Analysis method for optimizing wear resistance of Cr12 cast ball based on heat treatment process adjustment

By setting up a composite heat treatment process space and multi-dimensional evaluation indicators, and combining nanoindentation testing and electron backscattering scanning, the problem of Cr12 cast balls being hard but not tough was solved, and the wear resistance performance was optimized and the stability of mass production was achieved.

CN123159102APending Publication Date: 2026-11-24ANHUI SANFANG NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611351302.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-02
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

The existing heat treatment process for Cr12 cast balls ignores the mechanical matching relationship between microscopic multiphase structures, resulting in materials that are hard but not tough, and are prone to spalling under impact conditions. Furthermore, it lacks objective mathematical model guidance and relies on manual experience for optimization.

Method used

By setting up a composite heat treatment process space, combining nanoindentation testing and electron backscatter diffraction scanning, the hardness gradient matching coefficient and phase transformation hardening layer depth are calculated. A multidimensional evaluation index is established using grey relational analysis, the optimal heat treatment process parameters are output, and a PID algorithm is applied for closed-loop temperature control.

Benefits of technology

The quantitative evaluation of the microstructure and mechanical matching of Cr12 cast balls was achieved, which improved the wear resistance and stability of mass production, and ensured the material's real service performance and the consistency of finished product quality under complex working conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123159102A_ABST
    Figure CN123159102A_ABST
Patent Text Reader

Abstract

This invention discloses a method for optimizing the wear resistance of Cr12 cast balls based on adjustments to the heat treatment process, belonging to the field of performance optimization analysis technology. The method involves setting a composite process space including austenitization, controlled interrupted quenching, and carbon partitioning, and extracting the input feature matrix to perform heat treatment on the samples. Micro-area hardness data is obtained using nanoindentation testing, and the hardness gradient matching coefficient is calculated and threshold screening is performed. Wear tests are conducted on qualified samples to obtain the macroscopic volumetric wear rate, and the effective phase transformation hardening layer depth is calculated using electron backscatter diffraction scanning. The above indicators are constructed into a sequence, and a correlation model is established using the information entropy weight method and grey relational analysis. The optimal process scheme is output and applied to mass production using PID closed-loop control. This invention achieves quantitative evaluation of micromechanical and dynamic phase transformation characteristics, outputs optimal process parameters, and improves the wear resistance of Cr12 cast balls.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of performance optimization analysis technology, and specifically relates to a method for optimizing the wear resistance of Cr12 cast balls based on the adjustment of heat treatment process flow. Background Technology

[0002] Cr12 high-carbon high-chromium cast iron, due to its high content of high-hardness eutectic carbides, has a high initial hardness and is widely used in ball mills and semi-autogenous mills in industries such as mining and cement as the core grinding media (cast balls) to undertake the task of crushing and grinding ores.

[0003] In current industrial production, the heat treatment process for Cr12 cast balls mainly employs a conventional high-temperature austenitizing quenching combined with low-temperature tempering. The aim of this process is to partially dissolve the carbides and obtain as much martensite matrix as possible after quenching, in order to achieve extremely high macroscopic hardness. When adjusting and evaluating the heat treatment process, existing analytical methods typically employ a trial-and-error approach. This involves setting several different quenching temperatures, conducting macroscopic wear tests after treatment, and evaluating the wear resistance by measuring the mass difference before and after the test (macroscopic weight loss method).

[0004] Existing technologies only focus on macroscopic hardness and macroscopic weight loss, ignoring the mechanical matching relationship between microscopic multiphase structures. This results in materials that are often hard but not tough, and are prone to spalling under impact conditions. At the same time, existing evaluation methods lack quantitative analysis of the dynamic evolution of the subsurface structure of materials during wear (such as strain-induced phase transformation), and process optimization is highly dependent on human experience and lacks objective mathematical model guidance. Summary of the Invention

[0005] (a) Technical problems to be solved To address the problems in related technologies, this invention provides an optimization analysis method for the wear resistance of Cr12 cast balls based on adjustments to the heat treatment process, thereby overcoming the aforementioned technical problems in existing related technologies.

[0006] (II) Technical Solution To solve the above-mentioned technical problems, the present invention is achieved through the following technical solution: This invention provides a method for optimizing the wear resistance of Cr12 cast balls based on adjustments to the heat treatment process, comprising the following steps: S1. Obtain Cr12 cast ball samples to be optimized, and set a composite heat treatment process space including full austenitization, controlled interrupted quenching, and carbon partitioning. The process parameters in the composite heat treatment process space are extracted as the input feature matrix, and the Cr12 cast ball samples are heat-treated to obtain heat-treated cast ball samples. S2. Perform microscopic mechanical property mapping test on the heat-treated cast ball sample to obtain micro-area hardness data and elastic modulus data, and calculate the hardness gradient matching coefficient. S3. Determine whether the hardness gradient matching coefficient is within the compatibility threshold range; if so, perform a simulated working condition impact wear test on the heat-treated cast ball sample, record the macroscopic volume wear rate, and perform electron backscatter diffraction scanning on the wear subsurface layer to calculate the effective phase transformation hardening layer depth; otherwise, discard the heat-treated cast ball sample and the corresponding input feature matrix. S4. Construct the macroscopic volumetric wear rate, hardness gradient matching coefficient, and effective phase transformation hardening layer depth into an evaluation index sequence; use grey relational analysis to establish a grey comprehensive correlation model between the input feature matrix and the evaluation index sequence; S5. Calculate the gray comprehensive correlation degree of each input feature matrix in the composite heat treatment process space using the gray comprehensive correlation degree model; take the input feature matrix corresponding to the maximum value of the gray comprehensive correlation degree as the optimal heat treatment process flow adjustment scheme, and mass-produce Cr12 casting balls. By setting up a composite heat treatment process space and extracting process parameters as input feature matrices, and combining microscopic mechanical property mapping tests and simulated working condition impact and wear tests, a multi-dimensional evaluation index sequence is obtained. A mathematical model of the input feature matrix and the evaluation index sequence is established using grey relational analysis, realizing a quantitative mapping from process parameters to macroscopic, microscopic, and dynamic performance. This avoids the limitations of relying solely on macroscopic weight loss evaluation and can objectively output a heat treatment process adjustment scheme that optimizes comprehensive performance, thereby improving the process stability and wear resistance of Cr12 cast balls in mass production.

[0007] Preferably, step S1 includes the following steps: S11. Set the first temperature range as the complete austenitizing temperature range, and set the first time range as the complete austenitizing holding time range. S12. Set a second temperature range as the temperature range for controlled interrupted quenching treatment, wherein the quenching temperature range is between the martensitic transformation start temperature and the martensitic transformation end temperature of Cr12 material. S13. Set a third temperature range as the carbon partitioning temperature range, and the temperature value in the partitioning temperature range is greater than the temperature value in the quenching temperature range; set a second time range as the carbon partitioning time range. S14. Orthogonally combine the values ​​of each interval in S11-S13 to form a composite heat treatment process space containing multiple sets of process parameters; and form a multidimensional input feature matrix by combining the same set of process parameters in the composite heat treatment process space. By setting the temperature and time ranges for complete austenitization, controlled interrupted quenching, and carbon partitioning treatment respectively, and performing orthogonal combinations, a composite heat treatment process space covering multiple possibilities of microstructure evolution was constructed. This provides a comprehensive parameter basis for subsequently finding the optimal ratio of martensite to carbon-rich retained austenite, ensuring the data diversity and integrity of the input feature matrix.

[0008] Preferably, the specific steps of S2 include: S21. Cut the heat-treated cast ball sample radially and perform mechanical polishing and electrolytic polishing to prepare a test section that meets the surface roughness requirements; S22. Use a nanoindenter to perform matrix grid point testing on the test section and record the load-depth correlation curve for each indentation point. S23. Based on the load-depth correlation curve, the micro-area hardness data and elastic modulus data corresponding to each indentation point are calculated using the contact mechanics model. S24. Map and classify the micro-area hardness data and elastic modulus data into martensitic matrix phase data, carbon-rich residual austenite phase data and eutectic carbide phase data. S25. Extract the average hardness values ​​of the eutectic carbide phase data, martensite matrix phase data, and carbon-rich retained austenite phase data; based on the average hardness values, calculate the hardness gradient matching coefficient using the hardness gradient matching calculation formula. Micro-area hardness and elastic modulus data were extracted using a nanoindenter and mapped to the martensitic matrix phase, carbon-rich residual austenite phase, and eutectic carbide phase. By calculating the hardness gradient matching coefficient, the mechanical differences between different phases within the microstructure were transformed into calculable quantitative indicators, providing objective data support for evaluating the interfacial stress transfer state of materials under stress.

[0009] Preferably, the specific steps in S3 for determining whether the hardness gradient matching coefficient is within the compatibility threshold range include: The hardness gradient matching coefficient is compared with the upper limit of the compatibility threshold and the lower limit of the compatibility threshold; When the hardness gradient matching coefficient is greater than or equal to the lower limit of the compatibility threshold and less than or equal to the upper limit of the compatibility threshold, it is determined that the hardness gradient matching coefficient is within the compatibility threshold range, and the step of performing a simulated working condition impact wear test on the heat-treated cast ball sample is executed; otherwise, the step of removing the heat-treated cast ball sample and the corresponding input feature matrix is ​​executed. By setting a compatibility threshold range for pre-screening of samples, process parameters with unreasonable micromechanical matching can be eliminated in advance, avoiding time-consuming wear tests on invalid samples and improving the execution efficiency of the overall analysis and optimization process.

[0010] Preferably, the specific steps for recording the macroscopic volumetric wear rate in step S3 include: S311. Weigh the initial mass of the heat-treated cast ball sample before testing; S312. Place the heat-treated cast ball sample into a dynamic load abrasive wear tester and conduct continuous testing according to preset impact energy parameters, rotation speed parameters and abrasive parameters. S313. After the test, clean and dry the heat-treated cast ball sample, and weigh the mass of the heat-treated cast ball sample after wear after the test. S314. Based on the initial mass, the mass after wear, and the density, total sliding friction distance, and average normal load of the heat-treated cast ball sample, calculate the macroscopic volumetric wear rate using the volumetric wear rate calculation formula. Dynamic abrasive wear tests were conducted under set impact energy, rotational speed, and abrasive parameters. The macroscopic volumetric wear rate was calculated by combining the initial mass, post-wear mass, density, and friction test parameters of the sample. Standardized and repeatable macroscopic performance evaluation indicators were provided, which intuitively reflect the material's ability to resist wear under actual working conditions under different heat treatment processes.

[0011] Preferably, the specific steps for calculating the effective phase change hardening layer depth in step S3 include: S321. Cut a subsurface sample to a predetermined depth vertically downward along the wear surface of the heat-treated cast ball sample. S322. Use an electron backscatter diffractometer to scan the subsurface sample along the depth direction to obtain phase distribution scanning results including the volume fraction of residual austenite at different depths. S323. Based on the retained austenite volume fraction and depth data, plot a gradient curve of the retained austenite volume fraction as a function of depth. S324. On the gradient curve, find the vertical depth coordinates corresponding to when the residual austenite volume fraction recovers to the initial level of the unworn matrix, and obtain the effective phase transformation hardening layer depth. The residual austenite volume fraction gradient curve of the worn subsurface was obtained using electron backscatter diffraction, and the effective phase transformation hardening layer depth was calculated. The strain-induced phase transformation behavior of the material during the wear process was quantitatively characterized, which made up for the shortcomings of traditional static microstructure evaluation and provided a key indicator for evaluating the dynamic wear resistance of the material.

[0012] Preferably, the specific steps of S4 include: S41. The macroscopic volume wear rate, hardness gradient matching coefficient and effective phase transformation hardening layer depth corresponding to the same set of input feature matrices constitute an initial evaluation index sequence. S42. The initial evaluation index sequence is dimensionless to obtain a standardized evaluation index sequence. S43. Calculate the absolute difference between the standardized evaluation index sequence and the ideal reference sequence, and use the resolution coefficient to calculate the correlation coefficient of each index. S44. Calculate the weighting coefficients corresponding to the macroscopic volume wear rate, hardness gradient matching coefficient, and effective phase change hardening layer depth, and perform weighted summation based on the correlation coefficients of each index to obtain the gray comprehensive correlation model corresponding to the input feature matrix. By making the macroscopic volumetric wear rate, hardness gradient matching coefficient, and effective phase transformation hardening layer depth dimensionless, and using grey relational analysis to calculate the weighted sum of the correlation coefficient and weight coefficient, a comprehensive correlation model between multi-objective evaluation indicators and input feature matrix was established, realizing multi-dimensional objective evaluation of complex process parameters.

[0013] Preferably, the specific rules for calculating the macroscopic volumetric wear rate, hardness gradient matching coefficient, and weighting coefficient corresponding to the effective phase transformation hardening layer depth in step S44 are as follows: Based on the standardized evaluation index sequence, the information entropy value of each index is calculated; based on the information entropy value of each index, the first weight coefficient corresponding to the macroscopic volume wear rate, the second weight coefficient corresponding to the hardness gradient matching coefficient, and the third weight coefficient corresponding to the effective phase change hardening layer depth are calculated using the weight calculation formula. By employing the information entropy weighting method, weight coefficients are calculated based on the information entropy values ​​of various evaluation index data. This method relies on the degree of variation in the data itself to objectively assign weights, eliminating subjective biases caused by manually setting weights and improving the scientific rigor and accuracy of the correlation model.

[0014] Preferably, the specific steps of S5 include: S51. Substitute all the input feature matrices in the composite heat treatment process space into the gray comprehensive correlation model, and output the gray comprehensive correlation values ​​corresponding to all input feature matrices. S52. Compare all gray comprehensive correlation values ​​and extract the maximum value among the gray comprehensive correlation values; and extract the input feature matrix corresponding to the maximum value as the optimal heat treatment process adjustment scheme; input the optimal heat treatment process adjustment scheme into the control system of the automated heat treatment production line to control the batch production of the Cr12 casting balls; By calculating and extracting the input feature matrix with the highest gray comprehensive correlation value through model calculation, the theoretically optimal combination of process parameters was output. This was then applied to an automated heat treatment production line, realizing the transformation of optimization analysis results into actual industrial production and ensuring that the mass-produced Cr12 casting balls have the best wear resistance.

[0015] Preferably, after inputting the optimal heat treatment process adjustment scheme into the control system of the automated heat treatment production line, step S52 further includes a step of performing closed-loop temperature control on the batch production process: High-frequency thermocouples arranged in the quenching tank and the distribution tank of the heat treatment furnace are used to collect quenching oil temperature data and distribution salt bath temperature data in real time. The quenching oil temperature data and the salt bath temperature data are transmitted to the control system. The system determines whether the temperature fluctuations of the quenching oil temperature data and the salt bath temperature data exceed the temperature fluctuation threshold. If so, the control system automatically adjusts the heating tube power or the cooling heat exchanger flow rate through a proportional-integral-derivative adjustment algorithm to maintain the actual temperature consistent with the temperature parameters in the optimal heat treatment process adjustment scheme. Otherwise, the current heating tube power or cooling heat exchanger flow rate remains unchanged. High-frequency thermocouples are used to collect temperature data in real time, and proportional-integral-derivative (PID) control algorithms are used to control the heating or cooling units. This eliminates temperature fluctuations caused by changes in furnace loading in industrial production and ensures that the actual production process parameters are consistent with the optimal parameters output by the model.

[0016] (III) Beneficial Effects The present invention has the following beneficial effects: This invention provides a parameter basis for regulating the ratio of martensite to carbon-rich residual austenite in Cr12 casting balls by setting a composite heat treatment process space that includes austenitization, controlled interrupted quenching, and carbon partitioning. By combining nanoindentation testing to extract micro-area hardness and elastic modulus and calculating the hardness gradient matching coefficient, the mechanical synergistic deformation capability within the microstructure is transformed into a quantifiable numerical index. By using a set compatibility threshold range, unreasonable parameter combinations with mechanical mismatch are eliminated, thus improving the efficiency of optimization analysis.

[0017] In the performance evaluation stage, this invention combines dynamic load abrasive wear testing with electron backscatter diffraction scanning technology. It not only assesses the overall wear resistance of the material through macroscopic volumetric wear rate, but also quantitatively characterizes the dynamic phase transformation self-hardening characteristics of the material under impact conditions by calculating the effective phase transformation hardening layer depth. This evaluation system, which combines microscopic static mechanical properties with macroscopic dynamic phase transformation characteristics, comprehensively reflects the material's real service performance under complex working conditions.

[0018] This invention utilizes grey relational analysis and information entropy weighting to establish a comprehensive correlation model between a multidimensional evaluation index sequence and an input feature matrix; it achieves objective weighting and quantitative optimization of multi-objective parameters, outputting the optimal heat treatment process parameters; and, in conjunction with a temperature closed-loop control system based on a PID algorithm, it is applied to mass production to ensure the accurate execution of process parameters and improve the consistency of finished Cr12 casting ball quality.

[0019] Of course, any product implementing this invention does not necessarily need to achieve all of the advantages described above at the same time. Attached Figure Description

[0020] To more clearly illustrate the technical solutions of the embodiments of the invention, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the invention. For those skilled in the art, the drawings can be obtained from these drawings without creative effort.

[0021] Figure 1 This is a schematic diagram of the process flow of the present invention, which is a method for optimizing the wear resistance of Cr12 cast balls based on the adjustment of the heat treatment process. Figure 2 This is a schematic diagram of the spatial construction process of the composite heat treatment process in this invention; Figure 3 This is a schematic diagram of the temperature-time process curve for the three-stage composite heat treatment of Cr12 cast balls in this invention. Figure 4 This is a schematic diagram of the information entropy weight-grey comprehensive correlation evaluation model in this invention. Detailed Implementation

[0022] The technical solutions of the embodiments of the invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the invention, and not all embodiments. Based on the embodiments of the invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the invention.

[0023] This embodiment provides a detailed description of a mass production line for Cr12 cast iron balls manufactured by a mining wear-resistant materials company. Cr12 high-carbon, high-chromium alloy cast iron has a carbon mass fraction of approximately 2.0-2.3% and a chromium mass fraction of approximately 11.5-13.0%. Due to the presence of a large amount of high-hardness M7C3 type eutectic carbides, it plays a core role in ore crushing and grinding in large semi-autogenous mills and ball mills. The cast balls not only withstand intense abrasive wear but also bear the enormous impact load from drops of tens of meters. Traditional processes often employ high-temperature quenching combined with low-temperature tempering during heat treatment, relying solely on the hardness of the martensitic matrix and static carbides to resist wear. This hard but not tough microstructure is highly susceptible to microscopic cleavage fracture under strong impact conditions, leading to the peeling of carbides along the phase interface, macroscopically manifested as a persistently high breakage rate.

[0024] To resolve the above issues, please refer to [link / reference]. Figure 1 This invention discloses a method for optimizing the wear resistance of Cr12 cast balls based on adjustments to the heat treatment process, comprising the following steps: S1. Obtain a Cr12 cast ball sample to be optimized, and set a composite heat treatment process space including full austenitization, controlled interrupted quenching, and carbon partitioning; extract the process parameters in the composite heat treatment process space as the input feature matrix; perform heat treatment on the Cr12 cast ball sample according to the input feature matrix to obtain a heat-treated cast ball sample. Please see Figure 2 S1 includes the following steps: S11. Set the first temperature range as the complete austenitizing temperature range, and set the first time range as the complete austenitizing holding time range. Specifically, in Example S11, a Cr12 as-cast blank ball with qualified chemical composition was obtained from the raw material library as a sample; the complete austenitizing temperature range was set to 1000℃ to 1080℃, and the complete austenitizing holding time range was set to 1.5 hours to 2.5 hours; at the crystallographic level, the Cr12 as-cast microstructure contains coarse network eutectic carbides and dispersed secondary carbides; when heated to this temperature range, the secondary carbides, mainly of the Cr23C6 type, dissolve and solidify into the face-centered cubic (FCC) austenitic matrix, giving the matrix sufficient carbon and chromium concentrations; if the austenitizing temperature is below 1000℃, the alloying elements will not dissolve sufficiently, resulting in insufficient subsequent martensite hardness; if it is above 1080℃, it will cause the austenitic grains to grow rapidly, seriously damaging the material's toughness; therefore, the set range ensures that the austenitizing process achieves a balance between solid solution strengthening and grain refinement. S12. Set a second temperature range as the temperature range for controlled interrupted quenching treatment, wherein the quenching temperature range is between the martensitic transformation start temperature and the martensitic transformation end temperature of Cr12 material. Specifically, in Example S12, the cooling curve of this batch of Cr12 material was measured using a high-precision differential dilatometer. Based on the inflection point of the expansion curve, the martensitic transformation start temperature Ms was determined to be approximately 285°C, and the martensitic transformation end temperature Mf was approximately 90°C. Accordingly, the temperature range for controlled interrupted quenching was set to 180°C to 250°C. During heat treatment, the high-temperature austenitic cast balls were rapidly quenched into a constant-temperature nitrate bath at the set temperature. The controlled interrupted quenching is a controlled step in the quench-partition (QP) process, which refers to stopping the cooling of the austenitized cast balls when the temperature is between the martensitic transformation start temperature Ms and the martensitic transformation end temperature Mf, so as to retain some untransformed austenite for subsequent carbon partitioning. According to the Koistinen-Marburger phase transformation kinetic equation, when the quenching temperature is between Ms and Mf, austenite will undergo incomplete diffusionless shearing and transform into body-centered cubic (BCT) primary martensite. By controlling the quenching temperature, the volume fraction of primary martensite can be precisely controlled, with a target range of 60%-70%. The remaining 30%-40% is retained as untransformed austenite, providing acceptor phases for subsequent carbon partitioning. S13. Set a third temperature range as the carbon partitioning temperature range, and ensure that the temperature value in the partitioning temperature range is greater than the temperature value in the quenching temperature range; set a second time range as the carbon partitioning time range. Specifically, in Example S13, the carbon fractionation temperature range was set to 260°C to 350°C, and the fractionation time range was set to 30 minutes to 120 minutes. During the fractionation stage, the cast balls were transferred to a second nitrate bath at a slightly higher temperature. Under the action of the thermodynamic driving force, i.e., the chemical potential gradient, the carbon atoms in the primary martensite that were in a supersaturated state diffused through the interstitial diffusion mechanism and entered the untransformed austenite through the phase interface. Since the fractionation temperature avoided the sensitive area of ​​large-scale carbide precipitation, carbon atoms were enriched in the austenite. The carbon-enriched residual austenite had significantly improved room temperature stability and no longer underwent secondary martensitic phase transformation during the subsequent cooling to room temperature. Thus, a hard martensitic-bonded and tough carbon-enriched residual austenite multiphase matrix was constructed inside the material. S14. The temperature values ​​within the complete austenitizing temperature range, the time values ​​within the complete austenitizing holding time range, the temperature values ​​within the quenching temperature range, the temperature values ​​within the partitioning temperature range, and the time values ​​within the partitioning time range are orthogonally combined to form the composite heat treatment process space containing multiple sets of process parameters; the same set of process parameters in the composite heat treatment process space is used to form a multidimensional input feature matrix. Specifically, in embodiment S14, the above five parameters are orthogonally combined experimentally designed according to preset step sizes, such as a temperature step size of 10°C and a time step size of 30 minutes, to generate different combinations of process parameters; each set of parameter combinations constitutes a five-dimensional input feature matrix; for example, matrix No. 1 contains [1020°C, 1.5h, 200°C, 280°C, 60min]; the multi-purpose box-type heat treatment furnace is controlled to automatically heat treat each group of Cr12 cast ball samples according to these matrix parameters, resulting in a numbered heat-treated cast ball sample library; The above embodiments, by clearly defining the range of each temperature and time interval and constructing a composite heat treatment process space using an orthogonal combination method, cover the entire process parameters of austenitization, controlled interrupted quenching, and carbon partitioning; this provides systematic data input for studying the influence of different parameter combinations on the microstructure and macroscopic properties of Cr12 cast balls, ensuring the comprehensiveness of subsequent optimization analysis; S2. Perform micro-mechanical property mapping test on the heat-treated cast ball sample to obtain micro-area hardness data and elastic modulus data of the heat-treated cast ball sample; calculate the hardness gradient matching coefficient based on the micro-area hardness data and the elastic modulus data; S2 includes the following steps: S21. Cut the heat-treated cast ball sample radially and perform mechanical polishing and electrolytic polishing to prepare a test section that meets the preset surface roughness requirements; Specifically, in Example S21, a slow diamond wire cutter was used to radially cut the heat-treated cast ball sample to avoid introducing cutting thermal stress. Subsequently, the sample was mechanically polished step-by-step using silicon carbide sandpaper ranging from 400 to 2000 mesh, and then mechanically polished on a velvet polishing cloth using a silica suspension with a particle size of 0.05 micrometers. To completely remove the residual stress layer generated by mechanical polishing, an electrolytic polishing was performed using a 1:9 volume ratio of perchloric acid to glacial acetic acid mixed solution, with an electrolytic voltage set at 20V and a time of 15 seconds. Finally, a test section with a surface roughness Ra of less than 10 nanometers was prepared to meet the surface flatness requirements of nanoindentation testing. S22. Use a nanoindenter to perform matrix grid point testing on the test section and record the load-depth correlation curve for each indentation point. Specifically, in Example S22, a nanoindenter equipped with a Berkovich pyramidal diamond indenter was used; a 100×100 matrix grid was set on the test section, with a grid spacing of 2 micrometers, and a total of 10,000 micro-area indentation tests were performed; the instrument was set to a maximum loading force of 10 millinewtons (mN), and the loading and unloading rates were both set to 0.5 mN / s, and the maximum load was maintained for 5 seconds to eliminate creep effects; the indenter displacement and sensor force were acquired at high frequency, and a complete load-depth correlation curve for each indentation point was recorded; S23. Based on the load-depth correlation curve, the micro-area hardness data and elastic modulus data corresponding to each indentation point are calculated using a contact mechanics model. Specifically, in embodiment S23, the classic Oliver-Pharr contact mechanics model is used to process the load-depth correlation curve; the contact stiffness S, i.e., the slope of the unloading curve in the initial stage, is fitted from the first third of the unloading curve. dP / dh m Unit: mN / nm; Calculate the true contact depth between the indenter and the specimen. h c The unit is nm; the formula is: ,in h max The maximum indentation depth is the maximum displacement depth of the indenter, expressed in nm. P max Maximum load, in mN; ε A constant related to the geometry of the indenter, the Berkovich indenter is taken as 0.75; the constant ε Based on the ISO 14577 standard specification published by the International Organization for Standardization, the geometry of the Berkovich pyramidal diamond indenter is set. Further calculate the projected contact area between the indenter and the material. A , A for h c polynomial functions of multiple degrees The constants C1 to C5 were obtained by fitting the standard fused silica sample with a series of calibrated indentation experiments under known loads using the least squares method; the micro-area hardness data were then calculated. ; Calculate the reduced elastic modulus based on the unloading curve. ;in β is the indenter shape correction factor in the Oliver-Pharr nanoindentation method, used to convert a non-axisymmetric pyramidal indenter into an axisymmetric conical indenter, to fit the elastic modulus calculation formula of classical Hertzian contact mechanics. According to the ISO 14577 standard published by the International Organization for Standardization, the Berkovich triangular pyramidal diamond indenter is set to 1.034; using the formula... Inversely estimating the elastic modulus of the sample material E ,in γ The Poisson's ratio of the sample material was obtained by measuring the ultrasonic velocity. E i and γ iThe values ​​are the elastic modulus and Poisson's ratio of the diamond indenter, which are 1141 GPa and 0.07, respectively. S24. Combining scanning electron microscope images, the micro-area hardness data and the elastic modulus data are mapped and classified into martensitic matrix phase data, carbon-rich residual austenite phase data, and eutectic carbide phase data. Specifically, in Example S24, micron-sized cross marks were made at the four corners of the nanoindentation test area using a focused ion beam (FIB); the sample was transferred to a field emission scanning electron microscope (SEM), and the cross marks were used for high-precision alignment of the coordinate system; combining the SEM morphology contrast with the elemental distribution of the energy dispersive spectroscopy (EDS), these 10,000 indentation points were mapped to their respective microphases, and the data of the martensitic matrix phase, carbon-rich residual austenite phase, and eutectic carbide phase were obtained. S25. Extract the average hardness values ​​of the eutectic carbide phase data, the martensitic matrix phase data, and the carbon-rich retained austenite phase data respectively; based on the average hardness values ​​of the eutectic carbide phase data, the martensitic matrix phase data, and the carbon-rich retained austenite phase data, calculate the hardness gradient matching coefficient using the hardness gradient matching calculation formula. Specifically, in Example S25, the classified data are statistically averaged to extract the average hardness value of the eutectic carbide phase data. H c (Typically between 12-15 GPa), average hardness value of martensitic matrix phase data H m and the average hardness value of carbon-rich residual austenite phase data H a The H c Typically between 12-15 GPa, the H m Typically between 7-9 GPa, the H a Typically between 4 and 5 GPa; Hardness gradient matching coefficient H match The calculation formula is The above formula quantifies the micromechanical compatibility within the material. H m - H a It characterizes the deformation coordination ability between martensite and austenite within the matrix; H c - H m It characterizes the stress transfer gradient between the extremely hard carbide and the matrix;H match The value reflects the smoothness of stress transmission between different phase interfaces when the microstructure is subjected to external impact loads; The above embodiments utilize nanoindentation technology combined with contact mechanics models to objectively calculate the micro-area hardness and elastic modulus, and correlate them with specific microstructures; by calculating the hardness gradient matching coefficient, the mechanical gradient between martensite, austenite and carbides is quantified, providing accurate numerical basis for evaluating the micro-coordinated deformation capability of materials. S3. Determine whether the hardness gradient matching coefficient is within the compatibility threshold range; if so, perform a simulated working condition impact wear test on the heat-treated cast ball sample, record the macroscopic volume wear rate, and perform electron backscatter diffraction scanning on the wear subsurface layer to calculate the effective phase transformation hardening layer depth; otherwise, discard the heat-treated cast ball sample and the corresponding input feature matrix. S3 includes the following steps: The compatibility threshold range is based on the stress intensity factor and crack tip plastic zone theory in fracture mechanics. Specifically, a micromechanical model including the matrix and carbides is established using finite element analysis software. A boundary load equivalent to 3.5 Joules of impact energy is applied, and the critical stress ratio range at the phase interface where microcrack initiation does not occur is extracted. This stress ratio range is mapped to the hardness gradient matching coefficient, and the lower limit and upper limit of the compatibility threshold are derived. For example, the lower limit of the compatibility threshold is 0.45, and the upper limit of the compatibility threshold is 0.75, which constitutes the preset compatibility threshold range [0.45, 0.75]. when H match When the sample falls within the range of [0.45, 0.75], it indicates that the hardness gradient transition between the three microphases is reasonable. Under impact load, the soft austenite phase can undergo moderate plastic deformation to absorb impact energy, the martensite can provide sufficient support force, and the carbides are not prone to interfacial debonding and cracking. Therefore, this sample is allowed to enter the time-consuming wear test stage. when H match When the value is less than 0.45, it means the denominator is too large or the numerator is too small, the matrix is ​​generally soft, and the carbides are easily pulled out as a whole under abrasive cutting; when H match When the value is greater than 0.75, it means that the residual austenite content is very low or not sufficiently carbon-rich and softened, and the matrix exhibits strong brittleness and cannot buffer impact energy; such process parameters are determined to have no optimization value and are directly removed from the database, which greatly saves the cost of subsequent experiments. Based on this, the following tests are performed on the qualified samples: S311. Using a high-precision electronic balance with an accuracy of 0.001 grams, weigh the initial mass M1 of the heat-treated cast ball sample, in g. S312. Place the heat-treated cast ball sample into a dynamic load abrasive wear tester and conduct continuous testing according to preset impact energy parameters, rotation speed parameters and abrasive parameters. Specifically, in embodiment S312, the dynamic load abrasive wear testing machine is equipped with a cam lifting impact mechanism and a spindle rotation mechanism; the single impact energy parameter corresponding to the cam drop is set to 3.5 Joules to simulate the impact of steel balls falling in a ball mill; the spindle speed parameter is set to 200 rpm; and the abrasive parameters are selected as quartz sand with a Mohs hardness of 7 and a particle size of 10-15 mm; the testing machine runs continuously for 100 hours to simulate real harsh working conditions; S313. Place the tested sample in anhydrous ethanol for ultrasonic cleaning for 20 minutes to remove the quartz sand particles embedded on the surface. After drying, weigh the worn mass M2 in g. S314. Obtain the density, total sliding friction distance, and average normal load of the heat-treated cast ball sample; based on the initial mass, the mass after wear, the density, the total sliding friction distance, and the average normal load, calculate the macroscopic volumetric wear rate using the volumetric wear rate calculation formula; Specifically, in Example S314, the density of the Cr12 material was obtained. ρ Take 7.65 × 10 -3 g / mm 3 The total sliding friction distance recorded by the spindle encoder of the testing machine L The unit is meters (m); and the average normal load collected by the force sensor. F Unit: N; calculated using the volumetric wear rate formula. Calculate macroscopic volumetric wear rate W This refers to the volume loss of material per unit of frictional work consumed. The smaller the value, the better the macroscopic wear resistance. The unit is mm. 3 / (N·m); The above embodiments screened samples by setting an objective compatibility threshold, eliminating process parameters with extremely poor mechanical matching; and conducted tests and calculated the macroscopic volumetric wear rate under uniform dynamic load abrasive wear tester parameters, obtaining a quantitative index reflecting the material's ability to resist wear under simulated real working conditions. Furthermore, a deeper microscopic exploration of the wear mechanism was conducted to extract dynamic phase transition characteristics: S321. Cut a subsurface sample to a predetermined depth vertically downward along the wear surface of the heat-treated cast ball sample. Specifically, in Example S321, a subsurface sample with a depth of 500 micrometers was cut vertically downward along the worn surface using a precision slow-speed cutter; in order to avoid artificial strain-induced phase transformation of the residual austenite caused by mechanical grinding, the sample was only subjected to very slight vibration polishing treatment. S322. The subsurface sample is scanned along the depth direction using an electron backscatter diffractometer to obtain the phase distribution scanning results; the phase distribution scanning results include the volume fraction of retained austenite at different depths. Specifically, in Example S322, the sample was placed at a 70-degree angle in a field emission scanning electron microscope and scanned using an electron backscatter diffractometer (EBSD). The scanning step size was set to 0.1 micrometers. The austenite phase and martensite phase were distinguished by calibrating the Kikuchi pattern of the face-centered cubic (FCC) zone axis and the body-centered cubic (BCT) zone axis. Only data points with a confidence index (CI) greater than 0.1 were accepted, thereby obtaining the residual austenite volume fraction at different depth levels. S323. Based on the retained austenite volume fraction and depth data, plot the gradient curve of retained austenite volume fraction as a function of depth. Specifically, in embodiment S323, at the outermost layer of the wear contact, due to the extremely high impact crushing stress, dislocation slip and stacking fault accumulation inside the austenite lattice are activated, inducing diffusionless martensitic shear, i.e., the TRIP effect; therefore, almost all of the residual austenite at the outermost layer is transformed into high-hardness martensite with an extremely low volume fraction. As the depth extends inward, the impact stress decreases exponentially, the phase transformation driving force decreases, and the volume fraction of residual austenite gradually increases, forming a characteristic gradient curve. S324. On the gradient curve, find the vertical depth coordinate corresponding to when the residual austenite volume fraction recovers to the initial level of the unworn matrix; define the vertical depth coordinate as the effective phase transformation hardening layer depth. Specifically, in Example S324, the initial residual austenite content measured in the unworn area in S2 is extracted as a baseline; the vertical depth coordinate corresponding to the intersection of the curve and the baseline is found on the gradient curve, and this depth is the effective phase transformation hardening layer depth Dtrip; Dtrip quantifies the thickness of the material that can spontaneously generate deformation-strengthened armor when actually subjected to stress. The larger the value, the stronger the dynamic self-hardening ability of the material, which not only makes the surface wear-resistant, but also effectively prevents microcracks from propagating into the center; The embodiment described above uses electron backscatter diffraction technology to extract the residual austenite volume fraction of the worn subsurface and plots a gradient curve; by finding the depth coordinates to restore the initial level, the effective phase transformation hardening layer depth is obtained; this objectively reflects the dynamic phase transformation strengthening ability of the material during the stress process and improves the performance evaluation dimensions. S4. Construct an evaluation index sequence from the macroscopic volumetric wear rate, the hardness gradient matching coefficient, and the effective phase transformation hardening layer depth; and establish a grey comprehensive correlation model between the input feature matrix and the evaluation index sequence using grey relational analysis. Please see Figure 3 S4 includes the following steps: S41. The macroscopic volume wear rate, the hardness gradient matching coefficient and the effective phase change hardening layer depth corresponding to the same set of input feature matrices constitute an initial evaluation index sequence. Specifically, in embodiment S41, it is assumed that the first i The test results corresponding to the input feature matrix are the macroscopic volumetric wear rate. W i Hardness gradient matching coefficient H match,i Effective phase transformation hardening layer depth D trip,i These three values ​​constitute the first i The initial evaluation index sequence for the group; S42. The initial evaluation index sequence is dimensionless to obtain a standardized evaluation index sequence. Specifically, in embodiment S42, since the three indicators have different dimensions and different optimization directions, standardization is necessary; for the macroscopic volumetric wear rate... W i The smaller the value, the better; a minimization formula is used for processing. For the effective phase transformation hardening layer depth... D trip,i The larger the better, using a maximization formula; for the hardness gradient matching coefficient H match,i The closer to the ideal median value, the better. The median value formula is adopted, and the optimal target value is set to 0.60. After processing, all indicators are converted into dimensionless values ​​in the interval [0,1], forming a standardized evaluation indicator sequence. S43. Calculate the absolute difference between the standardized evaluation index sequence and the preset ideal reference sequence, and use the resolution coefficient to calculate the correlation coefficient of each index. Specifically, in embodiment S43, an ideal reference sequence in which all indicators reach the optimal state 1 is constructed; the absolute difference Δ between each standardized indicator and 1 is calculated. ij Resolution coefficient ψ Based on grey system theory, to ensure the correlation coefficient has good discriminative power during calculation and to reduce the interference of extreme value data, a standard constant value of 0.5, commonly used in the industry, is adopted; the correlation coefficient calculation formula is then used. The correlation coefficients of each indicator were calculated; among them, , ; ξ ij Indicates the first i Group sample, first j The correlation coefficient of the indicators; x 0j The first part represents the ideal reference sequence. jThe indicator values ​​are all 1 here; x ij Indicates the first i Group sample, first j The standardized value of the indicator; Δ ij Indicates the absolute difference; Δ min Δ represents the minimum absolute difference among all samples and all indicators, i.e., the minimum difference between the two extremes; max This represents the maximum value among all absolute differences of all samples and all indicators, i.e., the maximum difference between the two extremes; S44. Calculate the weighting coefficients corresponding to the macroscopic volume wear rate, hardness gradient matching coefficient, and effective phase change hardening layer depth, and perform weighted summation based on the correlation coefficients of each index to obtain the gray comprehensive correlation model corresponding to the input feature matrix. Specifically, in embodiment S44, to avoid subjective bias caused by manually assigning weights, the information entropy weighting method is used; the calculation of the first... j The first item under the indicator i The feature proportion of each sample ; Calculate the information entropy value of each indicator ,in , n The total number of samples; if the data for a certain indicator varies greatly, its information entropy is... E j The smaller the value, the richer the information provided by the indicator in the evaluation system; this is indicated by the weighting formula. The first weight coefficient, second weight coefficient, and third weight coefficient are calculated; for example, the first weight coefficient is calculated to be 0.42, the second weight coefficient to be 0.23, and the third weight coefficient to be 0.35; the correlation coefficient is then... ξ ij With weight W j The weighted summation yields the final output value Gamma of the grey comprehensive correlation model. The embodiment described above performs dimensionless processing on macroscopic and microscopic, static and dynamic evaluation indicators, and uses the information entropy weighting method to objectively assign weights to each indicator; combined with grey relational analysis to calculate the comprehensive correlation degree, a mathematical evaluation model that does not rely on human experience is established, realizing a unified quantitative evaluation of multi-dimensional performance indicators. S5. Calculate the gray comprehensive correlation degree value corresponding to each input feature matrix in the composite heat treatment process space using the gray comprehensive correlation degree model; output the input feature matrix corresponding to the maximum value among the gray comprehensive correlation degree values ​​as the optimal heat treatment process flow adjustment scheme; and mass-produce Cr12 casting balls according to the optimal heat treatment process flow adjustment scheme. S5 includes the following steps: S51. Substitute all the input feature matrices within the composite heat treatment process space into the gray comprehensive correlation model; use the gray comprehensive correlation model to output the gray comprehensive correlation values ​​corresponding to all the input feature matrices; S52. Compare all the gray comprehensive correlation values ​​and extract the maximum value among the gray comprehensive correlation values; and extract the set of input feature matrices corresponding to the maximum value; The extracted set of input feature matrices is used as the optimal heat treatment process adjustment scheme, and the optimal heat treatment process adjustment scheme is input into the control system of the automated heat treatment production line to control the batch production of the Cr12 casting balls. Specifically, please refer to Figure 4 In Example S52, the Gamma values ​​of all qualified samples are iterated. It is assumed that the maximum Gamma value is 0.912 according to the model calculation. The corresponding set of input feature matrices is: complete austenitizing temperature 1030℃, holding time 2.0 hours, quenching temperature 205℃, partitioning temperature 320℃, and partitioning time 45 minutes. This set of parameters takes into account both microscopic compatibility and dynamic wear resistance. The optimal parameters are sent to the workshop PLC via industrial Ethernet; high-frequency thermocouples arranged in the quenching tank and distribution tank of the heat treatment furnace are used to collect quenching oil temperature data and distribution salt bath temperature data in real time; the quenching oil temperature data and the distribution salt bath temperature data are transmitted to the control system; it is determined whether the temperature fluctuation of the quenching oil temperature data and the distribution salt bath temperature data exceeds the preset temperature fluctuation threshold; the temperature fluctuation threshold is calculated by step response testing of the thermal inertia of the heat treatment furnace under no-load and full-load conditions, combined with the sensitivity analysis of the phase transformation of Cr12 material to temperature fluctuation, and the maximum allowable temperature deviation range is ±2℃. If the preset temperature fluctuation threshold is exceeded, the control system automatically adjusts the heating tube power or cooling heat exchanger flow rate through a proportional-integral-derivative (PID) adjustment algorithm to maintain the actual temperature consistent with the temperature parameters set in the optimal heat treatment process adjustment scheme; if the preset temperature fluctuation threshold is not exceeded, the current heating tube power or cooling heat exchanger flow rate remains unchanged. The formula for the PID control algorithm is as follows: ;in, u ( t This indicates the controller output signal, such as the power of the heating element or the flow rate regulation of the cooling heat exchanger; e ( t This indicates the temperature deviation, which is the difference between the set temperature and the actual temperature. K p This represents the proportional gain, which provides an immediate response to the current deviation. Ki It represents the integral gain, which eliminates steady-state error and adjusts for accumulated deviations. K d This represents the differential gain, which is used to suppress overshoot in advance based on the rate of change of the deviation. t The time variable is represented; the proportional gain, integral gain, and derivative gain are obtained by applying an open-loop step signal to the actual heat treatment furnace temperature control system, recording the delay time and maximum heating rate of the temperature response curve, and then substituting them into the Ziegler-Nichols empirical formula. When a large number of cold-cast balls fall into the quenching tank, causing a sudden drop in local oil temperature, the proportional term... K p Rapid response increases heating power; integral term K i Eliminate long-term static errors to ensure a final temperature precisely matches 205℃; Differential term K d The suppression effect is applied in advance according to the rate of temperature drop to prevent temperature overshoot; through PID closed-loop control, the instability of heat treatment quality caused by the fluctuation of furnace loading in large-scale industrial production is eliminated. The above embodiments directly output the optimal process parameters using the established grey comprehensive correlation model and apply them to the control system; temperature closed-loop control is performed through objectively tuned PID algorithm, eliminating the influence of external interference on temperature and ensuring the accurate execution of optimized parameters in actual mass production; For example, taking Cr12 as-cast blank balls from the same batch as an example, after being treated with the traditional 1050℃ quenching combined with 250℃ tempering process, the martensite in its microstructure is extremely hard but lacks toughness, and the hardness gradient matching coefficient is... H match The value was 0.32; no significant effective phase change hardening layer depth was detected in the EBSD scan. D trip Approaching 0, lacking dynamic self-hardening ability; macroscopic volumetric wear rate during operation in a ball mill. W Reaching 2.9×10 -4 mm 3 / (N·m), and the actual ball breakage rate on site reached 4.8%; Using the optimal process output by this invention, after austenitizing at 1030℃ for 2.0 h, controlled interrupted quenching at 205℃, and fractionation treatment at 320℃ for 45 min, its... H match The value was optimized to 0.62, resulting in a smooth transition in micromechanics; more importantly, the effective phase transformation hardening layer depth of the wear subsurface was improved. D tripThe wear rate reached 135 micrometers; during the wear process, the residual austenite in the subsurface layer underwent a strain-induced phase transformation, forming a self-hardening layer that could effectively buffer impact loads; ultimately, the measured macroscopic volumetric wear rate decreased to 1.05 × 10⁻⁶. -4 mm 3 / (N·m), the wear resistance life is increased by nearly 1.8 times, and the on-site ball breakage rate is reduced to below 0.15%.

[0025] This invention starts with microstructure regulation, altering the material phase composition through a composite heat treatment process space. In terms of evaluation, it abandons single macroscopic indicators, introducing nanoindentation technology to quantify the mechanical matching degree between microphases, and utilizing electron backscattering diffraction technology to quantify the dynamic phase transition depth during wear. For data processing, it employs information entropy weighting and grey relational analysis to establish a subjectively unbiased mathematical model, achieving optimization of process parameters. PID closed-loop control translates theoretical parameters into industrial production lines. This invention provides a complete analytical method encompassing parameter setting, micromechanical evaluation, dynamic performance quantification, mathematical modeling optimization, and industrial closed-loop control, eliminating the blindness of traditional trial-and-error approaches and achieving quantitative optimization and stable production of the comprehensive wear resistance of Cr12 cast balls.

[0026] In the description of this specification, references to terms such as "an embodiment," "example," "specific example," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.

[0027] The preferred embodiments of the invention disclosed above are merely illustrative of the invention. These preferred embodiments do not exhaustively describe all details, nor do they limit the invention to the specific implementations described. Clearly, many modifications and variations can be made based on the content of this specification. This specification selects and specifically describes these embodiments to better explain the principles and practical applications of the invention, thereby enabling those skilled in the art to better understand and utilize the invention.

Claims

1. A method for optimizing the wear resistance of Cr12 cast balls based on adjustments to the heat treatment process, characterized by the following steps: S1. Obtain Cr12 cast ball samples to be optimized, and set a composite heat treatment process space including full austenitization, controlled interrupted quenching, and carbon partitioning. The process parameters in the composite heat treatment process space are extracted as the input feature matrix, and the Cr12 cast ball samples are heat-treated to obtain heat-treated cast ball samples. S2. Perform microscopic mechanical property mapping test on the heat-treated cast ball sample to obtain micro-area hardness data and elastic modulus data, and calculate the hardness gradient matching coefficient. S3. Determine whether the hardness gradient matching coefficient is within the compatibility threshold range; if so, perform a simulated working condition impact wear test on the heat-treated cast ball sample, record the macroscopic volume wear rate, and perform electron backscatter diffraction scanning on the wear subsurface layer to calculate the effective phase transformation hardening layer depth; otherwise, discard the heat-treated cast ball sample and the corresponding input feature matrix. S4. Construct the macroscopic volumetric wear rate, hardness gradient matching coefficient, and effective phase transformation hardening layer depth into an evaluation index sequence; use grey relational analysis to establish a grey comprehensive correlation model between the input feature matrix and the evaluation index sequence; S5. Calculate the grey comprehensive correlation degree of each input feature matrix in the composite heat treatment process space using the grey comprehensive correlation degree model. The input feature matrix corresponding to the maximum value in the gray comprehensive correlation degree is used as the optimal heat treatment process adjustment scheme for the mass production of Cr12 casting balls.

2. The Cr12 cast ball wear resistance performance optimization analysis method based on heat treatment process adjustment according to claim 1, characterized in that, S1 includes the following steps: S11. Set the first temperature range as the complete austenitizing temperature range, and set the first time range as the complete austenitizing holding time range. S12. Set a second temperature range as the temperature range for controlled interrupted quenching treatment, wherein the quenching temperature range is between the martensitic transformation start temperature and the martensitic transformation end temperature of Cr12 material. S13. Set a third temperature range as the carbon partitioning temperature range, and the temperature value in the partitioning temperature range is greater than the temperature value in the quenching temperature range; set a second time range as the carbon partitioning time range. S14. The values ​​of each interval in S11-S13 are orthogonally combined to form a composite heat treatment process space containing multiple sets of process parameters; the same set of process parameters in the composite heat treatment process space are used to form a multidimensional input feature matrix.

3. The Cr12 cast ball wear resistance performance optimization analysis method based on heat treatment process adjustment according to claim 1, characterized in that, The specific steps of S2 include: S21. Cut the heat-treated cast ball sample radially and perform mechanical polishing and electrolytic polishing to prepare a test section that meets the surface roughness requirements; S22. Use a nanoindenter to perform matrix grid point testing on the test section and record the load-depth correlation curve for each indentation point. S23. Based on the load-depth correlation curve, the micro-area hardness data and elastic modulus data corresponding to each indentation point are calculated using the contact mechanics model. S24. Map and classify the micro-area hardness data and elastic modulus data into martensitic matrix phase data, carbon-rich residual austenite phase data and eutectic carbide phase data. S25. Extract the average hardness values ​​of the eutectic carbide phase data, martensite matrix phase data, and carbon-rich residual austenite phase data; based on the average hardness values, calculate the hardness gradient matching coefficient using the hardness gradient matching calculation formula.

4. The Cr12 cast ball wear resistance performance optimization analysis method based on heat treatment process adjustment according to claim 3, characterized in that, The specific steps in S3 for determining whether the hardness gradient matching coefficient is within the compatibility threshold range include: The hardness gradient matching coefficient is compared with the upper limit of the compatibility threshold and the lower limit of the compatibility threshold; When the hardness gradient matching coefficient is greater than or equal to the lower limit of the compatibility threshold and less than or equal to the upper limit of the compatibility threshold, it is determined that the hardness gradient matching coefficient is within the compatibility threshold range, and the step of performing a simulated working condition impact wear test on the heat-treated cast ball sample is executed; otherwise, the step of removing the heat-treated cast ball sample and the corresponding input feature matrix is ​​executed.

5. The Cr12 cast ball wear resistance performance optimization analysis method based on heat treatment process adjustment according to claim 1, characterized in that, The specific steps for recording the macroscopic volumetric wear rate in S3 include: S311. Weigh the initial mass of the heat-treated cast ball sample before testing; S312. Place the heat-treated cast ball sample into a dynamic load abrasive wear tester and conduct continuous testing according to preset impact energy parameters, rotation speed parameters and abrasive parameters. S313. After the test, clean and dry the heat-treated cast ball sample, and weigh the mass of the heat-treated cast ball sample after wear after the test. S314. Based on the initial mass, the mass after wear, and the density, total sliding friction distance, and average normal load of the heat-treated cast ball sample, calculate the macroscopic volumetric wear rate using the volumetric wear rate calculation formula.

6. The method for optimizing the wear resistance of Cr12 cast balls based on heat treatment process adjustment according to claim 1, characterized in that, The specific steps for calculating the effective phase transformation hardening layer depth in S3 include: S321. Cut a subsurface sample to a predetermined depth vertically downward along the wear surface of the heat-treated cast ball sample. S322. Use an electron backscatter diffractometer to scan the subsurface sample along the depth direction to obtain phase distribution scanning results including the volume fraction of residual austenite at different depths. S323. Based on the retained austenite volume fraction and depth data, plot a gradient curve of the retained austenite volume fraction as a function of depth. S324. On the gradient curve, find the vertical depth coordinates corresponding to when the residual austenite volume fraction recovers to the initial level of the unworn matrix, and obtain the effective phase transformation hardening layer depth.

7. The method for optimizing the wear resistance of Cr12 cast balls based on heat treatment process adjustment according to claim 1, characterized in that, The specific steps of S4 include: S41. The macroscopic volume wear rate, hardness gradient matching coefficient and effective phase transformation hardening layer depth corresponding to the same set of input feature matrices constitute an initial evaluation index sequence. S42. The initial evaluation index sequence is dimensionless to obtain a standardized evaluation index sequence. S43. Calculate the absolute difference between the standardized evaluation index sequence and the ideal reference sequence, and use the resolution coefficient to calculate the correlation coefficient of each index. S44. Calculate the weighting coefficients corresponding to the macroscopic volume wear rate, hardness gradient matching coefficient, and effective phase transformation hardening layer depth, and perform a weighted summation based on the correlation coefficients of each index to obtain the gray comprehensive correlation model corresponding to the input feature matrix.

8. The method for optimizing the wear resistance of Cr12 cast balls based on heat treatment process adjustment according to claim 7, characterized in that, The specific rules for calculating the macroscopic volumetric wear rate, hardness gradient matching coefficient, and weighting coefficient corresponding to the effective phase transformation hardening layer depth in S44 are as follows: Based on the standardized evaluation index sequence, the information entropy value of each index is calculated; based on the information entropy value of each index, the first weight coefficient corresponding to the macroscopic volume wear rate, the second weight coefficient corresponding to the hardness gradient matching coefficient, and the third weight coefficient corresponding to the effective phase change hardening layer depth are calculated using the weight calculation formula.

9. The method for optimizing the wear resistance of Cr12 cast balls based on heat treatment process adjustment according to claim 1, characterized in that, The specific steps of S5 include: S51. Substitute all the input feature matrices in the composite heat treatment process space into the gray comprehensive correlation model, and output the gray comprehensive correlation values ​​corresponding to all input feature matrices. S52. Compare all gray comprehensive correlation values ​​and extract the maximum value among the gray comprehensive correlation values; and extract the input feature matrix corresponding to the maximum value as the optimal heat treatment process adjustment scheme; input the optimal heat treatment process adjustment scheme into the control system of the automated heat treatment production line to control the batch production of the Cr12 casting balls.

10. The method for optimizing the wear resistance of Cr12 cast balls based on heat treatment process adjustment according to claim 9, characterized in that, S52, after inputting the optimal heat treatment process adjustment scheme into the control system of the automated heat treatment production line, also includes a step of performing closed-loop temperature control on the batch production process: High-frequency thermocouples arranged in the quenching tank and the distribution tank of the heat treatment furnace are used to collect quenching oil temperature data and distribution salt bath temperature data in real time. The quenching oil temperature data and the salt bath temperature data are transmitted to the control system. The system determines whether the temperature fluctuations of the quenching oil temperature data and the salt bath temperature data exceed the temperature fluctuation threshold. If so, the control system automatically adjusts the heating tube power or the cooling heat exchanger flow rate through a proportional-integral-derivative adjustment algorithm to maintain the actual temperature consistent with the temperature parameters in the optimal heat treatment process adjustment scheme. Otherwise, the system keeps the current heating tube power or cooling heat exchanger flow rate unchanged.