Composite anti-reflection film structure for silica light transmission window and method of making

By setting a three-layer composite antireflective film structure on the surface of the silica light-transmitting window, the problem of stress release caused by single material and multi-layer stacking in the prior art is solved, achieving broadband high-efficiency antireflection and mechanical stability, and improving optical performance and imaging quality.

CN123156339APending Publication Date: 2026-11-24SHENGLAN SEMICON (CHANGZHOU) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611258249.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-19
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

The existing antireflective film structure material system for silica light-transmitting windows is too simple to meet the high-efficiency antireflection requirements of the 400-700nm wide wavelength band. Moreover, the multi-layer stacking makes it difficult to release the interface stress, which can easily cause film warping and cracking, resulting in high cost and affecting imaging quality.

Method used

A three-layer composite antireflective film structure is set on the surface of a silicon dioxide light-transmitting window, including a silicon nitride substrate layer, a silicon-based transition layer, and a silicon-based top layer. By adjusting the refractive index and stress characteristics of each layer, a step-type quasi-gradient distribution is formed, and compressive stress is used to offset tensile stress, thus simplifying the film structure.

Benefits of technology

It achieves broadband and efficient anti-reflection, reduces the overall residual stress of the composite film layer, improves the environmental reliability and mass production yield of the optical window, enhances optical transmittance and mechanical stability, and avoids warping and cracking problems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123156339A_ABST
    Figure CN123156339A_ABST
Patent Text Reader

Abstract

The application provides a composite anti-reflection film structure for a silica light-transmitting window and a preparation method thereof, and belongs to the field of film layer preparation. The surface of the silica light-transmitting window is sequentially provided with a silicon nitride base layer, a silicon base transition layer and a silicon base top layer. The silicon nitride base layer is covered on the surface of the silica light-transmitting window, has a first refractive index, and forms a tensile stress in the layer. The first refractive index is greater than the refractive index of the silica light-transmitting window. The silicon base transition layer is covered on the surface of the silicon nitride base layer, has a second refractive index, and forms a compressive stress in the layer. The second refractive index is less than or equal to the refractive index of the silica light-transmitting window. The silicon base top layer is covered on the surface of the silicon base transition layer, has a third refractive index, and forms a compressive stress in the layer. The third refractive index is less than the first refractive index and greater than the second refractive index. The sum of the compressive stresses of the silicon base top layer and the silicon base transition layer can offset the tensile stress of the silicon nitride base layer. The application is specially used for the silica light-transmitting window and has excellent optical performance and high reliability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of thin films, and more particularly to a composite antireflective film structure and preparation method for a silicon dioxide light-transmitting window. Background Technology

[0002] In modern high-end camera lenses, optical sensing modules, and micro / nano optical devices, silicon dioxide (SiO2) is widely used as a light-transmitting window material due to its excellent optical transmittance and chemical stability. To reduce interface reflection, improve light transmittance, and eliminate glare, an anti-reflective coating is usually prepared on the surface of the silicon dioxide light-transmitting window.

[0003] Currently, most antireflective coatings for silica light-transmitting windows employ a single-layer structure with a limited material system, making it difficult to meet the high-efficiency antireflection requirements across a wide wavelength range of 400-700nm, resulting in significant bandwidth limitations. To address this issue, the industry often draws inspiration from composite antireflective coating technologies applied to glass or silicon substrates. While these technologies can achieve broadband antireflection through multi-layer stacking, direct application to silica light-transmitting windows presents significant drawbacks: First, the complex film structure and multi-layer stacking make it difficult to release interfacial stress, easily leading to film warping and cracking, and the complex and costly process. Second, the presence of numerous high-to-low refractive index abrupt transitions between film layers increases light scattering loss, affecting image quality.

[0004] Therefore, there is an urgent need to develop a composite antireflective film structure that is specifically designed for silica light-transmitting windows and possesses both excellent optical performance and high reliability. Summary of the Invention

[0005] The technical problem to be solved by the present invention is to provide a composite antireflective film structure and preparation method for silicon dioxide light-transmitting windows, which is specifically designed for silicon dioxide light-transmitting windows and has both excellent optical performance and high reliability.

[0006] To address the aforementioned problems, this invention provides a composite antireflective film structure for a silicon dioxide light-transmitting window. The structure comprises, sequentially, the following layers on the surface of the silicon dioxide light-transmitting window: a silicon nitride substrate layer covering the surface of the silicon dioxide light-transmitting window, the silicon nitride substrate layer having a first refractive index and tensile stress within the layer, the first refractive index being greater than the refractive index of the silicon dioxide light-transmitting window; a silicon-based transition layer covering the surface of the silicon nitride substrate layer, the silicon-based transition layer having a second refractive index and compressive stress within the layer, the second refractive index being less than or equal to the refractive index of the silicon dioxide light-transmitting window; and a silicon-based top layer covering the surface of the silicon-based transition layer, the silicon-based top layer having a third refractive index and compressive stress within the layer, the third refractive index being less than the first refractive index and greater than the second refractive index. The sum of the compressive stresses of the silicon-based top layer and the silicon-based transition layer can offset the tensile stress of the silicon nitride substrate layer.

[0007] In one embodiment, the silicon nitride substrate is a silicon-rich silicon nitride layer with a thickness of 110-132 nm and a first refractive index of 2.12-2.30.

[0008] In one embodiment, the silicon nitride substrate layer is selected from one of a titanium silicon nitride layer, a niobium silicon composite nitride layer, and a zirconium-doped silicon nitride layer.

[0009] In one embodiment, the silicon-based transition layer is a fluorine-doped silicon oxide layer with a thickness of 36–50 nm and a second refractive index of 1.38–1.45.

[0010] In one embodiment, the silicon-based transition layer is selected from one of a carbon-doped silicon oxide layer, a carbon oxy silicon layer, and a fluorine oxy silicon layer.

[0011] In one embodiment, the silicon-based top layer is a fluorine-doped carbon-oxygen silicon layer with a thickness of 80–94 nm, and the third refractive index is 1.47–1.58.

[0012] In one embodiment, the silicon-based top layer is selected from one of a boron-aluminum co-doped carbon-oxygen silicon layer, a zirconium-doped fluorine-silicon layer, or a hard silicon-oxygen carbon layer containing methylsilane.

[0013] In one embodiment, the compressive stress of the silicon-based top layer is greater than the compressive stress of the silicon-based transition layer.

[0014] In one embodiment, the composite antireflective film structure further includes an anti-fingerprint layer disposed on the surface of the silicon-based top layer.

[0015] This invention also provides a method for preparing a composite antireflective film structure for a silicon dioxide light-transmitting window, comprising the following steps: depositing a silicon nitride substrate layer on the surface of the silicon dioxide light-transmitting window; by setting the proportions of each reactant, the silicon nitride substrate layer is made to have a first refractive index and tensile stress is formed within the layer, wherein the first refractive index is greater than the refractive index of the silicon dioxide light-transmitting window; depositing a silicon-based transition layer on the surface of the silicon nitride substrate layer; by setting the proportions of each reactant, the silicon-based transition layer is made to have a second refractive index and compressive stress is formed within the layer, wherein the second refractive index is less than or equal to the refractive index of the silicon dioxide light-transmitting window; depositing a silicon-based top layer on the surface of the silicon-based transition layer; by setting the proportions of each reactant, the silicon-based top layer is made to have a third refractive index and compressive stress is formed within the layer, wherein the third refractive index is less than the first refractive index and greater than the second refractive index, and the sum of the compressive stress of the silicon-based top layer and the silicon-based transition layer can offset the tensile stress of the silicon nitride substrate layer.

[0016] In one embodiment, the silicon nitride substrate is a silicon-rich silicon nitride layer with a thickness of 110~132nm and a first refractive index of 2.12–2.30. The step of depositing the silicon nitride substrate layer on the surface of the silicon dioxide light-transmitting window further includes: using a silicon source and NH3 as reactants, and employing a plasma-enhanced chemical vapor deposition process to form the silicon-rich silicon nitride layer on the surface of the silicon dioxide light-transmitting window. By setting the flow rate ratio of the silicon source to NH3, the silicon-rich silicon nitride layer is made to have a first refractive index, and tensile stress is formed within the layer.

[0017] In one embodiment, the silicon-based transition layer is a fluorine-doped silicon oxide layer with a thickness of 36–50 nm and a second refractive index of 1.38–1.45. The step of depositing the silicon-based transition layer on the surface of the silicon nitride substrate further includes: using a silicon source, N2O, and a fluorine source as reactants, and employing a plasma-enhanced chemical vapor deposition process to form in-situ fluorine doping on the surface of the silicon nitride substrate, thereby forming the fluorine-doped silicon oxide layer. By setting the flow rate ratio of the silicon source, N2O, and fluorine source, as well as the flow rate percentage of the fluorine source in the total reactants, the fluorine-doped silicon oxide layer is made to have a second refractive index, and compressive stress is formed within the layer.

[0018] In one embodiment, the silicon-based top layer is a fluorine-doped silicon-oxygen layer with a thickness of 80–94 nm and a third refractive index of 1.47–1.58. The step of depositing the silicon-based top layer on the surface of the silicon-based transition layer further includes: using a silicon source, CO2, and a fluorine source as reactants, and employing a plasma-enhanced chemical vapor deposition process to form in-situ fluorine doping on the surface of the silicon-based transition layer, thereby forming the fluorine-doped silicon-oxygen layer. By setting the flow rate ratio of the silicon source, CO2, and fluorine source, as well as the flow rate percentage of the fluorine source in the total reactants, the fluorine-doped silicon-oxygen layer is made to have a third refractive index, and compressive stress is formed within the layer.

[0019] In one embodiment, prior to the step of depositing a silicon nitride substrate layer on the surface of the silicon dioxide light-transmitting window, the preparation method further includes: performing vacuum pretreatment on the silicon dioxide light-transmitting window to remove organic impurities on the surface of the silicon dioxide light-transmitting window and improve the adhesion of the film layer.

[0020] In one embodiment, after the step of depositing a silicon-based top layer on the surface of the silicon-based transition layer, the fabrication method further includes forming an anti-fingerprint layer on the active surface of the silicon-based top layer.

[0021] The above-mentioned technical solution forms a composite antireflective film structure with three layers on the surface of the silica light-transmitting window. Compared with the traditional five-layer or higher composite antireflective film structure, the number of film layers is significantly reduced. The composite antireflective film structure provided by the present invention is arranged according to a step-type quasi-gradient of refractive index from low refractive index (i.e., the refractive index of the silica light-transmitting window) → maximum refractive index (i.e., the refractive index of the silicon nitride substrate layer) → minimum refractive index (i.e., the refractive index of the silicon-based transition layer) → intermediate refractive index (i.e., the refractive index of the silicon-based top layer). It achieves excellent interference destructive effect over a wide spectral range, effectively reduces Fresnel reflection and scattering loss at the multilayer interface, and realizes broadband and efficient antireflection. Meanwhile, the composite antireflective film structure provided in this invention introduces tensile stress into the silicon nitride substrate layer and compressive stress into the silicon-based transition layer and the silicon-based top layer, respectively. The synergistic effect of the two compressive stresses offsets the tensile stress in the silicon nitride substrate layer, minimizing the overall residual stress of the composite film layer (e.g., reducing it to a weak compressive level below 79 MPa). This fundamentally solves the warping, cracking, and peeling problems caused by the accumulation of interfacial stress in traditional multilayer films, significantly improving the environmental reliability and mass production yield of optical windows. The composite antireflective film structure possesses excellent temperature and humidity stability and mechanical compatibility, and can be widely applied in optical sensing modules, micro-imaging devices, micro / nano optical functional windows, and other scenarios.

[0022] It should be understood that the above general description and the following detailed description are exemplary and explanatory only, and are not intended to limit the invention. Techniques, methods, and apparatus known to those skilled in the art may not be discussed in detail, but where appropriate, such techniques, methods, and apparatus should be considered part of the specification. Attached Figure Description

[0023] To more clearly illustrate the technical solutions in the embodiments of the present invention, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0024] Figure 1 This is a schematic diagram of the composite antireflective film structure for a silicon dioxide light-transmitting window provided in an embodiment of the present invention; Figure 2 This is a schematic diagram of the steps in a method for preparing a composite antireflective film structure for a silicon dioxide light-transmitting window according to an embodiment of the present invention. Detailed Implementation

[0025] The technical solutions in the embodiments of the present invention will now be clearly and completely described with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of them. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0026] Figure 1 This is a schematic diagram of the composite antireflective film structure for a silicon dioxide light-transmitting window provided in an embodiment of the present invention, as shown below. Figure 1 As shown, a silicon nitride substrate layer 110, a silicon-based transition layer 120, and a silicon-based top layer 130 are sequentially disposed on the surface of the silicon dioxide light-transmitting window 100.

[0027] The silicon nitride substrate layer 110 covers the surface of the silicon dioxide light-transmitting window 100. The silicon nitride substrate layer 110 has a first refractive index and tensile stress is formed within the layer. The first refractive index is greater than the refractive index of the silicon dioxide light-transmitting window 100.

[0028] The silicon-based transition layer 120 covers the surface of the silicon nitride substrate layer 110. The silicon-based transition layer 120 has a second refractive index and compressive stress is formed within the layer. The second refractive index is less than or equal to the refractive index of the silicon dioxide light-transmitting window 100.

[0029] The silicon-based top layer 130 covers the surface of the silicon-based transition layer 120. The silicon-based top layer 130 has a third refractive index and compressive stress is formed within the layer. The third refractive index is less than the first refractive index and greater than the second refractive index. The sum of the compressive stress of the silicon-based top layer 130 and the silicon-based transition layer 120 can offset the tensile stress of the silicon nitride substrate layer 110.

[0030] Compared to existing technologies with numerous film layers, this invention uses only three layers to form a high-performance composite antireflective film structure. It has fewer interfaces, requires no additional transition substrate, and avoids cyclic stacking, resulting in stronger light transmission stability. The composite antireflective film structure follows the refractive index variation from the silica transmission window 100 to the air side in its optical design: the refractive index of the silica transmission window 100 (lowest) transitions sequentially to the refractive index of the silicon nitride substrate 110 (highest), the refractive index of the silicon-based transition layer 120 (lowest), and the refractive index of the silicon-based top layer 130 (middle), forming a step-type quasi-gradient distribution. This achieves excellent destructive interference effects over a wide spectral range, effectively reducing Fresnel reflection and scattering losses at multilayer interfaces, realizing broadband and efficient antireflection, and significantly improving the optical transmittance of the silica transmission window 100. In terms of mechanical stability, by limiting the intrinsic tensile stress of the silicon nitride substrate 110 (i.e., the tensile stress formed during the deposition process) and the intrinsic compressive stress of the silicon-based transition layer 120 and the silicon-based top layer 130 (i.e., the compressive stress formed during the deposition process), a stress complementary system is formed. The sum of the compressive stresses of the two layers can offset the tensile stress of the silicon nitride substrate 110 to the maximum extent, and control the overall residual stress of the composite antireflection film structure to within 79 MPa. This completely avoids the stress failure risk common in traditional thick films or complex multilayer films, and takes into account both excellent optical performance and mechanical stability.

[0031] In one embodiment, the silicon dioxide light-transmitting window 100 can be obtained by etching a silicon dioxide substrate. The refractive index of the silicon dioxide light-transmitting window 100 is approximately 1.46.

[0032] The silicon nitride substrate 110 directly covers the surface of the silicon dioxide light-transmitting window 100, serving as the optical and mechanical base layer of the composite antireflective film structure. The silicon nitride substrate 110 has a first refractive index, which is greater than the refractive index of the silicon dioxide light-transmitting window 100, and the silicon nitride substrate 110 has the largest refractive index in the composite antireflective film structure.

[0033] The tensile stress formed in the silicon nitride substrate 110 can offset the compressive stress of the silicon-based transition layer 120 and the silicon-based top layer 130, thereby avoiding the risk of warping and cracking common in multilayer films.

[0034] In this embodiment, the silicon nitride substrate 110 is a silicon-rich silicon nitride layer with a thickness of 110-132 nm and a first refractive index of 2.12-2.30. Specifically, the thickness of the silicon-rich silicon nitride layer can be 110 nm, 115 nm, 123 nm, or 132 nm. Preferably, the first refractive index is 2.15, and the thickness of the silicon-rich silicon nitride layer is 115 nm.

[0035] In other embodiments of the present invention, the silicon nitride substrate 110 may also be selected from one of a titanium silicon nitride layer, a niobium silicon composite nitride layer, or a zirconium-doped silicon nitride layer.

[0036] The silicon nitride substrate 110 serves as the optical and mechanical reference layer for the composite antireflective film structure. On one hand, its highest refractive index creates a significant refractive index difference with the silicon dioxide light-transmitting window 100, providing the necessary optical path difference for broadband interference antireflection in the composite antireflective film structure. Furthermore, during the deposition process, it can simultaneously fill the microscopic irregularities on the surface of the silicon dioxide light-transmitting window 100, significantly improving the interfacial bonding of subsequent film layers. Moreover, a single high-refractive-index design can replace multiple high-refractive-index functional layers in a traditional five-layer film system, simplifying the film structure from the source and avoiding light scattering losses caused by multiple interfaces. On the other hand, it inherently generates controllable tensile stress, eliminating the need for an additional stress buffer layer. The stress can be precisely offset by the synergy of the compressive stress of the two upper layers, stably controlling the residual stress of the composite antireflective film structure within a weak compressive range of less than 79 MPa. This completely avoids the risks of warping, cracking, and interlayer delamination caused by the gradual accumulation of stress in traditional multilayer films.

[0037] The silicon-based transition layer 120 covers the surface of the silicon nitride substrate layer 110, serving as an intermediate transition layer between optical and mechanical aspects. The silicon-based transition layer 120 has a second refractive index. The second refractive index is less than or equal to the refractive index of the silicon dioxide light-transmitting window 100, and in the composite antireflective film structure, the refractive index of the silicon nitride substrate layer 110 is the smallest.

[0038] The silicon-based transition layer 120 forms compressive stress, which can offset part of the tensile stress in the silicon nitride substrate layer 110.

[0039] In this embodiment, the silicon-based transition layer 120 is a fluorine-doped silicon oxide layer with a thickness of 36–50 nm and a second refractive index of 1.38–1.45. Specifically, the thickness of the silicon-based transition layer 120 is 36 nm, 40 nm, or 50 nm. Preferably, the second refractive index is 1.38, and the thickness of the silicon-based transition layer 120 is 40 nm.

[0040] In other embodiments of the present invention, the silicon-based transition layer 120 may also be selected from one of a carbon-doped silicon oxide layer, a carbon oxy silicon layer, or a fluorine oxy silicon layer.

[0041] The silicon-based transition layer 120 forms a low-refractive-index node between the high-refractive-index silicon nitride substrate layer 110 and the medium-refractive-index silicon-based top layer 130. This not only significantly widens the overall refractive index span of the composite antireflective film structure to enhance the intensity of wide interference destructive forces, but also effectively blocks the penetration paths of water vapor and impurities through the dense network of low-refractive-index layers, solving the problem of weather resistance degradation caused by the porous interface in traditional multilayer films. Simultaneously, the intrinsically weak compressive stress within the silicon-based transition layer 120 absorbs the tensile stress of the silicon nitride substrate layer 110, achieving a smooth transition of the stress gradient in a three-layer structure. This avoids the risk of interface delamination caused by stress accumulation in traditional five-layer or higher film systems, ultimately achieving a balance between optical antireflection and mechanical stability with the fewest possible film layers.

[0042] The silicon-based top layer 130 covers the surface of the silicon-based transition layer 120, serving as the topmost layer of the composite antireflective film structure.

[0043] The silicon-based top layer 130 has a third refractive index, which is less than the first refractive index and greater than the second refractive index. In the composite antireflective film structure, the refractive index of the silicon-based top layer 130 is of intermediate size, that is, the refractive index of the silicon-based top layer 130 is greater than the refractive index of the silicon-based transition layer 120 and less than the refractive index of the silicon nitride substrate layer 110.

[0044] The compressive stress formed in the silicon-based top layer 130 can offset part of the tensile stress in the silicon nitride base layer 110, and thus together with the silicon-based transition layer 120, offset all the tensile stress in the silicon nitride base layer 110.

[0045] In this embodiment, the silicon-based top layer 130 is a fluorine-doped silicon-oxygen layer with a thickness of 80–94 nm and a third refractive index of 1.47–1.58. Specifically, the thickness of the fluorine-doped silicon-oxygen layer can be 80 nm, 85 nm, 90 nm, or 94 nm. Preferably, the third refractive index is 1.47, and the thickness of the fluorine-doped silicon-oxygen layer is 85 nm. The fluorine-doped silicon-oxygen layer integrates four major functions: low refractive index and anti-reflection, high hardness and wear resistance, ultraviolet shielding, and native hydrophobicity, thereby improving its resistance to friction, damp heat, and fingerprints.

[0046] In other embodiments of the present invention, the silicon-based top layer 130 is selected from one of a boron-aluminum co-doped carbon-oxygen silicon layer, a zirconium-doped fluorine-silicon layer, or a hard silicon-oxygen carbon layer containing methylsilane. These silicon-based top layers 130 are multifunctional low-refractive-index surface layers, forming controllable weak compressive stress within the thin film, while simultaneously achieving broadband antireflection, ultraviolet shielding, high hardness and wear resistance, and hydrophobicity and oleophobicity.

[0047] The silicon-based top layer 130 serves as the refractive index bridging layer at the outermost end of the composite antireflective film system. Its refractive index is between that of the silicon-based transition layer 120 and air, reducing the abrupt change in refractive index between the surface layer and air compared to traditional MgF2 antireflective films. This fundamentally suppresses the sharp increase in reflectivity at large incident angles, effectively eliminating edge color shift and ghosting issues in wide-angle lenses. Simultaneously, the controllable compressive stress inherently formed by the silicon-based top layer 130 and the weak compressive stress of the silicon-based transition layer 120 complement each other. Together, they offset the tensile stress of the silicon nitride substrate layer 110, suppressing the overall residual stress of the composite antireflective film structure within a weak compressive range of less than 79 MPa.

[0048] In some embodiments, the compressive stress of the silicon-based top layer 130 is greater than that of the silicon-based transition layer 120. The compressive stress of the silicon-based transition layer 120 is controlled within the weak compressive stress range, serving as a stress buffer layer to support the silicon nitride substrate 110. This prevents excessive compressive stress from directly impacting the high tensile stress of the silicon nitride substrate 110, thereby reducing stress abrupt defects such as interlayer microcracks and peeling at the source. Furthermore, a relatively larger controllable compressive stress can be applied to the silicon-based top layer 130. This not only utilizes the buffering effect of the silicon-based transition layer 120 to prevent stress from being directly transmitted to the silicon nitride substrate 110, but also forms a gradient synergy with the weak compressive stress of the silicon-based transition layer 120, more efficiently offsetting the tensile stress of the silicon nitride substrate 110 and stably suppressing the overall residual stress of the composite film layer to a lower weak compressive stress level.

[0049] In one embodiment, the silicon nitride substrate 110 is a silicon-rich silicon nitride layer with a thickness of 110–132 nm and a first refractive index of 2.12–2.30; the silicon-based transition layer 120 is a fluorine-doped silicon oxide layer with a thickness of 36–50 nm and a second refractive index of 1.38–1.45; and the silicon-based top layer 130 is a fluorine-doped silicon carbide layer with a thickness of 80–94 nm and a third refractive index of 1.47–1.58. This composite antireflective coating structure enables single-cavity continuous plasma-enhanced chemical vapor deposition (PECVD) deposition without equipment switching or vacuum breaking, achieving low-temperature deposition at 80–120°C. This simplifies the process, reduces equipment and labor costs, ensures uniform thickness of the curved lens, and provides high process stability.

[0050] In one embodiment, the composite antireflective film structure further includes an anti-fingerprint layer disposed on the surface of the silicon-based top layer 130. The anti-fingerprint layer effectively resists fingerprint residue and can further fill micropore defects in the silicon-based top layer 130, improving the film's abrasion resistance life. In one embodiment, the anti-fingerprint layer is a perfluoropolyether (AF) anti-fingerprint layer.

[0051] This invention also provides a method for preparing a composite antireflective film structure for a silica light-transmitting window. For example... Figure 2 The diagram illustrates the steps of a method for preparing a composite antireflective film structure for a silicon dioxide light-transmitting window according to an embodiment of the present invention. The preparation method includes: Step S20: A silicon nitride substrate layer is deposited on the surface of the silicon dioxide light-transmitting window. By setting the proportions of each reactant, the silicon nitride substrate layer is made to have a first refractive index, and tensile stress is formed within the layer. The first refractive index is greater than the refractive index of the silicon dioxide light-transmitting window. This proportion is the flow rate ratio.

[0052] During the deposition process, the vapor precursor conformally fills the nanoscale pits and micro-scratches on the surface of the silica light-transmitting window, achieving in-situ smoothing of the substrate surface. This not only physically fills the micro-unevenness on the surface of the silica light-transmitting window, but also activates the dangling bonds on the substrate surface through plasma bombardment, prompting the silicon nitride mesh and the silica light-transmitting window to form a Si-O-Si covalent bond interface, greatly improving the film adhesion and eliminating the risk of interlayer delamination from the root.

[0053] During the deposition of a silicon nitride substrate layer on the surface of the silicon dioxide light-transmitting window, a uniform and controllable intrinsic tensile stress is accumulated. This tensile stress is not a process defect, but a necessary feature of the composite antireflective film structure described in this invention. In some embodiments, the magnitude of the tensile stress can be adjusted by regulating the atomic ratio of the elements in the reactants.

[0054] In one embodiment, the deposition process is selected based on the material of the silicon nitride substrate, and the deposition process includes a plasma-enhanced chemical vapor deposition (PECVD) process.

[0055] In one embodiment, the silicon nitride substrate layer is a silicon-rich silicon nitride layer with a thickness of 110-132 nm and a first refractive index of 2.12-2.30. The step of depositing the silicon nitride substrate layer on the surface of the silicon dioxide light-transmitting window further includes: using a silicon source and NH3 as reactants, and employing a plasma-enhanced chemical vapor deposition process to form the silicon-rich silicon nitride layer on the surface of the silicon dioxide light-transmitting window. By setting the flow rate ratio of the silicon source to NH3, the silicon-rich silicon nitride layer is made to have a first refractive index, and tensile stress is formed within the layer. The silicon source includes one or more of Si2H6, SiH2Cl2, or SiH4.

[0056] Specifically, with the same deposition thickness, using SiH4 as the silicon source, when the SiH4 to NH3 flow ratio is a constant, the first refractive index of the silicon-rich silicon nitride layer is a corresponding constant, and the tensile stress formed in the layer is a corresponding constant. When the SiH4 to NH3 flow ratio is modified to another constant, the first refractive index of the silicon-rich silicon nitride layer is another corresponding constant, and the tensile stress formed in the layer is another corresponding constant.

[0057] As an example, when depositing the silicon nitride substrate with a thickness of 115 nm, the refractive index of the final silicon-rich silicon nitride layer is 2.12 when the flow ratio of SiH4 to NH3 is 0.84 (the atomic ratio of N atoms to Si atoms is 0.98); the refractive index of the final silicon-rich silicon nitride layer is 2.30 when the flow ratio of SiH4 to NH3 is 1.02 (the atomic ratio of N atoms to Si atoms is 0.75); and the refractive index of the final silicon-rich silicon nitride layer is 2.41 when the flow ratio of SiH4 to NH3 is 1.13 (the atomic ratio of N atoms to Si atoms is 0.61).

[0058] In this step, increasing the proportion of silicon source in the reaction gas (i.e., increasing the Si / N atomic ratio) will significantly increase the Si-Si bond density inside the silicon nitride substrate. As the silicon enrichment level increases, the network structure of the silicon nitride substrate undergoes intrinsic distortion, which in turn induces and increases the intrinsic tensile stress inside the film.

[0059] This invention achieves simultaneous control of the refractive index and tensile stress of silicon-rich silicon nitride layers by adjusting the proportion of the gaseous precursor.

[0060] As an example, in some embodiments, the silicon nitride substrate layer is selected from one of a titanium silicon nitride layer, a niobium silicon composite nitride layer, and a zirconium-doped silicon nitride layer.

[0061] Step S21: A silicon-based transition layer is deposited on the surface of the silicon nitride substrate. By setting the proportions of each reactant, the silicon-based transition layer is made to have a second refractive index, and compressive stress is formed within the layer. The second refractive index is less than or equal to the refractive index of the silicon dioxide light-transmitting window. This proportion is a flow rate ratio.

[0062] During the deposition of a silicon-based transition layer on the surface of the silicon nitride substrate, a uniform and controllable intrinsic compressive stress is accumulated. This compressive stress is not a process defect, but a necessary feature of the composite antireflective film structure of the present invention. In some embodiments, the magnitude of the compressive stress can be adjusted by regulating the atomic ratio of characteristic elements in the reactants.

[0063] In one embodiment, the deposition process is selected based on the material of the silicon-based transition layer, and the deposition process includes plasma-enhanced chemical vapor deposition.

[0064] In one embodiment, the silicon-based transition layer is a fluorine-doped silicon oxide layer with a thickness of 36–50 nm and a second refractive index of 1.38–1.45. The step of depositing the silicon-based transition layer on the surface of the silicon nitride substrate further includes: using a silicon source, N2O, and a fluorine source as reactants, and employing plasma-enhanced chemical vapor deposition to form in-situ fluorine doping on the surface of the silicon nitride substrate, thereby forming the fluorine-doped silicon oxide layer. By setting the flow rate ratio of the silicon source, N2O, and fluorine source, as well as the flow rate percentage of the fluorine source in the total reactants, the fluorine-doped silicon oxide layer is made to have a second refractive index, and compressive stress is formed within the layer. The silicon source includes one or more of Si2H6, SiH2Cl2, or SiH4. The fluorine source includes one or two of CF4 or SiF4.

[0065] Specifically, with the same deposition thickness, using SiH4 as the silicon source and CF4 as the fluorine source, and with the flow ratio of SiH4, N2O and CF4 being a constant and the proportion of CF4 in the total flow being a constant, the second refractive index of the silicon-based transition layer is a corresponding constant, and the compressive stress formed within the layer is a corresponding constant. When the flow ratio of SiH4, N2O and CF4 is modified to another constant, and the proportion of CF4 in the total flow is another constant, the second refractive index of the silicon-based transition layer is another corresponding constant, and the compressive stress formed within the layer is another corresponding constant.

[0066] As an example, when depositing the silicon-based transition layer with a thickness of 40 nm, when the flow rate ratio of SiH4, N2O and CF4 is 23:200:7, CF4 accounts for 3.04% of the total flow rate of the reactant gas (i.e., the molar percentage of F atoms in the silicon-based transition layer is approximately 2.2%), and the refractive index of the final silicon-based transition layer is 1.45; when the flow rate ratio of SiH4, N2O and CF4 is 69:450:35, CF4 accounts for 6.32% of the total flow rate of the reactant gas (i.e., the molar percentage of F atoms in the silicon-based transition layer is approximately 5.8%), and the refractive index of the final silicon-based transition layer is 1.38.

[0067] In this step, by changing the proportion of CF4 in the total flow rate of the reactant gas, the actual doping concentration of F atoms in the silicon-based transition layer can be controlled, thereby achieving controllable adjustment of the intrinsic compressive stress of the layer. The F atoms generated by the plasma decomposition of CF4 replace the bridging oxygen / non-bridging oxygen sites in the Si-O network, breaking the continuous Si-O-Si crosslinking chains, reducing the network crosslinking density of the film, and causing the porosity to gradually increase with the increase of F doping amount; as the constraint force of the network on the film structure decreases, the intrinsic compressive stress originally generated by plasma bombardment and lattice distortion will be gradually released, macroscopically manifested as a regular decrease in compressive stress with increasing F atom concentration.

[0068] This invention achieves simultaneous control of the refractive index and compressive stress of silicon-rich silicon nitride layers by adjusting the proportion of gaseous precursors and the concentration of F atoms.

[0069] In the existing technology, after the formation of the silicon oxide transition layer, a post-fluorination treatment is usually performed. The purpose is to solve the defects of uneven fluorine doping, film moisture absorption and metal electrode corrosion in the traditional process. The existing method is to put the prepared silicon oxide film into a plasma environment containing fluorine gas for secondary bombardment, wetting or thermal annealing diffusion, so that fluorine atoms can penetrate from the surface into the interior of the film.

[0070] In this embodiment, in-situ fluorine doping is achieved during the deposition process, eliminating the need for post-fluorination treatment and greatly simplifying the process flow.

[0071] As an example, in some embodiments, the silicon-based transition layer is selected from one of a carbon-doped silicon oxide layer, a carbon oxy silicon layer, and a fluorine oxy silicon layer.

[0072] Step S22: A silicon-based top layer is deposited on the surface of the silicon-based transition layer. By setting the proportions of each reactant, the silicon-based top layer is made to have a third refractive index, and compressive stress is formed within the layer. The third refractive index is less than the first refractive index and greater than the second refractive index. The sum of the compressive stresses of the silicon-based top layer and the silicon-based transition layer can offset the tensile stress of the silicon nitride substrate layer. This proportion is a flow rate ratio.

[0073] During the deposition of the silicon-based top layer on the surface of the silicon-based transition layer, a uniform and controllable intrinsic compressive stress is accumulated. This compressive stress is not a process defect, but a necessary feature of the composite antireflective film structure described in this invention. In some embodiments, the magnitude of the compressive stress can be adjusted by regulating the atomic ratio of characteristic elements in the reactants.

[0074] In one embodiment, the deposition process is selected based on the material of the silicon-based top layer, and the deposition process includes plasma-enhanced chemical vapor deposition.

[0075] In one embodiment, the silicon-based top layer is a fluorine-doped silicon-oxygen layer with a thickness of 80–94 nm and a third refractive index of 1.47–1.58. The step of depositing the silicon-based top layer on the surface of the silicon-based transition layer further includes: using a silicon source, CO2, and a fluorine source as reactants, and employing plasma-enhanced chemical vapor deposition to form in-situ fluorine doping on the surface of the silicon-based transition layer, thereby forming the fluorine-doped silicon-oxygen layer. By setting the flow rate ratio of the silicon source, CO2, and fluorine source, as well as the flow rate percentage of the fluorine source in the total reactants, the fluorine-doped silicon-oxygen layer is made to have a third refractive index, and compressive stress is formed within the layer. The silicon source includes one or more of monomethylsilane, trimethylsilane, tetramethylsilane, or diethoxymethylsilane. The fluorine source includes one or two of CF4 or perfluoromethylsilane.

[0076] Specifically, with the same deposition thickness, using monomethylsilane (CH3SiH3) as the silicon source and CF4 as the fluorine source, when the flow ratio of CH3SiH3, CO2, and CF4 is a constant and the proportion of CF4 in the total flow is a constant, the third refractive index of the silicon-based top layer is a corresponding constant, and the compressive stress formed in the layer is a corresponding constant. When the flow ratio of CH3SiH3, CO2, and CF4 is modified to another constant and the proportion of CF4 in the total flow is another constant, the third refractive index of the silicon-based top layer is another corresponding constant, and the compressive stress formed in the layer is another corresponding constant.

[0077] As an example, when depositing the silicon-based top layer with a thickness of 85 nm, when the flow ratio of CH3SiH3, CO2, and CF4 is 75:250:12, CF4 accounts for 3.56% of the total flow of the reactant gas (i.e., the molar percentage of F atoms in the silicon-based top layer is approximately 3.4%), and the refractive index of the final silicon-based top layer is 1.58; when the flow ratio of CH3SiH3, CO2, and CF4 is 75:450:40, CF4 accounts for 7.08% of the total flow of the reactant gas (i.e., the molar percentage of F atoms in the silicon-based top layer is approximately 7.4%), and the refractive index of the final silicon-based top layer is 1.47.

[0078] In this step, by changing the proportion of CF4 in the total flow rate of the reactant gas, the actual doping concentration of F atoms in the silicon-based top layer can be controlled, thereby achieving controllable adjustment of the intrinsic compressive stress of the layer. The F atoms generated by the plasma decomposition of CF4 replace the bridging oxygen / non-bridging oxygen sites in the Si-O network, breaking the continuous Si-O-Si crosslinking chains, reducing the network crosslinking density of the film, and causing the porosity to gradually increase with the increase of F doping amount; as the constraint force of the network on the film structure decreases, the intrinsic compressive stress originally generated by plasma bombardment and lattice distortion will be gradually released, macroscopically manifested as a regular decrease in compressive stress with increasing F atom concentration.

[0079] As an example, in some embodiments, the silicon-based top layer is selected from one of a boron-aluminum co-doped carbon-oxygen silicon layer, a zirconium-doped fluorine-silicon layer, or a hard silicon-oxygen carbon layer containing methylsilane.

[0080] In one embodiment, dual-frequency radio frequency PECVD (13.56MHz + 400kHz) can be used during plasma-enhanced chemical vapor deposition to control the ion bombardment intensity and further reduce the residual stress of the film.

[0081] In one embodiment, when the silicon nitride substrate, silicon-based transition layer, and silicon-based top layer are all prepared using the same process, such as plasma-enhanced chemical vapor deposition (PECVD), they can be carried out in the same reaction chamber, achieving continuous deposition in a single chamber without switching equipment or breaking the vacuum. This allows for low-temperature deposition at 80–120°C without annealing, simplifying the process, reducing equipment and labor costs, ensuring uniform thickness of curved lenses, and providing high process stability. It is also suitable for low-temperature plastic lenses at 80–120°C.

[0082] In one embodiment, the silicon nitride substrate, silicon-based transition layer, and silicon-based top layer all utilize silicon-based organic / inorganic vapor phase precursors and are prepared using the same process. Continuous deposition is achieved by simply changing the gas ratio. The entire process is conducted under uninterrupted vacuum, eliminating dust pollution from lens transport and eliminating the need for electron beam evaporation equipment. PECVD plasma fully coats the curved lens, resulting in a film thickness uniformity deviation of <0.9% and no significant increase in edge reflectivity for wide-angle lenses.

[0083] In some embodiments, prior to the step of depositing a silicon nitride substrate layer on the surface of the silica light-transmitting window, the preparation method further includes: performing vacuum pretreatment on the silica light-transmitting window to remove organic impurities from the surface of the silica light-transmitting window and improve film adhesion. For example, the silica light-transmitting window may be subjected to ultrasonic cleaning with pure water, purging and drying with high-purity nitrogen, followed by argon plasma or oxygen plasma pre-cleaning to remove organic impurities from the surface of the silica light-transmitting window and improve film adhesion.

[0084] In some embodiments, after the step of depositing a silicon-based top layer on the surface of the silicon-based transition layer, the preparation method further includes forming an anti-fingerprint layer on the surface of the active silicon-based top layer. For example, a 7 nm to 12 nm perfluoropolyether (AF) anti-fingerprint layer is directly sprayed or roll-coated onto the surface of the active silicon-based top layer to further improve the surface's anti-fouling performance. This layer can be directly wet-coated and cured without complex pretreatment, seamlessly integrating with the three-layer PECVD in-situ continuous deposition process. Without compromising the simplified film structure, it endows the optical window with excellent anti-fouling and self-cleaning functions, significantly improving the imaging clarity and maintenance convenience of high-end lenses in complex usage environments.

[0085] In some embodiments, the perfluoropolyether anti-fingerprint layer can be omitted, and the fluorine flow rate can be increased during the deposition stage of the silicon-based top layer to achieve a native superhydrophobic surface.

[0086] As an example, the present invention also provides an embodiment of a method for preparing a composite antireflective film structure for a silica light-transmitting window.

[0087] A three-layer film structure was deposited using a PECVD device with an ICP power of 200W-400W. The temperature of the silica light-transmitting window was 80℃-100℃, the pressure inside the reaction chamber was 5Pa-20Pa, and the values ​​of Ar=80-130sccm and He=100-140sccm were specified.

[0088] Step 1: Vacuum pretreatment of silica light-transmitting window The silica light-transmitting window is ultrasonically cleaned with pure water and purged and dried with high-purity nitrogen before being sent into a PECVD single vacuum chamber. Argon plasma pre-cleaning is performed for 90–150 seconds, with the basic vacuum degree of the chamber being 0.06–0.18 Pa, to remove organic impurities from the substrate surface and improve the adhesion of the film layer.

[0089] Step 2: Apply the first, second, and third coatings sequentially using PECVD on the silica light-transmitting window.

[0090] Step (1): Introduce SiH4 and NH6, and adjust the flow ratio to prepare a silicon-rich SiNX high-refractive-fold layer.

[0091] The first coating layer is deposited on the silicon dioxide light-transmitting window. The specific coating process is as follows: The temperature of the silica light-transmitting window was 100°C, Ar=120sccm, He=130sccm, ICP power was 350 W, the pressure of the reaction chamber was set and stabilized at 10 Pa, SiH4=6.9sccm was fixed, and only the NH3 flow rate was changed.

[0092] When the flow ratio of SiH4 to NH3 was set to 0.84 and the [N] / [Si] atomic ratio was set to 0.98, the refractive index of the resulting silicon-rich SiNx high-refractive-index layer was 2.12. When the flow ratio of SiH4 to NH3 was set to 1.02 and the [N] / [Si] atomic ratio was set to 0.75, the refractive index of the resulting silicon-rich SiNx high-refractive-index layer was 2.30. When the flow ratio of SiH4 to NH3 was set to 1.13 and the [N] / [Si] atomic ratio was set to 0.61, the refractive index of the resulting silicon-rich SiNx high-refractive-index layer was 2.41.

[0093] The deposition rate was 23.5 nm / min, the deposition time was 4.89 minutes, and the deposition thickness was 115 nm.

[0094] Step (2): Introduce SiH4, N2O, and CF4, and adjust the flow rate ratio to prepare a fluorine-doped SiOx transition layer.

[0095] When step (1) reaches the preset time, during the switching of adjacent film layers, the plasma source is cut off and gas is exchanged in situ. The cavity is kept under vacuum and constant at 100°C, and the flow rates of Ar, He, and SiH4 are kept constant. The NH3 gas valve is quickly closed, while the N2O and CF4 gas valves are opened simultaneously. Fluorine-doped SiOx transition layer is deposited in situ; the gas flow is dynamically balanced in situ for 30 seconds, and the residual NH3 in the cavity is completely exhausted using the carrier gas.

[0096] With N₂O = 60.0 sccm and CF₄ = 2.1 sccm, CF₄ accounts for 3.04% of the total reactant gas flow rate, and the molar percentage of F atoms in the film is approximately 2.2%. The final refractive index of the obtained fluorine-doped SiO₂ transition layer is 1.45. With N₂O = 45.0 sccm and CF₄ = 3.5 sccm, CF₄ accounts for 6.32% of the total reactant gas flow rate, and the molar percentage of F atoms in the film is approximately 5.8%. The final refractive index of the obtained fluorine-doped SiO₂ transition layer is 1.38.

[0097] Re-enable ICP power to 350 W. Perform in-situ continuous deposition for 2.2 minutes at a rate of 18.0 nm / min, with the film thickness controlled at 40 nm.

[0098] Step (3): Introduce CH3SiH3, CO2, and CF4, and adjust the flow ratio to prepare a fluorine-doped SiOC multifunctional surface layer; When step (2) reaches the preset time, during the switching of adjacent membrane layers, the plasma source is cut off and gas is exchanged in situ. The cavity is kept at a constant vacuum of 100°C, and the Ar and He carrier gas flow rates are kept constant. The SiH4 and N2O gas valves are quickly closed, and the monomethylsilane (CH3SiH3) and CO2 gas valves are introduced, and the CF4 flow rate is adjusted. The methylsilane flow rate is fixed at 7.5 sccm, and the CO2 to CF4 ratio is finely adjusted. The in-situ equilibrium is maintained for 30 seconds, and the automatic pressure valve (APC) ensures that the cavity pressure is stable at 10 Pa.

[0099] With CO2 = 25.0 sccm and CF4 = 1.2 sccm, the refractive index of the fluorine-doped SiOC multifunctional surface layer obtained was 1.58. With CO2 = 45.0 sccm and CF4 = 4.0 sccm, the refractive index of the fluorine-doped SiOC multifunctional surface layer obtained was 1.47.

[0100] ICP power was restarted to 350 W, and in-situ continuous deposition was performed at a rate of 20.0 nm / min for 4.25 minutes, with the film thickness controlled at 85 nm. The film thickness uniformity deviation of the curved lens was <0.9%.

[0101] Step 3: Post-processing Vacuum cooling: After deposition, disconnect the RF power supply and close all reaction gas valves (methylsilane, CO2, CF4). Maintain the flow of Ar and He carrier gases and allow in-situ cooling for 5-10 minutes under a vacuum of 10 Pa.

[0102] Breaking the vacuum and removing the lens: When the substrate temperature safely drops below 60°C, turn off the carrier gas, fill the system with high-purity nitrogen to break the vacuum, and remove the lens.

[0103] AF anti-fingerprint layer wet coating: The lens coated with the composite anti-reflective film structure is directly sent to the wet coating workstation, and a 7 nm–12 nm perfluoropolyether (AF) anti-fingerprint layer is directly sprayed or roller-coated on the active SiOC surface, and then cured according to the specifications.

[0104] The present invention prepared Examples 1 to 3 using the above-described preparation method. In Examples 1 to 3, SiH4 and NH3 were used as reactant gases when preparing the silicon nitride substrate layer, SiH4, N2O, and CF4 were used as reactant gases when preparing the silicon-based transition layer, and CH3SiH3, CO2, and CF4 were used as reactant gases when preparing the silicon-based top layer.

[0105] An uncoated silicon dioxide substrate was introduced as Comparative Example 1, and a lens with a multilayer film (SiO2 / TiO2 alternating) deposited by conventional electron beam evaporation was introduced as Comparative Example 2.

[0106] The comprehensive performance test results of each group of samples are shown in Table 1: (1) Reflectance test: The reflectance spectra of normal incidence and 35° oblique incidence in the 400nm–700nm band were tested using a UV-Vis-NIR spectrophotometer (Cary 5000).

[0107] (2) Residual stress test: The overall residual stress of the film was calculated by measuring the change in the radius of curvature of the substrate before and after coating using the Stoney formula.

[0108] Table 1

[0109] It should be noted that references to "an embodiment," "an embodiment," "an exemplary embodiment," "some embodiments," etc., in the specification indicate that the described embodiments may include specific features, structures, or characteristics, but each embodiment may not necessarily include that specific feature, structure, or characteristic. Furthermore, such phrases do not necessarily refer to the same embodiment. In addition, when a specific feature, structure, or characteristic is described in connection with an embodiment, whether explicitly described or not, implementing such a feature, structure, or characteristic in conjunction with other embodiments is within the knowledge of those skilled in the art.

[0110] It should be noted that the terms "comprising" and "having," and their variations, used in this invention document are intended to cover non-exclusive inclusion. The terms "first," "second," etc., are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence, unless explicitly indicated by the context. It should be understood that such data used interchangeably where appropriate. Furthermore, embodiments and features within embodiments of this invention can be combined with each other unless otherwise specified. In addition, descriptions of well-known components and technologies have been omitted in the above description to avoid unnecessarily obscuring the concepts of this invention. In the various embodiments described above, each embodiment focuses on its differences from other embodiments; similar or identical parts between embodiments can be referred to interchangeably.

[0111] The above description is only a preferred embodiment of the present invention. It should be noted that those skilled in the art can make several improvements and modifications without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. A composite antireflective film structure for a silica light-transmitting window, characterized in that, The following components are sequentially disposed on the surface of the silicon dioxide light-transmitting window: a silicon nitride substrate layer covering the surface of the silicon dioxide light-transmitting window, the silicon nitride substrate layer having a first refractive index and tensile stress forming within the layer, the first refractive index being greater than the refractive index of the silicon dioxide light-transmitting window; a silicon-based transition layer covering the surface of the silicon nitride substrate layer, the silicon-based transition layer having a second refractive index and compressive stress forming within the layer, the second refractive index being less than or equal to the refractive index of the silicon dioxide light-transmitting window; and a silicon-based top layer covering the surface of the silicon-based transition layer, the silicon-based top layer having a third refractive index and compressive stress forming within the layer, the third refractive index being less than the first refractive index and greater than the second refractive index, the sum of the compressive stress of the silicon-based top layer and the silicon-based transition layer being able to offset the tensile stress of the silicon nitride substrate layer.

2. The composite antireflective film structure according to claim 1, characterized in that, The silicon nitride substrate is a silicon-rich silicon nitride layer with a thickness of 110~132nm and a first refractive index of 2.12–2.

30.

3. The composite antireflective film structure according to claim 1, characterized in that, The silicon nitride substrate is selected from one of the following: a titanium silicon nitride layer, a niobium silicon composite nitride layer, or a zirconium-doped silicon nitride layer.

4. The composite antireflective film structure according to claim 1, characterized in that, The silicon-based transition layer is a fluorine-doped silicon oxide layer with a thickness of 36–50 nm and a second refractive index of 1.38–1.

45.

5. The composite antireflective film structure according to claim 1, characterized in that, The silicon-based transition layer is selected from one of the following: a carbon-doped silicon oxide layer, a carbon-oxygen silicon layer, and a fluorine-oxygen silicon layer.

6. The composite antireflective film structure according to claim 1, characterized in that, The silicon-based top layer is a fluorine-doped carbon-oxygen silicon layer with a thickness of 80–94 nm, and the third refractive index is 1.47–1.

58.

7. The composite antireflective film structure according to claim 1, characterized in that, The silicon-based top layer is selected from one of the following: boron-aluminum co-doped carbon-oxygen silicon layer, zirconium-doped fluorine-silicon layer, or hard silicon-oxygen carbon layer containing methylsilane.

8. The composite antireflective film structure according to claim 1, characterized in that, The compressive stress in the silicon-based top layer is greater than the compressive stress in the silicon-based transition layer.

9. The composite antireflective film structure according to claim 1, characterized in that, The composite antireflective film structure also includes an anti-fingerprint layer, which is disposed on the surface of the silicon-based top layer.

10. A method for preparing a composite antireflective film structure for a silica light-transmitting window, characterized in that, The method includes the following steps: depositing a silicon nitride substrate layer on the surface of the silicon dioxide light-transmitting window; by setting the proportions of each reactant, the silicon nitride substrate layer has a first refractive index and tensile stress is formed within the layer, the first refractive index being greater than the refractive index of the silicon dioxide light-transmitting window; depositing a silicon-based transition layer on the surface of the silicon nitride substrate layer; by setting the proportions of each reactant, the silicon-based transition layer has a second refractive index and compressive stress is formed within the layer, the second refractive index being less than or equal to the refractive index of the silicon dioxide light-transmitting window; depositing a silicon-based top layer on the surface of the silicon-based transition layer; by setting the proportions of each reactant, the silicon-based top layer has a third refractive index and compressive stress is formed within the layer, the third refractive index being less than the first refractive index and greater than the second refractive index, and the sum of the compressive stress of the silicon-based top layer and the silicon-based transition layer being able to offset the tensile stress of the silicon nitride substrate layer.

11. The preparation method according to claim 10, characterized in that, The silicon nitride substrate is a silicon-rich silicon nitride layer with a thickness of 110~132nm and a first refractive index of 2.12–2.

30. The step of depositing the silicon nitride substrate layer on the surface of the silicon dioxide light-transmitting window further includes: using a silicon source and NH3 as reactants, and employing a plasma-enhanced chemical vapor deposition process to form the silicon-rich silicon nitride layer on the surface of the silicon dioxide light-transmitting window. By setting the flow rate ratio of the silicon source to NH3, the silicon-rich silicon nitride layer is made to have a first refractive index, and tensile stress is formed within the layer.

12. The preparation method according to claim 10, characterized in that, The silicon-based transition layer is a fluorine-doped silicon oxide layer with a thickness of 36–50 nm and a second refractive index of 1.38–1.

45. The step of depositing the silicon-based transition layer on the surface of the silicon nitride substrate further includes: using a silicon source, N2O, and a fluorine source as reactants, and employing a plasma-enhanced chemical vapor deposition process to form in-situ fluorine doping on the surface of the silicon nitride substrate, thereby forming the fluorine-doped silicon oxide layer. By setting the flow rate ratio of the silicon source, N2O, and fluorine source, as well as the flow rate percentage of the fluorine source in the total reactants, the fluorine-doped silicon oxide layer is made to have a second refractive index, and compressive stress is formed within the layer.

13. The preparation method according to claim 10, characterized in that, The silicon-based top layer is a fluorine-doped silicon-oxygen layer with a thickness of 80–94 nm and a third refractive index of 1.47–1.

58. The step of depositing the silicon-based top layer on the surface of the silicon-based transition layer further includes: using silicon source, CO2, and fluorine source as reactants, and employing plasma-enhanced chemical vapor deposition to form in-situ fluorine doping on the surface of the silicon-based transition layer, thereby forming the fluorine-doped silicon-oxygen layer. By setting the flow ratio of silicon source, CO2, and fluorine source, as well as the flow percentage of fluorine source in the total reactants, the fluorine-doped silicon-oxygen layer is made to have a third refractive index and compressive stress is formed within the layer.

14. The preparation method according to claim 10, characterized in that, Before the step of depositing a silicon nitride substrate layer on the surface of the silicon dioxide light-transmitting window, the preparation method further includes: performing vacuum pretreatment on the silicon dioxide light-transmitting window to remove organic impurities on the surface of the silicon dioxide light-transmitting window and improve the adhesion of the film layer.

15. The preparation method according to claim 10, characterized in that, After the step of depositing a silicon-based top layer on the surface of the silicon-based transition layer, the fabrication method further includes forming an anti-fingerprint layer on the active surface of the silicon-based top layer.