High-density high-capacity transmission preconnectorized optical cable

By introducing DOPO-ZIF-8 flame retardant into polyethylene sheath material, the problem of insufficient flame retardancy of polyethylene sheath material was solved, and the flame retardant and mechanical properties of high-density, high-capacity transmission optical cables were improved.

CN123156399APending Publication Date: 2026-11-24HENGTONG OPTIC ELECTRIC CO LTD +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611665033.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-27
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing polyethylene sheath materials have poor flame retardancy, making it difficult to meet the application requirements of optical cables in places such as computer rooms and data centers. At the same time, their toughness and bending strength are insufficient.

Method used

DOPO-ZIF-8 flame retardant was prepared by organic modification of zinc zeolite imidazole ester skeleton material ZIF-8 with DOPO-maleic acid. This flame retardant was then added to polyethylene to form a nitrogen-phosphorus flame retardant through ion exchange, thereby improving the flame retardant performance of the polyethylene sheath material while maintaining good toughness and flexural strength.

Benefits of technology

It significantly improves the limiting oxygen index of polyethylene sheath material, reaching UL-94 V-1 to V-0 levels, exhibits excellent flame retardant properties, is not prone to agglomeration, and maintains good bending strength and toughness, making it suitable for the inner and outer sheaths of high-density, high-capacity transmission pre-connected optical cables.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123156399A_ABST
    Figure CN123156399A_ABST
Patent Text Reader

Abstract

This invention relates to the field of optical cable technology and discloses a high-density, high-capacity transmission pre-connected optical cable. The optical cable of this invention includes a central reinforcement member, a micro-tube unit, and an outer sheath. This invention adds DOPO-ZIF-8 flame retardant to the polyethylene sheath material. DOPO-ZIF-8 contains a large amount of zinc ions, which can catalyze the cross-linking of polyethylene into carbon at high temperatures. It also contains imidazole nitrogen-containing heterocycles, which form a nitrogen-phosphorus flame retardant with the large amount of DOPO structure in the skeleton, significantly improving the limiting oxygen index of the polyethylene sheath material, achieving a UL-94 rating of V-1 to V-0, demonstrating excellent flame retardant performance. After organic modification, ZIF-8 is less prone to agglomeration and has better dispersibility. When added to the polyethylene sheath material, it has less impact on the mechanical strength of polyethylene, maintaining good flexural strength and toughness, and is less prone to cracking. It is suitable for the inner and outer sheath materials of high-density, high-capacity transmission pre-connected optical cables.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of optical cable technology, specifically to a high-density, high-capacity transmission pre-connected optical cable. Background Technology

[0002] High-capacity transmission pre-connected optical cables mainly consist of a central reinforcing member, micro-tube units, wrapping tape, tear cord, and sheath material. The micro-tube units include optical fibers, water-blocking yarn, aramid fiber yarn, and an inner sheath. They are primarily used in computing data centers, telecommunications operator networks, industrial intelligent manufacturing, and the Industrial Internet of Things (IIoT). The outer sheath mainly serves a protective function and is required to have good flame retardancy, toughness, and crack resistance.

[0003] Polyethylene (PE) sheathing material is ideal for optical cables due to its high toughness, good cold resistance, and excellent corrosion resistance. However, PE is flammable and has poor flame retardancy, making it unsuitable for practical applications of optical cables in computer rooms and data centers. Therefore, flame retardants need to be added to PE sheathing material to improve its flame retardancy, such as inorganic flame retardants like aluminum hydroxide and zinc borate, and organic flame retardants like DOPO and phenyl phosphate. Patent CN120473231B discloses a fire-fighting-specific double flame-retardant power cable and its preparation method. This method involves heating and melting a P / N / S / Si quaternary modified boron nitride flame retardant and linear low-density polyethylene, then extruding the mixture to obtain a PE flame-retardant outer sheath, which exhibits good flame-retardant properties. However, the PE flame-retardant outer sheath of this patent does not demonstrate good bending strength and toughness.

[0004] Zinc zeolite imidazole ester framework material ZIF-8 is a novel nanomaterial containing abundant N and Zn elements. N can be used as a gas source for flame retardants, while Zn can catalyze char formation, showing broad application prospects in flame retardants and other fields. Summary of the Invention

[0005] This invention solves the problem of poor flame retardancy of sheath materials and optical cables, while maintaining good toughness.

[0006] This invention provides a high-density, high-capacity transmission pre-connected optical cable, which consists of a central reinforcement, a micro-tube unit, wrapping tape, tear cord, and an outer sheath; the micro-tube unit consists of optical fiber, water-blocking yarn, fiber yarn, and an inner sheath; and a high-density miniaturized connector is provided at the end of the optical cable.

[0007] Preferably, the central reinforcing member is a non-metallic glass fiber rod.

[0008] Preferably, the strap is made of polyester nonwoven fabric.

[0009] Preferably, the tear rope is a polyester fiber tear rope.

[0010] Preferably, the fiber yarn is aramid fiber yarn.

[0011] Preferably, the inner sheath is made of polyvinyl chloride sheath material or halogen-free flame-retardant sheath material.

[0012] Preferably, the micro-bulb unit comprises 8-128 optical fibers forming an optical fiber group, with the fiber specifications being 180-200μm. The high-density miniaturized connector is a multi-core push-pull optical fiber connector (32-core MPO connector), an ultra-miniature high-density multi-core connector (64-core or 128-core SN-MT quad connector), or a micro multi-core connector (16-core MMC connector), enabling high-density, high-capacity transmission pre-connected optical cables to meet the needs of high-density, high-capacity data transmission applications.

[0013] Preferably, the outer sheath of the high-density, high-capacity transmission pre-connected optical cable is made of polyvinyl chloride sheath material or halogen-free flame-retardant sheath material.

[0014] The preferred method for preparing the halogen-free flame-retardant sheath material is as follows: (1) Add an aqueous ethanol solution and zinc zeolite imidazole ester framework material to the reaction vessel, disperse them ultrasonically in an ultrasonic instrument, introduce carbon dioxide and stir. Carbon dioxide reacts with water to form carbonic acid, and carbonic acid ionizes to produce H2O. + and carbonate CO3 2- H + Attacking the N atom of imidazole breaks the Zn-N coordination bond, and then the carbonate anion reacts with Zn. 2+ Coordination occurs, followed by filtration, washing with water, and drying to obtain CO3 containing carbonate ions. 2- CO3-ZIF-8.

[0015] (2) Add ethylene glycol and CO3-ZIF-8 to the reaction vessel, disperse them by ultrasonication, then add DOPO-maleic acid and stir. The carboxyl groups of DOPO-maleic acid react with the carbonate ions of CO3. 2- Ion exchange occurs, thereby modifying a large amount of DOPO structure into the ZIF-8 matrix. After filtration, the matrix is ​​washed sequentially with N,N-dimethylformamide, ethanol, and water, and then dried to obtain DOPO-ZIF-8 flame retardant.

[0016] (3) Add polyethylene, polyethylene wax, DOPO-ZIF-8 flame retardant and antioxidant to the mixer, mix and then extrude the material through a twin-screw extruder and pelletize it to obtain halogen-free flame retardant sheath material.

[0017] Preferably, the preparation method of the zinc zeolite imidazole ester framework material in (1) is as follows: add deionized water and 2-methylimidazole to the reaction vessel, stir, add an aqueous solution of zinc nitrate hexahydrate, stir at room temperature for 5 hours, centrifuge, wash with water and methanol, and dry to obtain the zinc zeolite imidazole ester framework material ZIF-8.

[0018] Preferably, the carbon dioxide flow rate in (1) is 5-10 mL / min.

[0019] Preferably, the stirring in (1) is carried out at room temperature for 2-3 hours.

[0020] Preferably, the mass ratio of CO3-ZIF-8 and DOPO-maleic acid in (2) is 100:(30-70).

[0021] Preferably, in (2), the stirring is carried out at 85-95℃ for 6-12 hours.

[0022] Preferably, in (3), the mass ratio of polyethylene, polyethylene wax, DOPO-ZIF-8 flame retardant and antioxidant is 100:(0.3-0.8):(20-35):(0.1-0.3).

[0023] Preferably, in (3), the temperature of each section of the twin-screw extruder is 155-190℃ and the screw speed is 60-120r / min.

[0024] Preferably, optical cables are used for data transmission.

[0025] The beneficial technical effects of this invention are: in ethylene glycol medium, utilizing the DOPO-maleic acid carboxyl group and the carbonate ion of CO3-ZIF-8, CO3 2- Ion exchange occurs, thereby modifying a large amount of DOPO structure into the ZIF-8 matrix, which is then added to polyethylene to obtain a halogen-free flame-retardant sheath material (used as both inner and outer sheath materials). The ZIF-8 zinc zeolite imidazole ester skeleton material contains a large amount of zinc ions, which can catalyze the crosslinking of polyethylene into char at high temperatures. It also contains imidazole nitrogen-containing heterocycles, which form nitrogen-phosphorus flame retardants with the large amount of DOPO structure in the skeleton, significantly improving the limiting oxygen index of the polyethylene sheath material. Moreover, it achieves UL-94 ratings from V-1 to V-0, demonstrating excellent flame-retardant performance.

[0026] After organic modification, the ZIF-8 of this invention is less prone to agglomeration and has better dispersibility. When added to polyethylene, it has less impact on the mechanical strength of polyethylene, can maintain good flexural strength and toughness, and is not prone to cracking. The prepared polyethylene sheath material has good mechanical properties and flame retardant properties, and is suitable for the inner and outer sheath materials of high-density, high-capacity transmission pre-connected optical cables. Attached Figure Description

[0027] Figure 1 This is a schematic diagram of the structure of a high-density, high-capacity transmission pre-connected optical cable.

[0028] Figure 2 The infrared spectrum is that of the DOPO-ZIF-8 flame retardant in Example 1. Detailed Implementation

[0029] The technical solution of the present invention will be clearly and completely described below with reference to the embodiments. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0030] Add 450 mL of deionized water and 127 g of 2-methylimidazole to the reaction vessel, stir, and then add 70 mL of an aqueous solution containing 10 g of zinc nitrate hexahydrate. Stir at room temperature for 5 h, centrifuge, wash with water and methanol, and dry to obtain the zinc zeolite imidazole ester framework material ZIF-8.

[0031] 90 mL of toluene, 90 mL of tetrahydrofuran, 162 g of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO), and 87 g of maleic acid were added to a reaction vessel. The mixture was heated to 110 °C, stirred, and refluxed for 12 h. After cooling, the mixture was filtered, the precipitate was collected, and dried to obtain DOPO-maleic acid, with the structural formula [insert structural formula here]. .

[0032] Example 1

[0033] A high-density, high-capacity pre-connected optical cable, consisting of... Figure 1 As shown, the optical cable consists of a non-metallic glass fiber rod central reinforcement (central reinforcement), micro-tube units, polyester non-woven fabric wrapping tape (wrapping tape), polyester fiber tear cord (tear cord), and halogen-free flame-retardant sheath material (as outer sheath). The micro-tube units are made of 32 cores of 200μm optical fibers and halogen-free flame-retardant sheath material (as inner sheath); 18 micro-tube units are arranged in a specific order and fixed with polyester non-woven fabric wrapping tape to form the cable core; water-blocking yarn, aramid fiber yarn, and polyester fiber tear cord are evenly placed outside the cable core (optical fiber), and then a layer of halogen-free flame-retardant sheath material (as outer sheath) is extruded; a 32-core MPO connector is provided at the end of the optical cable.

[0034] The preparation method of halogen-free flame-retardant sheath material is as follows: (1) Add 5L of 98% ethanol aqueous solution and 150g of zinc zeolite imidazole ester framework material to the reaction vessel, disperse it ultrasonically in an ultrasonic instrument, introduce carbon dioxide at a flow rate of 5mL / min, stir at room temperature for 3h, filter, wash with water, and dry to obtain CO3-ZIF-8.

[0035] (2) Add 4L of ethylene glycol and 150g of CO3-ZIF-8 to the reaction vessel, sonicate in an ultrasonic instrument for 20min, then add 60g of DOPO-maleic acid, heat to 90℃, stir and react for 8h, filter, wash with N,N-dimethylformamide, ethanol and water in sequence, dry, and obtain DOPO-ZIF-8 flame retardant. Figure 2 In the infrared spectrum, 1413 cm⁻¹ -1 The absorption peak at 748 cm⁻¹ is the imidazole ring skeleton in the ZIF-8 zinc zeolite imidazole ester framework material. -1 It is an imidazole ring skeleton SP 2 CH bond-plane out-of-plane bending vibration peak, 3453 cm⁻¹ -1 The absorption peak is at 1735 cm⁻¹, representing the -OH group of the carboxyl group in DOPO-maleic acid. -1 The absorption peak is at 1568 cm⁻¹, representing the C=O group of DOPO-maleic acid. -1 The absorption peak is at 1249 cm⁻¹, representing the benzene ring skeleton of DOPO-maleic acid. -1 It is the absorption peak of P=O of DOPO-maleic acid.

[0036] (3) Add 2kg of polyethylene (model LDPE 1800H, Suzhou Xinleda Plastics, the same below), 10g of polyethylene wax (model Honeywell AC-6, Jinan Woneng New Materials, the same below), 400g of DOPO-ZIF-8 flame retardant and 5g of antioxidant 1010 to the mixer. After mixing, the material is extruded through a twin-screw extruder. The temperature of each section is 155℃, 175℃, 190℃ and 190℃, and the screw speed is 100r / min. Pelletize to obtain halogen-free flame retardant sheath material.

[0037] Comparative Example 1 A high-density, high-capacity pre-connected optical cable comprises a non-metallic glass fiber rod central reinforcement, micro-tube units, polyester non-woven fabric wrapping tape, polyester fiber tear cord, and polyethylene sheath material (as the outer sheath). The micro-tube units are made of 32 core 200μm optical fibers and polyethylene sheath material (as the inner sheath); 18 micro-tube units are arranged in a specific order and fixed with polyester non-woven fabric wrapping tape to form the cable core; water-blocking yarn, aramid fiber yarn, and polyester fiber tear cord are evenly placed outside the cable core, and then a layer of polyethylene sheath material (as the outer sheath) is extruded; a 32-core MPO connector is provided at the end of the optical cable.

[0038] The preparation method of polyethylene sheath material is as follows: (1) Add 2kg polyethylene, 10g polyethylene wax, 400g CO3-ZIF-8 and 5g antioxidant 1010 to the mixer. After mixing, the material is extruded through a twin-screw extruder with temperatures of 155℃, 175℃, 190℃ and 190℃ in each section and a screw speed of 100r / min. The material is then pelletized to obtain polyethylene sheath material.

[0039] Comparative Example 2 A high-density, high-capacity pre-connected optical cable comprises a non-metallic glass fiber rod central reinforcement, micro-tube units, polyester non-woven fabric wrapping tape, polyester fiber tear cord, and polyethylene sheath material (as the outer sheath). The micro-tube units are made of 32 core 200μm optical fibers and polyethylene sheath material (as the inner sheath); 18 micro-tube units are arranged in a specific order and fixed with polyester non-woven fabric wrapping tape to form the cable core; water-blocking yarn, aramid fiber yarn, and polyester fiber tear cord are evenly placed outside the cable core, and then a layer of polyethylene sheath material (as the outer sheath) is extruded; a 32-core MPO connector is provided at the end of the optical cable.

[0040] The preparation method of polyethylene sheath material is as follows: (2) Add 4L of ethylene glycol and 150g of zinc zeolite imidazole ester skeleton material ZIF-8 to the reaction vessel, sonicate and disperse in an ultrasonic instrument for 20min, then add 60g of DOPO-maleic acid, heat to 90℃, stir and react for 8h, filter, wash with N,N-dimethylformamide, ethanol and water in sequence, dry, and obtain ZIF-8 flame retardant.

[0041] (3) Add 2kg polyethylene, 10g polyethylene wax, 400g ZIF-8 flame retardant and 5g antioxidant 1010 to the mixer. After mixing, the material is extruded through a twin-screw extruder with temperatures of 155℃, 175℃, 190℃ and 190℃ in each section and a screw speed of 100r / min. The material is then pelletized to obtain polyethylene sheath material.

[0042] Comparative Example 3 A high-density, high-capacity pre-connected optical cable comprises a non-metallic glass fiber rod central reinforcement, micro-tube units, polyester non-woven fabric wrapping tape, polyester fiber tear cord, and polyethylene sheath material (as the outer sheath). The micro-tube units are made of 32 core 200μm optical fibers and polyethylene sheath material (as the inner sheath); 18 micro-tube units are arranged in a specific order and fixed with polyester non-woven fabric wrapping tape to form the cable core; water-blocking yarn, aramid fiber yarn, and polyester fiber tear cord are evenly placed outside the cable core, and then a layer of polyethylene sheath material (as the outer sheath) is extruded; a 32-core MPO connector is provided at the end of the optical cable.

[0043] The preparation method of polyethylene sheath material is as follows: (1) CO3-ZIF-8 was prepared according to the method of Example 1.

[0044] (2) Add 4L of ethylene glycol and 150g of CO3-ZIF-8 to the reaction vessel, sonicate for 20min in an ultrasonic instrument, then add 60g of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO), heat to 90℃, stir for 8h, filter, wash with N,N-dimethylformamide, ethanol and water in sequence, and dry to obtain ZIF-8 flame retardant.

[0045] (3) Add 2kg polyethylene, 10g polyethylene wax, 400g ZIF-8 flame retardant and 5g antioxidant 1010 to the mixer. After mixing, the material is extruded through a twin-screw extruder with temperatures of 155℃, 175℃, 190℃ and 190℃ in each section and a screw speed of 100r / min. The material is then pelletized to obtain polyethylene sheath material.

[0046] Example 2

[0047] A high-density, high-capacity pre-connected optical cable comprises a non-metallic glass fiber rod central reinforcement, micro-tube units, polyester non-woven fabric wrapping tape, polyester fiber tear cord, and halogen-free flame-retardant sheath material (as the outer sheath). The micro-tube units are made of 16 cores of 200μm optical fibers, aramid fiber yarn, and halogen-free flame-retardant sheath material (as the inner sheath). Eighteen micro-tube units are arranged in a specific order and fixed with polyester non-woven fabric wrapping tape to form the cable core. Water-blocking yarn, aramid fiber yarn, and polyester fiber tear cord are evenly placed outside the cable core, and then a layer of halogen-free flame-retardant sheath material (as the outer sheath) is extruded. A 16-core MMC connector is provided at the end of the optical cable.

[0048] The preparation method of halogen-free flame-retardant sheath material is as follows: (1) Add 6L of 98% ethanol aqueous solution and 200g of zinc zeolite imidazole ester framework material to the reaction vessel, disperse it ultrasonically in an ultrasonic instrument, introduce carbon dioxide at a flow rate of 10mL / min, stir at room temperature for 2h, filter, wash with water, and dry to obtain CO3-ZIF-8.

[0049] (2) Add 4.5L of ethylene glycol and 200g of CO3-ZIF-8 to the reaction vessel, sonicate for 20min in an ultrasonic instrument, then add 60g of DOPO-maleic acid, heat to 95℃, stir for 6h, filter, wash with N,N-dimethylformamide, ethanol and water in sequence, and dry to obtain DOPO-ZIF-8 flame retardant.

[0050] (3) Add 2kg polyethylene, 12g polyethylene wax, 500g DOPO-ZIF-8 flame retardant and 6g antioxidant 1010 to the mixer. After mixing, the material is extruded through a twin-screw extruder with temperatures of 155℃, 175℃, 190℃ and 190℃ in each section and a screw speed of 60r / min. The material is then pelletized to obtain halogen-free flame-retardant sheath material.

[0051] Example 3

[0052] A high-density, high-capacity pre-connected optical cable comprises a central reinforcing member, micro-tube units, water-blocking tape, polyester fiber tear cord, and halogen-free flame-retardant sheath material (as the outer sheath). Each micro-tube unit consists of 64 200μm optical fibers, water-blocking yarn, aramid fiber yarn, and halogen-free flame-retardant sheath material (as the inner sheath). Sixteen micro-tube units are arranged in a specific order and fixed with water-blocking tape to form the cable core. Water-blocking yarn, aramid fiber yarn, and polyester fiber tear cord are evenly placed outside the cable core, and then a layer of halogen-free flame-retardant sheath material (as the outer sheath) is extruded. At the ends of the optical cable, a 64-core SN-MT quad connector is provided according to the number of unit cables.

[0053] The preparation method of halogen-free flame-retardant sheath material is as follows: (1) Add 6L of 98% ethanol aqueous solution and 180g of zinc zeolite imidazole ester framework material to the reaction vessel, disperse it ultrasonically in an ultrasonic instrument, introduce carbon dioxide at a flow rate of 5mL / min, stir at room temperature for 2h, filter, wash with water, and dry to obtain CO3-ZIF-8.

[0054] (2) Add 5L of ethylene glycol and 180g of CO3-ZIF-8 to the reaction vessel, sonicate in an ultrasonic instrument for 30min, then add 126g of DOPO-maleic acid, heat to 85℃, stir and react for 12h, filter, wash with N,N-dimethylformamide, ethanol and water in sequence, dry, and obtain DOPO-ZIF-8 flame retardant.

[0055] (3) Add 2kg polyethylene, 6g polyethylene wax, 600g DOPO-ZIF-8 flame retardant and 3g antioxidant 1010 to the mixer. After mixing, the material is extruded through a twin-screw extruder with temperatures of 155℃, 175℃, 190℃ and 190℃ in each section and a screw speed of 120r / min. The material is then pelletized to obtain halogen-free flame-retardant sheath material.

[0056] Example 4

[0057] A high-density, high-capacity pre-connected optical cable comprises a central reinforcing member, micro-tube units, water-blocking tape, polyester fiber tear cord, and halogen-free flame-retardant sheath material (as the outer sheath). Each micro-tube unit consists of 128 180µm optical fibers, water-blocking yarn, aramid fiber yarn, and halogen-free flame-retardant sheath material (as the inner sheath). Fifty-four micro-tube units are arranged in a specific order and fixed with water-blocking tape to form the cable core. Water-blocking yarn, aramid fiber yarn, and polyester fiber tear cord are evenly placed outside the cable core, and then a layer of halogen-free flame-retardant sheath material (as the outer sheath) is extruded. At the ends of the optical cable, 128-core SN-MT quad-connectors are provided according to the number of unit cables.

[0058] The preparation method of halogen-free flame-retardant sheath material is as follows: (1) Add 6.5L of 98% ethanol aqueous solution and 240g of zinc zeolite imidazole ester framework material to the reaction vessel, disperse it ultrasonically in an ultrasonic instrument, introduce carbon dioxide at a flow rate of 5mL / min, stir at room temperature for 3h, filter, wash with water, and dry to obtain CO3-ZIF-8.

[0059] (2) Add 5L of ethylene glycol and 240g of CO3-ZIF-8 to the reaction vessel, sonicate in an ultrasonic instrument for 20min, then add 132g of DOPO-maleic acid, heat to 90℃, stir and react for 10h, filter, wash with N,N-dimethylformamide, ethanol and water in sequence, dry, and obtain DOPO-ZIF-8 flame retardant.

[0060] (3) Add 2kg polyethylene, 16g polyethylene wax, 700g DOPO-ZIF-8 flame retardant and 2g antioxidant 1010 to the mixer. After mixing, the material is extruded through a twin-screw extruder with temperatures of 155℃, 175℃, 190℃ and 190℃ in each section and a screw speed of 100r / min. The material is then pelletized to obtain halogen-free flame-retardant sheath material.

[0061] The sheath material was injection molded to form test strips. The oxygen index was tested according to GB / T 2406.1-2008 standard. The vertical burning performance was tested according to UL-94 method. The flexural strength was tested according to GB / T 9341-2008 standard. The performance test results of the inner sheath material are shown in Table 1.

[0062] Table 1 Performance of Sheathing Material

[0063] As shown in Table 1, the polyethylene sheath material in Example 1 contained DOPO-ZIF-8 flame retardant. ZIF-8 zinc zeolite imidazole ester skeleton material contains a large amount of zinc ions, which can catalyze the crosslinking of polyethylene into char at high temperatures. It also contains imidazole nitrogen-containing heterocycles, which, together with the large amount of DOPO structures in the skeleton, form a nitrogen-phosphorus flame retardant, significantly improving the limiting oxygen index of the polyethylene sheath material. UL-94 ratings reached V-1 to V-0, demonstrating excellent flame retardant performance. Furthermore, after organic modification, ZIF-8 is less prone to agglomeration and has better dispersibility. When added to polyethylene, it has less impact on the mechanical strength of polyethylene, maintaining good flexural strength and excellent toughness. Examples 2 to 4, with the addition of different amounts of DOPO-ZIF-8 flame retardant, also showed good flame retardant performance, flexural strength, and toughness in their polyethylene sheath materials.

[0064] Compared with Example 1, Comparative Example 1 only added CO3-ZIF-8 and did not contain DOPO structure. The limiting oxygen index of the polyethylene outer sheath was lower, the UL-94 test was not passed, the flame retardant performance was poor, and the ZIF-8 had poor dispersibility and was prone to agglomeration, resulting in lower flexural strength of the sheath material.

[0065] The zinc zeolite imidazole ester skeleton material ZIF-8 in Comparative Example 2 does not contain carbonate anions, making it difficult to undergo ion exchange with the carboxyl groups of DOPO-maleic acid. After washing, DOPO-maleic acid is easily washed away from ZIF-8, resulting in a low limiting oxygen index of the sheath material, failure to pass the UL-94 test, poor flame retardant performance, and low flexural strength.

[0066] Comparative Example 3's 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO) does not contain a carboxyl group, making it difficult to undergo ion exchange with the carbonate anions of CO3-ZIF-8. After washing, DOPO is easily eluted from ZIF-8, resulting in a low limiting oxygen index of the sheath material, failure to pass the UL-94 test, poor flame retardant properties, and low flexural strength.

[0067] The present invention also provides the following embodiments: Example 5

[0068] A high-density, high-capacity pre-connected optical cable is composed of a non-metallic glass fiber rod central reinforcement, micro-tube units, polyester non-woven fabric wrapping tape, polyester fiber tear cord, and polyvinyl chloride sheath material (as the outer sheath). The micro-tube units are made of 32 cores of 200μm optical fibers and polyvinyl chloride sheath material (as the inner sheath); 18 micro-tube units are arranged in a specific order and fixed with polyester non-woven fabric wrapping tape to form the cable core; water-blocking yarn, aramid fiber yarn, and polyester fiber tear cord are evenly placed outside the cable core, and then a layer of polyvinyl chloride sheath material (as the outer sheath) is extruded; a 32-core MPO connector is provided at the end of the optical cable.

[0069] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution of the present invention, should be covered within the scope of protection of the present invention.

Claims

1. A high-density, high-capacity pre-connected optical cable, characterized in that, The high-density, high-capacity transmission pre-connected optical cable includes a central reinforcement, a micro-tube unit, a wrapping tape, a tear cord, and an outer sheath; the micro-tube unit includes optical fiber, water-blocking yarn, fiber yarn, and an inner sheath; a high-density miniaturized connector is provided at the end of the optical cable. The outer sheath of the high-density, high-capacity transmission pre-connected optical cable is made of polyvinyl chloride (PVC) or halogen-free flame-retardant material; the halogen-free flame-retardant material is prepared by the following method. (1) Add an aqueous ethanol solution and zinc zeolite imidazole ester framework material to the reaction vessel, disperse it ultrasonically in an ultrasonic instrument, introduce carbon dioxide and stir, filter, wash with water, and dry to obtain CO3-ZIF-8. (2) Add ethylene glycol and CO3-ZIF-8 to the reaction vessel, disperse them ultrasonically in an ultrasonic instrument, and then add the following: DOPO-maleic acid was stirred, filtered, washed successively with N,N-dimethylformamide, ethanol, and water, and dried to obtain DOPO-ZIF-8 flame retardant. (3) Add polyethylene, polyethylene wax, DOPO-ZIF-8 flame retardant and antioxidant to the mixer, mix and then extrude the material through a twin-screw extruder and pelletize it to obtain halogen-free flame retardant sheath material.

2. The high-density, high-capacity pre-connected optical cable according to claim 1, characterized in that, The central reinforcement is a non-metallic fiberglass rod; the wrapping strap is a polyester non-woven fabric wrapping strap.

3. The high-density, high-capacity pre-connected optical cable according to claim 1, characterized in that, The tear rope is made of polyester fiber; the fiber yarn is made of aramid fiber; and the inner sheath is made of polyvinyl chloride sheath material or halogen-free flame-retardant sheath material.

4. The high-density, high-capacity pre-connected optical cable according to claim 1, characterized in that, A single micro-bulb tube contains 8-128 optical fibers, with fiber specifications of 180-200μm.

5. The high-density, high-capacity pre-connected optical cable according to claim 1, characterized in that... High-density miniaturized connectors include multi-core push-pull fiber optic connectors, ultra-small high-density multi-core connectors, or micro multi-core connectors.

6. The high-density, high-capacity pre-connected optical cable according to claim 1, characterized in that, The zinc zeolite imidazole ester framework material was prepared by the following method: deionized water and 2-methylimidazole were added to a reaction vessel, stirred, and then an aqueous solution of zinc nitrate hexahydrate was added dropwise. The reaction was stirred at room temperature, centrifuged, and the precipitate was washed with water and methanol and dried to obtain the zinc zeolite imidazole ester framework material.

7. The high-density, high-capacity pre-connected optical cable according to claim 1, characterized in that, (1) The flow rate of carbon dioxide is 5-10 mL / min; and / or, (1) the stirring is carried out at room temperature for 2-3 h.

8. The high-density, high-capacity pre-connected optical cable according to claim 1, characterized in that, (2) The mass ratio of CO3-ZIF-8 and DOPO-maleic acid is 100:(30-70), and / or, the stirring in (2) is carried out at 85-95℃ for 6-12h.

9. The high-density, high-capacity pre-connected optical cable according to claim 1, characterized in that, (3) The mass ratio of polyethylene, polyethylene wax, DOPO-ZIF-8 flame retardant and antioxidant is 100: (0.3-0.8): (20-35): (0.1-0.3).

10. The high-density, high-capacity pre-connected optical cable according to claim 1, characterized in that, (3) The temperature of each section of the twin-screw extruder is 155-190℃ and the screw speed is 60-120r / min.

Citation Information

Patent Citations

  • Fire-fighting special double flame-retardant power cable and preparation method thereof

    CN120473231B