A photonic computing chip and a method of fabricating the same

By employing a suspended structure in silicon-based photonic computing chips to block thermal crosstalk, the problems of thermal crosstalk and insufficient programmability are solved, enabling high-precision computing and flexible applications while reducing energy consumption and process complexity.

CN123156366APending Publication Date: 2026-11-24SHANDONG YUNHAI GUOCHUANG CLOUD COMPUTING EQUIP IND INNOVATION CENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611327154.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-28
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing silicon-based photonic computing chips suffer from thermal crosstalk, resonant wavelength shift, and large phase noise, and lack programmability, making it difficult to meet the needs of high-precision AI inference tasks and flexible applications.

Method used

An air gap is created between the cladding and heater layer above the microring resonator and the substrate, which blocks lateral heat conduction and allows the resonant wavelength to be tuned through the heater layer.

Benefits of technology

It effectively reduces thermal crosstalk, improves computational accuracy and programmability, reduces energy consumption and process complexity, enhances thermal management and the number of reconfigurable cells, and simplifies the packaging process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123156366A_ABST
    Figure CN123156366A_ABST
Patent Text Reader

Abstract

This application relates to the field of photonic integration and discloses a photonic computing chip and its fabrication method. The chip includes a substrate; a microring resonator disposed on the surface of the substrate; a cladding layer disposed on a portion of the ring region of the microring resonator and disposed along the direction of the inner connection line of the microring resonator; and a heater layer disposed on the surface of the cladding layer. The cladding layer and the heater layer form a suspended structure above the microring resonator, and an air gap exists between the suspended structure and the upper surface of the substrate. By forming a suspended structure for the cladding layer and the heater layer, thermal crosstalk between adjacent microring resonators can be reduced, the probability of passive wavelength shift can be reduced, heat loss to the substrate can be reduced, and the thermal efficiency of the heater layer can be improved. Furthermore, the reduction in thermal crosstalk allows for dense integration of microheaters without the need for an additional thermal isolation layer, increasing the number of reconfigurable units while reducing process complexity and production costs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of photonic integration, and in particular to a photonic computing chip and its fabrication method. Background Technology

[0002] With the ever-increasing demand for computing power from applications such as artificial intelligence, big data processing, and high-performance computing, traditional electronic computing architectures are facing increasingly severe bottlenecks in terms of power consumption, bandwidth, and parallel processing capabilities. Photonic computing, with its ultra-high speed and ultra-low power consumption of optical signal transmission and the high parallelism supported by wavelength division multiplexing (WDM) technology, is considered one of the important technological paths to overcome these bottlenecks. Silicon Photonic Integrated Circuits (SiPICs), relying on mature CMOS (Complementary Metal Oxide Semiconductor) planar manufacturing processes, can achieve high-density integration of photonic devices at a controllable cost, showing broad application prospects in optical communication, optical interconnection, and optical sensing.

[0003] Microring resonators (MRRs) are core functional components in silicon-based photonic integrated circuits. Due to their compact structure, ease of large-scale integration, and inherent support for wavelength division multiplexing (WDM), they are widely used to construct weight adjustment and signal processing units in photonic computing chips. Utilizing the thermo-optical effect of silicon, thermo-optical tuning of the MRR's resonant wavelength via a microheater is a primary technique for realizing programmable photonic computing. However, this approach still faces bottlenecks in practical applications.

[0004] First, in silicon-based photonic chips, multiple resonant resonators (MRRs) are densely integrated on the same substrate. The heat generated by a single microheater can be conducted to neighboring MRRs through the substrate, causing a passive shift in the resonant wavelength. Simultaneously, process fluctuations in silicon planar manufacturing, such as etching depth deviations, uneven film thickness, and temperature drift, further exacerbate the resonant wavelength shift and increase phase noise. These factors collectively lead to the accumulation of computational errors, making it difficult to meet the stringent weight accuracy requirements of high-precision AI inference tasks. Existing technologies can mitigate thermal crosstalk by using an external heating isolation layer. However, thermal isolation layers often require additional chip area and increase process complexity. Second, photonic chips lack programmability. Most existing MRR-based photonic chips employ a fixed functional architecture. Once manufactured, their computational topology and configuration parameters are fixed, making dynamic reconstruction difficult for different computational tasks (such as CNNs (Convolutional Neural Networks) and RNNs (Recurrent Neural Networks), severely limiting the chip's versatility and application flexibility.

[0005] Therefore, how to solve the above-mentioned technical problems should be a key focus for those skilled in the art. Summary of the Invention

[0006] The purpose of this application is to provide a photonic computing chip and its fabrication method to effectively reduce thermal crosstalk of micro-ring resonators, achieve high precision, low error, and programmable tuning of the photonic computing chip, while reducing process complexity and production costs.

[0007] To address the aforementioned technical problems, this application provides a photonic computing chip, comprising: Substrate; A microring resonator disposed on the surface of the substrate; The cladding is disposed in a portion of the ring region of the microring resonator and along the direction of the internal connection line of the microring resonator. A heater layer disposed on the surface of the cladding; The cladding layer and the heater layer form a suspended structure above the microring resonator, and there is an air gap between the suspended structure and the upper surface of the substrate.

[0008] Alternatively, the heater layer may include a first heater film and a second heater film; The first heater film is disposed on the surface of the cladding located in the ring region of the microring resonator; The second heater film is disposed along the inner connection line of the microring resonator and is connected to the first heater film.

[0009] Alternatively, the thickness of the second heater film may be greater than the thickness of the first heater film.

[0010] Alternatively, the cladding disposed on a portion of the ring region of the microring resonator is distributed symmetrically about the center of the microring resonator.

[0011] This application also provides a method for fabricating a photonic computing chip, comprising: Fabricate a microring resonator on the surface of a substrate; A sacrificial layer is deposited on the surface of the substrate and the microring resonator, and a growth window is opened on the sacrificial layer at a position corresponding to a portion of the ring region of the microring resonator; A cladding layer is grown within the growth window and above the inner ring connection of the microring resonator. A heater layer is grown on the upper surface of the cladding; The sacrificial layer is removed so that the cladding and the heater layer form a suspended structure above the microring resonator, with an air gap between the suspended structure and the upper surface of the substrate.

[0012] Alternatively, growing a heater layer on the upper surface of the cladding includes: A patterned photoresist layer is formed on the surface of the cladding layer and the sacrificial layer; A heater layer material is grown on the surface of the patterned photoresist layer and the cladding layer located within the growth window; The patterned photoresist layer and the heater layer material located on the patterned photoresist layer are peeled off to form a first heater film; A patterned photoresist layer is formed on the surface of the first heater film and the sacrificial layer; A heater layer material is grown on the surface of the patterned photoresist layer and the cladding layer located above the inner ring connection of the microring resonator; The patterned photoresist layer and the heater layer material located on the patterned photoresist layer are peeled off to form a second heater film.

[0013] Alternatively, when growing the heater layer material, the growth method is magnetron sputtering, the target material is a titanium target, the sputtering gas includes argon and nitrogen, the flow ratio of argon and nitrogen is in the range of 4:1 to 9:1, and the sputtering temperature is lower than the softening point temperature of the sacrificial layer.

[0014] Alternatively, growing a cladding layer within the growth window and above the inner ring connection of the microring resonator includes: A cladding layer is grown within the growth window and above the inner ring line of the microring resonator using plasma-enhanced deposition. The reaction gases include silane and nitrous oxide, with a flow ratio of silane to nitrous oxide ranging from 10:1 to 70:1. The radio frequency power ranges from 30W to 70W, and the reaction temperature ranges from 150℃ to 300℃.

[0015] Alternatively, depositing a sacrificial layer on the surfaces of the substrate and the microring resonator includes: Phosphosilicate glass or borosilicate glass is deposited on the surfaces of the substrate and the microring resonator to form a sacrificial layer.

[0016] Alternatively, removing the sacrificial layer may include: The sacrificial layer is etched using a hydrofluoric acid solution or a buffered oxide etchant.

[0017] This application constructs a suspended structure for the cladding and heater layers, with an air gap between them and the substrate. Due to the extremely low thermal conductivity of air, this suspended structure effectively blocks the lateral conduction of heat generated by the heaters to adjacent areas via the substrate. This significantly reduces thermal crosstalk between adjacent micro-ring resonators, decreases the probability of passive wavelength shift, and reduces the accumulation of computational errors, thus improving the weight configuration accuracy and overall computational accuracy of the photonic computing chip. Simultaneously, the suspended structure concentrates heat within the micro-ring resonator region, reducing heat loss to the substrate and improving the thermal efficiency of the heater layer. This results in lower power consumption required to achieve the same tuning effect, contributing to a reduction in the chip's overall energy consumption. The reduction in thermal crosstalk and the improvement in thermal efficiency further enhance tuning accuracy, while improved thermal stability effectively reduces errors. Furthermore, the reduction in thermal crosstalk allows for dense integration of micro-heaters without the need for additional thermal isolation layers, significantly increasing the number of reconfigurable units. The suspended structure also optimizes thermal management, eliminating the need for complex thermal isolation layers during packaging. This simplifies the packaging and testing process, reduces process complexity and production costs, and facilitates the industrial-scale mass production of photonic computing chips. In addition, the heat generated by the heater layer is concentrated on both sides of the micro-ring resonator ring, making thermal regulation more controllable, thus improving the programmability of the photonic computing chip.

[0018] In addition, this application also provides a preparation method with the above advantages. Attached Figure Description

[0019] To more clearly illustrate the technical solutions of the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0020] Figure 1 This is a schematic diagram of the structure of a photonic computing chip provided in an embodiment of this application; Figure 2 A cross-sectional schematic diagram of a photonic computing chip provided in an embodiment of this application; Figure 3 This is a top view schematic diagram of a photonic computing chip provided in an embodiment of this application; Figure 4 This is a flowchart illustrating a method for fabricating a photonic computing chip according to an embodiment of this application. Figures 5 to 15 This is a process flow diagram of the fabrication of a photonic computing chip provided in an embodiment of this application; Figure reference numerals: 1. Substrate, 2. Microring resonator, 3. Cladding, 4. Heater layer, 5. Air gap, 6. Silicon layer, 7. Sacrificial layer, 8. Growth window, 9. Silicon dioxide layer, 10. Patterned photoresist layer. Detailed Implementation

[0021] To enable those skilled in the art to better understand the present application, the present application will be further described in detail below with reference to the accompanying drawings and specific embodiments. Obviously, the described embodiments are merely some embodiments of the present application, and not all embodiments. Based on the embodiments in this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.

[0022] Many specific details are set forth in the following description in order to provide a full understanding of the invention. However, the invention may also be practiced in other ways different from those described herein, and those skilled in the art can make similar extensions without departing from the spirit of the invention. Therefore, the invention is not limited to the specific embodiments disclosed below.

[0023] As described in the background section, existing photonic computing chips suffer from problems such as thermal crosstalk, resonant wavelength shift, large phase noise, and insufficient programmability.

[0024] In view of this, this application provides a photonic computing chip, please refer to... Figures 1 to 3 It can include: Substrate 1; Micro-ring resonator 2 disposed on the surface of substrate 1; The cladding 3 is disposed in a portion of the ring region of the microring resonator 2 and along the direction of the inner ring connection of the microring resonator 2. Heater layer 4 disposed on the surface of cladding 3; The cladding layer 3 and the heater layer 4 form a suspended structure above the micro-ring resonator 2, and there is an air gap 5 between the suspended structure and the upper surface of the substrate 1.

[0025] Substrate 1 serves as the structural support base for the photonic computing chip. In some embodiments of this application, the material of substrate 1 can be silicon dioxide (SiO2). Exemplarily, a silicon dioxide layer can be grown on a silicon substrate using a thermal oxidation method as substrate 1. The thickness of this silicon dioxide layer can be on the order of micrometers to ensure sufficient mechanical strength and flatness. Of course, substrate 1 can also be made of other insulating materials with appropriate mechanical strength and thermal stability, as long as they can meet the support requirements and process compatibility requirements of the photonic computing chip during operation.

[0026] The micro-ring resonator 2 is a ring resonant structure made of silicon-based waveguides. It is a core functional component in the photonic computing chip and is used to realize functions such as resonance enhancement and wavelength selection of optical signals. Its resonant wavelength can be shifted with temperature, so the thermo-optic effect can be used for tunable operation.

[0027] In some embodiments of this application, the microring resonator 2 can be implemented by fabricating a silicon layer on the surface of the substrate 1 and etching it to form a ring waveguide. In some embodiments of this application, the thickness of the silicon layer can be 220 nm.

[0028] The micro-ring resonator 2 has a planar closed-loop waveguide structure. Optical signals propagate within the ring in a whispering-gallery mode. Optical signals satisfying the resonance condition undergo coherent enhancement within the ring, while non-resonant signals are suppressed or transmitted. The diameter and ring width of the micro-ring resonator 2 can be designed according to the target resonant wavelength and coupling efficiency requirements; this application does not impose specific limitations on these aspects.

[0029] The cladding 3 located in the partial ring region of the microring resonator 2 comprises two independent parts, and the cladding 3 arranged along the inner ring connection direction of the microring resonator 2 is connected to these two independent cladding parts.

[0030] The function of cladding 3 is to maintain optical field confinement and provide optical isolation buffer for subsequent metal heater processes.

[0031] In some embodiments of this application, the cladding 3 may be made of materials such as silicon dioxide. The cladding 3 covers a portion of the ring area of ​​the microring resonator 2 and extends along the internal connection direction of the microring resonator 2. The internal connection direction refers to the direction of the connection path leading from the ring area of ​​the microring resonator 2 into the interior of the microring.

[0032] The heater layer 4 can generate Joule heat when energized, and conduct it to the micro-ring resonator 2 through the cladding layer 3. This allows the effective refractive index of the micro-ring resonator 2 to be changed by utilizing the thermo-optical effect of silicon material, thereby achieving tuning of the resonant wavelength.

[0033] In some embodiments of this application, the material of heater layer 4 can be titanium nitride (TiN). Titanium nitride has advantages such as good chemical stability, strong resistance to electromigration, and compatibility with CMOS processes, making it suitable as a heater material in photonic computing chips. Of course, other conductive thin film materials can also be used for heater layer 4, such as doped polycrystalline silicon, tungsten, platinum, etc.

[0034] The cladding layer 3 and the heater layer 4 have a consistent pattern distribution in planar space. That is, in the direction perpendicular to the surface of the substrate 1, the planar projection pattern of the cladding layer 3 and the planar projection pattern of the heater layer 4 are basically coincident.

[0035] The suspended structure refers to the fact that there is no solid contact support between the cladding layer 3 and the heater layer 4 above the micro-ring resonator 2 and the substrate 1. Instead, the cladding layer 3 is connected to the surrounding structure through both ends, so that the cladding layer 3 and the heater layer 4 are suspended above the micro-ring resonator 2.

[0036] The air gap 5 located between the suspended structure and the upper surface of the substrate 1 serves as thermal insulation. In some embodiments of this application, the height of the air gap 5 is determined by the thickness of the sacrificial layer and can be adjusted according to actual design requirements; for example, the height of the air gap 5 can be from hundreds of nanometers to several micrometers. The suspended structure can be formed as follows: after fabricating the microring resonator 2, a sacrificial layer is first deposited, then a cladding layer 3 and a heater layer 4 are fabricated on the sacrificial layer, and finally the sacrificial layer is removed to form the air gap 5.

[0037] In this embodiment, the suspended structure blocks the heat conduction path between the heater layer 4 and the substrate 1 via an air gap 5. Air has a low thermal conductivity (approximately 0.024 W / (m·K)), which significantly improves thermal isolation compared to solid materials (such as silicon dioxide, which has a thermal conductivity of approximately 1.4 W / (m·K)). Therefore, the heat generated by the heater layer 4 cannot diffuse outward through the substrate 1 but is concentrated in the micro-ring resonator 2 region. On the one hand, this reduces thermal crosstalk between a single micro-heater and adjacent micro-ring resonators 2, reducing the passive resonant wavelength shift caused by thermal conduction in adjacent micro-ring resonators 2, thus providing a basis for high-precision weighting configuration. On the other hand, the concentrated heat reduces heat loss to the substrate 1, improving thermal efficiency and reducing the overall power consumption of the photonic computing chip. The reduction in thermal crosstalk and the improvement in thermal efficiency jointly improve tuning accuracy, while the improvement in thermal stability effectively reduces computational errors.

[0038] In this application, the photonic computing chip can be used as a programmable linear computing unit in an optical computing chip, or as a light source or nonlinear computing unit.

[0039] In this embodiment, the cladding layer 3 and heater layer 4 are configured into a suspended structure, with an air gap 5 between them and the substrate 1. Due to the extremely low thermal conductivity of air, this suspended structure effectively blocks the lateral conduction of heat generated by the heater to adjacent areas via the substrate 1. This significantly reduces thermal crosstalk between adjacent micro-ring resonators 2, decreases the probability of passive wavelength shift, and reduces the accumulation of computational errors, thus improving the weight configuration accuracy and overall computational accuracy of the photonic computing chip. Simultaneously, the suspended structure concentrates heat within the micro-ring resonator 2 region, reducing heat loss to the substrate 1 and improving the thermal efficiency of the heater layer 4. This results in lower power consumption required to achieve the same tuning effect, contributing to a reduction in the chip's overall energy consumption. The reduction in thermal crosstalk and the improvement in thermal efficiency further enhance tuning accuracy, while improved thermal stability effectively reduces errors. Furthermore, the reduction in thermal crosstalk allows for dense integration of micro-heaters without the need for additional thermal isolation layers, significantly increasing the number of reconfigurable units. The suspended structure also optimizes thermal management, eliminating the need for complex thermal isolation layers during packaging. This simplifies the packaging and testing process, reduces process complexity and production costs, and facilitates the industrial-scale mass production of photonic computing chips. Furthermore, the heat generated by heater layer 4 is concentrated on both sides of the micro-ring resonator 2, making thermal control more precise and thus enhancing the programmability of the photonic computing chip.

[0040] Based on the above embodiments, in one embodiment of this application, the heater layer 4 includes a first heater film 41 and a second heater film 42; the first heater film 41 is disposed on the surface of the cladding 3 located in the ring region of the microring resonator 2; the second heater film 42 is disposed along the inner ring connection direction of the microring resonator 2 and connected to the first heater film 41.

[0041] The cladding 3 covers a portion of the ring region of the microring resonator 2, so the position of the first heater film 41 on the surface of the cladding 3 in this portion of the ring region corresponds to the ring region of the microring resonator 2.

[0042] The first heater film 41 is used to directly heat and tune the microring resonator 2. When the first heater film 41 is energized, the current flows in the film, generating Joule heating. The heat is conducted to the microring resonator 2 through the underlying cladding 3, causing the temperature of the microring resonator 2 to rise. This, in turn, utilizes the thermo-optical effect of silicon material to change its effective refractive index, thereby achieving tuning of the resonant wavelength. The shape of the first heater film 41 in its planar structure corresponds to the ring region of the microring resonator 2.

[0043] Since the cladding 3 on the partial ring comprises two parts, the first heater also comprises two independent parts. The second heater film 42 is arranged along the inner connection direction of the micro-ring resonator 2, and its two ends are respectively connected to the first heater film 41. Since the second heater film 42 is also made of a conductive material (e.g., titanium nitride), it also has resistance and generates Joule heat when energized. Therefore, the second heater film 42 can provide auxiliary heating to the internal region of the micro-ring resonator 2 while serving as an electrical connection.

[0044] In some embodiments of this application, the first heater film 41 and the second heater film 42 can be made of the same material (e.g., titanium nitride) to ensure good interface contact between the two and reduce contact resistance.

[0045] In this embodiment, by setting a first heater film 41 and a second heater film 42, the second heater film 42 is set along the inner connection direction of the ring and connected to the first heater film 41, forming a complete electrical path, so that the external driving circuit can supply power to the first heater film 41 located in the region on the micro ring through the second heater film 42. At the same time, the second heater film 42 itself can also provide auxiliary heating, increasing the heating uniformity of the heater layer 4.

[0046] It should be noted that this application does not limit the thickness relationship between the first heater film 41 and the second heater film 42, and can be set by the user.

[0047] In some embodiments of this application, the thickness of the second heater film 42 may be greater than the thickness of the first heater film 41.

[0048] The first heater film 41 is directly disposed on the ring region of the microring resonator 2, and its thickness determines the heating efficiency and resistance value of the heater layer 4. Since the first heater film 41 is located directly above the microring resonator 2, the heat it generates needs to be conducted through the cladding 3 to the microring resonator 2. Therefore, the thickness of the first heater film 41 should not be too thick to ensure that heat can be quickly and responsively transferred to the microring resonator 2. Exemplarily, in some embodiments of this application, the thickness of the first heater film 41 can be 50 nm.

[0049] The second heater film 42 is disposed along the inner connection direction of the ring, and one of its main functions is to transmit external electrical signals from the inner region of the micro-ring to the first heater film 41. Since the connection path of the second heater film 42 is relatively long, in order to reduce its resistance and thus reduce unnecessary power loss and heat generation (except for auxiliary heating requirements), the thickness of the second heater film 42 can be set to be greater than that of the first heater film 41. A thicker second heater film 42 has lower sheet resistance, enabling the transmission of electrical signals from the outside to the first heater film 41 with a smaller voltage drop, thereby improving the efficiency of electrical power utilization. At the same time, a thicker second heater film 42 also has better mechanical strength and resistance to electromigration, which is beneficial to improving the long-term reliability of the device. Exemplarily, in some embodiments of this application, the thickness of the second heater film 42 can be 350 nm.

[0050] In this embodiment, the thickness of the second heater film 42 is greater than that of the first heater film 41, so that the first heater film 41 located in the ring region can maintain a good heating response speed and heating efficiency, while the second heater film 42 located in the inner connection direction of the ring can realize the transmission of electrical signals with lower resistance. The difference in thickness between the two takes into account the different requirements of heating function and conductive connection function, which is beneficial to reduce overall power consumption and improve the reliability of the device.

[0051] Based on any of the above embodiments, in some embodiments of this application, in the photonic computing chip, the cladding 3 disposed on a portion of the ring region of the microring resonator 2 is symmetrically distributed about the center of the microring resonator 2.

[0052] The cladding 3 does not cover the entire circumference of the microring resonator 2, but only a portion of the ring area. This portion of the ring area is symmetrically distributed about the center of the microring resonator 2; that is, the cladding 3 occupies multiple discrete segments on the circumference of the microring, and these segments are centrally symmetrical with respect to the center of the microring. For example, the cladding 3 may occupy two symmetrical arc segments at the top and bottom of the microring, two symmetrical arc segments on the left and right sides of the microring, or one symmetrical arc segment in each of the four quadrants of the microring. The symmetrical distribution of the cladding 3 ensures that the heater layer 4 located on the surface of the cladding 3 is also symmetrically distributed.

[0053] The heating effect of heater layer 4 on microring resonator 2 depends on its distribution and coverage area on the microring. When heater layer 4 is symmetrically distributed with respect to the center of the microring, the resulting thermal field is symmetrically distributed on the microring, and the thermal effect on each location of the microring resonator 2 tends to be uniform. This symmetrical thermal field distribution is beneficial for the better stability and consistency of the resonant wavelength tuning of the microring resonator 2, avoiding the problem of uneven resonant wavelength shift caused by local overheating or insufficient local temperature. In addition, the symmetrical structural design also facilitates the drawing of photolithography patterns and process implementation, which is beneficial for improving manufacturing accuracy.

[0054] In this embodiment, the cladding 3 is symmetrically distributed about the center of the micro-ring resonator 2, so that the heating effect of the heater layer 4 on the micro-ring resonator 2 is symmetrical, which is beneficial to improving the tuning accuracy and thermal field uniformity.

[0055] This application also provides a method for fabricating a photonic computing chip; please refer to [reference needed]. Figure 4 The method may include: Step S101: Fabricate a microring resonator on the surface of the substrate.

[0056] For example, a layer of silicon dioxide can be grown on a silicon substrate using a thermal oxidation method, and the thickness of the silicon dioxide layer can be on the order of micrometers.

[0057] One way to fabricate a microring resonator on a substrate is to first form a silicon layer on the substrate, and then pattern the silicon layer into a ring waveguide structure of the microring resonator through photolithography and etching processes.

[0058] The silicon layer can be formed using molecular beam epitaxy (MBE) or chemical vapor deposition (CVD) techniques. By precisely controlling epitaxial process parameters (such as temperature, gas flow rate, and deposition time), the uniformity of the silicon layer thickness can be ensured. In some embodiments of this application, the silicon layer thickness can be 220 nm. After the silicon layer is formed, photoresist is spin-coated onto the silicon layer. Following exposure and development processes, the pattern of the microring resonator is defined on the photoresist layer. Then, etching techniques are used to remove the silicon regions not protected by the photoresist, forming the microring resonator structure.

[0059] In some embodiments of this application, the etching process can employ inductively coupled plasma (ICP) etching technology. The etching gas can be a fluorine-containing gas, such as a mixture of C4F8, SF6, and O2, wherein the flow ratio of C4F8 to SF6 can be controlled within the range of 3:1 to 3:4. The RF power can be 0 to 500W, and the bias voltage can be 50 to 300V. Specific etching conditions can be adjusted according to specific circumstances. After etching, residual photoresist is removed. In other embodiments of this application, electron beam direct writing or other photolithography methods can also be used to define the micro-ring pattern; this application does not specifically limit this method.

[0060] Step S102: Deposit a sacrificial layer on the surface of the substrate and the microring resonator, and open growth windows on the sacrificial layer at positions corresponding to the portion of the ring region of the microring resonator.

[0061] The sacrificial layer is a temporary support layer used to form the air gap. Its material should have different etching selectivity than the cladding and heater layer materials so that it can be selectively removed in subsequent processes without damaging the cladding and heater layers.

[0062] The thickness of the sacrificial layer determines the height of the subsequent air gap, which can be adjusted according to actual design requirements, for example, from hundreds of nanometers to several micrometers.

[0063] After the sacrificial layer is deposited, planarization can be performed to ensure that the subsequent cladding and heater layers have a smooth surface.

[0064] After the sacrificial layer is deposited, the location of the growth window is defined on the sacrificial layer using photolithography. This growth window corresponds to a portion of the on-ring region of the microring resonator. Then, an etching process is used to remove the sacrificial layer at the location of the growth window, exposing a portion of the on-ring region of the underlying microring resonator, so that the subsequent cladding layer can grow in this region and contact the microring resonator. The size and shape of the growth window can be determined according to the design pattern of the cladding layer. In some embodiments of this application, the growth windows can be symmetrically distributed about the center of the microring resonator.

[0065] It should be noted that this application does not specifically limit the sacrificial layer, which can be set by the user.

[0066] In some embodiments of this application, depositing a sacrificial layer on the surfaces of the substrate and the microring resonator includes: Phospho-sillicate glass (PSG) or boro-phospho-sillicate glass (BPSG) is deposited on the surfaces of the substrate and the microring resonator to form a sacrificial layer.

[0067] PSG and BPSG have the following advantages as sacrificial layer materials: First, PSG and BPSG can be deposited using conventional chemical vapor deposition techniques (such as low-pressure chemical vapor deposition or PECVD), which are mature processes and produce films with good uniformity. Second, the etching characteristics of PSG and BPSG are different from those of silicon dioxide. The etching rates of PSG and BPSG in hydrofluoric acid solutions or buffered oxide etching solutions are significantly higher than those of undoped silicon dioxide, so they can be easily selectively removed by wet etching.

[0068] Step S103: Grow a cladding layer within the growth window and above the inner ring connection of the microring resonator.

[0069] The cladding material can be silicon dioxide.

[0070] It should be noted that this application does not limit the growth method of the cladding; the method can be chosen freely.

[0071] In some embodiments of this application, growing a cladding layer within the growth window and above the inner ring connection of the microring resonator includes: Plasma-enhanced deposition is used to grow a cladding layer within the growth window and above the inner ring connection of the microring resonator. The reaction gases include silane and nitrous oxide, with a flow ratio of silane to nitrous oxide ranging from 10:1 to 70:1. The radio frequency power ranges from 30W to 70W, and the reaction temperature ranges from 150℃ to 300℃.

[0072] Plasma-enhanced chemical vapor deposition (PECVD) technology can deposit high-quality silicon dioxide thin films at lower temperatures, which helps to avoid thermal damage to existing device structures. It also has advantages such as high film density, good step coverage, moderate deposition rate, and good compatibility with photolithography processes.

[0073] For example, the flow ratio of silane (SiH4) and nitrous oxide (N2O) can be 10:1, 20:1, 30:1, 40:1, 50:1, 60:1 or 70:1, etc., the radio frequency power can be 30W, 40W, 50W, 60W or 70W, etc., and the reaction temperature can be 150℃, 180℃, 200℃, 250℃ or 300℃, etc.

[0074] Silane is used as the silicon source, and nitrous oxide as the oxygen and nitrogen sources, respectively. Under plasma irradiation, they undergo a chemical reaction to form a silicon dioxide thin film. The flow ratio of silane to nitrous oxide affects the deposition rate, refractive index, density, and stress characteristics of the silicon dioxide film. When the flow ratio of silane to nitrous oxide is in the range of 10:1 to 70:1, the deposited silicon dioxide film can be guaranteed to have appropriate quality and optical properties. The radio frequency power range is 30W to 70W, which affects the plasma density and energy, thus influencing the deposition rate and density of the film. The reaction temperature range is 150℃ to 300℃. PECVD technology can deposit films at relatively low temperatures, which helps to avoid thermal damage to existing device structures (such as microring resonators) and also avoids thermal impact on the sacrificial layer.

[0075] When growing the cladding using PECVD technology, the silicon dioxide cladding of the designed thickness can be obtained under the above process conditions. After the cladding growth is complete, photolithography and etching processes are performed on the cladding to remove unwanted cladding material, retaining the cladding pattern located within the growth window and above the ring connection direction of the microring resonator. The cladding contacts the ring region of the microring resonator within the growth window, providing electrical isolation and structural support for the subsequent fabrication of the heater layer.

[0076] The thickness of the silica cladding can be determined according to design requirements, ranging from hundreds of nanometers to several micrometers. After the cladding is grown, annealing can be performed to improve the film density and optical uniformity.

[0077] Step S104: Grow a heater layer on the upper surface of the cladding.

[0078] The material of the heater layer should have good electrical conductivity and thermal stability, and be able to generate Joule heat when energized.

[0079] In some embodiments of this application, the material of the heater layer can be titanium nitride (TiN) or the like. The heater layer can be grown using physical vapor deposition techniques, such as magnetron sputtering.

[0080] During the growth of the heater layer, a patterned photoresist layer is first formed on the surfaces of the cladding and sacrificial layers. This patterned photoresist layer has openings at the locations where the heater layer needs to be grown. Then, the heater layer material is grown on the patterned photoresist layer and the exposed cladding surface. Finally, the patterned photoresist layer and the heater layer material above it are stripped off, and the remaining heater layer material is the patterned heater layer. The heater layer is located on the upper surface of the cladding, and its pattern corresponds to the pattern of the cladding.

[0081] Step S105: Remove the sacrificial layer to form a suspended structure above the microring resonator with the cladding and heater layers, and an air gap between the suspended structure and the upper surface of the substrate.

[0082] Because of the etching selectivity between the sacrificial layer material and the cladding and heater layer materials, an etchant with a high etching rate for the sacrificial layer and a low etching rate for the cladding and heater layers can be used to remove the sacrificial layer. After the sacrificial layer is removed, the space originally occupied by the sacrificial layer becomes an air gap, and the cladding and heater layers are suspended above the microring resonator, connected to the substrate only through the edge of the cladding.

[0083] The specific method for removing the sacrificial layer can be determined based on the material of the sacrificial layer, and no specific limitation is made in this application.

[0084] In some embodiments of this application, when the sacrificial layer is PSG or BPSG, removing the sacrificial layer includes etching the sacrificial layer using a hydrofluoric acid solution or a buffered oxide etchant.

[0085] Hydrofluoric acid (HF) solution can be a diluted aqueous solution of hydrofluoric acid with a volume concentration of 1% to 10%.

[0086] Buffered oxide etchant (BOE) is a mixed solution of hydrofluoric acid and ammonium fluoride (NH4F), such as a BOE solution with a volume ratio of NH4F to HF of 6:1. Buffered oxide etchant maintains a stable pH value through the buffering effect of ammonium fluoride, resulting in a more uniform and controllable etching rate, which is beneficial for obtaining a smooth etched surface.

[0087] Selective etching using hydrofluoric acid solution or buffered oxide etchant removes the sacrificial layer, creating a suspended structure while protecting the cladding and heater layers, providing thermally isolated air gaps for the photonic computing chip. This removal method is simple, easy to control, and suitable for mass production.

[0088] In some embodiments of this application, a packaging and testing process is performed after the microring resonator is fabricated.

[0089] Wafer-level testing and characterization: Optical frequency domain reflectance characterization technology can be used to test the wafer, obtaining the distance-domain propagation curve of the optical signal in the microring resonator. Spectral line analysis can then be used to quickly extract the frequency response and propagation loss characteristics of the microring, and the resonant wavelength shift can be extracted, thereby verifying whether the tuning capability of the microheater meets design expectations. If the test results do not meet the requirements, corresponding adjustments or compensations can be made in subsequent processes.

[0090] For suspended microheater structures, special handling methods are required during packaging to prevent damage. For example, a temporary protective layer can be used to cover the suspended structure before packaging to prevent mechanical damage or contamination during subsequent processes. Then, a flip-chip packaging method can be used, placing the chip's input / output terminals downwards to prevent the suspended structure from being subjected to external pressure during packaging. Low-stress packaging materials can be selected to reduce the adverse effects of packaging stress on the microheater. Micro-grating couplers can also be designed on the surface of the microring resonator chip to achieve self-aligned coupling between the optical fiber and the microring waveguide. During packaging, a high-precision automatic alignment system is used to precisely align the optical fiber and the microring waveguide to reduce optical coupling loss.

[0091] After packaging, the performance of the microheater needs to be tested. For example, the power consumption and temperature stability of the microheater can be evaluated by measuring the resonant wavelength tuning range and tuning speed of the microring resonator under different power input conditions. A closed-loop calibration system can also be designed to compensate for resonant wavelength deviations caused by process variations through calibration algorithms, thereby further improving the computational accuracy and reliability of the photonic computing chip.

[0092] In this embodiment, a suspended structure is formed using a sacrificial layer process. An air gap thermally isolates the heater layer from the substrate, reducing thermal crosstalk and improving thermal efficiency, thereby enhancing the computational accuracy of the photonic computing chip. This fabrication method is based on silicon planar manufacturing processes, is compatible with CMOS processes, and is suitable for mass production.

[0093] Based on the above embodiments, in one embodiment of this application, the method for fabricating a photonic computing chip may include: Step S201: Fabricate a microring resonator on the surface of the substrate.

[0094] Step S202: Deposit a sacrificial layer on the surface of the substrate and the microring resonator, and open growth windows on the sacrificial layer at positions corresponding to the portion of the ring region of the microring resonator.

[0095] Step S203: Grow a cladding layer within the growth window and above the inner ring connection of the microring resonator.

[0096] Step S204: Form a patterned photoresist layer on the surface of the cladding and sacrificial layers.

[0097] The patterned photoresist layer is formed by spin-coating photoresist, exposure and development processes, and has an opening at the location where the first heater film needs to be fabricated. The pattern of the opening is consistent with the design pattern of the first heater film.

[0098] Step S205: Growing heater layer material on the surface of the patterned photoresist layer and the cladding layer located within the growth window.

[0099] After the heater layer material is grown, it covers both the upper surface of the patterned photoresist layer and the surface of the cladding layer exposed in the opening. In some embodiments of this application, the heater layer material can be grown by magnetron sputtering. Magnetron sputtering is a physical vapor deposition technique that uses high-energy particles to bombard the surface of a target, causing target atoms to be sputtered and deposited on the substrate surface to form a thin film. In some embodiments of this application, the target can be a titanium target, and the sputtering gas can include argon (Ar) and nitrogen (N2), where argon is used to generate plasma, and nitrogen is used to react with titanium to generate titanium nitride.

[0100] It should be noted that the growth process of the heater layer material is not limited in this application and depends on the specific circumstances.

[0101] In some embodiments of this application, when growing the heater layer material, the growth method is magnetron sputtering, the target material is a titanium target, the sputtering gas includes argon and nitrogen, the flow ratio of argon and nitrogen is in the range of 4:1 to 9:1, and the sputtering temperature is lower than the softening point temperature of the sacrificial layer.

[0102] For example, the flow ratio of argon to nitrogen can be 4:1, 5:1, 6:1, 7:1, 8:1, or 9:1, etc.

[0103] The sputtering temperature should be controlled below the softening point temperature of the sacrificial layer to prevent softening, flow, or decomposition of the sacrificial layer during the growth of the heater layer material, thereby avoiding damage to the sacrificial layer pattern or contamination of subsequent processes. For example, when the sacrificial layer is PSG or BPSG, its softening point temperature is typically above 800°C, while the process temperature of magnetron sputtering can usually be controlled at a lower temperature (e.g., 200°C to 400°C). Therefore, by selecting appropriate sputtering power and cooling methods, the sputtering temperature can be ensured to be below the softening point temperature of the sacrificial layer.

[0104] In the sputtering gas, argon is used as the working gas to maintain plasma discharge, while nitrogen is used as the reactant gas to react with titanium to form titanium nitride. The flow ratio of argon to nitrogen can be adjusted within the range of 4:1 to 9:1. A relatively high argon flow rate results in a higher plasma density and a higher sputtering rate; a relatively high nitrogen flow rate increases the nitrogen content in the titanium nitride film, leading to a corresponding change in the film's resistivity. By adjusting the flow ratio of argon and nitrogen, the composition and resistivity of the titanium nitride film can be controlled to meet the design requirements of the heater layer.

[0105] The heater layer material is grown by magnetron sputtering. Titanium nitride thin films are prepared by reactive sputtering of a titanium target with argon and nitrogen. The resistivity of the film can be adjusted by controlling the flow ratio of argon and nitrogen. By controlling the sputtering temperature below the softening point of the sacrificial layer, damage to the sacrificial layer during the process can be avoided, which helps to ensure the quality of the heater layer and the integrity of the device structure.

[0106] Step S206: Peel off the patterned photoresist layer and the heater layer material located on the patterned photoresist layer to form a first heater film.

[0107] During the stripping process, a suitable stripping solution is used to dissolve the patterned photoresist layer, thereby removing the heater layer material located above the patterned photoresist layer. The heater layer material located on the cladding surface is retained, forming the first heater film. The first heater film is located on the cladding surface of the ring region of the microring resonator.

[0108] Step S207: A patterned photoresist layer is formed on the surface of the first heater film and the sacrificial layer.

[0109] In this step, the patterned photoresist layer is used to define the pattern of the second heater film. It has an opening at the location where the second heater film needs to be fabricated, and the opening is located above the direction of the inner connection line of the microring resonator.

[0110] Step S208: Growing heater layer material on the surface of the patterned photoresist layer and the cladding layer located above the inner loop connection of the microring resonator.

[0111] Similar to the steps described above, the heater layer material is grown to cover the patterned photoresist layer and the surface of the cladding exposed in the opening.

[0112] Step S209: Peel off the patterned photoresist layer and the heater layer material located on the patterned photoresist layer to form a second heater film.

[0113] After peeling, the heater layer material on the cladding surface remains, forming a second heater film. The second heater film is positioned along the inner ring line and is connected to the first heater film.

[0114] Step S210: Remove the sacrificial layer to form a suspended structure above the microring resonator with an air gap between the suspended structure and the upper surface of the substrate.

[0115] In this embodiment, the first heater film and the second heater film are fabricated by two photolithography and lift-off processes, respectively, so that the patterns and thicknesses of the two can be controlled independently, which is beneficial to optimizing the electrical and thermal properties of the heater layer.

[0116] The preparation method in this application will be described in detail below.

[0117] Step S1: Prepare the substrate.

[0118] A silicon dioxide layer was grown on the surface of a silicon substrate using a thermal oxidation method to serve as the device substrate. The thickness of this silicon dioxide layer was on the order of micrometers to ensure sufficient mechanical support and electrical isolation. After substrate fabrication, it underwent cleaning and drying to remove surface contaminants.

[0119] Step S2: Grow a silicon layer.

[0120] like Figure 5 As shown, a silicon layer 6 with a thickness of 220 nanometers is grown on substrate 1 using molecular beam epitaxy (MBE) or chemical vapor deposition (CVD) techniques, which is used for subsequent fabrication of microring resonator 2.

[0121] Step S3: Fabricate the micro-ring resonator structure.

[0122] like Figure 6 As shown, photoresist is spin-coated onto silicon layer 6, and the ring waveguide pattern of microring resonator 2 is defined through exposure and development processes. Then, inductively coupled plasma (ICP) etching is used to remove the silicon regions not protected by the photoresist, forming microring resonator 2. The etching gas is a mixture of C4F8, SF6, and O2, with the C4F8 to SF6 flow ratio controlled within the range of 3:1 to 3:4. The RF power can range from 0 to 500 W, and the bias voltage from 50 to 300 V. After etching, the residual photoresist is removed, resulting in the silicon waveguide microring resonator located on the substrate surface.

[0123] Step S4: Deposit the sacrificial layer and open the growth window.

[0124] like Figure 7 and Figure 8 As shown, a sacrificial layer 7 is deposited on the surfaces of substrate 1 and microring resonator 2. The sacrificial layer 7 is made of phosphosilicate glass or borosilicate glass, and the deposition method can be low-pressure chemical vapor deposition or plasma-enhanced chemical vapor deposition. After deposition, the position of a growth window 8 is defined on the sacrificial layer 7 using photolithography. The growth window 8 corresponds to a portion of the ring region of the microring resonator 2 (e.g., an arc segment symmetrically distributed about the center of the microring). Then, the sacrificial layer 7 at the location of the growth window 8 is removed using dry or wet etching, exposing the upper surface of the underlying microring resonator 2 so that the subsequent cladding layer 3 material can directly contact the microring resonator 2 in this region.

[0125] Step S5: Grow the cladding and visualize it.

[0126] like Figure 9 , Figure 10and Figure 11 As shown, plasma-enhanced chemical vapor deposition (PECVD) is used to deposit a silicon dioxide layer 9 within the growth window and above the inner ring connection direction of the micro-ring resonator 2. During deposition, the reactive gases are silane and nitrous oxide, with a flow ratio controlled within the range of 10:1 to 70:1, an RF power range of 30W to 70W, and a reaction temperature of 150℃ to 300℃. After deposition, a patterned photoresist layer 10 is formed on the silicon dioxide layer 9. The silicon dioxide layer 9 is then photolithographically and etched to remove unnecessary areas, retaining the cladding layer 3 pattern located within the growth window 8 and along the inner ring connection direction (diameter), thus obtaining the cladding layer 3. Etching can be performed using reactive ion etching or buffered oxide etchant. Finally, the cladding layer 3 covers a portion of the ring area of ​​the micro-ring resonator 2 and above the inner ring connection line.

[0127] Step S6: Fabricate the first heater film.

[0128] like Figure 12 and Figure 13 As shown, photoresist is spin-coated onto the surfaces of cladding layer 3 and sacrificial layer 7, and the pattern of the first heater film is defined by photolithography, forming a patterned photoresist layer 10. The pattern corresponds to the portion of cladding layer 3 located on the ring region of the microring resonator 2. Then, a titanium nitride (TiN) film is deposited using magnetron sputtering. A titanium target is used as the sputtering target, and argon and nitrogen are used as the sputtering gases. The argon to nitrogen flow ratio is controlled between 4:1 and 9:1, and the sputtering temperature is set below the softening point temperature of the sacrificial layer (e.g., below 800°C) to avoid deformation of the sacrificial layer. The deposited titanium nitride thickness is 50 nanometers. After deposition, a lift-off process is used to remove the photoresist and the titanium nitride above it. The remaining titanium nitride film forms the first heater film 41, which is located on the surface of cladding layer 3 in the ring region of the microring resonator 2.

[0129] Step S7: Fabricate the second heater film.

[0130] like Figure 14 and Figure 15 As shown, photoresist is spin-coated again, and the pattern of the second heater film 42 is defined by photolithography, forming a patterned photoresist layer 10. The pattern corresponds to the inner connection direction of the micro-ring resonator 2 and is connected to the first heater film 41. Next, titanium nitride is deposited again using magnetron sputtering, with the sputtering conditions the same as in step S6, and a deposition thickness of 350 nanometers. After deposition, the photoresist and the titanium nitride layer above it are stripped off, leaving the titanium nitride film to form the second heater film 42. The second heater film 42 extends along the inner connection direction (diameter), and its two ends are connected to two segments of the first heater film 42, respectively.

[0131] Step S8: Remove the sacrificial layer to form a suspended structure.

[0132] like Figure 2 As shown, the wafer, after completing the above process, is immersed in an etching solution to remove the sacrificial layer 7. The etching solution is a diluted hydrofluoric acid aqueous solution (volume concentration 1%–10%) or a buffered oxide etching solution (BOE, NH4F:HF = 6:1). During etching, the wafer can be gently agitated or a magnetic stirrer can be used to ensure uniform etching. The etching time is determined based on the thickness of the sacrificial layer 7 and the etching rate to ensure that the sacrificial layer 7 is completely removed. After etching, the wafer is immediately rinsed in flowing deionized water for at least 5–10 minutes to thoroughly remove residual fluoride ions and prevent corrosion of the device. After the sacrificial layer 7 is removed, the cladding layer 3 and the heater layer 4 are suspended above the microring resonator 2, forming an air gap 5 between them and the upper surface of the substrate 1, thus obtaining a suspended structure.

[0133] Step S9: Wafer-level testing and characterization.

[0134] Before packaging, the fabricated wafer is tested to verify the device's performance. Optical frequency domain reflectance characterization technology is used to test the microring resonator on the wafer, obtaining the distance-domain propagation curve of the optical signal within the microring. Through spectral line analysis, the frequency response characteristics and propagation loss features of the microring can be quickly extracted, and the resonant wavelength offset can be extracted, thereby verifying whether the actual tuning capability of the microheater meets design expectations. If deviations occur in the test results, the relevant data can be recorded for reference in subsequent closed-loop calibration.

[0135] Step S10: Encapsulation process.

[0136] For the suspended microheater structure, a special packaging process is employed to prevent structural damage. Before packaging, a temporary protective layer (such as photoresist or a peelable polymer) is applied to the wafer surface to cover the suspended structure and prevent mechanical contact or particulate contamination during subsequent operations. Then, a flip-chip packaging method is used, placing the chip with its input / output terminals facing down and the suspended structure facing up to avoid external pressure. Low-stress materials (such as low-modulus epoxy resin) are selected for the packaging to reduce the impact of packaging stress on the thermal performance and structural stability of the microheater. A micro-grating coupler is designed on the surface of the microring resonator chip to achieve self-aligned coupling between the optical fiber and the microring waveguide. During packaging, a high-precision automatic alignment system is used to precisely align the optical fiber and the microring waveguide to reduce optical coupling loss. After alignment, curing or soldering is performed to complete the packaging.

[0137] Step S11: Post-packaging testing and calibration.

[0138] After packaging, the electrothermal tuning performance of the microheater is comprehensively tested. The power consumption characteristics and temperature stability of the heater are evaluated by measuring the resonant wavelength tuning range and tuning speed of the microring resonator under different power inputs. Simultaneously, a closed-loop calibration system is designed. Utilizing process deviation data obtained from wafer-level testing, a calibration algorithm compensates for resonant wavelength shifts caused by process fluctuations such as etching depth deviations and film thickness inhomogeneities, thereby improving the chip's computational accuracy. The calibration algorithm can be based on a lookup table or real-time feedback adjustment; the specific implementation method can be determined according to application requirements.

[0139] The various embodiments in this specification are described in a progressive manner. Each embodiment focuses on the differences from other embodiments. The same or similar parts between the various embodiments can be referred to each other.

[0140] The photonic computing chip and its fabrication method provided in this application have been described in detail above. Specific examples have been used to illustrate the principles and implementation methods of this application. The descriptions of the embodiments above are only for the purpose of helping to understand the methods and core ideas of this application. It should be noted that those skilled in the art can make several improvements and modifications to this application without departing from the principles of this application, and these improvements and modifications also fall within the protection scope of this application.

Claims

1. A photonic computing chip, characterized in that, include: Substrate; A microring resonator disposed on the surface of the substrate; The cladding is disposed in a portion of the ring region of the microring resonator and along the direction of the internal connection line of the microring resonator. A heater layer disposed on the surface of the cladding; The cladding layer and the heater layer form a suspended structure above the microring resonator, and there is an air gap between the suspended structure and the upper surface of the substrate.

2. The photonic computing chip as described in claim 1, characterized in that, The heater layer includes a first heater film and a second heater film; The first heater film is disposed on the surface of the cladding located in the ring region of the microring resonator; The second heater film is disposed along the inner connection line of the microring resonator and is connected to the first heater film.

3. The photonic computing chip as described in claim 2, characterized in that, The thickness of the second heater film is greater than the thickness of the first heater film.

4. The photonic computing chip as described in claim 1, characterized in that, The cladding disposed on a portion of the ring region of the microring resonator is symmetrically distributed about the center of the microring resonator.

5. A method for fabricating a photonic computing chip, characterized in that, include: Fabricate a microring resonator on the surface of a substrate; A sacrificial layer is deposited on the surface of the substrate and the microring resonator, and a growth window is opened on the sacrificial layer at a position corresponding to a portion of the ring region of the microring resonator; A cladding layer is grown within the growth window and above the inner ring connection of the microring resonator. A heater layer is grown on the upper surface of the cladding; The sacrificial layer is removed to form a suspended structure above the microring resonator, with an air gap between the suspended structure and the upper surface of the substrate.

6. The method for fabricating a photonic computing chip as described in claim 5, characterized in that, The growth of a heater layer on the upper surface of the cladding includes: A patterned photoresist layer is formed on the surface of the cladding layer and the sacrificial layer; A heater layer material is grown on the surface of the patterned photoresist layer and the cladding layer located within the growth window; The patterned photoresist layer and the heater layer material located on the patterned photoresist layer are peeled off to form a first heater film; A patterned photoresist layer is formed on the surface of the first heater film and the sacrificial layer; A heater layer material is grown on the surface of the patterned photoresist layer and the cladding layer located above the inner ring connection of the microring resonator; The patterned photoresist layer and the heater layer material located on the patterned photoresist layer are peeled off to form a second heater film.

7. The method for fabricating a photonic computing chip as described in claim 6, characterized in that, When growing the heater layer material, the growth method is magnetron sputtering, the target material is a titanium target, the sputtering gas includes argon and nitrogen, the flow ratio of argon and nitrogen is in the range of 4:1 to 9:1, and the sputtering temperature is lower than the softening point temperature of the sacrificial layer.

8. The method for fabricating a photonic computing chip as described in claim 5, characterized in that, The cladding grown within the growth window and above the inner ring connection of the microring resonator includes: A cladding layer is grown within the growth window and above the inner ring line of the microring resonator using plasma-enhanced deposition. The reaction gases include silane and nitrous oxide, with a flow ratio of silane to nitrous oxide ranging from 10:1 to 70:

1. The radio frequency power ranges from 30W to 70W, and the reaction temperature ranges from 150℃ to 300℃.

9. The method for fabricating a photonic computing chip as described in claim 5, characterized in that, The sacrificial layer deposited on the surfaces of the substrate and the microring resonator includes: Phosphosilicate glass or borophosphosilicate glass is deposited on the surfaces of the substrate and the microring resonator to form a sacrificial layer.

10. The method for fabricating a photonic computing chip as described in claim 9, characterized in that, Removing the sacrificial layer includes: The sacrificial layer is etched using a hydrofluoric acid solution or a buffered oxide etchant.