Electrochromic coating with gradual spectral selectivity
By constructing film thickness and doping concentration gradients in a single-layer electrochromic active layer, the problem of gradient spectral selectivity control in existing electrochromic glasses is solved, achieving continuous smooth transition and independent spectral management, reducing system complexity and cost, and improving the performance and comfort of smart dimming glass.
Patent Information
- Application Number
- CN202611686602.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-29
- Publication Date
- 2026-11-24
AI Technical Summary
Existing electrochromic smart dimming glass faces technical bottlenecks in achieving spatial gradient spectral selectivity, making it impossible to achieve continuous smooth transition and independent control of visible light transmittance and near-infrared radiant heat. Furthermore, the zoned design is highly complex and costly.
A gradient variation in film thickness and dopant concentration is constructed in a single-layer electrochromic active layer. The film thickness increases and the dopant concentration increases linearly through magnetron sputtering, achieving synergistic gradient control of visible light transmittance and near-infrared modulation depth. Combined with an all-solid-state electrolyte layer and partitioned driving electrodes, the gradient effect and process reliability are ensured.
It achieves a smooth and continuous transition from high-transparency to high-shading areas, balancing visibility and heat insulation performance, reducing system complexity and cost, and improving intelligence and driving comfort.
Smart Images

Figure CN123156499A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of smart dimming glass technology, and more specifically, to an electrochromic coating with gradient spectral selectivity. Background Technology
[0002] Smart dimming glass, as an intelligent window material capable of dynamically adjusting its optical transmittance in response to external electrical signals or environmental stimuli, has broad application prospects in fields such as building energy-saving curtain walls, automotive sunroofs and windshields, and aviation windows. Based on different working principles, existing smart dimming glass is mainly divided into three categories: polymer-dispersed liquid crystal type, suspended particle type, and electrochromic type. Among them, electrochromic smart dimming glass has become the mainstream direction for current technological research and industrial application due to its comprehensive advantages such as continuously adjustable transmittance, low driving voltage, good open-circuit memory effect, and wide operating temperature range. In recent years, with the rapid development of the new energy vehicle industry, the demand for zoned dimming glass that combines high-transmittance viewing areas and efficient sunshade areas has become increasingly urgent, driving electrochromic technology towards more refined spectral management and spatial dimension control.
[0003] However, existing electrochromic smart dimming glass still faces significant technical bottlenecks in achieving spatially gradient spectral selectivity. Current mainstream commercial solutions employ a partitioned design, dividing the glass substrate into multiple independent dimming zones using physically isolated or patterned electrodes. Different driving voltages are applied to each zone to achieve differentiated transmittance. For example, Fuyao Glass Industry Group Co., Ltd. proposed a partitioned electrochromic glass structure with a shading zone, transition zone, and main viewing zone in its published Chinese patent CN117818310B. While this partitioned design meets the need for partial shading in automotive windshields to some extent, it is essentially a discrete spatial control method. There are obvious visual jumps and transmittance steps between adjacent zones, making it impossible to achieve a smooth, continuous transition from high-transmittance to high-shading zones, affecting driver visual comfort and overall aesthetics. Furthermore, the partitioned structure requires independent electrode leads and driving circuits for each zone, increasing system complexity and manufacturing costs.
[0004] On the other hand, regarding spectral selectivity, traditional electrochromic materials such as tungsten oxide often exhibit coupled modulation of visible and near-infrared light during ion insertion / extraction. This means that while overall transmittance decreases, near-infrared shielding capability increases, making independent control of visible light transmittance and near-infrared radiant heat difficult. In recent years, researchers have successfully achieved decoupled control of the visible-near-infrared dual-band spectrum by doping tungsten oxide with transition metals such as molybdenum, vanadium, and niobium. For example, it has been reported that molybdenum-nitrogen co-doped tungsten trioxide hydrate nanosheets maintain high transmittance in the visible light band while achieving a high modulation depth in the near-infrared band. However, these studies mainly focus on optimizing the electrochemical performance of homogeneous films and have not yet combined dual-band spectral selectivity with gradual spatial control, failing to meet the application requirements of simultaneously achieving differentiated spectral management at different spatial locations on the same glass sheet.
[0005] In summary, current technologies lack a solution capable of simultaneously achieving spatially continuous gradient and spectrally selective modulation within a single-layer electrochromic active layer. Therefore, developing a smart dimming glass technology that is structurally simple, process-compatible, and capable of directly forming a continuously gradient spectrally selective coating during integrated coating processes is of significant practical importance and commercial value for promoting the industrial application of next-generation high-performance smart dimming glass. Summary of the Invention
[0006] The technical problem to be solved by the present invention is to overcome the shortcomings of the prior art and provide an electrochromic coating with gradient spectral selectivity that can simultaneously achieve spatial continuous gradient and spectral selectivity in a single-layer electrochromic active layer.
[0007] The technical solution adopted by the present invention to solve its technical problem is: an electrochromic coating with gradient spectral selectivity, the coating comprising a single-layer electrochromic active layer disposed on a transparent conductive substrate, wherein the electrochromic active layer simultaneously satisfies the following conditions along a first direction of the glass plane: The film thickness increases monotonically from the first end to the second end; The atomic percentage of the dopant element increases monotonically from the first end to the second end; Wherein, the first end corresponds to the high-transmittance field of view region, and its visible light transmittance in the colored state is higher than that of the high-shading shading region corresponding to the second end; and the modulation depth of the electrochromic active layer in the near-infrared band monotonically increases from the first end to the second end along the first direction. The electrochromic active layer is deposited by magnetron sputtering. The monotonically increasing film thickness is achieved by linearly moving the mask, and the monotonically increasing concentration of doped elements is achieved by linearly increasing the auxiliary target power during co-sputtering.
[0008] By simultaneously constructing film thickness gradient and doping concentration gradient in the same monolayer electrochromic active layer, a continuous and smooth transition from high transmittance region to high shielding region is achieved, avoiding visual jumps and transmittance steps caused by discrete control in existing partitioned splicing designs. At the same time, the synergistic gradient of film thickness and doping concentration makes the near-infrared modulation depth increase synchronously and monotonically in the same direction, realizing spatial decoupling control of visible light transmittance and near-infrared shielding capability, and balancing visual clarity and heat insulation performance on the same piece of glass.
[0009] Preferably, the thickness of the electrochromic active layer monotonically increases from 60nm~100nm to 180nm~250nm from the first end to the second end, and the atomic percentage of the dopant element monotonically increases from 1at%~3at% to 5at%~8at% from the first end to the second end. This thickness increase pattern and dopant concentration variation ensure the effectiveness of the gradient amplitude, achieving an optimal balance between the gradient effect and process reliability, and avoiding insufficient transmittance change due to excessively small thickness difference or stress cracking of the film layer due to excessively large dopant concentration difference.
[0010] The first end has a visible light transmittance of 55% to 85% in the tinted state, while the second end has a visible light transmittance of 5% to 25% in the tinted state. This ensures that the field of vision still has sufficient light transmittance in the tinted state to meet the needs of safe driving, while the sunshade area can effectively block most of the visible light to reduce glare. The two end have a transmittance difference of at least 30 percentage points, which is enough to produce a clear sense of gradient in the human eye.
[0011] The electrochromic active layer has a minimum modulation depth of 15% to 35% and a maximum modulation depth of 55% to 80% in the near-infrared band of 800nm to 2500nm. This ensures that the high-transmittance area maintains visible light transmission while still having a certain near-infrared shielding capability, while the shading area has efficient near-infrared blocking performance. The difference in near-infrared modulation depth between the two is at least 20 percentage points, achieving spatial decoupling management of visible light and near-infrared.
[0012] Preferably, the electrochromic active layer is made of molybdenum-doped tungsten oxide with the chemical formula Mo. x W 1-x O3, wherein x increases linearly from 0.01 to 0.03 to 0.05 to 0.08 along the first direction, and the electrochromic active layer is an amorphous structure.
[0013] This invention selects molybdenum-doped tungsten oxide as the active layer material. By utilizing molybdenum ion doping to introduce additional energy level states and oxygen vacancies, the absorption range in the near-infrared band is effectively broadened and the modulation depth is improved. The amorphous structure avoids the obstruction of ion transport by grain boundaries, which is beneficial to improving the response speed and cycle stability. The x value increases gradually from 0.01~0.03 to 0.05~0.08 along the gradient direction, so that the near-infrared modulation capability is enhanced synchronously with the increase of molybdenum content, forming a synergistic effect with the film thickness gradient.
[0014] More preferably, the thickness of the electrochromic active layer linearly increases from 80 nm to 220 nm along the first direction, and the atomic percentage of molybdenum, Mo / (W+Mo), linearly increases from 2 at% to 6 at% along the first direction. This combination exhibits optimal overall performance: linearity of visible light transmittance gradient R 2 With a value ≥0.99, the near-infrared modulation depth is smoothly increased from about 20% to about 60%, and the coloring response time is controlled within 8s, which is the preferred implementation window for this technical solution.
[0015] Preferably, the coating further includes an ion storage layer and a solid electrolyte layer stacked sequentially, the solid electrolyte layer being disposed between the electrochromic active layer and the ion storage layer, and the solid electrolyte layer being a lithium-ion conductor doped with aluminum, wherein the molar ratio of lithium to aluminum is 3~5:1.
[0016] An aluminum-doped lithium-ion conductor solid electrolyte layer is introduced, in which aluminum exists in the electrolyte network in the form of an aluminum-oxygen tetrahedral network. By adjusting the network structure, the lithium-ion conductivity is improved and the interfacial bonding force and mechanical stability between the electrolyte and adjacent film layers are enhanced. As the only migratory charge carrier, lithium ions maintain good kinetic characteristics to ensure a rapid coloring / fading response. The all-solid-state structure completely eliminates the risk of leakage and volatilization of liquid electrolytes.
[0017] More preferably, the material of the solid electrolyte layer is selected from at least one of lithium phosphorus oxynitride compound, aluminum-doped lithium phosphate, or lithium aluminum phosphorus oxide, the thickness of the solid electrolyte layer is 200 nm to 500 nm, and its ionic conductivity at 25 °C is 1 × 10⁻⁶. -6 S / cm ~ 1×10 -4 Materials such as LiPON, Al-doped Li3PO4, or Li-Al-PO exhibit good chemical stability and interfacial compatibility; the thickness balances ion transport efficiency and mechanical strength; and the ionic conductivity range ensures uniform coloring / fading.
[0018] More preferably, the material of the ion storage layer is copper-doped nickel oxide, with the chemical formula Cu. y Ni 1-yO, where y is 0.08~0.15, and the ion storage layer is a neutral coloring material, whose chromatic coordinates in the colored state are... Value and The absolute values of all values are less than 5.
[0019] This invention uses copper-doped nickel oxide as the counter electrode material, effectively suppressing the brownish-yellow bias of pure NiO during the coloring process, resulting in a neutral gray tone; color coordinates Value and The absolute values of all values are less than 5, which ensures that the entire glass pane is uniformly neutral in color and free from color deviation in the tinted state, meeting the stringent requirements for appearance quality of automotive windshields and high-end building curtain walls.
[0020] Preferably, the opening width of the linearly moving mask increases linearly along the first direction, the mask moving speed is 50 mm / min to 120 mm / min, and the auxiliary target is a molybdenum metal target, whose DC sputtering power linearly increases from 3 W to 8 W to 15 W to 25 W along the first direction. This process window ensures the linearity of the film thickness gradient and the doping concentration gradient, ensuring that the Mo doping ratio is precisely controllable along the gradient direction, and achieving a high process yield in mass production.
[0021] Preferably, the coating further includes a plurality of independently driven transparent conductive electrode regions disposed along the first direction, wherein the plurality of independently driven transparent conductive electrode regions divide the electrochromic active layer into 3 to 8 driving partitions along the first direction, each driving partition being connected to an independent voltage control unit, and the driving voltage range of each driving partition being 0.5V to 3.5V.
[0022] By dividing the gradient coating into 3 to 8 independent drive zones and connecting each zone to an independent voltage control unit, the dynamic adjustment capability of the gradient curve is realized. Each zone can be independently adjusted within the range of 0.5 to 3.5V, thereby flexibly changing the shape and position of the gradient curve according to external lighting conditions and user needs. This allows the same piece of glass to adapt to various usage scenarios, greatly improving the product's intelligence level.
[0023] More preferably, there are five independently driven transparent conductive electrode regions, evenly spaced along the first direction, with driving voltages ranging from 0.8V to 1.5V, 1.5V to 2.0V, 2.0V to 2.5V, 2.5V to 2.8V, and 2.8V to 3.2V from the first end to the second end, respectively. This voltage distribution matches the spatial distribution of the film thickness / doping gradient, allowing each region to operate within its optimal voltage range, ensuring the continuity of the gradient curve while reducing overall power consumption.
[0024] Specifically, in the colored state, the difference in visible light transmittance between any two adjacent points along the first direction of the electrochromic active layer does not exceed 10%, and the linear correlation coefficient R of the visible light transmittance change curve along the first direction is... 2 ≥0.98; After 3000 square wave voltage cycles, the optical modulation depth retention rate of the electrochromic active layer at a wavelength of 633nm is ≥85%, and after being placed in an environment of 85℃ and 85% relative humidity for 1000h, the linear correlation coefficient R of its visible light transmittance change curve along the first direction is ≥0.98. 2 ≥0.95. The gradient linearity and durability indicators achieved by this invention ensure the visual uniformity and long-term reliability of the product in actual use. The linearity indicator guarantees that no abrupt changes or step-like appearance can be observed with the naked eye, and the durability indicator proves the coating's ability to withstand automotive-grade environments.
[0025] This coating can be widely used in various scenarios such as building curtain walls, car windshields, car sunroofs, aviation windows and display cases. Utilizing its spatial gradient spectral selectivity, it can achieve functions such as energy-saving heat insulation, anti-glare shading, privacy protection and exhibit protection in different applications, and has significant market universality and commercial value.
[0026] Compared with existing technologies, this invention has the following advantages: By simultaneously constructing film thickness gradients and doping concentration gradients in the same monolayer electrochromic active layer, this invention achieves a continuous and smooth transition from high transmittance to high shielding regions, overcoming the visual jumps and transmittance abrupt changes caused by discrete control in existing partitioned splicing designs; the synergistic gradients of film thickness and doping concentration enable the near-infrared modulation depth to increase synchronously and monotonically in the same direction, achieving spatial decoupling control of visible light transmittance and near-infrared shielding capability, balancing visual clarity and heat insulation performance on the same piece of glass; the use of a molybdenum-doped tungsten oxide amorphous active layer and an aluminum-doped lithium-ion conductor all-solid-state electrolyte improves the near-infrared modulation depth while ensuring rapid response and long-term cycling stability; combined with partitioned independent drive and environmental adaptive control strategies, the gradient shading strip can dynamically shift with the solar altitude angle, significantly improving the level of intelligence and driving comfort; this solution is compatible with existing magnetron sputtering production lines and has good industrialization prospects. Attached Figure Description
[0027] Figure 1 This is a schematic cross-sectional view of the electrochromic coating with gradient spectral selectivity prepared in Example 1 of the present invention. Detailed Implementation
[0028] The present invention will now be described in detail through examples. Unless otherwise stated, all raw materials used are commercially available.
[0029] In this article, ITO refers to indium tin oxide transparent conductive oxide; LiPON refers to lithium phosphorusoxynitride solid electrolyte; XPS refers to X-ray photoelectron spectroscopy; XRD refers to X-ray diffraction; T_vis refers to the average transmittance of visible light from 380nm to 780nm, weighted by a D65 light source; NIR refers to the near-infrared band from 800nm to 2500nm; DAC refers to an exponential mode converter; RH refers to relative humidity; and sccm refers to cubic centimeters per minute under standard conditions.
[0030] Example 1
[0031] 1. Substrate preparation and preprocessing Ultra-clear low-iron float glass with dimensions of 300mm × 500mm and a thickness of 3.0mm was selected as the substrate. The substrate underwent the following cleaning process in sequence: 30s of roller brushing with a 2% (w / w) detergent solution → 20s of rinsing with deionized water → 5min of ultrasonic cleaning with a 2% (w / w) dilute nitric acid solution → 5min of ultrasonic cleaning with anhydrous ethanol → drying with high-purity nitrogen. The cleaned substrate was immediately transferred to the magnetron sputtering chamber and evacuated to a base vacuum level ≤6×10⁻⁶. -4 Pa, then an Ar / O2 mixed gas (volume ratio 4:1) is introduced, and plasma activation treatment is performed for 5 min at a radio frequency power of 100W to remove residual organic matter on the surface and increase surface energy.
[0032] 2. Deposition of antireflective / UV blocking hard coating A four-layer dielectric antireflection film was sequentially deposited on an activated glass substrate using radio frequency magnetron sputtering to form a stacked structure. The first SiO2 layer was deposited at room temperature using a SiO2 ceramic target (99.99% purity, 76.2 mm diameter) with a radio frequency power of 150 W, an Ar gas atmosphere of 40 sccm, and a working pressure of 0.5 Pa, resulting in a film thickness of 70 nm. The second TiO2 layer was deposited at room temperature using a TiO2 ceramic target (99.99% purity) with a radio frequency power of 180 W, an Ar / O2 mixed gas atmosphere of 36 sccm / 4 sccm, and a working pressure of 0.5 Pa, resulting in a film thickness of 50 nm. This SiO2 / TiO2 sequence was repeated once to obtain a four-layer antireflection film with a total thickness of 240 nm (70 nm + 50 nm + 70 nm + 50 nm). After deposition, the substrate was annealed in air at 250 °C for 30 min to solidify and stabilize the film structure. The resulting antireflective coating has an average reflectivity of less than 1.5% in the visible light band (380nm~780nm) and a blocking rate of more than 95% for ultraviolet light (wavelength <380nm).
[0033] 3. Deposition of the first transparent conductive layer (bottom ITO) An ITO thin film was deposited on an antireflective coating using radio frequency magnetron sputtering. The target material was an In₂O₃:SnO₂ ceramic target (mass ratio 90:10, purity 99.99%). Process parameters: Base vacuum ≤ 6 × 10⁻⁶. -4 The working gas was an Ar / O2 mixture (49.6 sccm / 0.4 sccm), with a working pressure of 0.4 Pa, an RF power of 300 W, a substrate temperature of 250 °C, and a deposition film thickness of 200 nm. The resulting ITO thin film had a sheet resistance of 8 Ω / sq to 10 Ω / sq and a visible light transmittance greater than 88%. This layer was a homogeneous film with no gradient change along the first direction (X-direction) of the glass plane.
[0034] 4. Deposition of the electrochromic active layer (Mo-WO3 continuous dual gradient layer) This step is the core process, which uses a dual-target co-sputtering method combined with a linear moving mask to prepare an amorphous Mo-WO3 thin film with both thickness gradient and molybdenum doping concentration gradient along the X direction on the underlying ITO.
[0035] Equipment configuration: The main target is a WO3 ceramic target (99.99% purity, 76.2mm diameter), connected to an RF power supply; the auxiliary target is a Mo metal target (99.95% purity, 76.2mm diameter), connected to a DC power supply. A linearly moving mask is placed between the substrate and the target. The mask is a thin stainless steel plate with linearly tapered slits along a first direction. The distance between the mask and the substrate is 4mm, and the distance between the mask and the target is 60mm. The mask is driven by a stepper motor and moves back and forth uniformly at a speed of 80mm / min along the X direction. The equivalent exposure time at position X on the substrate is t(X) = w(X) / v, where w(X) is the slit width corresponding to that position, and v is the mask moving speed. The film thickness is expressed as d(X) = n·r·w(X) / v, calibrated by maskless full-time deposition. In this embodiment, n=10, r=39.5nm / min, and v=80mm / min are used. The slit width is calculated from the target film thickness (82nm at the first end and 223nm at the second end) to be 16.6mm at the first end and 45.2mm at the second end, that is, the slit width increases linearly along the first direction.
[0036] Process parameters: The RF power of the WO3 target is fixed at 200W; the DC power of the Mo target increases linearly from 5W at the beginning along the X direction to 20W at the end, with a ramp rate of 4W / min; the working gas is an Ar / O2 mixture (20sccm / 1sccm), with a working pressure of 0.5Pa; the substrate temperature is maintained at 250℃; the mask moving speed is 80mm / min, starting from X=0mm and stopping at X=300mm, with a single pass time of 3.75min; in this embodiment, the mask reciprocates 10 times (n=10), with a total deposition time of 37.5min. The DC power of the Mo target increases synchronously from 5W to 20W according to the above linear law in each pass, and resets to 5W at the end of the pass before starting the next pass.
[0037] Gradient results: Along the X-axis from the first end (X=0mm, corresponding to the high-transmittance field of view) to the second end (X=300mm, corresponding to the high-shading area), the film thickness linearly increases from 82nm to 223nm, and the molybdenum atomic percentage (Mo / (W+Mo)) linearly increases from 2.1at% to 6.0at%. After joint calibration using X-ray photoelectron spectroscopy (XPS) and profilometry, the film thickness deviation is ≤±3nm, the molybdenum content deviation is ≤±0.2at%, and the linear correlation coefficient R0 is ≤±3nm. 2 ≥0.993. X-ray diffraction (XRD) tests showed that the film has an amorphous structure.
[0038] Except for the active layer deposition step, during the deposition of the bottom layer ITO, LiPON, Cu-NiO and the top layer ITO, the substrate stage moves in a uniform reciprocating motion along the direction perpendicular to X, with the scanning stroke covering 500 mm of the substrate side length, to ensure that the 76.2 mm circular target achieves a thickness uniformity within ±5% on the 300 mm × 500 mm substrate; during the active layer deposition, the stage remains stationary, and only the mask moves.
[0039] 5. Deposition of the solid electrolyte layer (LiPON) A LiPON solid electrolyte film was deposited on a Mo-WO3 active layer using radio frequency magnetron sputtering. The target material was a Li3PO4 ceramic target (99.9% purity, 76.2 mm diameter). Process parameters: Base vacuum ≤ 6 × 10⁻⁶. -4 The working gas was an Ar / N2 mixture (20 sccm / 30 sccm), with a working pressure of 0.4 Pa, an RF power of 260 W, and deposition at room temperature, resulting in a film thickness of 300 nm. The obtained LiPON film exhibited an ionic conductivity of 3.2 × 10⁻⁶ at 25 °C. -6 S / cm. This layer is a homogeneous film with no gradient change.
[0040] The electrolyte in this embodiment is an aluminum-free LiPON-based system, serving as a basic control structure for aluminum-doped electrolyte schemes.
[0041] 6. Deposition of the ion storage layer (Cu-NiO) A Cu-doped NiO thin film was deposited as an ion storage layer (counter electrode) on a LiPON electrolyte layer using DC reactive magnetron sputtering. The target material was a Cu-Ni alloy target (atomic ratio Cu:Ni = 1:8, purity 99.95%). Process parameters: working gas was an Ar / O2 mixture (50 sccm / 3 sccm), working pressure 3.5 Pa, DC power 300 W, room temperature deposition, and film thickness 200 nm. The obtained Cu... 0.11 Ni 0.89 O film in neutral coloring state, according to Standard measured color coordinates The value is -1.8. The value is +2.3, and the absolute values are all less than 5, presenting a neutral gray tone with no obvious color cast.
[0042] 7. Deposition of the second transparent conductive layer (top ITO) A top-layer ITO thin film was deposited on a Cu-NiO ion storage layer using radio frequency magnetron sputtering. The target material was the same as the bottom ITO layer. Process parameters: working gas was an Ar / O2 mixture (49.6 sccm / 0.4 sccm), working pressure was 0.4 Pa, radio frequency power was 300 W, deposition was performed at room temperature (to avoid high-temperature damage to the underlying electrolyte), and the film thickness was 150 nm. The sheet resistance of the resulting ITO thin film was 10 Ω / sq~12 Ω / sq.
[0043] 8. Etching, edge sealing and busbar fabrication Laser etching was used to remove each thin film layer within a 5mm width along the glass edge, exposing the staggered steps of the bottom and top ITO layers, forming an insulating isolation band. After completing the edge etching, laser etching was further used along the X direction at four equally spaced partition boundaries (X=60mm, 120mm, 180mm, 240mm) to cut the top ITO, forming an isolation channel with a width of approximately 0.3mm. This divided the top ITO into five electrically isolated driving partitions, while the bottom ITO remained continuous as a common electrode. The laser power and scanning parameters were set to remove only the top ITO without penetrating the LiPON electrolyte layer. After etching, optical microscopy confirmed that each isolation channel was intact and there were no short circuits between adjacent partitions. During fading, a reverse voltage of -1.0V to -3.0V was applied to each partition relative to the bottom ITO common electrode. Then, UV-curable epoxy resin was coated as an edge sealing layer and cured under 395nm UV light for 30s. Butyl rubber was then applied to the outer ring to enhance the sealing performance. At the five reserved busbar windows, five partition busbar electrodes are fabricated using silver paste screen printing technology, which are evenly distributed along the X direction, corresponding to five independent drive partitions (each partition is 60mm wide).
[0044] 9. Electrochemical activation and performance testing The prepared electrochromic coated glass was connected to a multichannel potentiostat, and a pre-lithiation activation treatment was first performed by applying a constant voltage of 1.5V for 60s. Then, a cycle stability test was conducted at a square wave voltage of ±3.0V (frequency 0.05Hz).
[0045] Optical performance testing: A PerkinElmer Lambda 1050 ultraviolet-visible-near-infrared spectrophotometer equipped with an integrating sphere was used. Under D65 standard light source and 10° field of view, nine sampling points (X=0mm, 37.5mm, 75mm, 112.5mm, 150mm, 187.5mm, 225mm, 262.5mm, 300mm) were taken at equal intervals along the X direction. The visible light transmittance and modulation depth in the near-infrared band (800nm~2500nm) were measured in the faded state (faded to steady state from -3.0V and then held at 0V for 60s) and the colored state (3.0V). The test results are shown in Table 1.
[0046] In this paper, the near-infrared modulation depth ΔT_NIR is defined as the difference between the average transmittance of the band in the faded state and the colored state, that is, ΔT_NIR = T_NIR (faded state) - T_NIR (colored state), where T_NIR is the average transmittance of equally spaced sampling points in the 800nm~2500nm band.
[0047] Table 1 Optical performance data of each sampling point along the X direction in Example 1
[0048] As shown in Table 1, along the X-direction from the first end to the second end, the visible light transmittance of the colored state continuously decreases from 64.8% to 13.9%, while the near-infrared modulation depth continuously increases from 21% to 61%. Both show a good linear relationship, with a linear correlation coefficient R0. 2 The values are 0.985 and 0.970, respectively. The maximum difference in visible light transmittance between adjacent sampling points is 8.6%, which is less than the limit of 10%.
[0049] Response time test: Under a 3.0V step voltage, the full-area coloring response time (the time required for the transmittance change to reach a steady-state value of 90%) is 6.2s~7.8s; under a -3.0V step voltage, the fading response time is 8.5s~11.3s.
[0050] Cyclic stability test: After 3000 square wave voltage cycles at ±3.0V and 0.05Hz, the optical modulation depth retention rate at 633nm wavelength is 87.3%, which is greater than the limit of 85%.
[0051] Damp heat aging test: After placing the sample in a constant temperature and humidity chamber at 85℃ and 85% relative humidity for 1000 hours, remove it and measure the colored visible light transmittance at 9 sampling points along the X direction again. The linear correlation coefficient R of the change curve is then calculated. 2 The value is 0.963, which is greater than the limit of 0.95, indicating that the coating still maintains good gradient linearity in a humid and hot environment.
[0052] 10. Partition driver verification Connect the five partition buses to the independent output terminals of the five-channel potentiostat, apply the driving voltage according to the voltage sequence shown in Table 2, and verify the independent dimming function of each partition.
[0053] Table 2 Voltage Allocation of Each Drive Zone in Example 1
[0054] Test results show that each zone can independently reach the target transmittance range under its own recommended voltage, and the transmittance transition between adjacent zones is smooth, without any visible abrupt changes or steps.
[0055] It should be noted that the recommended drive voltages in Table 2 are used to fine-tune the transmittance operating point of each zone under static conditions; the main value of independent zone drive lies in the reshaping of the position and shape of the gradient curve under dynamic conditions, such as shifting the shading strip according to changes in the solar altitude angle, which is something that a single voltage full-chip drive cannot achieve.
[0056] See attached document Figure 1 The coating, from bottom to top, comprises: a glass substrate, an antireflective / UV blocking hard coating (four-layer stacked SiO2 / TiO2), a bottom ITO transparent conductive layer, a Mo-WO3 continuous dual-gradient electrochromic active layer, a LiPON solid electrolyte layer, a Cu-NiO ion storage layer, and a top ITO transparent conductive layer. The Mo-WO3 active layer exhibits distinct iridescent interference fringes along the X-direction, visually reflecting the dual-gradient characteristics of its film thickness (82nm→223nm) and molybdenum doping concentration (2.1at%→6.0at%) continuously and linearly increasing along the first direction. This provides a structural basis for achieving a gradual change in visible light transmittance from the high-transmittance field of view to the high-shading sun-shading area, and a simultaneous increase in near-infrared modulation depth.
[0057] Example 2
[0058] The substrate selected was ultra-white low-iron float glass with dimensions of 300mm × 500mm and a thickness of 3.2mm. The cleaning process was the same as in Example 1. After being transferred to the magnetron sputtering chamber, a vacuum was evacuated to ≤6×10⁻⁶. -4 Pa was introduced, and plasma activation was performed for 5 minutes at 100W RF power using Ar / O2 (4:1).
[0059] The antireflective / UV blocking hard coating uses the same four-layer SiO2 / TiO2 dielectric antireflective stack as in Example 1, with the thickness and process parameters of each layer remaining unchanged. After deposition, it is annealed at 250°C for 30 min in air. The bottom ITO layer uses an In2O3:SnO2 (90:10wt%) ceramic target, RF 300W, Ar / O2=49.6sccm / 0.4sccm, 0.4Pa, 250°C, film thickness 200nm, and sheet resistance 8~10Ω / sq.
[0060] The electrochromic active layer is the core change in this embodiment. The main target is a WO3 ceramic target (99.99% purity), with a fixed RF power of 200W; the secondary target is a Mo metal target (99.95% purity), with DC power linearly increasing from an initial 3W to a final 15W. The working gas is Ar / O2 = 20 sccm / 1 sccm, the working pressure is 0.5 Pa, and the substrate temperature is 250℃. The mask-substrate distance is 4mm, the mask moving speed is 50mm / min, and the single-pass time from X=0mm to X=300mm is 6.0min. In this embodiment, the mask reciprocates 10 times (n=10), with a total deposition time of 60min. The slit width is 12.7mm on the first end and 31.6mm on the second end. The DC power of the Mo target linearly increases from 3W to 15W synchronously in each single pass. The resulting film thickness increased linearly from 100 nm at the first end to 250 nm at the second end, and the molybdenum atomic percentage (Mo / (W+Mo)) increased linearly from 3 at% to 8 at%. After joint calibration using XPS and a profilometer, the film thickness deviation was ≤ ±4 nm, the molybdenum content deviation was ≤ ±0.3 at%, and the linear correlation coefficient R0 was ≤ ±0.3 at%. 2 ≥0.991. XRD testing confirmed it to be an amorphous structure. In this end-cap combination, the 250 nm thick end and 8 at% Mo are both upper limits, designed to verify the film integrity and cycling stability under high doping and high concentration conditions.
[0061] The solid electrolyte layer uses LiPON material, with a Li3PO4 ceramic target (99.9% purity), Ar / N2 = 20 sccm / 30 sccm, 0.4 Pa, RF 260 W, room temperature deposition, and a film thickness of 300 nm. In this embodiment, aluminum doping was achieved through co-sputtering of a lithium phosphate ceramic target (RF 260 W) and an alumina ceramic target (RF 40 W) (without using a metal-organic aluminum precursor). The Li / Al molar ratio was determined to be 5:1 by XPS. The introduction of Al increased the ionic conductivity to 8.5 × 10⁻⁶. -6 S / cm. This high Li / Al ratio focuses on verifying the near-infrared modulation response under lithium-ion kinetics-dominated conditions.
[0062] The ion storage layer used Cu-NiO, with a Cu:Ni alloy target (99.95% purity) at an atomic ratio of 1:8. The Ar / O2 ratio was 50 sccm / 3 sccm, the pressure was 3.5 Pa, DC 300 W, and deposition was performed at room temperature, resulting in a film thickness of 200 nm. The obtained Cu... 0.11 Ni 0.89 O film according to Standard measured color states =-2.1, =+1.9, all absolute values are less than 5, and it is neutral gray.
[0063] The top-layer ITO deposition parameters are the same as in Example 1, with a film thickness of 150 nm and a sheet resistance of 10 Ω / sq to 12 Ω / sq. The etching, sealing, and busbar fabrication processes are the same as in Example 1, with five equally spaced drive zones set along the X direction.
[0064] The performance test results are as follows: along the X direction, the tinted visible light transmittance at 9 sampling points decreases from 58.3% at the first end to 9.7% at the second end, while the near-infrared modulation depth increases from 18% to 67%. The maximum transmittance difference between adjacent sampling points is 9.8%. The visible light transmittance variation curve R... 2 =0.989, near-infrared modulation depth R 2 =0.987. The coloring response time at 3.0V step voltage is 7.5s~9.1s, and the fading response time at -3.0V is 10.2s~13.5s. After 3000 cycles of ±3.0V square wave at 0.05Hz, the modulation depth retention rate at 633nm is 86.1%. After aging at 85℃ / 85%RH for 1000h, R... 2 =0.952. Each zone independently achieves the target transmittance at the recommended voltage, with a smooth transition and no abrupt changes.
[0065] Example 3
[0066] The substrate was selected as ultra-clear low-iron float glass with dimensions of 300mm × 500mm and a thickness of 2.5mm. The cleaning and plasma activation processes were the same as in Example 1. The parameters of the anti-reflective coating and the underlying ITO were consistent with those in Example 1.
[0067] The electrochromic active layer is the core change in this embodiment. The RF power of the main target, WO3 ceramic, is fixed at 200W; the DC power of the auxiliary target, Mo metal, linearly increases from 8W to 25W. The working gas is Ar / O2 = 20 / 1 sccm, 0.5 Pa, and the substrate temperature is 250℃. The mask moving speed is 120mm / min, and the single pass from X=0 to X=300mm takes 2.5min. In this embodiment, the mask reciprocates 10 times (n=10), with a total deposition time of 25min. The slit width is 18.2mm on the first end and 54.7mm on the second end. The DC power of the Mo target linearly increases from 8W to 25W synchronously in each single pass. The resulting film thickness linearly increases from 60nm at the first end to 180nm at the second end, and the molybdenum atomic percentage linearly increases from 1at% to 5at%. After calibration, the film thickness deviation is ≤±3nm, the molybdenum content deviation is ≤±0.2at%, and the linear correlation coefficient R is ≤±3nm. 2 ≥0.994. XRD confirmed it to be amorphous.
[0068] The solid electrolyte layer was constructed using aluminum-doped lithium phosphate (Al-doped Li3PO4), co-sputtered from a Li3PO4 ceramic target (99.9% purity) and an Al2O3 ceramic target (99.99% purity). The Li3PO4 target RF power was 260 W, the Al2O3 target RF power was 70 W, the Ar / N2 ratio was 20 sccm / 30 sccm, the deposition temperature was 0.4 Pa, and the deposition was carried out at room temperature, resulting in a film thickness of 400 nm. The Li / Al molar ratio was 3.5:1, and the resulting ionic conductivity was 5.6 × 10⁻⁶. -6 S / cm. Increasing the aluminum doping ratio helps improve the ionic conductivity of the electrolyte and enhance its interfacial bonding with adjacent film layers, which complements the active layer doping gradient formed by the high Mo power ramp-up. The above Li / Al molar ratio was calibrated by the Li and Al atomic concentration ratio measured by XPS depth profiling, with the average taken from three different locations for each sample.
[0069] The ion storage layer used Cu-NiO, with a Cu:Ni atomic ratio alloy target (99.95% purity) of 1:5.7, corresponding to y=0.15. Deposition was performed at Ar / O2=50 sccm / 3 sccm, 3.5 Pa, DC 300 W, and room temperature, resulting in a film thickness of 200 nm. 0.15 Ni 0.85 O film coloring state according to Standard measurement =-0.9, =+3.1, with absolute values all less than 5, exhibiting a slightly warm neutral gray tone.
[0070] The top layer ITO, etching, edge sealing and busbar fabrication are the same as in Example 1, with 5 equally spaced drive partitions set.
[0071] The performance test results are as follows: along the X direction, the tinted visible light transmittance at 9 sampling points decreases from 71.2% at the first end to 22.4% at the second end, while the near-infrared modulation depth increases from 16% to 58%. The maximum transmittance difference between adjacent sampling points is 7.3%. 2 =0.994. 3.0V step coloring response time: 5.8s~7.1s; -3.0V fading response time: 7.9s~10.2s. After 3000 cycles of ±3.0V square wave, the modulation depth retention rate at 633nm is 88.5%. After aging at 85℃ / 85%RH for 1000h, R... 2 =0.961.
[0072] Example 4
[0073] The substrate was selected as ultra-white low-iron float glass with dimensions of 300mm × 500mm and a thickness of 3.0mm. Cleaning and activation were the same as in Example 1. The anti-reflective coating and the underlying ITO parameters were the same as in Example 1.
[0074] The film thickness linearly increased from 80 nm at the first end to 220 nm at the second end; the Mo / (W+Mo) ratio linearly increased from 2 at% to 6 at%; the WO3 target RF power was 200 W; the Mo target DC power increased from 5 W to 20 W; the mask speed was 80 mm / min; the mask reciprocated 10 times (n=10); the total deposition time was 37.5 min; the slit width was 16.2 mm at the first end and 44.6 mm at the second end; the Ar / O2 ratio was 20 sccm / 1 sccm; the pressure was 0.5 Pa; and the temperature was 250 °C. The gradient results were consistent with those of Example 1, and the linearity of film thickness and doping was R0. 2 All values are ≥0.993, confirming the amorphous state.
[0075] The solid electrolyte layer was prepared using lithium aluminum phosphorus oxide (Li-Al-PO) via co-sputtering with an Al₂O₃ target (RF260W) and a Nitrogen dioxide (N₂) atmosphere. The Ar / N₂ ratio was 20 sccm / 25 sccm, the deposition was carried out at 0.4 Pa, and the film thickness was 250 nm. The Li / Al molar ratio was approximately 3:1. The resulting ionic conductivity was 6.3 × 10⁻⁶. -6 S / cm. Compared to LiPON, the Li-Al-PO system has better flexibility and interfacial bonding with adjacent layers, making it suitable for large-size substrates.
[0076] The ion storage layer was Cu-NiO, and the target was a Cu:Ni alloy target with an atomic ratio of 1:10.5 (purity 99.95%), corresponding to y=0.087. Deposition was performed at Ar / O2=50 / 3 sccm, 3.5 Pa, DC 300 W, and room temperature, with a film thickness of 200 nm. The resulting film exhibited a colored state. =-2.5, =+1.2, with absolute values all less than 5, exhibiting a slightly cool neutral gray color.
[0077] The top layer of ITO deposition is the same as in Example 1, with a film thickness of 150 nm.
[0078] The etching and sealing processes are the same as in Example 1, except that the isolation channels are set at positions that are integer multiples of X=37.5mm, with a total of 7 channels, dividing the top ITO layer into 8 electrically isolated drive zones. In this example, 8 independent drive zones are set along the X direction, each zone being 37.5mm wide. The drive voltages of the 8 zones from the first end to the second end are 0.5V, 1.0V, 1.5V, 2.0V, 2.5V, 2.8V, 3.2V, and 3.5V, respectively. Each zone is connected to a multi-channel DAC driver board based on an STM32F407 microcontroller. The output of each DAC is buffered by an operational amplifier before driving the corresponding silver paste bus electrode.
[0079] In automatic mode, a light sensor located on the upper edge of the glass collects solar irradiance and incident angle in real time. The STM32F407 microcontroller calculates the target position of the sunshade strip based on the incident angle and outputs the driving voltage of each zone according to the zone interpolation algorithm, so as to realize the continuous translation of the sunshade strip as the solar altitude angle changes. The glass installation posture is the conventional tilt angle of the windshield. When the solar altitude angle decreases, the projection position of the incident light on the glass shifts downward, and the sunshade strip translates accordingly.
[0080] Performance test results: The chromatic visible light transmittance at 9 sampling points along the X direction decreased from 65.1% at the first end to 14.2% at the second end, while the near-infrared modulation depth increased from 22% to 62%. Under independent 8-zone drive, the transmittance transition of each zone was smooth, with no visible abrupt changes. In manual mode, the transmittance error of each zone at the target voltage was <±2%. In automatic mode, during a continuous 8-hour sunshine simulation test, the position of the shading strip smoothly shifted down by approximately 120mm as the solar altitude angle decreased from 85° to 15°, without any abrupt changes. Cyclic stability: After 3000 cycles of ±3.0V square wave, the 633nm modulation depth retention rate was 87.8%. After aging at 85℃ / 85%RH for 1000 hours, R... 2 =0.958.
[0081] Example 5
[0082] The substrate was selected as ultra-white low-iron float glass with dimensions of 300mm × 500mm and a thickness of 3.0mm. The cleaning process was the same as in Example 1. After being transferred to the magnetron sputtering chamber, a vacuum was evacuated to ≤6×10⁻⁶. -4 Pa, introduce Ar / O2 mixed gas (volume ratio 4:1), and perform plasma activation treatment for 5 min under radio frequency power of 100W.
[0083] The antireflective / UV-blocking hard coating was deposited using a radio frequency magnetron sputtering method, consisting of a four-layer SiO2 / TiO2 dielectric antireflective stack. The first SiO2 layer was deposited at a SiO2 ceramic target (99.99% purity, 76.2 mm diameter) with a radio frequency power of 150 W, Ar 40 sccm, 0.5 Pa, at room temperature, resulting in a film thickness of 70 nm. The second TiO2 layer was deposited at a TiO2 ceramic target (99.99% purity) with a radio frequency power of 180 W, Ar / O2 = 36 sccm / 4 sccm, 0.5 Pa, at room temperature, resulting in a film thickness of 50 nm. This process was repeated once, resulting in a total thickness of 240 nm (70 nm + 50 nm + 70 nm + 50 nm). After deposition, the coating was annealed at 250 °C for 30 min in air. The resulting antireflective coating exhibited an average reflectivity of less than 1.5% in the visible light band (380 nm to 780 nm) and a UV light blocking rate greater than 95% for wavelengths <380 nm.
[0084] The ITO substrate was deposited using radio frequency magnetron sputtering. The target material was an In₂O₃:SnO₂ ceramic target (mass ratio 90:10, purity 99.99%). The base vacuum was ≤6×10⁻⁶. -4 Pa, Ar / O2 = 49.6 sccm / 0.4 sccm, 0.4 Pa, RF power 300 W, substrate temperature 250 °C, film thickness 200 nm. The resulting ITO thin film has a sheet resistance of 8 Ω / sq~10 Ω / sq and a visible light transmittance greater than 88%. This layer is a homogeneous film with no gradient change along the X direction.
[0085] The electrochromic active layer is the core of this embodiment. The main target is a WO3 ceramic target (99.99% purity, 76.2 mm diameter), with a fixed RF power of 200 W; the auxiliary target is a Mo metal target (99.95% purity, 76.2 mm diameter), with DC power linearly increasing from an initial 5 W to a final 20 W at a rate of 4 W / min. The working gas is Ar / O2 = 20 sccm / 1 sccm, the working pressure is 0.5 Pa, and the substrate temperature is 250 °C. The mask is a thin stainless steel plate with linearly tapered slits along a first direction. The distance between the mask and the substrate is 4 mm, and the distance between the mask and the target is 60 mm. Driven by a stepper motor, it reciprocates at a constant speed of 80 mm / min along the X direction. A single pass from X=0 mm to X=300 mm takes 3.75 min, with a total of 10 passes (n=10), for a total deposition time of 37.5 min. The slit width is 16.2 mm at the first end and 44.6 mm at the second end. The DC power of the Mo target linearly increases from 5 W to 20 W synchronously within each pass. The resulting film thickness linearly increases from 80 nm at the first end to 220 nm at the second end, and the molybdenum atomic percentage (Mo / (W+Mo)) linearly increases from 2 at% to 6 at%. The chemical formula can be represented as Mo. x W 1-xO3, where x increases linearly from 0.02 to 0.06. After joint calibration using XPS and a profilometer, the film thickness deviation was ≤ ±2 nm, the molybdenum content deviation was ≤ ±0.15 at%, and the linear correlation coefficient of film thickness R0 was ≤ ±0.15 at%. 2 ≥0.996, linearity of doping concentration R 2 ≥0.995.
[0086] The solid electrolyte layer was aluminum-doped lithium phosphate (Al-doped Li3PO4). The targets were co-sputtered using a Li3PO4 ceramic target (99.9% purity, 76.2 mm diameter) and an Al2O3 ceramic target (99.99% purity, 76.2 mm diameter). The Li3PO4 target RF power was 260 W, and the Al2O3 target RF power was 60 W. The working gas ratio was Ar / N2 = 20 sccm / 30 sccm, at 0.4 Pa, and deposition was carried out at room temperature, resulting in a film thickness of 300 nm. The Li / Al molar ratio was approximately 4:1. The resulting aluminum-doped lithium phosphate film had an ionic conductivity of 4.8 × 10⁻⁶. -6 S / cm. This material exhibits both good chemical stability and interfacial compatibility with adjacent layers, and Al doping further enhances ionic conductivity and mechanical strength.
[0087] The ion storage layer used Cu-NiO, with a Cu:Ni alloy target (99.95% purity) of 1:8 atomic ratio, corresponding to y=0.11. The deposition conditions were: Ar / O2=50 sccm / 3 sccm, 3.5 Pa, DC power 300 W, room temperature deposition, and a film thickness of 200 nm. 0.11 Ni 0.89 O film in colored state according to Standard measured color coordinates =-1.8, =+2.3, with absolute values all less than 5, exhibiting a neutral gray tone. This copper doping ratio effectively suppresses the brownish-yellow bias of pure NiO, resulting in a uniform color across the entire glass sheet without any color deviation.
[0088] The top layer of ITO was deposited using radio frequency magnetron sputtering, with the same target material as the bottom layer of ITO. The Ar / O2 ratio was 49.6 sccm / 0.4 sccm, the Pa ratio was 0.4, the radio frequency power was 300 W, and the deposition was performed at room temperature (to avoid high-temperature damage to the underlying electrolyte). The film thickness was 150 nm. The resulting ITO film had a sheet resistance of 10 Ω / sq to 12 Ω / sq.
[0089] The etching, sealing, and busbar fabrication processes are the same as in Example 1. Laser etching is used to remove each thin film layer along a 5mm width from the glass edge, exposing the bottom and top ITO layers to form an insulating isolation strip. UV-cured epoxy resin is then applied (cured at 395nm UV light for 30s), and butyl rubber is applied around the outer ring to enhance sealing. Five partitioned busbar electrodes are fabricated at the reserved window using silver paste screen printing, evenly spaced along the X-direction, with each partition being 60mm wide.
[0090] In this embodiment, the voltage sequence used for the five driving zones from the first end to the second end is: 0.8V, 1.5V, 2.0V, 2.5V, and 3.2V.
[0091] The performance test results are as follows: along the X direction, the tinted visible light transmittance at 9 sampling points decreases from 66.5% at the first end to 13.2% at the second end, while the near-infrared modulation depth increases from 20% to 63%. The maximum transmittance difference between adjacent sampling points is 7.8%. The visible light transmittance variation curve R... 2 =0.996, near-infrared modulation depth R 2 =0.994. The tinting response time at 3.0V step change is 5.5s~6.8s, and the fading response time at -3.0V is 7.2s~9.5s. After 3000 cycles of ±3.0V square wave at 0.05Hz, the modulation depth retention rate at 633nm is 89.2%. Visible light transmittance change curve R after aging at 85℃ / 85%RH for 1000h. 2 =0.972. Each zone independently achieves the target transmittance under the optimal voltage, with a smooth transition and no abrupt changes.
[0092] Example 6
[0093] The substrate selected was ultra-white low-iron float glass with dimensions of 300mm × 500mm and a thickness of 2.8mm. The cleaning process was the same as in Example 1. After being transferred to the magnetron sputtering chamber, a vacuum was evacuated to ≤6×10⁻⁶. -4 Pa, Ar / O2 (4:1) was introduced, and plasma activation was performed at 100W radio frequency power for 5 minutes.
[0094] The deposition parameters of the antireflective / UV blocking hard coating and the underlying ITO are the same as in Example 1. The total thickness of the four-layer SiO2 / TiO2 stack is 240 nm, with visible light reflectance <1.5% and UV blocking rate >95%. The underlying ITO film is 200 nm thick, with sheet resistance of 8~10 Ω / sq and visible light transmittance >88%.
[0095] The electrochromic active layer is the core change in this embodiment. The main target, a WO3 ceramic target (99.99% purity), has a fixed RF power of 200W; the auxiliary target, a Mo metal target (99.95% purity), has a DC power that linearly increases from an initial 3W to an end of 15W at a rate of 3.2W / min. The working gas is Ar / O2 = 20 sccm / 1 sccm, 0.5 Pa, and the substrate temperature is 250℃. The mask moving speed is 80mm / min, and the single pass from X=0 to X=300mm takes 3.75min. In this embodiment, the mask reciprocates 10 times (n=10), with a total deposition time of 37.5min. The slit width is 17.2mm on the first end and 42.5mm on the second end. The DC power of the Mo target linearly increases from 3W to 15W synchronously in each single pass. The resulting film thickness linearly increases from 85 nm at the first end to 210 nm at the second end, and the molybdenum atomic percentage linearly increases from 1.5 at% to 5.5 at%, corresponding to the chemical formula Mo. x W 1-x In O3, x increases from 0.015 to 0.055. After calibration, the film thickness deviation is ≤ ±3 nm, the molybdenum content deviation is ≤ ±0.2 at%, and the film thickness R... 2 ≥0.994, doping concentration R 2 ≥0.993. XRD confirmed it to be an amorphous structure. This combination of low power and low doping results in lower film stress and a denser film layer, which is beneficial for long-term cycling stability.
[0096] The solid electrolyte layer was prepared using lithium aluminum phosphate oxide (Li-Al-PO). It was prepared by co-sputtering a Li3PO4 target (99.9% purity) with an RF power of 260 W and an Al2O3 target (99.99% purity) with an RF power of 50 W, followed by a reaction under N2 atmosphere. The Ar / N2 ratio was 20 sccm / 28 sccm, the deposition temperature was 0.4 Pa, and the film thickness was 350 nm at room temperature. The Li / Al molar ratio was approximately 4.5:1. The resulting Li-Al-PO film had an ionic conductivity of 3.9 × 10⁻⁶. -6 S / cm. Compared to LiPON, this material has better flexibility and interfacial bonding with adjacent layers, making it suitable for mass production of large-size substrates.
[0097] The ion storage layer was Cu-NiO, and the target material was a Cu:Ni alloy target with an atomic ratio of 1:10.5 (purity 99.95%), corresponding to y=0.087. The deposition conditions were Ar / O2=50sccm / 3sccm, 3.5 Pa, DC power 300W, room temperature, and a film thickness of 200nm. The resulting film color state was determined according to... Standard measurement =-2.6, =+1.0, with absolute values all less than 5, exhibiting a slightly cool neutral gray color. The low copper doping ratio makes the film closer to the electrochemical performance of pure NiO, while still maintaining good neutral color shift suppression.
[0098] The top layer of ITO deposition is the same as in Example 1, with a film thickness of 150 nm and a sheet resistance of 10 Ω / sq to 12 Ω / sq.
[0099] The etching, edge sealing, and busbar fabrication are the same as in Example 1. Five equally spaced drive zones are set along the X direction, each zone being 60mm wide. The drive voltages of the five zones, from the first end to the second end, are 1.0V, 1.6V, 2.1V, 2.6V, and 3.1V, respectively.
[0100] The performance test results are as follows: along the X direction, the tinted visible light transmittance at 9 sampling points decreases from 68.2% at the first end to 15.6% at the second end, while the near-infrared modulation depth increases from 18% to 59%. The maximum transmittance difference between adjacent sampling points is 7.1%. The visible light transmittance variation curve R... 2 =0.994, near-infrared modulation depth R 2 =0.992. The coloring response time under a 3.0V step change is 5.2s~6.5s, and the fading response time under -3.0V is 6.8s~9.0s. After 3000 cycles of ±3.0V square wave at 0.05Hz, the modulation depth retention rate at 633nm is 90.1%, the highest among all values, demonstrating the positive contribution of the low-doping, low-power combination to cycle stability. After aging at 85℃ / 85%RH for 1000h, R... 2 =0.968.
[0101] Example 7
[0102] The substrate was selected as ultra-white low-iron float glass with dimensions of 300mm × 500mm and a thickness of 3.2mm. The cleaning and activation processes were the same as in Example 1.
[0103] The antireflective coating has the same parameters as the underlying ITO layer in Example 1. The total thickness of the four-layer SiO2 / TiO2 stack is 240 nm, and the visible light reflectance is <1.5%. The underlying ITO film is 200 nm thick, and the sheet resistance is 8 Ω / sq~10 Ω / sq.
[0104] The electrochromic active layer is the core change in this embodiment. The main target, a WO3 ceramic target (99.99% purity), has a fixed RF power of 200W; the auxiliary target, a Mo metal target (99.95% purity), has a DC power that linearly increases from an initial 8W to a final 25W, with a ramp rate of 6.8W / min. The working gas is Ar / O2 = 20 sccm / 1 sccm, 0.5 Pa, and the substrate temperature is 250℃. The mask movement speed is 120mm / min, and the single pass from X=0 to X=300mm takes 2.5min, which is the highest mask movement speed combination among all embodiments. In this embodiment, the mask reciprocates 14 times (n=14), with a total deposition time of 35min. The slit width is 16.9mm on the first end and 46.6mm on the second end. The DC power of the Mo target linearly increases from 8W to 25W synchronously in each single pass. The resulting film thickness linearly increases from 78 nm at the first end to 215 nm at the second end, and the percentage of molybdenum atoms linearly increases from 3.2 at% to 7.8 at%, corresponding to the chemical formula Mo. x W 1-x In O3, x increases from 0.032 to 0.078. After calibration, the film thickness deviation is ≤ ±4 nm, the molybdenum content deviation is ≤ ±0.3 at%, and the film thickness R... 2 ≥0.990, doping concentration R 2 ≥0.989. XRD confirmed it to be an amorphous structure. Under the combination of high doping and high power, the near-infrared modulation depth reached the highest value among all embodiments, but the film stress increased.
[0105] The solid electrolyte layer uses LiPON material, with a Li3PO4 ceramic target (99.9% purity), Ar / N2 ratio of 20 sccm / 30 sccm, Pa at 0.4 Pa, RF power of 260 W, and deposition at room temperature, resulting in a film thickness of 500 nm. Aluminum doping was achieved through co-sputtering with an alumina ceramic target (40 W RF) added to the lithium phosphate target (without using a metal-organic aluminum precursor), with a Li / Al molar ratio of approximately 5:1. The resulting film has an ionic conductivity of 9.2 × 10⁻⁶. -6 S / cm. The combination of maximum thickness and maximum Li / Al ratio aims to verify the potential for further improvement in near-infrared modulation depth under conditions of high ionic conductivity.
[0106] The ion storage layer uses Cu-NiO, and the target material is a Cu:Ni alloy target with an atomic ratio of 1:5.7 (purity 99.95%), corresponding to y=0.15. The deposition conditions are Ar / O2=50sccm / 3sccm, 3.5 Pa, DC power 300W, room temperature deposition, and a film thickness of 200nm. The resulting film color states are as follows: Standard measurement =-0.7, =+3.5, with absolute values all less than 5, exhibiting a slightly warm neutral gray hue. The high copper doping ratio gives the film a slightly warmer color tone.
[0107] The top layer of ITO deposition is the same as in Example 1, with a film thickness of 150 nm and a sheet resistance of 10 Ω / sq to 12 Ω / sq.
[0108] The etching, edge sealing, and busbar fabrication are the same as in Example 1, except that the isolation channels are set at positions that are integer multiples of X=37.5mm, with a total of 7 channels, dividing the top ITO layer into 8 electrically isolated drive zones. In this example, 8 independent drive zones are set along the X direction, each zone being 37.5mm wide. The drive voltages of the 8 zones from the first end to the second end are 0.8V, 1.2V, 1.6V, 2.0V, 2.4V, 2.7V, 3.0V, and 3.2V, respectively.
[0109] The performance test results are as follows: along the X direction, the chromatic visible light transmittance at 9 sampling points decreases from 63.2% at the first end to 8.5% at the second end, while the near-infrared modulation depth increases from 24% to 71%. The maximum transmittance difference between adjacent sampling points is 9.5%. The visible light transmittance variation curve R... 2 =0.991, near-infrared modulation depth R 2 =0.989. The coloring response time at 3.0V step voltage is 6.8s~8.5s, and the fading response time at -3.0V is 9.5s~14.2s. After 3000 cycles of ±3.0V square wave at 0.05Hz, the modulation depth retention rate at 633nm is 85.6%. After aging at 85℃ / 85%RH for 1000h, R... 2 =0.951.
[0110] Comparative Example 1 The difference between this comparative example and Example 1 is that the electrochromic active layer only has a film thickness gradient, but not a molybdenum doping concentration gradient; that is, the Mo doping concentration remains constant along the X direction. All other process conditions are exactly the same as in Example 1.
[0111] The substrate was selected as ultra-white low-iron float glass with dimensions of 300mm × 500mm and a thickness of 3.0mm. The cleaning, plasma activation, anti-reflective coating, and ITO deposition parameters were all consistent with those in Example 1.
[0112] The electrochromic active layer was sputtered using a single target, employing only a WO3 ceramic target (99.99% purity, 76.2 mm diameter), omitting the Mo metal target. The WO3 target RF power was fixed at 200 W. The working gas was Ar / O2 = 20 sccm / 1 sccm, with a working pressure of 0.5 Pa and a substrate temperature of 250 °C. The mask moving speed was 80 mm / min, and the single-pass time from X=0 mm to X=300 mm was 3.75 min. In this comparative example, the mask reciprocated 10 times (n=10), with a total deposition time of 37.5 min. The slit width was the same as in Example 1 (16.6 mm on the first end and 45.2 mm on the second end). The resulting film thickness increased linearly from 82 nm at the first end to 223 nm at the second end, consistent with the film thickness gradient in Example 1. However, the molybdenum atomic percentage Mo / (W+Mo) remained constant along the X direction, measured by XPS as 0 at% (pure WO3), indicating no doping gradient.
[0113] The solid electrolyte layer uses LiPON, with a Li3PO4 ceramic target (99.9% purity), Ar / N2 ratio of 20 sccm / 30 sccm, 0.4 Pa, RF power of 260 W, room temperature deposition, and a film thickness of 300 nm. The ion storage layer uses Cu-NiO, with a Cu:Ni = 1:8 atomic ratio alloy target, Ar / O2 ratio of 50 sccm / 3 sccm, 3.5 Pa, DC power of 300 W, room temperature deposition, and a film thickness of 200 nm. The top layer ITO deposition, etching, edge sealing, and busbar fabrication are the same as in Example 1, with five equally spaced driving zones set along the X direction.
[0114] The performance test results are as follows: the tinted visible light transmittance at 9 sampling points along the X direction decreases from 67.8% at the first end to 12.5% at the second end. The linear correlation coefficient R of the visible light transmittance change curve is... 2 =0.985, with a maximum transmittance difference of 9.2% between adjacent sampling points. However, in the 800nm~2500nm near-infrared band, as the modulation depth increases from 12% at the first end to 48% at the second end, the linear correlation coefficient R of the modulation depth change curve is... 2=0.862, significantly lower than 0.970 in Example 1. Compared with Example 1, the near-infrared modulation depth of Comparative Example 1 is only 12% at the thin end (X=0mm), lower than 21% in Example 1; at the thick end (X=300mm), it is 48%, lower than 61% in Example 1; and the modulation depth in the middle region (X=150mm) is only 31%, 16 percentage points lower than 47% in the same position in Example 1. This indicates that without molybdenum doping, the near-infrared modulation capability of pure WO3 is significantly insufficient, especially the modulation depth in the middle region shows obvious nonlinear fluctuations, making it impossible to achieve a smooth near-infrared gradient from the high-transmittance area to the shaded area. The coloring response time under a 3.0V step is 7.5s~9.8s, and the fading response time is 10.5s~14.2s, both slower than in Example 1. After 3000 cycles of ±3.0V square wave, the modulation depth retention rate at 633nm is 82.1%, lower than the limits of 87.3% and 85% in Example 1. After aging at 85℃ / 85%RH for 1000 hours, R 2 =0.941, which is lower than the limits of 0.963 and 0.95 in Example 1.
[0115] Comparative Example 2 The difference between this comparative example and Example 1 is that the electrochromic active layer only has a molybdenum doping concentration gradient, but not a film thickness gradient; that is, the film thickness remains constant along the X direction. All other process conditions are exactly the same as in Example 1.
[0116] The substrate was selected as ultra-white low-iron float glass with dimensions of 300mm × 500mm and a thickness of 3.0mm. The cleaning, plasma activation, anti-reflective coating, and ITO deposition parameters were all consistent with those in Example 1.
[0117] The electrochromic active layer was co-sputtered using a dual-target system. The primary target was a WO3 ceramic target (99.99% purity) with a fixed RF power of 200W. The secondary target was a Mo metal target (99.95% purity), with the DC power linearly increasing from an initial 5W to a final 20W at a rate of 4W / min. The working gas was Ar / O2 = 20 sccm / 1 sccm, with a working pressure of 0.5 Pa and a substrate temperature of 250℃. In this comparative example, no mask was placed in front of the primary target. The substrate stage performed a uniform reciprocating scanning motion perpendicular to the X-direction to maintain uniform film thickness. To create a doping concentration gradient while maintaining uniform film thickness, an auxiliary mask with an opening width linearly increasing along the X-direction was placed in front of the Mo metal target. The opening width linearly increased from 12 mm at the first end to 34 mm at the second end, thus increasing the Mo deposition flux along the X-direction. The deposition time was fixed at 3.75 min, and the resulting film thickness remained constant along the X direction, measuring 142 ± 5 nm (mean 142 nm) using a profilometer. The molybdenum atomic percentage Mo / (W+Mo) increased linearly from 2.1 at% at the first end to 6.0 at% at the second end, consistent with the doping gradient in Example 1.
[0118] The solid electrolyte layer, ion storage layer, top ITO layer, etching, edge sealing and busbar fabrication are all the same as in Example 1, with 5 equally spaced drive zones set along the X direction.
[0119] The performance test results are as follows: the tinted visible light transmittance at 9 sampling points along the X direction decreased from 73.5% at the first end to 65.2% at the second end, a difference of only 8.3 percentage points, far less than the 50.9 percentage points (64.8% → 13.9%) in Example 1. The linear correlation coefficient R of the visible light transmittance change curve is... 2 =0.978, although showing a certain linear trend, the transmittance change is too small to produce a clear sense of gradual gradation in the human eye. In the 800~2500nm near-infrared band, the modulation depth increases from 18% at the first end to 45% at the second end, and the linear correlation coefficient R of the modulation depth change curve is... 2 =0.981, linearity is acceptable, but the absolute value of modulation depth is low—18% at the thin end, similar to 21% in Example 1, but 45% at the thick end, much lower than 61% in Example 1. The coloring response time at 3.0V step is 5.0s~6.5s (due to uniform film thickness, the response is relatively fast), and the fading response time at -3.0V is 7.0s~9.5s. After 3000 cycles of ±3.0V square wave, the modulation depth retention rate at 633nm is 86.5%. After aging at 85℃ / 85%RH for 1000h, R... 2 =0.955.
[0120] Comparative Example 3 The difference between this comparative example and Example 1 is that the electrochromic active layer has neither a film thickness gradient nor a doping concentration gradient; that is, the film thickness and Mo doping concentration remain constant along the X direction. All other process conditions are exactly the same as in Example 1.
[0121] The substrate was selected as ultra-white low-iron float glass with dimensions of 300mm × 500mm and a thickness of 3.0mm. The cleaning, plasma activation, anti-reflective coating, and ITO deposition parameters were all consistent with those in Example 1.
[0122] The electrochromic active layer was co-sputtered using a dual-target system. The primary target was a WO3 ceramic target (99.99% purity) with a fixed RF power of 200W; the secondary target was a Mo metal target (99.95% purity) with a fixed DC power of 12.5W. The working gas was Ar / O2 = 20 sccm / 1 sccm, with a working pressure of 0.5 Pa and a substrate temperature of 250℃. No mask was used; the substrate stage was moved in a uniform reciprocating motion perpendicular to the X-axis for a fixed deposition time of 3.75 min. The resulting film thickness remained constant along the X-axis, measured by a profilometer as 148 ± 4 nm. The molybdenum atomic percentage (Mo / (W+Mo)) remained constant along the X-axis, measured by XPS as 4.1 at%. This comparative example demonstrates that the film thickness and doping concentration are completely uniform across the entire glass substrate, with no spatial gradient.
[0123] The solid electrolyte layer, ion storage layer, top ITO layer, etching, edge sealing, and busbar fabrication were all the same as in Example 1. Since the active layer is a homogeneous film, no zoned driving was required, but five busbar electrodes were still fabricated for comparative testing.
[0124] The performance test results are as follows: The average visible light transmittance in the tinted state at 9 sampling points along the X direction is 33.5±1.2%, with a maximum deviation of only 1.2 percentage points, indicating that the entire glass exhibits uniform transmittance after tinting, without any spatial gradient effect. The average visible light transmittance in the faded state is 84.2±0.8%. In the near-infrared band of 800nm~2500nm, the average modulation depth is 46±2%, also without spatial variation. The tinting response time at 3.0V step is 5.8s, and the fading response time at -3.0V is 8.2s. After 3000 cycles of ±3.0V square wave, the modulation depth retention rate at 633nm is 86.8%.
[0125] The comparison of the three comparative examples is summarized in Table 3.
[0126] Table 3 Summary and Comparison
[0127] As shown in the table above, although Comparative Example 1 can produce a sufficient range of visible light transmittance variation, the spatial linearity of the near-infrared modulation depth is severely degraded (R0). 2 =0.862), and both the cycling stability and damp heat aging performance were unqualified; Comparative Example 2, although it could maintain the linearity of the near-infrared modulation depth (R 2 =0.981), but the visible light transmittance changes by only 8.3 percentage points, which cannot meet practical requirements; Comparative Example 3 has no spatial gradient capability at all. However, the embodiments of the present invention have both film thickness gradient and doping concentration gradient, which can maintain excellent linearity of near-infrared modulation depth and high absolute value of modulation depth while the visible light transmittance changes significantly, and meet all the requirements of cycle stability and damp heat aging.
Claims
1. An electrochromic coating with gradient spectral selectivity, characterized in that, The coating includes a single-layer electrochromic active layer disposed on a transparent conductive substrate, wherein the electrochromic active layer simultaneously satisfies the following conditions along a first direction of the glass plane: The film thickness increases monotonically from the first end to the second end; The atomic percentage of the dopant element increases monotonically from the first end to the second end; Wherein, the first end corresponds to the high-transmittance field of view region, and its visible light transmittance in the colored state is higher than that of the high-shading shading region corresponding to the second end; and the modulation depth of the electrochromic active layer in the near-infrared band monotonically increases from the first end to the second end along the first direction. The electrochromic active layer is deposited by magnetron sputtering. The monotonically increasing film thickness is achieved by linearly moving the mask, and the monotonically increasing concentration of doped elements is achieved by linearly increasing the auxiliary target power during co-sputtering.
2. The electrochromic coating with gradient spectral selectivity according to claim 1, characterized in that, The thickness of the electrochromic active layer increases monotonically from 60nm~100nm to 180nm~250nm from the first end to the second end, and the atomic percentage of the doped element increases monotonically from 1at%~3at% to 5at%~8at% from the first end to the second end.
3. The electrochromic coating with gradient spectral selectivity according to claim 1, characterized in that, The electrochromic active layer is made of molybdenum-doped tungsten oxide, with the chemical formula Mo. x W 1-x O3, wherein x increases linearly from 0.01 to 0.03 to 0.05 to 0.08 along the first direction, and the electrochromic active layer is an amorphous structure.
4. The electrochromic coating with gradient spectral selectivity according to claim 3, characterized in that, The thickness of the electrochromic active layer increases linearly from 80 nm to 220 nm along the first direction, and the atomic percentage of molybdenum Mo / (W+Mo) increases linearly from 2 at% to 6 at% along the first direction.
5. The electrochromic coating with gradient spectral selectivity according to claim 1, characterized in that, The coating also includes an ion storage layer and a solid electrolyte layer stacked sequentially. The solid electrolyte layer is disposed between the electrochromic active layer and the ion storage layer, and the solid electrolyte layer is a lithium-ion conductor doped with aluminum, wherein the molar ratio of lithium to aluminum is 3~5:
1.
6. The electrochromic coating with gradient spectral selectivity according to claim 5, characterized in that, The solid electrolyte layer is made of at least one of lithium phosphorus oxynitride, aluminum-doped lithium phosphate, or lithium aluminum phosphorus oxide. The thickness of the solid electrolyte layer is 200 nm to 500 nm, and its ionic conductivity at 25°C is 1 × 10⁻⁶. -6 S / cm ~ 1×10 - 4 S / cm.
7. The electrochromic coating with gradient spectral selectivity according to claim 5, characterized in that, The ion storage layer is made of copper-doped nickel oxide, with the chemical formula Cu. y Ni 1-y O, where y is 0.08~0.15, and the ion storage layer is a neutral coloring material, whose chromatic coordinates in the colored state are... Value and The absolute values of all values are less than 5.
8. The electrochromic coating with gradient spectral selectivity according to claim 1, characterized in that, The opening width of the linear moving mask increases linearly along the first direction, the mask moving speed is 50mm / min to 120mm / min, and the auxiliary target is a molybdenum metal target, whose DC sputtering power increases linearly from 3W to 8W to 15W to 25W along the first direction.
9. The electrochromic coating with gradient spectral selectivity according to claim 1, characterized in that, The coating also includes a plurality of independently driven transparent conductive electrode regions arranged along the first direction. The plurality of independently driven transparent conductive electrode regions divide the electrochromic active layer into 3 to 8 driving partitions along the first direction. Each driving partition is connected to an independent voltage control unit, and the driving voltage range of each driving partition is 0.5V to 3.5V.
10. The electrochromic coating with gradient spectral selectivity according to claim 9, characterized in that, The plurality of independently driven transparent conductive electrode regions are five in number, and are equally spaced along the first direction. Their driving voltages from the first end to the second end are 0.8V~1.5V, 1.5V~2.0V, 2.0V~2.5V, 2.5V~2.8V and 2.8V~3.2V respectively.
Citation Information
Patent Citations
Light control glass and vehicle
CN117818310B