A silver mirror with a wide incident angle range and low polarization sensitivity and a preparation process thereof

By introducing a double-layer protective film structure on the silver mirror and optimizing the matching of film thickness and refractive index, the problems of high reflectivity, low polarization sensitivity and long-term environmental tolerance of the silver mirror in a wide band and wide angle are solved, and the stability and long-term reliability of the high-precision optical system are realized.

CN123156342APending Publication Date: 2026-11-24SHANGHAI INSTITUTE OF TECHNICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611342883.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-01
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing silver mirrors cannot simultaneously achieve high reflectivity, low polarization sensitivity, and long-term environmental tolerance over a wide wavelength and angle, which affects the imaging consistency and measurement accuracy of the optical system.

Method used

A dual-layer protective film structure is adopted, including a first dielectric protective film Al₂O₃ and a second dielectric protective film SiO₂. The film thickness and refractive index matching are optimized to form a dense, pinhole-free film layer of atomic layer deposition for the protection of silver films.

Benefits of technology

It maintains high reflectivity over a wide wavelength range, reduces polarization sensitivity, enhances oxidation and corrosion resistance, and extends service life, making it suitable for high-precision optical systems and extreme environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123156342A_ABST
    Figure CN123156342A_ABST
Patent Text Reader

Abstract

This invention discloses a silver reflector with low polarization sensitivity over a wide incident angle range and its fabrication process, belonging to the field of optical thin film technology. The silver reflector with low polarization sensitivity over a wide incident angle range has a double-layer protective film structure on its silver film. The double-layer protective film structure includes a first dielectric protective film and a second dielectric protective film. The first dielectric protective film is in contact with the silver film, wherein the first dielectric protective film is an Al2O3 film layer, and the second dielectric protective film is a SiO2 film layer. The thickness of the second dielectric protective film ensures that the reflectivity of short-wavelength s-rays and p-rays tends to be the same. The total optical thickness of the first and second dielectric protective films is less than one-quarter of the short-wavelength, and the thickness ratio of the first and second dielectric protective films is less than 2:5. This invention, by introducing a double-layer protective film structure on the surface of the silver reflector, ensures its high reflectivity characteristics over a wide wavelength range of 400-2500 nm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of optical thin film technology, and particularly relates to a silver reflector with low polarization sensitivity over a wide incident angle range and its fabrication process. Background Technology

[0002] Silver, due to its extremely high reflectivity in the visible to near-infrared band (400-2500 nm), is widely used in advanced optical measurement systems and aerospace optical remote sensing instruments. However, silver thin films have poor chemical stability and are highly susceptible to corrosion from oxygen, water vapor, and sulfides in the environment, leading to performance degradation. To extend its service life, traditionally, a dielectric protective layer with a thickness of more than 100 nm is applied to the silver surface using coating processes such as thermal evaporation, sputtering, and chemical vapor deposition to prevent oxidation and corrosion of silver by the external environment. However, thick dielectric films inevitably introduce significant thin-film interference effects, causing severe separation in amplitude and phase of the s / p polarization components of the reflected light, greatly increasing polarization sensitivity, and thus seriously interfering with the consistency of imaging and measurement accuracy of the optical system.

[0003] Although schemes exist to suppress polarization differentiation by compensating phase through the stacking of multilayer dielectric thin films, they still face irreconcilable technical challenges in practical applications. It is difficult to simultaneously achieve a combination of comprehensive performance indicators such as "ultra-wideband high reflectivity, wide-angle low polarization sensitivity, and long-term environmental durability," thus significantly limiting the engineering application potential of silver mirrors under extremely complex conditions. Therefore, there is an urgent need to develop a novel silver mirror structure that aims to maintain excellent high reflectivity within the ultra-wide spectral range of 400-2500 nm while achieving low polarization sensitivity over a wide angle and excellent long-term environmental tolerance, ensuring its long-term stable operation in wide-band, large-angle, and harsh space environments. Summary of the Invention

[0004] To address the aforementioned technical problems, this invention provides a silver reflector with low polarization sensitivity over a wide incident angle range and its fabrication process. This silver reflector can achieve high reflectivity in the 400-2500 nm wavelength band, low polarization sensitivity over a wide angle (0-60°), and long-term environmental tolerance, thereby meeting the requirements of high-precision optical systems for high reflection efficiency, low polarization sensitivity, and long-term reliability over a wide wavelength band.

[0005] To achieve the above objectives, the present invention adopts the following technical solution:

[0006] A silver reflector with a wide incident angle range and low polarization sensitivity has a double-layer protective film structure on its silver film. The double-layer protective film structure includes a first dielectric protective film and a second dielectric protective film. The first dielectric protective film is in contact with the silver film. The first dielectric protective film is an Al2O3 film layer, and the second dielectric protective film is a SiO2 film layer.

[0007] The thickness of the second dielectric protective film makes the reflectivity of s-rays and p-rays in the short-wavelength band (400~450 nm) tend to be the same.

[0008] The total optical thickness of the first dielectric protective film and the second dielectric protective film is less than one-quarter of the short-wavelength, and the ratio of the physical thickness of the first dielectric protective film and the second dielectric protective film is less than 2:5.

[0009] Both the first and second dielectric protective films are dense, pinhole-free films deposited by atomic layer deposition.

[0010] The beneficial effects of this invention are as follows:

[0011] (1) By introducing a double-layer protective film structure (Ag / Al2O3 / SiO2) on the surface of the silver film, the present invention ensures the high reflectivity of the silver mirror in a wide wavelength range of 400-2500 nm. At the same time, by optimizing the matching of film thickness and refractive index, the polarization reflectivity of p and s light is made to be nearly consistent, and the polarization sensitivity cos(2ψ) can be controlled within ±0.015, where ψ is the elliptic parameter and tan(ψ) is defined as the amplitude ratio of the reflectivity coefficients of p light and s light.

[0012] (2) The double-layer protective film structure of the present invention effectively blocks oxygen and sulfides from contacting the silver film, significantly improving the silver reflector's resistance to oxidation, sulfidation and environmental corrosion. Thus, it can maintain long-term stable optical performance in extreme environments such as high humidity, high temperature, high energy oxygen and high pollution, and can greatly extend the service life of the low polarization silver reflector.

[0013] (3) The preparation process of the present invention is highly compatible. It can be used to achieve film deposition by conventional industrial methods such as atomic layer deposition, electron beam evaporation or resistive evaporation without additional special process conditions. The film uniformity and repeatability are excellent, ensuring the dense coverage of the ultrathin protective film and making it feasible for large-scale industrial application.

[0014] (4) This invention breaks through the technical bottleneck of existing silver reflectors that are difficult to balance low polarization and long-term stability, and provides a solution with simple structure, excellent performance and controllable cost. It is applicable to high-power laser systems, precision microscopic imaging, astronomical observation and aerospace optical devices, and meets the requirements for long-term reliable operation under wide band, high energy efficiency and extreme environmental conditions. Attached Figure Description

[0015] Figure 1 This is a schematic diagram of the structure of the silver reflector with a wide incident angle range and low polarization sensitivity according to the present invention.

[0016] Figure 2 This is a cross-sectional TEM image of 5 nm Al2O3 prepared on a silicon wafer in Example 1 of the present invention.

[0017] Figure 3 The reflectance spectrum of the silver mirror with a wide incident angle range and low polarization sensitivity prepared in Example 1 of the present invention is shown in the range of 400-2500 nm.

[0018] Figure 4 The measured cos(2ψ) spectra of the silver reflector with a wide incident angle range and low polarization sensitivity prepared in Example 1 of the present invention at incident angles of 30°, 45° and 60°.

[0019] Figure 5 The reflectance spectrum of the silver mirror with a wide incident angle range and low polarization sensitivity prepared in Example 2 of the present invention is shown in the range of 450-2500 nm.

[0020] Figure 6 The measured cos(2ψ) spectra of the silver reflector with a wide incident angle range and low polarization sensitivity prepared in Example 2 of the present invention at incident angles of 30°, 45°, 60° and 75°.

[0021] In the attached drawings, the reference numerals are: 1-mirror body; 2-adhesive layer; 3-silver film; 4-first dielectric protective film; 5-second dielectric protective film. Detailed Implementation

[0022] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention. Furthermore, the technical features involved in the various embodiments of this invention described below can be combined with each other as long as they do not conflict with each other.

[0023] Example 1

[0024] See Figure 1 This embodiment provides a silver reflector with a wide incident angle range (0-60°) and low polarization sensitivity. The reflector structure consists of a reflector body 1, an adhesive layer 2, a silver film 3 and a double-layer protective film structure from bottom to top. The double-layer protective film structure includes a first dielectric protective film 4 and a second dielectric protective film 5. The first dielectric protective film 4 is in contact with the silver film 3.

[0025] The materials, physical thicknesses, and functions of each of the above-mentioned membrane layers are as follows:

[0026] The material of the mirror body 1 is fused silica sheet, which provides mechanical support with high flatness and low coefficient of thermal expansion for the entire multilayer film structure; the adhesive layer 2 is made of NiCr alloy with a thickness of about 20 nm, which provides adhesion between the silver film 3 and the mirror body 1.

[0027] The silver film 3 is made of high-purity metallic silver and has a vapor deposition thickness of about 120 nm. It is the key layer to achieve high reflectivity of 400-2500 nm. The thickness of the silver film 3 is determined by the reflection band. To minimize the transmittance of the reflection band, a thicker silver film can be used on curved or rough surfaces to avoid insufficient thickness in some areas.

[0028] The first dielectric protective film 4 is made of Al2O3 thin film with a thickness of 5 nm. Its functions include: firstly, serving as a transitional adhesive layer between the silver film and SiO2; and secondly, acting as an atomic-level isolation layer to block the direct oxidation of the silver film by highly reactive oxygen free radicals during the subsequent preparation of the SiO2 protective film using plasma-enhanced atomic layer deposition (PEALD). Its TEM image is shown below. Figure 2 As shown, an ultra-thin, continuous, and dense state is displayed. The thickness of the first dielectric protective film 4 must be greater than the thickness threshold required to achieve a continuous film state, in order to avoid corrosion by the subsequent plasma oxygen process of the dielectric coating, while also providing better adhesion.

[0029] The second dielectric protective film 5 is a SiO2 thin film with a thickness of 25 nm. This layer serves as an outer protective film to improve environmental stability and mechanical durability, while also acting as an optical phase control layer to precisely regulate the phase difference and amplitude ratio of the s and p polarization components in the reflected light, thereby reducing polarization separation. The thickness of the second dielectric protective film is determined by the band polarization characteristics of the target silver reflector. The thickness is gradually increased to make the short-wavelength s and p light tend to have the same reflectivity. The initial thickness used to achieve polarization consistency is approximately the same. At this point, a larger thickness is required for lower refractive indices, which helps to improve the protective performance.

[0030] The design of the double-layer protective film structure of the present invention can not only effectively protect the silver reflector from corrosion, but also achieve the synergy of the high reflectivity and low polarization sensitivity characteristics of the silver reflector.

[0031] In terms of process implementation, firstly, thermally evaporated silver monolayer films, atomically deposited alumina and silicon oxide monolayer films are deposited on substrates including silicon wafers and fused silica. Ellipsometry and spectral analysis are used to calibrate the deposition thickness and refractive index of each material. Subsequently, the calibration parameters are imported into thin-film design software for structural optimization, and precise fabrication is achieved in conjunction with a thin-film deposition control system.

[0032] The specific steps of the fabrication process for the wide incident angle range, low polarization sensitivity silver reflective mirror coating in this embodiment are as follows:

[0033] S1: Pre-treat the mirror body 1; specifically, clean the mirror body 1 with acetone, ethanol, and deionized water in sequence, and then let it air dry.

[0034] S2: Argon ion bombardment treatment is performed on the pretreated mirror body 1; specifically, the dried mirror body 1 is placed in a vacuum chamber, the temperature of the mirror body 1 is kept at room temperature, and the vacuum is evacuated to 5×10⁻⁶. -3 Below Pa; the mirror body 1 was bombarded with argon ions using a Hall ion source, with an anode voltage of 120 V and an anode current of 5 A for 10 minutes;

[0035] S3: An adhesive layer is deposited on the mirror body after the treatment in step S2 by room temperature evaporation; specifically, an adhesive layer 2 with a thickness of 20 nm is deposited on the mirror body 1 by room temperature evaporation at a rate of 0.3 nm / s.

[0036] S4: A silver film 3 is deposited on the adhesive layer 2 by room temperature evaporation; specifically, a silver film 3 with a thickness of 120 nm is deposited on the adhesive layer 2 by room temperature evaporation at a rate of 2 nm / s.

[0037] S5: A first dielectric protective film 4 with a thickness of 5 nm is deposited on the silver film 3 by thermal atomic layer deposition; specifically, the vacuum chamber is vented, the sample obtained in step S4 is taken out, and then the sample is quickly transferred to the atomic layer deposition reaction chamber, heated to 80°C, and held at that temperature for 1.5 hours; the first dielectric protective film 4 is grown on the silver film 3 by thermal atomic layer deposition of trimethylaluminum and H2O.

[0038] S6: A second dielectric protective film 5 with a thickness of 25 nm is deposited on the first dielectric protective film 4 using plasma-enhanced atomic layer deposition; specifically, the second dielectric protective film 5 is deposited on the first dielectric protective film 4 using a plasma-enhanced atomic layer deposition process of bis(tert-butylamino)silane and oxygen; after the coating is completed, heating is stopped, the gas is released, and the sample is taken out for testing.

[0039] To verify the feasibility of this embodiment, we systematically tested the optical performance of the fabricated silver mirror with a wide incident angle range and low polarization sensitivity.

[0040] Figure 3 The reflectance spectrum of the silver mirror with a wide incident angle range and low polarization sensitivity prepared in Example 1 of the present invention is shown in the range of 400-2500 nm. Figure 3 The results show that the average reflectance is as high as 98.7% in the ultra-wide spectral range of 400-2500 nm.

[0041] Figure 4 The measured cos(2ψ) spectra of the silver reflector with a wide incident angle range and low polarization sensitivity prepared in Example 1 of the present invention at incident angles of 30°, 45° and 60°. Figure 4The results show that within an incident angle of 30°, the cos(2ψ) value is controlled within ±0.01; within an incident angle of 60°, the cos(2ψ) value is controlled within ±0.015, meaning the maximum polarization sensitivity does not exceed 1.5%. This makes the reflectivity of p- and s-polarized light nearly uniform across the entire wavelength range, effectively suppressing polarization separation and ensuring the consistency and stability of the reflected light signal. This verifies the reliability and feasibility of the design proposed in this embodiment.

[0042] This embodiment maintains broadband high reflectivity while significantly reducing polarization sensitivity. Furthermore, it achieves long-term protection of the silver film through a composite ultrathin protective film, greatly improving the device's environmental stability and optical consistency. Compared to traditional silver mirrors, this embodiment not only solves the polarization sensitivity problem but also effectively extends the device's lifespan, enhancing its application value in high-end optical systems, lasers, space optics, and imaging equipment.

[0043] Example 2

[0044] The overall structure of this embodiment is the same as that of Embodiment 1, consisting of a mirror body 1, an adhesive layer 2, a silver film 3, a first dielectric protective film 4, and a second dielectric protective film 5, from bottom to top. The mirror body 1 is made of K9 glass, the adhesive layer 2 is a 50 nm thick Cr layer, the silver film 3 is 150 nm thick, the first dielectric protective film 4 is a 10 nm thick Al2O3 film, and the second dielectric protective film 5 is a 33 nm thick SiO2 film.

[0045] The preparation process is the same as in Example 1.

[0046] This embodiment achieves differentiated polarization control across different wavelength ranges by adjusting the thickness ratio of the first dielectric protective film 4 and the second dielectric protective film 5, thereby meeting the personalized needs of specific application scenarios. In the design scheme of this embodiment, we optimize the film thickness combination of Al2O3 and SiO2 to achieve low polarization characteristics under large incident angle conditions. Specifically, this embodiment is applicable to a longer wavelength range, and the available protective film is thicker. The Al2O3 film layer is thicker (10nm) to achieve a more continuous and dense structure, ensuring a larger tolerance in the coating process. Compared with the shortest reflection wavelength of 400nm in Embodiment 1, this embodiment only needs to ensure polarization consistency around 450nm, and the SiO2 film layer can also have a larger thickness (33nm) to achieve better protection against water vapor and other corrosion.

[0047] Figure 5 The reflectance spectrum of the silver mirror with a wide incident angle range and low polarization sensitivity prepared in Example 2 of the present invention is shown in the range of 450-2500 nm. Figure 5As shown, the silver reflector with low polarization sensitivity and wide incident angle range prepared in this embodiment has an average reflectivity of 98.1% in the 450-2500 nm band.

[0048] Figure 6 The measured cos(2ψ) spectra of the silver reflector with a wide incident angle range and low polarization sensitivity prepared in Example 2 of the present invention at incident angles of 30°, 45°, 60° and 75°. Figure 6 Experimental results show that, within a large incident angle range of 75°, the maximum polarization sensitivity cos(2ψ) of this mirror in the 450-1200 nm band can be stably controlled within ±0.015, which is far superior to conventional silver mirrors. At the same time, this embodiment can achieve low polarization reflection in the visible light region, making it suitable for imaging and display fields; and can significantly optimize p / s polarization consistency in the infrared region, making it suitable for optical communication, infrared detection and laser systems.

[0049] Compared to the broadband low-polarization design of Example 1, this embodiment further provides design freedom and flexibility. By precisely controlling the thickness ratio of the protective layer Al2O3 to SiO2, high reflectivity can be maintained while achieving differentiated optimization of polarization sensitivity for different operating wavelengths, thereby meeting the needs of various complex application scenarios such as optical imaging, laser systems, and space exploration. The above results fully demonstrate that the thickness ratio control strategy provided in this embodiment can effectively expand the application space of low-polarization silver mirrors, giving them stronger optical adaptability and engineering application value.

[0050] Those skilled in the art will readily understand that the above description is merely a preferred embodiment of the present invention. The above embodiments are provided only for the purpose of describing the present invention and are not intended to limit the present invention. Parts not described in detail in this specification are well-known in the art and are not intended to limit the scope of the present invention. The scope of the present invention is defined by the appended claims. All equivalent substitutions and modifications made without departing from the spirit and principle of the present invention should be covered within the scope of the present invention.

Claims

1. A silver reflector with a wide incident angle range and low polarization sensitivity, characterized in that, The silver film of the wide incident angle range low polarization sensitivity silver reflector is provided with a double protective film structure. The double protective film structure includes a first dielectric protective film and a second dielectric protective film. The first dielectric protective film is in contact with the silver film. The first dielectric protective film is an Al2O3 film layer and the second dielectric protective film is a SiO2 film layer. The thickness of the second dielectric protective film makes the reflectivity of short-wavelength S-rays and P-rays tend to be the same. The total optical thickness of the first dielectric protective film and the second dielectric protective film is less than one-quarter of the short-wavelength, and the ratio of the physical thickness of the first dielectric protective film and the second dielectric protective film is less than 2:

5. Both the first and second dielectric protective films are dense, pinhole-free films deposited by atomic layer deposition.

2. The silver reflector with a wide incident angle range and low polarization sensitivity according to claim 1, characterized in that, The thickness of the silver film is 100-300 nm; the thickness of the first dielectric protective film is 4-20 nm; and the thickness of the second dielectric protective film is 20-50 nm.

3. The silver reflector with a wide incident angle range and low polarization sensitivity according to claim 1, characterized in that, The wide incident angle range, low polarization sensitivity silver reflector comprises, from bottom to top: a reflector body, an adhesive layer, a silver film, and a double-layer protective film structure.

4. The silver reflector with a wide incident angle range and low polarization sensitivity according to claim 3, characterized in that, The material of the reflector body is one of glass, fused silica, aluminum, titanium, surface-modified silicon carbide, and beryllium mirror.

5. The silver reflector with a wide incident angle range and low polarization sensitivity according to claim 3, characterized in that, The adhesive layer is a single film or a multilayer composite film formed of Al2O3, Ni, Cr, NiCr alloy, or NiCrN alloy. The thickness of the adhesive layer is 10-50 nm.

6. The fabrication process of the silver reflector with a wide incident angle range and low polarization sensitivity according to any one of claims 1 to 5, characterized in that, The silver film is deposited by room temperature vapor deposition, and the first dielectric protective film and the second dielectric protective film are deposited by atomic layer deposition.

7. The fabrication process of the silver reflector with a wide incident angle range and low polarization sensitivity according to claim 6, characterized in that, The adhesive layer is deposited by room temperature vapor deposition; The first dielectric protective film is deposited by thermal atomic layer deposition, and the second dielectric protective film is deposited by plasma-enhanced atomic layer deposition at a deposition temperature of 60-120℃.

8. The fabrication process of the silver reflector with a wide incident angle range and low polarization sensitivity according to claim 7, characterized in that, The fabrication process of the silver reflector with a wide incident angle range and low polarization sensitivity includes the following steps: S1: Pre-process the mirror body; S2: Argon ion bombardment treatment is performed on the pre-treated mirror body; S3: An adhesive layer is deposited on the mirror body after the process in step S2 by room temperature vapor deposition. S4: A silver film is deposited on the adhesive layer by room temperature vapor deposition; S5: A first dielectric protective film is deposited on the silver film using thermal atomic layer deposition; S6: A second dielectric protective film is deposited on the first dielectric protective film using plasma-enhanced atomic layer deposition.

9. The fabrication process of the silver reflector with a wide incident angle range and low polarization sensitivity according to claim 8, characterized in that, The pretreatment in step S1 specifically involves cleaning the mirror body; The argon ion bombardment treatment in step S2 has a bombardment time of 5 to 20 minutes, an anode voltage of 120 to 300 V, and an anode current of 2 to 10 A. The rate of room temperature evaporation in step S3 is 0.2~0.6 nm / s.

10. The fabrication process of the silver reflector with a wide incident angle range and low polarization sensitivity according to claim 8, characterized in that, The rate of room temperature evaporation in step S4 is 2~3 nm / s; The raw materials for thermal atomic layer deposition in step S5 are trimethylaluminum and water; The raw materials for plasma-enhanced atomic layer deposition in step S6 are bis(tert-butylamino)silane and oxygen.