrix.
[0093] at the same time, Figure 1 (b) is a DSC comparison image of the composite opal film before etching prepared by steps 1 to 5 of Example 1 and the finally prepared inverse opal crystal film. Figure 1 (c) is a DSC comparison image of the composite opal film before etching prepared by steps 1 to 5 of Example 2 and the finally prepared inverse opal crystal film. Figure 1 (d) is a DSC comparison image of the composite opal film before etching prepared by steps 1 to 5 of Example 3 and the finally prepared inverse opal crystal film. Figure 1 (b)- Figure 1 (d) It can be seen that the glass transition temperature of the inverse opal film is higher than that of room temperature, indicating that the polymethyl methacrylate skeleton is in the glassy state at room temperature. The movement of polymer chain segments is significantly restricted, which can effectively suppress chain rearrangement and pore wall shrinkage during long-term storage, and provide rigid support for the long-term stability of the three-dimensional ordered porous structure.
[0094] (2) For example Figure 2 As shown, the residual mass of the pure polymethyl methacrylate film prepared in step 3 of Example 1 after calcination at 600 °C is approximately 2.435–2.510 wt%, which is at a low level; and the difference in residual weight before and after etching is only 0.075 wt%, with no significant difference. This result further verifies that hydrofluoric acid etching does not cause significant chemical corrosion or thermal decomposition of the polymethyl methacrylate matrix, and the thermal stability of the matrix material remains consistent before and after etching.
[0095] (3) Figure 3 The thermogravimetric analysis (TG) curves of the blue, green, and red inverse opal photonic crystal thin films obtained in Examples 1-3 before and after etching are shown. Figure 3 (a) is a TG comparison diagram of the composite opal film before etching prepared in steps 1 to 5 of Example 1 and the finally prepared inverse opal crystal film. Figure 3 (b) is a TG comparison diagram of the composite opal film before etching prepared in steps 1 to 5 of Example 2 and the finally prepared inverse opal crystal film. Figure 3 (c) is a TG comparison diagram of the composite opal film before etching prepared in steps 1 to 5 of Example 3 and the finally prepared inverse opal crystal film. Figure 3 (a) Figure 3(b) Figure 3 As shown in (c), the composite opal films prepared in steps 1 to 5 of Examples 1-3 before etching have relatively high residual mass after calcination at 600℃ due to the presence of silica bulk crystal templates, which are 3.890 wt% (blue), 2.682 wt% (green), and 3.106 wt% (red), respectively. After etching with hydrofluoric acid to finally obtain the inverse opal crystal film, the residual mass is significantly reduced to 2.811 wt% (blue), 1.837 wt% (green), and 2.313 wt% (red), respectively. The difference in residual weight before and after etching is the silica loading, which is 1.079 wt% (blue), 0.845 wt% (green), and 0.793 wt% (red), respectively, indicating that the silica template has been mostly removed, leaving only a very small amount of inorganic components, which does not affect the porous structure and optical properties of the inverse opal.
[0096] Depend on Figure 3 It can be seen that the residual mass of the blue small-pore sample finally prepared in Example 1 is slightly higher (2.811 wt%) than that of the green sample finally prepared in Example 2 (1.837 wt%) and the red large-pore sample finally prepared in Example 3 (2.313 wt%). The silica loading decreases with the increase of template particle size (1.079 → 0.845 → 0.793 wt%), which is related to the higher specific surface area of small-diameter silica microspheres and the relatively higher proportion of silica component in the system, which is consistent with the control law of template particle size.
[0097] Experimental Example 2: Characterization of Microscopic Morphology and Structural Order
[0098] Test samples: silica gel crystal template (blue silica gel crystal template prepared by steps 1 and 2 of Example 1), blue inverse opal photonic crystal film finally prepared in Example 1, polyurethane-based inverse opal film prepared in Comparative Example 4, and film obtained by heat-treating the film prepared in Example 1 at 40°C, 60°C, 80°C, and 100°C for 1 h respectively.
[0099] Test methods: Surface and cross-sectional morphology were characterized using field emission scanning electron microscopy (FEI Quattro S) with an accelerating voltage of 5-10 kV. The samples were sputtered with gold before testing. The long-range order of the structure was analyzed using two-dimensional fast Fourier transform.
[0100] Results and Analysis:
[0101] (1) Morphology of colloidal crystal template: Figure 4 Microscopic morphology images of silica gel crystalline templates obtained by field emission scanning electron microscopy, along with images showing further processing. (See attached images.) Figure 4As shown in (a), in the silica gel crystal template prepared by steps 1 and 2 of Example 1, the silica microspheres exhibit a hexagonal close-packed structure, good monodispersity, and uniform particle size; Figure 4 As shown in (b), the spatial frequency distribution map after the micromorphology map is processed by two-dimensional Fourier fast transform presents regular concentric diffraction rings, indicating that the structure has long-range periodicity.
[0102] (2) Surface morphology of inverse opal: Figure 5 Microscopic morphology images and further processing images of the inverse opal photonic crystal thin film prepared in Example 1, obtained by field emission scanning electron microscopy. Figure 5 As shown in (a), after template impregnation and etching, the polymethyl methacrylate inverse opal film prepared in Example 1 forms a regularly arranged porous structure on its surface. The pores are circular, with clear boundaries and uniform diameter. Figure 5 As shown in (b), the spatial frequency distribution map after the micromorphology image is processed by two-dimensional Fourier fast transform presents discrete hexagonal symmetric diffraction spots, corresponding to the long-range order of the inverse opal structure.
[0103] (3) Cross-sectional morphology: such as Figure 6 As shown, the porous structure of the polymethyl methacrylate inverse opal film prepared in Example 1 is continuously distributed along the thickness direction of the film, with orderly interlayer stacking, no obvious discontinuities or large areas of disorder, and the pore structure runs through the entire thickness of the film.
[0104] (4) Appearance after long-term storage: such as Figure 7 As shown, after being stored at room temperature in the dark for 10 months, the polymethyl methacrylate inverse opal film prepared in Example 1 still maintained a regularly arranged porous structure on its surface. In contrast, as... Figure 8 As shown, under the same storage conditions, the polyurethane-based inverse opal film underwent significant structural degradation in less than a month, with blurred pore edges, irregular pore shapes, and some pores completely collapsing.
[0105] (5) Morphological changes after heat treatment: such as Figure 9 As shown, after the polymethyl methacrylate inverse opal film prepared in Example 1 was heat-treated at 40℃, 60℃, 80℃ and 100℃ for 1 h, the porous structure of polymethyl methacrylate inverse opal could still be maintained. As the temperature increased, the pore edges showed slight passivation and the pore size slightly shrank, but no large-area collapse occurred, indicating that the system has a certain thermal structural stability within 100℃.
[0106] Experimental Example 3: Solvent-responsive optical properties and cycling stability test
[0107] Test samples: Blue, green, and red inverse opal photonic crystal films obtained in Examples 1-3.
[0108] Test method: The reflectance spectrum of the sample was tested in reflectance mode using a fiber optic spectrometer (AvaSpec-ULS2048CL-EVO) with a wavelength range of 400~800 nm. The reflectance spectra of the original sample and the sample after treatment with saturated NaCl, MgCl2, NaBr solution and glycerol were tested respectively. The sample was subjected to 50 cycles of ethanol wetting-drying and 50 cycles of deionized water wetting-drying, and the wavelength of the reflectance peak after each drying cycle was recorded.
[0109] Results and Analysis:
[0110] (1) Optical response in different media: such as Figure 10 As shown, the sample prepared in Example 1 has a single Bragg reflection peak in the visible light region; after treatment with saturated salt solution and glycerol, the position and shape of the reflection peak are not significantly shifted compared with the original sample, and the peak intensity fluctuates slightly, indicating that the neutral salt and glycerol environment will not destroy the ordered structure of the inverse opal.
[0111] (2) Ethanol cycling response characteristics: such as Figure 11 As shown, the blue, green, and red samples prepared in Examples 1-3, when wetted with ethanol, all exhibited reflection peaks shifted below the visible light band, and their structural color disappeared. After drying, the reflection peaks returned to their initial wavelength positions. After 50 wet-dry cycles, the reflection peak wavelengths of the three samples showed no significant shift, with fluctuations less than 5 nm, indicating that the ethanol response has good reversibility.
[0112] (3) Water cycle response characteristics: such as Figure 12 As shown, after wetting with deionized water, the reflection peaks of all three samples prepared in Examples 1-3 exhibited a red shift, with the red sample showing the largest red shift. After drying, the reflection peaks returned to their initial wavelengths. After 50 cycles, the wavelength stability of the reflection peaks was comparable to that of ethanol cycling, and no irreversible structural collapse occurred.
[0113] Experimental Example 4: Photoactivated Emission and Chiral Optical Properties Test
[0114] Test samples: Blue, green, and red inverse opal photonic crystal films prepared in Examples 1-3 with 1 wt% chiral copper (I) cluster loading, and blue inverse opal photonic crystal films prepared in Examples 4-7 with different chiral copper (I) cluster loadings (0.1 wt%, 0.5 wt%, 2 wt%, 3 wt%); and blue inverse opal photonic crystal films prepared in Examples 8-12 with different chiral copper (I) cluster loadings (0.1 wt%, 0.5 wt%, 1 wt%, 2 wt%, 3 wt%).
[0115] Test methods: Steady-state fluorescence emission spectra and photoactivation kinetic curves were measured using a fluorescence spectrometer (FLS-980, Edinburgh Instruments) with an excitation wavelength of 365 nm; the fluorescence spectra of samples with different loading amounts were integrated to obtain the integrated luminescence intensity; the circularly polarized emission and circular dichroism signals of the samples were measured using a circularly polarized emission spectrometer, and the luminescence asymmetry factor |glum| was calculated.
[0116] Results and Analysis:
[0117] (1) Correlation between loading amount and fluorescence intensity: Figure 13 The images show the fluorescence intensity of inverse opal photonic crystal films with different chiral copper (I) cluster loadings in Examples 1 and 4-12. Figure 13 (a) Thin films doped with R-configuration chiral copper (I) clusters with different chiral copper (I) cluster loadings (0.1 wt%, 0.5 wt%, 1 wt%, 2 wt%, 3 wt%) prepared in Examples 1 and 4-7. Figure 13 (b) Thin films doped with S-configuration chiral copper (I) clusters at different chiral copper (I) cluster loadings (0.1 wt%, 0.5 wt%, 1 wt%, 2 wt%, 3 wt%) prepared in Examples 8-12. Figure 13 As shown, the R-configuration and S-configuration chiral copper (I) cluster-doped films prepared in this invention both have fluorescence emission peaks around 440 nm, with no significant difference in peak shape. When the loading of chiral copper (I) clusters increases from 0.1 wt% to 1 wt%, the integrated fluorescence intensity of the samples gradually increases, reaching a peak at 1 wt%. When the loading continues to increase to 2 wt% and 3 wt%, the integrated fluorescence intensity shows a decreasing trend. It is speculated that this is because, at low loading, the number of luminescent units increases with increasing loading, while at high loading, molecular aggregation leads to enhanced non-radiative quenching.
[0118] (2) The influence of photonic structure on photoactivation dynamics: such as Figure 14 As shown, the red, green, and blue inverse opal films with different structural colors prepared in Examples 1-3, after being irradiated with 365 nm ultraviolet light, all exhibited a rapid increase in luminescence intensity followed by a plateau after prolonged irradiation time. The photoactivation response rates differed among the three samples, with the red sample reaching steady state in the shortest time, followed by the green sample, and the blue sample taking the longest. This difference can be attributed to the localized modulation of emitted light by different photonic bandgap structures; the varying degrees of matching between the reflection band and the emission spectrum can regulate the local light field distribution and light extraction efficiency.
[0119] (3) Circularly polarized light emission properties: such as Figure 15As shown, the R-configuration chiral copper (I) cluster-doped inverse opal film prepared in Example 1 and the S-configuration chiral copper (I) cluster-doped inverse opal film prepared in Example 10 both exhibit mirror-symmetric distributions in their circularly polarized emission signals, indicating that chiral characteristics are preserved in the composite system. The signal peak positions of both the S-configuration chiral copper (I) cluster-doped inverse opal structure and the R-configuration chiral copper (I) cluster-doped inverse opal structure correspond to the fluorescence emission peak positions. The highest calculated value of the circularly polarized emission asymmetry factor |glum| for the R-configuration chiral copper (I) cluster-doped inverse opal film prepared in Example 1 is 2.4 × 10⁻⁶. -2 No circularly polarized emission signal or circular dichroism signal was detected in the blank inverse opal films of Comparative Examples 1-3, further proving that the chiral optical response of the system is entirely derived from the introduced chiral copper (I) cluster; the inverse opal photonic structure mainly plays a role in regulating the luminescence efficiency, rather than being the source of the chiral signal.
[0120] (4) Circular dichroism properties: such as Figure 16 As shown, the inverse opal doped with S-configuration chiral copper (I) clusters prepared in Example 10 and the inverse opal doped with R-configuration chiral copper (I) clusters prepared in Example 1 both exhibit mirror-symmetric circular dichroism signals, confirming the ground-state chiral characteristics of the materials.
[0121] It should be noted that although the above embodiments have been described herein, this does not limit the scope of patent protection of the present invention. Therefore, any changes and modifications made to the embodiments described herein based on the innovative concept of the present invention, or equivalent structural or procedural transformations made using the content of the present invention's specification and drawings, directly or indirectly applying the above technical solutions to other related technical fields, are all included within the scope of patent protection of the present invention.
Claims
1. A long-lasting and stable inverse opal photonic crystal thin film, characterized in that, It includes a rigid polymethyl methacrylate three-dimensional ordered porous inverse opal framework and chiral copper (I) cluster light-emitting units loaded in the pores of the rigid polymethyl methacrylate three-dimensional ordered porous inverse opal framework; the inverse opal photonic crystal film simultaneously possesses intrinsic structural color, reversible solvent-responsive optical properties and photoactivated circularly polarized light-emitting properties.
2. The long-lasting and stable inverse opal photonic crystal thin film according to claim 1, characterized in that, The pore size of the inverse opal framework is 200~700 nm, and the loading of the chiral copper (I) cluster is 0.1~3 wt%, with the loading based on the mass of the rigid polymethyl methacrylate three-dimensional ordered porous inverse opal framework.
3. The long-lasting and stable inverse opal photonic crystal thin film according to claim 1, characterized in that, The chiral copper (I) cluster is an R-configuration or S-configuration chiral copper (I) complex, prepared by a coordination reaction of copper hexafluorophosphate tetraacetonitrile and 4-ethynylpyridine with one of R-binaphthyldiphenylphosphine or S-binaphthyldiphenylphosphine.
4. The long-lasting and stable inverse opal photonic crystal thin film according to claim 1, characterized in that, The inverse opal photonic crystal film retains its regularly arranged porous structure on its surface even after being stored at room temperature in the dark for 10 months.
5. A method for preparing a long-lasting and stable inverse opal photonic crystal thin film as described in any one of claims 1 to 4, characterized in that, It includes the following steps: Step 1: Monodisperse silica microspheres were prepared using the modified Stobel method, with tetraethyl orthosilicate as the silicon source, anhydrous ethanol and deionized water as solvents, and ammonia as the catalyst. The particle size of the microspheres was controlled by adjusting the concentration of ammonia. After the reaction, the microspheres were obtained by centrifugation and ethanol washing. Step 2: The monodisperse silica microspheres are dispersed in anhydrous ethanol to prepare a colloidal suspension, and silica crystalline templates are prepared on a hydrophilic substrate by coating-evaporation induced self-assembly method; Step 3: Cast a polymethyl methacrylate solution containing chiral copper (I) clusters onto the silica gel crystal template, and obtain a composite opal film after the solvent evaporates; Step 4: The silica gel crystal template is removed by etching with hydrofluoric acid solution, and the inverse opal photonic crystal film is obtained after washing and drying.
6. The preparation method according to claim 5, characterized in that, Step 1 specifically includes: Material mixing: First, mix tetraethyl orthosilicate, deionized water, and the first part of anhydrous ethanol, stir to dissolve, then add a mixture of ammonia and the second part of anhydrous ethanol, stir evenly to obtain a reaction solution, wherein the volume fraction of ammonia in the reaction solution is 9-22%; Hydrolysis stage: The reaction solution is hydrolyzed for 10-30 minutes at 15-25℃ and 800-1200 rpm to generate silanol from tetraethyl orthosilicate. Growth stage: Reduce the stirring speed to 200-400 rpm, maintain 15-25℃ and continue the reaction for 4-8 hours; Post-processing: After the reaction was completed, the solid was separated by centrifugation and washed 2-4 times with anhydrous ethanol to obtain monodisperse silica microspheres.
7. The preparation method according to claim 5, characterized in that, In step 3, the polymethyl methacrylate solution containing chiral copper (I) clusters is obtained by mixing a dichloromethane solution of a polymethyl methacrylate monolayer with a dimethyl sulfoxide solution of chiral copper (I) clusters. After casting, it is first left to stand at room temperature in the dark, and then dried at a constant temperature of 35-45℃.
8. The preparation method according to claim 7, characterized in that, The chiral copper (I) cluster is prepared by dissolving copper hexafluorophosphate tetraacetonitrile and 4-ethynylpyridine, and one of R-binaphthyldiphenylphosphine or S-binaphthyldiphenylphosphine, in a mixed solvent of dichloromethane and methanol at a molar ratio of 1:1:
1. After stirring at room temperature until the solid is completely dissolved, triethylamine is added to catalyze the reaction. After filtration, the filtrate is allowed to stand at room temperature in the dark to evaporate, thus obtaining chiral copper (I) cluster crystals.
9. The preparation method according to claim 5, characterized in that, Step 2 includes: dispersing the monodisperse silica microspheres in anhydrous ethanol to prepare a colloidal suspension with a mass fraction of 2%-6%, ultrasonically dispersing the suspension, and then adding 40-60 μL of the suspension to one end of a hydrophilic glass slide. The suspension is then coated using an automatic coating machine at a speed of 5-15 mm / s. -1 Apply the coating using a scraping method at a specific speed. In step 4, the mass fraction of the hydrofluoric acid solution is 5%~15%, the total etching time is 8~16 h, and the etching is oscillated for 3~5 min every 1~3 h.
10. The application of a long-lasting and stable inverse opal photonic crystal thin film according to any one of claims 1 to 4, characterized in that, The inverse opal photonic crystal thin film is used to prepare optical anti-counterfeiting labels, multi-level information encryption devices, or dynamic optical display devices.