Resist underlayer film material, pattern forming method, and resist underlayer film forming method

By using a multilayer photoresist method with a photoresist underlayer material of a specific structure, the problems of reduced resolution and insufficient etch selectivity caused by thinning of photoresist films are solved. This enables the formation of photoresist underlayers with high etch resistance and flatness in semiconductor manufacturing, and is suitable for the micro-patterning of complex substrate structures.

CN123156522APending Publication Date: 2026-11-24SHIN ETSU CHEMICAL CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202610686335.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2025-05-22
Filing Date
2026-05-19
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

In existing semiconductor manufacturing technologies, as patterns become finer and photoresist films become thinner, resolution decreases, aspect ratio increases, pattern collapses, and etching selectivity is insufficient, making it difficult to form a photoresist underlayer film with high etch resistance and flatness on the substrate.

Method used

The multilayer resist method is adopted, using a resist lower layer film material with a specific structure. This material contains a compound or resin with a specific ratio of general formula (2) and general formula (3) terminal group structure, combined with an organic solvent, and forms a resist lower layer film through heat treatment, thereby improving flatness, film formation and etching characteristics.

Benefits of technology

In areas where planarization is difficult, such as wide trench structures, a resist underlayer film with excellent planarity and film-forming properties is formed, exhibiting appropriate etching characteristics. It is suitable for fine patterning in multilayer resist methods, and is especially effective in mitigating substrate unevenness and height differences in semiconductor device manufacturing, thereby improving pattern transfer effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123156522A_ABST
    Figure CN123156522A_ABST
Patent Text Reader

Abstract

The present invention relates to a resist underlayer film material, a pattern forming method, and a resist underlayer film forming method. The present invention provides a resist underlayer film material that forms a resist underlayer film having excellent planarity and film formability even on a processed substrate having a portion with planarization difficulty, and further gives a resist underlayer film having appropriate etching characteristics. A resist underlayer film material contains (A) a compound or a resin represented by the following general formula (1), and (B) an organic solvent. In the formula, Y is either of a terminal group structure represented by the following general formula (2) and a terminal group structure represented by the following general formula (3), and when the proportion of the terminal group structure represented by the following general formula (2) and the terminal group structure represented by the following general formula (3) that constitute the Y is a and b, respectively, the following relationships are satisfied: a + b = 1.0, 0.70 ≤ a ≤ 0.99, and 0.01 ≤ b ≤ 0.30, and n is an integer of 1 to 10.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a resist underlayer film material that can be used for micro-patterning using a multilayer resist method in the semiconductor device manufacturing process, a patterning method using the material, and a resist underlayer film formation method. Background Technology

[0002] With the increasing integration and speed of LSI (Lithium-ion Sensor), the miniaturization of pattern sizes has progressed rapidly. Photolithography, along with this miniaturization, has achieved the formation of fine patterns through the shortening of light source wavelengths and the appropriate selection of corresponding resist compositions. At its core is the use of a single-layer positive photoresist composition. This single-layer positive photoresist composition utilizes a switching mechanism where the resist resin contains a framework resistant to dry etching using chlorine-based or fluorine-based gas plasmas, and the exposed area dissolves. This dissolution of the exposed area forms a pattern, and the remaining resist pattern serves as an etching mask for dry etching of the substrate.

[0003] However, when the thickness of the photoresist film used is directly reduced, that is, when the pattern width is reduced, the resolution of the photoresist film decreases. Furthermore, if the photoresist film is to be developed using a developer, the aspect ratio will become too large, resulting in pattern collapse. Therefore, as the pattern becomes finer, the photoresist film becomes thinner and thinner.

[0004] On the other hand, the processing of substrates typically involves using a patterned photoresist film as an etching mask and employing dry etching. However, in reality, no dry etching method can achieve complete etch selectivity between the photoresist film and the substrate. Therefore, the photoresist film can be damaged and collapse during substrate processing, preventing the accurate transfer of the photoresist pattern onto the substrate. Consequently, with the miniaturization of patterns, there is an increasing demand for photoresist compositions with higher dry etching resistance. However, to improve resolution, there is a growing need for photoresist compositions using resins with low light absorption at the exposure wavelength. Therefore, as the exposure light becomes shorter wavelengths such as i-rays, KrF, and ArF, the resins have gradually changed to phenolic varnish resins, polyhydroxystyrene, and resins with aliphatic polycyclic skeletons. However, in reality, the etching rate under dry etching conditions during substrate processing is becoming increasingly faster, and the most recent photoresist compositions with high resolution tend to have reduced etching resistance.

[0005] Therefore, it becomes necessary to use thinner photoresist films with weaker etching resistance to dry etch the substrates being processed, and ensuring the quality of materials and processing in this step is important.

[0006] One method to solve this problem is the multilayer resist method. This method involves inserting an intermediate film with a different etching selectivity than the photoresist film (i.e., the upper resist film) between the upper resist film and the substrate being processed. After the upper resist film is patterned, the pattern is used as a dry etching mask to transfer the pattern onto the intermediate film using dry etching. Then, the intermediate film is used as a dry etching mask to transfer the pattern onto the substrate being processed using dry etching.

[0007] One type of multilayer photoresist method is the three-layer photoresist method, which can be performed using common photoresist compositions used in single-layer photoresist methods. This three-layer photoresist method involves, for example, forming an organic film such as phenolic varnish resin on the substrate as the lower photoresist film, forming a silicon-containing film on top of it as the intermediate photoresist film, and forming a conventional organic photoresist film on top of it as the upper photoresist film. When dry etching using fluorine-based gas plasma, the organic upper photoresist film exhibits good etch selectivity for the silicon-containing intermediate photoresist film, so the pattern of the upper photoresist film can be transferred onto the silicon-containing intermediate photoresist film using dry etching with fluorine-based gas plasma. According to this method, even if a resist composition that is difficult to form with a pattern having sufficient film thickness for direct processing of the substrate is used, or a resist composition that does not have sufficient dry etching resistance for substrate processing is used, a pattern can still be transferred onto a silicon-containing film (resist intermediate film). If the pattern transfer is then performed using dry etching with oxygen-based or hydrogen-based gas plasma, a pattern of an organic film (resist underlayer film) with sufficient dry etching resistance for substrate processing, such as phenolic varnish resin, can be obtained. Such resist underlayer films, such as those described in Patent Document 1, are already well known.

[0008] In recent years, research on the fabrication of semiconductor devices with novel structures such as multi-gate structures has been actively underway. Correspondingly, there is a growing demand for superior flatness and filling properties in the underlayer resist compared to previous methods. For example, when the substrate being processed has micro-patterned structures such as holes, trenches, and fins, the underlayer resist is required to fill the gaps within the patterns. Furthermore, when the substrate being processed has height differences, or when there are densely patterned areas and unpatterned regions on the same wafer, the underlayer resist is needed to planarize the film surface. By planarizing the surface of the underlayer resist, thickness variations in the overlying intermediate and upper resist films can be suppressed, and the focus tolerance of photolithography and the tolerance of subsequent substrate processing steps can be prevented from decreasing.

[0009] Furthermore, organic film materials with excellent packing properties and flatness are not limited to the lower layer film for multilayer photoresists. For example, they can also be widely used as planarization materials in semiconductor device manufacturing, such as substrate planarization before patterning using nanoimprinting. Moreover, CMP is generally used for overall planarization in semiconductor device manufacturing processes. However, CMP is a high-cost process, and there is a need for alternative materials to replace CMP as materials for overall planarization.

[0010] To form a planarization film for planarizing uneven semiconductor substrates, a resist underlayer material containing a low-viscosity and high-thermal-flow compound has been proposed (Patent Document 2). However, this material, for example, exhibits significantly reduced moisture permeability on hydrophobic substrates treated with hexamethyldisilazane (hereinafter referred to as HMDS), leading to problems such as pinholes and film edge recession. Furthermore, in state-of-the-art devices, the resist underlayer film also thins as the patterned upper layer film is miniaturized, making it more difficult to ensure moisture permeability. To improve the moisture permeability of the underlayer material and enhance adhesion to the substrate, a resist underlayer material with an amide structure as a polar functional group has been proposed (Patent Document 3). However, while this resist underlayer material combines moisture permeability and planarization on silicon substrates, its moisture permeability on hydrophobic substrates remains insufficient. Therefore, there is a need for a lower film material that balances excellent flatness, moisture permeability to hydrophobic substrates, and sufficient etch resistance, as well as a patterning method for using it.

[0011] Furthermore, as mentioned above, the structure of the substrate being processed has become more complex. Consequently, research has been conducted on the use of novel materials with high electron mobility, such as strained silicon and gallium arsenide, as well as ultrathin polycrystalline silicon with angstrom-level cell control, with the aim of forming films on a wide variety of substrate surface shapes and materials. Therefore, in order to ensure processing tolerance, not only excellent flatness but also the ability to form films regardless of the material and shape of the substrate has become an important characteristic.

[0012] Existing technical documents

[0013] Patent documents

[0014] [Patent Document 1] Japanese Patent Application Publication No. 2004-205685

[0015] [Patent Document 2] Japanese Patent Application Publication No. 2017-119670

[0016] [Patent Document 3] Japanese Patent Application Publication No. 2021-196467 Summary of the Invention

[0017] (The problem the invention aims to solve)

[0018] In view of the above, the present invention aims to provide a photoresist underlayer film material that can form a photoresist underlayer film with excellent planarity and film-forming properties even on a substrate with particularly difficult planarization areas such as wide trench structures during the micro-patterning process of semiconductor device manufacturing, thereby providing a photoresist underlayer film material with appropriate etching characteristics, and a patterning method and a photoresist underlayer film forming method using the material.

[0019] (Methods for solving problems)

[0020] To address the aforementioned issues, the present invention provides a resist underlayer film material, characterized by containing (A) a compound or resin represented by the following general formula (1), and

[0021] (B) Organic solvents.

[0022] [Chemistry 1]

[0023]

[0024] In the formula, W is an n-valent organic group with 2 to 50 carbon atoms. Y is any of the terminal group structures represented by the following general formula (2) and general formula (3), wherein when the proportions of the terminal group structures represented by the following general formula (2) and general formula (3) constituting the aforementioned Y are a and b respectively, the following relationships are satisfied: a + b = 1.0, 0.70 ≤ a ≤ 0.99, and 0.01 ≤ b ≤ 0.30. n is an integer from 1 to 10.

[0025] [Chemistry 2]

[0026]

[0027] In the formula, dashed lines represent atomic bonds. Z represents an aromatic group with 6 to 20 carbon atoms and a (m+1) valence. A is a single bond or -O-(CH2). p - m is an integer from 1 to 5. p is an integer from 1 to 10.

[0028] [Chemistry 3]

[0029]

[0030] In the formula, the dashed lines represent atomic bonds.

[0031] If such a resist underlayer material is used, then in the micro-patterning process using the multilayer resist method, even on the substrate with particularly difficult planarization areas such as wide trench structures, a resist underlayer film with excellent planarity and film-forming properties can still be formed. This underlayer film exhibits more suitable etching characteristics and can form a resist underlayer film with excellent film-forming properties, for example, for hydrophobic substrates treated with HMDS. Furthermore, if the resist underlayer material has proportions a and b as described above, a resist underlayer film with a suitable balance between planarity and film-forming properties can be formed. In particular, by introducing the terminal group structure represented by the above general formula (2), opposing properties such as thermal fluidity and heat resistance can be balanced. Moreover, by introducing the terminal group structure represented by the above general formula (3), adhesion to the substrate can be imparted, and the film-forming properties can be further improved. In particular, it is effective in suppressing the retreat of film edges.

[0032] Furthermore, it is preferable that A in the aforementioned general formula (2) is -OCH2-.

[0033] If the resist underlayer material is such, the film shrinkage (shrinkage) caused by thermosetting is suppressed, resulting in a resist underlayer material with better flatness.

[0034] Furthermore, it is preferable that the aforementioned general formula (2) is any of the following general formulas (4), (5) and (6).

[0035] [Chemistry 4]

[0036]

[0037] In the formula, the dashed lines represent atomic bonds.

[0038] If the resist underlayer material is of this type, it will not only improve the flatness due to shrinkage inhibition, but also endow it with many properties such as heat resistance and etching resistance, thus forming a resist underlayer film with better processing margin.

[0039] Furthermore, it is preferable that W in the aforementioned general formula (1) is represented by the following general formula (7).

[0040] [Chemistry 5]

[0041]

[0042] In the formula, dashed lines represent atomic bonds. R 1 It is a hydrogen atom, or an alkyl or acyl group having 1 to 20 carbon atoms. The aforementioned alkyl or acyl groups may also contain an oxygen atom and / or a nitrogen atom. 1 Y is an n-valent organic group with 1 to 47 carbon atoms. 1 It can be a single bond or a carbonyl group. n is an integer from 1 to 10.

[0043] By having W in the aforementioned general formula (1) having a partial structure represented by the aforementioned general formula (7), the resist underlayer film material of the present invention can be given better thermal fluidity, and thus better flatness.

[0044] In this case, W in the aforementioned general formula (7) 1 The structure represented by any of the following expressions is better.

[0045] [Chemistry 6]

[0046]

[0047] [Chemistry 7]

[0048]

[0049] In the formula, the dashed lines represent atomic bonds.

[0050] Such a resist underlayer material can form a resist underlayer film with better film-forming properties and flatness, and can be manufactured particularly easily.

[0051] Furthermore, it is preferable that the polystyrene equivalent weight-average molecular weight of the aforementioned compound (A) or resin is below 3,000.

[0052] Such a resist underlayer material has low viscosity, high thermal fluidity, and excellent flatness, and can form a resist underlayer film that combines such excellent flatness with film-forming properties for hydrophobic substrates.

[0053] Furthermore, it is preferable that the aforementioned organic solvent (B) is a mixture of one or more organic solvents with a boiling point of less than 180°C and one or more organic solvents with a boiling point of 180°C or higher.

[0054] If such a resist underlayer material is used, the flatness of the formed resist underlayer film can be better without relying on the design of the substrate such as the density of the pattern.

[0055] The resist lower film material of the present invention may further contain selected...

[0056] (C) Alkali-generating agents

[0057] (D) Surfactants,

[0058] (E) Crosslinking agent,

[0059] (F) Plasticizers, and

[0060] (G) pigment

[0061] One or more of the groups formed.

[0062] Thus, in the resist lower film material of the present invention, in order to suppress the retreat of the film edge, (C) an alkali generating agent may be added; in order to improve the coatability during spin coating, (D) a surfactant may be added; in order to further promote the crosslinking and curing reaction, (E) a crosslinking agent may be added; in order to further improve the filling properties and / or flatness, (F) a plasticizer may be added; and in order to adjust the light absorption properties, (G) a pigment may be added. By the presence or absence / selection of these various additives, the performance can be fine-tuned according to the requirements of film formation, curing, filling, optical properties, etc., which is ideal for practical use.

[0063] Furthermore, it is preferable that the aforementioned (C) alkali-generating agent is a compound that exhibits alkalinity due to thermal decomposition.

[0064] If the resist is used as the underlying film material, then during film firing, the three adjacent hydroxyl groups in component (A) exhibit ionicity, thus increasing the interaction with the substrate. Therefore, it is assumed that better film-forming properties can be achieved. By adjusting the amount added, both excellent thermal fluidity and ideal interaction with the substrate can be achieved.

[0065] Furthermore, it is preferable that the base generating agent mentioned above (C) is a compound represented by any of the following general formulas (8), (9) and (10).

[0066] [Chemistry 8]

[0067]

[0068] In the above formula, R 01 ~R 03 Each can independently represent a linear, branched, or cyclic alkyl or alkenyl group with 1 to 10 carbon atoms that can be substituted with or have heteroatom insertions, or an aryl or aralkyl group with 6 to 18 carbon atoms that can be substituted with or have heteroatom insertions. Also, R 01 R 02 and R 03 Any two of them can also bond to each other and form a ring together with the sulfur atom in the formula. X - This refers to anions that are organic or inorganic and can be considered as relative ions. However, X... - Excluding OH - R 04 and R 05 Each aryl group is independently composed of 6 to 20 carbon atoms, and some or all of the hydrogen atoms in this aryl group may be substituted by straight-chain, branched, or cyclic alkyl or alkoxy groups having 1 to 10 carbon atoms. Also, R 04 and R 05 They can also bond with each other and form a ring together with the iodine atom in the formula. R 06 R 07 R 08 and R 09Each can independently represent a hydrogen atom, or a linear, branched, or cyclic alkyl or alkenyl group with 1 to 20 carbon atoms that may be substituted with heteroatoms or have heteroatom insertions, or an aryl or aralkyl group with 6 to 18 carbon atoms that may be substituted with heteroatoms or have heteroatom insertions. Also, R 06 R 07 R 08 and R 09 Any two or more of them can bond with each other and form a ring together with the nitrogen atom in the formula.

[0069] Furthermore, the aforementioned anion X in the aforementioned general formulas (8), (9) and (10) - It is preferable to select ions with structures represented by any of the following general formulas (11), (12) and (13), and anions from the group consisting of chloride ions, bromide ions, iodide ions, fluoride ions, cyanide ions, nitrate ions and nitrite ions.

[0070] [Chemistry 9]

[0071]

[0072] In the above formula, R 10 This indicates a linear, branched, or cyclic alkyl, alkenyl, aralkyl, or aryl group with 1 to 20 carbon atoms, which may also contain an ether group, ester group, or carbonyl group. One or more hydrogen atoms in these groups may also be substituted with halogen atoms, hydroxyl groups, carboxyl groups, amino groups, and / or cyano groups. R 11 This indicates an aryl group with 6 to 20 carbon atoms. One or more hydrogen atoms in this aryl group may also be substituted with halogen atoms, hydroxyl groups, carboxyl groups, amino groups, and / or cyano groups. R 12 R 13 and R 14 Each group independently represents a hydrogen atom, or a halogen atom other than fluorine, or may contain an ether group, ester group, or carbonyl group, and is a straight-chain, branched, or cyclic alkyl, alkenyl, aralkyl, or aryl group with 1 to 20 carbon atoms. One or more hydrogen atoms in these groups may also be substituted with a halogen atom, hydroxyl group, carboxyl group, amino group, and / or cyano group. Also, R 12 R 13 and R 14 Two or more of them can also bond together to form a ring.

[0073] Furthermore, X in the aforementioned general formulas (8), (9) and (10) - The boiling point of the conjugate acid XH is below 200℃, which is even better.

[0074] By appropriately selecting an alkali-generating agent that exhibits alkalinity due to thermal decomposition (thermal alkali-generating agent), the alkalinity can be adjusted according to the firing temperature of the underlying film material of the photoresist, thus more reliably balancing film formation and flatness. Furthermore, during firing, it completely decomposes or evaporates and does not remain in the fired film, therefore it does not adversely affect properties other than film formation. Also, in this specification, the boiling point is the value at 1 atm (1013 hPa).

[0075] Furthermore, the aforementioned (E) crosslinking agent is preferably a compound represented by the following general formula (14).

[0076] [Chemistry 10]

[0077]

[0078] In the formula, Q is a single bond or a q-valent hydrocarbon group with 1 to 20 carbon atoms. R 16 It is hydrogen or an alkyl group having 1 to 20 carbon atoms. q is an integer from 1 to 5.

[0079] If such a crosslinking agent is used, the crosslinking reaction will still proceed even without the presence of an acid-generating agent, thus achieving improved curing properties without compromising the film-forming properties of the alkali-generating agent. Furthermore, the crosslinking agent represented by general formula (14) contains phenolic hydroxyl groups, so it is expected that a higher improvement in film-forming properties can be achieved through the action of the alkali-generating agent.

[0080] Furthermore, the present invention provides a pattern forming method, which is a method for forming a pattern on a substrate being processed, characterized by the following steps:

[0081] (I-1) A coating film is obtained by coating the resist underlayer film material of the present invention onto a substrate to be processed, and the coating film is heat-treated to form a resist underlayer film.

[0082] (I-2) On the aforementioned lower resist film, an upper resist film is formed using a photoresist material.

[0083] (I-3) The aforementioned upper layer of the photoresist is exposed to a pattern, and then developed with a developer to form a pattern on the aforementioned upper layer of the photoresist.

[0084] (I-4) Using the upper resist film with the aforementioned pattern as a mask, dry etch the lower resist film to transfer the pattern onto the lower resist film.

[0085] (I-5) Using the patterned resist lower layer film as a mask, the substrate to be processed is processed to form a pattern on the substrate to be processed.

[0086] Furthermore, the present invention provides a pattern forming method, which is a method for forming a pattern on a substrate being processed, characterized by the following steps:

[0087] (II-1) A coating film is obtained by coating the resist underlayer film material of the present invention onto a substrate to be processed, and the coating film is heat-treated to form a resist underlayer film.

[0088] (II-2) An intermediate resist film is formed on the aforementioned lower resist film.

[0089] (II-3) On the aforementioned intermediate resist film, a photoresist material is used to form an upper resist film.

[0090] (II-4) The aforementioned photoresist upper film is exposed to a pattern, and then developed with a developer to form a pattern on the aforementioned photoresist upper film.

[0091] (II-5) Using the upper resist film with the aforementioned pattern as a mask, dry etch the aforementioned intermediate resist film to transfer the pattern onto the intermediate resist film.

[0092] (II-6) Using the resist intermediate film with the aforementioned pattern transferred as a mask, dry etch the aforementioned resist lower layer film to transfer the pattern onto the aforementioned resist lower layer film, and

[0093] (II-7) Using the patterned resist lower layer film as a mask, the above-mentioned substrate is processed to form a pattern on the substrate.

[0094] Furthermore, the present invention provides a pattern forming method, which is a method for forming a pattern on a substrate being processed, characterized by the following steps:

[0095] (III-1) A coating film is obtained by coating the resist underlayer film material of the present invention onto the substrate to be processed, and the coating film is heat-treated to form a resist underlayer film.

[0096] (III-2) An inorganic hard mask intermediate film, selected from the group consisting of silicon oxide film, silicon nitride film, and silicon oxide nitride film, is formed on the aforementioned photoresist lower layer film.

[0097] (III-3) An organic thin film is formed on the aforementioned inorganic hard mask intermediate film.

[0098] (III-4) A photoresist top layer film is formed on the aforementioned organic thin film using a photoresist material.

[0099] (III-5) The aforementioned upper layer of the photoresist is exposed to a pattern, and then developed with a developer to form a pattern on the aforementioned upper layer of the photoresist.

[0100] (III-6) Using the resist film with the aforementioned pattern as a mask, dry etch the aforementioned organic thin film and the aforementioned inorganic hard mask intermediate film to transfer the pattern onto the aforementioned organic thin film and the aforementioned inorganic hard mask intermediate film.

[0101] (III-7) Using the aforementioned inorganic hard mask intermediate film with the transferred pattern as a mask, dry etch the aforementioned photoresist underlayer film to transfer the pattern onto the aforementioned photoresist underlayer film, and

[0102] (III-8) Using the patterned resist lower layer film as a mask, the above-mentioned substrate is processed to form a pattern on the substrate.

[0103] Thus, the resist lower layer film material of the present invention can be ideally used in various pattern forming methods such as 2-layer resist processing, 3-layer resist processing using a resist intermediate film, and 4-layer resist processing using an organic thin film. In these pattern forming methods, the formation of the resist lower layer film can effectively mitigate the unevenness and / or height difference of the substrate being processed, making it suitable for optical lithography of the resist upper layer film.

[0104] Furthermore, the pattern forming method of the present invention can utilize CVD or ALD to form the aforementioned inorganic hard mask intermediate film.

[0105] The patterning method of the present invention, for example, can combine an inorganic hard mask intermediate film formed by CVD or ALD with a photoresist underlayer film formed by spin coating.

[0106] Furthermore, in the pattern forming method of the present invention, a structure with a height of 30 nm or more or a substrate with a height difference can be used as the substrate to be processed.

[0107] Furthermore, in the pattern forming method of the present invention, a substrate with a static contact angle of 50° or more with water can be used as the substrate to be processed.

[0108] The resist underlayer film material of the present invention has excellent filling characteristics / flatness and film-forming properties for hydrophobic substrates, and is particularly useful in the microprocessing of substrates with such structures or height differences.

[0109] Furthermore, the present invention provides a method for forming a photoresist underlayer film, which is a method for forming a photoresist underlayer film acting as an organic planarization film used as a manufacturing step of a semiconductor device, characterized by comprising the following steps:

[0110] The resist lower layer film material of the present invention is spin-coated onto the substrate to be processed, and

[0111] The substrate coated with the aforementioned photoresist underlayer film material is heat-treated at a temperature between 100°C and 600°C for 10 to 600 seconds to harden and form the photoresist underlayer film.

[0112] Furthermore, the present invention provides a method for forming a photoresist underlayer film, which is a method for forming a photoresist underlayer film acting as an organic planarization film used as a manufacturing step of a semiconductor device, characterized by comprising the following steps:

[0113] The resist lower layer film material of the present invention is spin-coated onto the substrate to be processed.

[0114] The substrate coated with the aforementioned photoresist underlayer film material is heat-treated in a gas environment with an oxygen concentration of 1% or more and 21% or less to harden and form a photoresist underlayer film.

[0115] This method promotes the cross-linking reaction during the formation of the resist underlayer film, and further suppresses mixing with the upper layer film. Furthermore, by appropriately adjusting the heat treatment temperature, time, and oxygen concentration within the aforementioned ranges, suitable application properties such as packing characteristics / flatness and hardening characteristics of the resist underlayer film can be obtained.

[0116] Furthermore, the present invention provides a method for forming a photoresist underlayer film, which is a method for forming a photoresist underlayer film acting as an organic planarization film used as a manufacturing step of a semiconductor device, characterized by comprising the following steps:

[0117] The resist lower layer film material of the present invention is spin-coated onto the substrate to be processed, and

[0118] The substrate coated with the aforementioned resist underlayer film material is heat-treated in a gas environment with an oxygen concentration of less than 1% by volume to harden and form the resist underlayer film.

[0119] Using this method, even if the substrate being processed contains components that are unstable to heating in an oxygen environment, the substrate can still be protected from degradation. It can also promote the cross-linking reaction during the formation of the lower resist film and suppress mixing with the upper film to a greater extent, which is useful.

[0120] Alternatively, a structure with a height of 30 nm or more or a substrate with a height difference can be used as the aforementioned substrate to be processed.

[0121] Furthermore, a substrate with a static contact angle of 50° or more with water can be used as the aforementioned substrate for processing.

[0122] The method for forming a resist underlayer film of the present invention uses the resist underlayer film material of the present invention, which is capable of forming a resist underlayer film with excellent filling characteristics and / or flatness and film-forming properties for hydrophobic substrates, and is particularly suitable for forming a resist underlayer film on a substrate having such a structure or height difference.

[0123] (The effect of the invention)

[0124] As explained above, the resist underlayer material of the present invention, in the micro-patterning process using the multilayer resist method, can still form a resist underlayer film with excellent planarity and film-forming properties, even on the substrate being processed where planarization is particularly difficult, such as wide trench structures. This underlayer film can exhibit appropriate etching characteristics. Therefore, the resist underlayer material, patterning method, and resist underlayer film formation method of the present invention are particularly suitable for planarization of multilayer resist processes using substrates with elevation differences and unevenness, and are extremely useful for micro-patterning in semiconductor device manufacturing. Especially in the micro-patterning process using multilayer resist in semiconductor device manufacturing, even without acid generators, even on substrates with particularly difficult planarization areas such as wide trench structures, excellent planarity is still achieved, allowing the formation of a substrate-independent resist underlayer film. This provides resist underlayer film materials with appropriate etching / optical properties, patterning methods using the aforementioned materials, and resist underlayer film formation methods. In particular, the three adjacent hydroxyl groups of the terminal structure represented by general formula (3) in compound (A) or resin exhibit strong interaction with the substrate surface, thereby suppressing pinholes and edge shrinkage (receding) even when forming a resist underlayer film on a wafer that has undergone hydrophobic treatment such as HMDS treatment. Attached Figure Description

[0125] [ Figure 1 [Illustrative diagram of an example of the pattern forming method of the present invention using a three-layer resist treatment.]

[0126] [ Figure 2 [Illustrative diagram of the edge retreat evaluation method in the embodiment.]

[0127] [ Figure 3 [Illustrative diagram of the landfill characteristic evaluation method in the embodiments]

[0128] [ Figure 4 [Illustrative diagram of the flatness evaluation method in the embodiments] Detailed Implementation

[0129] As mentioned above, the aim is to develop a resist underlayer material that can form a resist underlayer with excellent film-forming properties and planarity, even on a substrate with areas particularly difficult to planarize, such as wide trench structures, during the micro-patterning process using a multilayer resist method in the semiconductor device manufacturing process, thereby possessing excellent embedding properties, appropriate etching properties, and optical properties, as well as a patterning method and a resist underlayer film formation method using the aforementioned material.

[0130] In order to achieve a high degree of embedding properties and / or flatness and excellent film-forming properties in multilayer photolithography using a resist underlayer film, the inventors of this application explored various resist underlayer film materials and patterning methods. As a result, it was discovered that if a resist underlayer film material containing a portion of a terminal group structure having three adjacent hydroxyl groups and a portion that imparts thermal fluidity to other portions of the terminal group structure before curing and can induce a curing reaction through a rigid ring structure is used as the main component, then even on a substrate with particularly difficult-to-planarize areas, a resist underlayer film with excellent flatness and film-forming properties can still be formed. This underlayer film further exhibits suitable etching properties, thus completing the present invention.

[0131] That is, the present invention provides a resist lower film material, characterized by containing

[0132] (A) The compounds or resins represented by the following general formula (1), and

[0133] (B) Organic solvents.

[0134] [Chemistry 11]

[0135]

[0136] In the formula, W is an n-valent organic group with 2 to 50 carbon atoms. Y is any of the terminal group structures represented by the following general formula (2) and general formula (3), wherein when the proportions of the terminal group structures represented by the following general formula (2) and general formula (3) constituting the aforementioned Y are a and b respectively, the following relationships are satisfied: a + b = 1.0, 0.70 ≤ a ≤ 0.99, and 0.01 ≤ b ≤ 0.30. n is an integer from 1 to 10.

[0137] [Chemistry 12]

[0138]

[0139] In the formula, dashed lines represent atomic bonds. Z represents an aromatic group with 6 to 20 carbon atoms and a (m+1) valence. A is a single bond or -O-(CH2). p - m is an integer from 1 to 5. p is an integer from 1 to 10.

[0140] [Chemistry 13]

[0141]

[0142] In the formula, the dashed lines represent atomic bonds.

[0143] The present invention will be described in detail below, but the present invention is not limited thereto.

[0144] <Resistant Underlayer Film Material>

[0145] The resist underlayer material of the present invention, for example, is a resist underlayer material that can be used in the multilayer resist method described above, containing...

[0146] (A) Compounds or resins represented by the following general formula (1), and (B) organic solvents.

[0147] [Chemistry 14]

[0148]

[0149] In the formula, W is an n-valent organic group with 2 to 50 carbon atoms. Y is any of the terminal group structures represented by the following general formula (2) and general formula (3), wherein when the proportions of the terminal group structures represented by the following general formula (2) and general formula (3) constituting the aforementioned Y are a and b respectively, the following relationships are satisfied: a + b = 1.0, 0.70 ≤ a ≤ 0.99, and 0.01 ≤ b ≤ 0.30. n is an integer from 1 to 10.

[0150] [Chemistry 15]

[0151]

[0152] In the formula, dashed lines represent atomic bonds. Z represents an aromatic group with 6 to 20 carbon atoms and a (m+1) valence. A is a single bond or -O-(CH2). p - m is an integer from 1 to 5. p is an integer from 1 to 10.

[0153] [Chemistry 16]

[0154]

[0155] In the formula, the dashed lines represent atomic bonds.

[0156] The resist lower film material of the present invention contains (A) a compound or resin represented by the above general formula (1) (hereinafter referred to as "a compound or resin containing three adjacent hydroxyl groups in a portion of the (A) terminal group structure" or (A) component) as a main component, wherein the (A) component contains a portion of the terminal group structure containing a structure having three adjacent hydroxyl groups (the terminal group structure represented by the above general formula (3)) and can impart thermal fluidity to other portions of the terminal group structure and can cause a hardening reaction via a rigid ring structure (the terminal group structure represented by the above general formula (2)).

[0157] More specifically, the terminal group structure of the above general formula (2) functions as a thermosetting group. This terminal group structure contributes as a substituent to impart thermal fluidity before curing, and can induce a curing reaction through the rigid ring structure during curing, thus achieving both the opposite properties of thermal fluidity and heat resistance. Even without an acid-generating agent, the curing reaction will still proceed, thus maximizing the effect of the alkali-generating agent.

[0158] Furthermore, the terminal group structure of the above general formula (3) can act as an adhesion group and a film-forming auxiliary group. By having a terminal group structure with three adjacent hydroxyl groups as described in the above general formula (3), the affinity with the substrate is improved, resulting in good flatness. In addition, the adhesion to the substrate is improved, thereby preventing the occurrence of pinholes in the film, peeling from the substrate, and shrinkage of the film edge caused during film formation.

[0159] Furthermore, in the resist lower film material of the present invention, a portion of the (A) terminal group structure contains a compound or resin with three adjacent hydroxyl groups. When the ratio of the terminal group structure represented by the above general formula (2) and the terminal group structure represented by the above general formula (3) constituting Y is a and b respectively, it conforms to the relationships a + b = 1.0, 0.70 ≤ a ≤ 0.99, and 0.01 ≤ b ≤ 0.30. With such a ratio a and b containing the terminal group structure represented by the above general formula (2) and the terminal group structure represented by the above general formula (3), a portion of the (A) terminal group structure containing three adjacent hydroxyl groups can achieve an ideal balance of flatness, film-forming properties, and etching characteristics without sacrificing any of these.

[0160] In summary, if the resist underlayer material of the present invention is used, a resist underlayer film with excellent planarity and film-forming properties can still be formed even on a processed substrate with particularly difficult planarization areas, and this underlayer film can further exhibit appropriate etching characteristics.

[0161] The resist lower film material of the present invention may also contain, as an essential component, (A) a compound or resin containing three adjacent hydroxyl groups as part of the terminal group structure, and (B) components other than organic solvents as optional components.

[0162] The necessary and optional components of the resist underlayer film material of the present invention are described in detail below in sequence.

[0163] [(A) Compounds or resins whose terminal group structure contains three adjacent hydroxyl groups]

[0164] In the resist underlayer material of the present invention, the compound or resin containing three adjacent hydroxyl groups in a part of the (A) terminal group structure exhibits excellent substrate affinity. Therefore, it is believed that even on processed substrates with complex microstructures and various surface materials, a resist underlayer film with excellent film-forming properties can still be formed. In particular, it exhibits excellent film-forming properties for hydrophobic substrates treated with HMDS.

[0165] The molecular weight (molecular weight) of the compound or resin containing three adjacent hydroxyl groups in part of the terminal group structure of (A) is preferably 300 to 3,000, and more preferably 500 to 2,500, in terms of the weight-average molecular weight converted from polystyrene. If the molecular weight is 300 or higher, the film-forming properties are excellent, and there is no contamination of the apparatus due to the increase of sublimation during curing. If the molecular weight is 3,000 or lower, the complex viscosity of the resin decreases during firing, thus exhibiting high thermal fluidity and excellent flatness and / or landfill properties. Furthermore, in this invention, the molecular weight can be defined as the weight-average molecular weight (Mw) of polystyrene obtained by gel permeation chromatography (GPC) using tetrahydrofuran as the eluent. The number-average molecular weight (Mn) and the dispersion (Mw / Mn) can also be determined in this manner. The dispersion of component (A) can be 1.0 to 2.5, but the dispersion of the compound containing three adjacent hydroxyl groups in part of the terminal group structure of (A) is preferably 1.0 to 1.5.

[0166] In the aforementioned general formula (2), the dashed lines represent atomic bonds. Z represents an aromatic group with 6 to 20 carbon atoms and a (m+1) valence. Z is an (m+1) valence group that has removed (m+1) hydrogen atoms from an aromatic compound with 6 to 20 carbon atoms. Examples of aromatic compounds with 6 to 20 carbon atoms include benzene, naphthalene, phenanthrene, anthracene, pyrene, biphenyl, toluene, xylene, methylnaphthalene, and fluorene. Considering the thermal fluidity and ease of obtaining raw materials, benzene or naphthalene is preferred. m is an integer from 1 to 5. To obtain good flatness, m is preferred to be 1 to 3. A is a single bond or -O-(CH2). p - where p is an integer from 1 to 10. For good flatness, A is better when it is p = 1 -OCH2-.

[0167] The ideal structure of the aforementioned general formula (2) can be exemplified by the following.

[0168] [Chemistry 17]

[0169]

[0170] In particular, if A in general formula (2) is the (A) component of -OCH2-, it can suppress film shrinkage (shrinkage) caused by thermosetting and form a resist lower layer film with better flatness.

[0171] The ideal structures of the aforementioned general formula (2) can be exemplified by formulas (4) to (6).

[0172] [Chemistry 18]

[0173]

[0174] In the resist lower film material of the present invention, the terminal group structure represented by the above general formula (2) can act as a thermosetting group. As exemplified by formulas (4) to (6) as particularly ideal structures, when the substituent A is -OCH2- with a p=1 relationship and located at the beta position of naphthalene, it is presumed that the thermosetting mechanism is carried out via the ring structure shown in the following reaction formula. In this case, the substituent contributes to the thermal fluidity before curing, but the curing reaction is carried out via a rigid ring structure, so the opposite characteristics of thermal fluidity and heat resistance can be taken into account. Since the curing reaction will still take place without an acid generating agent, the effect of the alkali generating agent can be maximized.

[0175] [Chemistry 19]

[0176]

[0177] In the resist lower film material of the present invention, the terminal group structure represented by the aforementioned general formula (3) can act as an adhesion group and a film-forming auxiliary group. (A) The component has an improved affinity with the substrate and exhibits good flatness by having a terminal group structure with three adjacent hydroxyl groups as represented by the aforementioned general formula (3). Furthermore, the adhesion to the substrate is improved, thereby preventing the occurrence of pinholes in the film, peeling from the substrate, and shrinkage of the film edge caused during film formation.

[0178] Furthermore, when the ratio (terminal group ratio) of the terminal groups in the aforementioned general formulas (2) and (3) constituting the terminal group Y in the aforementioned general formula (1) is a and b respectively, it must satisfy the relationship a + b = 1.0, 0.70 ≤ a ≤ 0.99, 0.01 ≤ b ≤ 0.30 (assuming a + b = 100, 70 ≤ a ≤ 99, 1 ≤ b ≤ 30). More preferably, it is 0.75 ≤ a ≤ 0.97, 0.03 ≤ b ≤ 0.25, and even more preferably, it is 0.80 ≤ a ≤ 0.95, 0.05 ≤ b ≤ 0.20. If the terminal group ratio is adjusted within the above range, thermosetting properties can be maintained while also taking into account flatness and film-forming properties. The terminal group ratio can be calculated using 1H NMR from the terminal group containing a triple bond to the terminal group containing a phenolic hydroxyl group.

[0179] In the aforementioned general formula (1), W is an n-valent organic group with 2 to 50 carbon atoms, and n is an integer from 1 to 10. Therefore, W is a 1 to 10-valent organic group with a structure in which 1 to 10 hydrogen atoms have been removed from an organic compound with 2 to 50 carbon atoms. A compound having an organic group W with 2 to 50 carbon atoms having 1 to 10 hydrogen atoms added to W has at least one of the terminal structures represented by the aforementioned general formulas (2) and (3), and the organic group represented by W may also contain linear, branched, or cyclic saturated or unsaturated hydrocarbon groups, aromatic groups, heteroaromatic groups, ether groups, hydroxyl groups, ester groups, ketone groups, amino groups, halogen groups, thioether groups, carboxyl groups, sulfonyl groups, imide groups, cyano groups, aldehyde groups, imino groups, urea groups, carbamate groups, carbonate groups, nitro groups, sulfonic acid groups, etc. In terms of balancing good flatness and sufficient thermosetting properties, n of 2 to 4 is preferred.

[0180] Depending on the application, the etching resistance, heat resistance, optical properties, polarity, and flexibility of the resist underlayer film material can be adjusted by appropriately selecting W, Y, and n in the compound of the above general formula (1). Among these, regarding optical properties, when the resist underlayer film material has appropriate optical properties at a wavelength of 193 nm, it can suppress reflected light during exposure in multilayer ArF lithography, thus becoming a material with excellent resolution. Furthermore, in order to suppress reflected light, the optical constants of the resist underlayer film material are preferably in the range of a refractive index n of about 1.4 to 1.9 and an attenuation coefficient k of 0.1 to 0.5.

[0181] Furthermore, it is preferable that W in the aforementioned general formula (1) is represented by the following general formula (7).

[0182] [Chemistry 20]

[0183]

[0184] In the formula, dashed lines represent atomic bonds. R 1 It is a hydrogen atom, or an alkyl or acyl group having 1 to 20 carbon atoms. The aforementioned alkyl or acyl groups may also contain an oxygen atom and / or a nitrogen atom. 1 Y is an n-valent organic group with 1 to 47 carbon atoms. 1 It can be a single bond or a carbonyl group. n is an integer from 1 to 10.

[0185] By having a partial structure represented by the aforementioned general formula (7), W in the aforementioned general formula (1) can impart higher thermal fluidity to the resist underlayer film material of the present invention, thus imparting good flatness.

[0186] In the aforementioned general formula (7), R 1Examples of suitable atoms include hydrogen, methyl, methoxymethyl, 1-ethoxyethyl, 1-(2-ethylhexyloxy)ethyl, 2-tetrahydropiperanyl, allyl, benzyl, propyrynyl, formyl, acetyl, propionyl, butyryl, hexanoyl, eicosyl, acrylyl, methacrylyl, propioloyl, methoxyacetyl, benzoyl, 4-acetamide benzoyl, aminoformyl, N-methylaminoformyl, and N,N-dimethylaminoformyl. Among these, hydrogen, acetyl, and acrylyl are preferred, with hydrogen being the most desirable.

[0187] In the aforementioned general formula (7), Y 1 Y represents a single bond or a carbonyl group. 1 Carbonyl groups are preferred.

[0188] W in the aforementioned general formula (7) 1 It is an n-valent organic group with 1 to 47 carbon atoms. W 1 The organic groups with 1 to 47 carbon atoms may also contain straight-chain, branched, or cyclic saturated or unsaturated hydrocarbon groups, aromatic groups, heteroaromatic groups, ether groups, hydroxyl groups, ester groups, ketone groups, amino groups, halogen groups, thioether groups, carboxyl groups, sulfonyl groups, imide groups, cyano groups, aldehyde groups, imino groups, urea groups, carbamate groups, carbonate groups, nitro groups, and sulfonic acid groups. n is an integer from 1 to 10, and n of 2 to 4 is preferred for balancing good flatness and sufficient thermosetting properties.

[0189] W in the aforementioned general formula (7) 1 The following structures can be listed as ideal examples.

[0190] [Chemistry 21]

[0191]

[0192] [Chemistry 22]

[0193]

[0194] In the formula, the dashed lines represent atomic bonds.

[0195] If it contains such component (A), it will become a resist underlayer film with better film-forming properties and flatness, and it can be manufactured particularly easily.

[0196] By appropriately selecting R according to the required performance and application of the present invention 1 W 1 Y 1 The values ​​of , , and n can be used to adjust properties such as etching resistance, heat resistance, optical constants, polarity, flexibility, and hardening properties.

[0197] [(A) A method for synthesizing compounds or resins whose terminal group structure contains three adjacent hydroxyl groups]

[0198] (A) A compound or resin whose terminal group structure contains three adjacent hydroxyl groups can be obtained, for example, by reacting an epoxy compound containing a portion corresponding to W in the above general formula (1), a compound containing a triple bond containing a portion corresponding to the structure represented by the above general formula (2), and a compound containing a portion having three adjacent hydroxyl groups corresponding to the structure represented by the above general formula (3), but is not limited to this method. For specific examples, please refer to the synthesis examples in the following sections.

[0199] In the photoresist underlayer film material of the present invention, one of the compounds or resins represented by the aforementioned general formula (1) may be used alone, or two or more may be used in combination. It may also be used in the form of a mixture containing the compound or resin represented by general formula (1) and other compounds. When used in the form of a mixture, it is preferable that the compound or resin represented by general formula (1) accounts for 10% or more by mass of all solid components other than the organic solvent in (B) of the photoresist underlayer film material, and more preferably 20% or more by mass. A sufficient blending effect is obtained when the content is 10% or more by mass.

[0200] If the resist underlayer material contains component (A) in such a content, a resist underlayer film with better flatness and film-forming properties can be formed, and it can be manufactured in particular easily.

[0201] In the resist underlayer film material of the present invention, in addition to the compound represented by the aforementioned general formula (1), other substances may also be mixed in. The mixing substance has the effect of, for example, improving the spin-coating film-forming properties and the embedding characteristics on substrates with elevation differences when mixed with the compound represented by the aforementioned general formula (1). The substances that may be mixed in this case are not particularly limited, and known substances may be used; specifically, acrylic resins, styrene resins, phenolic resins, polyether resins, epoxy resins, and compounds containing phenolic hydroxyl groups are preferred. The amount of the mixing substance is preferably 1 to 100 parts by mass relative to 100 parts by mass of the compound or resin represented by the aforementioned general formula (1), and more preferably 2 to 50 parts by mass.

[0202] Furthermore, in the resist lower film material of the present invention, the amount of component (A) can be set to, for example, 3 to 15 by mass.

[0203] [(B) Organic solvents]

[0204] The organic solvent (B) that can be used in the resist lower film material of the present invention is not particularly limited as long as it can dissolve one or more compounds or resins that contain three adjacent hydroxyl groups in part of the terminal group structure of (A). It is preferred that it can dissolve any component, such as the above-mentioned blending substances, and the alkali generating agent (C), surfactant (D), crosslinking agent (E), plasticizer (F), and pigment (G) described later.

[0205] Specifically, the solvents described in paragraphs

[0091] to

[0092] of Japanese Patent Application Publication No. 2007-199653 may be added. More specifically, it is preferable to use propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, 2-heptanone, cyclopentanone, cyclohexanone and γ-butyrolactone, or a mixture containing one or more of them.

[0206] The amount of organic solvent should be adjusted according to the set film thickness of the resist underlayer film, and is usually in the range of 100 to 50,000 parts by mass relative to 100 parts by mass of the compound or resin (component (A)) containing 3 adjacent hydroxyl groups in part of the terminal group structure of the aforementioned (A).

[0207] Furthermore, in the resist lower film material of the present invention, (B) the organic solvent is preferably a mixture of one or more organic solvents with a boiling point less than 180°C and one or more organic solvents with a boiling point of 180°C or higher (hereinafter also referred to as "high boiling point solvents").

[0208] Organic solvents with a boiling point less than 180°C include, specifically, propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, 2-heptanone, cyclopentanone, and cyclohexanone.

[0209] Organic solvents with a boiling point above 180°C are acceptable as long as they can dissolve all components of the lower layer film material of the resist of this invention. There are no special limitations; these solvents can be hydrocarbons, alcohols, ketones, esters, ethers, chlorinated solvents, etc. Specific examples include 1-octanol, 2-ethylhexanol, 1-nonanol, 1-decanol, 1-undecylol, ethylene glycol, 1,2-propanediol, 1,3-butanediol, 2,4-pentanediol, 2-methyl-2,4-pentanediol, 2,5-hexanediol, 2,4-heptanediol, and 2-ethyl-1,3-hexanediol. Alkanediol, diethylene glycol, dipropylene glycol, triethylene glycol, tripropylene glycol, glycerol, n-nonyl acetate, ethylene glycol monohexyl ether, ethylene glycol mono-2-ethylhexyl ether, ethylene glycol monophenyl ether, ethylene glycol monobenzyl ether, diethylene glycol monoethyl ether, diethylene glycol monoisopropyl ether, diethylene glycol mono-n-butyl ether, diethylene glycol monoisobutyl ether, diethylene glycol monohexyl ether, diethylene glycol monophenyl ether, diethylene glycol monobenzyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, diethylene glycol butyl methyl ether, triethylene glycol dimethyl ether, triethylene glycol monomethyl ether, triethylene glycol... Diethylene glycol n-butyl ether, triethylene glycol butyl methyl ether, tetraethylene glycol dimethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol mono-n-propyl ether, dipropylene glycol mono-n-butyl ether, tripropylene glycol dimethyl ether, tripropylene glycol monomethyl ether, tripropylene glycol mono-n-propyl ether, tripropylene glycol mono-n-butyl ether, ethylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate, triacetin, propylene glycol diacetate, dipropylene glycol monoethyl ether... Propyl ether, dipropylene glycol methyl ether acetate, 1,4-butanediol diacetate, 1,3-butanediol diacetate, 1,6-hexanediol diacetate, triethylene glycol diacetate, γ-butyrolactone, methyl benzoate, ethyl benzoate, propyl benzoate, butyl benzoate, dihexyl malonate, diethyl succinate, dipropyl succinate, dibutyl succinate, dihexyl succinate, dimethyl adipate, diethyl adipate, and dibutyl adipate, etc., may be used alone or in combination.

[0210] Organic solvents with a boiling point of 180°C or higher can be appropriately selected from those mentioned above, depending on the temperature at which the resist underlayer film material of the present invention is heat-treated. A boiling point of 180°C to 300°C is preferred for organic solvents with a boiling point of 180°C or higher, and 200°C to 300°C is more ideal. With such a boiling point, there is no risk of excessively rapid evaporation during baking (heat treatment) due to a low boiling point, thus ensuring sufficient thermal fluidity during film formation. It is believed that a resist underlayer film with excellent filling characteristics and / or flatness can be formed. Furthermore, with such a boiling point, there is no risk of residue remaining in the film after baking due to an excessively high boiling point, thus avoiding any adverse effects on film properties such as etching resistance.

[0211] Furthermore, when using organic solvents with a boiling point above 180°C, the doping amount is preferably 1 to 30 parts by mass relative to 100 parts by mass of organic solvents with a boiling point below 180°C. Such a doping amount avoids the risk of insufficient thermal fluidity during baking due to too little doping, or excessive doping resulting in residues in the film and deterioration of film properties such as etching resistance, which is ideal.

[0212] [(C) Alkali-producing agent]

[0213] The resist underlayer material of the present invention, by containing an alkali-generating agent, can form a resist underlayer film with excellent film-forming properties even on a hydrophobic substrate treated with HMDS. To maximize the effect of the alkali-generating agent, it is preferable to avoid the simultaneous presence of an acid-generating agent.

[0214] In this invention, the alkali-generating agent refers to a substance whose chemical structure changes and produces an alkali due to external stimuli such as light and heat; it is also called a "latent alkali" or "alkali precursor." The alkali produced is not only a common alkali such as ammonia or amine, but can also be a chemical species that enhances the ionicity of three adjacent hydroxyl groups in a portion of the terminal group structure of component (A).

[0215] The alkali-generating agent in component (C) is not particularly limited, and a known alkali-generating agent can be used as needed. However, when forming a film using the resist underlayer film material of the present invention, it is assumed that heating is performed, and that during heating, the three adjacent hydroxyl groups in a portion of the terminal group structure of component (A) are ionic and their interaction with the substrate increases, thereby improving film formation. Therefore, it is preferable that the aforementioned alkali-generating agent in (C) is a compound that exhibits alkalinity due to thermal decomposition. The reason is that, by adjusting the amount of component (C) added, the thermal fluidity of the film formed from the resist underlayer film material and its interaction with the substrate can be balanced in such a resist underlayer film material.

[0216] Thus, when an alkali-generating agent that exhibits alkalinity due to thermal decomposition (also known as a thermal alkali-generating agent) is used as component (C), the resulting alkali is a cation that becomes excessive in the system due to the evaporation or decomposition of anions. Examples include triphenylsulfonium cation and tetrabutylammonium cation. Due to this type of alkali, the ionicity (polarity) of the three adjacent hydroxyl groups in part of the terminal group structure of component (A) is increased. Even on substrates treated with hydrophobicity such as HMDS, the interaction with polar groups such as silanol groups on the surface can improve the moisture permeability of the resist underlayer film material to the substrate and suppress film edge retreat (shrinkage). On the other hand, before heating, i.e. before alkali generation, the above-mentioned effects do not occur, thus maintaining the fluidity of the resist underlayer film material itself. In this way, a resist underlayer film with superior film-forming properties can be formed.

[0217] Furthermore, it is preferable that the base-generating agent mentioned above (B) is represented by any of the following general formulas (8), (9) and (10).

[0218] [Chemistry 23]

[0219]

[0220] In the above formula, R 01 ~R 03 Each can independently represent a linear, branched, or cyclic alkyl or alkenyl group with 1 to 10 carbon atoms that can be substituted with or have heteroatom insertions, or an aryl or aralkyl group with 6 to 18 carbon atoms that can be substituted with or have heteroatom insertions. Also, R 01 R 02 and R 03 Any two of them can also bond to each other and form a ring together with the sulfur atom in the formula. X - This refers to anions that are organic or inorganic and can be considered as relative ions. However, X... - Excluding OH - R 04 and R 05 Each aryl group is independently composed of 6 to 20 carbon atoms, and some or all of the hydrogen atoms in this aryl group may be substituted by straight-chain, branched, or cyclic alkyl or alkoxy groups having 1 to 10 carbon atoms. Also, R 04 and R 05 They can also bond with each other and form a ring together with the iodine atom in the formula. R 06 R 07 R 08 and R 09 Each can independently represent a hydrogen atom, or a linear, branched, or cyclic alkyl or alkenyl group with 1 to 20 carbon atoms that may be substituted with heteroatoms or have heteroatom insertions, or an aryl or aralkyl group with 6 to 18 carbon atoms that may be substituted with heteroatoms or have heteroatom insertions. Also, R 06 R 07 R 08 and R 09 Any two or more of them can bond with each other and form a ring together with the nitrogen atom in the formula.

[0221] R in the aforementioned general formula (8) 01 R 02 and R 03Examples, specifically, include alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, tert-butyl, cyclopropyl, cyclopentyl, cyclohexyl, cyclopropylmethyl, 4-methylcyclohexyl, cyclohexylmethyl, norbornel, and adamantyl; alkyl groups such as vinyl, allyl, propenyl, butenyl, hexenyl, and cyclohexenyl; aryl groups such as phenyl, naphthyl, and thiophene; aralkyl groups such as benzyl; and aralkyl groups such as 1-phenylethyl and 2-phenylethyl, with aryl groups being preferred. Furthermore, a portion of the hydrogen atoms in these groups can be replaced with heteroatoms such as oxygen, sulfur, nitrogen, or halogen atoms, or heteroatoms such as oxygen, sulfur, or nitrogen atoms can be inserted. This can result in the formation or insertion of hydroxyl, cyano, carbonyl, ether bonds, ester bonds, sulfonate bonds, carbonate bonds, lactone rings, sulopentalide rings, carboxylic anhydrides, and haloalkyl groups.

[0222] R 01 R 02 and R 03 When any two of the atoms are bonded to each other directly or via an oxygen atom, methylene group, sulfonic acid group, or carbonyl group, in addition to the dibenzothiophene skeleton and the phenoxathiin skeleton, some of the structures shown below can be cited, but are not limited to these. Furthermore, in the following formula, substituents may be present at any position on the aromatic ring.

[0223] [Chemistry 24]

[0224]

[0225] More specifically, examples of sulfonium cations include: triphenylsulfonium, 4-hydroxyphenyl diphenylsulfonium, bis(4-hydroxyphenyl)phenylsulfonium, tri(4-hydroxyphenyl)sulfonium, 4-tert-butoxyphenyl diphenylsulfonium, bis(4-tert-butoxyphenyl)phenylsulfonium, tri(4-tert-butoxyphenyl)sulfonium, 3-tert-butoxyphenyl diphenylsulfonium, bis(3-tert-butoxyphenyl)phenylsulfonium, tri(3-tert-butoxyphenyl)sulfonium, 4-tert-butylphenyl diphenylsulfonium, tri(4-tert-butylphenyl)sulfonium, 3,4-di-tert-butoxyphenyl diphenylsulfonium, bis(3,4-di-tert-butoxyphenyl)sulfonium, and bis(3,4-di-tert-butoxyphenyl)sulfonium. (Butoxyphenyl)phenylsulfonium, tris(3,4-di-tert-butoxyphenyl)sulfonium, diphenyl(4-thiophenoxyphenyl)sulfonium, 10-phenylphenoxathiamonium, S-phenyldibenzothiamonium, 4-tert-butoxycarbonylmethoxyphenyldiphenylsulfonium, tris(4-tert-butoxycarbonylmethoxyphenyl)sulfonium, (4-tert-butoxyphenyl)bis(4-dimethylaminophenyl)sulfonium, tris(4-dimethylaminophenyl)sulfonium, 2-naphthyldiphenylsulfonium, (4-hydroxy-3,5-dimethylphenyl)diphenylsulfonium, and (4-hexyloxy-3,5-dimethylphenyl)diphenylsulfonium, etc. Further examples include 4-methacryloyloxyphenyl diphenylsulfonium, 4-acryloyloxyphenyl diphenylsulfonium, 4-methacryloyloxyphenyl dimethylsulfonium, 4-acryloyloxyphenyl dimethylsulfonium, (4-methacryloyloxy-3,5-dimethylphenyl)diphenylsulfonium, and (4-acryloyloxy-3,5-dimethylphenyl)diphenylsulfonium. More preferably, it includes triphenylsulfonium, 4-tert-butylphenyl diphenylsulfonium, 4-tert-butoxyphenyl diphenylsulfonium, 10-phenylphenoxathiane, and S-phenyldibenzothiaphenonium. Among these, triphenylsulfonium, 4-tert-butylphenyl diphenylsulfonium, or 4-tert-butoxyphenyl diphenylsulfonium are particularly preferred.

[0226] R in the aforementioned general formula (9) 04 and R 05 Examples, specifically, are given for phenyl, naphthyl, and substituents, where the substitution positions are arbitrary. Examples include tolyl, xylyl, trimethylphenyl, ethylphenyl, isopropylphenyl, tert-butylphenyl, 1-adamantylphenyl, triisopropylphenyl, tricyclohexylphenyl, methoxyphenyl, ethoxyphenyl, butoxyphenyl, hydroxyphenyl, dihydroxyphenyl, trimethoxyphenyl, methylthiophenyl, biphenyl, fluorophenyl, difluorophenyl, bromophenyl, iodophenyl, N,N-diphenylaminophenyl, acetoxyphenyl, acetaminophenyl, 2,2,2-trifluoroethoxyphenyl, (2-methoxyethoxy)phenyl, hydroxynaphthyl, dihydroxynaphthyl, 2,2,2-trifluoroethoxynaphthyl, and (2-methoxyethoxy)naphthyl, but are not limited to these.

[0227] Regarding R 04 and R 05For this purpose, unsubstituted phenyl groups or phenyl groups having a substituent selected from halogen atoms, alkyl groups, and alkoxy groups at the para position of the iodine atom are preferred. In particular, phenyl, 4-tert-butylphenyl, or 4-fluorophenyl are preferred.

[0228] R 04 and R 05 When the atoms are bonded directly to each other or separated by oxygen atoms, methylene groups, sulfonic acid groups, or carbonyl groups, some of the structures shown below can be cited, but are not limited to these. Furthermore, in the following formulas, substituents may be present at any position on the aromatic ring.

[0229] [Chemistry 25]

[0230]

[0231] More specifically, examples of monazine cations include, but are not limited to, those shown below. Also, in the following formula, tBu is tert-butyl and Ph is phenyl.

[0232] [Chemistry 26]

[0233]

[0234] Ammonium cations represented by the aforementioned general formula (10) include, for example, ammonia, aliphatic amines of grade I, II and III, mixed amines, aromatic amines, heterocyclic amines, nitrogen-containing compounds with carboxyl groups, nitrogen-containing compounds with sulfonyl groups, nitrogen-containing compounds with hydroxyl groups, nitrogen-containing compounds with hydroxyphenyl groups, nitrogen-containing compounds with alcoholic nitrogen-containing compounds, etc., in which a proton is added to the nitrogen atom, and quaternary ammonium cations.

[0235] Specifically, examples of Class I aliphatic ammonium compounds include methylammonium, ethylammonium, n-propylammonium, isopropylammonium, n-butylammonium, isobutylammonium, sec-butylammonium, tert-butylammonium, pentylammonium, tert-pentylammonium, cyclopentylammonium, hexylammonium, cyclohexylammonium, heptylammonium, octylammonium, nonylammonium, decylammonium, dodecylammonium, hexadecylammonium, aminomethylammonium, and 2-aminoethylammonium, etc. Examples of Class II aliphatic ammonium compounds include dimethylammonium, diethylammonium, di-n-propylammonium, diisopropylammonium, di-n-butylammonium, diisobutylammonium, disec-butylammonium, dipentylammonium, dicyclopentylammonium, dihexylammonium, dicyclohexylammonium, and diheptylammonium. Dioctylammonium, dinonylammonium, didecylammonium, di(dodecyl)ammonium, di(hexadecyl)ammonium, methyl(methylamino)methylammonium, and methyl-2-(methylamino)ethylammonium, etc., and third-order aliphatic ammoniums include trimethylammonium, triethylammonium, tri-n-propylammonium, triisopropylammonium, tri-n-butylammonium, triisobutylammonium, trisec-butylammonium, tripentylammonium, tricyclopentylammonium, trihexylammonium, tricyclohexylammonium, triheptylammonium, trioctylammonium, trinonylammonium, tridecaylammonium, tri(dodecyl)ammonium, tri(hexadecyl)ammonium, dimethyl(dimethylamino)methylammonium, and dimethyl(2-dimethylaminoethyl)ammonium, etc.

[0236] Furthermore, examples of mixed ammonium compounds include dimethyl ethyl ammonium, methyl propyl ammonium, benzyl ammonium, phenethyl ammonium, and benzyl dimethyl ammonium. Specific examples of aromatic ammonium and heterocyclic ammonium derivatives include anilinetonium derivatives (e.g., anilinetonium, N-methylanilinetonium, N-ethylanilinetonium, n-propylanilinetonium, N,N-dimethylanilinetonium, 2-methylanilinetonium, 3-methylanilinetonium, 4-methylanilinetonium, ethylanilinetonium with any substitution position, propylanilinetonium with any substitution position, trimethylanilinetonium with any substitution position, 2-nitroanilinetonium, 3-nitroanilinetonium, 4-nitroanilinetonium, 2,4-dinitroanilinetonium, 2,6-dinitroanilinetonium, 3,5-dinitroanilinetonium, and N,N-dimethyltoluidinetonium with any substitution position), diphenyl(p-tolyl)ammonium, and methyldiphenyl Ammonium, triphenylammonium, aminophenylammonium with arbitrary substitution, naphthylammonium, aminonaphthylammonium with arbitrary substitution, pyrrolinium derivatives (e.g., pyrrolinium, 2H-pyrrolinium, 1-methylpyrrolinium, 2,4-dimethylpyrrolinium, 2,5-dimethylpyrrolinium, and N-methylpyrrolinium, etc.), oxazolium derivatives (e.g., oxazolium, and isoxazolium, etc.), thiazolylium derivatives (e.g., thiazolylium, and isothiazolium, etc.), imidazolylium derivatives (e.g., imidazolylium, 4-methylimidazolylium, and 4-methyl-2-phenylimidazolylium, etc.), pyrrolinium derivatives, furazonium derivatives, pyrrolinium derivatives (e.g., pyrrolinium, and 2-methyl-1-... Pyrrolidineonium, etc.), pyrrolidineonium derivatives (e.g., pyrrolidineonium, N-methylpyrrolidineonium, pyrrolidoneonium, and N-methylpyrrolidoneonium), imidazolineonium derivatives, imidazolineonium derivatives, pyridinium derivatives (e.g., pyridinium, methylpyridinium, ethylpyridinium, propylpyridinium, butylpyridinium, 4-(1-butylpentane) 4-(1-ethylpropyl)pyridinium, dimethylpyridinium, trimethylpyridinium, triethylpyridinium, phenylpyridinium, 3-methyl-2-phenylpyridinium, 4-tert-butylpyridinium, diphenylpyridinium, benzylpyridinium, methoxypyridinium, butoxypyridinium, dimethoxypyridinium, 4-pyrrolidinylpyridinium, 2-(1-ethylpropyl)pyridinium (Pinidine, aminopyridinium, and dimethylaminopyridinium, etc.), pyridazinium derivatives, pyrimidine derivatives, pyrazinium derivatives, pyrazolinium derivatives, pyrazolidine derivatives, piperidinium derivatives, piperazine derivatives, morpholinium derivatives, indolineium derivatives, isoindolineium derivatives, 1H-indolineium derivatives, indolineium derivatives, quinolinium derivatives (e.g., quinolinium), isoquinolinium derivatives, cyclophosphine derivatives, quinazolinium derivatives, quinoxaline derivatives, phthalazinium derivatives, purineium derivatives, pteridineium derivatives, carbazoleium derivatives, phenanthridineium derivatives, acridineium derivatives, phenazinium derivatives, and 1,10-phenanthrolineium derivatives, etc.

[0237] Furthermore, nitrogen-containing compounds with carboxyl groups include carboxyphenylammonium, carboxyindolinetonium, and amino acid derivatives (such as nicotinic acid, alanine, arginine, aspartic acid, glutamic acid, glycine, histidine, isoleucine, glycylleucine, leucine, methionine, phenylalanine, threonine, lysine, 3-aminopyrazine-2-carboxylic acid, and methoxyalanine, etc., proton addition products). Nitrogen-containing compounds with sulfonyl groups include 3-pyridinium sulfonic acid. Nitrogen-containing compounds with hydroxyl groups, nitrogen-containing compounds with hydroxyphenyl groups, and alcoholic nitrogen-containing compounds include 2-hydroxypyridinium, hydroxyanilinetonium with arbitrary substitution positions, hydroxy-methyl-anilinetonium with arbitrary substitution positions, hydroxyquinolinetonium, and dihydroxyquinolinetonium. Linonium, 2-hydroxyethylammonium, bis(2-hydroxyethyl)ammonium, tri(2-hydroxyethyl)ammonium, ethylbis(2-hydroxyethyl)ammonium, diethyl(2-hydroxyethyl)ammonium, hydroxypropylammonium, bis(hydroxypropyl)ammonium, tri(hydroxypropyl)ammonium, 4-(2-hydroxyethyl)morpholinium, 2-(2-hydroxyethyl)pyridinium, 1-(2-hydroxyethyl)piperazineium, 1-[2-(2-hydroxyethoxy)ethyl]piperazineium, (2-hydroxyethyl)piperazineium, 1-(2-hydroxyethyl)pyrrolidineium, 1-(2-hydroxyethyl)-2-pyrrolidoneium, 2,3-dihydroxypropylpiperidineium, 2,3-dihydroxypropylpyrrolidineium, 8-hydroxyjulonidinium, and 3-hydroxyquinine cycloonium, etc.

[0238] Specific examples of quaternary ammonium salts include tetramethylammonium, triethylmethylammonium, tetraethylammonium, tetrabutylammonium, tetraoctylammonium, didecyldimethylammonium, tridecylmethylammonium, hexadecyltrimethylammonium, stearyltrimethylammonium, benzyltrimethylammonium, benzyltriethylammonium, benzyltributylammonium, and 2-hydroxyethyltrimethylammonium.

[0239] Quaternary ammonium cations are preferred, especially tetramethylammonium cations, tetraethylammonium cations, or tetrabutylammonium cations.

[0240] At this point, the aforementioned anion X in the general formulas (8), (9) and (10) - It is preferable to select any anion from the group consisting of chloride ions, bromide ions, iodide ions, fluoride ions, cyanide ions, nitrate ions, and nitrite ions, which have structures represented by any of the following general formulas (11), (12) and (13).

[0241] [Chemistry 27]

[0242]

[0243] In the above formula, R 10This indicates a linear, branched, or cyclic alkyl, alkenyl, aralkyl, or aryl group with 1 to 20 carbon atoms, which may also contain an ether group, ester group, or carbonyl group. One or more hydrogen atoms in these groups may also be substituted with halogen atoms, hydroxyl groups, carboxyl groups, amino groups, and / or cyano groups. R 11 This indicates an aryl group with 6 to 20 carbon atoms. One or more hydrogen atoms in this aryl group may also be substituted with halogen atoms, hydroxyl groups, carboxyl groups, amino groups, and / or cyano groups. R 12 R 13 and R 14 Each group independently represents a hydrogen atom, or a halogen atom other than fluorine, or may contain an ether group, ester group, or carbonyl group, and is a straight-chain, branched, or cyclic alkyl, alkenyl, aralkyl, or aryl group with 1 to 20 carbon atoms. One or more hydrogen atoms in these groups may also be substituted with a halogen atom, hydroxyl group, carboxyl group, amino group, and / or cyano group. Also, R 12 R 13 and R 14 Two or more of them can also bond together to form a ring.

[0244] Specific examples of carboxylate anions represented by the aforementioned general formula (11) include formate anion, acetate anion, propionate anion, butyrate anion, isobutyrate anion, valerate anion, isovalerate anion, pterovalerate anion, hexanoate anion, caprylate anion, cyclohexanecarboxylate anion, cyclohexylacetate anion, laurate anion, myristate anion, palmitate anion, stearate anion, phenylacetate anion, diphenylacetate anion, phenoxyacetate anion, and mandelic acid anion. (acid) anion, benzoylcarboxylate anion, cinnamate anion, dihydrocinnamate anion, benzoate anion, methylbenzoate anion, salicylate anion, naphtholic acid anion, anthraquinone carboxylate anion, anthraquinone carboxylate anion, glycolate anion, trimethylacetate anion, lactate anion, methoxyacetate anion, 2-(2-methoxyethoxy)acetate anion, 2-(2-(2-methoxyethoxy)ethoxy) Acetate anions, bisphenol acid anions, monochloroacetic acid anions, dichloroacetic acid anions, trichloroacetic acid anions, trifluoroacetic acid anions, pentafluoropropionic acid anions, heptafluorobutyrate anions, and 2-hydroxy-2,2-bis(trifluoromethyl)acetic acid anions, etc., and monoanions of dicarboxylic acids such as succinic acid, tartaric acid, glutaric acid, pimelic acid, sebacic acid, phthalic acid, isophthalic acid, terephthalic acid, naphthalene dicarboxylic acid, cyclohexane dicarboxylic acid, and cyclohexene dicarboxylic acid can also be listed.

[0245] Specific examples of the arene sulfonate anion represented by the aforementioned general formula (12) include benzenesulfonate, 4-toluenesulfonate, 2-toluenesulfonate, xylenesulfonate with any substitution position, trimethylbenzenesulfonate, mesitylenesulfonate, 4-methoxybenzenesulfonate, 4-ethylbenzenesulfonate, 2,4,6-triisopropylbenzenesulfonate, 1-naphthalenesulfonate, 2-naphthalenesulfonate, anthraquinone-1-sulfonate, anthraquinone-2-sulfonate, 4-(4-methylbenzenesulfonyloxy)benzenesulfonate, 3,4-bis(4-methylbenzenesulfonyloxy)benzenesulfonate, 6-(4-methylbenzenesulfonyloxy)naphthalene-2-sulfonate, 4-phenoxybenzenesulfonate, 4-diphenylmethylbenzenesulfonate, 2,4-dinitrobenzenesulfonate, and dodecylbenzenesulfonate, etc.

[0246] Specific examples of alkyl sulfonate anions represented by the aforementioned general formula (13) include methane sulfonate, ethane sulfonate, propane sulfonate, butane sulfonate, pentane sulfonate, hexane sulfonate, cyclohexane sulfonate, octane sulfonate, and 10-camphor sulfonate.

[0247] Furthermore, X in the aforementioned general formulas (8), (9) and (10) - It is preferable for the conjugate acid XH to have a boiling point below 200℃.

[0248] By appropriately selecting an alkali-generating agent that exhibits alkalinity due to thermal decomposition (thermal alkali-generating agent), the alkalinity can be adjusted according to the firing temperature of the underlying film material of the photoresist, thus achieving a balance between film formation and flatness. Furthermore, since it decomposes or evaporates completely during firing and leaves no residue in the film after firing, it will not adversely affect properties other than film formation.

[0249] X in the aforementioned general formulas (8), (9) and (10) - It is preferred to use trifluoroacetate anion, pentafluoropropionate anion, 2-hydroxy-2,2-bis(trifluoromethyl)acetate anion, chloride ion, or nitrate ion.

[0250] The examples of the base-generating agents described in (C) above can be any combination of the specific examples of the aforementioned cations and anions, but are not limited to these. Furthermore, an ideal structure can be shown below. Also, in the following formula, tBu is tert-butyl.

[0251] [Chemistry 28]

[0252]

[0253] Regarding the aforementioned alkali-generating agent (C), by using one compound alone or in combination of two or more compounds, alkalinity can be exhibited depending on the firing temperature of the resist underlayer film material, thus appropriately adjusting the balance between film formation and flatness on hydrophobic substrates. The amount of alkali-generating agent (C) added is preferably 0.1 to 10 parts by weight, more preferably 0.3 to 3 parts by weight, relative to 100 parts by weight of the aforementioned compound or resin (component (A)). If the amount of alkali-generating agent (C) added is within the aforementioned range, sufficient improvement in film formation can be obtained without the risk of deterioration of film surface uniformity due to decomposition and sublimation, or a decrease in the curing properties of the compound or resin due to alkalinity.

[0254] [(D) Surfactant]

[0255] In the resist lower film material of the present invention, a surfactant (D) may be added to improve the coatability during spin coating. The surfactant (D) may be, for example, those described in

[0142] to

[0147] of Japanese Patent Application Publication No. 2009-269953. The amount of surfactant (D) added is preferably 0.001 to 20 parts by weight, more preferably 0.01 to 10 parts by weight, relative to 100 parts by weight of the aforementioned component (A).

[0256] [(E) Crosslinking agent]

[0257] Furthermore, in the lower layer film material of the resist of the present invention, a crosslinking agent (E) may be added to improve hardening properties and further suppress cross-mixing with the upper layer film. There are no particular limitations on the crosslinking agent (E), and various known crosslinking agents can be widely used. Examples include melamine-based crosslinking agents, glycourea-based crosslinking agents, benzoguanamine-based crosslinking agents, urea-based crosslinking agents, β-hydroxyalkylamide-based crosslinking agents, isocyanurate-based crosslinking agents, aziridine-based crosslinking agents, oxazoline-based crosslinking agents, epoxy-based crosslinking agents, and phenol-based crosslinking agents (e.g., hydroxymethyl or alkoxymethyl type crosslinking agents of polynuclear phenols). The amount of crosslinking agent added is preferably 1 to 60 parts by weight, and more preferably 10 to 50 parts by weight, relative to 100 parts by weight of component (A) mentioned above.

[0258] Melamine-based crosslinking agents, specifically, include hexamethoxymethylmelamine, hexabutoxymethylmelamine, their alkoxy and / or hydroxyl-substituted derivatives, and their partial self-condensing derivatives. Glycourea-based crosslinking agents, specifically, include tetramethoxymethylglycourea, tetrabutoxymethylglycourea, their alkoxy and / or hydroxyl-substituted derivatives, and their partial self-condensing derivatives. Benzylguanidine-based crosslinking agents, specifically, include tetramethoxymethylbenzylguanidine, tetrabutoxymethylbenzylguanidine, their alkoxy and / or hydroxyl-substituted derivatives, and their partial self-condensing derivatives. Urea-based crosslinking agents, specifically, include dimethoxymethyldimethoxyethylurea, its alkoxy and / or hydroxyl-substituted derivatives, and their partial self-condensing derivatives. β-Hydroxyalkylamide-based crosslinking agents, specifically, include N,N,N',N'-tetra(2-hydroxyethyl)hexamethylenediamide. Isocyanurate crosslinking agents include, specifically, triglycidyl isocyanurate and triallyl isocyanurate. Aziridine crosslinking agents include, specifically, 4,4'-bis(ethyleneiminocarbonylamino)diphenylmethane and 2,2-dihydroxymethylbutanol-tris[3-(1-aziridine)propionate]. Oxazoline crosslinking agents include, specifically, 2,2'-isopropylidene bis(4-benzyl-2-oxazoline), 2,2'-isopropylidene bis(4-phenyl-2-oxazoline), 2,2'-isopropylidene bis(4-phenyl-2-oxazoline), 2,2'-methylene bis-4,5-diphenyl-2-oxazoline, 2,2'-methylene bis-4-phenyl-2-oxazoline, 2,2'-methylene bis-4-tert-butyl-2-oxazoline, 2,2'-bis(2-oxazoline), 1,3-phenylene bis(2-oxazoline), 1,4-phenylene bis(2-oxazoline), and 2-isopropylidene oxazoline copolymers. Epoxy crosslinking agents, specifically, include diglycidyl ether, ethylene glycol diglycidyl ether, 1,4-butanediol diglycidyl ether, 1,4-cyclohexanediethanol diglycidyl ether, poly(glycidyl methacrylate), trimethylolethane triglycidyl ether, trimethylolpropane triglycidyl ether, and neopentyl tetroxide tetraglycidyl ether.

[0259] To maximize the effect of the alkali-generating agent, a polynuclear phenolic crosslinking agent that will undergo crosslinking even without an acid-generating agent is more ideal. Furthermore, polynuclear phenolic crosslinking agents themselves contain phenolic hydroxyl groups, so it is expected that a higher degree of improvement in film-forming properties can be obtained through the action of the alkali-generating agent. Specifically, polynuclear phenolic crosslinking agents can be exemplified by compounds represented by the following general formula (14).

[0260] [Chemistry 29]

[0261]

[0262] In the formula, Q is a single bond or a q-valent hydrocarbon group with 1 to 20 carbon atoms. R 16It is hydrogen or an alkyl group having 1 to 20 carbon atoms. q is an integer from 1 to 5.

[0263] Q is a single bond or a q-valent hydrocarbon group with 1 to 20 carbon atoms. q is an integer from 1 to 5, preferably 2 or 3. Specifically, Q can be a group that has removed q hydrogen atoms from methane, ethane, propane, butane, isobutane, pentane, cyclopentane, hexane, cyclohexane, methylpentane, methylcyclohexane, dimethylcyclohexane, trimethylcyclohexane, benzene, toluene, xylene, ethylbenzene, ethylisopropylbenzene, diisopropylbenzene, methylnaphthalene, ethylnaphthalene, and eicosane. R 16 It is a hydrogen atom or an alkyl group having 1 to 20 carbon atoms. Specifically, examples of alkyl groups having 1 to 20 carbon atoms include methyl, ethyl, propyl, isopropyl, butyl, isobutyl, pentyl, isopentyl, hexyl, octyl, ethylhexyl, decyl, and eicosyl, with hydrogen atoms or methyl being preferred.

[0264] Examples of compounds represented by the above general formula (14) are specifically listed below. Among them, considering the improvement of the hardening properties and film thickness uniformity of the resist underlayer film, triphenolmethane, triphenol ethane, 1,1,1-tris(4-hydroxyphenyl)ethane, or the hexamethoxymethylated form of tris(4-hydroxyphenyl)-1-ethyl-4-isopropylbenzene are preferred.

[0265] [Chemistry 30]

[0266]

[0267] [Chemistry 31]

[0268]

[0269] In the formula, R 16 As stated above.

[0270] [(F) Plasticizer]

[0271] Furthermore, in the resist underlayer film material of the present invention, a plasticizer (F) may be added to further improve flatness and / or landfill characteristics. There are no particular limitations on the plasticizer (F), and a wide range of known plasticizer systems can be used. Examples include low molecular weight compounds such as phthalates, adipates, phosphates, trimellitic esters, and citrates, as well as polyether-based, polyester-based, and polyacetal-based polymers as described in Japanese Patent Application Laid-Open No. 2013-253227. The amount of plasticizer (F) added is preferably 5 to 500 parts by weight, and more preferably 10 to 200 parts by weight, relative to 100 parts by weight of component (A) mentioned above.

[0272] [(G) pigment]

[0273] Furthermore, in the resist lower film material of the present invention, a (G) pigment can be added to improve the resolution during patterning of multilayer photolithography. There are no particular limitations on the (G) pigment, as long as it is a compound with appropriate absorption at the exposure wavelength; a wide range of known compounds can be used. Examples include benzene compounds, naphthalene compounds, anthracene compounds, phenanthrene compounds, pyrene compounds, isocyanate compounds, and triazine compounds. The amount of (G) pigment added is preferably 0.01 to 10 parts by weight, and more preferably 0.1 to 5 parts by weight, relative to 100 parts by weight of the aforementioned component (A).

[0274] As explained above, the resist underlayer material of the present invention, in the micro-patterning process using the multilayer resist method, can still form a resist underlayer film with excellent planarity and film-forming properties even on the substrate being processed, where planarization is particularly difficult, such as in areas with wide trench structures. This underlayer film can exhibit more suitable etching characteristics. Therefore, the resist underlayer material, patterning method, and resist underlayer film formation method of the present invention are particularly suitable for use in multilayer resist processing for planarization of substrates including uneven surfaces and irregularities, and are extremely useful in micro-patterning for semiconductor device manufacturing. Especially in the micro-patterning process using multilayer resist in semiconductor device manufacturing, even without the presence of acid-generating agents, excellent planarity is still achieved on the substrate being processed, even in areas where planarization is particularly difficult, such as wide trench structures. A substrate-independent resist film can be formed, thereby providing resist film materials with appropriate etching / optical properties, patterning methods using the aforementioned materials, and resist film formation methods. In particular, due to the strong interaction between the three adjacent hydroxyl groups of the terminal structure represented by general formula (3) in compound (A) or resin and the substrate surface, pinholes and edge shrinkage (receding) can still be suppressed even when forming a resist film on a wafer that has undergone hydrophobic treatment such as HMDS treatment.

[0275] <Pattern Formation Methods>

[0276] Furthermore, the present invention provides a pattern forming method (2-layer resist treatment), which is a method for forming a pattern on a substrate being processed, characterized by the following steps:

[0277] (I-1) A coating film is obtained by coating the resist underlayer film material of the present invention onto a substrate to be processed, and the coating film is heat-treated to form a resist underlayer film.

[0278] (I-2) On the aforementioned lower resist film, an upper resist film is formed using a photoresist material.

[0279] (I-3) The aforementioned upper layer of the photoresist is exposed to a pattern, and then developed with a developer to form a pattern on the aforementioned upper layer of the photoresist.

[0280] (I-4) Using the upper resist film with the aforementioned pattern as a mask, dry etch the lower resist film to transfer the pattern onto the lower resist film.

[0281] (I-5) Using the patterned resist lower layer film as a mask, the substrate to be processed is processed to form a pattern on the substrate to be processed.

[0282] Furthermore, the present invention provides a pattern forming method (3-layer resist treatment), which is a method for forming a pattern on a substrate being processed, characterized by the following steps:

[0283] (II-1) A coating film is obtained by coating the resist underlayer film material of the present invention onto a substrate to be processed, and the coating film is heat-treated to form a resist underlayer film.

[0284] (II-2) An intermediate resist film is formed on the aforementioned lower resist film.

[0285] (II-3) On the aforementioned intermediate resist film, a photoresist material is used to form an upper resist film.

[0286] (II-4) The aforementioned photoresist upper film is exposed to a pattern, and then developed with a developer to form a pattern on the aforementioned photoresist upper film.

[0287] (II-5) Using the upper resist film with the aforementioned pattern as a mask, dry etch the aforementioned intermediate resist film to transfer the pattern onto the intermediate resist film.

[0288] (II-6) Using the resist intermediate film on which the aforementioned pattern has been transferred as a mask, dry etch the aforementioned resist lower layer film to transfer the pattern onto the aforementioned resist lower layer film, and,

[0289] (II-7) Using the patterned resist lower layer film as a mask, the above-mentioned substrate is processed to form a pattern on the substrate.

[0290] Furthermore, the present invention provides a pattern forming method (4-layer resist treatment), which is a method for forming a pattern on a substrate being processed, characterized by the following steps:

[0291] (III-1) A coating film is obtained by coating the resist underlayer film material of the present invention onto the substrate to be processed, and the coating film is heat-treated to form a resist underlayer film.

[0292] (III-2) An inorganic hard mask intermediate film, selected from the group consisting of silicon oxide film, silicon nitride film, and silicon oxide nitride film, is formed on the aforementioned photoresist lower layer film.

[0293] (III-3) An organic thin film is formed on the aforementioned inorganic hard mask intermediate film.

[0294] (III-4) A photoresist top layer film is formed on the aforementioned organic thin film using a photoresist material.

[0295] (III-5) The aforementioned upper layer of the photoresist is exposed to a pattern, and then developed with a developer to form a pattern on the aforementioned upper layer of the photoresist.

[0296] (III-6) Using the resist film with the aforementioned pattern as a mask, dry etch the aforementioned organic thin film and the aforementioned inorganic hard mask intermediate film to transfer the pattern onto the aforementioned organic thin film and the aforementioned inorganic hard mask intermediate film.

[0297] (III-7) Using the aforementioned inorganic hard mask intermediate film with the transferred pattern as a mask, dry etch the aforementioned photoresist underlayer film to transfer the pattern onto the aforementioned photoresist underlayer film, and

[0298] (III-8) Using the patterned resist lower layer film as a mask, the above-mentioned substrate is processed to form a pattern on the substrate.

[0299] The thickness of the resist lower layer film formed using the patterning method of the present invention can be appropriately selected, for example, 2 to 20,000 nm, especially 50 to 15,000 nm. In the case of a resist lower layer film for a 3-layer process, a silicon-containing resist intermediate film (intermediate layer film) and a silicon-free resist upper layer film can be formed on it. In the case of a resist lower layer film for a 2-layer process, a silicon-containing resist upper layer film or a silicon-free resist upper layer film can be formed on it.

[0300] The pattern forming method of the present invention is applicable to various types of multilayer resist processing, such as silicon-containing two-layer resist processing, silicon-containing three-layer resist processing, silicon-containing intermediate film-containing four-layer resist processing, silicon-containing intermediate film-containing organic thin film-containing four-layer resist processing, and silicon-free two-layer resist processing.

[0301] As described above, with the resist underlayer material of the present invention, even on a substrate with areas particularly difficult to planarize, such as wide trench structures, a resist underlayer film with excellent planarity and film-forming properties can still be formed, and this underlayer film can exhibit more suitable etching characteristics. Furthermore, the resist underlayer film formed from the resist underlayer material of the present invention can exhibit high adhesion to the substrate being processed. Therefore, with the pattern forming method of the present invention, even on a substrate with areas where planarization is difficult due to height differences, fine patterns can still be formed on the substrate with high precision.

[0302] [3-layer corrosion resist treatment]

[0303] The pattern forming method of the present invention will be described below using a three-layer resist treatment as an example, but the pattern forming method of the present invention is not limited to this treatment. In this case, a lower resist film can be formed on the substrate being processed using the lower resist film material of the present invention. An intermediate resist film can be formed on the lower resist film using, for example, a resist film material containing silicon atoms. An upper resist film can be formed on top of the intermediate resist film using a resist film material (photoresist material) containing a photoresist composition, thus forming a multilayer resist film. After exposing the patterned circuit area of ​​the upper resist film, it is developed with a developer to form a resist pattern on the upper resist film. Using the upper resist film with the formed pattern as a mask, the intermediate resist film is dry-etched to transfer the pattern onto the intermediate resist film. Using the intermediate resist film with the formed pattern as a mask, the lower resist film is etched to transfer the pattern onto the lower resist film. Furthermore, using the lower resist film with the formed pattern as a mask, the substrate is processed to form the pattern on the substrate.

[0304] The resist interlayer containing silicon atoms exhibits resistance to etching by oxygen or hydrogen. Therefore, as mentioned above, it is preferable to use an etching gas mainly composed of oxygen or hydrogen for etching the resist underlayer when the resist interlayer is used as a mask.

[0305] Furthermore, in the pattern forming method of the present invention, a lower resist film can be formed on at least the substrate to be processed using the lower resist film material of the present invention. An inorganic hard mask intermediate film selected from the group consisting of silicon oxide film, silicon nitride film, and silicon oxide nitride film is formed on the lower resist film as a resist intermediate film. An upper resist film is formed on the inorganic hard mask intermediate film using a resist film material composed of photoresist composition. After exposing the pattern circuit area of ​​the upper resist film, it is developed with a developer to form a resist pattern on the upper resist film. The obtained resist pattern is used as an etching mask to dry etch the inorganic hard mask intermediate film, thereby transferring the pattern onto the inorganic hard mask intermediate film. The obtained inorganic hard mask intermediate film pattern is used as an etching mask to dry etch the lower resist film, thereby transferring the pattern onto the lower resist film. The obtained lower resist film pattern is used as a mask to process the substrate, thereby forming a pattern on the substrate.

[0306] As mentioned above, when forming an inorganic hard mask intermediate film on top of the resist layer, silicon oxide, silicon nitride, or silicon oxide nitride (SiON) films can be formed using methods such as CVD and ALD. Methods for forming nitride films are described in Japanese Patent Application Publication No. 2002-334869 or WO2004 / 066377. The thickness of the inorganic hard mask is, for example, 5~200 nm, preferably 10~100 nm. Among these, SiON films, which offer high performance in terms of anti-reflection coatings, are most ideal for ArF exposure applications.

[0307] A three-layer photoresist interlayer with a silicon-containing resist is suitable, particularly for polysilsesquioxane-based interlayers. Polysilsesquioxane-based interlayers readily exhibit anti-reflective properties during excimer laser exposure, thereby suppressing reflected light during exposure of the pattern on the upper resist layer, resulting in excellent resolution. Especially in 193nm exposure applications, if a material containing a large amount of aromatic groups is used as the lower resist layer, the k-value increases, leading to increased substrate reflectance. However, the reflection can be suppressed by the resist interlayer, reducing substrate reflectance to below 0.5%. For resist interlayers with anti-reflective properties, anthracene is suitable for 248nm and 157nm exposures, while for 193nm exposures, suspended phenyl groups or light-absorbing groups with silicon-silicon bonds, cross-linked with acid or heat, are ideal.

[0308] In this situation, compared to CVD, spin coating is a simpler and more cost-effective method for forming silicon-containing photoresist intermediate films.

[0309] The method for forming a photoresist underlayer film using the photoresist underlayer film material of the present invention includes, for example, the photoresist underlayer film formation method of the present invention as described in detail below, but is not limited thereto.

[0310] The top resist layer in a three-layer photoresist film can be either positive or negative, and can use the same photoresist composition as commonly used. When forming the top resist layer using the aforementioned photoresist composition, spin coating is preferred, similar to the method used when forming the bottom resist layer. After spin coating, the photoresist composition is pre-baked, preferably at 60–180°C for 10–300 seconds. Then, exposure is performed as usual, followed by post-exposure baking (PEB) and development to obtain the resist pattern. Furthermore, the thickness of the top resist layer is not particularly limited, but 30–500 nm, especially 50–400 nm, is preferred.

[0311] Furthermore, exposure light can include high-energy rays with wavelengths below 300nm, specifically excimer lasers of 248nm, 193nm, and 157nm, soft X-rays of 3~20nm, electron beams, and X-rays with wavelengths less than 3nm.

[0312] Then, the obtained resist pattern is used as a mask for etching. In the three-layer process, the etching of the intermediate resist film is performed using a chlorofluorocarbon-based gas with the resist pattern as a mask. Next, using the intermediate resist film pattern as a mask, the lower resist film is etched using oxygen or hydrogen.

[0313] The etching of the substrate can also be performed using conventional methods. For example, if the substrate is a low-dielectric-constant insulating film based on SiO2, SiN, or silicon dioxide, etching with chlorofluorocarbon (CFC) gases as the primary method is performed. If it is p-Si, Al, or W, etching with chlorine or bromine gases as the primary method is performed. When etching the substrate with CFC gases, the silicon-containing interlayer film in the three-layer process is peeled off simultaneously with the substrate processing. When etching the substrate with chlorine or bromine gases, the peeling off of the silicon-containing interlayer film requires a separate dry etching and peeling process with CFC gases after the substrate processing.

[0314] Furthermore, the substrate to be processed can be, for example, a substrate on which the layer to be processed has been formed. There are no special limitations on the substrate; materials different from the layer to be processed, such as Si, α-Si, p-Si, SiO2, SiN, SiON, W, TiN, and Al, can be used. The layer to be processed can be various Low-k films and barrier films, such as Si, SiO2, SiON, SiN, p-Si, α-Si, W, TiN, W-Si, Al, Cu, and Al-Si, typically forming thicknesses of 50–10,000 nm, especially 100–5,000 nm. Moreover, the substrate to be processed can be a substrate with a static contact angle to water of 50° or more.

[0315] The pattern formation method of the present invention is also suitable for processing structures with a height of 30 nm or more, or substrates with varying heights. By forming and planarizing the lower resist film of the present invention on a substrate with varying heights, the thickness of the subsequently formed intermediate and upper resist films can be made uniform, thus making it easier to ensure the depth of field (DOF) during optical lithography, which is ideal. Furthermore, it is also useful when using a substrate with a static contact angle of 50° or more with water as the substrate to be processed.

[0316] In one example of a three-layer resist treatment, using Figure 1 The details are as follows.

[0317] When treating with three layers of resist, first as follows Figure 1 As shown in (A), a photoresist lower layer film 3 is formed on the processed layer 2 stacked on the substrate 1 using the photoresist lower layer film material of the present invention. Then, a photoresist intermediate film 4 is formed on the photoresist lower layer film 3, and a photoresist upper layer film 5 is formed thereon.

[0318] Secondly, such as Figure 1As shown in (B), the important portion 6 of the upper resist film is exposed, subjected to PEB (exposure and baking) and development, to form the upper resist film pattern 5a. Figure 1 (C)). Using the obtained upper resist film pattern 5a as a mask, the intermediate resist film 4 is etched using CF-based gas to form the intermediate resist film pattern 4a. Figure 1 (D)). After removing the upper resist film pattern 5a, the obtained intermediate resist film pattern 4a is used as a mask to perform oxygen-based or hydrogen-based plasma etching on the lower resist film 3 to form the lower resist film pattern 3a. Figure 1 (E)). After further removing the intermediate resist film pattern 4a, the lower resist film pattern 3a is used as a mask to etch the layer 2 to form pattern 2a on the layer 2. Figure 1 (F)).

[0319] When using an inorganic hard mask interlayer, the resist interlayer 4 is an inorganic hard mask interlayer. When an organic thin film is coated, an organic thin film layer is placed between the resist interlayer 4 and the upper resist film 5. The etching of the organic thin film is sometimes performed continuously before the etching of the resist interlayer 4, and sometimes only the organic thin film is etched first, and then the etching apparatus is changed before etching the resist interlayer 4.

[0320] [4-layer corrosion resist treatment]

[0321] Furthermore, the present invention can also be ideally used in four-layer resist processing using organic thin films. In this case, at least on the substrate being processed, a lower resist film is formed using the lower resist film material of the present invention. An inorganic hard mask intermediate film selected from the group consisting of silicon oxide films, silicon nitride films, and silicon oxide nitride films is formed on the lower resist film. An organic thin film is formed on the inorganic hard mask intermediate film. An upper resist film is formed on the organic thin film using an upper resist film material composed of a photoresist composition. The upper resist film is then... The patterned circuit area is exposed and then developed with a developer to form a resist pattern on the upper resist film. The obtained resist pattern is used as an etching mask, and the organic thin film and the aforementioned inorganic hard mask intermediate film are dry-etched to transfer the pattern onto the organic thin film and the inorganic hard mask intermediate film. The obtained inorganic hard mask intermediate film pattern is used as an etching mask, and the above-mentioned resist lower film is dry-etched to transfer the pattern onto the resist lower film. The obtained resist lower film pattern is used as a mask to process the substrate and form the pattern on the substrate.

[0322] A photoresist film can also be formed on top of the photoresist interlayer as the upper layer. However, as mentioned above, an organic thin film can also be formed on top of the photoresist interlayer by spin coating, and then a photoresist film can be formed on top of that. When a SiON film is used as the photoresist interlayer, and an organic antireflective film (BARC) with light-absorbing groups at the exposure wavelength is used as the organic thin film, two layers of antireflective films, SiON film and organic thin film, can be used in excimer exposure to suppress reflection even at wetting exposures with high NA values ​​exceeding 1.0. Other advantages of forming an organic thin film include reducing the trailing of the photoresist pattern on the SiON film. Furthermore, when an Adhesive Layer (ADL) film with excellent affinity to the upper photoresist is used as the organic thin film, it can suppress the pattern collapse of the photoresist.

[0323] Examples of three-layer and four-layer resist treatments have been given above, but the resist lower film forming material of the present invention is also useful in two-layer resist treatments using a resist lower film and a resist upper film.

[0324] <Method for Forming the Underlayer Film of Resist>

[0325] This invention provides a method for forming a photoresist underlayer film, which is a method for forming a photoresist underlayer film acting as an organic planarization film used as a manufacturing step of a semiconductor device, characterized by comprising the following steps:

[0326] The resist lower layer film material of the present invention is spin-coated onto the substrate to be processed, and

[0327] A substrate coated with the aforementioned photoresist underlayer film is heat-treated at a temperature of 100°C or higher and 600°C or lower for 10 to 600 seconds to harden and form a photoresist underlayer film.

[0328] Furthermore, a method for forming a resist underlayer film is provided, which is a method for forming a resist underlayer film acting as an organic planarization film used as a manufacturing step of a semiconductor device, characterized by comprising the following steps:

[0329] The resist lower layer film material of the present invention is spin-coated onto the substrate to be processed, and

[0330] The substrate coated with the aforementioned photoresist underlayer film material is heat-treated in a gas environment with an oxygen concentration of 1% or more and 21% or less to harden it, thereby forming the photoresist underlayer film.

[0331] Alternatively, a method for forming a photoresist underlayer film is provided, which is a method for forming a photoresist underlayer film acting as an organic planarization film used as a manufacturing step of a semiconductor device, characterized by comprising the following steps:

[0332] The resist lower layer film material of the present invention is spin-coated onto the substrate to be processed, and

[0333] The substrate coated with the aforementioned resist underlayer film material is heat-treated in a gas environment with an oxygen concentration of less than 1% by volume to harden and form the resist underlayer film.

[0334] In the method for forming the resist lower layer film of the present invention, the aforementioned resist lower layer film material is coated onto the substrate to be processed using a spin coating method or the like. By using a spin coating method, good embedding characteristics can be obtained. After spin coating, the solvent is evaporated, and to prevent mixing with the resist upper layer film and the resist intermediate film, and to promote the crosslinking reaction, baking is performed. Baking is performed, for example, at a temperature range of 100°C or higher and 600°C or lower, preferably 100°C or higher and 300°C or lower, more preferably 150°C or higher and 280°C or lower, for example, for a range of 10 seconds to 600 seconds, preferably 10 to 300 seconds. By appropriately adjusting the baking temperature and time within the above range, planarity / embedding characteristics and curing characteristics suitable for the application can be obtained. If the baking temperature is 100°C or higher, curing will proceed sufficiently, and mixing with the upper layer film or the intermediate film will not occur. If the baking temperature is below 600℃, the thermal decomposition of the base resin can be suppressed, the film thickness will not decrease, and the film surface will become uniform.

[0335] Regarding the gas environment during baking, either an oxygen-containing environment (oxygen concentration of 1% to 21% by volume) in the air or a non-oxygen environment (oxygen concentration of nitrogen) can be selected as needed. For example, when the substrate being processed is easily oxidized by air, heat treatment in a gas environment with an oxygen concentration of less than 1% by volume (non-oxygen environment) can form a hardened film, which can suppress substrate damage.

[0336] Furthermore, the pattern forming method and the resist underlayer film forming method of the present invention are ideally suited for using a substrate with a structure or height difference of 30 nm or more as the substrate to be processed. The resist underlayer film forming method of the present invention is particularly useful when forming a void-free planarized organic film on a substrate with a structure or height difference of 30 nm or more. Moreover, it is also useful when using a substrate with a static contact angle to water of 50° or more as the substrate to be processed.

[0337] Example

[0338] The following examples and comparative examples illustrate the present invention in detail, but the invention is not limited by these descriptions. Furthermore, the molecular weight and dispersity were determined according to the following method. The weight-average molecular weight (Mw) and number-average molecular weight (Mn) of polystyrene obtained by gel permeation chromatography (GPC) using tetrahydrofuran as the eluent were determined, and the dispersity (Mw / Mn) was calculated based on these results.

[0339] Synthesis of compounds used in the lower layer film material of resist synthesis

[0340] The synthesis of compounds (A-1) to (A-10) for the resist underlayer film material and compounds (R-1) and (R-2) for the comparative examples respectively uses the following epoxy compounds: any of the compounds in group A (a-1) to (a-5), compounds containing triple bonds; any of the compounds in group B (b-1) to (b-3), compounds having 3 adjacent hydroxyl groups; and any of the compounds in group C (c-1) to (c-2).

[0341] [Chemistry 32]

[0342]

[0343] [Chemistry 33]

[0344]

[0345] [Chemistry 34]

[0346]

[0347] In the above structural formula, the bonds represented by thick solid lines are those extending from the paper towards the front, while the bonds represented by thick dashed lines are those extending from the paper towards the distance. The same applies below.

[0348] [Synthetic Example 1] Synthesis of compound (A-1)

[0349] 10.21 g of an epoxide compound (a-1), 7.54 g of a carboxylic acid compound containing a triple bond (b-1), 1.46 g of a compound with three adjacent hydroxyl groups (c-1), and 60 g of 2-methoxy-1-propanol were stirred into a homogeneous solution under nitrogen atmosphere at an internal temperature of 100°C. Then, 0.68 g of benzyltriethylammonium chloride was added to this homogeneous solution, and the mixture was stirred at an internal temperature of 110°C for 12 hours. After cooling to room temperature, 200 ml of methyl isobutyl ketone was added to the mixture, and the solution was washed twice with 100 g of 1% ammonia solution, twice with 100 g of 3% nitric acid solution, and five times with 100 g of ultrapure water. The organic layer was dried under reduced pressure to obtain compound (A-1). The weight-average molecular weight (Mw) and dispersion (Mw / Mn) were determined using GPC, yielding the following results.

[0350] [Chemistry 35]

[0351]

[0352] (A-1): Mw=910, Mw / Mn=1.01

[0353] In the structural formula of R, the dashed line at one end, which is not explicitly shown, represents an atomic bond. The same applies below.

[0354] [Synthesis Example 2] Synthesis of compound (A-2)

[0355] 10.21 g of an epoxide compound (a-1), 12.22 g of a carboxylic acid compound containing a triple bond (b-2), 1.15 g of a compound with three adjacent hydroxyl groups (c-2), and 60 g of 2-methoxy-1-propanol were stirred into a homogeneous solution under nitrogen atmosphere at an internal temperature of 100°C. Then, 0.68 g of benzyltriethylammonium chloride was added to this homogeneous solution, and the mixture was stirred at an internal temperature of 110°C for 12 hours. After cooling to room temperature, 200 ml of methyl isobutyl ketone was added to the mixture, and the solution was washed twice with 100 g of 1% ammonia solution, twice with 100 g of 3% nitric acid solution, and five times with 100 g of ultrapure water. The organic layer was dried under reduced pressure to obtain compound (A-2). The weight-average molecular weight (Mw) and dispersion (Mw / Mn) were determined using GPC, yielding the following results.

[0356] [Chemistry 36]

[0357]

[0358] (A-2): Mw=970, Mw / Mn=1.02

[0359] [Synthetic Example 3] Synthesis of Compound (A-3)

[0360] 6.15 g of an epoxide compound (a-2), 3.29 g of a carboxylic acid compound containing a triple bond (b-1), 1.44 g of a compound with three adjacent hydroxyl groups (c-2), and 60 g of 2-methoxy-1-propanol were stirred into a homogeneous solution under nitrogen atmosphere at an internal temperature of 100°C. Then, 0.34 g of benzyltriethylammonium chloride was added to this homogeneous solution, and the mixture was stirred at an internal temperature of 110°C for 12 hours. After cooling to room temperature, 200 ml of methyl isobutyl ketone was added to the mixture, and the mixture was washed twice with 100 g of 1% ammonia solution, twice with 100 g of 3% nitric acid solution, and five times with 100 g of ultrapure water. The organic layer was dried under reduced pressure to obtain compound (A-3). The weight-average molecular weight (Mw) and dispersion (Mw / Mn) were determined using GPC, yielding the following results.

[0361] [Chemistry 37]

[0362]

[0363] (A-3): Mw=1250, Mw / Mn=1.25

[0364] [Synthetic Example 4] Synthesis of Compound (A-4)

[0365] 6.15 g of an epoxide compound (a-2), 6.38 g of a carboxylic acid compound containing a triple bond (b-2), 0.31 g of a compound with three adjacent hydroxyl groups (c-1), and 60 g of 2-methoxy-1-propanol were stirred at an internal temperature of 100°C under nitrogen atmosphere to form a homogeneous solution. Then, 0.34 g of benzyltriethylammonium chloride was added to this homogeneous solution, and the mixture was stirred at an internal temperature of 110°C for 12 hours. After cooling to room temperature, 200 ml of methyl isobutyl ketone was added to the mixture, and the solution was washed twice with 100 g of 1% ammonia solution, twice with 100 g of 3% nitric acid solution, and five times with 100 g of ultrapure water. The organic layer was dried under reduced pressure to obtain compound (A-4). The weight-average molecular weight (Mw) and dispersion (Mw / Mn) were determined using GPC, yielding the following results.

[0366] [Chemistry 38]

[0367]

[0368] (A-4): Mw=1330, Mw / Mn=1.26

[0369] [Synthetic Example 5] Synthesis of Compound (A-5)

[0370] 4.95 g of an epoxide compound (a-3), 4.75 g of a carboxylic acid compound containing a triple bond (b-2), 1.78 g of a compound with three adjacent hydroxyl groups (c-1), and 60 g of 2-methoxy-1-propanol were stirred at an internal temperature of 100°C under nitrogen atmosphere to form a homogeneous solution. Then, 0.34 g of benzyltriethylammonium chloride was added to this homogeneous solution, and the mixture was stirred at an internal temperature of 110°C for 12 hours. After cooling to room temperature, 200 ml of methyl isobutyl ketone was added to the mixture, and the solution was washed twice with 100 g of 1% ammonia solution, twice with 100 g of 3% nitric acid solution, and five times with 100 g of ultrapure water. The organic layer was dried under reduced pressure to obtain compound (A-5). The weight-average molecular weight (Mw) and dispersion (Mw / Mn) were determined using GPC, yielding the following results.

[0371] [Chemistry 39]

[0372]

[0373] (A-5): Mw=2230, Mw / Mn=1.33

[0374] [Synthetic Example 6] Synthesis of Compound (A-6)

[0375] 4.95 g of an epoxide compound (a-3), 5.35 g of a carboxylic acid compound containing a triple bond (b-3), 0.58 g of a compound with three adjacent hydroxyl groups (c-2), and 60 g of 2-methoxy-1-propanol were stirred at 100°C under nitrogen atmosphere to form a homogeneous solution. Then, 0.34 g of benzyltriethylammonium chloride was added to this homogeneous solution, and the mixture was stirred at 110°C for 12 hours. After cooling to room temperature, 200 ml of methyl isobutyl ketone was added to the mixture, and the solution was washed twice with 100 g of 1% ammonia solution, twice with 100 g of 3% nitric acid solution, and five times with 100 g of ultrapure water. The organic layer was dried under reduced pressure to obtain compound (A-6). The weight-average molecular weight (Mw) and dispersion (Mw / Mn) were determined using GPC, yielding the following results.

[0376] [Chemistry 40]

[0377]

[0378] (A-6): Mw=2310, Mw / Mn=1.35

[0379] [Synthesis Example 7] Synthesis of compound (A-7)

[0380] 8.44 g of an epoxide compound (a-4), 10.86 g of a carboxylic acid compound containing a triple bond (b-2), 2.31 g of a compound with three adjacent hydroxyl groups (c-2), and 60 g of 2-methoxy-1-propanol were stirred at an internal temperature of 100°C under nitrogen atmosphere to form a homogeneous solution. Then, 0.68 g of benzyltriethylammonium chloride was added to this homogeneous solution, and the mixture was stirred at an internal temperature of 110°C for 12 hours. After cooling to room temperature, 200 ml of methyl isobutyl ketone was added to the mixture, and the solution was washed twice with 100 g of 1% ammonia solution, twice with 100 g of 3% nitric acid solution, and five times with 100 g of ultrapure water. The organic layer was dried under reduced pressure to obtain compound (A-7). The weight-average molecular weight (Mw) and dispersion (Mw / Mn) were determined using GPC, yielding the following results.

[0381] [Chemistry 41]

[0382]

[0383] (A-7): Mw=750, Mw / Mn=1.05

[0384] [Synthetic Example 8] Synthesis of Compound (A-8)

[0385] 8.44 g of an epoxide compound (a-4), 11.30 g of a carboxylic acid compound containing a triple bond (b-3), 0.52 g of a compound with three adjacent hydroxyl groups (c-1), and 60 g of 2-methoxy-1-propanol were stirred at an internal temperature of 100°C under nitrogen atmosphere to form a homogeneous solution. Then, 0.68 g of benzyltriethylammonium chloride was added to this homogeneous solution, and the mixture was stirred at an internal temperature of 110°C for 12 hours. After cooling to room temperature, 200 ml of methyl isobutyl ketone was added to the mixture, and the mixture was washed twice with 100 g of 1% ammonia solution, twice with 100 g of 3% nitric acid solution, and five times with 100 g of ultrapure water. The organic layer was dried under reduced pressure to obtain compound (A-8). The weight-average molecular weight (Mw) and dispersion (Mw / Mn) were determined using GPC, and the following results were obtained.

[0386] [Chemistry 42]

[0387]

[0388] (A-8): Mw=800, Mw / Mn=1.06

[0389] [Synthesis Example 9] Synthesis of compound (A-9)

[0390] 8.92 g of an epoxide compound (a-5), 18.73 g of a carboxylic acid compound containing a triple bond (b-2), 1.25 g of a compound with three adjacent hydroxyl groups (c-1), and 60 g of 2-methoxy-1-propanol were stirred at an internal temperature of 100°C under nitrogen atmosphere to form a homogeneous solution. Then, 1.02 g of benzyltriethylammonium chloride was added to this homogeneous solution, and the mixture was stirred at an internal temperature of 110°C for 12 hours. After cooling to room temperature, 200 ml of methyl isobutyl ketone was added to the mixture, and the mixture was washed twice with 100 g of 1% ammonia solution, twice with 100 g of 3% nitric acid solution, and five times with 100 g of ultrapure water. The organic layer was dried under reduced pressure to obtain compound (A-9). The weight-average molecular weight (Mw) and dispersion (Mw / Mn) were determined using GPC, yielding the following results.

[0391] [Chemistry 43]

[0392]

[0393] (A-9): Mw=1060, Mw / Mn=1.01

[0394] [Synthetic Example 10] Synthesis of compound (A-10)

[0395] 8.92 g of an epoxide compound (a-5), 16.90 g of a carboxylic acid compound containing a triple bond (b-2), 2.66 g of a compound with three adjacent hydroxyl groups (c-2), and 60 g of 2-methoxy-1-propanol were stirred at an internal temperature of 100°C under nitrogen atmosphere to form a homogeneous solution. Then, 1.02 g of benzyltriethylammonium chloride was added to this homogeneous solution, and the mixture was stirred at an internal temperature of 110°C for 12 hours. After cooling to room temperature, 200 ml of methyl isobutyl ketone was added to the mixture, and the solution was washed twice with 100 g of 1% ammonia solution, twice with 100 g of 3% nitric acid solution, and five times with 100 g of ultrapure water. The organic layer was dried under reduced pressure to obtain compound (A-10). The weight-average molecular weight (Mw) and dispersion (Mw / Mn) were determined using GPC, yielding the following results.

[0396] [Chemistry 44]

[0397]

[0398] (A-10): Mw=1080, Mw / Mn=1.02

[0399] [Comparative Synthesis Example 1] Comparative Example: Synthesis of Compound (R-1)

[0400] 9.43 g of epoxide compound (a-5), 21.52 g of carboxylic acid compound (b-2) containing a triple bond, and 60 g of 2-methoxy-1-propanol were stirred at an internal temperature of 100°C under nitrogen atmosphere to form a homogeneous solution. Then, 1.00 g of benzyltriethylammonium chloride was added to this homogeneous solution, and the mixture was stirred at an internal temperature of 110°C for 12 hours. After cooling to room temperature, 200 ml of methyl isobutyl ketone was added to the mixture, and the mixture was washed twice with 100 g of 1% ammonia solution, twice with 100 g of 3% nitric acid solution, and five times with 100 g of ultrapure water. The organic layer was dried under reduced pressure to obtain the comparative example compound (R-1). The weight-average molecular weight (Mw) and dispersion (Mw / Mn) were determined using GPC, and the following results were obtained.

[0401] [Chemistry 45]

[0402]

[0403] (R-1): Mw=1100, Mw / Mn=1.04

[0404] [Comparative Synthesis Example 2] Comparative Example: Synthesis of Compound (R-2)

[0405] 9.42 g of epoxide compound (a-5), 17.92 g of carboxylic acid compound (b-2) containing a triple bond, 2.66 g of 3,4-dihydroxyphenylacetic acid, and 60 g of 2-methoxy-1-propanol were stirred at an internal temperature of 100°C under nitrogen atmosphere to form a homogeneous solution. Then, 1.00 g of benzyltriethylammonium chloride was added to this homogeneous solution, and the mixture was stirred at an internal temperature of 110°C for 12 hours. After cooling to room temperature, 200 ml of methyl isobutyl ketone was added to the mixture, and the mixture was washed twice with 100 g of 1% ammonia solution, twice with 100 g of 3% nitric acid solution, and five times with 100 g of ultrapure water. The organic layer was dried under reduced pressure to obtain the comparative example compound (R-2). The weight-average molecular weight (Mw) and dispersion (Mw / Mn) were determined using GPC, and the following results were obtained.

[0406] [Chemistry 46]

[0407]

[0408] (R-2): Mw=1220, Mw / Mn=1.06

[0409] [Comparative Synthesis Example 3] Comparative Example: Synthesis of Polymer (R-3)

[0410] A homogeneous solution was prepared by mixing 78.8 g of 2,7-diynepropoxynaphthalene, 21.6 g of 37% formalin solution, and 250 g of 1,2-dichloroethane under nitrogen atmosphere at 70°C. Then, 5 g of methanesulfonic acid was slowly added to this homogeneous solution, and the mixture was stirred at 80°C for 12 hours. After cooling to room temperature, 500 g of methyl isobutyl ketone was added to the mixture. The organic layer was washed five times with 200 g of pure water and then dried under reduced pressure. 300 mL of THF was added to the residue, and the polymer was reprecipitated with 2000 mL of hexane. The precipitated polymer was separated by filtration and dried under reduced pressure to obtain the comparative polymer (R-3). The weight-average molecular weight (Mw) and dispersion (Mw / Mn) were determined using GPC, yielding the following results.

[0411] [Chemistry 47]

[0412]

[0413] (R-3): Mw=2700, Mw / Mn=1.54

[0414] Preparation of resist underlayer film materials (UDL-1~16, comparative UDL-1~3)

[0415] Any one of the above compounds (A-1) to (A-10), comparative example compounds (R-1) and (R-2), and comparative example polymer (R-3) was dissolved in propylene glycol monomethyl ether acetate (PGMEA) as an organic solvent (B) containing 0.1% by mass of PF6320 (manufactured by OMNOVA) as a surfactant (D). The solution was then filtered through a 0.1 μm fluoropolymer filter to prepare photoresist underlayer film materials (UDL-1 to 10, comparative UDL-1 to 3). Furthermore, any one of the compounds (BG1) to (BG3) as alkali generating agents was dissolved together with compound (A-9) in the above PGMEA in the proportions shown in Table 1. This process was repeated in the same manner as for photoresist underlayer film material (UDL-9) to prepare photoresist underlayer film materials (UDL-11 to 13). Furthermore, using compound (X1) as a crosslinking agent, the same process as with the photoresist underlayer material (UDL-11) was used to prepare photoresist underlayer material (UDL-14). Furthermore, using 1,6-diacetoxyhexane (1,6-DAH) as a high-boiling-point solvent (boiling point 260°C) or tripropylene glycol monomethyl ether (TPM) (boiling point 242°C), the same process as with photoresist underlayer materials (UDL-4) and (UDL-6) was used to prepare photoresist underlayer materials (UDL-15) and (UDL-16).

[0416] Compounds (X1), (BG1), (BG2) and (BG3) are shown below.

[0417] [Chemistry 48]

[0418]

[0419] [Table 1]

[0420]

[0421] Example 1: Evaluation of film-forming properties (Examples 1-1 to 1-16, Comparative Examples 1-1 to 1-3)

[0422] The prepared photoresist underlayer materials (UDL-1~16, comparative UDL-1~3) were coated onto the bare-Si substrate, the SiON-treated substrate, and the hexamethyldisilazane (HMDS)-treated substrate shown in Table 2, respectively. The resulting coatings were then fired at 250°C for 60 seconds to form photoresist underlayers with a thickness of 100 nm. Each formed photoresist underlayer was observed using an optical microscope (Nikon ECLIPSE L200) to check for any coating abnormalities. HMDS treatment was performed under two conditions: 90°C × 60 seconds and 120°C × 120 seconds. Furthermore, the water contact angle of each substrate was measured using a contact angle meter (DM-701R manufactured by Kyowa Interface Science Co., Ltd.). The results showed that the bare-Si substrate had a water contact angle of less than 15°, the SiON-treated substrate had a water contact angle of 46°, the HMDS-treated substrate (90°C × 60 seconds) had a water contact angle of 58°, and the HMDS-treated substrate (120°C × 120 seconds) had a water contact angle of 66°. HMDS treatment, involving high temperature and long-term treatment, resulted in substrates that were more hydrophobic and made it difficult to ensure film formation. Also, in this evaluation, the film thickness was minimized to assess the coating performance, which is a stringent evaluation condition prone to film formation abnormalities.

[0423] [Table 2]

[0424]

[0425] As shown in Table 2, Examples 1-1 to 1-16, which used the resist underlayer film material of the present invention, were able to form uniform resist underlayer films without coating abnormalities not only on bare-Si substrates, but also on SiON-treated substrates, HMDS-treated (90°C × 60 seconds) substrates, and HMDS-treated (120°C × 120 seconds) substrates. During film firing, Comparative Examples 1-1 and 1-2 showed numerous pinholes on the HMDS-treated (120°C × 120 seconds) substrate, confirming coating abnormalities. Therefore, it can be seen that, as described in Japanese Patent Application Publication No. 2023-180781, by not combining a compound containing phenolic hydroxyl groups with an alkali generating agent, but instead introducing a terminal group structure with three adjacent hydroxyl groups as described above (3) as part of the terminal group structure, the film formation properties on the substrate can be improved. On the other hand, Comparative Examples 1-3, which contain polymers, were also able to form films on SiON-treated substrates and HMDS substrates.

[0426] Example 2: Evaluation of Edge Recedement (Examples 2-1 to 2-16, Comparative Examples 2-1 to 2-3)

[0427] The resist lower layer film materials (UDL-1~16, comparative UDL-1~3) prepared above were coated on 12-inch bare-Si substrates and HMDS-treated (120℃×120 seconds) substrates with an edge removal width of 2 mm, respectively. The obtained coatings were then fired at 250℃ for 60 seconds. Figure 2As shown in (G), a resist lower layer film (organic film) with a thickness of 100 nm was formed on substrate 7. A film thickness measuring device (ONTO INNOVATION Atlas-XP) was used. + For the formed resist underlayer film, measurements were performed at four locations on each substrate, within a radius of 145mm~149mm from the center of the substrate (9mm). Figure 2 (G) of 8). Figure 2 (H) reveals the average film thickness mark 10 on the bare-Si substrate and the average film thickness mark 11 on the HMDS substrate. As shown here, the point with an average film thickness of 0 nm is identified as the film edge 12, and the difference between the film edge positions on the bare-Si substrate and the HMDS processed substrate is identified as the edge setback distance 13. The results are shown in Table 3. It can be considered that the smaller the edge setback distance 13, the better the coating performance of the HMDS substrate.

[0428] [Table 3]

[0429]

[0430] As shown in Table 3, in Examples 2-1 to 2-16, which used the resist lower film material of the present invention, i.e., examples using a terminal group structure having three adjacent hydroxyl groups as part of the terminal group structure of the above general formula (3), the edge retreat distance was approximately 0.2 mm or less. Considering the error in film thickness measurement, it can be considered that there was almost no edge retreat. In Comparative Examples 2-1 and 2-16, the edge retreat of the film on the HMDS-treated substrate was very large, and the film edge could not be confirmed within the measurement range. Therefore, it can be seen that the present invention is not a combination of a phenolic hydroxyl-containing compound and an alkali generating agent as described in Japanese Patent Application Publication No. 2023-180781, but is useful for improving the edge retreat of the film on the HMDS substrate. On the other hand, in Comparative Examples 2-3 containing a polymer, no edge retreat occurred on the HMDS substrate.

[0431] Example 3: Evaluation of Landfill Characteristics (Examples 3-1 to 3-16, Comparative Examples 3-1 to 3-3)

[0432] The resist underlayer materials (UDL-1~16, comparative UDL-1~3) prepared above were respectively coated on SiO2 wafer substrates with a dense hole pattern (hole diameter 0.16 μm, hole depth 0.50 μm, and distance between the centers of two adjacent holes 0.32 μm), and fired at 250°C for 60 seconds to form the resist underlayer film. The substrate used was as follows. Figure 3The substrate 14 (SiO2 wafer substrate) with a dense hole pattern is shown in (I) (top view) and (J) (cross-sectional view). The cross-sectional shape of each wafer substrate was observed using a scanning electron microscope (SEM) to confirm whether the holes were filled with a resist underlayer 15 without any pores (voids). The results are shown in Table 4. In this evaluation, porosity occurred inside the holes when a resist underlayer material with poor filling properties was used. In this evaluation, when a resist underlayer material with good filling properties was used, as shown in Table 4... Figure 3 As shown in (K), the interior of the hole is non-porous and filled with a resist underlayer film.

[0433] [Table 4]

[0434]

[0435] As shown in Table 4, the resist underlayer film materials of the present invention used in Examples 3-1 to 3-16 can fill the pore pattern without pores, indicating excellent landfill characteristics. On the other hand, in Comparative Example 3-3, due to the presence of a polymer different from the (A) component contained in the resist underlayer film material of the present invention, poor landfilling, which is believed to be due to insufficient thermal fluidity, occurred.

[0436] Example 4 Flatness Evaluation (Examples 4-1 to 4-16, Comparative Examples 4-1 to 4-3)

[0437] The resist lower film materials (UDL-1~16, comparative UDL-1~3) prepared above were respectively coated on patterns with large isolated trenches. Figure 4 On a substrate 16 (SiO2 wafer substrate) with a trench width of 10 μm and a trench depth of 0.1 μm, the resist underlayer 17 was fired at 250°C for 60 seconds. The height difference between the trench and non-trench areas was observed using an NX10 atomic force microscope (AFM) manufactured by Park Systems. Figure 4 (delta 17 in (M)). The results are shown in Table 5. In this evaluation, the smaller the height difference, the better the flatness. Furthermore, in this evaluation, a resist film material with a thickness of about 0.2 μm was used to flatten the trench pattern with a depth of 0.10 μm. In order to evaluate the quality of flatness, this became a strict evaluation condition.

[0438] [Table 5]

[0439]

[0440] As shown in Table 5, the resist underlayer film materials of the present invention used in Examples 4-1 to 4-16 have a smaller height difference between the trench portion and the non-trench portion compared to Comparative Example 4-3, which contains a polymer with a different (A) component than the resist underlayer film material of the present invention, indicating excellent flatness.

[0441] Furthermore, based on the results of Examples 3 and 4 above, it can be seen that the resist underlayer material according to the present invention can still form a resist underlayer film with excellent flatness and film-forming properties even on a substrate with particularly difficult planarization areas.

[0442] Example 5: Pattern Formation Test (Examples 5-1 to 5-16, Comparative Examples 5-1 to 5-3)

[0443] UDL-1~16 and Comparative Examples UDL-1~3 prepared above were coated onto SiO2 substrates with trench patterns (trench width 10 μm, trench depth 0.10 μm) having formed a 200 nm thick SiO2 film after HMDS treatment (120 °C × 120 s). The resulting coatings were then baked at 250 °C for 60 s on a bare Si substrate in atmospheric conditions to achieve a film thickness of 200 nm, forming a lower resist film. A silicon-containing intermediate resist material (SOG-1) was then coated onto the lower resist film, and the coating was baked at 220 °C for 60 s to form a 35 nm thick intermediate resist film. Finally, an upper resist material (SL resist for ArF) was coated onto the intermediate resist film, and the coating was baked at 105 °C for 60 s to form a 100 nm thick upper resist film. A protective film (TC-1) is coated onto the top layer of the resist film, and the coating is baked at 90°C for 60 seconds to form a protective film with a thickness of 50 nm.

[0444] As a top layer film material for resist (SL resist for ArF), it is prepared by dissolving polymer (RP1), acid generator (PAG1), and basic compound (Amine1) in a solvent containing 0.1% by mass of FC-430 (manufactured by Sumitomo 3M Co., Ltd.) in the proportions shown in Table 6, and filtering it through a 0.1 μm fluororesin filter.

[0445] [Table 6]

[0446]

[0447] The structural formulas of the polymer (RP1), acid generator (PAG1), and basic compound (Amine1) used are shown below.

[0448] [Chemistry 49]

[0449]

[0450] As the impregnation protective film material (TC-1), it is prepared by dissolving the protective film polymer (PP1) in an organic solvent according to the proportions in Table 7, and filtering the mixture through a 0.1 μm fluoropolymer filter.

[0451] [Table 7]

[0452]

[0453] The structural formula of the polymer (PP1) used is shown below.

[0454] [Transformation 50]

[0455]

[0456] As a silicon-containing photoresist interlayer material (SOG-1), it is prepared by dissolving a polymer (represented by ArF silicon-containing interlayer polymer (SiP1)) and a crosslinking catalyst (CAT1) in an organic solvent containing 0.1% by mass of FC-4430 (manufactured by Sumitomo 3M) in the proportions shown in Table 8, and filtering the mixture through a fluoropolymer filter with a pore size of 0.1 μm.

[0457] [Table 8]

[0458]

[0459] The structural formulas of the ArF silicon-containing intermediate membrane polymer (SiP1) and crosslinking catalyst (CAT1) used are shown below.

[0460] [Chemistry 51]

[0461]

[0462] Next, the exposure was performed using an ArF immersion exposure apparatus (Nikon, NSR-S610C, NA 1.30, σ 0.98 / 0.65, 35-degree dipole s-polarized illumination, 6% half-step phase shift mask) while varying the exposure amount. The image was then baked at 100°C for 60 seconds (PEB) and developed with a 2.38% by mass tetramethylammonium hydroxide (TMAH) aqueous solution for 30 seconds. A positive line and spacing pattern with a resist linewidth of 50 nm to 30 nm was obtained with a pitch of 100 nm.

[0463] Secondly, using the Telius etching apparatus created by Tokyo Powertech, dry etching was used to process a silicon-containing photoresist intermediate film with the photoresist pattern as a mask, a photoresist lower layer film with the silicon-containing intermediate film as a mask, and a SiO2 film with the lower layer film as a mask.

[0464] The etching conditions are as follows.

[0465] The transfer conditions of resist pattern for SOG film (silicon resist intermediate film).

[0466] Chamber pressure 10.0 Pa

[0467] RF power 1,500W

[0468] CF4 gas flow rate 15 sccm

[0469] O2 gas flow rate 75 sccm

[0470] 15 seconds

[0471] SOG film patterning for the transfer conditions of the resist underlayer film.

[0472] Chamber pressure 2.0 Pa

[0473] RF power 500W

[0474] Ar gas flow rate 75 sccm

[0475] O2 gas flow rate 45 sccm

[0476] 120 seconds

[0477] The transfer conditions of the lower layer film pattern for the SiO2 film.

[0478] Chamber pressure 2.0 Pa

[0479] RF power 2,200W

[0480] C5F 12 Gas flow rate 20 sccm

[0481] C2F6 gas flow rate 10 sccm

[0482] Ar gas flow rate 300 sccm

[0483] O2 gas flow rate 60 sccm

[0484] 90 seconds

[0485] The cross-sections of the patterns were observed using an electron microscope (S-4700) manufactured by Hitachi, Ltd., and the shapes were compared and summarized in Table 9.

[0486] [Table 9]

[0487]

[0488] As shown in Table 9, in Examples 5-1 to 5-16 using the resist underlayer film material of the present invention, the resist upper layer film pattern was successfully transferred to the substrate, confirming that the resist underlayer film material of the present invention is suitable for use in microprocessing using a multilayer resist method. On the other hand, in Comparative Examples 5-1 to 5-2, as shown in the film formation evaluation results of Comparative Examples 1-1 and 1-2, pinholes occurring during film formation caused pattern collapse during pattern processing, preventing pattern formation. In Comparative Example 5-3, as in Comparative Examples 3-3 and 4-3, the filling characteristics and flatness were poor, resulting in pattern collapse during pattern processing and preventing pattern formation.

[0489] As can be seen from the above, if the resist lower layer film material of the present invention is used, it has good film-forming properties and excellent filling characteristics / flatness. Therefore, it is extremely useful as an organic film material used in the multilayer resist method. Furthermore, if the pattern forming method of the present invention uses this resist lower layer film material, it can still form fine patterns with high precision even on substrates with height differences in the processed body.

[0490] This specification includes the following specifications.

[0491] [1] A resist underlayer film material, characterized in that it contains:

[0492] (A) The following compounds or resins represented by general formula (1), and

[0493] (B) Organic solvents,

[0494] [Chemistry 52]

[0495]

[0496] In the formula, W is an n-valent organic group with 2 to 50 carbon atoms, Y is any of the terminal group structures represented by general formula (2) and general formula (3) below. When the proportions of the terminal group structures represented by general formula (2) and general formula (3) constituting Y are a and b respectively, they satisfy the relationships a + b = 1.0, 0.70 ≤ a ≤ 0.99, and 0.01 ≤ b ≤ 0.30, and n is an integer from 1 to 10.

[0497] [Chemistry 53]

[0498]

[0499] In the formula, the dashed line represents an atomic bond, Z represents an aromatic group with 6 to 20 carbon atoms and a (m+1) valence, and A is a single bond or -O-(CH2). p - where m is an integer from 1 to 5, and p is an integer from 1 to 10.

[0500] [Chemistry 54]

[0501]

[0502] In the formula, the dashed lines represent atomic bonds.

[0503] [2] The resist underlayer film material as in [1], wherein A in the general formula (2) is -OCH2-.

[0504] [3] The resist underlayer film material as in [1] or [2], wherein the general formula (2) is any one of the following general formulas (4), (5) and (6),

[0505] [Chemistry 55]

[0506]

[0507] In the formula, the dashed lines represent atomic bonds.

[0508] [4] The resist underlayer film material of any of [1] to [3], wherein W in the general formula (1) is represented by the following general formula (7),

[0509] [Chemistry 56]

[0510]

[0511] In the formula, the dashed line represents the atomic bond, R 1 It is a hydrogen atom, or an alkyl or acyl group having 1 to 20 carbon atoms, which may also contain an oxygen atom and / or a nitrogen atom. 1 Y is an n-valent organic group with 1 to 47 carbon atoms. 1 It can be a single bond or a carbonyl group, and n is an integer from 1 to 10.

[0512] [5] As in [4], the resist underlayer film material, wherein W in the general formula (7) 1 Let any one of the following expressions represent the structure.

[0513] [Chemistry 57]

[0514]

[0515] [Chem.58]

[0516]

[0517] In the formula, the dashed lines represent atomic bonds.

[0518] [6] The resist underlayer film material of any one of [1] to [5], wherein the polystyrene equivalent weight average molecular weight of the (A) compound or resin is less than 3,000.

[0519] [7] The resist underlayer film material of any one of [1] to [6], wherein the (B) organic solvent is a mixture of one or more organic solvents with a boiling point less than 180°C and one or more organic solvents with a boiling point of 180°C or higher.

[0520] [8] The resist underlayer film material of any of [1] to [7] also contains selected from

[0521] (C) Alkali-generating agents

[0522] (D) Surfactants,

[0523] (E) Crosslinking agent,

[0524] (F) Plasticizers, and

[0525] (G) pigment

[0526] One or more of the groups formed.

[0527] [9] As in [8], the resist underlayer film material, wherein the (C) alkali generating agent is a compound that exhibits alkalinity due to thermal decomposition.

[0528]

[10] The resist underlayer film material as in [9], wherein the (C) alkali generating agent is a compound represented by any one of the following general formulas (8), (9) and (10).

[0529] [Chemistry 59]

[0530]

[0531] In the above formula, R 01 ~R 03 Each can independently represent a linear, branched, or cyclic alkyl or alkenyl group with 1 to 10 carbon atoms that can be substituted with or have heteroatom insertions, or an aryl or aralkyl group with 6 to 18 carbon atoms that can be substituted with or have heteroatom insertions. Also, R 01 R 02 and R 03 Any two atoms in X can also bond to each other and form a ring together with the sulfur atom in the formula. - This refers to anions that are organic or inorganic and can be classified as relative ions, but X... - Excluding OH - R 04 and R 05 Each aryl group is independently composed of 6 to 20 carbon atoms, and some or all of the hydrogen atoms of this aryl group may be substituted by straight-chain, branched, or cyclic alkyl or alkoxy groups having 1 to 10 carbon atoms. Furthermore, R... 04 and R 05 They can also bond with each other and form a ring together with the iodine atoms in the formula, R 06R 07 R 08 and R 09 Each can independently represent a hydrogen atom, or a linear, branched, or cyclic alkyl or alkenyl group with 1 to 20 carbon atoms that may be substituted with heteroatoms or have heteroatom insertions; or it can represent an aryl or aralkyl group with 6 to 18 carbon atoms that may be substituted with heteroatoms or have heteroatom insertions. Also, R 06 R 07 R 08 and R 09 Any two or more of them can bond with each other and form a ring together with the nitrogen atom in the formula.

[0532]

[11] As in

[10] , the resist underlayer film material, wherein the anion X in the general formulas (8), (9) and (10) is... - The term "anion" refers to anion that has a structure represented by any of the following general formulas (11), (12), and (13), and anion that is part of the group consisting of chloride ions, bromide ions, iodide ions, fluoride ions, cyanide ions, nitrate ions, and nitrite ions.

[0533] [Transformation 60]

[0534]

[0535] In the above formula, R 10 This indicates a linear, branched, or cyclic alkyl, alkenyl, aralkyl, or aryl group with 1 to 20 carbon atoms, which may also contain an ether group, ester group, or carbonyl group. One or more hydrogen atoms in these groups may be substituted with halogen atoms, hydroxyl groups, carboxyl groups, amino groups, and / or cyano groups. R 11 R represents an aryl group with 6 to 20 carbon atoms, wherein one or more hydrogen atoms in the aryl group may be substituted with halogen atoms, hydroxyl groups, carboxyl groups, amino groups, and / or cyano groups. 12 R 13 and R 14 Each group independently represents a hydrogen atom, or a halogen atom other than fluorine, or may contain an ether group, ester group, or carbonyl group, and is a straight-chain, branched, or cyclic alkyl, alkenyl, aralkyl, or aryl group with 1 to 20 carbon atoms. One or more hydrogen atoms in these groups may be substituted with halogen atoms, hydroxyl groups, carboxyl groups, amino groups, and / or cyano groups. Furthermore, R 12 R 13 and R 14 Two or more of them can also bond together to form a ring.

[0536]

[12] As in

[10] or

[11] , the resist underlayer film material, wherein X in the general formula (8), (9) and (10) - The boiling point of the conjugate acid XH is below 200℃.

[0537]

[13] The resist underlayer film material of any one of [8] to

[12] , wherein the (E) crosslinking agent is a compound represented by the following general formula (14),

[0538] [Chemistry 61]

[0539]

[0540] In the formula, Q is a single bond, or a q-valent hydrocarbon group with 1 to 20 carbon atoms, and R 16 It is hydrogen or an alkyl group having 1 to 20 carbon atoms, and q is an integer from 1 to 5.

[0541]

[14] A pattern forming method is a method for forming a pattern on a substrate to be processed, characterized by having the following steps:

[0542] (I-1) A resist underlayer material of any one of [1] to

[13] is coated onto a substrate to obtain a coating film, and the coating film is heat-treated to form a resist underlayer film.

[0543] (I-2) An upper resist film is formed on the lower resist film using a photoresist material.

[0544] (I-3) The upper layer of the photoresist is exposed to a pattern, and then developed with a developer to form a pattern on the upper layer of the photoresist.

[0545] (I-4) Using the upper resist film with the pattern already formed as a mask, dry etch the lower resist film to transfer the pattern onto the lower resist film.

[0546] (I-5) The patterned resist underlayer film is used as a mask to process the substrate to be processed, thereby forming a pattern on the substrate to be processed.

[0547]

[15] A pattern forming method is a method for forming a pattern on a substrate to be processed, characterized by having the following steps:

[0548] (II-1) A resist underlayer material of any one of [1] to

[13] is coated onto a substrate to obtain a coating film, and the coating film is heat-treated to form a resist underlayer film.

[0549] (II-2) An intermediate resist film is formed on the lower layer of the resist film.

[0550] (II-3) A photoresist upper film is formed on the intermediate film of this resist using a photoresist material.

[0551] (II-4) The upper layer of the photoresist is exposed to a pattern, and then developed with a developer to form a pattern on the upper layer of the photoresist.

[0552] (II-5) Using the upper resist film with the pattern already formed as a mask, dry etch the intermediate resist film to transfer the pattern onto the intermediate resist film.

[0553] (II-6) Using the resist intermediate film with the transferred pattern as a mask, dry etch the resist lower layer film to transfer the pattern onto the resist lower layer film, and

[0554] (II-7) The patterned resist underlayer film is used as a mask to process the substrate to be processed, thereby forming a pattern on the substrate to be processed.

[0555]

[16] A pattern forming method is a method for forming a pattern on a substrate to be processed, characterized by having the following steps:

[0556] (III-1) A resist underlayer material of any one of [1] to

[13] is coated onto a substrate to obtain a coating film, and the coating film is heat-treated to form a resist underlayer film.

[0557] (III-2) An inorganic hard mask intermediate film, selected from the group consisting of silicon oxide film, silicon nitride film, and silicon oxide nitride film, is formed on the lower layer of the resist film.

[0558] (III-3) An organic thin film is formed on the intermediate film of the inorganic hard mask.

[0559] (III-4) A photoresist top layer film is formed on this organic thin film using a photoresist material.

[0560] (III-5) The upper layer of the photoresist is exposed to a pattern, and then developed with a developer to form a pattern on the upper layer of the photoresist.

[0561] (III-6) Using the resist film on which the pattern has been formed as a mask, dry etch the organic film and the intermediate film of the inorganic hard mask to transfer the pattern onto the organic film and the intermediate film of the inorganic hard mask.

[0562] (III-7) Using the inorganic hard mask intermediate film with the transferred pattern as a mask, dry etch the photoresist underlayer film to transfer the pattern onto the photoresist underlayer film, and

[0563] (III-8) The patterned resist underlayer film is used as a mask to process the substrate to be processed, thereby forming a pattern on the substrate to be processed.

[0564]

[17] The patterning method of

[16] wherein the inorganic hard mask intermediate film is formed by CVD or ALD.

[0565]

[18] The pattern forming method of any of

[14] to

[17] uses a structure or substrate with a height difference of 30 nm or more as the substrate to be processed.

[0566]

[19] The pattern forming method of any of

[14] to

[17] uses a substrate with a static contact angle of 50° or more with water as the substrate to be processed.

[0567]

[20] A method for forming a photoresist underlayer film, which is a method for forming a photoresist underlayer film acting as an organic planarization film used as a manufacturing step of a semiconductor device, characterized by comprising the following steps:

[0568] Spin-coating a resist underlayer material, such as any one of [1] to

[13] , onto the substrate being processed, and

[0569] The substrate coated with the photoresist underlayer film is heat-treated at a temperature between 100°C and 600°C for 10 to 600 seconds to harden and form the photoresist underlayer film.

[0570]

[21] A method for forming a photoresist underlayer film, which is a method for forming a photoresist underlayer film acting as an organic planarization film used as a manufacturing step of a semiconductor device, characterized by comprising the following steps:

[0571] Spin-coating a resist underlayer material, such as any one of [1] to

[13] , onto the substrate being processed, and

[0572] The substrate coated with the photoresist underlayer film is heat-treated in a gas environment with an oxygen concentration of 1% or more and 21% or less to harden and form the photoresist underlayer film.

[0573]

[22] A method for forming a photoresist underlayer film, which is a method for forming a photoresist underlayer film acting as an organic planarization film used as a manufacturing step of a semiconductor device, is characterized by comprising the following steps:

[0574] Spin-coating a resist underlayer material, such as any one of [1] to

[13] , onto the substrate being processed, and

[0575] The substrate coated with the photoresist underlayer film is heat-treated in a gas environment with an oxygen concentration of less than 1% by volume to harden and form the photoresist underlayer film.

[0576]

[23] The method for forming a resist underlayer film according to any one of

[20] to

[22] uses a substrate with a structure or height difference of 30 nm or more as the substrate to be processed.

[0577]

[24] The method for forming a resist underlayer film according to any one of

[20] to

[23] uses a substrate with a static contact angle of 50° or more with water as the substrate to be processed.

[0578] Furthermore, the present invention is not limited to the embodiments described above. The embodiments described above are illustrative, and those that have substantially the same structure and perform the same effect as the technical concept described in the claims of the present invention are all included within the technical scope of the present invention.

[0579] Explanation of reference numerals in the attached figures

[0580] 1:Substrate

[0581] 2: Processed layer

[0582] 2a: Pattern formed on the processed layer

[0583] 3: Underlayer film of resist

[0584] 3a: Pattern of the underlayer resist film

[0585] 4: Resist Interlayer

[0586] 4a: Pattern of the resist interlayer

[0587] 5: Top layer of resist film

[0588] 5a: Pattern of the upper layer of the resist film

[0589] 6: Important Parts (Exposed Sections)

[0590] 7: Resist lower layer film coated on substrate

[0591] 8: Film thickness measurement locations (4 locations)

[0592] 9: Center of substrate

[0593] 10: Average film thickness spot diagram on bare-Si substrate

[0594] 11: Average film thickness dot plot on HMDS substrate

[0595] 12: Film edge

[0596] 13: Edge back distance

[0597] 14: Substrate with dense hole pattern

[0598] 15: Underlayer film of resist

[0599] 16: Substrate with a large isolated trench pattern

[0600] 17: Underlayer film of resist

[0601] delta 17: The height difference of the resist underlayer between the trench section and the non-trench section.

Claims

1. A resist underlayer film material, characterized in that it contains: (A) The following compounds or resins represented by general formula (1), and (B) Organic solvents, In the formula, W is an n-valent organic group with 2 to 50 carbon atoms, Y is any of the terminal group structures represented by general formula (2) and general formula (3) below. When the proportions of the terminal group structures represented by general formula (2) and general formula (3) constituting Y are a and b respectively, they satisfy the relationships a + b = 1.0, 0.70 ≤ a ≤ 0.99, and 0.01 ≤ b ≤ 0.30, and n is an integer from 1 to 10. In the formula, the dashed line represents an atomic bond, Z represents an aromatic group with 6 to 20 carbon atoms and a (m+1) valence, and A is a single bond or -O-(CH2). p - where m is an integer from 1 to 5, and p is an integer from 1 to 10. In the formula, the dashed lines represent atomic bonds.

2. The resist underlayer film material according to claim 1, wherein, In the general formula (2), A is -OCH2-.

3. The resist underlayer film material according to claim 1, wherein, The general formula (2) is any one of the following general formulas (4), (5) and (6). In the formula, the dashed lines represent atomic bonds.

4. The resist underlayer film material according to claim 1, wherein, In this general formula (1), W is represented by the following general formula (7). In the formula, the dashed line represents the atomic bond, R 1 It is a hydrogen atom, or an alkyl or acyl group having 1 to 20 carbon atoms, which may also contain an oxygen atom and / or a nitrogen atom. 1 Y is an n-valent organic group with 1 to 47 carbon atoms. 1 It can be a single bond or a carbonyl group, and n is an integer from 1 to 10.

5. The resist underlayer film material according to claim 4, wherein, In the general formula (7), W 1 Let any one of the following expressions represent the structure. In the formula, the dashed lines represent atomic bonds.

6. The resist underlayer film material according to claim 1, wherein, The polystyrene equivalent weight-average molecular weight of the (A) compound or resin is less than 3,000.

7. The resist underlayer film material according to claim 1, wherein, The organic solvent (B) is a mixture of one or more organic solvents with a boiling point less than 180°C and one or more organic solvents with a boiling point greater than 180°C.

8. The resist underlayer film material according to claim 1, further comprising selected from... (C) Alkali-generating agents (D) Surfactants, (E) Crosslinking agent, (F) Plasticizers, and (G) pigment One or more of the groups formed.

9. The resist underlayer film material according to claim 8, wherein, The (C) base-generating agent is a compound that exhibits basicity due to thermal decomposition.

10. The resist underlayer film material according to claim 9, wherein, The (C) base-generating agent is a compound represented by any one of the following general formulas (8), (9) and (10). In the above formula, R 01 ~R 03 Each can independently represent a linear, branched, or cyclic alkyl or alkenyl group with 1 to 10 carbon atoms that can be substituted with or have heteroatom insertions, or an aryl or aralkyl group with 6 to 18 carbon atoms that can be substituted with or have heteroatom insertions. Also, R 01 R 02 and R 03 Any two atoms in X can also bond to each other and form a ring together with the sulfur atom in the formula. - This refers to anions that are organic or inorganic and can be classified as relative ions, but X... - Excluding OH - R 04 and R 05 Each aryl group is independently composed of 6 to 20 carbon atoms, and some or all of the hydrogen atoms of this aryl group may be substituted by straight-chain, branched, or cyclic alkyl or alkoxy groups having 1 to 10 carbon atoms. Furthermore, R... 04 and R 05 They can also bond with each other and form a ring together with the iodine atoms in the formula, R 06 R 07 R 08 and R 09 Each can independently represent a hydrogen atom, or a linear, branched, or cyclic alkyl or alkenyl group with 1 to 20 carbon atoms that may be substituted with heteroatoms or have heteroatom insertions; or it can represent an aryl or aralkyl group with 6 to 18 carbon atoms that may be substituted with heteroatoms or have heteroatom insertions. Also, R 06 R 07 R 08 and R 09 Any two or more of them can bond with each other and form a ring together with the nitrogen atom in the formula.

11. The resist underlayer film material according to claim 10, wherein, The anion X in general formulas (8), (9) and (10) - The term "anion" refers to anion that has a structure represented by any of the following general formulas (11), (12), and (13), and anion that is part of the group consisting of chloride ions, bromide ions, iodide ions, fluoride ions, cyanide ions, nitrate ions, and nitrite ions. In the above formula, R 10 This indicates a linear, branched, or cyclic alkyl, alkenyl, aralkyl, or aryl group with 1 to 20 carbon atoms, which may also contain an ether group, ester group, or carbonyl group. One or more hydrogen atoms in these groups may be substituted with halogen atoms, hydroxyl groups, carboxyl groups, amino groups, and / or cyano groups. R 11 R represents an aryl group with 6 to 20 carbon atoms, wherein one or more hydrogen atoms in the aryl group may be substituted with halogen atoms, hydroxyl groups, carboxyl groups, amino groups, and / or cyano groups. 12 R 13 and R 14 Each group independently represents a hydrogen atom, or a halogen atom other than fluorine, or may contain an ether group, ester group, or carbonyl group, and is a straight-chain, branched, or cyclic alkyl, alkenyl, aralkyl, or aryl group with 1 to 20 carbon atoms. One or more hydrogen atoms in these groups may be substituted with halogen atoms, hydroxyl groups, carboxyl groups, amino groups, and / or cyano groups. Furthermore, R 12 R 13 and R 14 Two or more of them can also bond together to form a ring.

12. The resist underlayer film material according to claim 10, wherein, X in general formulas (8), (9) and (10) - The boiling point of the conjugate acid XH is below 200℃.

13. The resist underlayer film material according to claim 8, wherein, The (E) crosslinking agent is a compound represented by the following general formula (14). In the formula, Q is a single bond, or a q-valent hydrocarbon group with 1 to 20 carbon atoms, and R 16 It is hydrogen or an alkyl group having 1 to 20 carbon atoms, and q is an integer from 1 to 5.

14. A pattern forming method, characterized by comprising the following steps: (I-1) A coating is obtained by coating a substrate with a resist underlayer material according to any one of claims 1 to 13, and the coating is heat-treated to form a resist underlayer film. (I-2) An upper resist film is formed on the lower resist film using a photoresist material. (I-3) The upper layer of the photoresist is exposed to a pattern, and then developed with a developer to form a pattern on the upper layer of the photoresist. (I-4) Using the upper resist film with the pattern already formed as a mask, dry etch the lower resist film to transfer the pattern onto the lower resist film. (I-5) The patterned resist underlayer film is used as a mask to process the substrate to be processed, thereby forming a pattern on the substrate to be processed.

15. A pattern forming method, characterized by comprising the following steps: (II-1) A coating is obtained by coating a substrate with a resist underlayer material according to any one of claims 1 to 13, and the coating is heat-treated to form a resist underlayer film. (II-2) An intermediate resist film is formed on the lower layer of the resist film. (II-3) A photoresist upper film is formed on the intermediate film of this resist using a photoresist material. (II-4) The upper layer of the photoresist is exposed to a pattern, and then developed with a developer to form a pattern on the upper layer of the photoresist. (II-5) Using the upper resist film with the pattern already formed as a mask, dry etch the intermediate resist film to transfer the pattern onto the intermediate resist film. (II-6) Using the resist intermediate film with the transferred pattern as a mask, dry etch the resist lower layer film to transfer the pattern onto the resist lower layer film, and (II-7) The patterned resist underlayer film is used as a mask to process the substrate to be processed, thereby forming a pattern on the substrate to be processed.

16. A pattern forming method, characterized by comprising the following steps: (III-1) A coating is obtained by coating a substrate with the resist underlayer material according to any one of claims 1 to 13, and the coating is heat-treated to form a resist underlayer film. (III-2) An inorganic hard mask intermediate film, selected from the group consisting of silicon oxide film, silicon nitride film, and silicon oxide nitride film, is formed on the lower layer of the resist film. (III-3) An organic thin film is formed on the intermediate film of the inorganic hard mask. (III-4) A photoresist top layer film is formed on this organic thin film using a photoresist material. (III-5) The upper layer of the photoresist is exposed to a pattern, and then developed with a developer to form a pattern on the upper layer of the photoresist. (III-6) Using the resist film on which the pattern has been formed as a mask, dry etch the organic film and the intermediate film of the inorganic hard mask to transfer the pattern onto the organic film and the intermediate film of the inorganic hard mask. (III-7) Using the inorganic hard mask intermediate film with the transferred pattern as a mask, dry etch the photoresist underlayer film to transfer the pattern onto the photoresist underlayer film, and (III-8) The patterned resist underlayer film is used as a mask to process the substrate to be processed, thereby forming a pattern on the substrate to be processed.

17. The pattern forming method according to claim 16, wherein, The inorganic hard mask intermediate film is formed using CVD or ALD methods.

18. The pattern forming method according to claim 14, wherein a structure having a height of 30 nm or more or a substrate having a height difference is used as the substrate to be processed.

19. The pattern forming method according to claim 14, wherein a substrate having a static contact angle with water of 50° or more is used as the substrate to be processed.

20. A method for forming a photoresist underlayer film, which is a method for forming a photoresist underlayer film acting as an organic planarization film used as a manufacturing step of a semiconductor device, characterized by comprising the following steps: Spin-coating the resist underlayer material according to any one of claims 1 to 13 onto the substrate being processed, and The substrate coated with the photoresist underlayer film is heat-treated at a temperature between 100°C and 600°C for 10 to 600 seconds to harden and form the photoresist underlayer film.

21. A method for forming a photoresist underlayer film, which is a method for forming a photoresist underlayer film acting as an organic planarization film used as a manufacturing step of a semiconductor device, characterized by comprising the following steps: Spin-coating the resist underlayer material according to any one of claims 1 to 13 onto the substrate being processed, and The substrate coated with the photoresist underlayer film is heat-treated in a gas environment with an oxygen concentration of 1% or more and 21% or less to harden and form the photoresist underlayer film.

22. A method for forming a photoresist underlayer film, which is a method for forming a photoresist underlayer film acting as an organic planarization film used as a manufacturing step of a semiconductor device, characterized by comprising the following steps: Spin-coating the resist underlayer material according to any one of claims 1 to 13 onto the substrate being processed, and The substrate coated with the photoresist underlayer film is heat-treated in a gas environment with an oxygen concentration of less than 1% by volume to harden and form the photoresist underlayer film.

23. The method for forming a resist underlayer film according to claim 20, wherein a substrate having a structure with a height of 30 nm or more or a height difference is used as the substrate to be processed.

24. The method for forming a resist underlayer film according to claim 20, wherein a substrate having a static contact angle with water of 50° or more is used as the substrate to be processed.

Citation Information

Patent Citations

  • Method and device for forming silicon nitride film, and method for preprocessing of cleaning thereof

    JP2002334869A

  • Pattern forming method, and material for forming underlayer film

    JP2004205685A

  • Photoresist underlayer film forming material and pattern forming method

    JP2007199653A

  • New photoacid generator, resist material using the same, and pattern forming method

    JP2009269953A

  • Organic film material, method for forming organic film and method for forming pattern using the same, and heat-decomposable polymer

    JP2013253227A