A pre-corrosion aluminum alloy fatigue failure prediction method integrating material microstructure information, corrosion morphology characteristics and mechanical parameters
By dividing aluminum alloy specimens into micro-mesh areas and combining three-dimensional corrosion morphology and microstructure characteristics, a failure location and life prediction model was trained. This solved the problem of neglecting the influence of microstructure in existing methods, and achieved accurate prediction of fatigue crack initiation location and improved stability of life prediction.
Patent Information
- Application Number
- CN202611254258.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-18
- Publication Date
- 2026-11-24
AI Technical Summary
Existing fatigue assessment methods for aluminum alloys neglect the influence of microstructure, lack effective prediction of fatigue crack initiation locations, and lack data support at a fine scale, leading to discrepancies between prediction results and actual values.
The pre-corroded aluminum alloy specimen area was divided into multiple micro-grids, and the three-dimensional corrosion morphology and microstructure features were extracted. A failure location prediction model was trained, and a fatigue life prediction model was trained in combination with in-situ fatigue test data to achieve a comprehensive prediction of fatigue crack initiation location and life.
It enables accurate prediction of fatigue crack initiation location at the microscale, improves the accuracy and stability of fatigue life prediction, and reduces the impact of single local area feature fluctuations on prediction.
Smart Images

Figure CN123161735A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of fatigue performance evaluation and structural integrity prediction of metallic materials, and in particular to a method for predicting fatigue failure of pre-corroded aluminum alloys by integrating material microstructure information, corrosion morphology characteristics and mechanical parameters. Background Technology
[0002] Aluminum alloys, especially aluminum-lithium alloys, are widely used in critical load-bearing structures in aerospace and other fields due to their excellent specific strength and specific stiffness. However, corrosive media in the service environment can cause localized damage such as pitting on the material surface. These damages, acting as stress concentration sources, can significantly accelerate the initiation and propagation of fatigue cracks.
[0003] Existing fatigue assessment methods for pre-corroded metallic materials have the following main technical shortcomings: (1) Ignoring the influence of microstructure: Traditional models treat materials as homogeneous continuums and ignore the decisive role of microstructure features such as grain size, grain boundary orientation, and Schmidt factor on the location of fatigue crack initiation and fatigue life, resulting in deviations between the prediction results and physical reality.
[0004] (2) Single prediction target: Existing methods are mostly focused on predicting the total fatigue life, lacking effective means to predict the key failure location of "where fatigue cracks will initiate".
[0005] (3) Lack of data support at a fine scale: Macroscopic experiments are difficult to capture the initiation and early propagation of microcracks, resulting in a lack of reasonable characterization of the micro-damage evolution mechanism in the lifetime prediction model.
[0006] Therefore, there is an urgent need for a method that can integrate the intrinsic microstructure of materials and the morphology of corrosion damage at multiple scales, and simultaneously predict the failure location and lifetime. Summary of the Invention
[0007] The purpose of this invention is to provide a method for predicting fatigue failure of pre-corroded aluminum alloys by integrating material microstructure information, corrosion morphology characteristics, and mechanical parameters. This method can solve the problems of insufficient characterization of microstructure influence and separation between failure location and fatigue life prediction in existing fatigue assessments. It enables failure location prediction based on micro-region grids and allows the failure location prediction results to be further involved in fatigue life prediction.
[0008] To achieve the above objectives, the present invention provides the following solution: A method for predicting fatigue failure of pre-corroded aluminum alloys by integrating material microstructure information, corrosion morphology characteristics, and mechanical parameters includes: The pre-corrosion area of the pre-corrosion aluminum alloy specimen is divided into multiple micro-grids. The three-dimensional corrosion morphology and microstructure features of each micro-grid are extracted. The failure location prediction model is trained by using whether fatigue cracks are initiated in each micro-grid as a label. Based on the crack initiation mesh observed in the in-situ fatigue experiment, the corresponding local features of the initiation region are extracted; The fatigue life prediction model is trained by taking global three-dimensional corrosion morphology features, global microstructure features, local features of the initiation area and fatigue loading condition parameters as inputs and the total number of fatigue cycles as labels. The pre-corrosion area of the target pre-corrosion aluminum alloy specimen is divided into multiple micro-grids. The three-dimensional corrosion morphology and microstructure characteristics of each micro-grid are input into the failure location prediction model to obtain the crack initiation probability of each micro-grid. Select micro-grids where the crack initiation probability exceeds a preset threshold, extract the local features of the initiation region corresponding to the selected micro-grids, and take the arithmetic mean of the local features of the initiation region. The arithmetic mean, the global three-dimensional corrosion morphology characteristics, global microstructure characteristics, and fatigue loading condition parameters of the target pre-corroded aluminum alloy specimen are input into the fatigue life prediction model to obtain the fatigue life prediction results of the target pre-corroded aluminum alloy specimen.
[0009] Preferably, the pre-corrosion area of the pre-corrosion aluminum alloy specimen is divided into multiple micro-grids, and the three-dimensional corrosion morphology and microstructure characteristics of each micro-grid are extracted, including: Obtain three-dimensional corrosion morphology images, grain orientation images, and microstructure images of the pre-corroded area; Using the corrosion pit outline and grain boundary features within the pre-corrosion area as the positioning reference, three or more non-collinear feature points are determined in the three-dimensional corrosion morphology map, grain orientation map, and microstructure image. Spatial registration is then performed on the three-dimensional corrosion morphology map, grain orientation map, and microstructure image based on the feature points. The pre-corrosion area is divided into multiple micro-grids. Based on the spatially registered three-dimensional corrosion morphology map and grain orientation map, the three-dimensional corrosion morphology features and microstructure features are extracted according to the spatial range of each micro-grid.
[0010] Preferably, the three-dimensional corrosion morphology features of each micro-region mesh are extracted, including: The least squares method was used to fit the reference plane of the pre-corrosion area. The area that is below the reference plane and is continuously distributed is defined as the corrosion pit. The boundary of the corrosion pit is determined by the closed contour line with the largest height change rate at the edge of the pit. Determine the maximum depth, average depth, equivalent area, equivalent volume, aspect ratio, and spacing of each corrosion pit based on its boundary. For a microgrid containing multiple corrosion pits, the maximum value among the maximum depths of each corrosion pit is selected as the maximum depth of the microgrid. The average depth of each corrosion pit is taken as the average depth of the microgrid. The equivalent area and equivalent volume of each corrosion pit are summed to obtain the equivalent area and equivalent volume of the microgrid. The aspect ratio and spacing of each corrosion pit are averaged to obtain the aspect ratio and spacing of the microgrid. The root mean square height, skewness, kurtosis, maximum peak height, maximum depression depth, and maximum height are determined based on all three-dimensional topographic point clouds within each micro-region grid, forming the three-dimensional corrosion topographic features of each micro-region grid.
[0011] Preferably, the microstructural features of each micro-region grid are extracted, including: The crystal orientation at each measurement point is determined based on electron backscatter diffraction data, and the fitted ellipse angle, aspect ratio, grain area, grain perimeter, and grain boundary orientation difference angle are extracted. Based on the angle between the slip surface normal and the direction of the external force axis, and the angle between the slip direction and the direction of the external force axis, the Schmidt factor of multiple slip systems corresponding to each measurement point is determined, and the largest Schmidt factor is selected as the Schmidt factor of the corresponding measurement point. The arithmetic mean of the Schmidt factor of each measurement point in the micro-region grid is taken, and the arithmetic mean is used as the Schmidt factor feature of the corresponding micro-region grid. The Schmidt factor feature, the fitted ellipse angle, the aspect ratio of the fitted ellipse, the grain area, the grain perimeter, and the grain boundary orientation difference angle are used as the microstructure features of each micro-region grid.
[0012] Preferably, the label is whether fatigue cracks have initiated in each micro-region mesh, including: During the in-situ fatigue test, microstructure images of the pre-corroded area were collected according to the set number of cycles, and the initiation location of fatigue cracks was determined based on the microstructure images. The corresponding micro-region mesh is determined based on the location of the initiation. The micro-region mesh with initiating fatigue cracks is labeled as 1, and the micro-region mesh without initiating fatigue cracks is labeled as 0.
[0013] Preferably, training the failure location prediction model includes: Using the micro-area grid data used to train the failure location prediction model as the training set, the three-dimensional corrosion morphology and microstructure features of each micro-area grid are normalized according to the minimum and maximum features of the training set, and the training set is balanced by synthetic minority oversampling technique. A lightweight gradient booster was used to establish a failure location prediction model. A binary classification objective function was used as the training objective, and the binary log loss and the area under the receiver operating characteristic curve were used to evaluate the failure location prediction model. A hyperparameter optimization approach based on the Parsons estimator sampling algorithm based on tree structure is adopted to optimize the number of leaf nodes, learning rate, maximum depth, regularization coefficient, minimum split gain, sample sampling parameters, and feature sampling parameters of the failure location prediction model.
[0014] Preferably, based on the crack initiation mesh observed in the in-situ fatigue experiment, the corresponding local features of the initiation region are extracted, including: Based on the spatial location of the crack initiation grid, determine the corresponding electron backscatter diffraction data and three-dimensional corrosion morphology data. Based on electron backscatter diffraction data and three-dimensional corrosion morphology data, the local maximum grain boundary orientation difference angle, local average Schmidt factor, and local skewness of the crack initiation grid were determined, and these factors were used as local characteristics of the initiation region.
[0015] Preferably, the fatigue life prediction model is trained by taking global three-dimensional corrosion morphology features, global microstructure features, local features of the initiation region, and fatigue loading condition parameters as inputs, and using the total number of fatigue cycles as the label, including: The candidate feature set is composed of global three-dimensional corrosion morphology features, global microstructure features, local features of the initiation region, and fatigue loading condition parameters including peak stress, stress ratio and loading frequency. Calculate the Pearson correlation coefficient between each candidate feature in the candidate feature set and the total number of fatigue cycles, and select candidate features whose absolute value of the Pearson correlation coefficient exceeds the preset correlation coefficient threshold to form an optimized feature set; The fatigue life prediction model is trained by taking the optimized feature set as input, the total number of fatigue cycles as labels, using a lightweight gradient booster and a regression objective function as the training objective.
[0016] Preferably, the pre-corrosion area of the target pre-corrosion aluminum alloy specimen is divided into multiple micro-grids. The three-dimensional corrosion morphology and microstructure characteristics of each micro-grid are input into the failure location prediction model to obtain the crack initiation probability of each micro-grid, including: The pre-corrosion area of the target pre-corrosion aluminum alloy specimen was divided into multiple micro-grids, and the three-dimensional corrosion morphology and microstructure features of each micro-grid were extracted. Based on the minimum and maximum feature values determined during the training of the failure location prediction model, the three-dimensional corrosion morphology and microstructure characteristics of the target pre-corroded aluminum alloy specimen are normalized. The normalized three-dimensional corrosion morphology and microstructure features are input into the failure location prediction model to obtain the crack initiation probability of each micro-region mesh.
[0017] Preferably, micro-grids with a crack initiation probability exceeding a preset threshold are selected, local features of the initiation region corresponding to the selected micro-grids are extracted, and the arithmetic mean of the local features of the initiation region is taken, including: Compare the crack initiation probability of each micro-region mesh with a preset threshold, and select the micro-region mesh whose crack initiation probability exceeds the preset threshold; Determine the local maximum grain boundary orientation difference angle, local average Schmidt factor, and local skewness of the selected microgrid area respectively; The arithmetic mean of the local maximum grain boundary orientation difference angle, local average Schmidt factor, and local skewness of the selected micro-region grid are taken respectively, and the obtained arithmetic mean is used as the local characteristics of the initiation region of the target pre-corroded aluminum alloy specimen.
[0018] The present invention discloses the following beneficial effects: (1) This invention divides the pre-corrosion area of the pre-corrosion aluminum alloy specimen into multiple micro-grids, and combines the three-dimensional corrosion morphology features, microstructure features and fatigue crack initiation labels of each micro-grid to train the failure location prediction model. This allows corrosion damage information and material microstructure information to participate in crack initiation judgment at the same micro-scale, which can reduce the problem of insufficient characterization of local micro-differences when judging based solely on macro-corrosion state, and achieve refined prediction of fatigue crack initiation location in the pre-corrosion area.
[0019] (2) This invention extracts local features of the crack initiation region based on the crack initiation mesh observed in the in-situ fatigue experiment, and uses the global three-dimensional corrosion morphology features, global microstructure features, local features of the initiation region and fatigue loading condition parameters together for fatigue life prediction model training. This allows fatigue life prediction to consider the overall corrosion state of the specimen, the overall microstructure state, the local state of the crack initiation region and the loading conditions at the same time, which can improve the completeness of the characterization of micro-damage differences and the influence of loading conditions.
[0020] (3) The present invention obtains the crack initiation probability of each micro-region grid of the target pre-corroded aluminum alloy specimen through the failure location prediction model, and extracts the local features of the initiation area from the micro-region grid where the crack initiation probability exceeds the preset threshold, so that the failure location prediction result can be further used as the source of local features for fatigue life prediction, thereby avoiding the independence of failure location prediction and fatigue life prediction, and realizing the continuous transmission of failure location prediction result to fatigue life prediction process.
[0021] (4) The present invention takes the arithmetic mean of the local features of the initiation region corresponding to the selected micro-area grid, and inputs the arithmetic mean together with the global three-dimensional corrosion morphology features, global microstructure features and fatigue loading condition parameters of the target pre-corroded aluminum alloy specimen into the fatigue life prediction model. This makes the life prediction result subject to the local high-risk area features and the overall state of the specimen at the same time, which can reduce the impact of the fluctuation of a single local area feature on the fatigue life judgment and improve the stability of the fatigue life prediction result. Attached Figure Description
[0022] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0023] Figure 1 A flowchart of the method provided in an embodiment of the present invention; Figure 2 This is a schematic diagram of the overall processing relationship for predicting fatigue failure of pre-corroded aluminum alloys provided in an embodiment of the present invention; Figure 3 This is a schematic diagram of specimen surface meshing, multi-source data localization, and feature extraction provided in an embodiment of the present invention; Figure 4 This is a superimposed analysis diagram of fatigue crack propagation path and material microstructure provided in an embodiment of the present invention; Figure 5 This is a histogram of prediction results between the SMOTE-processed data and the original data provided in this embodiment of the invention. Figure 6 This is a comparison chart of the predicted crack initiation probability distribution and experimental observation results provided in an embodiment of the present invention; Figure 7 The importance ranking diagram of the influence of material microstructure features and three-dimensional corrosion morphology features on the fatigue crack initiation location is provided in the embodiments of the present invention; Figure 8 The heatmap showing the correlation between global three-dimensional corrosion morphology features, global microstructure features, local features of the initiation region, loading conditions, and SEM in-situ fatigue life is provided for embodiments of the present invention. Figure 9 This is a scatter plot comparing predicted fatigue life and experimental fatigue life provided in an embodiment of the present invention. Figure 10 This is a ranking chart showing the importance of various features for fatigue life prediction provided in the embodiments of the present invention. Detailed Implementation
[0024] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0025] To make the above-mentioned objects, features and advantages of the present invention more apparent and understandable, the present invention will be further described in detail below with reference to the accompanying drawings and specific embodiments.
[0026] Figure 1 The method flowchart provided in the embodiments of the present invention is as follows: Figure 1 As shown, this embodiment provides a method for predicting fatigue failure of pre-corroded aluminum alloys by integrating material microstructure information, corrosion morphology characteristics, and mechanical parameters, including: Step 100: Divide the pre-corrosion area of the pre-corrosion aluminum alloy specimen into multiple micro-grids, extract the three-dimensional corrosion morphology and microstructure features of each micro-grid, and use whether fatigue cracks are initiated in each micro-grid as a label to train the failure location prediction model. Step 200: Extract the corresponding local features of the initiation region based on the crack initiation mesh observed in the in-situ fatigue experiment; Step 300: Take the global three-dimensional corrosion morphology features, global microstructure features, local features of the initiation area and fatigue loading condition parameters as inputs, and the total fatigue cycle number as the label to train the fatigue life prediction model. Step 400: Divide the pre-corrosion area of the target pre-corrosion aluminum alloy specimen into multiple micro-grids, input the three-dimensional corrosion morphology and microstructure characteristics of each micro-grid into the failure location prediction model, and obtain the crack initiation probability of each micro-grid. Step 500: Select micro-area meshes where the crack initiation probability exceeds a preset threshold, extract the local features of the initiation region corresponding to the selected micro-area meshes, and take the arithmetic mean of the local features of the initiation region. Step 600: Input the arithmetic mean, the global three-dimensional corrosion morphology characteristics, global microstructure characteristics and fatigue loading condition parameters of the target pre-corroded aluminum alloy specimen into the fatigue life prediction model to obtain the fatigue life prediction results of the target pre-corroded aluminum alloy specimen.
[0027] Figure 2 This is a schematic diagram illustrating the overall processing relationship for predicting fatigue failure of pre-corroded aluminum alloys according to an embodiment of the present invention. Figure 2As shown, multi-dimensional feature data were collected from the pre-corroded aluminum alloy specimens after specimen preparation and pre-corrosion treatment. After completing the multi-dimensional feature data collection, a failure location prediction dataset was constructed based on the three-dimensional corrosion morphology features, microstructure features, and crack initiation state corresponding to the micro-region grids, and a failure location prediction model was trained. Local features of the initiation region were further extracted based on the crack initiation grids determined by in-situ fatigue experiments. Global three-dimensional corrosion morphology features, global microstructure features, local features of the initiation region, and fatigue loading condition parameters were used to construct a fatigue life prediction dataset and select features, and a fatigue life prediction model was trained. For the target pre-corroded aluminum alloy specimen, the crack initiation probability of each micro-region grid was first determined using the failure location prediction model. Then, based on the crack initiation probability, the local features of the initiation region required for fatigue life prediction were determined, ultimately completing the joint prediction of failure location and fatigue life.
[0028] In implementing this invention, a pre-corroded aluminum alloy fatigue specimen is first prepared. The aluminum alloy used can be selected from 2XXX series aluminum alloys, such as 2024 aluminum alloy and 2050 aluminum alloy, or from 7XXX series aluminum alloys, such as 7075 aluminum alloy and 7050 aluminum alloy, or other high-strength aerospace aluminum alloys. The specimen is preferably machined into a dog-bone shaped microscale specimen suitable for in-situ observation using scanning electron microscopy (SEM). The preferred dimensions of the parallel sections are 3 mm in length, 1.5 mm in width, and 0.8 mm in thickness. Depending on the in-situ loading equipment and the size of the observation window, the overall size of the specimen can be adjusted proportionally, or a plate-shaped specimen with a central opening can be used. The adjustment principle is to ensure that the subsequent pre-corrosion treatment area and the microscopic characterization area are within the effective observation range of the SEM and electron backscatter diffraction (EBSD) systems.
[0029] Mechanical or electrolytic polishing is performed on the central area of the gauge length section of the specimen to remove the surface work-hardened layer and achieve a mirror-like finish. The polished area serves as the test area for subsequent pre-corrosion treatment and microscopic characterization. The center of the test area corresponds to the geometric center of the parallel section of the specimen, thus enabling pre-corrosion treatment, three-dimensional corrosion morphology measurement, EBSD measurement, and SEM in-situ fatigue observation to be performed on the same spatial area.
[0030] Subsequently, accelerated pre-corrosion treatment was performed on the test area to create a surface morphology simulating corrosion damage under service conditions. The corrosion solution used was EXCO exfoliation corrosion solution conforming to ASTM G34, with a composition of 4.0 M NaCl, 0.5 M KNO3, and 0.1 M HNO3. The corrosion temperature was controlled between 20 °C and 25 °C, and the corrosion time was determined within the range of 2 h to 24 h based on the expected degree of corrosion damage. To obtain typical and distinguishable pre-corrosion damage states, corrosion durations of 8 h and 16 h were used, respectively.
[0031] Immediately after the predetermined corrosion time is reached, the specimen is removed from the corrosion solution and sequentially ultrasonically cleaned in deionized water and anhydrous ethanol for at least 3 minutes each time to remove residual corrosion products and corrosion solution from the specimen surface. After cleaning, the specimen is dried in an oven at 40℃~50℃, or by blowing it with cold air. Once the specimen surface is fully dry, it is stored in a desiccator for later use.
[0032] To ensure that the damage morphology formed by pre-corrosion provides statistically representative corrosion feature samples for subsequent model training, the statistical representativeness of corrosion damage in the pre-corrosion treated area is assessed. Specifically, at least three fields of view are randomly selected within the area to be tested, each field of view being approximately 0.2 mm × 0.2 mm. Surface images of the corresponding fields of view are obtained using an optical microscope or a scanning electron microscope, and the results are combined with the three-dimensional morphology measurement results for assessment.
[0033] When the number of corrosion pits in each field of view is no less than 5, the deepest corrosion pit in the field of view is no less than 5 μm, and the projected area coverage of the corrosion pits in the field of view is within the range of 5% to 50%, the current pre-corrosion state is determined to meet the requirements for subsequent feature extraction and model training. If the above conditions cannot be met simultaneously, the corrosion time is adjusted and the pre-corrosion process is repeated until the above statistical representativeness conditions are met. Through the above judgment, it is possible to avoid insufficient number of effective corrosion pit samples due to insufficient corrosion degree, and to avoid insufficient effective discrimination of corrosion morphology distribution due to excessive corrosion degree.
[0034] After pre-corrosion treatment, three-dimensional corrosion morphology data, EBSD microstructure data, and SEM in-situ fatigue test data were collected before and during the SEM in-situ fatigue test. The three-dimensional corrosion morphology data were used to characterize the size, spatial height, and surface morphology of corrosion pits; the EBSD microstructure data were used to characterize the grain, grain boundary, and crystal orientation; and the SEM in-situ fatigue test data were used to determine the initiation location, initiation time, and propagation path of fatigue cracks.
[0035] To ensure that data obtained from different measurement methods correspond to the same spatial location on the specimen surface, spatial registration was performed on the 3D corrosion morphology data, EBSD microstructure data, and SEM in-situ fatigue experimental data. Using the corrosion pit contours and grain boundary features within the test area that could be repeatedly identified in different measurement results as positioning benchmarks, the corrosion morphology images acquired by the 3D morphologist, the grain orientation images acquired by the EBSD system, and the microstructure images acquired by the SEM were imported into the same image processing software. ImageJ or Aztec Crystal could be used for image processing.
[0036] In the 3D corrosion morphology image, grain orientation image, and microstructure image, three or more non-collinear corresponding feature points are manually or automatically identified. These feature points can be selected as the center of an isolated corrosion pit, a grain boundary intersection, or other feature locations that can be stably identified in different images. Based on these corresponding feature points, the images are overlaid and aligned to ensure that the 3D corrosion morphology data, EBSD microstructure data, and SEM in-situ fatigue experimental data correspond pixel-by-pixel in spatial location.
[0037] Regarding the temporal correspondence, 3D corrosion morphology data and EBSD microstructure data were acquired before the fatigue experiment to characterize the initial corrosion morphology and initial microstructure of the specimen. SEM in-situ images were acquired during the fatigue experiment at set cycle intervals, for example, once every 500 cycles. The actual acquisition interval could be determined by considering fatigue loading conditions and crack evolution rate. The initiation time and propagation path of fatigue cracks were determined based on the continuously acquired SEM in-situ images, and the cycle number corresponding to the first observation of a microcrack was recorded as the crack initiation time.
[0038] Figure 3 This is a schematic diagram illustrating specimen surface meshing, multi-source data localization, and feature extraction provided in an embodiment of the present invention. Figure 3 As shown, the Identify section in the figure is used to identify fatigue cracks in SEM microstructure images. Crack 1 and Crack 2 are marked in the figure, and the corresponding local identification areas are given. The Locate section is used to establish the spatial correspondence between different characterization data. One side shows the three-dimensional corrosion morphology and mesh division, and the other side shows the EBSD grain orientation information and the same mesh division. The red positioning points are used to determine the corresponding positions in different data. The Extract section is used to extract features from the spatially corresponded micro-area mesh. The upper three-dimensional morphology map represents the surface spatial position in the X, Y, and Z directions and is marked with Sp. It can further obtain three-dimensional corrosion morphology parameters such as Aspect ratio, Ssk, Volume, Sku, and Particles. The lower grain fitting map is used to obtain microstructure parameters such as SF, Grain area, Grain perimeter, and Fit ellipse angle. Figure 3 The process shown achieves the correspondence between fatigue crack location, three-dimensional corrosion morphology, and EBSD microstructure information within the same microgrid.
[0039] When processing the three-dimensional corrosion morphology data, the reference plane of the evaluation area is fitted using the least squares method according to the ISO 25178 standard, and this reference plane is used as the zero plane for calculating the morphology height. Regions in the three-dimensional point cloud data that are below the reference plane and continuously distributed are identified as corrosion pits. The boundaries of the corrosion pits are determined by the closed contour lines with the largest rate of height change at the pit edges.
[0040] For each identified corrosion pit, the maximum depth, average depth, equivalent area, equivalent volume, aspect ratio, and spacing are extracted. The maximum depth is the maximum depth of each measurement point within the corrosion pit relative to the reference plane; the average depth is the average depth of each measurement point within the corrosion pit relative to the reference plane; the equivalent area is the area enclosed by the corrosion pit boundary projected onto the reference plane; the equivalent volume is obtained by integrating the area of each measurement point within the corrosion pit using its depth value; the aspect ratio is determined based on the length-to-width ratio of the smallest bounding rectangle of the corrosion pit boundary; and the spacing is determined based on the average distance between the center points of adjacent corrosion pit boundaries.
[0041] When a microgrid contains multiple corrosion pits, grid-level statistics are performed on the corrosion pit parameters. The maximum depth of the microgrid is taken as the maximum value among the maximum depths of all corrosion pits within the grid; the average depth of the microgrid is taken as the average of the average depths of all corrosion pits; the equivalent area of the microgrid is taken as the sum of the equivalent areas of all corrosion pits within the grid; the equivalent volume of the microgrid is taken as the sum of the equivalent volumes of all corrosion pits; the aspect ratio and spacing of the microgrid are taken as the average values of the corresponding parameters of each corrosion pit within the grid.
[0042] In addition to the morphological parameters corresponding to individual corrosion pits, surface height statistical parameters are calculated based on all three-dimensional points within each micro-region grid, according to ISO 25178 standard. The calculation scope is not limited to the interior of the corrosion pit. Surface height statistical parameters include root mean square height Sq, skewness Ssk, kurtosis Sku, maximum peak height Sp, maximum depression depth Sv, maximum height Sz, and arithmetic mean height Sa. Specifically, Sq characterizes the degree of variation of surface height relative to the reference plane; Ssk characterizes the skewness of the height distribution; Sku characterizes the sharpness of the height distribution; Sp represents the height between the highest peak and the mean plane; Sv represents the depth between the deepest depression and the mean plane; and Sz characterizes the maximum height range formed by the maximum peak and the maximum depression.
[0043] In specific data processing, the candidate features for three-dimensional corrosion morphology also include the average and maximum values of the corrosion pit area, the average and maximum values of the corrosion pit volume, the corrosion area obtained from three-dimensional morphology measurements, the number of corrosion pits in the pre-corrosion region, the corrosion pit density per unit square millimeter, the average and maximum values of the equivalent sphere radius of the corrosion pit, the average and maximum values of the maximum depth, the average and maximum values of the average depth, the average and maximum values of the maximum height, the average and maximum values of the average height, the average and maximum values of the aspect ratio, and the average and maximum values of the spacing. These parameters, together with Sq, Ssk, Sku, Sp, Sv, Sz, and Sa, constitute the three-dimensional corrosion morphology features that can be used for failure location prediction and fatigue life prediction.
[0044] Microstructural information was obtained using EBSD technology. The crystal orientation at each measurement point was determined by analyzing the Kikuchi bands in the backscattered diffraction pattern, and Euler angles were used to represent the crystal orientation. The microstructural features extracted from the EBSD data include at least the Schmitt factor SF, the fitted ellipse angle, the aspect ratio of the fitted ellipse, the grain area, the grain perimeter, and the grain boundary orientation difference angle.
[0045] The Schmidt factor SF is calculated according to the following formula: In the formula, The angle between the normal to the slip surface and the direction of the external force axis. It is the angle between the sliding direction and the direction of the external force axis. The value range is 0 to 0.5; The larger the value, the greater the shear stress on the corresponding slip system, and the easier it is for the corresponding slip system to be activated.
[0046] For face-centered cubic aluminum alloys, the {111}<110> slip system family is selected, resulting in 12 possible slip systems. For each measurement point within each grain, the SF value corresponding to each of the 12 slip systems is calculated, and the maximum value is taken as the representative SF value for that measurement point, characterizing the slip system most easily activated at that location. When a microgrid contains multiple grains or multiple measurement points, the arithmetic mean of the representative SF values of all measurement points within the grid is taken, and this arithmetic mean is used as the Schmitt factor characteristic of the corresponding microgrid.
[0047] Furthermore, the candidate features of the microstructure can include the average, minimum, and maximum values of the Schmidt factor, the average, minimum, and maximum values of the grain area, the average, minimum, and maximum values of the grain perimeter, the average, minimum, and maximum values of the fitted ellipse angle, the average, minimum, and maximum values of the fitted ellipse aspect ratio, and the minimum and maximum values of the orientation difference angle.
[0048] While acquiring the aforementioned morphological and microstructural information, the fatigue loading condition parameters of the SEM in-situ fatigue experiment were recorded. These parameters included at least the peak stress, stress ratio, and loading frequency, to ensure that corrosion damage, material microstructure, and external loading conditions were considered simultaneously during fatigue life prediction.
[0049] The pre-corrosion area was uniformly divided into N micro-grids, each serving as a data unit for failure location prediction. Three-dimensional corrosion morphology and microstructure features were extracted for each micro-grid, and in-situ fatigue experiments using SEM were conducted to determine whether fatigue crack initiation had occurred in the corresponding micro-grid. Micro-grids with fatigue crack initiation were labeled 1, while those without were labeled 0, thus forming the failure location prediction dataset.
[0050] Before model training, the extracted feature parameters are normalized using Min-Max to eliminate differences in units and magnitudes between different parameters. The normalization formula is: In the formula, These are the original eigenvalues. This represents the minimum value of the corresponding feature in the training set. This represents the maximum value of the corresponding feature in the training set. The normalized eigenvalues take values in the range [0,1].
[0051] Normalized parameters and Determined solely based on training set data. Data from the test set and the target pre-corroded aluminum alloy specimens were all derived from the same set determined during the training phase. and Normalization is performed without redetermining the normalization parameters using data from the test set or the target specimen.
[0052] To address the imbalance between fatigue crack initiation and non-initiation samples, a synthetic minority oversampling technique (SMOTE) is used to balance the training set. This technique generates minority class samples to improve the class distribution of the training data. SMOTE is used for training data balancing, while the independent test data maintains its original sample distribution.
[0053] The failure location prediction model was constructed using the LightGBM algorithm. The LightGBM classification model used 'binary' as the objective function and binary logloss as the loss function during training. Both binary logloss and the area under the receiver operating characteristic (AUC) curve were monitored, with AUC used as the primary evaluation metric for classification performance. The raw predicted values obtained by the model were converted into crack initiation probabilities within the range of 0 to 1 using the sigmoid function.
[0054] The hyperparameters of the LightGBM classification model are searched using the Optuna framework combined with the TPE sampling algorithm. `num_leaves` represents the number of leaf nodes in a single tree, with a search range of [2, 100]; `learning_rate` represents the learning rate, with a search range of [0.01, 0.3]; `max_depth` represents the maximum depth of the tree, with a search range of [2, 20]; `lambda_l1` represents the L1 regularization coefficient, with a search range of [0, 50]; `lambda_l2` represents the L2 regularization coefficient, with a search range of [0, 50]; `min_gain_to_split` represents the minimum gain for splitting, with a search range of [0, 15]; `bagging_fraction` represents the sampling ratio, with a search range of [0.2, 1.0]; `bagging_freq` represents the sampling frequency, with a search range of [0, 10]; and `feature_fraction` represents the feature sampling ratio, with a search range of [0.2, 1.0].
[0055] In one model training method, the original samples are isolated according to the specimens, with 80% of the sample data used as training data and 20% as independent test data, ensuring that different micro-region grids corresponding to the same specimen are not simultaneously included in the training data and independent test data. Subsequently, SMOTE sample balancing is performed only on the training data. During the model parameter optimization process, the SMOTE-processed training data is divided into training subsets and validation subsets in an 8:2 ratio.
[0056] During training, `early_stopping_rounds=50` was set, and training was stopped if the validation set evaluation metric failed to improve for 50 consecutive rounds. Optuna performed 300 complete hyperparameter search trials, determining the hyperparameter combination based on the classification evaluation results of the validation set. After hyperparameter optimization, the LightGBM failure location prediction model was retrained on SMOTE-processed training data using the determined hyperparameter combination. The generalization performance of the model was then evaluated using unprocessed original independent test data.
[0057] After training, the failure location prediction model can obtain the crack initiation probability in the range of 0 to 1 for each micro-grid area of the target specimen. The higher the crack initiation probability, the higher the probability of fatigue crack initiation in the corresponding micro-grid area. Arranging the crack initiation probabilities according to the spatial position of each micro-grid area on the specimen surface can form a failure risk distribution.
[0058] The local features of the initiation region used in fatigue life prediction are determined based on the fatigue crack initiation region. During the training phase, based on the crack initiation grid positions actually observed in in-situ SEM fatigue experiments, local features are extracted from the corresponding grid's EBSD data and 3D corrosion morphology data using the aforementioned spatial registration relationship. These local features include the local maximum grain boundary orientation difference angle, the local average Schmidt factor, and the local skewness (Ssk). In specific fatigue experiments, the local grain area can also be extracted from the EBSD data corresponding to the crack initiation grid to characterize the local grain-scale state at the crack initiation location.
[0059] Figure 4 This is a superimposed analysis diagram of fatigue crack propagation path and material microstructure provided for embodiments of the present invention. Figure 4 As shown, the left image uses the Schmidt factor distribution to distinguish different grain regions. The black curve represents the fatigue crack propagation path, and the white area marks the pit sidewall. The Schmidt factor color scale ranges from 0.28 to 0.50. Grain regions with SF=0.46, SF=0.48, SF=0.47, SF=0.47, SF=0.45, SF=0.29, and SF=0.50 are marked near the crack. The scale bar is 15 μm. The right image overlays grain boundaries and fatigue crack propagation paths onto the microstructure image. Different colored grain boundaries correspond to different grain boundary orientation difference angles. The grain boundary orientation difference angles marked in the image include 41.7°, 13.9°, 20.1°, 37.1°, 51.1°, 54.5°, and 36.7°. Locations ① and ②, as well as local angle information at 42° and 36°, are also marked near the crack path. The scale bar is 15 μm. Figure 4 It is possible to establish the correspondence between fatigue crack paths, corrosion pit sidewalls, Schmidt factor distribution, and grain boundary orientation difference angles in the same spatial location, and thereby determine the local microstructural features corresponding to the crack initiation region.
[0060] The candidate inputs used to train the fatigue life prediction model include four categories of features. The first category is global three-dimensional corrosion morphology features, including maximum pit depth, average depth, area, and skewness (Ssk). The second category is global microstructure features, including average grain area and average Schmidt factor. The third category is local features of the initiation region. The fourth category is fatigue loading condition parameters, including peak stress, stress ratio, and loading frequency. The total number of fatigue cycles of the specimen is used as the fatigue life label.
[0061] Correlation analysis was performed on the above candidate features, and the Pearson correlation coefficient between each candidate feature and the total number of fatigue cycles was calculated. The Pearson correlation coefficient was calculated according to the following formula: In the formula, These can be candidate feature parameters, such as maximum pit depth, average Schmidt factor, or other candidate features; This is the fatigue life label, i.e., the total number of fatigue cycles. for and The Pearson correlation coefficient between the candidate features and fatigue life is used to determine the relationship. A higher absolute value of the Pearson correlation coefficient indicates a stronger correlation between the corresponding candidate feature and fatigue life. In one specific implementation, candidate features with an absolute Pearson correlation coefficient greater than 0.2 are selected to form an optimized feature set.
[0062] The fatigue life prediction model was built using the LightGBM algorithm, with 'regression' as the regression training objective. The optimized feature set obtained through correlation screening was used as the model input, and the total number of fatigue cycles was used as the label to complete the fatigue life prediction model training. The hyperparameters of the fatigue life prediction model could also be optimized using the Optuna framework combined with the TPE sampling algorithm, and the coefficient of determination R was used to determine the parameters. 2 Regression evaluation indicators are used to evaluate the fatigue life prediction performance.
[0063] For the pre-corroded aluminum alloy specimen requiring fatigue failure prediction, three-dimensional corrosion morphology data and EBSD microstructure data were obtained using the aforementioned data acquisition method. The target pre-corroded area was divided into multiple micro-grids, and the three-dimensional corrosion morphology and microstructure features of each micro-grid were extracted. The various features of the target specimen were determined when training the failure location prediction model. and After normalization, the three-dimensional corrosion morphology and microstructure features of each micro-region grid are input into the trained failure location prediction model to obtain the crack initiation probability corresponding to each micro-region grid.
[0064] The local features of the initiation region of the target specimen for fatigue life prediction are determined based on the crack initiation probability of each micro-grid. Specifically, a preset threshold can be set to 0.5, and all micro-grids with a crack initiation probability exceeding 0.5 are selected. The local maximum grain boundary orientation difference angle, local average Schmidt factor, local skewness, and other local features of the initiation region corresponding to the training stage are extracted from the selected micro-grids. For the same local feature, the arithmetic mean of the corresponding feature values of all selected micro-grids is taken. The arithmetic mean of each local feature forms the local features of the initiation region of the target pre-corroded aluminum alloy specimen.
[0065] The global three-dimensional corrosion morphology, global microstructure, local features of the initiation region determined by the crack initiation probability, and fatigue loading condition parameters of the target pre-corroded aluminum alloy specimen are input into the fatigue life prediction model to obtain the predicted fatigue life of the target pre-corroded aluminum alloy specimen under the current corrosion damage state and loading conditions. The predicted fatigue life is expressed as the total number of fatigue cycles. Through the above processing, the crack initiation probability of each micro-region mesh and the specimen-level fatigue life prediction results can be obtained simultaneously for the same target pre-corroded aluminum alloy specimen.
[0066] To further illustrate the specific implementation process of this invention, aerospace-grade 2050-T8 aluminum-lithium alloy sheet was used for the experiment. A dog-bone shaped microscale specimen suitable for in-situ SEM observation was machined along the rolling direction of the sheet, with parallel section dimensions of 3 mm long × 1.5 mm wide × 0.8 mm thick. A 0.5 mm × 0.5 mm area was selected at the center of the gauge length section of the specimen as the test area. An EXCO solution prepared according to ASTM G34 standard was used to immerse and etch the test area under a -0.8 bar vacuum condition. The etching times were set to 8 h and 16 h, respectively, to form an array of corrosion pits of different degrees.
[0067] The pre-corrosion area was scanned using a white-light interferometric 3D topology analyzer. An Infinite Focus G5 instrument with a vertical resolution of 40 nm was used. The obtained 3D point cloud data was imported into Mountains Map software for processing to reconstruct the 3D morphology of the corrosion pits within the pre-corrosion area. The pre-corrosion area was uniformly divided into 48 micro-grids, and the 3D corrosion morphology features of each micro-grid were extracted according to the ISO 25178 standard.
[0068] The three-dimensional corrosion morphology parameters recorded in this implementation process include the average and maximum area, average and maximum volume, corrosion area, particle number, density, average and maximum equivalent sphere radius, average and maximum depth, average and maximum average depth, average and maximum maximum height, average and maximum average height, average and maximum aspect ratio, and average and maximum spacing. Area is used to characterize the area of corrosion pits within the pre-corrosion region; volume is used to characterize the volume of corrosion pits; corrosion area is obtained from three-dimensional morphology measurements; particle number represents the number of corrosion pits within the pre-corrosion region; density represents the number of corrosion pits per square millimeter; radius represents the radius of the equivalent sphere of the corrosion pit; maximum and average depths characterize the depth state of the corrosion pits; aspect ratio characterizes the planar shape of the corrosion pits; and spacing characterizes the spatial distribution distance between corrosion pits. Sq, Ssk, Sp, Sv, Sku, Sz, and Sa are also recorded, where Sz is jointly characterized by Sp and Sv to represent the maximum height range of the surface.
[0069] Before the fatigue test, the gauge length of the specimen was scanned using an EBSD system with a scan step size of 1 μm, and the EBSD data was processed using Aztec Crystal software. The average, minimum, and maximum values of the Schmidt factor, grain area, grain perimeter, fitted ellipse angle, fitted ellipse aspect ratio, and orientation difference angle were recorded for each micro-region grid.
[0070] Subsequently, in-situ fatigue tests were conducted using SEM images. The loading frequency was set to 10 Hz, the stress ratio R=0.1, and the peak stresses were set to 324 MPa, 378 MPa, and 432 MPa, respectively. The initiation of fatigue cracks in each micro-region was observed in real time using in-situ SEM images. Micro-regions with microcrack initiation were labeled as 1, while those without microcrack initiation were labeled as 0.
[0071] In this process, 24 pre-corroded aluminum alloy specimens were prepared. The surface of each specimen was divided into 48 micro-grids, resulting in 1,152 sets of grid-level data. Each set of data included 38 characteristic parameters and one crack initiation label. During the data partitioning process, it was ensured that micro-grids corresponding to the same specimen were not simultaneously included in the training data and independent test data. The training data was balanced using SMOTE.
[0072] Figure 5 This is a histogram showing the prediction results of the SMOTE-processed data and the original data provided in an embodiment of the invention. For example... Figure 5As shown, the left side represents SMOTE data, and the right side represents RAW data. The horizontal axis represents the predicted result, and the vertical axis represents the count. The dashed lines in both subplots are at 0.5, representing the classification threshold. The SMOTE data plot is labeled R... 2 =93.78%, MSE=1.5%, and the results of four other statistical items, TT, TN, FT and FN, are also listed, with corresponding labels in the figure: 0.499%, 0.478%, 0.016% and 0.007%, respectively; RAW data is labeled R 2 =93.81%, MSE=0.7%, and TT, TN, FT and FN are labeled in the figure as 0.048%, 0.952%, 0.000% and 0.000%, respectively. The predicted values of the two sets of data are mainly distributed in the regions close to 0 and close to 1, and there are relatively few prediction results near the 0.5 classification threshold.
[0073] When using raw, independent test data without SMOTE processing for validation, with a classification threshold of 0.5, no false positives or false negatives were observed, and all test samples obtained classification results consistent with the experimental labels. The crack initiation probabilities corresponding to each micro-region grid can also be arranged according to their spatial location on the specimen surface to form a crack initiation probability distribution.
[0074] Figure 6 This is a comparison chart of the predicted crack initiation probability distribution and experimental observation results provided in an embodiment of the present invention. Figure 6 As shown, the left side displays the SEM microstructure image of the specimen surface. Three yellow boxes and arrows mark the three experimental observation areas I1, I2, and I3, respectively, with a scale bar of 200 μm. The right side shows the corresponding micro-grid superimposed on the specimen area, with each micro-grid indicating the corresponding crack initiation probability. The background color represents the three-dimensional height Z, with the height range shown on the right being approximately 536.8 μm to 744.4 μm. Crack initiation probabilities of approximately 0.97110, 0.93153, and 0.94972 are observed in the locally high-probability regions corresponding to I1, I2, and I3, respectively. By comparing the probability distributions of the SEM experimental observation areas and the micro-grid regions, the actual fatigue crack initiation areas can be compared with the high crack initiation probability areas determined by the model at the same spatial location.
[0075] Figure 7 This is a ranking diagram showing the importance of the influence of material microstructure features and three-dimensional corrosion morphology features on the fatigue crack initiation location, as provided in embodiments of the present invention. Figure 7As shown, the figure uses two filling methods to distinguish between microstructure and morphology features, labeled "Microstructure" and "Morphology" respectively; the horizontal axis is labeled "Importance". The importance of each feature in the figure, from highest to lowest, includes: maximum orientation difference angle (5.67%), average Schmidt factor (4.81%), skewness (Ssk) (3.98%), minimum Schmidt factor (3.93%), average fitted ellipse angle (3.70%), average aspect ratio (3.60%), minimum fitted ellipse aspect ratio (3.38%), average grain area (3.37%), kurtosis (Sku) (3.31%), minimum fitted ellipse angle (3.22%), maximum fitted ellipse aspect ratio (3.20%), maximum aspect ratio (3.20%), maximum fitted ellipse angle (3.17%), average fitted ellipse aspect ratio (3.16%), average spacing (2.79%), maximum grain perimeter (2.72%), maximum spacing (2.71%), maximum area (2.69%), minimum grain perimeter (2.64%), and maximum peak height (Sp). 2.64%, maximum volume 2.46%, number of grains 2.35%, minimum orientation difference angle 2.30%, maximum grain area 2.17%, maximum average depth 2.17%, minimum grain area 2.12%, average area 2.09%, and maximum depression depth Sv 2.03%.
[0076] The above results indicate that grain boundary orientation difference angle, Schmidt factor, and surface morphology skewness are all major characteristics influencing the location of fatigue crack initiation. A larger grain boundary orientation difference corresponds to more pronounced dislocation pile-up and local stress concentration near the grain boundary; a higher Schmidt factor corresponds to slip systems that are more easily activated under external loads; and skewness (Ssk) characterizes the asymmetry of the height distribution on the corroded surface, thus reflecting the influence of corrosion morphology on the local stress state.
[0077] In fatigue life prediction experiments, based on the crack initiation mesh locations actually identified in in-situ SEM fatigue experiments, the local maximum grain boundary orientation difference angle, local average Schmidt factor, and local grain area are extracted from the corresponding EBSD data, and combined with the local skewness in the corresponding three-dimensional corrosion morphology data to form local features of the initiation region. Global three-dimensional corrosion morphology features, global microstructure features, local features of the initiation region, and fatigue loading condition parameters are collectively incorporated into the fatigue life prediction candidate feature set.
[0078] The Pearson correlation coefficients between candidate features and fatigue life were calculated, and candidate features with an absolute Pearson correlation coefficient greater than 0.2 were selected. A total of 29 features were obtained in this implementation process, and a fatigue life prediction dataset was established using these selected features.
[0079] Figure 8The heatmap provided in this embodiment of the invention shows the correlation between global three-dimensional corrosion morphology features, global microstructure features, local features of the initiation region, loading conditions, and in-situ fatigue life via SEM. Figure 8 As shown, different colors represent the positive and negative directions and absolute values of the Pearson correlation coefficient. In the figure, the average Schmidt factor corresponds to -0.06, the minimum Schmidt factor to -0.00, and the maximum Schmidt factor to 0.00; the average grain area to 0.29, the minimum grain area to 0.00, and the maximum grain area to 0.25; the average grain perimeter to 0.45, the minimum grain perimeter to 0.00, and the maximum grain perimeter to -0.05; the average fitted ellipse angle to -0.01; the minimum fitted ellipse angle to -0.12, and the maximum fitted ellipse angle to 0.00; the average fitted ellipse aspect ratio to -0.08, the minimum fitted ellipse aspect ratio to 0.04, and the maximum fitted ellipse aspect ratio to -0.15; the minimum orientation difference angle to 0.00, and the maximum orientation difference angle to -0.03; Load to -0.63; and Corrosion area (a) to -0.42. (b) Corresponds to -0.43; number of particles corresponds to 0.47, density corresponds to 0.55, average area corresponds to -0.44, maximum area corresponds to -0.27, average volume corresponds to -0.42, maximum volume corresponds to -0.27, average equivalent sphere radius corresponds to -0.09, maximum equivalent sphere radius corresponds to -0.05, average maximum depth corresponds to -0.45, maximum maximum depth corresponds to -0.35; average depth corresponds to -0.44, average depth corresponds to -0.33, average maximum height corresponds to -0.30, maximum height corresponds to -0. The average height is -0.10, the average value corresponds to -0.33, the maximum value corresponds to -0.29, the average aspect ratio is 0.00, the maximum aspect ratio is 0.22, the average spacing is -0.31, the maximum spacing is -0.26; Sq corresponds to -0.40, Ssk corresponds to 0.15, Sku corresponds to -0.13, Sp corresponds to -0.29, Sv corresponds to -0.56, Sz corresponds to -0.50, Sa corresponds to -0.37, the local average Schmidt factor corresponds to -0.29, the maximum local orientation difference angle corresponds to -0.35, and the local Ssk corresponds to 0.16. Corrosion area (a) and Corrosion area (b) are two corrosion area characteristics recorded in the experimental data graph.
[0080] A fatigue life prediction model was trained using LightGBM combined with Optuna. To compare the impact of different feature combinations on fatigue life prediction, the same training and testing data were used, with the same random seed, to build Model A and Model B respectively. Model A used global 3D corrosion morphology features, global microstructure features, local features of the initiation region, and fatigue loading condition parameters as input; Model B used global 3D corrosion morphology features, local features of the initiation region, and fatigue loading condition parameters as input, but did not include EBSD global microstructure features. Training data accounted for 80%, and testing data accounted for 20%.
[0081] The fatigue life prediction performance is determined by the coefficient of determination R. 2 The normalized mean square error (NMSE) is used for evaluation. The coefficient of determination R0 is... 2 Calculate according to the following formula: In the formula, For the first The actual fatigue life of each sample, in cycles; For the first Predicted fatigue life for each sample, in cycles; This is the arithmetic mean of the actual fatigue life.
[0082] Normalized mean square error (NMSE) is calculated using the following formula: In the formula, For the sample size, , and The meaning of the above-mentioned coefficient of determination The parameters in the text have the same meaning.
[0083] When the actual fatigue life is plotted on the x-axis and the predicted fatigue life on the y-axis, the 1.5x error band satisfies: In logarithmic coordinates, the 1.5x error band is located on both sides of the ideal prediction line.
[0084] In this implementation process, the R of model A 2 The accuracy was 95.2%, and the NMSE was 8%; the R-squared value of model B was... 2 The R-squared value was 91.07%, and the NMSE was 13.05%. Compared with Model B, Model A's R-squared value was 91.07%, and its NMSE was 13.05%. 2The improvement was approximately 4 percentage points, while the NMSE decreased from 13.05% to 8%. Both Model A and Model B include local features of the initiation region. The difference between the two is that Model A further includes global EBSD microstructural features. Therefore, the above comparison results are used to reflect the change in fatigue life prediction performance after introducing global microstructural features under the current experimental data conditions.
[0085] Figure 9 This is a scatter plot comparing predicted fatigue life and experimental fatigue life provided in an embodiment of the present invention. Figure 9 As shown, the horizontal axis represents Experimental fatigue life, and the vertical axis represents Predicted fatigue life. Both axes use a logarithmic scale, and the coordinate range covers approximately 10... 4 ~10 6 Cycle number. The solid black line indicates the position where the predicted fatigue life equals the experimental fatigue life, and the two dashed red lines represent the 1.5-error band. In the legend, training data is represented by solid blue-green circles, test data by solid dark red circles, test data without EBSD by solid gray triangles, and training data without EBSD by hollow gray triangles. When using a fatigue life prediction model that includes the global microstructure features of EBSD, all predicted points in the figure are within the 1.5-error band; the control model that does not include the global microstructure features of EBSD has two sample points outside the 1.5-error band.
[0086] Figure 10 This is a ranking diagram showing the importance of various features for fatigue life prediction provided in embodiments of the present invention. For example... Figure 10As shown, different fill colors represent four types of features: Morphology, Microstructure, Local features, and Load. The horizontal axis represents Importance. In the figure, the peak stress σmax is 10.55%, the maximum grain area is 8.98%, the maximum average depth is 8.78%, the maximum spacing is 8.59%, the maximum local orientation difference angle (LODA(max)) is 8.59%, Sp is 7.42%, density is 6.06%, the average maximum depth is 5.08%, the maximum average height is 4.30%, the average maximum height is 4.30%, the average grain area is 3.52%, the number of grains is 3.13%, Sq is 3.13%, the Corrosion area (a) is 2.73%, the maximum maximum depth is 2.73%, the local average Schmidt factor is 1.95%, the maximum area is 1.95%, the average volume is 1.56%, and the Corrosion area... (b) The average aspect ratio is 1.56%, the average spacing is 1.17%, Sz is 0.78%, Sa is 0.78%, Sv is 0.78%, the maximum aspect ratio is 0.39%, the average height is 0.39%, the average depth is 0.39%, the average grain perimeter is 0.39%, the maximum volume is 0.00%, and the average area is 0.00%. LODA in the figure represents the Local Orientation Difference Angle. From the above importance results, it can be seen that the fatigue life prediction in this implementation process is simultaneously affected by fatigue loading conditions, three-dimensional corrosion morphology, overall microstructure, and local characteristics of the initiation region.
[0087] In other implementations, the failure location prediction model and fatigue life prediction model are not limited to LightGBM. Depending on the sample size, feature distribution, and specific prediction task, XGBoost, random forest, support vector regression, or neural networks can be used to build the corresponding classification or regression models.
[0088] Feature selection methods are not limited to Pearson correlation coefficient; Spearman correlation coefficient can also be used for feature correlation analysis. The correlation coefficient threshold is not limited to 0.2; the appropriate threshold can be determined based on the actual data distribution and model performance.
[0089] Three-dimensional corrosion morphology data are not limited to being obtained using a white light interferometer; they can also be obtained using morphology measurement equipment with submicron vertical resolution, such as a laser confocal microscope or an atomic force microscope.
[0090] The spatial division of the pre-corrosion region is not limited to uniform rectangular microgrids. Based on the spatial distribution characteristics of corrosion pits within the pre-corrosion region, adaptive meshes or Voronoi diagrams can also be used for region division, and a spatial correspondence between three-dimensional corrosion morphology features, microstructure features, and fatigue crack initiation states can be established in each region after division.
[0091] In addition to being applicable to 2050-T8 aluminum-lithium alloy, the above method is also applicable to the prediction of pre-corrosion fatigue failure of other aluminum alloys. When the corresponding three-dimensional corrosion morphology information, material microstructure information and fatigue loading data can be obtained, and the data correspondence between failure location prediction and fatigue life prediction can be established, it can also be used for the prediction of pre-corrosion fatigue failure of titanium alloys or high-strength steel and other metal structural materials.
[0092] The various embodiments in this specification are described in a progressive manner, with each embodiment focusing on its differences from other embodiments. Similar or identical parts between embodiments can be referred to interchangeably. For the systems disclosed in the embodiments, since they correspond to the methods disclosed in the embodiments, the descriptions are relatively simple; relevant parts can be referred to the method section.
[0093] Specific examples have been used to illustrate the principles and implementation methods of this invention. The descriptions of the above embodiments are only for the purpose of helping to understand the method and core ideas of this invention. Furthermore, those skilled in the art will recognize that, based on the ideas of this invention, there will be changes in the specific implementation methods and application scope. Therefore, the content of this specification should not be construed as a limitation of this invention.
Claims
1. A method for predicting fatigue failure of pre-corroded aluminum alloys by integrating material microstructure information, corrosion morphology characteristics, and mechanical parameters, characterized in that, include: The pre-corrosion area of the pre-corrosion aluminum alloy specimen is divided into multiple micro-grids. The three-dimensional corrosion morphology and microstructure features of each micro-grid are extracted. The failure location prediction model is trained by using whether fatigue cracks are initiated in each micro-grid as a label. Based on the crack initiation mesh observed in the in-situ fatigue experiment, the corresponding local features of the initiation region are extracted; The fatigue life prediction model is trained by taking the global three-dimensional corrosion morphology features, global microstructure features, local features of the initiation region, and fatigue loading condition parameters as inputs and the total fatigue cycle count as a label. The pre-corrosion area of the target pre-corrosion aluminum alloy specimen is divided into multiple micro-grids. The three-dimensional corrosion morphology and microstructure characteristics of each micro-grid are input into the failure location prediction model to obtain the crack initiation probability of each micro-grid. Select micro-grids where the crack initiation probability exceeds a preset threshold, extract local features of the initiation region corresponding to the selected micro-grids, and take the arithmetic mean of the local features of the initiation region. The arithmetic mean, the global three-dimensional corrosion morphology features, global microstructure features, and fatigue loading condition parameters of the target pre-corroded aluminum alloy specimen are input into the fatigue life prediction model to obtain the fatigue life prediction results of the target pre-corroded aluminum alloy specimen.
2. The method for predicting fatigue failure of pre-corroded aluminum alloys according to claim 1, characterized in that, The pre-corrosion area of the pre-corrosion aluminum alloy specimen was divided into multiple micro-grids, and the three-dimensional corrosion morphology and microstructure features of each micro-grid were extracted, including: Obtain three-dimensional corrosion morphology images, grain orientation images, and microstructure images of the pre-corrosion area; Using the corrosion pit outline and grain boundary features within the pre-corrosion area as positioning references, three or more non-collinear feature points are determined in the three-dimensional corrosion morphology image, the grain orientation image, and the microstructure image. Spatial registration is then performed on the three-dimensional corrosion morphology image, the grain orientation image, and the microstructure image based on the feature points. The pre-corrosion area is divided into multiple micro-grids. Based on the spatially registered three-dimensional corrosion morphology map and the grain orientation map, the three-dimensional corrosion morphology features and the microstructure features are extracted according to the spatial range of each micro-grid.
3. The method for predicting fatigue failure of pre-corroded aluminum alloys according to claim 1, characterized in that, Extracting the three-dimensional corrosion morphology features of each micro-region mesh, including: The least squares method is used to fit the reference plane of the pre-corrosion area. The areas that are lower than the reference plane and are continuously distributed are identified as corrosion pits. The boundary of the corrosion pit is determined by the closed contour line with the largest height change rate at the edge of the pit. The maximum depth, average depth, equivalent area, equivalent volume, aspect ratio, and spacing of each corrosion pit are determined based on the boundaries of the corrosion pits. For a microgrid containing multiple corrosion pits, the maximum value among the maximum depths of each corrosion pit is selected as the maximum depth of the microgrid. The average depth of each corrosion pit is taken as the average depth of the microgrid. The equivalent area and equivalent volume of each corrosion pit are summed to obtain the equivalent area and equivalent volume of the microgrid. The aspect ratio and spacing of each corrosion pit are averaged to obtain the aspect ratio and spacing of the microgrid. The root mean square height, skewness, kurtosis, maximum peak height, maximum depression depth, and maximum height are determined based on all three-dimensional topographic point clouds within each micro-region grid, forming the three-dimensional corrosion topographic features of each micro-region grid.
4. The method for predicting fatigue failure of pre-corroded aluminum alloys according to claim 1, characterized in that, Extracting the microstructural features of each of the aforementioned micro-region grids, including: The crystal orientation at each measurement point is determined based on electron backscatter diffraction data, and the fitted ellipse angle, aspect ratio, grain area, grain perimeter, and grain boundary orientation difference angle are extracted. Based on the angle between the slip surface normal and the direction of the external force axis, and the angle between the slip direction and the direction of the external force axis, the Schmidt factor of multiple slip systems corresponding to each measurement point is determined, and the largest Schmidt factor is selected as the Schmidt factor of the corresponding measurement point. The arithmetic mean of the Schmidt factor of each measurement point in the micro-region grid is taken, and the arithmetic mean is used as the Schmidt factor feature of the corresponding micro-region grid. The Schmidt factor feature, the fitted ellipse angle, the aspect ratio of the fitted ellipse, the grain area, the grain perimeter, and the grain boundary orientation difference angle are used as the microstructure features of each micro-region grid.
5. The method for predicting fatigue failure of pre-corroded aluminum alloys according to claim 1, characterized in that, Using whether fatigue cracks initiate in each of the aforementioned micro-regions as a label, including: During the in-situ fatigue test, microstructure images of the pre-corrosion area were collected according to a set number of cycles, and the initiation location of fatigue cracks was determined based on the microstructure images. The corresponding micro-region mesh is determined based on the initiation location. The label of the micro-region mesh where fatigue cracks have initiated is set to 1, and the label of the micro-region mesh where fatigue cracks have not initiated is set to 0.
6. The method for predicting fatigue failure of pre-corroded aluminum alloys according to claim 1, characterized in that, Training the failure location prediction model includes: Using the micro-area grid data used to train the failure location prediction model as the training set, the three-dimensional corrosion morphology features and microstructure features of each micro-area grid are normalized according to the feature minimum and feature maximum values of the training set, and the training set is balanced using synthetic minority oversampling technology. The failure location prediction model was established using a lightweight gradient booster, with a binary classification objective function as the training objective, and the failure location prediction model was evaluated using binary log loss and area under the receiver operating characteristic curve. The number of leaf nodes, learning rate, maximum depth, regularization coefficient, minimum split gain, sample sampling parameters, and feature sampling parameters of the failure location prediction model are optimized by using a hyperparameter optimization method based on the Parsons estimator sampling algorithm based on tree structure.
7. The method for predicting fatigue failure of pre-corroded aluminum alloys according to claim 1, characterized in that, Based on the crack initiation mesh observed in the in-situ fatigue experiment, the corresponding local features of the initiation region are extracted, including: Based on the spatial location of the crack initiation grid, determine the electron backscatter diffraction data and three-dimensional corrosion morphology data corresponding to the crack initiation grid; Based on the electron backscatter diffraction data and the three-dimensional corrosion morphology data, the local maximum grain boundary orientation difference angle, the local average Schmidt factor, and the local skewness of the crack initiation grid are determined, and the local maximum grain boundary orientation difference angle, the local average Schmidt factor, and the local skewness are used as local features of the initiation region.
8. The method for predicting fatigue failure of pre-corroded aluminum alloys according to claim 1, characterized in that, Using global three-dimensional corrosion morphology features, global microstructure features, local features of the initiation region, and fatigue loading condition parameters as inputs, and with the total number of fatigue cycles as the label, a fatigue life prediction model is trained, including: The global three-dimensional corrosion morphology features, the global microstructure features, the local features of the initiation region, and the fatigue loading condition parameters including peak stress, stress ratio, and loading frequency are combined to form a candidate feature set; Calculate the Pearson correlation coefficient between each candidate feature in the candidate feature set and the total number of fatigue cycles, and select candidate features whose absolute value of the Pearson correlation coefficient exceeds a preset correlation coefficient threshold to form an optimized feature set; The fatigue life prediction model is trained by taking the optimized feature set as input, the total number of fatigue cycles as label, using a lightweight gradient booster and a regression objective function as training objective.
9. The method for predicting fatigue failure of pre-corroded aluminum alloys according to claim 1, characterized in that, The pre-corrosion region of the target pre-corrosion aluminum alloy specimen is divided into multiple micro-grids. The three-dimensional corrosion morphology and microstructure characteristics of each micro-grid are input into the failure location prediction model to obtain the crack initiation probability of each micro-grid, including: The pre-corrosion area of the target pre-corrosion aluminum alloy specimen is divided into multiple micro-grids, and the three-dimensional corrosion morphology and microstructure features of each micro-grid are extracted respectively. Based on the minimum and maximum feature values determined during the training of the failure location prediction model, the three-dimensional corrosion morphology and microstructure features of the target pre-corroded aluminum alloy specimen are normalized. The normalized three-dimensional corrosion morphology features and microstructure features are input into the failure location prediction model to obtain the crack initiation probability of each microgrid.
10. The method for predicting fatigue failure of pre-corroded aluminum alloys according to claim 1, characterized in that, Select micro-grids where the crack initiation probability exceeds a preset threshold, extract local features of the initiation region corresponding to the selected micro-grids, and take the arithmetic mean of the local features of the initiation region, including: Compare the crack initiation probability of each micro-grid with the preset threshold, and select the micro-grid whose crack initiation probability exceeds the preset threshold; Determine the local maximum grain boundary orientation difference angle, local average Schmidt factor, and local skewness of the selected microgrid area respectively; The arithmetic mean of the local maximum grain boundary orientation difference angle, the local average Schmidt factor, and the local skewness of the selected micro-region grid are respectively taken, and the obtained arithmetic mean is used as the local feature of the initiation region of the target pre-corroded aluminum alloy specimen.