Double-sided alignment micro-nano suspension diaphragm photolithography method

By fixing amine sites on the pore walls of the silicon nitride suspended film and connecting the acid layer and the receiving layer with through adhesive pillars, the positional error problem of the two-sided marking formation was solved, realizing a more stable double-sided alignment micro/nano suspended film photolithography method, improving the stability of pattern alignment and the integrity of marking.

CN123156533APending Publication Date: 2026-11-24SHENZHEN GOLDENKEN OPTICS ELECTRONICS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611660129.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-26
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

In the processing of silicon nitride suspended films, existing technologies make it difficult to independently form micro-nano patterns on both sides without introducing positional errors. Furthermore, the acid reception and edge confinement of cross-film marking transfer are mutually restrictive, leading to instability in the marking formation process.

Method used

Amine sites are fixed in the pore walls and connected to a through-gel column to form a single-sided acid-feeding layer and a back-side receiving layer without acid-generating agent. A two-sided reference is formed by the same marking exposure, and the gel phase connection is released during the development process to control the acid transfer path and edge restriction.

Benefits of technology

It improves the correlation between the two sides of the suspended membrane alignment marks, reduces the positional difference between the two sides of the marks, improves the concentration of the back receiving layer edge, and ensures the material correlation and pattern alignment stability during the mark formation stage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123156533A_ABST
    Figure CN123156533A_ABST
Patent Text Reader

Abstract

This invention relates to the field of photolithography materials and double-sided pattern alignment technology, and discloses a photolithography method for double-sided alignment of micro / nano suspended films. The method uses a silicon nitride suspended film with a through-hole reference region and a non-porous active region as the processing body. A silane layer containing terminal amino groups is fixed on the hole wall of the reference region. A protective polymer without photoacid-generating agents is used to form a through-link adhesive pillar and a back-side receiving layer, connecting the front-side acid-gathering layer and the back-side receiving layer via the adhesive pillar. Marking exposure is performed only on the front side, followed by heating, development, and transfer of the markings on both sides to a chromium layer. After removing the adhesive phase used for marking, each side completes the micro / nano pattern photolithography using the corresponding chromium markings. This method, by fixing the positional alignment of the acid-gathering sites with the continuous adhesive phase, converges the marking edges, reduces alignment deviations introduced by separately establishing markings, and balances the preservation of the pattern on the back-side receiving layer with subsequent independent imaging of the active region. It is suitable for double-sided pattern processing of suspended thin films for micro / nano devices.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of photolithography materials and double-sided pattern alignment technology, and discloses a photolithography method for double-sided alignment of micro-nano suspended films. Background Technology

[0002] Silicon nitride suspended films are used in micro / nano devices, electrode windows, and thin-film sensing structures. The relative positions of the patterns on both sides affect the electric field distribution, localized heating, and effective observation area. Current processing methods typically involve first forming a mark on one side, then using double-sided exposure equipment, transmission imaging, or windowing to expose the mark and establish a reference on the other side. Existing thin-film device technologies use the same mark for subsequent layers, while other research involves directly writing the resist on the back side using an electron beam penetrating the film. Acid transfer lithography is also used to transfer latent images between adjacent polymer layers. Each of these approaches has its applicable conditions. For thin films requiring independent micro / nano patterns on both sides, the formation process of the reference pattern and the resolution of the active pattern still need to be controlled separately.

[0003] The back side of the suspended film is located at the bottom of the silicon frame cavity, and the local adhesive layer is easily affected by solvent wetting, surface sites, and heat treatment conditions. When photoacid is transferred through adjacent adhesive layers, acid migration and the deprotection of unstable acid groups jointly determine the development profile; the amount of acid applied, acid capture, and development transition point all affect the edge position. While uniformly adding free amine to the receiving adhesive can suppress background reactions, it also consumes the effective acid at the center of the pattern, and the position of free alkali changes with diffusion. Exposing both sides separately introduces errors in mark readout and pattern formation for each side. If the film thickness, adhesive layer thickness, and via state are incompatible, the transmitted signal may only reach the surface layer, leaving residual adhesive that affects mark transfer.

[0004] Therefore, it is necessary to limit unwanted acid transfer while maintaining effective back-side reception, and to ensure that the restricted position persists throughout the marker formation stage. Simply increasing the exposure dose will expand the acid-affected area, while simply increasing the uniform alkali content will reduce the degree of center deprotection; these are not independent conditions that can be arbitrarily strengthened. The practical requirement is to establish a clear connection between the acid-catching position and the transmembrane pathway, so that the markers on both sides are formed from a single pattern event, and then the gel phase connection is terminated in a timely manner to prevent it from participating in the next imaging of the active area. The method should also provide the source of the pore wall sites, the formation mode of the continuous gel column, the developability conditions of the receiving layer, and the marker retention order, and use a control of canceling the fixed position to distinguish the effects of general alkali doping and position constraint. Summary of the Invention

[0005] To address the problems in existing technologies where acid reception and edge confinement mutually restrict each other in cross-membrane label transfer, and where independent label establishment on both sides introduces positional errors, this invention provides a bi-directional alignment micro / nano suspended film photolithography method.

[0006] To solve the above-mentioned technical problems, the present invention provides a method to fix amine sites on the pore wall and connect a single-sided acid-giving layer and a back-side receiving layer without acid-generating agent by a through-resin pillar; to form a two-sided reference by the same marking exposure, and then to perform two-sided patterning photolithography after the resist phase connection is released.

[0007] In practice, the polymer side groups contain acid-sensitive tert-butyloxycarbonyl groups. After photocatalytic removal, the proportion of phenolic hydroxyl groups increases, enabling the receiving layer to be removed in alkaline developer. The continuous polymer within the pores provides a mass transfer pathway, while the terminal amines fixed by silicon-oxygen bonds on the pore walls accept protons, transforming the easily mobile, uniform quencher into a positionally stable acid-catching boundary. The effective acid flux at the pattern center differs from that at the weakly exposed edges, and the limited acid-catching capacity has different effects on both. This spatial relationship is related to the fixed position and pathway contact conditions, and is analyzed in conjunction with the pore area distribution, witness film acidification response, and receiving layer profile.

[0008] Furthermore, in the above technical solution, the silicon nitride film has a thickness of 20 nm, a floating window of 50 µm × 50 µm, an active region of 20 µm × 20 µm, a pore size of 300 nm, a pitch of 600 nm, and a 5 µm gap between the reference region and the active region.

[0009] In practice, the film length defines the path required for transmembrane acid transport, while the pore size and pitch define the distribution scale of the pathways. The reference region pore array serves micron-level marking and does not directly replicate the 200nm lines of the active region. Vias are arranged outside the active region to prevent adhesive pillars from altering the effective surface of the device and from converting marking exposure into device patterning exposure. The 20nm film maintains a short transport distance with the thin receiving layer, and the multi-pore readout of the pore array reduces the impact of individual pore geometric differences on the marking center.

[0010] Furthermore, in the above technical solution, the non-porous platform of the through-hole reference area is covered by a polymethyl methacrylate protective film with a perforated opening, the oxidized surface of the hole wall remains exposed, and the platform protective film is removed after silane fixation.

[0011] In practice, the platform protective film restricts silane contact to the pore walls and orifice edges, preventing the fixed amine from covering the entire receiving surface. Silane in methanol can contact the exposed oxidized surface within the pores, which is separated by the protective polymer on the platform; curing and rinsing remove soluble substances, followed by the removal of the platform protective film with acetone. Without this positional separation, the fixed amine still has an acid-catching effect, but the acid-catching surface will penetrate the central bottom surface of the receiving layer, altering the effective acid pathway. The distribution of nitrogen and carbon fragments in the pore area is used to check the location of the fixed amine.

[0012] Furthermore, in the above technical solution, the 3-aminopropyltriethoxysilane and propyltriethoxysilane are mixed in a molar ratio of 1:9 to 1:3 in a 10 mmol / L methanol bath, and then contacted at 23°C for 180 min and cured at 100°C for 45 min.

[0013] In practice, triethoxysilane is first hydrolyzed under aqueous and silanol conditions on the surface, and then condenses with hydroxyl groups on the oxidized surface to form siloxane linkages. The terminal amino group does not participate in this siloxane linkage, retaining proton accepting ability. Propylsilane provides a common covering component without amino groups, changing the ratio of adjacent amine sites without changing the acid-trapping positions. 1:9 and 1:3 were used in Examples 2 and 3, respectively. The lower ratio retains more central acid flux, while the higher ratio increases edge trapping but also increases effective acid loss. The surface ratio is related to the competitive covering of the two silanes, and is analyzed in conjunction with the feed ratio and pore retention signal.

[0014] Furthermore, in the above technical solution, the through-link adhesive column, the back receiving layer and the acid-donating layer are all made of poly(p-tert-butyloxycarbonyloxystyrene), the orifice covering layer is 5 nm, and the receiving layer is 10-20 nm.

[0015] In practice, using the same polymer avoids introducing polymer distribution differences into transmembrane migration. The filler within the pores and the thin layers on both sides are in continuous contact after pre-baking, eliminating the need for acid to cross incompatible solvent layers or voids. The 10-20nm receiving layer reduces the axial path and residual film during development, while retaining the resist thickness for wet etching of the 5nm chromium layer. The lower limit of the thin layer corresponds to coverage continuity, while the upper limit corresponds to the time required for acid to reach the furthest depth; both are compared using examples with different film thicknesses. If air gaps form within the pores, simply increasing exposure cannot establish material bonding.

[0016] Furthermore, in the above technical solution, the 50nm acid layer contains 3% triphenylsulfonate perfluorobutane sulfonate relative to the polymer mass, and no free alkaline quencher is added to the glue column and the receiving layer.

[0017] In practice, the matte salt generates a strong acid after being irradiated by the acid-provided layer, which catalyzes the removal of tert-butyloxycarbonyl groups in the polymer. The backing layer does not contain an acid-producing agent, preventing the 248nm light directly transmitted to the back from being labeled using a different acid-producing reaction; the chemical changes on the back depend on the acid input from the adhesive columns. The receiving layer does not contain free base, retaining the deprotection capability of the pattern center; acid capture is primarily handled by the fixed pore wall sites. A 3% acid-provided ratio limits the initial acid inventory, and a 50nm adhesive thickness controls the scale of the acid-provided layer; both are merely basic conditions for transfer and reaction compatibility.

[0018] Furthermore, in the above technical solution, the acid-coated layer is pre-formed on an independent carrier and transferred to the pore cover layer by soft contact at 40°C for 30 seconds, without introducing the film-forming solvent during the transfer.

[0019] In practice, if the acid-generating solution is directly recoated onto the same polymer thin layer, the solvent will swell the original resin phase and carry the matte salt into the resin column or receiving layer, disrupting the boundary of one-sided acid generation. Pre-film soft contact allows the polymer surfaces to connect without providing a solution flow path for the matte salt, and the solvent removed by pre-baking no longer wets the original layer. The 40°C contact stage is lower than the post-baking temperature, primarily completing the contact process; the space writing of the acid still occurs during subsequent exposure and heating. This step is used to maintain the position of the acid-generating agent.

[0020] Furthermore, in the above technical solution, the marking exposure uses 248nm radiation and 80-120mJ / cm². 2 The front-side dose is applied, while the back-side receiver layer is not separately marked for exposure.

[0021] In practice, single-sided marking and exposure determine the planar location of the acid source; there is no second independent acid-generating pattern on the back side. The fixed amine first consumes the locally arriving acid; the center and low-dose edges form different degrees of deprotection under limited capture conditions, and the development transition point is jointly determined by the polymer state. (80-120 mJ / cm²) 2 The dose samples showed variations within the normal pattern formation range.

[0022] Furthermore, in the above technical solution, after the marking is exposed, it is heated at 105-115℃ for 60-90 seconds, and then cooled to 23℃ for double-sided development.

[0023] In practice, heating simultaneously increases acid migration and deprotection rates, and also accelerates the capture and deactivation processes. The degree of axial reach is determined by the transition points of diffusion, reaction, capture, and development. The 105-115℃ and 60-90s time are matched to the thickness of the film, the acid supply, and the receiving adhesive. Residual film increases at the low-temperature end, while edge migration is enhanced at the high-temperature end. Extending the time gradually approaches the reaction plateau. Lowering the temperature to 23℃ reduces continued migration before development, fixing the pattern formation stages on both sides within the same processing sequence.

[0024] Furthermore, in the above technical solution, the marking adhesive pattern is transferred to a 5nm chromium layer on each side, and after removing the continuous adhesive phase for marking, a new photoresist for the active area is formed. The new photoresist is not connected to the original adhesive pillars.

[0025] In practice, the resist patterns formed by the receiving layer and the acid-coated layer control the removal and retention of the chromium layer, transforming the alignment marks from a transient resist state into a material pattern that can be read further. Subsequently, resist removal severs the material pathways, preventing the acid from being carried to the other side by the original resist pillars during the next exposure of the active area. The newly formed 80nm resist layer is aligned according to the chromium marks on each side, only accommodating the required 200nm lines and 400nm pitch. The joint formation of the marks and the independent formation of the device pattern are two interdependent processes; the chromium layer, resist removal, and conventional exposure only serve as the foundation for implementing this interdependence.

[0026] Compared with the prior art, the beneficial effects of the present invention are as follows: 1. Improved the correlation between the two-sided alignment marks on the suspended film, reduced the positional differences caused by separate marking on both sides, and improved the concentration of the receiving layer edge on the back side. Fixed pore wall position, continuous adhesive columns, single-sided acid supply, and the absence of acid-generating agents on the back side collectively maintained the material correlation during the marking stage. Platform protection and a common polymer system reduced background variations in non-pore areas. Pre-formed transfer of the acid-supply layer improved the regional retention of the acid-generating agent, while the thin receiving layer and controlled heating balanced reception and development, maintaining the integrity of the mark transfer to the chromium layer.

[0027] 2. This method improves the process transition between the marking and micro / nano patterning stages, enhancing the stability of subsequent pattern alignment on both sides. Removing the continuous adhesive phase after chromium marking on both sides reduces interference from the original acid feeding path to subsequent imaging of the active area, while preserving the ability of each side to independently select patterns. By limiting the fixed amine coverage position and ensuring the receiving adhesive layer is free of free alkali, the direct competition between central development and background suppression is reduced, improving the consistency of residual film state and marker readout. This method maintains the respective processing functions of micron-level reference and nano-level patterning, making it suitable for double-sided pattern alignment on the thin film. Attached Figure Description

[0028] Figure 1 This is a spatial distribution diagram of amine-related nitrogen fragments fixed in the pore region according to the present invention.

[0029] Figure 2 This is a diagram showing the nitrogen chemical state changes of the silane witness tablets of the present invention.

[0030] Figure 3 This is a graph showing the development edge height of the back receiving layer of the present invention.

[0031] Figure 4 This is a cumulative distribution diagram of the double-sided pattern overlay deviation of the present invention. Detailed Implementation

[0032] In the following examples, unless otherwise stated, poly(p-tert-butyloxycarbonyloxystyrene) is a powder obtained according to a publicly disclosed synthetic route, with a polystyrene equivalent weight-average molecular weight of 12,000, and tert-butyloxycarbonyl-protected styrene repeating units as the main component; 3-aminopropyltriethoxysilane and propyltriethoxysilane have a purity of 98%, triphenylsulfonate perfluorobutane sulfonate is an electronic material grade powder, propylene glycol methyl ether acetate, methanol, and acetone are electronic grade, and the resistivity of ultrapure water is 18.2 MΩ·cm. The platform protection uses polymethyl methacrylate with a weight-average molecular weight of 950,000, and the soft contact carrier is a pre-cured polydimethylsiloxane sheet. The membrane is a 20nm low-stress silicon nitride suspension membrane supported by a silicon frame, with a window size of 50µm × 50µm, an active region of 20µm × 20µm, and a reference region with a pore size of 300nm, a pitch of 600nm, and a 5µm gap from the active region. Each side of the reference region has a 5nm chromium layer; the pores penetrate the membrane and the chromium layer, and the pore walls contain native oxide surfaces. The membrane was provided by a raw material chip of specified dimensions. Each sample used three independent chips, all of which were equilibrated at 23℃ and 45% relative humidity for 30 minutes before testing.

[0033] Example 1: This example is a representative preferred embodiment of a biplane alignment micro / nano suspended film photolithography method.

[0034] Formula: The silane bath is prepared in 10 mL portions, with a total silane content of 0.100 mmol. It contains 4.4274 mg of 3-aminopropyltriethoxysilane and 16.5088 mg of propyltriethoxysilane. 9.9 mL of methanol is added initially, then the volume is increased to 10 mL. The platform protective adhesive consists of 0.1000 g of polymethyl methacrylate and 9.9000 g of propylene glycol methyl ether acetate. The through-coating solution consists of 0.0500 g of poly(p-tert-butyloxycarbonyloxystyrene) and 9.9500 g of propylene glycol methyl ether acetate; the receiving solution consists of 0.1000 g of the same polymer and 9.9000 g of propylene glycol methyl ether acetate; the acid-feeding solution consists of 0.3000 g of the same polymer, 0.0090 g of triphenylsulfonium perfluorobutanesulfonate, and 9.6910 g of propylene glycol methyl ether acetate; the patterning solution consists of 0.5000 g of the same polymer, 0.0150 g of triphenylsulfonium perfluorobutanesulfonate, and 9.4850 g of propylene glycol methyl ether acetate. Each solution is prepared independently to a yield of 10.0000 g, with 0.1000 g used per batch and the remaining 9.9000 g stored in a sealed container. Residual coating liquid is collected separately, and the evaporated solvent is discharged. Film formation is measured by thickness, not by the quality of the recovered film. The formulations are not combined.

[0035] How to use: S1. Fix the three aforementioned raw material chips onto an open fixture that only contacts the silicon frame. Clean with 5 mL of acetone for 60 seconds at 23°C, then with 5 mL of methanol for 60 seconds. Slowly purge with dry nitrogen for 30 seconds, ensuring contact on both sides and that the suspended window is not subjected to jet positive pressure. Cover the two non-porous platforms of the reference area with a pre-fabricated platform protective film with perforated openings. The protective film is derived from the platform protective adhesive in this example, with a dry film thickness of 80 nm. The openings correspond one-to-one with the existing vias, and the via walls remain exposed. The active area continues to be covered with the same protective film. The protective film pattern uses the existing vias as the conventional positioning basis for the opening positions.

[0036] S2. Treat the exposed pore area with 10W oxygen plasma for 20s to make the hydroxyl groups on the oxide surface of the pore wall accessible. Immerse the chip in a 10mL silanization bath for 23°C for 180min; after removal, rinse three times with 5mL methanol and bake at 100°C for 45min. The aminopropyl-containing silane forms silicon-oxygen bonds with the oxide surface of the pore wall, with the terminal amino groups remaining at the pore boundary. Then, soak in 10mL acetone at 23°C for 60s to remove the platform protective film, wash with 5mL methanol for 30s, and slowly dry with nitrogen for 30s. The resulting silanized membrane on the pore wall enters S3, and the waste bath and each rinsing solution are collected separately.

[0037] S3. Mix the through-hole adhesive and the receiving adhesive separately at 23°C for 30 min, and filter through a 0.1µm polytetrafluoroethylene (PTFE) filter membrane. Wet both hole areas with the through-hole adhesive for 30 s, and spray in batches using 0.1000 g of batch dosage, ensuring the thin adhesive contacts and dries within the holes; pre-bake at 80°C for 120 s, retaining the polymer within the holes and the 5nm orifice capping layer on the front side. Form a 15nm layer on the back side with the receiving adhesive, pre-bake at 80°C for 120 s, ensuring continuous contact between the receiving layer and the lower end of the adhesive column. Separately, apply the acid-donating adhesive to an independent polydimethylsiloxane carrier and pre-bake at 80°C for 120 s to form a 50nm acid-donating layer, then transfer it to the front hole orifice capping layer with a soft contact at 40°C for 30 s, with the contact load borne by the silicon frame; remove the carrier, and do not add any more film-forming solvent. The resulting structure sequentially includes an acid-donating layer, an orifice capping layer, an adhesive column within the holes, and a back receiving layer; the latter two do not contain matte salt. The remaining coating liquid from each batch of 0.1000g adhesive solution is recycled separately and not mixed into the next batch of adhesive solution.

[0038] S4. Expose the acid-coated front layer at 248 nm with a 4µm wide micron-sized marking pattern, using a dose of 100mJ / cm². 2 The back side was not exposed separately. Both sides were then exposed to 110°C for 60 seconds, allowing the acid to be transferred to the back side via a continuous gel column and undergo proton acceptance with the amine fixed in the pore walls. After heating, the temperature was lowered to 23°C within 20 seconds under nitrogen atmosphere. The films were divided into a further processing group and a corresponding characterization group. The characterization group retained both the silanized state and the pre-development state; the processing parameters were the same for all groups.

[0039] In step S5, at 23°C, 10 mL of 2.38% tetramethylammonium hydroxide aqueous solution was used per batch for development, with each side developing for 30 seconds. A total of 5 mL of ultrapure water was used for rinsing each side for 20 seconds. The alignment resist pattern was used as a mask, and a chromium wet etching solution was applied at 23°C for 15 seconds. The etching solution consisted of 16 g of cerium ammonium nitrate and 8 mL of 70% nitric acid. 80 mL of ultrapure water was added to dissolve the etchant, and the solution was then brought to a final volume of 100 mL. 10 mL of this solution was used per batch, and both sides were treated in the same batch. The exposed 5 nm chromium area was removed, and both sides were retained to reference the pattern. The sheets were then rinsed with 5 mL of ultrapure water for 20 seconds. The substrate was then immersed in 10 mL of propylene glycol methyl ether acetate at 40°C for 120 seconds to remove the acid-donating layer, receiving layer, and polymer within the pores. The substrate was then cleaned with 5 mL of methanol for 30 seconds, dried under nitrogen for 30 seconds, and finally subjected to 5W oxygen plasma for 20 seconds to remove organic residues. The resulting chromium-labeled film proceeded to step S6, where the flow through the resist phase was terminated.

[0040] S6. Form new 80nm adhesive layers in the active area using a patterned adhesive solution, and pre-bake each side at 80℃ for 120s; align with the chromium markers retained on each side, and perform 248nm and 35mJ / cm² tests respectively. 2 The pattern was exposed, baked at 100°C for 60 seconds, developed in 10 mL of 2.38% tetramethylammonium hydroxide aqueous solution for 30 seconds per batch, and rinsed in 10 mL of ultrapure water for 20 seconds. Test patterns with a linewidth of 200 nm and a pitch of 400 nm were designed; the numerical aperture of the alignment instrument was 0.75, and focusing was performed face-by-face. Only independent pattern writing in the same sequence was performed on the other side; neither new resist layer was connected to the old resist pillars. The resulting film retained the double-sided lithographic pattern under silicon frame support for overlay and linewidth reading.

[0041] Example 2: The difference between this example and Example 1 is that the silane molar ratio in S2 is changed to 1:9, that is, 2.2137 mg of 3-aminopropyltriethoxysilane and 18.5724 mg of propyltriethoxysilane, with methanol added to 10 mL; the rest of the formula and S1, S3-S6 are all the same as in Example 1.

[0042] Example 3: The difference between this example and Example 1 is that the silane molar ratio in S2 is changed to 1:3, that is, 5.5343 mg of 3-aminopropyltriethoxysilane and 15.4770 mg of propyltriethoxysilane, with methanol added to 10 mL; the rest of the formula and S1, S3-S6 are all the same as in Example 1.

[0043] Example 4: The difference between this example and Example 1 is that the thickness of the back receiving layer in S3 is changed to 10nm, while the composition of the receiving adhesive and the thickness of the orifice coverage remain unchanged; S1, S2 and S4-S6 all refer to Example 1.

[0044] Example 5: The difference between this example and Example 1 is that the thickness of the back receiving layer in S3 is changed to 20nm, while the composition of the receiving adhesive and the thickness of the orifice coverage remain unchanged; S1, S2 and S4-S6 all refer to Example 1.

[0045] Example 6: The difference between this example and Example 1 is that the baking temperature after marking S4 is changed to 105℃, while the time remains 60s; all formulas and S1-S3, S5, and S6 refer to Example 1.

[0046] Example 7: The difference between this example and Example 1 is that the baking temperature after marking S4 is changed to 115℃, while the time remains 60s; all formulas and S1-S3, S5, and S6 refer to Example 1.

[0047] Example 8: The difference between this example and Example 1 is that the baking time after marking S4 is changed to 90s, while the temperature remains at 110℃; all formulas and S1-S3, S5 and S6 refer to Example 1.

[0048] Example 9: The difference between this example and Example 1 is that the exposure dose for the S4 front marking is changed to 80 mJ / cm. 2 All formulations, other S4 parameters, and S1-S3, S5, and S6 are referenced from Example 1.

[0049] Example 10: The difference between this example and Example 1 is that the exposure dose for the S4 front marking is changed to 120 mJ / cm. 2 All formulations, other S4 parameters, and S1-S3, S5, and S6 are referenced from Example 1.

[0050] Comparative Example 1: The difference between this comparative example and Example 1 is that in S2, 20.6360 mg of propyltriethoxysilane was used to replace all the amino-containing silanes, maintaining the total silane at 0.100 mmol and the bath volume at 10 mL, and the fixed amine site was removed. All other formulations are the same as in Example 1 for S1 and S3-S6. This control compares the labeling formation when the acid-trapping node is removed and the disclosed acid transfer principle is applied to a continuous colloidal phase.

[0051] Comparative Example 2: The difference between this comparative example and Example 1 is that S2 is the same as Comparative Example 1, without fixing the amine; in S3, 0.000027 g of 2,6-di-tert-butylpyridine is added to the receiving gel, the polymer remains at 0.1000 g, and propylene glycol methyl ether acetate is changed to 9.899973 g, for a total of 10.0000 g. The free alkali is uniformly introduced into the receiving gel, and the composition of the gel column in the pore remains unchanged; under the set surface area and receiving gel amount, the boundary is fixed with the contactable alkali equivalent, and the effect of changing the acid-catching position is compared, combined with the analysis results of differences in alkali structure and migration. The remaining formulations and S1, S4-S6 refer to Example 1.

[0052] Comparative Example 3: The difference between this comparative example and Example 1 is that S2 is the same as in Comparative Example 1. In S3, the receiving adhesive is changed to 0.1000g of poly(p-tert-butyloxycarbonyloxystyrene), 0.0030g of triphenylsulfonium perfluorobutane sulfonate, and 9.8970g of propylene glycol methyl ether acetate. In S4, the back side is marked with 248nm and 100mJ / cm according to the corresponding marking plate. 2 Independent exposures were performed, with each side positioned using the original silicon frame as a reference; post-baking was the same at 110°C for 60 seconds. The remaining formulations and S1, S5, and S6 are referenced in Example 1. This control is a controlled, independently marked route, incorporating several necessary differences regarding the absence of an acid-generating agent, the number of exposures, and the location of the fixed amine.

[0053] Test method: Nitrogen fragment peripore enrichment factor: After S2 rinsing, removal of the plateau protective film, and before S3 coating, the same-sized well areas of three chips for each sample were collected. Time-of-flight secondary ion mass spectrometry was used, with low-dose scanning of bismuth cluster primary ions and simultaneous recording of CN in the negative ion channel. − and SiO − Counting; 1.2µm × 1.2µm field of view, 49 × 49 pixels, pixel center spacing 25nm, recording four holes with a diameter of 300nm. The periphery region is defined as pixels with a radius of 110-190nm from the hole center, and the hole-free plateau is pixels with a distance greater than 230nm from the nearest hole center. The enrichment factor per chip is the periphery CN. − Average count divided by platform CN − Average counting, taking the arithmetic average of the 3 chips. SiO − Used for base channel verification. CN − The analysis was conducted in conjunction with the evidence from Kong Zhoufu and the N 1s testimonial film.

[0054] Nitrogen chemical state: Three silica witness sheets were prepared for each sample, corresponding to the S2 silane bath for batch treatment and rinsing; the witness sheets were kept with exposed oxide surfaces, and the platform protection was only used for the actual membranes. The state before acidification was recorded; 0.0150 g of perfluorobutyric acid was first added to 9.9 mL of ultrapure water and then diluted to 10 mL to prepare a 5.0 mmol / L acid solution. Each sheet was exposed for 30 s, dried under nitrogen, and the state after acidification was recorded. Monochromatic aluminum X-ray XPS was used, with N 1s ranging from 396-405 eV, intervals of 0.05 eV, 0.25 s per point, and a flux of 20 eV; the energy reference was 284.8 eV of C 1s. Responses near 399.6 eV and 401.6 eV were used to analyze the chemical states of free amines and protonated amines, respectively, and interpreted in conjunction with pore space measurement results.

[0055] Residual film thickness of the receiving layer: For each sample, three independent chips were collected using a tapping atomic force microscope after development in S4 and S5, respectively, along the same 1.0µm line segment at the marked edge, with a point spacing of 2nm, for a total of 501 points. The zero height point was the adjacent exposed chromium surface, and the instrument's longitudinal reading resolution was 0.01nm. The average residual film height of each chip was calculated by taking 125 points with a lateral position less than -250nm after development. The average of the three chips was the result, in nm. The final average value of the obtained height less than 0 was considered as zero residual film, and the original readings were not truncated.

[0056] Edge transition width: Using the complete height line after development as described above, the edge shape of the low plateau plus the height difference multiplied by a logarithmic function is fitted. The transition width is obtained from the difference in the horizontal coordinates corresponding to 10% and 90% of the fitted height difference, in nm. Each sample is the average of 3 chips; all point-by-point original readings are retained, and this width is used to characterize the development profile.

[0057] Pattern overlay error: Each sample consists of 3 chips, with each chip having 5×5 grid positions, totaling 75 positions. The center coordinates of the front and back sides are directly derived from the same coordinate measurement system. The back side mirror transformation uses a pre-fixed silicon frame coordinate system; this coordinate transformation relationship is uniformly adopted for all samples. The original table retains the front side's horizontal and vertical coordinates as well as the horizontal and vertical coordinates after the back side mirror transformation. Deviation per position r = [(back side horizontal coordinate - front side horizontal coordinate)] 2 + (back ordinate - front ordinate) 2 The square root of ] results in 75 r. 2 The square root of the mean, in nm. Recording resolution is 0.1 nm, and the method readout uncertainty is on the order of 20 nm.

[0058] Effective label ratio: 3 chips per sample, 4 candidate labels read per chip, for a total of 12. A unified criterion for a readable label is that the center deviation between the two sides is less than or equal to 150 nm, the label width on the back side is 3600-4400 nm, and the residual film thickness of the receiving layer is less than 2 nm. Ratio = Number of qualified labels / 12 × 100%, results in %. The original table retains the center coordinates, width, residual film height, and qualified count for each label.

[0059] The test results are shown in Table 1.

[0060] Table 1 Performance test results of each embodiment and comparative example sample Nitrogen fragment peripore enrichment factor Residual thickness of receiver layer (nm) Marker edge transition width (nm) Pattern overlay error (nm) Valid labeling percentage (%) Example 1 9.02 0.03 36.0 58.6 100.0 Example 2 5.02 0.04 38.1 57.5 100.0 Example 3 11.06 0.02 36.1 66.0 100.0 Example 4 9.15 0.03 34.5 50.6 100.0 Example 5 9.13 0.06 39.0 51.5 100.0 Example 6 9.15 0.34 67.0 53.8 100.0 Example 7 9.15 0.04 25.1 55.8 100.0 Example 8 9.20 0.01 33.4 59.4 100.0 Example 9 8.95 0.02 37.5 50.7 100.0 Example 10 9.09 0.02 36.0 46.6 100.0 Comparative Example 1 1.00 0.03 40.7 52.7 100.0 Comparative Example 2 1.00 0.04 32.9 66.7 100.0 Comparative Example 3 0.97 0.01 24.8 67.3 100.0 Results analysis: Depend on Figure 1It can be seen that Example 1 shows the formation of cyclic nitrogen-carbon fragment enrichment around the four pores, while Comparative Example 1, using amine-free propylsilane, shows a pore periphery signal close to the background. Both images use the same coordinate range and counting color scale, supporting the difference in localization of organic nitrogen-containing components in the pore regions. The spatial origin of acid-trapping sites is analyzed by combining rinsing retention conditions and the nitrogen chemical state of the witness sheet.

[0061] Depend on Figure 2 It can be seen that the silane witness sheets of the same batch in Example 1 have a free amine response of around 399.6 eV before acidification, and a protonated amine response of around 401.6 eV after acidification, while Comparative Example 1 maintains a low nitrogen background. This figure is used to analyze the chemical basis of fixed amine accepting protons, and to interpret the transmembrane transport process by combining the spatial distribution of the pore region and the change in the height of the receiving layer.

[0062] Depend on Figure 3 It can be seen that the back receiving layers of Example 1, Comparative Example 1, and Comparative Example 2 all have an edge transitioning from a low residual film area to a complete adhesive layer after development. The transition in Example 1 is relatively concentrated, the edge of Comparative Example 1 widens after the fixed acid-collecting sites are removed, and the edge position changes after the alkali is dispersed in the adhesive layer in Comparative Example 2. The curves retain point-by-point height fluctuations, supporting the different effects of fixed position and uniform alkali doping.

[0063] Depend on Figure 4 It can be seen that the overlay deviation of Example 1 is mainly distributed in a smaller range than that of Comparative Examples 2 and 3; the curve of Comparative Example 1 is located to the left of Example 1, indicating that the removal of the fixed amine did not worsen the overlay performance of this group. This result reflects the relationship between the marking edge and the final readout error. Each curve comes from 75 positions across 3 chips, and the steps represent the empirical cumulative proportion; no continuous curve interpolation was performed.

[0064] Among the various embodiments, Example 1 had a nitrogen fragment peripore enrichment factor of 9.02, a receiver layer residual film thickness of 0.03 nm, a marker edge transition width of 36.0 nm, and a pattern overlay error of 58.6 nm. Examples 2 (low silane ratio) and 3 (high silane ratio) had enrichment factors of 5.02 and 11.06, respectively, and edge widths of 38.1 nm and 36.1 nm, respectively. Examples 4 and 5 covered receiver layers of 10 nm and 20 nm, respectively, with residual films of 0.03 nm and 0.06 nm, respectively. In temperature, time, and dose samples, different indicators did not improve synchronously; receiver distance and effective acid loss jointly limited the residual film, while marker edge and readout dispersion jointly affected overlay. Example 1 represents a point of compatibility under various conditions.

[0065] Comparative Example 1, with the amine fixed on the pore wall removed, had a peripore enrichment factor of 1.00, an edge width of 40.7 nm, and an overlay error of 52.7 nm; its overlay value was smaller than that of Example 1. This control retained both the through-column gel and the single-sided acid supply, distinguishing the removal of the fixed acid-collecting boundary. Comparative Example 2 placed the alkali in the receiving gel, with an edge width of 32.9 nm and a residual film thickness of 0.04 nm. Its edge was narrower and its position changed, indicating that uniform alkali doping is not an equivalent replacement for fixing the pore wall position, but the different chemical structures and accessibility of the alkali also contribute to the difference. Comparative Example 3 exposed and formed markers, with an overlay error of 67.3 nm and an effective marking ratio of 100.0%; this control included multiple conditional differences, and the results were analyzed comprehensively by combining factors such as independent marker position error, acid-generating agent, and fixed amine position. Figure 1 and Figure 2 Supporting site location and proton acceptance prerequisites, Figure 3 Supports developing mode. Figure 4 It reflects the overlay distribution under given coordinate measurement conditions.

Claims

1. A photolithography method for bifacial alignment of micro / nano suspended films, characterized in that, Includes the following steps: S1. A silicon nitride suspension film having a non-porous active region and a through-hole reference region is provided. A silane layer containing terminal amino groups is fixed on the oxidized surface of the pore wall of the through-hole reference region, and the non-porous platform is separated from the silane layer containing terminal amino groups. S2. Fill the through hole with poly(p-tert-butyloxycarbonyloxystyrene) without photoacid-generating agent to form a through adhesive column connecting the front hole and the back receiving layer. The front hole contacts the acid-donating layer containing photoacid-generating agent. The back receiving layer does not contain photoacid-generating agent. S3. Only the acid layer is exposed with a marked pattern, and then heated so that the acid generated by the exposure enters the back receiving layer through the through-gel column, and the amino groups at the end of the pore wall remain fixed during the heating; S4. Develop the marking adhesive layers on the front and back sides. Transfer the selected two-sided adhesive patterns from the same marking exposure to the corresponding chromium layers. After removing the through-adhesive pillars, acid-coated layers, and back-side receiving layers, use the two-sided chromium markings as references for the photolithography of the micro-nano patterns on each side.

2. The photolithography method for bifacial alignment micro / nano suspended films according to claim 1, characterized in that, The silicon nitride suspended membrane has a thickness of 20 nm and a suspension window of 50 µm × 50 µm. The non-porous active region has a thickness of 20 µm × 20 µm. The via reference region is located outside the non-porous active region and is spaced 5 µm apart from it. The via has a diameter of 300 nm and a pitch of 600 nm.

3. The photolithography method for bifacial alignment micro / nano suspended films according to claim 1, characterized in that, Before the silane layer containing terminal amino groups is fixed, a polymethyl methacrylate protective film with through-hole openings is used to cover the non-porous platform of the through-hole reference area to expose the oxidized surface of the pore wall. The protective film is removed after silane fixation and rinsing.

4. The photolithography method for bifacial alignment micro / nano suspended films according to claim 3, characterized in that, The silane layer containing terminal amino groups is formed by 3-aminopropyltriethoxysilane and propyltriethoxysilane in a molar ratio of 1:9 to 1:3 in a silane bath, with a total concentration of 10 mmol / L. Methanol is used as the solvent, and the mixture is contacted at 23°C for 180 min and then cured at 100°C for 45 min.

5. The photolithography method for bifacial alignment micro / nano suspended films according to claim 1, characterized in that, The polymers of the through-hole column, the back receiving layer, and the acid-donating layer are all poly(p-tert-butyloxycarbonyloxystyrene). The through-hole column continuously occupies the space inside the hole and forms a 5nm covering layer at the front hole opening. The thickness of the back receiving layer is 10-20nm.

6. The photolithography method for bifacial alignment micro / nano suspended films according to claim 5, characterized in that, The thickness of the acid-coated layer is 50 nm, wherein the mass of triphenylsulfonate perfluorobutanesulfonate is 3% of the mass of poly(p-tert-butyloxycarbonyloxystyrene), and no free alkaline quencher is added to the through-hole adhesive column and the back receiving layer.

7. The photolithography method for bifacial alignment micro / nano suspended films according to claim 6, characterized in that, The acid-donating layer is first formed on an independent carrier, and then transferred to the front orifice cover layer by soft contact at 40°C for 30 seconds. During the transfer of the acid-donating layer, the through-hole adhesive column and the back receiving layer are not wetted by the film-forming solvent.

8. The photolithography method for bifacial alignment micro / nano suspended films according to claim 1, characterized in that, The marking pattern is exposed using 248nm radiation, with a frontal exposure dose of 80-120mJ / cm². 2 The back receiving layer does not receive independent mark exposure during the mark pattern exposure.

9. The photolithography method for bifacial alignment micro / nano suspended films according to claim 8, characterized in that, The heating temperature after the marking pattern is exposed is 105-115℃ for 60-90 seconds. After heating, the film is cooled to 23℃, and then the marking adhesive layers on both sides are developed.

10. The photolithography method for bifacial alignment micro / nano suspended films according to claim 1, characterized in that, The thickness of the chromium layer on each side used to receive the marking adhesive pattern is 5nm. After the chromium marking is transferred on both sides, the through adhesive pillar, the acid-giving layer and the back receiving layer are removed first. Then, new photoresist layers are formed in the non-porous active area and the patterns on each side are exposed. The new photoresist layers are not connected to the through adhesive pillars by continuous adhesive.