Fire resistant power cable and method of making the same

By using segmented locking strips and ceramicized silicone rubber layers with different softening points combined with an interface conversion coating in fire-resistant power cables, the problem of through-cracks in the ceramic shell of the cable under fire conditions was solved, and the interlayer bonding strength and fire resistance of the cable were improved.

CN123161968APending Publication Date: 2026-11-24ANHUI TIANKANG(GROUP) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611599789.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-15
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing fire-resistant power cables are prone to through-cracks under fire conditions due to uneven shrinkage of the ceramic shell and detachment of the fiber tape, and the interlayer bonding strength is insufficient, which affects the fire resistance performance of the cable.

Method used

The segmented locking strip is used with alternating through-window sections and non-porous crack-stopping sections. A radial locking key is formed by spiral wrapping. Combined with ceramicized silicone rubber layers with different softening points and interface conversion coating, the interlayer bonding force is enhanced. High-silica fiber rope provides pre-compression support for cabling.

Benefits of technology

It effectively blocked the propagation of cracks, reduced the probability of through cracks in the ceramic shell, improved the interlayer bonding strength and fire resistance of the cable, and ensured the integrity of the cable under flame and mechanical impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123161968A_ABST
    Figure CN123161968A_ABST
Patent Text Reader

Abstract

This invention discloses a fire-resistant power cable and its preparation method, relating to the technical field of wires and cables and fire-resistant insulating materials. It includes at least one insulated core and a cabling wrapping layer, an inner sheath, and an outer sheath covering the insulated core. The insulated core includes a conductor, a main insulation layer, and a composite fire-resistant layer disposed outside the main insulation layer. The composite fire-resistant layer comprises, from the inside out, a low-temperature ceramicized silicone rubber layer, a segmented locking tape, and a high-temperature ceramicized silicone rubber layer. The segmented locking tape is wrapped in a spiral manner, and alternating through-window sections and non-porous crack-stopping sections are arranged along the length of the tape. The through-window sections form a radial connection between the inner and outer ceramicized silicone rubber layers, and the non-porous crack-stopping sections maintain the lateral continuity of the tape and block cracks extending along the direction of the holes. Through the alternating distribution of through-window sections and non-porous crack-stopping sections in the segmented locking tape, the non-porous crack-stopping sections maintain lateral fiber continuity and can block cracks extending along continuous hole areas.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of wire and cable technology and fire-resistant insulation materials, specifically to a fire-resistant power cable and its preparation method. Background Technology

[0002] Fire-resistant power cables are mainly used in places requiring continuous power supply during fire, such as fire protection power supply, emergency lighting, smoke extraction, evacuation guidance, data centers, rail transit, hospitals, and high-rise buildings. Existing fire-resistant power cables typically use mica tape wrapping, inorganic fiber tape reinforcement, ceramicized silicone rubber extrusion, or a simple superposition of the above structures to form a fire-resistant layer.

[0003] Mica tape possesses good high-temperature insulation properties, but the mica sheets are brittle and prone to misalignment, localized cracking, or pulverization during cable bending, laying, and fire-induced impact and vibration. Ceramicized silicone rubber is flexible at room temperature and can form an inorganic ceramic shell when exposed to fire; however, its organic phase decomposition, glass phase softening, inorganic filler sintering, and structural shrinkage occur at different temperature stages. When the ceramicized layer is directly exposed to external flames, the outer side experiences a significantly higher temperature rise rate than the inner side near the main insulation layer, easily leading to radial temperature gradients and uneven shrinkage.

[0004] Existing methods involving fiber strips or open-pore reinforcement strips within ceramicized polymers, while able to constrain ceramic shell detachment to some extent, still present the following problems: Continuous open-pore strips easily form continuous weak paths along the pore arrangement direction. When the ceramic layer is subjected to periodic impacts, cracks can propagate along the continuous pore area, causing axial through-cracks in the refractory layer. The inner and outer ceramicized layers are typically extruded separately, vulcanized separately, or bonded solely through surface contact. After high-temperature decomposition, the organic interfacial bonding disappears, making radial separation of the inner and outer layers likely, and the fiber strips may also detach from the ceramic shell. Summary of the Invention

[0005] To address the shortcomings of existing technologies, this invention provides a fire-resistant power cable and its manufacturing method. By alternating the distribution of through-window sections and non-porous crack-stopping sections in the segmented locking strip, the non-porous crack-stopping sections maintain transverse fiber continuity, thus preventing cracks from propagating along continuous pore areas. The axial misalignment of through-window sections in adjacent wrapping rings avoids the formation of continuous axially weak areas by multiple wrapping rings, reducing the probability of through-cracks forming in the ceramic shell.

[0006] To achieve the above objectives, the present invention provides the following technical solution: a fire-resistant power cable, comprising at least one insulated core and a cable wrapping layer, an inner sheath, and an outer sheath covering the insulated core.

[0007] The insulated conductor core includes a conductor, a main insulation layer, and a composite fire-resistant layer disposed outside the main insulation layer. The composite fire-resistant layer, from the inside out, includes a low-temperature ceramicized silicone rubber layer, a segmented interlocking tape, and a high-temperature ceramicized silicone rubber layer.

[0008] The segmented locking tape is wrapped in a spiral manner, with alternating through-window sections and non-porous crack-stopping sections along the tape length. The through-window sections are used to form a radial connection between the inner and outer ceramicized silicone rubber, while the non-porous crack-stopping sections are used to maintain the lateral continuity of the tape and block cracks that propagate along the pore direction.

[0009] The through-window sections in adjacent wrapping rings are misaligned along the cable axis, preventing the perforated areas of adjacent wrapping rings from forming a continuous weak zone along the cable axis. When a crack occurs in a ceramic shell, the crack propagates to a non-perforated section or a non-perforated area of ​​an adjacent wrapping ring before being blocked or having its propagation direction changed.

[0010] During pressure extrusion, high-temperature ceramicized silicone rubber passes through a through-window, contacting and co-curing with low-temperature ceramicized silicone rubber in an incompletely vulcanized state. This forms radial keying within the through-window, traversing segmented interlocking bands. The radial keying simultaneously generates mechanical interlocking and co-curing bonding, reducing the risk of interlayer delamination before and after a fire.

[0011] The softening point of the glass powder contained in the low-temperature ceramicized silicone rubber layer is 500-580℃, while the softening point of the glass powder contained in the high-temperature ceramicized silicone rubber layer is 720-820℃, with a difference of 140-320℃ between the two.

[0012] In the initial stage of a fire, the glass powder in the low-temperature ceramicized silicone rubber layer, which is close to the main insulation layer and has a relatively low temperature, softens first. At a lower temperature, it fills the pores formed by the decomposition of the organic phase and bonds mica, wollastonite, and silica into a continuous thermal insulation layer. The high-temperature ceramicized silicone rubber layer on the outside uses glass powder with a higher softening point to prevent it from melting prematurely during the rapid heating phase. As the temperature of the outer layer increases further, the high-softening-point glass powder forms a high-viscosity glass phase, which, together with alumina short fibers, wollastonite, and segmented interlocking bands, forms a load-bearing ceramic skeleton.

[0013] The segmented locking tape is woven from high-silica fiber yarn with a silica content of not less than 94%. Side reinforcing bars extending continuously along the tape's length are provided on both sides of the segmented locking tape. These reinforcing bars are used to bear the wrapping tension and prevent the edges of the through-window from tearing during the wrapping process.

[0014] The through window segment is located between two edge ribs, and each through window segment has 2 to 4 rows of diamond-shaped through windows or rounded rectangular through windows. The opening ratio of the through window segment is 28% to 42%, and the width of the segmented locking strip is 10 to 25 mm and the thickness is 0.20 to 0.45 mm.

[0015] The non-porous crack arrestor section runs transversely between the two edge reinforcements, and its length along the strip length direction is 0.5 to 1.2 times the width of the segmented interlocking strip. The non-porous crack arrestor section does not have through holes, which can maintain the transverse continuous fiber bundle and form a periodic crack blocking zone.

[0016] The overlap rate of the segmented locking tape is 8% to 18%. When viewed along the cable axis, the projected overlap rate of the through window section in adjacent wrapping loops is no greater than 20%.

[0017] The axial projection overlap rate referred to in this invention is the ratio of the coincident length of the through window segment in the direction of the cable axis in two adjacent wrapping loops to the axial projection length of the shorter through window segment.

[0018] The area fill rate of the through-window is 75%–95%. The area fill rate is the ratio of the area of ​​the through-window occupied by the high-temperature ceramicized silicone rubber to the total area of ​​the through-window in the radial cross-section of the cable. At least one radial key is formed in each through-window, and the minimum cross-sectional area of ​​the radial key at the plane of the segmented locking band is 0.5–2.5 mm².

[0019] The low-temperature ceramicized silicone rubber layer comprises the following raw materials in parts by weight: 100 parts methyl vinyl silicone rubber; 25-40 parts phlogopite; 3-8 parts borosilicate glass powder with a softening point of 500-580℃; 8-18 parts acicular wollastonite; 15-30 parts magnesium hydroxide; 8-15 parts fumed silica; 2-5 parts zinc borate; 0.5-2 parts silane coupling agent; and 0.8-1.8 parts peroxide vulcanizing agent.

[0020] The glass powder particle size D50 in the low-temperature ceramicized silicone rubber layer is 2–6 μm. The mass ratio of acicular wollastonite to glass powder is 1.5:1 to 3.5:1.

[0021] In the low-temperature ceramicized silicone rubber layer, the low-softening-point glass powder can form a binder phase before the inner layer temperature reaches the outer layer temperature; phlogopite forms a layered heat-resistant insulating skeleton; acicular wollastonite inhibits sintering shrinkage and bridges microcracks; magnesium hydroxide decomposes upon heating and absorbs heat to generate magnesium oxide; zinc borate is conducive to the formation of a continuous borosilicate phase.

[0022] The high-temperature ceramicized silicone rubber layer comprises the following raw materials in parts by weight: 100 parts methyl vinyl silicone rubber; 30-50 parts phlogopite; 3-8 parts low-alkali zinc borosilicate glass powder with a softening point of 720-820℃; 6-14 parts alumina short fibers; 12-25 parts acicular wollastonite; 8-15 parts fumed silica; 0.5-2 parts silane coupling agent; and 0.8-1.8 parts peroxide vulcanizing agent.

[0023] The glass powder in the high-temperature ceramicized silicone rubber layer has a particle size D50 of 5–12 μm, and the mass ratio of acicular wollastonite to glass powder is 2.5:1–6:1.

[0024] Short alumina fibers and needle-like wollastonite form a cross-reinforced framework. High softening point glass powder forms a high-viscosity glass phase after the outer layer temperature is fully raised, reducing the risk of the outer ceramic body collapsing due to premature flow of the glass phase.

[0025] The difference in linear shrinkage rates between the low-temperature ceramicized silicone rubber layer and the high-temperature ceramicized silicone rubber layer after heat treatment at 950℃ for 30 minutes is no more than 4 percentage points.

[0026] The fiber surface of the segmented locking strip, the wall of the through-hole, and the surface of the non-porous crack-stopping section are provided with an interface conversion coating.

[0027] The interface conversion coating is formed by silica sol, boric acid and γ-methacryloxypropyltrimethoxysilane in a mass ratio of 100:4 to 10:1 to 3, and its dry weight gain is 2% to 6% of the mass of the segmented interlocking band.

[0028] The hydrolyzable groups in the silane component can condense with the hydroxyl groups on the surface of high-silica fibers, and their organic double bonds can participate in the formation of the silicone rubber interface network during peroxide vulcanization; silica sol and boric acid form a silicon-oxygen-boron-oxygen inorganic linkage phase at high temperature. Therefore, the interface conversion coating can play an interfacial bonding role in both the room temperature vulcanization stage and the high temperature ceramization stage.

[0029] The thickness of the low-temperature ceramicized silicone rubber layer is 0.5–1.0 mm, and the thickness of the high-temperature ceramicized silicone rubber layer is 0.8–1.6 mm.

[0030] When there are two or more insulated conductors, a high-silica fiber rope covered with low-temperature ceramicized silicone rubber is installed in the cabling gap between the insulated conductors. The thickness of the outer layer of the high-silica fiber rope is 0.2 to 0.6 mm, and its outer diameter after covering is 1.02 to 1.08 times the diameter of the tangent circle in the corresponding cabling gap.

[0031] During cabling, the sheathed high-silica fiber rope is subjected to radial compression, forming a pre-compression support. After a fire, the high-silica fiber rope and its outer ceramic sheath remain located at the center of the cabling, which reduces the degree of movement of the insulated cores toward the center and the degree of collision between the ceramic shells.

[0032] This invention also provides a method for preparing a fire-resistant power cable, comprising the following steps: Step S1: Twist the metal monofilaments to form a conductor, and extrude the main insulation layer over the conductor.

[0033] Step S2: The low-temperature ceramicized silicone rubber layer is extruded onto the outside of the main insulation layer and vulcanized to 10%–30% by infrared heating.

[0034] Step S3: The segmented locking tape is spirally wrapped around the low-temperature ceramicized silicone rubber layer with a wrapping tension of 4 to 12 N, the overlap rate is controlled at 8% to 18%, and the through window segments in the adjacent wrapping rings are axially misaligned.

[0035] In step S4, high-temperature ceramicized silicone rubber is extruded onto the outside of the segmented locking belt at a die head pressure of 4-10 MPa, so that the high-temperature ceramicized silicone rubber passes through the through window and comes into contact with the low-temperature ceramicized silicone rubber. The area filling rate of the high-temperature ceramicized silicone rubber to the through window is 75%-95%.

[0036] Step S5: The inner and outer layers of silicone rubber are vulcanized together using a microwave-hot air continuous vulcanization method at 260-340℃ for 30-180s, forming radial keying within the through-window to obtain the insulated wire core.

[0037] Step S6: The insulated wire cores are cabled, and the cable wrapping layer, inner sheath and outer sheath are formed in sequence.

[0038] Before wrapping the segmented locking strip, the segmented locking strip is activated by atmospheric pressure plasma, then dipped in an interface treatment solution, and dried at 100-130℃ to achieve a dry weight gain of 2%-6%.

[0039] In step S3, the leading edge position of the through window segment is identified by a photoelectric sensor, and the rotation speed of the wrapping head is servo-adjusted according to the cable travel speed and the pitch of the segmented locking tape, so that the axial projection overlap rate of the through window segment in adjacent wrapping rings is not greater than 20%.

[0040] Compared with existing technologies, this invention provides a fire-resistant power cable and its manufacturing method, which has the following beneficial effects: By alternating the through-window sections and non-porous crack-stopping sections of the segmented locking band, the non-porous crack-stopping sections maintain transverse fiber continuity, thus blocking cracks propagating along continuous pore areas. The axial misalignment of the through-window sections in adjacent wrapping rings prevents multiple wrapping rings from forming continuous axially weak areas, reducing the probability of through-cracks in the ceramic shell. High-temperature ceramicized silicone rubber passes through the through-windows and co-cures with the incompletely vulcanized low-temperature ceramicized silicone rubber, forming radial lock keys across the segmented locking band, ensuring that the segmented locking band is not simply sandwiched between two layers but is embedded in the overall silicone rubber network. The low-temperature and high-temperature ceramicized silicone rubber layers use glass powders with different softening points, enabling them to adapt to the radial temperature gradient of high outer layer temperature and low inner layer temperature under fire conditions, sequentially completing inner layer sealing and outer layer load-bearing ceramicization at different temperature stages. The interface conversion coating improves the adhesion between silicone rubber and high-silica fibers at room temperature and forms an inorganic interface bonding phase at high temperature, reducing the risk of fiber strip separation from the ceramic body after high temperature. The pre-compressed high-silica fiber ropes in the cabling gaps can maintain the relative position of the wire cores under fire impact conditions, reducing the collapse of the wire cores towards the center and the collision of ceramic shells. The above structure is not a simple superposition of various refractory materials, but a multi-scale crack-resistant system formed by a staggered crack-arresting structure, through-window radial keying, softening point gradient, and pre-compressed cabling support. Attached Figure Description

[0041] Figure 1 This is a scanning electron microscope image of the radial section of the through window in the unfired state of the composite fire-resistant layer in Example 2. Figure 2 This is a scanning electron microscope image of the radial key interface at the through window of the composite refractory layer in Example 2 after being kept at 950°C for 30 minutes. Detailed Implementation

[0042] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0043] Please see Figure 1 and Figure 2 This invention provides a technical solution for a fire-resistant power cable and its manufacturing method: Figure 1The reference numerals in the figures are as follows: 3: Low-temperature ceramicized silicone rubber layer; 4: Segmented interlocking band; 411: Through window; 44: High-silica fiber bundle in the segmented interlocking band; 5: High-temperature ceramicized silicone rubber layer; 6: Radial key formed through the through window; 61: Connection area between the radial key and the low-temperature ceramicized silicone rubber layer; 62: Continuous transition area between the radial key and the high-temperature ceramicized silicone rubber layer.

[0044] Figure 2 The reference numerals in the figures are as follows: 3: Ceramic body formed after firing the low-temperature ceramized silicone rubber layer; 4: Segmented interlocking band; 411: Through window; 44: High-silica fiber bundle; 5: Ceramic body formed after firing the high-temperature ceramized silicone rubber layer; 6: Ceramic bridge formed after firing the radial interlocking bond; 61: Connection area between the fired ceramic bridge and the low-temperature ceramized layer; 62: Connection area between the fired ceramic bridge and the high-temperature ceramized layer; P: Pores filled with epoxy resin; C: Local non-penetrating microcracks; D: Locally relatively dense interface connection area.

[0045] The example uses a three-core copper core power cable with a rated voltage of 0.6 / 1kV and a nominal conductor cross-sectional area of ​​6mm². The conductor is formed by stranding copper monofilaments, and the main insulation layer is a cross-linked polyethylene insulation layer with a nominal thickness of 0.7mm.

[0046] The particle size of phlogopite is 40–100 μm; the aspect ratio of acicular wollastonite is 8–15; the average length of alumina short fibers is 100–300 μm; and the specific surface area of ​​fumed silica is 150–220 m² / g.

[0047] The softening point of low-temperature and high-temperature glass powders shall be determined in accordance with GB / T 28195—2011 "Test Method for Softening Point of Glass".

[0048] The peroxide vulcanizing agent is an organic peroxide vulcanizing agent, and the dosage is calculated based on the mass of the active ingredient. The silane coupling agent is a silane coupling agent containing vinyl or methacryloxy groups.

[0049] The general preparation method of ceramicized silicone rubber compound is as follows: First, add methyl vinyl silicone rubber to a mixing equipment and plasticize it at 50-70℃ for 3-5 minutes; then add phlogopite, glass powder, acicular wollastonite, magnesium hydroxide or alumina short fibers, fumed silica, zinc borate and silane coupling agent in sequence, and mix for 10-15 minutes; after discharging the rubber and cooling it to below 40℃, add peroxide vulcanizing agent to a two-roll mill, pass it through a thin mill 5-8 times, and let it stand for no less than 8 hours before extrusion.

[0050] The degree of vulcanization was determined using a vulcanizer to establish a torque-time curve, and calculated using the following formula: Degree of vulcanization = (Measured torque - Minimum torque) ÷ (Maximum torque - Minimum torque) × 100%.

[0051] The determination of vulcanization characteristics and the use of instruments shall be carried out in accordance with the disc oscillating vulcanizer method specified in GB / T 9869.2—2025.

[0052] Example 1 Copper monofilaments are twisted together to form a 6mm² conductor, and a 0.7mm thick cross-linked polyethylene main insulation layer is extruded over the conductor.

[0053] By weight, the low-temperature ceramicized silicone rubber compound includes: 100 parts of methyl vinyl silicone rubber, 25 parts of phlogopite, 3 parts of borosilicate glass powder with a softening point of 500℃ and a D50 of 2μm, 8 parts of acicular wollastonite, 15 parts of magnesium hydroxide, 8 parts of fumed silica, 2 parts of zinc borate, 0.5 parts of silane coupling agent, and 0.8 parts of peroxide vulcanizing agent.

[0054] The above-mentioned rubber compound is extruded onto the outside of the main insulation layer to form a low-temperature ceramicized silicone rubber layer with a thickness of 0.5 mm, and infrared heating is used to make its vulcanization degree reach 10%.

[0055] The segmented locking strip is 10mm wide and 0.20mm thick. The through-window section has two rows of rounded rectangular through-windows with an opening ratio of 28%. The length of the non-porous crack-prevention section is 0.5 times the width of the segmented locking strip. Continuous edge reinforcements are provided on both sides of the segmented locking strip.

[0056] The segmented interlocking bands were activated by atmospheric pressure plasma. An interface treatment solution was prepared by mixing silica sol, boric acid, and γ-methacryloyloxypropyltrimethoxysilane at a solid mass ratio of 100:4:1. After dip coating, the solution was dried at 100°C to achieve a dry weight gain of 2%.

[0057] The spiral wrapping is performed with a wrapping tension of 4N, the overlap rate is 8%, and the axial projection overlap rate of the through window segment in the adjacent wrapping loops is 20%.

[0058] By weight, the high-temperature ceramicized silicone rubber compound includes: 100 parts methyl vinyl silicone rubber, 30 parts phlogopite, 3 parts low-alkali zinc borosilicate glass powder with a softening point of 820℃ and a D50 of 5μm, 6 parts alumina short fibers, 12 parts acicular wollastonite, 8 parts fumed silica, 0.5 parts silane coupling agent, and 0.8 parts peroxide vulcanizing agent.

[0059] High-temperature ceramicized silicone rubber was extruded under a die head pressure of 4MPa, with a through-window area filling rate of 75%, a minimum cross-sectional area of ​​0.5mm² for the radial key, and a layer thickness of 0.8mm for the high-temperature ceramicized silicone rubber.

[0060] The inner and outer layers are vulcanized together by continuous microwave-hot air curing at 260℃ for 30 seconds.

[0061] Three insulated cores are cabled together. A 0.2mm thick layer of low-temperature ceramicized silicone rubber is extruded over a high-silica fiber rope, and the outer diameter of the extruded material is 1.02 times the diameter of the inscribed circle between the cable strands. Subsequently, a cable wrapping layer, a low-smoke halogen-free polyolefin inner sheath, and a low-smoke halogen-free polyolefin outer sheath are sequentially applied to obtain a fire-resistant power cable.

[0062] In this embodiment, the difference in softening point between the two glass powders is 320°C.

[0063] Example 2 The low-temperature ceramicized silicone rubber compound includes: 100 parts of methyl vinyl silicone rubber, 32.5 parts of phlogopite, 5.5 parts of borosilicate glass powder with a softening point of 540℃ and a D50 of 4μm, 13.75 parts of acicular wollastonite, 22.5 parts of magnesium hydroxide, 11.5 parts of fumed silica, 3.5 parts of zinc borate, 1.25 parts of silane coupling agent, and 1.3 parts of peroxide vulcanizing agent.

[0064] A 0.75mm thick low-temperature ceramicized silicone rubber layer is extruded over the main insulation layer and vulcanized to 20% by infrared heating.

[0065] The segmented locking strip is 17.5mm wide and 0.325mm thick. The through window section has three rows of diamond-shaped through windows with an opening rate of 35%. The length of the non-porous crack-stopping section is 0.85 times the width of the segmented locking strip.

[0066] The solid mass ratio of silica sol, boric acid, and γ-methacryloyloxypropyltrimethoxysilane in the interface treatment solution was 100:7:2. Drying at 115°C resulted in a dry weight gain of 4%.

[0067] The segmented locking tape is wrapped with 8N wrapping tension, with an overlap rate of 13%. The axial projection overlap rate of the through window segment is 10% through photoelectric recognition and wrapping head servo control.

[0068] The high-temperature ceramicized silicone rubber compound includes: 100 parts of methyl vinyl silicone rubber, 40 parts of phlogopite, 5.5 parts of low-alkali zinc borosilicate glass powder with a softening point of 760℃ and a D50 of 8.5μm, 10 parts of alumina short fibers, 23.375 parts of acicular wollastonite, 11.5 parts of fumed silica, 1.25 parts of silane coupling agent, and 1.3 parts of peroxide vulcanizing agent.

[0069] High-temperature ceramicized silicone rubber was extruded with a die head pressure of 7MPa, resulting in a through-window area filling rate of 85%, a minimum cross-sectional area of ​​1.5mm² for the radial key, and a high-temperature ceramicized silicone rubber layer thickness of 1.2mm.

[0070] The vulcanization process involves continuous microwave-hot air curing at 300℃ for 105 seconds.

[0071] The high-silica fiber rope is coated with low-temperature ceramicized silicone rubber with a thickness of 0.4 mm, and the outer diameter after coating is 1.05 times the diameter of the inscribed circle in the cabling gap. The remaining cabling and sheathing steps are the same as in Example 1.

[0072] In this embodiment, the difference in softening point between the two glass powders is 220°C.

[0073] Example 3 The low-temperature ceramicized silicone rubber compound includes: 100 parts of methyl vinyl silicone rubber, 40 parts of phlogopite, 8 parts of borosilicate glass powder with a softening point of 580℃ and a D50 of 6μm, 18 parts of needle-like wollastonite, 30 parts of magnesium hydroxide, 15 parts of fumed silica, 5 parts of zinc borate, 2 parts of silane coupling agent, and 1.8 parts of peroxide vulcanizing agent.

[0074] The thickness of the low-temperature ceramicized silicone rubber layer is 1.0 mm, and the degree of infrared pre-curing is 30%.

[0075] The segmented locking strip is 25mm wide and 0.45mm thick. The through window section has four rows of through windows with an opening rate of 42%. The length of the non-porous crack-stopping section is 1.2 times the width of the segmented locking strip.

[0076] The solid mass ratio of silica sol, boric acid and γ-methacryloxypropyltrimethoxysilane in the interface treatment solution was 100:10:3. After drying at 130℃, the dry weight gain was 6%.

[0077] The wrapping tension of the segmented locking tape is 12N, the overlap rate is 18%, and the axial projection of the through window segments in adjacent wrapping loops does not overlap.

[0078] The high-temperature ceramicized silicone rubber compound includes: 100 parts of methyl vinyl silicone rubber, 50 parts of phlogopite, 8 parts of low-alkali zinc borosilicate glass powder with a softening point of 720℃ and a D50 of 12μm, 14 parts of alumina short fibers, 25 parts of needle-like wollastonite, 15 parts of fumed silica, 2 parts of silane coupling agent, and 1.8 parts of peroxide vulcanizing agent.

[0079] The headstock rubber pressure is 10MPa, the through-window area fill rate is 95%, the minimum cross-sectional area of ​​the radial locking key is 2.5mm², and the thickness of the high-temperature ceramicized silicone rubber layer is 1.6mm.

[0080] The process involves continuous vulcanization using microwave-hot air at 340℃ for 180 seconds.

[0081] The high-silica fiber rope is coated with low-temperature ceramicized silicone rubber with a thickness of 0.6 mm, and the outer diameter after coating is 1.08 times the diameter of the inscribed circle in the cable gap. The remaining steps are the same as in Example 1.

[0082] In this embodiment, the difference in softening point between the two glass powders is 140°C.

[0083] Example 4 Except for the following parameters, the structure and process are the same as in Example 2.

[0084] The amount of glass powder in the low-temperature ceramicized silicone rubber layer is 8 parts, and the amount of needle-shaped wollastonite is 12 parts, with a mass ratio of 1.5:1; the D50 of the low-temperature glass powder is 2μm.

[0085] The high-temperature ceramicized silicone rubber layer contains 8 parts of glass powder and 20 parts of acicular wollastonite, with a mass ratio of 2.5:1; the high-temperature glass powder has a D50 of 5μm.

[0086] The softening point of low-temperature glass powder is 520℃, and the softening point of high-temperature glass powder is 780℃.

[0087] Example 5 Except for the following parameters, the structure and process are the same as in Example 2.

[0088] The amount of glass powder in the low-temperature ceramicized silicone rubber layer is 3 parts, and the amount of needle-shaped wollastonite is 10.5 parts, with a mass ratio of 3.5:1; the D50 of the low-temperature glass powder is 6μm.

[0089] The amount of glass powder in the high-temperature ceramicized silicone rubber layer is 3 parts, and the amount of needle-shaped wollastonite is 18 parts, with a mass ratio of 6:1; the D50 of the high-temperature glass powder is 12μm.

[0090] The softening point of low-temperature glass powder is 560℃, and the softening point of high-temperature glass powder is 740℃.

[0091] All the following comparative examples are based on Example 2. Unless otherwise specified, the raw materials, dimensions, layer thicknesses and preparation conditions are the same as in Example 2.

[0092] Comparative Example 1 The segmented locking strip in Example 2, which alternately sets through-window sections and non-porous crack-stopping sections along the strip length, is replaced with a high-silica fiber strip with uniformly opened diamond-shaped through-windows along its entire length.

[0093] The width, thickness, total porosity, overlap rate, and interface treatment of the replaced fiber tape are the same as in Example 2, except that the non-porous crack-stopping section is not provided.

[0094] Comparative Example 2 The segmented locking strip structure of Embodiment 2 is retained, but photoelectric recognition and phase servo adjustment are cancelled, so that the through window segments in adjacent wrapping loops are basically aligned along the cable axis, with an axial projection overlap rate of 68%.

[0095] Comparative Example 3 The extruder head pressure of the high-temperature ceramicized silicone rubber was reduced from 7 MPa to 0.5 MPa, while other conditions remained unchanged.

[0096] Under low extrusion pressure, the high-temperature ceramicized silicone rubber fills 8% of the area of ​​the through window, failing to form an effective radial locking key with a cross-sectional area of ​​0.5 mm².

[0097] Comparative Example 4 The glass powder in both the low-temperature ceramicized silicone rubber layer and the high-temperature ceramicized silicone rubber layer was replaced with the same low-alkali zinc borosilicate glass powder with a softening point of 760°C. The amount and particle size of the glass powder were kept the same as those in the corresponding layer of Example 2.

[0098] Comparative Example 5 The plasma activation step of the segmented locking band is retained, but the interface treatment solution consisting of silica sol, boric acid and silane coupling agent is not applied.

[0099] Comparative Example 6 The high-silica fiber rope and its external low-temperature ceramicized silicone rubber coating are retained, but the diameter of the high-silica fiber rope matrix is ​​reduced so that the outer diameter after coating is equal to the diameter of the inscribed circle of the cable gap, that is, the outer diameter ratio changes from 1.05 times to 1.00 times, and no radial preload is formed.

[0100] Comparative Example 7 In Example 2, the pre-vulcanization degree of the low-temperature ceramicized silicone rubber layer was increased from 20% to 50%, while the other conditions remained unchanged.

[0101] Due to the excessively high degree of cross-linking in the low-temperature ceramicized silicone rubber layer, the interfacial interdiffusion and co-curing between the high-temperature ceramicized silicone rubber and the low-temperature ceramicized silicone rubber after the high-temperature ceramicized silicone rubber passes through the window are restricted.

[0102] Performance testing This application takes the circuit integrity under the combined action of flame and mechanical impact as the core performance, and uses room temperature electrical performance, interlayer bonding performance, post-fired ceramic shell strength and flame spread performance as auxiliary verification indicators.

[0103] GB / T 19216.1—2021 applies to the line integrity test of cables with rated voltage of 0.6 / 1kV and below and outer diameter exceeding 20mm under the combined action of flame and impact vibration at a temperature not lower than 830℃. GB / T 12706.1—2020 applies to extruded insulated power cables with rated voltages of 1kV and 3kV; GB / T 18380.12—2022 is the test method for vertical flame propagation of a 1kW premixed type single-insulated wire and cable; GB / T 2791—1995 is the test method for T-peel strength of flexible materials to flexible materials; GB / T 44540—2024 is a notched ring test method for the elastic modulus and flexural strength of ceramic tubes or rings. GB / T 2951.13—2008 specifies the test methods for dimensions, water absorption and shrinkage of cable insulation and sheath materials.

[0104] 1. Voltage test of finished cable The voltage test procedure for finished cables shall be carried out in accordance with the provisions of GB / T 12706.1—2020.

[0105] The sample length should be no less than 10m. Apply an AC voltage of 3.5kV between the conductors and between the conductor and the water bath electrode, maintain for 5min, and record whether breakdown or flashover occurs.

[0106] 2. Circuit integrity test under combined flame and impact conditions Since the outer diameter of each finished sample is greater than 20 mm, the test was conducted in accordance with the test apparatus, sample installation method, fire supply method, impact method, circuit connection method and failure criteria specified in GB / T 19216.1—2021.

[0107] This application sets the ignition and impact verification time to a uniform 120 minutes, with power maintained for 15 minutes after ignition is stopped. 135 minutes is designated as the uniform upper limit for observation. The first failure time is recorded when a fuse trips, an indicator light goes out, a conductor breaks, or a short circuit occurs between conductors during the test; if no failure occurs after completing all 135 minutes of observation, it is recorded as "≥135 minutes".

[0108] The aforementioned 120 min plus 15 min is the unified verification window used for cross-sectional comparison of samples in this application, and is not to be interpreted as a fixed fire resistance rating specified by the national standard for all products.

[0109] After the test, a 1m long visual inspection was carried out on the fire-exposed section, and the number of visible cracks that penetrated the composite refractory layer and had an axial length greater than 5mm was counted.

[0110] 3. Interlayer T-peel strength Referring to GB / T 2791—1995, a strip sample with a width of 15mm was cut from the composite fire-resistant layer of the cable along the axial direction. The high-temperature ceramicized silicone rubber layer and the low-temperature ceramicized silicone rubber layer were clamped separately in an unfired state and T-shaped peeling was performed.

[0111] Since the segmented interlocking band and radial interlocking key are located between the two layers, the test results are the apparent peel strength under the combined action of interfacial chemical bonding, mechanical interlocking and radial interlocking key.

[0112] Five samples were tested in each group, and the arithmetic mean was taken.

[0113] Take another 1m long cable and bend it 20 times according to the bending procedure in GB / T 12706.1—2020 that is compatible with the finished cable. Then cut a sample to test the T-peel strength after bending.

[0114] 4. Flexural strength of the annular ceramic shell after firing The composite refractory layer sample was heated to 950℃ in air, held at that temperature for 30 minutes, and then naturally cooled to room temperature.

[0115] A complete annular ceramic shell with a length of 20 mm was obtained from the burned cable, and the end face was trimmed and a single notch was machined. The bending strength of the annular ceramic shell was determined according to the notched ring method of GB / T 44540—2024, under the same span and loading rate.

[0116] Since the post-firing product of this invention is a high-silica fiber-reinforced ceramic composite material, rather than a homogeneous fine ceramic, this test serves as a comparative auxiliary indicator for each group of samples under exactly the same conditions, and its results are not directly equivalent to the standard performance level of homogeneous fine ceramic materials.

[0117] 5. High-temperature linear shrinkage rate Low-temperature ceramicized silicone rubber compound and high-temperature ceramicized silicone rubber compound were vulcanized into strip-shaped samples with a length of 100 mm, a width of 10 mm, and a thickness of 2 mm, respectively.

[0118] According to the principles of dimensional measurement and shrinkage calculation in GB / T 2951.13—2008, the initial gauge length of the specimen was measured; the specimen was heated to 950℃ and held for 30 minutes, and the gauge length after burning was measured after cooling.

[0119] Linear shrinkage rate is calculated using the following formula: Linear shrinkage rate = (initial gauge length - gauge length after firing) ÷ initial gauge length × 100%.

[0120] The difference in linear shrinkage between the inner and outer layers is the absolute value of the difference in their linear shrinkage rates.

[0121] 6. Single cable flame vertical spread test The test shall be conducted according to the 1kW premixed flame test method specified in GB / T 18380.12—2022. The maximum length of the charred area shall be recorded, and the presence of continuous burning drips shall be observed.

[0122] Table 1

[0123] Table 2

[0124] As can be seen from Table 1, Examples 1 to 5 were all able to complete the uniformly set 120-minute fire impact and 15-minute continued power-on observation, indicating that the present invention can form an effective fire-resistant structure.

[0125] All samples passed the voltage test at room temperature, and the vertical combustion char length was also within a similar range. This indicates that the differences in the integrity of the circuits in each comparative example were not caused by room temperature insulation failure or significant differences in the flame retardant performance of the outer sheath, but mainly by the structural differences in the composite refractory layer.

[0126] In Comparative Example 1, after removing the non-porous crack-arresting section, although the total porosity, fiber tape thickness, and interlaminar peel strength were similar to those of Example 2, the circuit integrity time under flame impact decreased from no less than 135 min to 74 min, the number of through cracks increased to 7 / m, and the bending strength of the annular ceramic shell after firing decreased to 6.1 MPa. This indicates that uniform continuous openings can form crack propagation channels, and the non-porous crack-arresting section has a substantial effect on preventing cracks. In Comparative Example 2, only the through-window segments in adjacent wrapping rings were axially aligned, and its room temperature peel strength remained basically unchanged, but the circuit integrity time decreased to 86 min, and 6 through cracks / m appeared. This result shows that the through-windows themselves are not necessarily better the more regularly aligned they are; axial misalignment can break the continuous weak paths between different wrapping rings. In Comparative Example 3, only the extrusion pressure of the high-temperature ceramicized silicone rubber was reduced, causing the through-window filling rate to decrease from 85% to 8%, and no effective radial key was formed. The initial T-peel strength decreased from 7.6 N / mm to 2.0 N / mm, and further decreased to 0.9 N / mm after bending, with a circuit integrity time of only 49 min. This proves that simply sandwiching the segmented interlocking band between two layers of silicone rubber cannot achieve the same effect as co-curing through windows; radial interlocking is the key structure for maintaining interlayer integrity. In Comparative Example 4, after replacing both the inner and outer glass powders with the same glass powder with a softening point of 760℃, the room temperature interlayer bonding strength did not change significantly, but the difference in linear shrinkage rate between the inner and outer layers after firing increased to 6.1 percentage points, the bending strength of the annular ceramic shell after firing decreased to 5.4 MPa, and the circuit integrity time decreased to 68 min. This indicates that the softening point gradient of the present invention is not an arbitrary selection of two conventional glass powders, but is used to adapt to the radial temperature distribution of external heat and internal cold, and to coordinate the ceramicization sequence of the inner and outer layers. In Comparative Example 5, after removing the interface conversion coating, the initial T-peel strength and the T-peel strength after bending decreased to 3.1 N / mm and 1.5 N / mm, respectively. After firing, the ceramic shell could still form, but local detachment occurred between the high-silica fiber tape and the ceramic phase, reducing the line integrity time to 92 min. This indicates that the interface conversion coating simultaneously improved both the room-temperature organic interface and the high-temperature inorganic interface. Comparative Example 6, by only eliminating the pre-compression state at the center of the cable, showed little impact on the room-temperature interlayer peel strength, but radial displacement occurred in each insulated core during impact, reducing the line integrity time to 106 min. This result indicates that the pre-compressed high-silica fiber rope primarily contributes to the overall cable structural stability, rather than improving the interlayer adhesion of individual insulated cores. In Comparative Example 7, after increasing the pre-vulcanization degree of the low-temperature ceramicized silicone rubber layer to 50%, although high-temperature ceramicized silicone rubber still existed within the through-window, the co-vulcanization degree between the two layers decreased, and the initial and bending T-peel strengths decreased to 4.1 N / mm and 2.4 N / mm, respectively. This demonstrates that controlling the pre-vulcanization degree between 10% and 30% can balance the inner layer shape stability, outer layer through-window filling, and interlayer co-vulcanization.

[0127] As can be seen from the comprehensive embodiments and comparative examples, the advancement of the present invention is not simply an increase in the thickness of the refractory layer or the amount of inorganic filler, but rather a result of the synergistic effect of the following technical features: alternating arrangement of through-window sections and non-porous crack-stopping sections to prevent cracking; misalignment of through-window sections of adjacent wrapping rings to interrupt axially continuous weak paths; co-sulfurization through windows to form radial locking keys to maintain the integrity of the inner and outer layers; a glass powder softening point gradient that is lower inside and higher outside to adapt to the radial temperature gradient; and an interface conversion coating and a pre-compression filling structure to maintain the stability of the local interface and the overall cable structure, respectively.

[0128] Depend on Figure 1 It can be seen that the segmented interlocking band is located between the low-temperature ceramicized silicone rubber layer and the high-temperature ceramicized silicone rubber layer. The high-temperature ceramicized silicone rubber passes through the through-window of the segmented interlocking band from the outside, and forms radial interlocking keys extending along the thickness direction of the composite refractory layer within the through-window. The upper end of the radial interlocking key has a continuous transition morphology with the high-temperature ceramicized silicone rubber layer, and the lower end contacts the low-temperature ceramicized silicone rubber layer and forms an interlocking connection. High-silica fiber bundles around the through-window are distributed on both sides of the radial interlocking key and are covered by the surrounding silicone rubber matrix. No continuous delamination gap was observed between the radial interlocking key and the low-temperature ceramicized silicone rubber layer that runs through the entire connection area. The above microstructure indicates that the high-temperature ceramicized silicone rubber does not only cover the outer surface of the segmented interlocking band, but can pass through the through-window to form a solid connection structure across the segmented interlocking band, morphologically supporting the mechanical interlocking and interlayer constraint effect of the radial interlocking key on the inner and outer ceramicized silicone rubber layers.

[0129] Depend on Figure 2 As can be seen, after the composite refractory layer of Example 2 was kept at 950℃ for 30 min, the low-temperature ceramicized silicone rubber layer and the high-temperature ceramicized silicone rubber layer respectively formed porous ceramic bodies, and the high-silica fiber bundles in the segmented interlocking bands remained between the two ceramicized layers. The radial interlocking keys in the through-window formed ceramic bridges extending along the thickness direction of the composite refractory layer after high-temperature treatment. The upper end of the ceramic bridge was continuously connected to the high-temperature ceramicized layer, and the lower end was solidly connected to the low-temperature ceramicized layer, spanning the area where the segmented interlocking bands were located. The high-silica fiber bundles were distributed on both sides of the ceramic bridge after the radial interlocking keys were fired, and some fibers were covered and embedded by the surrounding ceramic phase. No annular delamination extending continuously along the entire interface was observed between the ceramic bridge after the radial interlocking keys were fired and the inner and outer ceramicized layers; only a small number of local pores or non-penetrating microcracks existed. The above results indicate that the radial interlocking keys can still form an inorganic connection structure spanning the segmented interlocking bands after the thermal decomposition of the silicone rubber organic phase, providing a structural basis for the inner and outer ceramicized layers to maintain their integrity at high temperatures.

[0130] Although the present invention has been described in conjunction with specific embodiments, any equivalent substitutions or conventional adjustments made by those skilled in the art to conductor specifications, main insulation materials, sheath materials, through-window shapes, number of cores in cable, and conventional processing conditions without departing from the concept of the present invention shall fall within the protection scope defined by the claims of the present invention.

Claims

1. A fire-resistant power cable, comprising at least one insulated core and a cabling wrapping layer, an inner sheath, and an outer sheath covering the insulated core, wherein the insulated core comprises a conductor, a main insulation layer, and a composite fire-resistant layer, characterized in that: The composite refractory layer comprises, from the inside out, a low-temperature ceramicized silicone rubber layer, a segmented locking strip, and a high-temperature ceramicized silicone rubber layer; the segmented locking strip is spirally wrapped and alternately arranged with through-window sections and non-porous crack-preventing sections along its length, with the through-window sections of adjacent wrapping rings offset along the cable axis; the high-temperature ceramicized silicone rubber layer passes through the through-window section and is co-vulcanized with the low-temperature ceramicized silicone rubber layer to form radial locking keys that pass through the segmented locking strip and are spaced apart along the axial direction; the softening point of the glass powder contained in the low-temperature ceramicized silicone rubber layer is 140–320°C lower than that of the glass powder contained in the high-temperature ceramicized silicone rubber layer.

2. The fire-resistant power cable according to claim 1, characterized in that: The segmented locking band is woven from high-silica fiber yarn with a silica content of not less than 94%, and has side ribs extending continuously along the length of the band on both sides; the through window section is located between the two side ribs, and each through window section has 2 to 4 rows of diamond-shaped through windows or rounded rectangular through windows, with an opening rate of 28% to 42%; the non-porous crack-preventing section runs across between the two side ribs, and the length of the non-porous crack-preventing section along the length of the band is 0.5 to 1.2 times the width of the segmented locking band; the width of the segmented locking band is 10 to 25 mm and the thickness is 0.20 to 0.45 mm.

3. The fire-resistant power cable according to claim 2, characterized in that: The wrapping overlap rate of the segmented locking strip is 8% to 18%, and when viewed along the cable axis, the projection overlap rate of the through window segment in adjacent wrapping rings is no more than 20%; the area filling rate of the through window by the high-temperature ceramicized silicone rubber layer is 75% to 95%, and a radial locking key is formed in each through window. The minimum cross-sectional area of ​​the radial locking key located in the plane of the segmented locking strip is 0.5 to 2.5 mm².

4. The fire-resistant power cable according to claim 1, characterized in that: The low-temperature ceramicized silicone rubber layer comprises the following raw materials in parts by weight: 100 parts methyl vinyl silicone rubber, 25-40 parts phlogopite, 3-8 parts borosilicate glass powder with a softening point of 500-580℃, 8-18 parts acicular wollastonite, 15-30 parts magnesium hydroxide, 8-15 parts fumed silica, 2-5 parts zinc borate, 0.5-2 parts silane coupling agent, and 0.8-1.8 parts peroxide vulcanizing agent; The high-temperature ceramicized silicone rubber layer comprises the following raw materials in parts by weight: 100 parts methyl vinyl silicone rubber, 30-50 parts phlogopite, 3-8 parts low-alkali zinc borosilicate glass powder with a softening point of 720-820℃, 6-14 parts alumina short fibers, 12-25 parts acicular wollastonite, 8-15 parts fumed silica, 0.5-2 parts silane coupling agent, and 0.8-1.8 parts peroxide vulcanizing agent.

5. The fire-resistant power cable according to claim 4, characterized in that: The glass powder particle size D50 in the low-temperature ceramicized silicone rubber layer is 2-6 μm, and the glass powder particle size D50 in the high-temperature ceramicized silicone rubber layer is 5-12 μm; the mass ratio of acicular wollastonite to glass powder in the low-temperature ceramicized silicone rubber layer is 1.5:1 to 3.5:1, and the mass ratio of acicular wollastonite to glass powder in the high-temperature ceramicized silicone rubber layer is 2.5:1 to 6:1, and the difference in linear shrinkage rate between the two samples after being kept at 950℃ for 30 min is no greater than 4 percentage points.

6. The fire-resistant power cable according to claim 1, characterized in that: The fiber surface, through-hole wall, and non-porous crack-arresting section of the segmented locking strip are provided with an interface conversion coating. The interface conversion coating is formed by silica sol, boric acid, and γ-methacryloyloxypropyltrimethoxysilane in a mass ratio of 100:4 to 10:1 to 3 based on solids. The dry weight gain of the interface conversion coating is 2% to 6% of the mass of the segmented locking strip.

7. The fire-resistant power cable according to claim 1, characterized in that: The thickness of the low-temperature ceramicized silicone rubber layer is 0.5–1.0 mm, and the thickness of the high-temperature ceramicized silicone rubber layer is 0.8–1.6 mm. When there are two or more insulated cores, a high-silica fiber rope covered with low-temperature ceramicized silicone rubber is provided in the cabling gap between the insulated cores. The coating thickness of the high-silica fiber rope is 0.2–0.6 mm, and its outer diameter after coating is 1.02–1.08 times the diameter of the tangent circle in the corresponding cabling gap, so as to form radial preload support after cabling.

8. A method for preparing a fire-resistant power cable as described in any one of claims 1-7, characterized in that, Includes the following steps: S1, twisting metal monofilaments to form a conductor, and extruding the main insulation layer on the outside of the conductor; S2, Low-temperature ceramicized silicone rubber containing glass powder with a softening point of 500-580℃ is extruded outside the main insulation layer to form a low-temperature ceramicized silicone rubber layer in an incompletely vulcanized state. S3, a segmented locking strip is spirally wrapped around the low-temperature ceramicized silicone rubber layer. The segmented locking strip has alternating through-window sections and non-porous crack-stopping sections along the length direction, and controls the through-window sections in adjacent wrapping rings to be misaligned along the cable axis. S4, pressure extrusion of high-temperature ceramicized silicone rubber containing glass powder with a softening point of 720-820℃, passing it through a through-window and contacting it with low-temperature ceramicized silicone rubber, and then co-curing the two layers of silicone rubber to form radial lock keys in the through-window to obtain an insulated wire core. S5 involves assembling the insulated wire cores into a cable, and sequentially forming the cable wrapping layer, inner sheath, and outer sheath.

9. The method for preparing the fire-resistant power cable according to claim 8, characterized in that: After forming the low-temperature ceramicized silicone rubber layer in step S2, the degree of vulcanization is increased to 10%–30% by infrared heating, and then step S3 is carried out with a wrapping tension of 4–12 N. In step S4, the extruder head rubber pressure is 4–10 MPa, the area filling rate of the high-temperature ceramicized silicone rubber to the through window is 75%–95%, and the co-vulcanization adopts a microwave-hot air continuous vulcanization method at 260–340℃ for a vulcanization time of 30–180 s.

10. The method for preparing the fire-resistant power cable according to claim 9, characterized in that: Before step S3, the segmented locking strip is activated by atmospheric pressure plasma, then dipped in an interface treatment solution prepared by silica sol, boric acid and γ-methacryloxypropyltrimethoxysilane in a mass ratio of 100:4 to 10:1 to 3 (based on solid mass), and dried at 100 to 130°C until the dry weight gain is 2% to 6%. In step S3, a photoelectric sensor is used to identify the leading edge position of the through window segment, and the rotation speed of the wrapping head is servo-adjusted according to the cable travel speed so that the axial projection overlap rate of the through window segment in adjacent wrapping rings is not greater than 20%.