Long-life halogen-free low-smoke class a b1 grade fire-resistant intelligent early warning cable and preparation method

By using copper or aluminum alloy core conductors, double-layer irradiated insulation design, and halogen-free flame-retardant materials in the cable, the problems of cable service life and fire monitoring are solved, achieving long service life, low smoke and non-toxic flame-retardant performance, and real-time early warning effect.

CN123161964APending Publication Date: 2026-11-24ZHEJIANG WANMA CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510669059.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-23
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

The service life of existing cables cannot meet the durability requirements specified in the general building design code, and they cannot achieve real-time monitoring and early warning in the event of a fire, posing a risk of fire spread. Traditional insulation materials are highly toxic and have insufficient flame retardant properties.

Method used

It adopts copper or aluminum alloy core conductors, double-layer irradiated insulation design, combined with halogen-free flame-retardant wrapping layer and sheath layer, with inner and outer insulation material ratio of 3:7. Through dual-channel co-extrusion and irradiation cross-linking technology, a high weather-resistant and high flame-retardant insulation structure is formed, and multimode optical units are embedded in the cable for online temperature measurement.

Benefits of technology

It achieves a long cable life (greater than 70 years), flame retardant performance reaches B1 level, low smoke toxicity and corrosiveness, and can monitor cable temperature in real time and provide early warning, reducing fire risk and cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123161964A_ABST
    Figure CN123161964A_ABST
Patent Text Reader

Abstract

This invention discloses a long-life, halogen-free, low-smoke, Class A, B1-grade fire-resistant intelligent early warning cable and its manufacturing method. The cable is an armored multi-core cable or an unarmored multi-core cable, comprising multiple conductors. Each conductor is covered with a fire-resistant layer, which is then covered with an inner insulation layer. An outer insulation layer is then covered with an outer insulation layer, and a flame-retardant wrapping layer is provided outside the outer insulation layer. A filling material is provided between adjacent outer insulation layers, and multiple multimode optical units are embedded within the filling material. An oxygen barrier layer is provided outside the flame-retardant wrapping layer, and a sheath layer is provided outside the oxygen barrier layer. This invention employs a 3:7 ratio double-layer irradiated insulation design. The product has a long-term operating temperature of 105℃, a maximum linear temperature of 250℃, a design life greater than 70 years, and a theoretical test data analysis life greater than 110 years, meeting the B1 requirements. The combustion droplet / particulate level is not lower than d1, the smoke toxicity level is not lower than t0, and the flame-retardant performance meets the Class A bundled combustion test.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of power cable technology, and relates to Class A B1 fire-resistant cables, and more particularly to a long-life halogen-free low-smoke Class A B1 fire-resistant intelligent early warning cable and its preparation method. Background Technology

[0002] Currently, cross-linked polyethylene (XLPE) insulated power cables and polyvinyl chloride (PVC) insulated power cables are commonly used in the market. The former has an operating temperature of 90 degrees Celsius, which is much higher than the latter's operating temperature of 70 degrees Celsius. However, according to the regular operation and maintenance inspections of various power supply companies, although such products operate normally for 15 to 25 years, the performance of the insulation layer shows a linear decline, posing a potential risk to product quality.

[0003] The service life of currently used cross-linked polyethylene insulated power cables and polyvinyl chloride insulated power cables cannot meet the durability requirements stipulated in the General Code for Design of Civil Buildings. The service life of general buildings is 50-100 years, which cannot meet the requirement that power cables have the same service life as buildings.

[0004] Furthermore, firefighting measures are typically only taken after the cable has already caught fire, especially inside buildings where a cable fire already poses a threat to personal safety. The ability to comprehensively monitor cable operation has been a subject of ongoing research. If continuous monitoring of cables during operation were possible, timely responses to situations such as excessive overload current or sudden temperature increases during short circuits could be implemented, allowing for preventative measures to be taken before a fire ignites, thus avoiding severe consequences.

[0005] There are many reasons why electrical wires and cables can cause fires. For example, electrical wires and cables may age naturally. When electrical wires and cables are overloaded or short-circuited for a long time, and the circuit protection device fails to act in time or cut off the power, the overheating or sparking of the conductors can easily ignite nearby flammable materials.

[0006] There are two main types of commonly used insulation materials in China. One is polyvinyl chloride (PVC) insulation, which has a maximum operating temperature of 70℃, which is relatively low. More importantly, PVC is a toxic material containing chlorine, posing a health hazard. The other is cross-linked polyethylene (XLPE) insulation, which is non-toxic, but its maximum operating temperature is only 90℃, affecting the current carrying capacity of power cables. Both types have a theoretical service life of approximately 32 years, far shorter than the lifespan of important buildings and high-rise buildings.

[0007] Traditional cables struggle to meet the d0 performance of flame retardant B1. In the event of a fire, dripping material from the cable can ignite other flammable materials, causing the fire to spread. Furthermore, the system can only react after the cable has already caught fire, making real-time monitoring and prevention impossible. Summary of the Invention

[0008] To address the aforementioned issues, this invention provides a long-life, halogen-free, low-smoke, Class A, B1-grade fire-resistant intelligent early warning cable and its manufacturing method. The cable uses a copper core, aluminum alloy core, or aluminum core conductor, employs a 3:7 golden ratio double-layer irradiated insulation design, a flame-retardant wrapping layer, a halogen-free flame-retardant inner lining, and a halogen-free irradiated sheath layer. The product has a long-term operating temperature of 105℃, a maximum linear temperature of 250℃, a design life greater than 70 years, and a theoretical test data analysis life greater than 110 years. It meets the B1 requirements of GB31247-2014 "Classification of Combustion Performance of Cables and Optical Fibers," with a combustion droplet / particle level not lower than d1, a smoke toxicity level not lower than t0, and a corrosivity level not lower than a1. Its flame-retardant performance meets the Class A bundled combustion test requirements of GB / T18380-2008 "Combustion Tests of Cables and Optical Fibers under Flame Conditions."

[0009] To achieve the above objectives, the present invention adopts the following technical solution:

[0010] This invention first provides a long-life, halogen-free, low-smoke, Class A, B1-grade fire-resistant intelligent early warning cable. The cable is either an armored multi-core cable or a non-armored multi-core cable. The armored multi-core cable includes multiple conductors, each conductor is covered with a fire-resistant layer, the fire-resistant layer is covered with an inner insulation layer, the inner insulation layer is covered with an outer insulation layer, the outer insulation layer is covered with a flame-retardant wrapping layer, and there is a filler material between adjacent outer insulation layers. The filler material contains multiple multimode optical units, the flame-retardant wrapping layer is covered with an oxygen barrier layer, and the oxygen barrier layer is covered with a sheath layer.

[0011] As a preferred embodiment of the present invention, the unarmored multi-core cable includes multiple conductors, each conductor is covered with a fire-resistant layer, the fire-resistant layer is covered with an inner insulation layer, the inner insulation layer is covered with an outer insulation layer, the outer insulation layer is provided with a first flame-retardant wrapping layer, and a filling material is provided between adjacent outer insulation layers. The filling material contains multiple multimode optical units, the flame-retardant wrapping layer is provided with an oxygen barrier layer, the oxygen barrier layer is covered with an armor layer, the armor layer is covered with a second flame-retardant wrapping layer, and the second flame-retardant wrapping layer is provided with a sheath layer.

[0012] In a preferred embodiment of the present invention, the conductor is a copper core, an aluminum alloy core, or an aluminum core conductor; in the inner insulation layer and the outer insulation layer, the inner insulation layer accounts for 25%-35% and the outer insulation layer accounts for 65%-75%.

[0013] In a preferred embodiment of the present invention, the inner insulation layer comprises, by weight, 25-30 parts of base resin, 4-8 parts of compatibilizer, 1-6.5 parts of lubricant, and 0.5-3 parts of antioxidant; the outer insulation layer comprises, by weight, 25-30 parts of base resin, 4-8 parts of compatibilizer, 0.5-3 parts of lubricant, 55-65 parts of flame retardant, and 3-5 parts of additives.

[0014] In a preferred embodiment of the present invention, the additives include a smoke suppressant, a self-crosslinking agent, and a flame retardant synergist, wherein the mass ratio of the smoke suppressant, the self-crosslinking agent, and the flame retardant synergist is 2-3:0.5-1:5-10; the compatibilizer includes maleic anhydride grafted polymer or SEBS; the flame retardant is ultrafine magnesium hydroxide and / or ultrafine aluminum hydroxide; the flame retardant synergist is 7-n-pentoxy-4,5-dihydro-2H-[1,2,4]-triazoloquinoline-1-one; and the smoke suppressant is zinc borate.

[0015] As a preferred embodiment of the present invention, the raw material of the oxygen barrier layer contains 276.1 parts of ultrafine aluminum hydroxide with a particle size of 1μm-3μm and 137 parts of ultrafine magnesium hydroxide with a particle size of 1μm-3μm; the raw material of the sheath layer contains 0.52 parts of silica and 1.13 parts of ceramicized zinc borate with a particle size of 2μm-4.5μm.

[0016] This invention also provides a method for preparing the above-mentioned long-life halogen-free low-smoke Class A B1 fire-resistant intelligent early warning cable, the method comprising the following steps:

[0017] 1) Conductor: The conductor is a compacted stranded conductor or a profiled conductor with a compaction factor ≥0.92. The conductor material is copper core, aluminum alloy core or aluminum core;

[0018] 2) A refractory layer is formed by wrapping refractory material around the conductor;

[0019] 3) A double-channel, double-layer insulation co-extrusion method is used on the outside of the refractory layer to form an inner insulation layer and an outer insulation layer;

[0020] 4) Halogen-free filler material is used for filling during cabling. The multimode optical units are twisted together with the halogen-free filler material to form a cable, and a flame-retardant wrapping layer is set.

[0021] 5) An oxygen barrier layer is formed on the outside of the flame-retardant wrapping layer, and a sheath layer is formed on the outside of the oxygen barrier layer to obtain an armored multi-core cable.

[0022] Alternatively, step 5) can be replaced with step 5-1): forming an armor layer on the outside of the flame-retardant wrapping layer, forming a second flame-retardant wrapping layer on the outside of the armor layer, and forming a sheath layer on the outside of the second flame-retardant wrapping layer to obtain a non-armored multi-core cable.

[0023] As a preferred embodiment of the present invention, in step 3), the total thickness of the inner insulation layer and the outer insulation layer is 0.7-2.8 mm, the outer insulation layer accounts for 25%-35%, the inner insulation layer accounts for 65%-75%, the extrusion temperature is 140℃-180℃, the screw speed is controlled at 17r / min-25r / min, and crosslinking is performed by 1.5MeV-3.0MeV irradiation.

[0024] In a preferred embodiment of the present invention, in step 3), the melt viscosity ratio between the inner insulating layer and the outer insulating layer is 0.8-1.2; the difference in the linear thermal expansion coefficient of the inner insulating layer is 150-180 ppm / ℃, and the difference in the linear thermal expansion coefficient of the outer insulating layer is 140-170 ppm / ℃.

[0025] As a preferred embodiment of the present invention, in step 3), the crosslinking degree of the inner insulation layer is ≥75%, the crosslinking degree of the outer insulation layer is ≥60%, the irradiation dose of the inner insulation layer is 80kGy, and the irradiation dose of the outer insulation layer is 60kGy.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] 1) This invention utilizes a double insulation layer obtained through co-extrusion of an inner and outer insulation layer. The outer insulation layer (25-35%) bears the responsibility of resisting environmental stress (such as ultraviolet radiation, oxidation, and mechanical abrasion) and serving as a flame-retardant barrier, requiring the selection of materials with high weather resistance and high flame retardancy. A thinner layer can reduce the amount of high-performance materials used, thus lowering costs. The inner insulation layer (65-75%) provides insulation, resistance to bending fatigue, and flexibility, and must ensure a tight fit with the conductor and long-term electrical stability. A thicker inner insulation layer can enhance insulation strength and reduce the risk of leakage.

[0028] 2) In this invention, the flame retardant in the outer insulation layer is densely distributed to form a "protective shell," passing UL 94V-0 or VW-1 testing; the flame retardant synergist in the inner insulation layer slows the spread of flame; and the smoke density (transmittance ≥60%) and toxic gas release are significantly reduced when the inner insulation layer burns. The total cost is reduced by approximately 15%-20% (calculated based on the unit price of the outer insulation layer material being 1.5 times that of the inner insulation layer material), making it suitable for high-volume applications such as medium and high voltage cables.

[0029] 3) The cable of this invention has a long-term operating temperature of 105℃, a maximum line temperature of 250℃, a design life of more than 70 years, and a theoretical test data analysis life of more than 110 years.

[0030] 4) To meet the requirements of building operation and long service life, the cable of this invention uses a 105℃ halogen-free, low-smoke, flame-retardant polyolefin sheath material. This results in a tighter sheath coverage, higher hardness and smoothness, with an irradiation crosslinking degree of no more than 80% and permanent deformation of no more than 11%. After irradiation, the sheath's temperature resistance increases to 105℃, significantly extending its service life. The various physical and mechanical properties of the sheath exceed the requirements of national standards JG / T441 and JG / T442, and its flame-retardant performance meets the requirements of GB / T19666-2019 for flame-retardant Class A, B, or C performance and combustion performance level B1.

[0031] Based on the requirements of the product installation environment, special properties and special occasion requirements such as anti-ant, anti-rodent, anti-ultraviolet, and low temperature resistance (-50℃) can be achieved on the existing basis.

[0032] To achieve online temperature measurement performance of intelligent early warning cables, during the cable fabrication process, halogen-free filler material is used for filling on an active cable laying frame or a cable laying device that ensures that the optical fiber will not be damaged. During filling, the multimode optical unit (monitoring module) must be twisted together with the halogen-free filler material to ensure that the monitoring module will not be damaged. Attached Figure Description

[0033] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0034] Figure 1 This is a schematic diagram of Example 1.

[0035] Figure 2 This is a schematic diagram of Example 2.

[0036] In the figure, 1. Conductor; 2. Fire-resistant layer; 3. Inner insulation layer; 4. Outer insulation layer; 5. Halogen-free filler material; 6. First flame-retardant wrapping layer; 7. Oxygen barrier layer; 8. Multimode optical unit; 9. Sheath layer; 10. Armor layer; 11. Second flame-retardant wrapping layer. Detailed Implementation

[0037] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0038] This invention provides a long-life, halogen-free, low-smoke, Class A, B1-grade fire-resistant intelligent early warning cable, wherein the cable is an armored multi-core cable or an unarmored multi-core cable.

[0039] See Figure 1 The armored multi-core cable includes multiple conductors 1, each conductor 1 is covered with a fire-resistant layer 2, the fire-resistant layer 2 is covered with an inner insulation layer 3, the inner insulation layer 3 is covered with an outer insulation layer 4, the outer insulation layer 4 is provided with a first flame-retardant wrapping layer 6, the gaps between adjacent outer insulation layers 4 are provided with halogen-free filling material 5, the halogen-free filling material 5 is provided with multiple multimode optical units 8, the first flame-retardant wrapping layer 6 is provided with an oxygen barrier layer 7, and the oxygen barrier layer 7 is provided with a sheath layer 9.

[0040] See Figure 2 The unarmored multi-core cable includes multiple conductors 1, each conductor 1 is covered with a fire-resistant layer 2, the fire-resistant layer 2 is covered with an inner insulation layer 3, the inner insulation layer 3 is covered with an outer insulation layer 4, the outer insulation layer 4 is provided with a first flame-retardant wrapping layer 6, the gaps between adjacent outer insulation layers 4 are provided with halogen-free filling material 5, the halogen-free filling material 5 is provided with multiple multimode optical units 8, the first flame-retardant wrapping layer 6 is provided with an oxygen barrier layer 7, the oxygen barrier layer 7 is covered with an armor layer 10, the armor layer 10 is covered with a second flame-retardant wrapping layer 11, the second flame-retardant wrapping layer 11 is provided with a sheath layer 9.

[0041] In this invention, the conductor material is copper core, aluminum alloy core, or aluminum core, and it is a compacted stranded conductor or a profiled conductor. The compaction coefficient of the conductor reaches 0.92 or higher, and the DC resistance of the conductor at 20°C does not exceed the specification of GB / T3956. The conductor preparation is a common existing technology in this field, and therefore will not be described in detail.

[0042] To improve the service life of cables, this invention uses halogen-free flame-retardant polyolefin insulation material at 105℃. This material is halogen-free, non-toxic, environmentally friendly, and has excellent flame-retardant and insulation properties. The inner insulation layer, by weight, comprises 25-30 parts of base resin, 4-8 parts of compatibilizer, 1-6.5 parts of lubricant, and 0.5-3 parts of antioxidant. The outer insulation layer, by weight, comprises 25-30 parts of base resin, 4-8 parts of compatibilizer, 0.5-3 parts of lubricant, 55-65 parts of flame retardant, and 3-5 parts of additives.

[0043] The additives include smoke suppressants, self-crosslinking agents, and flame retardant synergists. The mass ratio of smoke suppressants, self-crosslinking agents, and flame retardant synergists is 2-3:0.5-1:5-10. The flame retardant synergist is 7-n-pentoxy-4,5-dihydro-2H-[1,2,4]-triazoloquinoline-1-one. The smoke suppressant is zinc borate.

[0044] Compatibilizers include maleic anhydride graft polymers or SEBS.

[0045] The flame retardant is ultrafine magnesium hydroxide and / or ultrafine aluminum hydroxide.

[0046] The insulation layer is manufactured using a dual-flow-channel, double-layer co-extrusion method. The insulation layer thickness is controlled between 0.70mm and 2.8mm. The process requirements are: the insulation uses a 25-35:65-75 ratio (double-layer co-extruded halogen-free low-smoke polyolefin insulation material with inner and outer insulation layer thicknesses of 25-35:65-75 (thinner outer layer and thicker inner layer).

[0047] In this invention, the outer insulation layer (25-35%) primarily serves as a resistance barrier against environmental stresses (such as ultraviolet radiation, oxidation, and mechanical wear) and a flame-retardant barrier, requiring the selection of materials with high weather resistance and high flame retardancy. A thinner layer reduces the amount of high-performance materials used, thus lowering costs.

[0048] Inner insulation layer (65-75%): Primarily responsible for insulation and flexibility, it must ensure a tight fit with the conductor and long-term electrical stability. A thicker inner insulation layer can enhance insulation strength and reduce the risk of leakage.

[0049] Considering cost and performance, the optimal ratio of the outer insulation layer to the inner insulation layer in this invention is 30% for the outer insulation layer and 70% for the inner insulation layer.

[0050] When the outer insulation layer uses a high-fill flame-retardant system (such as magnesium hydroxide / aluminum), excessive thickness can lead to poor processing fluidity and rough surface; a 3:7 ratio can balance flame-retardant efficiency and processability.

[0051] The inner insulation layer uses a low-smoke formulation (such as phosphorus and nitrogen flame retardants), and the thicker structure can reduce the escape rate of internal pyrolysis gases during combustion and delay smoke generation (meeting the low-smoke requirements of GB / T 18380.3).

[0052] The cost of using high-performance additives (such as UV inhibitors and scratch-resistant agents) in the outer insulation layer is relatively high. The total cost can be significantly reduced by thinning the proportion (30%).

[0053] The inner insulation layer is mainly composed of base resin (70%), which utilizes the natural flexibility and low cost advantages of polyolefins to improve economic efficiency.

[0054] During co-extrusion of two layers, the viscosity difference between the inner and outer insulation layers must be matched. A thinner outer layer and a thicker inner layer (3:7) can prevent uneven coating or interfacial delamination caused by excessively fast melt flow in the outer insulation layer.

[0055] For example, the outer insulation layer uses a high-viscosity flame-retardant formulation (requiring higher extrusion pressure), and a thinner thickness can reduce the impact on equipment load.

[0056] Mechanical properties: The thick inner insulation layer provides flexibility and resistance to bending fatigue (such as improved pass rate in dynamic flexural tests), while the thin outer insulation layer maintains surface hardness (Shore hardness can reach 90A or higher).

[0057] Flame retardant effect: The outer insulation layer has a dense distribution of flame retardant to form a "protective shell", which passes UL 94V-0 or VW-1 testing; the inner insulation layer has a flame retardant synergist to delay the spread of flame.

[0058] Low smoke characteristics: The inner insulation layer has a high proportion of low smoke formulation, which significantly reduces smoke density (transmittance ≥60%) and the release of toxic gases during combustion.

[0059] Reducing the thickness of the outer insulation layer can decrease the impact of high-fill flame-retardant systems on screw wear (e.g., when the magnesium hydroxide filling amount is >50%, an excessively thick outer insulation layer can easily lead to extrusion fluctuations). Optimizing the interfacial bonding strength avoids delamination or peeling caused by excessive thickness differences (peeling force ≥5N / mm).

[0060] The total cost is reduced by approximately 15%-20% (calculated based on the unit price of the outer insulation material being 1.5 times that of the inner insulation material), making it suitable for high-volume applications such as medium and high voltage cables.

[0061] The double-layer co-extrusion insulation process of the present invention is as follows:

[0062] Material compatibility: Ensure that the viscosity, polarity, and coefficient of thermal expansion of the inner insulation layer (such as cross-linked polyethylene, XLPE) and the outer insulation layer (such as low-smoke halogen-free flame retardant material) are matched to avoid delamination or interface defects.

[0063] 1. Melt viscosity ratio (inner insulation layer: outer insulation layer) ideal range: 0.8-1.2 (test conditions: 200℃, shear rate 1000 / s).

[0064] 2. Polarity matching requirements: The allowable range for the surface energy difference (outer insulation layer - inner insulation layer) is ≤5mN / m (measured by the contact angle method or pendant drop method).

[0065] Inner insulation layer (XLPE): surface energy approximately 28-32 mN / m; outer insulation layer (halogen-free flame-retardant material): surface energy needs to be controlled at 30-35 mN / m.

[0066] Difference in linear thermal expansion coefficient (CLTE)

[0067] Permissible difference: ≤10% (test temperature range -40℃ to 120℃).

[0068] Inner insulation layer (XLPE): CLTE 150-180ppm / ℃; Outer insulation layer (halogen-free flame retardant material): CLTE needs to be controlled at 140-170ppm / ℃.

[0069] Adjust the melt flow index (MI value) of the two materials to make the flow rates of the inner and outer insulation layer materials similar during extrusion, thus ensuring uniform thickness.

[0070] Inner insulation layer: Focus on electrical insulation performance and temperature resistance (e.g., adding antioxidants). Outer insulation layer: Focus on mechanical strength and resistance to environmental aging (e.g., adding UV absorbers and flame retardants).

[0071] Co-extrusion process parameters

[0072] Temperature control: (Extrusion temperature 140℃-180℃). The temperature gradient of each section of the extruder needs to be precisely controlled to avoid material degradation. The die temperature needs to balance the flowability of the two materials; generally, the temperature of the outer insulation layer is slightly lower than that of the inner insulation layer (temperature difference 5-10℃).

[0073] Extrusion speed: (screw speed controlled between 17 r / min and 25 r / min), the extrusion speeds of the inner and outer insulation layers must be synchronized (error).

[0074] <2%), precise control can be achieved through a servo motor. Adjust the screw speed and traction speed to ensure the concentricity of the insulation layer (deviation <5%).

[0075] Mold design: Use a dual-channel die head (such as a co-extrusion ring die head), optimize the channel length ratio (L / D) (usually 10:1-15:1), set up flow-blocking rings or guide channels to reduce interface turbulence and improve interlayer bonding.

[0076] Online detection and feedback use a laser diameter gauge to monitor the insulation layer thickness in real time (accuracy ±0.01mm), and an infrared thermal imager to monitor the temperature distribution on the extruded surface to prevent local overheating.

[0077] Irradiation crosslinking process:

[0078] Dosage optimization: Calculate the absorbed dose (typically 1.5 MeV-3.0 MeV radiation) based on material thickness and density. For double-layer structures, calculations must be performed layer by layer: the dose penetration of the inner insulation layer must meet a cross-linking degree ≥70%, and the outer insulation layer should avoid over-irradiation (Monte Carlo simulation of dose distribution can be used).

[0079] Dose rate control: Electron beam energy selection (commonly 1.5-3 MeV), excessive energy can easily lead to surface over-crosslinking. Beam current density uniformity adjustment (non-uniformity <5%), using multi-faceted irradiation or rotating devices.

[0080] Irradiation environment: Inert gas (such as nitrogen) protection to reduce oxidation side reactions. Control the irradiation chamber temperature (<40℃) to prevent heat accumulation that could lead to material deformation.

[0081] Crosslinking degree and performance balance

[0082] Crosslinking degree test:

[0083] Crosslinking degree is monitored using the gel content method (ASTM D2765) or the thermal stretching method (IEC 60811). Target values: crosslinking degree of inner insulation layer ≥75%, and crosslinking degree of outer insulation layer ≥60% (while also considering flexibility).

[0084] Performance matching: Inner insulation layer: Improves dielectric strength (≥30kV / mm) and heat distortion temperature (≥120℃). Outer insulation layer: Maintains elongation at break (≥200%) and resistance to environmental stress cracking (≥1000h).

[0085] Extrusion-irradiation speed matching: The production line speed (V) and irradiation dose rate (D) satisfy: D = P / (V·W), where P is the beam power and W is the irradiation width. In this invention, the line speed is 10-30 m / min, and the beam power is 20-50 kW. After the above irradiation crosslinking control, the insulation coating is tighter, and the compatibility of the insulation layer is better with the blending of compatibilizers and additives. The physical and mechanical properties do not decay. The crosslinking degree of the inner insulation layer is ≥75%, and that of the outer insulation layer is ≥60% (while also considering flexibility). The permanent deformation is no more than 11%. The temperature resistance of the insulation after irradiation is increased to 105℃, which greatly extends the breakdown strength and service life of the insulation layer.

[0086] Flame-retardant wrapping layer design and manufacturing process: To meet the requirements of building flame retardancy ratings of Class A, B or C and combustion performance reaching Class B1 operating environment, the product uses single-sided hot-melt halogen-free high flame-retardant tape with the adhesive side facing outwards for wrapping. The thickness is not less than 1 layer and not more than 3 layers, with an overlap rate of not less than 10% and not more than 25%. It is tightly bonded to the outer extruded sheath layer, and the contact area with the inner insulation layer of the outer sheath reaches 100%. The peel strength with the sheath is not less than 0.9 N / mm.

[0087] Design and manufacturing process of oxygen barrier and sheath: To meet the requirements of building operation and long service life, halogen-free low-smoke flame-retardant polyolefin sheath material is used. The flame retardant of this material is a mixed flame retardant, in which the ratio of ultrafine aluminum hydroxide with a particle size of 1μm-3μm and ultrafine magnesium hydroxide is 276.1 and 137, respectively, giving the product excellent flame-retardant and self-extinguishing properties.

[0088] Adding 0.52 parts of low-ratio silica and 1.13 parts of ceramicized zinc borate with a particle size of 2μm-4.5μm to the sheath layer achieves excellent flame-retardant crusting performance.

[0089] The extrusion temperature of the sheath layer is 140℃-180℃, and the screw speed is controlled at 17r / min-25r / min. After cross-linking by 1.5MeV-3.0MeV irradiation, the sheath layer has tighter coverage, higher hardness and smoothness, with a cross-linking degree of no more than 80% and permanent deformation of no more than 11%. The temperature resistance of the sheath layer after irradiation increases to 105℃, greatly extending its service life. The various physical and mechanical properties of the sheath layer are superior to the requirements of national standards JG / T441 and JG / T442, and its flame retardant performance can meet the requirements of flame retardant class A, B or C and combustion performance B1 level specified in GB / T19666-2019.

[0090] Based on the requirements of the product installation environment, special properties and special occasion requirements such as anti-ant, anti-rodent, anti-ultraviolet, and low temperature resistance (-50℃) can be achieved on the existing basis.

[0091] To achieve online temperature measurement performance of intelligent early warning cables, this invention employs a halogen-free filler material during the cable fabrication process. This material is used on an active cable laying frame or a cable laying device that ensures the optical fiber is not damaged. During the filling process, the multimode optical unit (monitoring module) is twisted together with the halogen-free filler material to ensure that the monitoring module is not damaged.

[0092] The multimode optical unit (monitoring module), in conjunction with terminal equipment and software, enables real-time online temperature monitoring, timely feedback of temperature changes, and alarms for abnormal temperature fluctuations, preventing cable faults and potential serious accidents such as fires. (Multimode optical cables should comply with the relevant provisions of "Multimode Optical Fiber for Communication" (GB / T 12357), and single-mode optical cables should comply with the relevant provisions of "Single-mode Optical Fiber for Communication" (GB / T 9771). Multimode optical cables are generally preferred.)

[0093] The main technical requirements for multimode optical units (monitoring modules) (attenuation of temperature measurement fiber optic channels) are as follows: maximum attenuation of 850nm wavelength fiber is no more than 2.5dB / km; maximum attenuation of 980nm wavelength fiber is no more than 0.5dB / km; maximum attenuation of 1300nm wavelength fiber is no more than 0.8dB / km; maximum attenuation of 1550nm wavelength fiber is no more than 0.3dB / km; and maximum single-point loss should not exceed 0.1dB.

[0094] The intelligent early warning cable system is a solution that integrates power transmission, communication, vibration, and cable temperature rise monitoring. It is equipped with a DAS vibration monitoring system and a DTS temperature measurement system to monitor the cable operating temperature and the surrounding environment in real time, playing a role in load monitoring, fault alarm location, and fire prevention.

[0095] Example 1

[0096] See Figure 1The cable provided in this embodiment is an armored multi-core cable including multiple conductors 1. Each conductor 1 is covered with a fire-resistant layer 2. The fire-resistant layer 2 is covered with an inner insulation layer 3. The inner insulation layer 3 is covered with an outer insulation layer 4. The outer insulation layer 4 is provided with a first flame-retardant wrapping layer 6. The gaps between adjacent outer insulation layers 4 are provided with halogen-free filling material 5. The halogen-free filling material 5 is provided with multiple multimode optical units 8. The first flame-retardant wrapping layer 6 is provided with an oxygen barrier layer 7. The oxygen barrier layer 7 is provided with a sheath layer 9.

[0097] The insulation material is halogen-free flame-retardant polyolefin insulation material with a temperature of 105℃. It is halogen-free, non-toxic, and environmentally friendly, and has excellent flame-retardant and insulation properties. The raw materials of the inner insulation layer are, by weight, 28.5 parts of the base resin ethylene-vinyl acetate copolymer, 6.5 parts of maleic anhydride graft polymer, 1 part of antioxidant 1010, and 1 part of lubricant silicone masterbatch.

[0098] The raw materials for the outer insulation layer, by weight, are: 28.5 parts of the base resin ethylene-vinyl acetate copolymer, 6.5 parts of maleic anhydride graft polymer, 1 part of antioxidant 1010, 1 part of lubricant silicone masterbatch, 61 parts of flame retardant 1μm-3μm ultrafine magnesium hydroxide, and 3.5 parts of additives.

[0099] The additives include smoke suppressant, self-crosslinking agent and flame retardant synergist, with a mass ratio of 2:1:4; the flame retardant synergist is 7-n-pentoxy-4,5-dihydro-2H-[1,2,4]-triazoloquinoline-1-one; the smoke suppressant is zinc borate.

[0100] The insulation layer is manufactured using a dual-flow-channel, double-layer co-extrusion method. The insulation layer thickness is controlled between 0.70mm and 2.8mm. The process requirements are: the insulation uses a 30:70 ratio (double-layer co-extruded halogen-free low-smoke polyolefin insulation material with inner and outer insulation layer thicknesses of 25-35:65-75 (thinner outer layer and thicker inner layer)).

[0101] The raw materials for the oxygen barrier layer include 276.1 parts of ultrafine aluminum hydroxide with a particle size of 1μm-3μm and 137 parts of ultrafine magnesium hydroxide with a particle size of 1μm-3μm.

[0102] The raw material of the sheath layer contains 0.52 parts of silica and 1.13 parts of ceramicized zinc borate with a particle size of 2μm-4.5μm.

[0103] The preparation method is as follows:

[0104] 1) Conductor (a common existing technology in this field): The conductor is a compacted stranded conductor or a profiled conductor with a compaction coefficient ≥0.92 and the conductor material is copper core, aluminum alloy core or aluminum core.

[0105] 2) A refractory layer is formed by wrapping refractory material around the conductor (a common existing technology in this field). The refractory layer material can be mica tape, ceramicized silicone rubber tape, or ceramicized mica tape, etc., and passes the fire resistance test specified in GB / T19666 standard.

[0106] 3) A double-channel double-layer insulation co-extrusion method is used on the outside of the fire-resistant layer to form an inner insulation layer (based on LDPE resin) and an outer insulation layer (based on EVA resin).

[0107] A co-extrusion annular die is used, with a flow channel length ratio (L / D) of 10:1. Flow-blocking rings or guide grooves are set to reduce interfacial turbulence and improve interlayer bonding.

[0108] The extrusion temperature is 140℃-180℃, the screw speed is controlled at 17r / min-25r / min, and it is cross-linked by 1.5MeV-3.0MeV irradiation. The cross-linking degree of the inner insulation layer is ≥75%, and the cross-linking degree of the outer insulation layer is ≥60%.

[0109] The production line speed is 20m / min, the beam power is 30kW, the irradiation dose of the inner insulation layer is 80kGy, and the irradiation dose of the outer insulation layer is 60kGy.

[0110] The total thickness of the inner and outer insulation layers is 0.7-2.8 mm, with the outer insulation layer accounting for 30% and the inner insulation layer accounting for 70%.

[0111] 4) Halogen-free filler material is used for filling during cabling. The multimode optical units are twisted together with the halogen-free filler material to form a cable, and a flame-retardant wrapping layer is set. This step is a common existing technology in this field.

[0112] 5) An oxygen barrier layer is formed on the outside of the flame-retardant wrapping layer, and a sheath layer is formed on the outside of the oxygen barrier layer to obtain an armored multi-core cable. The raw material of the oxygen barrier layer contains 276.1 parts of ultrafine aluminum hydroxide with a particle size of 1μm-3μm and 137 parts of ultrafine magnesium hydroxide with a particle size of 1μm-3μm.

[0113] The raw material of the sheath layer contains 0.52 parts of silica and 1.13 parts of ceramicized zinc borate with a particle size of 2μm-4.5μm.

[0114] The extrusion temperature of the sheath layer is 140℃-180℃, the screw speed is controlled at 17r / min-25r / min, and it is cross-linked by 1.5MeV-3.0MeV radiation.

[0115] Example 2

[0116] See Figure 2The cable in this embodiment is a non-armored multi-core cable, including multiple conductors 1. Each conductor 1 is covered with a fire-resistant layer 2. The fire-resistant layer 2 is covered with an inner insulation layer 3. The inner insulation layer 3 is covered with an outer insulation layer 4. The outer insulation layer 4 is provided with a first flame-retardant wrapping layer 6. The gaps between adjacent outer insulation layers 4 are provided with halogen-free filling material 5. Multiple multimode optical units 8 are provided in the halogen-free filling material 5. The first flame-retardant wrapping layer 6 is provided with an oxygen barrier layer 7. The oxygen barrier layer 7 is covered with an armor layer 10. The armor layer 10 is covered with a second flame-retardant wrapping layer 11. The second flame-retardant wrapping layer 11 is provided with a sheath layer 9.

[0117] The insulation material is halogen-free flame-retardant polyolefin insulation material with a temperature of 105℃. It is halogen-free, non-toxic, and environmentally friendly, and has excellent flame-retardant and insulation properties. The raw materials of the inner insulation layer are, by weight, 28.5 parts of the base resin ethylene-vinyl acetate copolymer, 6.5 parts of maleic anhydride graft polymer, 1 part of antioxidant 1010, and 1 part of lubricant silicone masterbatch.

[0118] The raw materials for the outer insulation layer, by weight, are: 28.5 parts of the base resin ethylene-vinyl acetate copolymer, 6.5 parts of maleic anhydride graft polymer, 1 part of antioxidant 1010, 1 part of lubricant silicone masterbatch, 61 parts of flame retardant 1μm-3μm ultrafine magnesium hydroxide, and 3.5 parts of additives.

[0119] The additives include smoke suppressant, self-crosslinking agent and flame retardant synergist, with a mass ratio of 2:1:4; the flame retardant synergist is 7-n-pentoxy-4,5-dihydro-2H-[1,2,4]-triazoloquinoline-1-one; the smoke suppressant is zinc borate.

[0120] The insulation layer is manufactured using a dual-flow-channel, double-layer co-extrusion method. The insulation layer thickness is controlled between 0.70mm and 2.8mm. The process requirements are: the insulation uses a 30:70 ratio (double-layer co-extruded halogen-free low-smoke polyolefin insulation material with inner and outer insulation layer thicknesses of 25-35:65-75 (thinner outer layer and thicker inner layer)).

[0121] The raw materials for the oxygen barrier layer include 276.1 parts of ultrafine aluminum hydroxide with a particle size of 1μm-3μm and 137 parts of ultrafine magnesium hydroxide with a particle size of 1μm-3μm.

[0122] The raw material of the sheath layer contains 0.52 parts of silica and 1.13 parts of ceramicized zinc borate with a particle size of 2μm-4.5μm.

[0123] The preparation method is as follows:

[0124] 1) Conductor (a common existing technology in this field): The conductor is a compacted stranded conductor or a profiled conductor with a compaction coefficient ≥0.92 and the conductor material is copper core, aluminum alloy core or aluminum core.

[0125] 2) A refractory layer is formed by wrapping refractory material around the conductor (a common existing technology in this field). The refractory layer material can be mica tape, ceramicized silicone rubber tape, or ceramicized mica tape, etc., and passes the fire resistance test specified in GB / T19666 standard.

[0126] 3) A double-channel double-layer insulation co-extrusion method is used on the outside of the fire-resistant layer to form an inner insulation layer (based on LDPE resin) and an outer insulation layer (based on EVA resin).

[0127] A co-extrusion annular die is used, with a flow channel length ratio (L / D) of 10:1. Flow-blocking rings or guide grooves are set to reduce interfacial turbulence and improve interlayer bonding.

[0128] The extrusion temperature is 140℃-180℃, the screw speed is controlled at 17r / min-25r / min, and it is cross-linked by 1.5MeV-3.0MeV irradiation. The cross-linking degree of the inner insulation layer is ≥75%, and the cross-linking degree of the outer insulation layer is ≥60%.

[0129] The production line speed is 20m / min, the beam power is 30kW, the irradiation dose of the inner insulation layer is 80kGy, and the irradiation dose of the outer insulation layer is 60kGy.

[0130] The total thickness of the inner and outer insulation layers is 0.7-2.8 mm, with the outer insulation layer accounting for 30% and the inner insulation layer accounting for 70%.

[0131] 4) Halogen-free filler material is used for filling during cabling. The multimode optical units are twisted together with the halogen-free filler material to form a cable, and a flame-retardant wrapping layer is set. This step is a common existing technology in this field.

[0132] 5) An oxygen barrier layer is formed on the outside of the flame-retardant wrapping layer, and a sheath layer is formed on the outside of the oxygen barrier layer to obtain an armored multi-core cable. The raw material of the oxygen barrier layer contains 276.1 parts of ultrafine aluminum hydroxide with a particle size of 1μm-3μm and 137 parts of ultrafine magnesium hydroxide with a particle size of 1μm-3μm.

[0133] The raw material of the sheath layer contains 0.52 parts of silica and 1.13 parts of ceramicized zinc borate with a particle size of 2μm-4.5μm.

[0134] The extrusion temperature of the sheath layer is 140℃-180℃, the screw speed is controlled at 17r / min-25r / min, and it is cross-linked by 1.5MeV-3.0MeV radiation.

[0135] The cable product of this invention can operate at a long-term temperature of 105℃, with a maximum line temperature of 250℃, a design life of over 70 years, and a theoretical test data analysis life of over 110 years, providing a reliable guarantee for the safe and stable operation of the product. Based on existing specifications, the product can be customized to meet the requirements of the laying environment, achieving special properties such as termite prevention, rodent prevention, UV protection, and low-temperature resistance (-45℃).

[0136] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any form or substance. It should be noted that those skilled in the art can make various improvements and additions without departing from the method of the present invention, and these improvements and additions should also be considered within the scope of protection of the present invention. Any modifications, alterations, and equivalent changes made by those skilled in the art based on the above-disclosed technical content without departing from the spirit and scope of the present invention are equivalent embodiments of the present invention. Furthermore, any modifications, alterations, and evolutions made to the above embodiments based on the essential technology of the present invention still fall within the scope of the technical solution of the present invention.

Claims

1. A long-life, halogen-free, low-smoke, Class A, B1-grade fire-resistant intelligent early warning cable, characterized in that... The cable is either an armored multi-core cable or an unarmored multi-core cable. The armored multi-core cable includes multiple conductors, each conductor is covered with a fire-resistant layer, the fire-resistant layer is covered with an inner insulation layer, the inner insulation layer is covered with an outer insulation layer, the outer insulation layer is covered with a flame-retardant wrapping layer, and there is a filler material between adjacent outer insulation layers. The filler material contains multiple multimode optical units, the flame-retardant wrapping layer is covered with an oxygen barrier layer, and the oxygen barrier layer is covered with a sheath layer.

2. The long-life halogen-free, low-smoke, Class A, B1 fire-resistant intelligent early warning cable according to claim 1, characterized in that, The unarmored multi-core cable includes multiple conductors, each conductor is covered with a fire-resistant layer, the fire-resistant layer is covered with an inner insulation layer, the inner insulation layer is covered with an outer insulation layer, the outer insulation layer is covered with a first flame-retardant wrapping layer, adjacent outer insulation layers are filled with a filling material, the filling material contains multiple multimode optical units, the flame-retardant wrapping layer is covered with an oxygen barrier layer, the oxygen barrier layer is covered with an armor layer, the armor layer is covered with a second flame-retardant wrapping layer, and the second flame-retardant wrapping layer is covered with a sheath layer.

3. The long-life halogen-free, low-smoke, Class A, B1 fire-resistant intelligent early warning cable according to claim 1 or 2, characterized in that, The conductor is a copper core, an aluminum alloy core, or an aluminum core conductor; in the inner insulation layer and the outer insulation layer, the outer insulation layer accounts for 25%-35% and the inner insulation layer accounts for 65%-75%.

4. The long-life halogen-free, low-smoke, Class A, B1 fire-resistant intelligent early warning cable according to claim 1 or 2, characterized in that, The inner insulation layer comprises, by weight, 25-30 parts of base resin, 4-8 parts of compatibilizer, 1-6.5 parts of lubricant, and 0.5-3 parts of antioxidant. The outer insulation layer comprises, by weight, 25-30 parts of base resin, 4-8 parts of compatibilizer, 0.5-3 parts of lubricant, 55-65 parts of flame retardant, and 3-5 parts of additives.

5. The long-life halogen-free, low-smoke, Class A, B1 fire-resistant intelligent early warning cable according to claim 4, characterized in that, The additives include a smoke suppressant, a self-crosslinking agent, and a flame retardant synergist, with a mass ratio of 2-3:0.5-1:5-10. The compatibilizer includes maleic anhydride grafted polymer or SEBS. The flame retardant is ultrafine magnesium hydroxide and / or ultrafine aluminum hydroxide. The flame retardant synergist is 7-n-pentoxy-4,5-dihydro-2H-[1,2,4]-triazoloquinoline-1-one. The smoke suppressant is zinc borate.

6. The long-life halogen-free, low-smoke, Class A, B1 fire-resistant intelligent early warning cable according to claim 1 or 2, characterized in that, The raw materials of the oxygen barrier layer include 276.1 parts of ultrafine aluminum hydroxide with a particle size of 1μm-3μm and 137 parts of ultrafine magnesium hydroxide with a particle size of 1μm-3μm; the raw materials of the sheath layer include 0.52 parts of silica and 1.13 parts of ceramicized zinc borate with a particle size of 2μm-4.5μm.

7. A method for preparing a long-life, halogen-free, low-smoke, Class A, B1 fire-resistant intelligent early warning cable, characterized in that, The preparation method includes the following steps: 1) Conductor: The conductor is a compacted stranded conductor or a profiled conductor with a compaction factor ≥0.

92. The conductor material is copper core, aluminum alloy core or aluminum core; 2) A refractory layer is formed by wrapping refractory material around the conductor; 3) A double-channel, double-layer insulation co-extrusion method is used on the outside of the refractory layer to form an inner insulation layer and an outer insulation layer; 4) Halogen-free filler material is used for filling during cabling. The multimode optical units are twisted together with the halogen-free filler material to form a cable, and a flame-retardant wrapping layer is set. 5) An oxygen barrier layer is formed on the outside of the flame-retardant wrapping layer, and a sheath layer is formed on the outside of the oxygen barrier layer to obtain an armored multi-core cable. Alternatively, step 5) can be replaced with step 5-1): forming an armor layer on the outside of the flame-retardant wrapping layer, forming a second flame-retardant wrapping layer on the outside of the armor layer, and forming a sheath layer on the outside of the second flame-retardant wrapping layer to obtain a non-armored multi-core cable.

8. The method for preparing a long-life halogen-free, low-smoke, Class A, B1 fire-resistant intelligent early warning cable according to claim 7, characterized in that, In step 3), the total thickness of the inner and outer insulation layers is 0.7-2.8 mm, the outer insulation layer accounts for 25%-35%, the inner insulation layer accounts for 65%-75%, the extrusion temperature is 140℃-180℃, the screw speed is controlled at 17r / min-25r / min, and crosslinking is performed by 1.5MeV-3.0MeV irradiation.

9. The method for preparing a long-life halogen-free, low-smoke, Class A, B1 fire-resistant intelligent early warning cable according to claim 7, characterized in that, In step 3), the melt viscosity ratio between the inner insulation layer and the outer insulation layer is 0.8-1.2; the difference in the linear thermal expansion coefficient of the inner insulation layer is 150-180 ppm / ℃, and the difference in the linear thermal expansion coefficient of the outer insulation layer is 140-170 ppm / ℃.

10. The method for preparing a long-life halogen-free, low-smoke, Class A, B1 fire-resistant intelligent early warning cable according to claim 7, characterized in that, In step 3), the crosslinking degree of the inner insulation layer is ≥75%, the crosslinking degree of the outer insulation layer is ≥60%, the irradiation dose of the inner insulation layer is 80 kGy, and the irradiation dose of the outer insulation layer is 60 kGy.