Low-temperature-resistant and weather-resistant cable and preparation method thereof
By combining modifiers and specific materials, low-temperature and weather-resistant cables are prepared, solving the problem of reduced cable flexibility in low-temperature environments and achieving reliability and safety in harsh low-temperature environments.
Patent Information
- Application Number
- CN202611398815.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-09
- Publication Date
- 2026-11-24
AI Technical Summary
Existing cables exhibit significantly reduced flexibility in low-temperature environments, making them prone to insulation cracking and sheath damage, thus failing to meet the stringent requirements of low-temperature applications.
The insulation layer is made of synergistic effect of dioctyl adipate and long-chain acrylic acid ester grafted with nitrile rubber, and the outer sheath uses polyether-type TPU and bis(4-aminocyclohexyl) ether materials. The low-temperature and weather-resistant cable is prepared by stranding and melt extrusion processes.
It improves the low-temperature resistance of the cable, enhances the flexibility of the insulation layer and outer sheath, reduces rigidity, and meets the requirements of low-temperature environments from -40℃ to -55℃.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention belongs to the field of cable technology, specifically relating to a low-temperature resistant and weather-resistant cable and its preparation method. Background Technology
[0002] When cables operate in extremely cold regions (such as high altitudes and polar regions), outdoors in winter, or in cold storage environments, the movement of molecular chains in their polymer components (especially the insulation and outer sheath) is hindered, causing the material to transition from a highly elastic state to a glassy state. This results in a significant decrease in flexibility and an increase in brittleness. Under laying, movement, or external mechanical stress, cables are highly susceptible to insulation cracking and sheath damage, leading to safety accidents such as short circuits and leakage. Furthermore, repeated thermal expansion and contraction caused by diurnal temperature variations accelerate material fatigue, affecting the long-term reliability of the cable. The low-temperature performance of existing ordinary cables typically only meets general national standards (such as cold impact / bending tests at -15℃ or -25℃), making it difficult to meet the application requirements of more stringent low-temperature scenarios (such as -40℃ or even -55℃). Therefore, improving the low-temperature resistance of cables has become an urgent technical problem to be solved in this field. Summary of the Invention
[0003] The purpose of this invention is to provide a low-temperature resistant and weather-resistant cable and its manufacturing method. The cable provided by this invention possesses excellent low-temperature and weather-resistant properties.
[0004] To achieve the above-mentioned objectives, the present invention provides the following technical solution: This invention provides a low-temperature and weather-resistant cable, comprising, from the inside out, a core assembly, a wrapping layer, an armor layer, and an outer sheath; a filler is disposed between the core assembly and the wrapping layer; The cable core assembly is composed of multiple cable cores twisted together; The cable core includes a conductor and an insulation layer arranged sequentially from the inside out; The insulating layer, by weight, is prepared from the following raw materials: 80-100 parts of low-density polyethylene, 10-20 parts of modifier, 5-10 parts of filler, 1-2 parts of silane coupling agent, 1-3 parts of crosslinking agent, 0.5-2 parts of antioxidant, and 0.1-0.5 parts of compatibilizer; the modifier includes dioctyl adipate and long-chain acrylate grafted with nitrile rubber. The outer protective layer is prepared from the following raw materials by mass: 80-100 parts of polyvinyl chloride, 5-10 parts of toughening agent, 5-10 parts of plasticizer, 0.1-0.5 parts of heat stabilizer, 1-5 parts of lubricant, 20-30 parts of filler and 0.5-2 parts of antioxidant; the toughening agent includes polyether-type TPU and bis(4-aminocyclohexyl) ether.
[0005] Preferably, the insulating layer is prepared from the following raw materials in parts by weight: 85-95 parts of low-density polyethylene, 12-18 parts of modifier, 6-9 parts of filler, 1-2 parts of silane coupling agent, 1-2 parts of crosslinking agent, 1-1.5 parts of antioxidant and 0.2-0.4 parts of compatibilizer.
[0006] Preferably, the mass ratio of dioctyl adipate to long-chain acrylate grafted with nitrile rubber is 1:(2~4).
[0007] Preferably, the mass ratio of dioctyl adipate to long-chain acrylate grafted with nitrile rubber is 1:3.
[0008] Preferably, the thickness of the insulating layer is 0.6~4mm.
[0009] Preferably, the outer protective layer is prepared from the following raw materials in parts by weight: 85-95 parts of polyvinyl chloride, 6-9 parts of toughening agent, 6-9 parts of plasticizer, 0.2-0.4 parts of heat stabilizer, 2-4 parts of lubricant, 22-28 parts of filler and 1-1.5 parts of antioxidant.
[0010] Preferably, the mass ratio of the polyether-type TPU to bis(4-aminocyclohexyl) ether is (1~3):1.
[0011] Preferably, the mass ratio of the polyether-type TPU to the bis(4-aminocyclohexyl) ether is 2:1.
[0012] Preferably, the thickness of the outer protective layer is 1.5~3mm.
[0013] Preferably, the thickness of the wrapping layer is 1~2mm.
[0014] Preferably, the thickness of the armor layer is 0.5~1mm.
[0015] This invention also provides a method for preparing the low-temperature resistant and weather-resistant cable described in the above technical solution, comprising: By twisting together monofilaments, a conductor is obtained; The insulating material is melted and extruded onto the outside of the conductor, and then cross-linked to obtain the cable core; Multiple cable cores and fillers are twisted together, then fixed with a wrapping layer, and then an armor layer is prepared using a gap wrapping process. Finally, the material of the outer sheath is melted and extruded onto the outside of the armor layer to obtain a low-temperature and weather-resistant cable.
[0016] The insulation layer of this invention uses dioctyl adipate and long-chain acrylic acid ester grafted with nitrile rubber. The synergistic effect of these two materials improves the low-temperature resistance of the insulation layer. The nitrile rubber contains cyano groups and unsaturated double bonds, which improve the low-temperature resistance of the outer sheath. Grafting with long-chain acrylic acid ester introduces flexible long chains, increasing flexibility, reducing rigidity, and improving low-temperature resistance. Dioctyl adipate is a cold-resistant plasticizer. The outer sheath uses polyether-type TPU and bis(4-aminocyclohexyl) ether. The synergistic effect of these two materials improves the low-temperature resistance of the insulation layer. The polyether-type TPU contains ether bonds in its molecular backbone structure. Because the ether bonds in its structure have low cohesive energy and are easily rotated, their addition improves the low-temperature flexibility of the outer sheath. The addition of bis(4-aminocyclohexyl) ether further improves the low-temperature performance of the outer sheath. Detailed Implementation
[0017] This invention provides a low-temperature and weather-resistant cable, comprising, from the inside out, a core assembly, a wrapping layer, an armor layer, and an outer sheath; a filler is disposed between the core assembly and the wrapping layer; The cable core assembly is composed of multiple cable cores twisted together; The cable core includes a conductor and an insulation layer arranged sequentially from the inside out; The insulating layer, by weight, is prepared from the following raw materials: 80-100 parts of low-density polyethylene, 10-20 parts of modifier, 5-10 parts of filler, 1-2 parts of silane coupling agent, 1-3 parts of crosslinking agent, 0.5-2 parts of antioxidant, and 0.1-0.5 parts of compatibilizer; the modifier includes dioctyl adipate and long-chain acrylate grafted with nitrile rubber. The outer protective layer is prepared from the following raw materials by mass: 80-100 parts of polyvinyl chloride, 5-10 parts of toughening agent, 5-10 parts of plasticizer, 0.1-0.5 parts of heat stabilizer, 1-5 parts of lubricant, 20-30 parts of filler and 0.5-2 parts of antioxidant; the toughening agent includes polyether-type TPU and bis(4-aminocyclohexyl) ether.
[0018] The present invention does not have any special limitation on the source of the raw materials, and commercially available products known to those skilled in the art can be used.
[0019] The low-temperature and weather-resistant cable provided by the present invention includes a core assembly; the core assembly is formed by stranding multiple cores; the core includes a conductor and an insulation layer arranged sequentially from the inside to the outside.
[0020] The present invention does not impose a special limit on the number of cable cores; the number can be adjusted according to actual needs.
[0021] The present invention does not impose any special limitations on the twisting operation; any operation known to those skilled in the art can be used.
[0022] In this invention, the conductor is preferably a copper wire. There is no particular limitation on the diameter of the copper wire; any copper wire well-known to those skilled in the art can be used.
[0023] In this invention, the insulating layer is prepared from the following raw materials in parts by weight: 80-100 parts of low-density polyethylene, 10-20 parts of modifier, 5-10 parts of filler, 1-2 parts of silane coupling agent, 1-3 parts of crosslinking agent, 0.5-2 parts of antioxidant, and 0.1-0.5 parts of compatibilizer. The insulating layer of this invention uses dioctyl adipate and long-chain acrylic acid ester grafted onto nitrile rubber. The synergistic effect of these two materials improves the low-temperature resistance of the insulating layer. The nitrile rubber contains cyano groups and unsaturated double bonds, which can improve the low-temperature resistance of the outer sheath. Grafting with long-chain acrylic acid ester introduces flexible long chains, increasing flexibility, reducing rigidity, and improving low-temperature resistance. Dioctyl adipate is a cold-resistant plasticizer.
[0024] In one embodiment, the mass fraction of the low-density polyethylene can be 81, 82, 83, 84, 85, 86, 87, 88, 89, 90, 91, 92, 93, 94, 95, 96, 97, 98, or 99 parts. In this invention, the low-density polyethylene is the base material.
[0025] In one embodiment, the melt index of the low-density polyethylene can be 70 g / 10 min (190 °C / 2.16 kg); the particle size of the low-density polyethylene can be 600 mesh.
[0026] In this invention, the modifier comprises dioctyl adipate and long-chain acrylate grafted nitrile rubber; the preferred mass ratio of dioctyl adipate to long-chain acrylate grafted nitrile rubber is 1:(2-4). As one embodiment, the mass fraction of the modifier can be 11, 12, 13, 14, 15, 16, 17, 18, or 19 parts; the mass ratio of dioctyl adipate to long-chain acrylate grafted nitrile rubber can be 1:3. This invention, by controlling the mass ratio of dioctyl adipate to long-chain acrylate grafted nitrile rubber, can further improve the low-temperature resistance of the cable.
[0027] This invention does not impose any particular limitation on the preparation method of the acrylic long-chain ester grafted nitrile rubber; any preparation method well known to those skilled in the art can be used. As one embodiment, the preparation method of the acrylic long-chain ester grafted nitrile rubber can be as follows: 500g of nitrile rubber is added to 5L of toluene, heated to 60℃ and stirred for 2h, then 50g of dodecyl acrylate and 1g of benzoyl peroxide are added, the temperature is raised to 80℃ and reacted for 5h, then restored to room temperature, methanol is added to precipitate and separate, the obtained solid is vacuum dried to constant weight and placed in a Soxhlet extractor, extracted for 24h using methanol as solvent, and the extracted product is vacuum dried to constant weight.
[0028] In this invention, the filler is preferably nano-boron nitride. As one embodiment, the filler can be in the following proportions by mass: 6, 7, 8, or 9 parts; the size of the nano-boron nitride can be 200 nm; and the nano-boron nitride can be hexagonal boron nitride nanosheets from Zhejiang Yamei Nanotechnology Co., Ltd.
[0029] This invention does not impose any particular limitation on the type of silane coupling agent; any silane coupling agent well-known to those skilled in the art can be used. As one embodiment, the silane coupling agent may be KH-550.
[0030] The present invention does not specifically limit the type of crosslinking agent; any crosslinking agent well known to those skilled in the art can be used. As one embodiment, the crosslinking agent may be present in 2 parts by mass; the crosslinking agent may be dicumyl peroxide (DCP).
[0031] This invention does not specifically limit the type of antioxidant; any antioxidant well-known to those skilled in the art can be used. As one embodiment, the antioxidant may be 1 part or 1.5 parts by weight; the antioxidant may be antioxidant 1010.
[0032] The present invention does not impose any particular limitation on the type of compatibilizer; any compatibilizer well known to those skilled in the art can be used. As one embodiment, the compatibilizer may be maleic anhydride-grafted polyethylene (PE-g-MAH); the mass fraction of the compatibilizer may be 0.2 parts, 0.3 parts, or 0.4 parts.
[0033] In this invention, the thickness of the insulation layer is preferably 0.6 to 4 mm. As one embodiment, the thickness of the insulation layer can be 1 mm, 2 mm, or 3 mm. Limiting the thickness of the insulation layer to the above range further improves the low-temperature resistance of the cable.
[0034] The low-temperature and weather-resistant cable provided by this invention includes a wrapping layer; a filler is disposed between the cable core assembly and the wrapping layer. In this invention, the filler is used to fill the gaps in the cable core assembly and maintain the roundness of the cable core assembly; the wrapping layer is used to bind and fix the cable core structure.
[0035] The present invention does not impose any special limitations on the material of the filler; any material well known to those skilled in the art can be used. The present invention also does not impose any special limitations on the amount of the filler; it is sufficient to fill the gaps in the cable core assembly and maintain the roundness of the cable core assembly.
[0036] The present invention does not have any special limitation on the material of the tape layer; any material well known to those skilled in the art can be used.
[0037] The present invention does not impose a specific limitation on the thickness of the wrapping layer; any thickness known to those skilled in the art can be used. As one embodiment, the thickness of the wrapping layer can be 1-2 mm.
[0038] The low-temperature and weather-resistant cable provided by this invention includes an armor layer. In this invention, the armor layer serves to provide mechanical protection.
[0039] The present invention does not have any special limitation on the material of the armor layer; any material well known to those skilled in the art can be used.
[0040] The present invention does not impose a specific limitation on the thickness of the armor layer; any thickness known to those skilled in the art can be used. As one embodiment, the thickness of the armor layer can be 0.5~1mm.
[0041] The low-temperature and weather-resistant cable provided by this invention includes an outer sheath. In this invention, the outer sheath is the outermost layer of protection, possessing excellent low-temperature impact strength, scratch resistance, and abrasion resistance, resisting physical damage during laying and use.
[0042] In this invention, the outer protective layer is prepared from the following raw materials in parts by weight: 80-100 parts of polyvinyl chloride, 5-10 parts of toughening agent, 5-10 parts of plasticizer, 0.1-0.5 parts of heat stabilizer, 1-5 parts of lubricant, 20-30 parts of filler and 0.5-2 parts of antioxidant.
[0043] In one embodiment, the polyvinyl chloride (PVC) can be in the following weight proportions: 81, 82, 83, 84, 85, 86, 87, 88, 89, 90, 91, 92, 93, 94, 95, 96, 97, 98, or 99 parts; the PVC can be SG-3 type PVC. In this invention, the PVC is the base material.
[0044] In this invention, the toughening agent comprises polyether-type TPU and bis(4-aminocyclohexyl) ether; the preferred mass ratio of the polyether-type TPU to bis(4-aminocyclohexyl) ether is (1~3):1. As one embodiment, the mass fraction of the toughening agent can be 6, 7, 8, or 9 parts; the mass ratio of the polyether-type TPU to bis(4-aminocyclohexyl) ether can be 2:1; the polyether-type TPU can be BASF 1180A. Limiting the mass ratio of the polyether-type TPU to bis(4-aminocyclohexyl) ether to the above range further improves low-temperature resistance.
[0045] In this invention, the plasticizer is preferably isooctyl stearate and diethylene glycol monobutyl ether adipate; the mass ratio of isooctyl stearate to diethylene glycol monobutyl ether adipate is preferably (1~2):1. The plasticizer used in this invention can reduce friction between PVC molecular chains, improve melt flowability, promote plasticization, and significantly reduce the embrittlement temperature, ensuring flexibility at low temperatures.
[0046] In one embodiment, the plasticizer may be present in 6, 7, 8 or 9 parts by weight.
[0047] This invention does not impose any particular limitation on the type of heat stabilizer; any heat stabilizer well-known to those skilled in the art can be used. As one embodiment, the mass fraction of the heat stabilizer can be 0.2 parts, 0.3 parts, or 0.4 parts; the heat stabilizer can be a calcium-zinc composite stabilizer; and the heat stabilizer can be produced by Dongguan Lihuang Rubber & Plastic Materials Co., Ltd.
[0048] This invention does not impose any particular limitation on the type of lubricant; any lubricant well-known to those skilled in the art can be used. As one embodiment, the lubricant may be present in 2, 3, or 4 parts by weight; the lubricant may be microcrystalline wax; and the lubricant may be manufactured by Dongguan Lihuang Rubber & Plastic Materials Co., Ltd.
[0049] In this invention, the filler is preferably carbon black, zinc oxide, and aluminum hydroxide; the mass ratio of carbon black, zinc oxide, and aluminum hydroxide is preferably 2:1:1. The filler used in this invention can improve the wear resistance of cables.
[0050] In one embodiment, the mass fraction of the filler can be 21, 22, 23, 24, 25, 26, 27, 28, or 29 parts.
[0051] This invention does not specifically limit the type of antioxidant; any antioxidant well-known to those skilled in the art can be used. As one embodiment, the antioxidant may be 1 part or 1.5 parts by weight; the antioxidant may be antioxidant 1010.
[0052] In this invention, the thickness of the outer sheath is preferably 1.5 to 3 mm. As one embodiment, the thickness of the outer sheath can be 2 mm. Limiting the thickness of the outer sheath to the above range further improves the low-temperature resistance of the cable.
[0053] The insulation layer of this invention uses dioctyl adipate and long-chain acrylic acid ester grafted with nitrile rubber. The synergistic effect of these two materials improves the low-temperature resistance of the insulation layer. The nitrile rubber contains cyano groups and unsaturated double bonds, which improve the low-temperature resistance of the outer sheath. Grafting with long-chain acrylic acid ester introduces flexible long chains, increasing flexibility, reducing rigidity, and improving low-temperature resistance. Dioctyl adipate is a cold-resistant plasticizer. The outer sheath uses polyether-type TPU and bis(4-aminocyclohexyl) ether. The synergistic effect of these two materials improves the low-temperature resistance of the insulation layer. The polyether-type TPU contains ether bonds in its molecular backbone structure. Because the ether bonds in its structure have low cohesive energy and are easily rotated, their addition improves the low-temperature flexibility of the outer sheath. The addition of bis(4-aminocyclohexyl) ether further improves the low-temperature performance of the outer sheath.
[0054] This invention also provides a method for preparing the low-temperature resistant and weather-resistant cable described in the above technical solution, comprising: By twisting together monofilaments, a conductor is obtained; The insulating material is melted and extruded onto the outside of the conductor, and then cross-linked to obtain the cable core; Multiple cable cores and fillers are twisted together, then fixed with a wrapping layer, and then an armor layer is prepared using a gap wrapping process. Finally, the material of the outer sheath is melted and extruded onto the outside of the armor layer to obtain a low-temperature and weather-resistant cable.
[0055] The present invention does not impose any special limitation on the preparation method of the low temperature and weather resistant cable. It can be prepared by using a preparation method well known to those skilled in the art according to the above process.
[0056] The preparation method provided by this invention is simple and suitable for industrial production.
[0057] The technical solutions of this invention will be clearly and completely described below with reference to the embodiments thereof. Obviously, the described embodiments are only a part of the embodiments of this invention, and not all of them. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without creative effort are within the scope of protection of this invention.
[0058] Example 1 An insulated cable consists of a core assembly, a wrapping layer, an armor layer, and an outer sheath arranged sequentially from the inside out. A polypropylene filler rope is provided between the cable core assembly and the wrapping layer; The cable core assembly is composed of three cable cores twisted together; The cable core consists of a conductor and an insulation layer arranged sequentially from the inside out; The insulating layer is prepared from the following raw materials in parts by weight: 80 parts of low-density polyethylene, 20 parts of modifier, 5 parts of filler, 2 parts of silane coupling agent KH-550, 1 part of crosslinking agent, 2 parts of antioxidant and 0.1 parts of compatibilizer; The low-density polyethylene has a melt index of 70 g / 10 min (190℃ / 2.16 kg) and a particle size of 600 mesh. The modifier is dioctyl adipate and long-chain acrylate grafted onto nitrile rubber. The mass ratio of dioctyl adipate and long-chain acrylate grafted with nitrile rubber is 1:2. The preparation method of the acrylic long-chain ester grafted nitrile rubber can be as follows: 500g of nitrile rubber is added to 5L of toluene, heated to 60℃ and stirred for 2h, then 50g of dodecyl acrylate and 1g of benzoyl peroxide are added, heated to 80℃ and reacted for 5h, then restored to room temperature, methanol is added to precipitate and separate, the obtained solid is vacuum dried to constant weight and then placed in a Soxhlet extractor, and extracted for 24h with methanol as solvent. The extracted product is then vacuum dried to constant weight. The filler is nano-boron nitride; The boron nitride nanosheets are hexagonal boron nitride nanosheets from Zhejiang Yamei Nanotechnology Co., Ltd. The crosslinking agent is dicumyl peroxide; The antioxidant is antioxidant 1010; The compatibilizer is PE-g-MAH, manufactured by Dongguan Dinghai Plastic & Chemical Co., Ltd. The thickness of the insulating layer is 0.8 mm; The material of the wrapping layer is non-woven fabric with a thickness of 1.5mm; The thickness of the armor layer is 0.5 mm; The outer protective layer is prepared from the following raw materials: by mass parts, the outer protective layer is prepared from the following raw materials: 100 parts of polyvinyl chloride, 5 parts of toughening agent, 10 parts of plasticizer, 0.1 parts of heat stabilizer, 5 parts of lubricant, 20 parts of filler and 0.5 parts of antioxidant; The polyvinyl chloride is SG-3 type polyvinyl chloride; The toughening agent is a polyether-type TPU and a bis(4-aminocyclohexyl) ether; The mass ratio of the polyether-type TPU to the bis(4-aminocyclohexyl) ether is 1:1; The polyether-type TPU is BASF 1180A from Germany; The plasticizer is isooctyl stearate and diethylene glycol monobutyl ether adipate; The mass ratio of isooctyl stearate to diethylene glycol monobutyl ether adipate is 1:1; The heat stabilizer is a calcium-zinc composite stabilizer; The heat stabilizer was produced by Dongguan Lihuang Rubber & Plastic Materials Co., Ltd. The lubricant is microcrystalline wax; The lubricant was produced by Dongguan Lihuang Rubber & Plastic Materials Co., Ltd. The filler is carbon black, zinc oxide, and aluminum hydroxide; The mass ratio of carbon black, zinc oxide and aluminum hydroxide is 2:1:1; The antioxidant is antioxidant 1010; The outer protective layer has a thickness of 1.5 mm; The method for preparing the low-temperature resistant and weather-resistant cable is as follows: Five 0.20mm diameter electrical round copper monofilaments are twisted together in a right-hand direction using a stranding machine, with a stranding pitch of 16 times, to obtain a conductor; The raw materials for the insulation layer are mixed in an internal mixer, then mixed at 130°C for 15 minutes, and then cooled to room temperature to obtain the compound. An extruder was used, with the barrel temperature set in sections from the feed section to the die head section at 95℃, 110℃, 125℃, 130℃, and 135℃, and the die temperature controlled at 130℃. The extruder continuously coated the outside of the conductor, and then crosslinked it for 30 minutes at a pressure of 1.3MPa, a temperature of 180℃, and a nitrogen atmosphere. After crosslinking, the conductor was cooled to obtain the cable core. The three cable cores and filler are twisted together, with a cable pitch of 13 times the outer diameter of the twist. Then, a non-woven fabric tape is wrapped around the cable in a left-hand overlapping manner to obtain a wrapping layer with an overlap rate of 20%. Then, galvanized steel strip is wrapped in reverse gap, and the preheating temperature of the steel strip wrapping is set to 50℃. The raw material for the outer sheath is fed into a single-screw extruder with a body temperature of 140°C and a die temperature of 170°C. The molten material is evenly coated on the outside of the armor layer, and then cooled and shaped to obtain an insulated cable.
[0059] Example 2 Based on Example 1, the following parameters are changed while other conditions remain unchanged: The insulating layer is prepared from the following raw materials in parts by weight: 100 parts of low-density polyethylene, 10 parts of modifier, 10 parts of filler, 1 part of silane coupling agent, 3 parts of crosslinking agent, 0.5 parts of antioxidant and 0.5 parts of compatibilizer. The outer protective layer is prepared from the following raw materials by mass: 80 parts polyvinyl chloride, 10 parts toughening agent, 5 parts plasticizer, 0.5 parts heat stabilizer, 1 part lubricant, 30 parts filler and 2 parts antioxidant.
[0060] Example 3 Based on Example 1, the following parameters are changed while other conditions remain unchanged: The insulating layer is prepared from the following raw materials by weight: 90 parts low-density polyethylene, 15 parts modifier, 8 parts filler, 1 part silane coupling agent, 2 parts crosslinking agent, 1 part antioxidant and 0.3 parts compatibilizer; The outer protective layer is prepared from the following raw materials by weight: 90 parts polyvinyl chloride, 8 parts toughening agent, 8 parts plasticizer, 0.3 parts heat stabilizer, 3 parts lubricant, 25 parts filler and 1.5 parts antioxidant.
[0061] Comparative Example 1 Based on Example 1, the long-chain acrylic acid ester grafted with nitrile rubber was omitted, while other conditions remained unchanged.
[0062] Comparative Example 2 Based on Example 1, dioctyl adipate was omitted, while other conditions remained unchanged.
[0063] Example 4 Based on Example 1, the mass ratio of dioctyl adipate and long-chain acrylate grafted with nitrile rubber was modified to 1:4, while other conditions remained unchanged.
[0064] Example 5 Based on Example 1, the mass ratio of dioctyl adipate and long-chain acrylate grafted with nitrile rubber was modified to 1:3, while other conditions remained unchanged.
[0065] Comparative Example 3 Based on Example 1, the polyether-type TPU was omitted, while other conditions remained unchanged.
[0066] Comparative Example 4 Based on Example 1, the bis(4-aminocyclohexyl) ether was omitted, while other conditions remained unchanged.
[0067] Example 6 Based on Example 1, the mass ratio of polyether-type TPU and bis(4-aminocyclohexyl) ether was modified to 1:3, while other conditions remained unchanged.
[0068] Example 7 Based on Example 1, the mass ratio of polyether-type TPU and bis(4-aminocyclohexyl) ether was modified to 1:2, while other conditions remained unchanged.
[0069] The insulation layer and outer sheath in Examples 1-7 and Comparative Examples 1-4 were subjected to performance tests, and the results are shown in Tables 1 and 2. Among them, tensile performance test: according to GB / T1004-2006 standard, the tensile strength and elongation at break were tested using a universal testing machine for electronic materials, and the tensile rate was 50 mm / min; low temperature impact test: according to GB / T2843-2008 standard, the low temperature impact strength of the samples was tested using a simply supported beam impact testing machine, and the temperature was -50℃.
[0070] Table 1. Insulation layer performance data in Examples 1-5 and Comparative Examples 1-2
[0071] Table 2 shows the performance data of the outer protective layer in Examples 1-3, Examples 6-7, and Comparative Examples 3-4.
[0072] As can be seen from Tables 1 and 2, the cable insulation material provided by this invention possesses excellent low-temperature resistance and weather resistance. Dioctyl adipate and long-chain acrylate grafted with nitrile rubber can synergistically improve the low-temperature resistance of the insulation layer; omitting either one will lead to a decrease in low-temperature resistance. Polyether-type TPU and bis(4-aminocyclohexyl) ether can synergistically improve the low-temperature resistance of the insulation layer; omitting either one will lead to a decrease in low-temperature resistance. Limiting the mass ratio of polyether-type TPU and bis(4-aminocyclohexyl) ether can further improve the low-temperature resistance.
[0073] The cables prepared in Examples 1-7 were used as samples for performance testing, and the results are shown in Table 3.
[0074] Low temperature impact test: According to clause 8.5 of GB / T2951.14-2008, the cooling temperature is -50±2℃, the time is 16h, the drop hammer mass is 1kg, the impact block mass is 200g, the drop height is 100mm, and the test requires that there should be no visible cracks on the surface. Low temperature bending test: According to clause 8.2 of GB / T2951.14-2008, the cooling temperature is -50±2℃, the time is 16h, the diameter of the test bar is 4~5 times the outer diameter of the cable, and it is wound 3~4 times. The test requires that there should be no visible cracks on the surface.
[0075] Table 3 Performance data of the cables prepared in Examples 1-7
[0076] As shown in Table 3, the cable prepared by this invention meets the design standards and can meet the working requirements under harsh outdoor low-temperature environments.
[0077] As can be seen from the above embodiments and comparative examples, the cable provided by the present invention has excellent low-temperature resistance and weather resistance.
[0078] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A low-temperature and weather-resistant cable, comprising, from the inside out, a core assembly, a wrapping layer, an armor layer, and an outer sheath; a filler is disposed between the core assembly and the wrapping layer; The cable core assembly is composed of multiple cable cores twisted together; The cable core includes a conductor and an insulation layer arranged sequentially from the inside out; The insulating layer, by weight, is prepared from the following raw materials: 80-100 parts of low-density polyethylene, 10-20 parts of modifier, 5-10 parts of filler, 1-2 parts of silane coupling agent, 1-3 parts of crosslinking agent, 0.5-2 parts of antioxidant, and 0.1-0.5 parts of compatibilizer; the modifier includes dioctyl adipate and long-chain acrylate grafted with nitrile rubber. The outer protective layer is prepared from the following raw materials by mass: 80-100 parts of polyvinyl chloride, 5-10 parts of toughening agent, 5-10 parts of plasticizer, 0.1-0.5 parts of heat stabilizer, 1-5 parts of lubricant, 20-30 parts of filler and 0.5-2 parts of antioxidant; the toughening agent includes polyether-type TPU and bis(4-aminocyclohexyl) ether.
2. The low-temperature resistant and weather-resistant cable according to claim 1, characterized in that, The insulating layer is prepared from the following raw materials by mass: 85-95 parts of low-density polyethylene, 12-18 parts of modifier, 6-9 parts of filler, 1-2 parts of silane coupling agent, 1-2 parts of crosslinking agent, 1-1.5 parts of antioxidant and 0.2-0.4 parts of compatibilizer.
3. The low-temperature resistant and weather-resistant cable according to claim 1 or 2, characterized in that, The mass ratio of dioctyl adipate and long-chain acrylate grafted with nitrile rubber is 1:(2~4).
4. The low-temperature resistant and weather-resistant cable according to claim 3, characterized in that, The mass ratio of dioctyl adipate and long-chain acrylate grafted with nitrile rubber is 1:
3.
5. The low-temperature resistant and weather-resistant cable according to claim 1, characterized in that, The thickness of the insulating layer is 0.6~4mm.
6. The low-temperature resistant and weather-resistant cable according to claim 1, characterized in that, The outer protective layer is prepared from the following raw materials by mass: 85-95 parts of polyvinyl chloride, 6-9 parts of toughening agent, 6-9 parts of plasticizer, 0.2-0.4 parts of heat stabilizer, 2-4 parts of lubricant, 22-28 parts of filler and 1-1.5 parts of antioxidant.
7. The low-temperature resistant and weather-resistant cable according to claim 1 or 6, characterized in that, The mass ratio of the polyether-type TPU to the bis(4-aminocyclohexyl) ether is (1~3):
1.
8. The low-temperature resistant and weather-resistant cable according to claim 7, characterized in that, The mass ratio of the polyether-type TPU to the bis(4-aminocyclohexyl) ether is 2:
1.
9. The low-temperature resistant and weather-resistant cable according to claim 1, characterized in that, The thickness of the outer protective layer is 1.5~3mm.
10. The low-temperature resistant and weather-resistant cable according to claim 1, characterized in that, The thickness of the wrapping layer is 1~2mm.
11. The low-temperature resistant and weather-resistant cable according to claim 1, characterized in that, The thickness of the armor layer is 0.5~1mm.
12. A method for preparing the low-temperature resistant and weather-resistant cable according to any one of claims 1 to 11, comprising: By twisting together monofilaments, a conductor is obtained; The insulating material is melted and extruded onto the outside of the conductor, and then cross-linked to obtain the cable core; Multiple cable cores and fillers are twisted together, then fixed with a wrapping layer, and then an armor layer is prepared using a gap wrapping process. Finally, the material of the outer sheath is melted and extruded onto the outside of the armor layer to obtain a low-temperature and weather-resistant cable.