航空航天用高压导线生产工艺
By combining fluorescence detection and silver plating polishing with a double-layer insulation design, the problem of partial discharge caused by surface defects in stranded conductors is solved, improving the insulation and oxidation resistance of the wires and making them suitable for the extreme environment of aerospace high-voltage power supplies.
Patent Information
- Application Number
- CN202611673978.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-28
- Publication Date
- 2026-11-24
AI Technical Summary
During the production process of existing high-voltage conductors for aerospace applications, defects such as burrs and protrusions may exist on the surface of the stranded conductors. These defects can become the starting point for partial discharge, corona discharge, and breakdown, leading to unstable performance of the conductors under extreme environments such as high altitude and low air pressure, wide temperature alternation, and high frequency vibration.
The process is monitored using fluorescent detection equipment. Defects in the stranded conductor are identified by an electric field-excited fluorescent layer. The surface quality of the conductor is improved by silver plating and electrolytic polishing. Then, a double-layer polyimide film is wrapped and an insulating layer is extruded to form a composite shielding layer to enhance the insulation performance.
It can effectively identify and repair defects in stranded conductors, reduce the risk of partial discharge and breakdown, improve the insulation, oxidation resistance and high-frequency conductivity of the conductors, and meet the long-term service requirements of complex aerospace environments.
Smart Images

Figure CN123161978A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of conductor technology, and in particular to a high-voltage conductor manufacturing process. Background Technology
[0002] High-voltage power supplies for aerospace vehicles, high-voltage electric propulsion for UAVs, in-satellite detection payloads, and high-voltage ignition systems for missiles have long been in service in high-altitude, low-pressure, wide-temperature alternation, high-frequency vibration, space radiation, aviation hydraulic oil, and fuel corrosion environments. The 50kV high-voltage level places stringent requirements on the insulation density, corona suppression, temperature resistance, mechanical creep resistance, and lightweighting of cables.
[0003] During the production of existing high-voltage conductors for aerospace applications, defects such as burrs and protrusions may exist on the surface of the stranded conductors. If these defects are directly introduced into the insulation extrusion process, they can become the starting point for partial discharge, corona discharge, and breakdown. Aerospace high-voltage conductors are extremely sensitive to corona discharge, partial discharge, and breakdown; therefore, it is necessary to detect defects in the stranded conductors in advance. Summary of the Invention
[0004] The purpose of this section is to outline some aspects of the embodiments of the present invention and to briefly introduce some preferred embodiments. Some simplifications or omissions may be made in this section, as well as in the abstract and title of the present application, to avoid obscuring the purpose of this section, the abstract and title of the invention. Such simplifications or omissions shall not be used to limit the scope of the present invention.
[0005] In view of the problems existing in the prior art, the present invention is proposed.
[0006] To solve the above-mentioned technical problems, the present invention provides the following technical solution:
[0007] Manufacturing process of high-voltage conductors for aerospace applications;
[0008] The process is monitored using a fluorescence detection device. The device includes a fluorescence excitation power supply and a fluorescence glass tube. The glass tube is open at both ends, serving as an inlet and an outlet, respectively. The inner diameter of the glass tube is 4.2-6.5 mm, and the outer diameter is 8-10 mm. A clamp for clamping one end of a stranded conductor is located inside the inlet, and another clamp for clamping one end of the stranded conductor is located outside the outlet. At least one clamp is conductive. A semi-transparent conductive metal layer is deposited on the inner side of the glass tube. A fluorescence layer, which is an electric field-excited electroluminescent fluorescent layer, is located inside the fluorescence layer. A protective glass tube with an inner diameter of 3.4-5.6 mm is located inside the fluorescence layer. The fluorescence excitation power supply... The source has two power output terminals, which are connected to a semi-transparent conductive metal layer and a conductive clamp, respectively. S1: A stranded conductor formed by twisting silver-plated copper wire is placed in a silver plating solution. The outer diameter of the stranded conductor is 0.4-1.2 mm. Electroplating is performed once, followed by electrolytic polishing, repeated at least twice. S2: After cleaning and drying, the stranded conductor is installed in a glass tube and clamped at both ends. S3: The fluorescence excitation power supply provides power, with the supply voltage controlled at 50%-80% of the voltage at which the entire stranded conductor excites the fluorescent layer to emit light. If a luminescent spot appears on the fluorescent layer of the glass tube, a defect is identified in the stranded conductor. S4: The stranded conductor is removed, and the defect location is locally mechanically polished using a cloth wheel, following the inspection in step S3.
[0009] The above design creates a relatively uniform electric field between the stranded conductor and the conductive metal layer. However, if defects such as burrs or protrusions are present on the surface of the stranded conductor, they can become the starting point for partial discharge if the conductor directly enters the insulation extrusion process. By utilizing an electric field-excited fluorescent layer, an electric field is created between the stranded conductor and the semi-transparent conductive metal layer. When defects such as burrs or protrusions exist on the stranded conductor, the electric field becomes locally concentrated, and the fluorescent layer is excited and emits light at the location of the concentrated electric field, thus visually identifying the defect. High-voltage conductors used in aerospace applications are highly sensitive to corona discharge, breakdown, and partial discharge. Fluorescent detection can eliminate defects in advance, reducing the risk of localized electric field concentration and breakdown within the insulation layer.
[0010] The semi-transparent conductive metal layer combines electrical conductivity and light transmission. Serving as one pole of the fluorescence excitation power source, it forms an electric field with the conductive clamps while allowing internal fluorescence to pass through, facilitating external observation or camera acquisition. The protective glass tube prevents the stranded conductor from directly scratching the fluorescent layer; simultaneously, the clamps at both ends of the glass tube tightly hold the stranded conductor, ensuring its stable and centered position within the glass tube during detection.
[0011] A stranded conductor is formed by twisting silver-plated copper wires. The stranded conductor is then immersed in a silver plating solution for the first silver plating. This process electroplats a layer of silver onto the surface of the stranded conductor and into the gaps between the individual wires, filling in microscopic pits created during the stranding process. Simultaneously, it integrates the existing silver plating layer with the new plating layer, eliminating the influence of surface oxide layers. After silver plating, the stranded conductor undergoes electrolytic polishing. Electrolytic polishing effectively removes any nodules, burrs, and deposits that may form during electroplating, achieving a mirror-like smooth surface. After the first electroplating and electrolytic polishing, the above steps are repeated for a second electroplating and electrolytic polishing cycle, at least twice. The first electroplating primarily repairs deep microscopic defects in the stranded conductor, filling larger pits; the first electrolytic polishing removes surface protrusions created by electroplating, resulting in a preliminary smooth surface; the second electroplating deposits a fine silver layer on the already smoothed surface, further filling in minor pits; and the second electrolytic polishing finally refines the surface, achieving a highly smooth and uniform finish.
[0012] First, silver plating is followed by electrolytic polishing, which repeatedly refines the surface of the stranded conductor, reducing surface roughness, burrs, and protrusions, thus minimizing defects at their source. Simultaneously, the silver plating layer significantly enhances the stranded conductor's oxidation resistance and high-frequency conductivity, meeting the requirements of long-term continuous operation in aerospace. The detection voltage is controlled at 50%-80% of the overall excitation emission level to avoid excessive voltage causing the entire stranded conductor to emit light and masking local defects, and also to avoid insufficient voltage failing to excite defect points, thereby improving defect identification sensitivity. Local mechanical polishing with a cloth wheel removes tiny burrs or protrusions, followed by re-inspection, forming a closed-loop process of detection, repair, and re-inspection.
[0013] Preferably, in step S5, the qualified stranded conductor is continuously wrapped with double-layer polyimide film to form a corona-resistant and pressure-equalizing inner layer. The thickness of a single layer of the corona-resistant and pressure-equalizing inner layer is 0.08-0.10 mm, the wrapping tension is 8-12 N, the overlap rate is 25%-30%, and it is low-temperature set at 60-80℃ after wrapping; in step S6, after the stranded conductor is wrapped with the corona-resistant and pressure-equalizing inner layer, it is simultaneously and integrally extruded with cross-linked ethylene-tetrafluoroethylene copolymer in a two-stage co-extrusion die to form a double-layer insulation layer. The extruder temperature gradient is controlled at 220-290℃, with the inner insulation extrusion pressure at 22-26MPa and the outer insulation extrusion pressure at 27-31MPa. The inner insulation thickness is 0.50-0.60mm, the outer insulation thickness is 0.50-0.60mm, and the total double insulation thickness is 1.0-1.2mm. After extrusion, the cable enters a cold water bath for constant temperature setting. Before the double insulation layer is extruded, the raw material particles of cross-linked ethylene-tetrafluoroethylene copolymer are heated in 80℃ hot air. Dry for 4 hours, controlling the moisture content to not exceed 0.02%; S7, uniformly transport the shaped cable to the electron beam irradiation channel for irradiation crosslinking, maintaining a nitrogen protective atmosphere in the electron beam irradiation channel. Apply a basic crosslinking dose of 60-90 kGy in the first stage; apply a supplementary crosslinking dose of 30-60 kGy in the second stage, and stabilize the total crosslinking dose of the first and second stages at 100-130 kGy; S8, clean the outer surface of the crosslinked cable with double insulation layer, uniformly coat it with conductive graphite emulsion, and then dry and cure it at a constant temperature of 100-120℃ to form a conductive uniform pressure coating; on the outside of the conductive uniform pressure coating, use silver-plated copper wire to braid to form a metal braided layer with a braiding coverage of 35%-40%, and after molding, obtain a composite shielding layer of conductive uniform pressure coating and metal braided layer; S9, use a single screw precision extruder to cover the outside of the composite shielding layer with a weather-resistant sheath of modified polyetheretherketone material with a thickness of 0.3-0.5 mm to form a complete conductor.
[0014] The double-layer polyimide film possesses high dielectric strength, high temperature resistance, and corona resistance. Its double-layer overlapping wrapping structure forms a continuous and stable electric field buffer zone, effectively and uniformly distributing the electric field strength on the stranded conductor surface. This suppresses 50kV high-voltage corona discharge and partial discharge phenomena at the source under high-altitude, low-pressure environments, thus strengthening the foundation of high-voltage insulation protection for conductors. The double-layer polyimide film is continuously overlapped, with each layer measuring 0.08-0.10mm, a wrapping tension of 8-12N, and an overlap rate of 25%-30%. This creates a relatively uniform corona-resistant, pressure-equalizing inner layer, alleviating electric field concentration on the stranded conductor surface. Low-temperature setting at 60-80℃ contributes to stable film layer bonding and reduces deformation during subsequent extrusion.
[0015] The cross-linked ethylene-tetrafluoroethylene copolymer is extruded simultaneously for both inner and outer layers, with an inner layer pressure of 22-26 MPa and an outer layer pressure of 27-31 MPa. This reduces interlayer bubbles, delamination, and interface defects, improving overall insulation integrity. The double-layer insulation is cross-linked by segmented electron beam irradiation to form a dense three-dimensional network structure, resulting in a structure free of micropores and delamination, exhibiting excellent creep resistance. It can withstand long-term operation in a wide temperature range of -65℃ to 200℃ and stably carry the continuous operating load of 50kV power frequency high voltage. The differentiated design of the double-layer gradient thickness allows the inner layer to focus on improving interlayer interface adhesion and the uniform pressure on the stranded conductor surface, while the outer layer focuses on strengthening mechanical protection and environmental isolation capabilities, synergistically ensuring the integrity, stability, and reliability of the high-voltage insulation system. The raw material particles are dried with hot air at 80℃ for 4 hours, resulting in a moisture content of less than 0.02%, which reduces defects such as bubbles and pinholes caused by moisture during extrusion.
[0016] The first stage involves basic crosslinking at 60-90 kGy, followed by a second stage at 30-60 kGy for supplementary crosslinking, with a total dose of 100-130 kGy. This approach ensures the degree of crosslinking while reducing excessive irradiation damage and improving the heat resistance and mechanical properties of the insulation layer.
[0017] The composite shielding layer of conductive uniform coating and metal braid can effectively suppress high-frequency electromagnetic interference, significantly reduce the overall weight of the shielding layer, and significantly improve the bending flexibility and spatial adaptability of the cable. It balances the high-voltage electric field shielding performance, electromagnetic compatibility performance and mechanical flexibility, and can be adapted to the complex, narrow and frequently bending cabling conditions in aerospace.
[0018] The weather-resistant sheath layer is made of modified polyetheretherketone (PEEK) material, with a thickness controlled at 0.3-0.5 mm. Modified PEEK material possesses high strength, low density, and high abrasion resistance. It can also withstand alternating high and low temperatures, corrosion from aviation hydraulic oil, and erosion from space ultraviolet and ionizing radiation. It exhibits extremely strong chemical stability and environmental adaptability. As the outermost protective structure of the cable, this sheath layer effectively isolates the insulation and shielding structure from damage caused by harsh external environments, ensuring the structural integrity and stable performance of the conductor during long-term service.
[0019] Preferably, during step S3, the voltage between the two power supply output terminals is gradually increased using the fluorescence excitation power supply. The minimum voltage value required to cause the entire fluorescent layer of the glass tube to emit light is recorded. The minimum voltage value is measured on at least three stranded conductors, and the average value is used as the reference voltage value. A gradually increasing test voltage is applied between the stranded conductor under test and the semi-transparent conductive metal layer. The upper limit of the test voltage is 50%-80% of the reference voltage value. If localized luminescence points appear on the fluorescent layer of the glass tube, a defect is determined to exist in the stranded conductor. Measuring the minimum overall luminescence voltage using at least three qualified or standard stranded conductors and using the average value as a reference reduces the influence of individual differences and power supply fluctuations. The 50%-80% reference voltage range serves as the upper limit of the test; this range can excite localized luminescence at defective points without causing the entire stranded conductor to emit light, facilitating the differentiation between localized defects and normal luminescence. The reference voltage value can be reused, facilitating the formation of a standardized testing procedure.
[0020] Preferably, during S1 electroplating and electrolytic polishing, the stranded conductor is placed in the silver plating solution, and the stranded conductor is used as the cathode to perform silver plating. The silver-plated stranded conductor is then used as the anode, and the silver plating solution is used as the electrolyte for electrolytic polishing. The silver plating and electrolytic polishing process is repeated 3-8 times. With each repetition, the silver plating time and the electrolytic polishing time are gradually shortened. The entire silver plating and electrolytic polishing process is completed within 60 minutes. Repeating the process 3-8 times gradually refines the surface, with multiple thin platings and light polishings, which makes it easier to obtain a uniform, dense, and smooth silver layer compared to a single thick plating followed by polishing. The gradually shortened time avoids over-plating or over-polishing, with the later stages focusing on fine finishing. This prevents the silver layer from becoming too thick, the stranded conductor from exceeding dimensional tolerances, or the silver layer from being excessively removed. Controlling the total time to 60 minutes avoids excessively long processes that could lead to oxidation, contamination, or low efficiency.
[0021] Preferably, before silver plating the stranded conductor in step S1, the entire stranded conductor is mechanically polished to remove surface burrs and protrusions. The polished stranded conductor is then cleaned with an organic solvent to remove surface impurities. After degreasing, the stranded conductor is placed in a 120-140℃ environment for low-temperature annealing to eliminate residual stranding stress and stabilize the conductor dimensions. Mechanical polishing quickly eliminates burrs and oxide protrusions on the stranded conductor surface, while low-temperature annealing at 120-140℃ stabilizes residual stranding stress. Annealing stabilizes conductor dimensions, reduces springback and deformation during subsequent insulation extrusion, significantly improves the surface smoothness and conductivity uniformity of the stranded conductor, and effectively suppresses electrical performance degradation caused by fretting wear of the stranded conductor.
[0022] Preferably, the diameter of the stranded conductor's single wire is 0.08-0.12 mm; the stranding pitch multiple is 8-16, and the compaction coefficient is 0.92-0.95; the silver plating solution contains a silver-cyanide complex, free potassium cyanide, and potassium carbonate; the silver concentration is 30-45 g / L, the free potassium cyanide concentration is 30-38 g / L, and the potassium carbonate concentration is 45-60 g / L; during the silver plating stage, the stranded conductor serves as the cathode, and the cathode current density is 0.5-3 A / dm³. 2 During the electrolytic polishing stage, the stranded conductor serves as the anode, with an anode current density of 0.5-3 A / dm³. 2 Silver plating and electropolishing both utilize a voltage of 2.5-3.5V. During both processes, the electrolyte is circulated and stirred at a speed of 100-400 RPM. The wires are 0.08-0.12mm monofilament, with a pitch ratio of 8-16 and a compaction coefficient of 0.92-0.95, balancing flexibility, conductivity, and structural density, making them suitable for aerospace high-voltage conductors. Silver-cyanide complexes provide silver ions, free potassium cyanide provides stability, and potassium carbonate enhances conductivity, contributing to a uniform silver layer. The conductivity is 0.5-3 A / dm³. 2 With a voltage of 2.5-3.5V, uniform silver plating and electropolishing can be achieved without excessive hydrogen evolution or charring. 100-400RPM can make the electrolyte concentration and temperature more uniform, reducing local unevenness in the plating.
[0023] Preferably, electropolishing employs a two-stage gradient current density; the first stage, the coarse polishing stage, has an anolyte current density of 1.5-3 A / dm³. 2 The duration is 10-60 seconds; the second stage of fine polishing: the anolyte current density gradually decreases to 0.5-1.5 A / dm³. 2 The duration is 30-180 seconds. Higher current density can accelerate the dissolution of surface protrusions, improve leveling efficiency, and avoid local over-polishing, silver layer damage, or conductor cross-section reduction caused by continuous high current; lower current density can finely trim the surface, reduce over-corrosion and pitting, and the smoother the stranded conductor surface and the more uniform the electric field distribution, the easier it is to identify the local luminescence of the fluorescent layer caused by electric field distortion at defect points.
[0024] The required immersion area of the stranded conductor for the current density is determined by the chemical silver plating calibration method. A section of stranded conductor is accurately weighed, silver-plated, polished, removed, cleaned, dried, and weighed after inspection for defects. The effective immersion area is calculated based on the weight gain and thickness of the plating.
[0025] Preferably, the outer wall of the glass tube is provided with scale lines along its length, and the scale lines are located between the clamps at the inlet and outlet of the glass tube. When a local luminescent spot appears on the fluorescent layer of the glass tube, the location of the defect point on the stranded conductor is determined according to the scale line corresponding to the luminescent spot. This enables the location of the defect point on the stranded conductor, allowing the operator to directly read the position and improve efficiency.
[0026] Preferably, the glass tube is placed in a darkroom for testing, and at least three cameras are arranged circumferentially around the glass tube. The signal output terminals of the cameras are connected to a microprocessor system. At least three scale lines are arranged around the circumference of the glass tube, with at least one scale line positioned at the location of each camera facing the glass tube. The semi-transparent conductive metal layer is transparent to light emitted from the fluorescent layer, and the cameras capture images of the luminescent points of the fluorescent layer through the semi-transparent conductive metal layer. The microprocessor system determines the location of the luminescent point based on the position of the camera receiving the luminescent signal and using the scale lines on the outer wall of the glass tube. The darkroom reduces ambient light interference, making it easier to identify weak luminescent points. At least three cameras can cover the circumference of the glass tube, preventing defects located on the back from being missed. The cameras can automatically analyze the location of the luminescent points, improving the automation and consistency of the detection process.
[0027] Preferably, the clamps at the inlet and outlet are rotatable clamps. These rotatable clamps are connected to a rotary drive mechanism, which is equipped with a control switch. The signal input of the control switch is connected to the control signal output of the microprocessor system. Based on the position of the local luminous point detected by the camera, the microprocessor system controls the rotary drive mechanism to rotate the stranded conductor, aligning the local luminous point with a predetermined scale line, and then stops the rotary drive mechanism. The microprocessor system determines the location of the defect point on the stranded conductor based on the position of the local luminous point on the scale line captured by the camera. By rotating the conductor, the luminous point is aligned with the predetermined scale line, avoiding misjudgment. The microprocessor-controlled rotary drive mechanism reduces manual operation, improves detection consistency and efficiency, and the rotation detection also prevents missed detection of luminous points.
[0028] Beneficial effects: By detecting the fluorescent layer of the fluorescent glass tube, defects such as burrs and protrusions can be identified, and repaired through localized mechanical polishing, reducing the risk of partial discharge and breakdown. Through a cycle of mechanical polishing, cleaning, annealing, silver plating, and electrolytic polishing, the surface quality and conductivity of the conductor are improved. The double-layer polyimide film possesses high dielectric strength, high temperature resistance, and corona resistance. The double-layer insulation layer is simultaneously extruded and cross-linked by segmented electron beam irradiation, enabling the double-layer insulation layer to withstand 50kV high voltage for extended periods. The composite shielding layer can effectively suppress high-frequency electromagnetic interference. The modified polyetheretherketone material possesses high strength, low density, and high wear resistance, while also being resistant to high and low temperature alternation, aviation hydraulic oil corrosion, and space ultraviolet irradiation and ionizing radiation erosion. Attached Figure Description
[0029] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort. Wherein:
[0030] Figure 1 This is a cross-sectional view of the fluorescent glass tube with stranded conductors installed in a manufacturing process for high-voltage conductors for aerospace applications according to the present invention.
[0031] Figure 2 This is a schematic diagram of the structure of a fluorescent glass tube with stranded conductors installed in a manufacturing process of a high-voltage conductor for aerospace applications according to the present invention.
[0032] Figure 3 This is a schematic cross-sectional view of the conductor structure in a manufacturing process for high-voltage conductors for aerospace applications according to the present invention.
[0033] In the diagram: 1. Fluorescent glass tube; 11. Glass tube; 12. Fluorescent layer; 13. Semi-transparent conductive metal layer; 14. Protective glass tube; 2. Clamp; 3. Stranded conductor; 4. Corona-resistant uniform voltage inner layer; 5. Double insulation layer; 51. Inner insulation layer; 52. Outer insulation layer; 6. Composite shielding layer; 7. Weather-resistant sheath. Detailed Implementation
[0034] To make the above-mentioned objectives, features and advantages of the present invention more readily understood, the specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings.
[0035] refer to Figures 1-2 Manufacturing process of high-voltage conductors for aerospace applications.
[0036] The process is monitored using a fluorescence detection device. The device includes a fluorescence excitation power supply and a fluorescence glass tube 1. The fluorescence glass tube 1 comprises a glass tube 11 with openings at both ends, serving as an inlet and an outlet, respectively. The inner diameter of the glass tube 11 is 4.2-6.5 mm, and the outer diameter is 8-10 mm. A clamp 2 for clamping one end of the stranded conductor 3 is provided inside the inlet, and another clamp 2 for clamping one end of the stranded conductor 3 is provided outside the outlet. At least one clamp 2 is a conductive clamp. A semi-transparent conductive metal layer 13 is deposited on the inner side of the glass tube 11. A fluorescence layer 12 is provided inside the semi-transparent conductive metal layer 13, and the fluorescence layer 12 is an electric field-excited electroluminescent fluorescence layer 12. A protective glass tube 14 is provided inside the fluorescence layer 12 to protect... The inner diameter of the glass tube 14 is 3.4-5.6 mm; the fluorescence excitation power supply has two power output terminals, which are respectively connected to the semi-transparent conductive metal layer 13 and the conductive clamp; S1, a stranded conductor 3 formed by twisting silver-plated copper wire is placed in a silver plating solution; the outer diameter of the stranded conductor 3 is 0.4-1.2 mm; electroplating is performed once, followed by electrolytic polishing, and the cycle is repeated at least twice; S2, after cleaning and drying, the stranded conductor 3 is installed in the glass tube 11 and clamped with the clamps 2 at both ends of the glass tube 11; S3, the fluorescence excitation power supply provides power, and the power supply voltage is controlled at 50%-80% of the voltage at which the fluorescence layer 12 is excited to emit light by the entire stranded conductor 3. If a light-emitting point appears in the fluorescence layer 12 of the glass tube 11, it is determined that there is a defect in the stranded conductor 3.
[0037] S4. Remove stranded conductor 3, and use a cloth wheel to perform local mechanical polishing on the defect location, and then perform the inspection in step S3.
[0038] In the above design, a relatively uniform electric field is formed between the stranded conductor 3 and the conductive metal layer. If defects such as burrs or protrusions on the surface of the stranded conductor 3 directly enter the insulation extrusion process, they will become the starting point of partial discharge. Using an electric field-excited fluorescent layer 12, an electric field is formed between the stranded conductor 3 and the semi-transparent conductive metal layer 13. When defects such as burrs or protrusions exist in the stranded conductor 3, the electric field becomes locally concentrated, and the fluorescent layer 12 will be excited and emit light at the concentrated location of the electric field, thus visually identifying the defect points. High-voltage conductors used in aerospace are very sensitive to corona, breakdown, and partial discharge. Fluorescent detection can eliminate defect points in advance, reducing the risk of subsequent local electric field concentration and breakdown within the insulation layer.
[0039] The semi-transparent conductive metal layer 13 has both conductive and light-transmitting functions. As one pole of the fluorescence excitation power source, it forms an electric field with the conductive clamp, while allowing internal fluorescence to pass through, facilitating external observation or camera acquisition. The protective glass tube 14 prevents the stranded conductor 3 from directly scratching the fluorescent layer 12; at the same time, the clamps 2 at both ends of the glass tube 11 clamp the stranded conductor 3, ensuring that the stranded conductor 3 remains centered and stable within the glass tube 11 during the detection process.
[0040] A stranded conductor 3 is formed by stranding silver-plated copper wires. The stranded conductor 3 is then immersed in a silver plating solution for the first silver plating. This plating coats the surface of the stranded conductor 3 and the gaps between the individual wires with a silver layer, filling in the microscopic pits created during the stranding process. Simultaneously, it integrates the existing silver plating layer with the new plating layer, eliminating the influence of the surface oxide layer. After silver plating, the stranded conductor 3 undergoes electrolytic polishing. Electrolytic polishing effectively removes any nodules, burrs, and deposits that may form during the electroplating process, achieving a mirror-like smooth surface. After the first electroplating and electrolytic polishing, the above electroplating and electrolytic polishing steps are repeated, i.e., a second electroplating and electrolytic polishing are performed, for at least two cycles. The first electroplating primarily repairs deep microscopic defects in the stranded conductor 3, filling larger pits; the first electrolytic polishing removes surface protrusions created by electroplating, resulting in a preliminary smooth surface; the second electroplating deposits a fine silver layer on the already smoothed surface, further filling in minor pits; and the second electrolytic polishing finally refines the surface, achieving a highly smooth and uniform state.
[0041] First, silver plating is followed by electrolytic polishing, which repeatedly refines the surface of the stranded conductor 3, reducing surface roughness, burrs, and protrusions, thus minimizing defects at the source. Simultaneously, the silver plating layer significantly enhances the stranded conductor 3's oxidation resistance and high-frequency conductivity, meeting the requirements of long-term continuous operation in aerospace. The detection voltage is controlled at 50%-80% of the overall excitation emission level to avoid excessively high voltage causing the entire stranded conductor 3 to emit light and masking local defects, and also to avoid excessively low voltage failing to excite defect points, thereby improving defect identification sensitivity. Local mechanical polishing with a cloth wheel removes tiny burrs or protrusions from defect points, followed by re-inspection, forming a closed-loop process of detection, repair, and re-inspection.
[0042] In use, silver-plated copper wire is first stranded to form a stranded conductor 3, with the outer diameter of the stranded conductor 3 controlled between 0.4-1.2 mm. The stranded conductor 3 is then immersed in a silver plating solution for electroplating, followed by electrolytic polishing. This process is repeated at least twice to repeatedly refine the surface of the stranded conductor 3, reduce surface roughness, minimize burrs and protrusions, and improve its oxidation resistance and high-frequency conductivity. Subsequently, the stranded conductor 3 is cleaned and dried, and then placed into a fluorescent glass tube 1. The stranded conductor 3 passes through the inlet and outlet openings at both ends of the glass tube 11. One end of the stranded conductor 3 is clamped by a clamp 2 inside the inlet and another clamp 2 outside the outlet, respectively. At least one clamp 2 is a conductive clamp, ensuring that the stranded conductor 3 is centered within the glass tube 11 and does not contact the protective glass tube 14. The semi-transparent conductive metal layer 13 inside the fluorescent glass tube 1 and the conductive clamps are connected to the two power output terminals of the fluorescent excitation power supply. Then, the fluorescence excitation power supply is turned on, and a detection voltage is applied between the semi-transparent conductive metal layer 13 and the conductive clamp, forming an electric field between the outer surface of the stranded conductor 3 and the semi-transparent conductive metal layer 13.
[0043] Because the fluorescent layer 12 uses an electric field-excited electroluminescent material, the electric field is relatively uniform in the normal area, and the fluorescent layer 12 emits only weak light or no light at all. When there are defects such as burrs or protrusions in the stranded conductor 3, the electric field at the defect location becomes locally concentrated, causing the fluorescent layer 12 at the corresponding location to show obvious luminescent points or bright spots. Operators can directly observe through the outside of the glass tube 11, or use image acquisition equipment such as cameras or industrial cameras to acquire fluorescence images through the semi-transparent conductive metal layer 13 and the protective glass tube 14, thereby locating the axial and circumferential positions of the defect points.
[0044] After the test is completed, the fluorescence excitation power supply is turned off, the clamp 2 is loosened, and the stranded conductor 3 is removed. For the points identified as defective, a cloth wheel is used for localized mechanical polishing, and after cleaning and drying, the conductors are reinstalled in the fluorescent glass tube 1. The conductors are then re-inspected through the fluorescent glass tube 1 until no abnormal luminescence points are found. Stranded conductors 3 that pass the re-inspection proceed to subsequent insulation extrusion processes. Stranded conductors 3 that cannot be repaired or still show defects after re-inspection are discarded or cut off to ensure the reliability of aerospace high-voltage conductors in terms of corona, partial discharge, and breakdown.
[0045] Example 1: Reference Figure 3 This is the first embodiment of the present invention.
[0046] Preferably, in step S5, the qualified stranded conductor 3 is continuously wrapped with double-layer polyimide film to form a corona-resistant and uniformly pressed inner layer 4. The thickness of a single layer of the corona-resistant and uniformly pressed inner layer 4 is 0.08-0.10 mm, the wrapping tension is 8-12 N, the overlap rate is 25%-30%, and it is low-temperature set at 60-80℃ after wrapping; in step S6, after the stranded conductor 3 is wrapped with the corona-resistant and uniformly pressed inner layer 4, it is simultaneously and integrally extruded with cross-linked ethylene-tetrafluoroethylene copolymer in a two-stage co-extrusion die head to form a double-layer insulation layer. 5. The extruder temperature gradient is controlled at 220-290℃, with the inner insulation layer 51 extrusion pressure at 22-26MPa and the outer insulation layer 52 extrusion pressure at 27-31MPa. The thickness of the inner insulation layer 51 is 0.50-0.60mm, the thickness of the outer insulation layer 52 is 0.50-0.60mm, and the total thickness of the double insulation layers is 1.0-1.2mm. After extrusion, the cable enters a cold water bath for constant temperature setting. Before extrusion of the double insulation layer 5, the raw material particles of the cross-linked ethylene-tetrafluoroethylene copolymer are... S7. Dry the cable with hot air at 80℃ for 4 hours, controlling the moisture content to not exceed 0.02%; S8. Transport the shaped cable to the electron beam irradiation channel at a uniform speed for irradiation crosslinking, maintaining the nitrogen protective atmosphere of the electron beam irradiation channel. Apply a basic crosslinking dose of 60-90kGy in the first stage; apply a supplementary crosslinking dose of 30-60kGy in the second stage, and stabilize the total crosslinking dose of the first and second stages at 100-130kGy; S9. Clean the outer surface of the crosslinked cable with double insulation layer 5, uniformly coat it with conductive graphite emulsion, and then dry and cure it in a constant temperature environment of 100-120℃ to form a conductive uniform pressure coating; on the outside of the conductive uniform pressure coating, use silver-plated copper wire to braid to form a metal braided layer with a braiding coverage of 35%-40%, and after molding, obtain a composite shielding layer 6 of conductive uniform pressure coating and metal braided layer; S0. Use a single screw precision extruder to coat the outside of the composite shielding layer 6 with a weather-resistant sheath 7 of modified polyether ether ketone material with a thickness of 0.3-0.5mm to form a complete conductor.
[0047] The double-layer polyimide film possesses high dielectric strength, high temperature resistance, and corona resistance. Its double-layer overlapping wrapping structure forms a continuous and stable electric field buffer zone, effectively and uniformly distributing the electric field strength on the surface of the stranded conductor 3. This suppresses 50kV high-voltage corona discharge and partial discharge phenomena at the source under high-altitude, low-pressure conditions, thus strengthening the foundation for high-voltage insulation protection of the conductor. The double-layer polyimide film continuously overlaps and wraps, with each layer measuring 0.08-0.10mm, a wrapping tension of 8-12N, and an overlap rate of 25%-30%. This forms a relatively uniform corona-resistant, pressure-equalizing inner layer 4, alleviating the concentration of the electric field on the surface of the stranded conductor 3. Low-temperature setting at 60-80℃ helps stabilize the film layer adhesion and reduces deformation during subsequent extrusion.
[0048] The cross-linked ethylene-tetrafluoroethylene copolymer is extruded simultaneously for both inner and outer layers, with an inner layer pressure of 22-26 MPa and an outer layer pressure of 27-31 MPa. This reduces interlayer bubbles, delamination, and interface defects, improving overall insulation performance. The double-layer insulation layer 5 is cross-linked by segmented electron beam irradiation to form a dense three-dimensional network structure. It is free of micropores and delamination, exhibiting excellent creep resistance and can withstand long-term operation in a wide temperature range of -65℃ to 200℃, stably carrying the continuous operating load of 50kV power frequency high voltage. The differential design of the double-layer gradient thickness allows the inner layer to focus on improving interlayer interface adhesion and surface pressure uniformity of the stranded conductor 3, while the outer layer focuses on strengthening mechanical protection and environmental isolation capabilities, synergistically ensuring the integrity, stability, and reliability of the high-voltage insulation system. The raw material particles are dried with hot air at 80℃ for 4 hours, with a moisture content of less than 0.02%, reducing defects such as bubbles and pinholes caused by moisture during extrusion.
[0049] The first stage involves basic crosslinking at 60-90 kGy, followed by a second stage at 30-60 kGy for supplementary crosslinking, with a total dose of 100-130 kGy. This approach ensures the degree of crosslinking while reducing excessive irradiation damage and improving the heat resistance and mechanical properties of the insulation layer.
[0050] The composite shielding layer 6, consisting of a conductive uniform coating and a metal braided layer, can effectively suppress high-frequency electromagnetic interference, significantly reduce the overall weight of the shielding layer, and significantly improve the bending flexibility and spatial adaptability of the cable. It balances the shielding performance of high-voltage electric fields, electromagnetic compatibility performance, and mechanical flexibility, and can be adapted to the complex, narrow, and frequently bending cabling conditions in aerospace.
[0051] The weather-resistant sheath consists of 7 layers made of modified polyetheretherketone (PEEK) material, with a thickness controlled between 0.3-0.5 mm. Modified PEEK material possesses high strength, low density, and high abrasion resistance, while also withstanding high and low temperature alternation, aviation hydraulic oil corrosion, and space ultraviolet and ionizing radiation erosion. It exhibits extremely strong chemical stability and environmental adaptability. As the outermost protective structure of the cable, this sheath layer effectively isolates the insulation and shielding structure from damage caused by harsh external environments, ensuring the structural integrity and stable performance of the conductor during long-term service.
[0052] In use, the qualified stranded conductor 3 is first wrapped with a double layer of polyimide film in continuous overlapping to form a corona-resistant and uniform inner layer 4. The thickness of a single layer of film is controlled at 0.08-0.10mm, the wrapping tension is 8-12N, and the overlap rate is 25%-30%. After wrapping, it is low-temperature sizing at 60-80℃ to make the film layer adhere stably and form a continuous and uniform electric field buffer zone, which alleviates the concentration of electric field on the surface of the stranded conductor 3 and suppresses corona discharge and partial discharge in high-altitude low-pressure environments from the source.
[0053] Subsequently, the stranded conductor 3, with the corona-resistant and uniformly pressed inner layer 4 wound around it, is fed into a two-stage co-extrusion die head, where a double-layer insulation layer 5 is simultaneously and integrally extruded using cross-linked ethylene-tetrafluoroethylene copolymer. Before extrusion, the cross-linked ethylene-tetrafluoroethylene copolymer raw material particles are dried in hot air at 80℃ for 4 hours, controlling the moisture content to not exceed 0.02%. The extruder temperature gradient is controlled at 220-290℃, the extrusion pressure of the inner insulation 51 is 22-26MPa, the extrusion pressure of the outer insulation 52 is 27-31MPa, the thickness of the inner insulation 51 is 0.50-0.60mm, the thickness of the outer insulation 52 is 0.50-0.60mm, and the total thickness of the double insulation is 1.0-1.2mm. After extrusion, the cable is placed in a cold water bath for constant temperature setting to reduce interlayer bubbles, delamination, and interface defects, thereby improving the overall insulation performance.
[0054] The shaped cable is uniformly fed into the electron beam irradiation channel for cross-linking, maintaining a nitrogen protective atmosphere within the channel. A basic cross-linking dose of 60-90 kGy is applied in the first stage, and a supplementary cross-linking dose of 30-60 kGy is applied in the second stage. The total cross-linking dose for both stages is stabilized at 100-130 kGy, enabling the double insulation layer 5 to form a dense three-dimensional network structure. This ensures the degree of cross-linking while reducing excessive irradiation damage and improving the insulation layer's heat resistance and mechanical properties.
[0055] Next, the outer surface of the cross-linked cable with double insulation layer 5 is cleaned and dust removed, and conductive graphite emulsion is evenly coated and dried and cured at a constant temperature of 100-120℃ to form a conductive uniform pressure coating. Then, silver-plated copper wire is braided on the outside of the conductive uniform pressure coating to form a metal braided layer with a braiding coverage of 35%-40%, thus obtaining a composite shielding layer 6 of conductive uniform pressure coating and metal braided layer, which is used to effectively suppress high-frequency electromagnetic interference and take into account shielding performance, electromagnetic compatibility performance and mechanical flexibility.
[0056] Finally, a weather-resistant sheath 7 made of modified polyetheretherketone (PEEK) material, with a thickness of 0.3-0.5 mm, is coated on the outside of the composite shielding layer 6 using a single-screw precision extrusion unit to form a complete conductor. The modified PEEK sheath has high strength, low density, and high wear resistance, and can withstand high and low temperature alternation, aviation hydraulic oil corrosion, and space ultraviolet radiation and ionizing radiation erosion. As the outermost protective structure, it effectively isolates the insulation layer and shielding structure from damage caused by harsh external environments, ensuring the conductor maintains structural integrity and stable performance during long-term service in the complex, confined, and frequently bending wiring conditions of aerospace applications, and stably bears the continuous operating load of 50kV power frequency high voltage.
[0057] Example 2: Reference Figures 1-2 This is the second embodiment of the present invention, which is based on the previous embodiment.
[0058] Preferably, during step S3, the voltage between the two power supply output terminals is gradually increased using the fluorescence excitation power supply, and the minimum voltage value required to cause the entire fluorescent layer 12 of the glass tube 11 to emit light is recorded. The minimum voltage value is measured on at least three stranded conductors 3, and the average value is taken as the reference voltage value. A gradually increasing test voltage is applied between the stranded conductor 3 to be tested and the semi-transparent conductive metal layer 13. The upper limit of the test voltage is 50%-80% of the reference voltage value. If local luminescence points appear on the fluorescent layer 12 of the glass tube 11, it is determined that there is a defect in the stranded conductor 3. Measuring the minimum overall luminescence voltage using at least three qualified or standard stranded conductors 3 and taking the average value as a reference reduces the influence of individual differences and power supply fluctuations. The 50%-80% reference voltage as the upper limit of the test range can excite local luminescence at defect points without causing the entire stranded conductor 3 to emit light, making it easy to distinguish between local defects and normal luminescence. The reference voltage value can be reused, facilitating the formation of a standardized testing procedure.
[0059] Preferably, during S1 electroplating and electrolytic polishing, the stranded conductor 3 is placed in the silver plating solution, and the stranded conductor 3 is used as the cathode to perform silver plating. The silver-plated stranded conductor 3 is then used as the anode, and the silver plating solution is used as the electrolyte for electrolytic polishing. The silver plating and electrolytic polishing process is repeated 3-8 times. With each repetition, the silver plating time and the electrolytic polishing time are gradually shortened. The entire silver plating and electrolytic polishing process is completed within 60 minutes. Repeating the process 3-8 times gradually refines the surface. Multiple thin platings and multiple light polishings make it easier to obtain a uniform, dense, and smooth silver layer than a single thick plating followed by polishing. The gradually shortened time avoids over-plating or over-polishing. The later stages focus on fine finishing to prevent excessively thick silver layers, out-of-tolerance dimensions of the stranded conductor 3, or excessive removal of the silver layer. Controlling the total time to 60 minutes avoids excessively long processes that could lead to oxidation, contamination, or low efficiency.
[0060] Preferably, before silver plating the stranded conductor 3 in step S1, the stranded conductor 3 is mechanically polished to remove surface burrs and protrusions; the polished stranded conductor 3 is then cleaned with an organic solvent to remove surface impurities; after degreasing, the stranded conductor 3 is placed in a 120-140℃ environment for low-temperature annealing to eliminate residual stranding stress and stabilize the dimensions of the stranded conductor 3. Mechanical polishing quickly eliminates burrs and oxide protrusions on the surface of the stranded conductor 3, while low-temperature annealing at 120-140℃ stabilizes residual stranding stress. Annealing can stabilize the conductor dimensions, reduce springback and deformation during subsequent insulation extrusion, significantly improve the surface smoothness and conductivity uniformity of the stranded conductor 3, and effectively suppress the electrical performance degradation caused by fretting wear of the stranded conductor 3.
[0061] Preferably, the diameter of the stranded conductor 3 is 0.08-0.12 mm; the stranding pitch is 8-16, and the compaction coefficient is 0.92-0.95; the silver plating solution contains a silver-cyanide complex, free potassium cyanide, and potassium carbonate; the silver concentration is 30-45 g / L, the free potassium cyanide concentration is 30-38 g / L, and the potassium carbonate concentration is 45-60 g / L; during the silver plating stage, the stranded conductor 3 serves as the cathode, and the cathode current density is 0.5-3 A / dm³. 2 During the electrolytic polishing stage, stranded conductor 3 serves as the anode, with an anode current density of 0.5-3 A / dm³. 2 Silver plating and electropolishing both utilize a voltage of 2.5-3.5V. During both processes, the electrolyte is circulated and stirred at a speed of 100-400 RPM. The wires are 0.08-0.12mm monofilament, with a pitch ratio of 8-16 and a compaction coefficient of 0.92-0.95, balancing flexibility, conductivity, and structural density, making them suitable for aerospace high-voltage conductors. Silver-cyanide complexes provide silver ions, free potassium cyanide provides stability, and potassium carbonate enhances conductivity, contributing to a uniform silver layer. The conductivity is 0.5-3 A / dm³. 2 With a voltage of 2.5-3.5V, uniform silver plating and electropolishing can be achieved without excessive hydrogen evolution or charring. 100-400RPM can make the electrolyte concentration and temperature more uniform, reducing local unevenness in the plating.
[0062] Preferably, electropolishing employs a two-stage gradient current density; the first stage, the coarse polishing stage, has an anolyte current density of 1.5-3 A / dm³. 2 The duration is 10-60 seconds; the second stage of fine polishing: the anolyte current density gradually decreases to 0.5-1.5 A / dm³. 2 The duration is 30-180 seconds. Higher current density can accelerate the dissolution of surface protrusions, improve leveling efficiency, and avoid local over-polishing, silver layer damage, or conductor cross-section reduction caused by continuous high current; lower current density can finely trim the surface, reduce over-corrosion and pitting, and the smoother the surface of stranded conductor 3, the more uniform the electric field distribution, and the easier it is to identify the local luminescence of fluorescent layer 12 caused by electric field distortion at defect points.
[0063] The required immersion area of the stranded conductor 3 for the current density is determined by the chemical silver plating calibration method. A section of stranded conductor 3 is accurately weighed, silver-plated, polished, removed, cleaned, dried, and weighed after inspection for defects. The effective immersion area is calculated based on the weight gain and thickness of the plating.
[0064] Before silver plating the stranded conductor 3, the entire stranded conductor 3 is mechanically polished to remove surface burrs and protrusions. After polishing, the stranded conductor 3 is cleaned with an organic solvent to remove surface impurities and oil. After degreasing, the stranded conductor 3 is placed in a 120-140℃ environment for low-temperature annealing and shaping to eliminate residual stress, stabilize the size of the stranded conductor 3, reduce springback and deformation during subsequent insulation extrusion, improve the surface flatness and conductivity uniformity of the stranded conductor 3, and suppress the deterioration of electrical performance caused by fretting wear of the stranded conductor 3.
[0065] The stranded conductor 3 is formed by stranding silver-plated copper wires with a single wire diameter of 0.08-0.12mm to balance flexibility, conductivity, and structural compactness, meeting the requirements for high-voltage conductors in aerospace applications. The stranded conductor 3 is placed in a silver plating solution; during the silver plating and electrolytic polishing processes, the electrolyte is circulated and stirred at a speed of 100-400 RPM to ensure more uniform electrolyte concentration and temperature, reducing uneven local plating.
[0066] The silver plating and electropolishing cycles are repeated 3-8 times; with each repetition, the silver plating time and the electropolishing time are gradually shortened, and the entire silver plating and electropolishing process is completed within 60 minutes. The electropolishing employs a two-stage gradient current density: the anolyte current density in the first stage rough polishing is 1.5-3 A / dm³. 2 The duration is 10-60 seconds; the anode current density in the second-stage fine polishing section gradually decreases to 0.5-1.5 A / dm³. 2 The duration is 30-180 seconds. Higher current densities can accelerate the dissolution of surface protrusions, improve leveling efficiency, and avoid local over-polishing, silver layer damage, or conductor cross-section reduction caused by consistently high current. Lower current densities can finely trim the surface, reduce over-corrosion and pitting, making the surface of stranded conductor 3 smoother and the electric field distribution more uniform, which facilitates subsequent fluorescence detection to identify defects. The required immersion area of stranded conductor 3 for the current density is determined using the chemical silver plating calibration method. A section of stranded conductor 3 is accurately weighed, silver-plated and polished, then removed, cleaned, dried, and weighed again after inspection for defects. The effective immersion area is calculated based on the weight gain and thickness of the plating.
[0067] After silver plating, electrolytic polishing, cleaning, and drying, the stranded conductor 3 is inserted into the fluorescent glass tube 1 and clamped with clamps 2 at both ends to ensure the stranded conductor 3 is centrally and stably positioned within the glass tube 11. During testing, the voltage between the two power supply output terminals of the fluorescent excitation power supply is gradually increased, and the minimum voltage value required to cause the entire fluorescent layer 12 of the glass tube 11 to emit light is recorded. The minimum voltage value is measured on at least three qualified or standard stranded conductors 3, and the average value is taken as the reference voltage value. Subsequently, a gradually increasing test voltage is applied between the stranded conductor 3 under test and the semi-transparent conductive metal layer 13, with the upper limit of the test voltage being 50%-80% of the reference voltage value. If local luminescence points appear on the fluorescent layer 12 of the glass tube 11, the stranded conductor 3 is deemed to have a defect; if no local luminescence points appear, the stranded conductor 3 is deemed qualified. This method can reduce the impact of individual differences and power fluctuations. The 50%-80% reference voltage as the upper limit of the test can excite local light emission at the defect point without causing the entire stranded conductor 3 to light up, making it easy to distinguish between local defects and normal light emission. In addition, the reference voltage value can be reused, which facilitates the formation of a standardized testing process.
[0068] After detecting defects, the stranded conductor 3 is removed, and the defective area is locally mechanically polished using a cloth wheel. After cleaning and drying, it is reinstalled and retested at a test voltage of 50%-80% of the aforementioned reference voltage value until no local luminous points are found. The stranded conductor 3 that passes the retest is then further processed according to Example 1, including wrapping the double-layer polyimide film corona-resistant uniform pressure inner layer 4, synchronously extruding the cross-linked ethylene-tetrafluoroethylene copolymer double-layer insulation layer 5, segmented electron beam irradiation cross-linking, preparation of the conductive uniform pressure coating and metal braided composite shielding layer 6, and coating with the modified polyetheretherketone weather-resistant sheath 7, ultimately forming a complete conductor.
[0069] Example 3: Reference Figures 1-2 This is the third embodiment of the present invention, which is based on the previous embodiment.
[0070] Preferably, the outer wall of the glass tube 11 is provided with scale lines along its length, and the scale lines are located between the clamp 2 at the inlet and the clamp 2 at the outlet of the glass tube 11. When a local luminescent point appears on the fluorescent layer 12 of the glass tube 11, the location of the defect point on the stranded conductor 3 is determined according to the scale line corresponding to the luminescent point. This enables the location of the defect point on the stranded conductor 3, allowing the operator to directly read the position and improving efficiency.
[0071] Preferably, the glass tube 11 is placed in a darkroom for testing. At least three cameras are arranged around the circumference of the glass tube 11, and the signal output terminals of the cameras are connected to a microprocessor system. At least three scale lines are arranged around the circumference of the glass tube 11, with at least one scale line positioned at the location of each camera facing the glass tube 11. The semi-transparent conductive metal layer 13 is transparent to light emitted from the fluorescent layer 12, and the cameras capture images of the luminescent points of the fluorescent layer 12 through the semi-transparent conductive metal layer 13. The microprocessor system determines the location of the luminescent point based on the position of the camera receiving the luminescent signal and using the scale lines on the outer wall of the glass tube 11. The darkroom reduces ambient light interference, making weak luminescent points easier to identify. At least three cameras can cover the circumference of the glass tube 11, preventing defects located on the back from being missed. The cameras can automatically analyze the location of the luminescent points, improving the automation and consistency of the detection process.
[0072] Preferably, the clamps 2 at the inlet and outlet are rotatable clamps 2; the rotatable clamps 2 are connected to a rotary drive mechanism, which is equipped with a control switch. The signal input terminal of the control switch is connected to the control signal output terminal of the microprocessor system; the microprocessor system controls the rotary drive mechanism to drive the stranded conductor 3 to rotate according to the position of the local light-emitting point detected by the camera, so that the local light-emitting point is aligned with a set scale line, and then controls the rotary drive mechanism to stop; the microprocessor system determines the position of the defect point on the stranded conductor 3 based on the position of the local light-emitting point on the scale line captured by the camera. By rotating the conductor, the light-emitting point is aligned with the set scale line, avoiding misjudgment. The microprocessor controls the rotary drive mechanism, reducing manual operation, improving detection consistency and efficiency, and the rotation detection also avoids missing any light-emitting points.
[0073] In use, at least three graduation lines are provided on the outer wall of the glass tube 11 along its length. The graduation lines are located between the inlet clamp 2 and the outlet clamp 2. The entire fluorescent glass tube 1 is placed in a dark room to reduce ambient light interference and make the faint luminous points easier to identify. At least three cameras are arranged around the circumference of the glass tube 11. The signal output terminals of the cameras are connected to the microprocessor system. Each camera facing the glass tube 11 corresponds to at least one graduation line. The semi-transparent conductive metal layer 13 is transparent to the light emitted by the fluorescent layer 12, and the cameras can capture images of the luminous points of the fluorescent layer 12 through the semi-transparent conductive metal layer 13.
[0074] When the fluorescence excitation power supply is turned on, if the stranded conductor 3 has defects such as burrs or protrusions, the electric field at the defect location will be locally concentrated, causing localized luminescence points to appear on the corresponding fluorescent layer 12. A camera captures images of the luminescence points on the fluorescent layer 12 through the semi-transparent conductive metal layer 13 and transmits the signals to the microprocessor system. Based on the camera position receiving the luminescence signal and the scale lines on the outer wall of the glass tube 11, the microprocessor system determines the axial and circumferential positions of the luminescence points, thereby locating the defects on the stranded conductor 3. At least three cameras can cover the circumference of the glass tube 11, preventing defects located on the back side from being missed, thus improving the automation and consistency of the detection process.
[0075] The clamps 2 at the inlet and outlet are rotatable clamps 2, connected to a rotary drive mechanism. This rotary drive mechanism has a control switch, whose signal input is connected to the control signal output of the microprocessor system. When the camera detects a localized luminous point, the microprocessor system controls the rotary drive mechanism to rotate the stranded conductor 3 according to the point's position, aligning the localized luminous point with a predetermined scale line. Then, the system stops the rotary drive mechanism. The microprocessor system then determines the axial and circumferential positions of the defect point on the stranded conductor 3 based on the camera's view of the localized luminous point on that scale line. Aligning the luminous point with the predetermined scale line by rotating the conductor avoids misjudgments, reduces manual operation, improves detection consistency and efficiency, and prevents missed detections of luminous points.
[0076] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the technical solutions of the present invention, and all such modifications or substitutions should be covered within the scope of the claims of the present invention.
Claims
1. A manufacturing process for high-voltage conductors used in aerospace, characterized by: Process monitoring is performed using fluorescence detection equipment; The fluorescence detection device includes a fluorescence excitation power supply and a fluorescence glass tube (1). The fluorescent glass tube (1) includes a glass tube (11) with openings at both ends, which serve as an inlet and an outlet, respectively. The inner diameter of the glass tube (11) is 4.2-6.5 mm, and the outer diameter of the glass tube (11) is 8-10 mm; A clamp (2) for clamping one end of the stranded conductor (3) is provided inside the inlet, and another clamp (2) for clamping one end of the stranded conductor (3) is provided outside the outlet. At least one clamp (2) is a conductive clamp. The inner side of the glass tube (11) is coated with a semi-transparent conductive metal layer (13). A fluorescent layer (12) is provided inside the semi-transparent conductive metal layer (13), and the fluorescent layer (12) is an electric field-excited electroluminescent fluorescent layer (12). A protective glass tube (14) is provided inside the fluorescent layer (12), and the inner diameter of the protective glass tube (14) is 3.4-5.6 mm; The fluorescence excitation power supply is provided with two power output terminals, which are respectively connected to the semi-transparent conductive metal layer (13) and the conductive clamp; S1. A stranded conductor (3) formed by twisting silver-plated copper wire is placed in a silver plating solution. Stranded conductor (3) outer diameter 0.4-1.2mm; First, perform electroplating, then electropolishing, repeating the process at least twice; S2. After cleaning and drying the stranded conductor (3), install it into the glass tube (11) and clamp it with the clamps (2) at both ends of the glass tube (11); S3. The fluorescent excitation power supply provides power, and the power supply voltage is controlled at 50%-80% of the voltage at which the fluorescent layer (12) is excited to emit light by the entire stranded conductor (3). If the fluorescent layer (12) of the glass tube (11) shows a light-emitting point, it is determined that there is a defect in the stranded conductor (3). S4. Remove the stranded conductor (3), and use a cloth wheel to perform local mechanical polishing on the defect location, and then perform the inspection in step S3.
2. The manufacturing process for high-voltage conductors for aerospace applications according to claim 1, characterized in that: During step S3, the fluorescence excitation power supply is used to gradually increase the voltage value between the two power supply output terminals, and the minimum voltage value that causes the entire fluorescent layer (12) of the glass tube (11) to emit light is recorded. Take at least three stranded conductors (3) and measure the minimum voltage value respectively, and take the average value as the reference voltage value; A gradually increasing test voltage is applied between the stranded conductor (3) to be tested and the semi-transparent conductive metal layer (13); The upper limit of the test voltage is 50%-80% of the reference voltage value; If local light-emitting spots appear on the fluorescent layer (12) of the glass tube (11), it is determined that there are defects in the stranded conductor (3).
3. The manufacturing process for high-voltage conductors for aerospace applications according to claim 1, characterized in that: During S1 electroplating and electrolytic polishing, the stranded conductor (3) is placed in the silver plating solution, and the stranded conductor (3) is used as the cathode to perform silver plating by passing an electric current through it. The silver-plated stranded conductor (3) is used as the anode, and the silver plating solution is used as the electrolyte. Electrolytic polishing is performed by passing an electric current through the conductor. Silver plating and electropolishing, repeated 3-8 times; Each time the process was repeated, the silver plating time and the electropolishing time were shortened successively. The entire silver plating and electropolishing process is completed within 60 minutes.
4. The manufacturing process for high-voltage conductors for aerospace applications according to claim 1, characterized in that: S5. The qualified stranded conductor (3) is continuously wrapped with double-layer polyimide film to form a corona-resistant and uniform pressure inner layer (4). The thickness of a single layer of the corona-resistant and uniform pressure inner layer (4) is 0.08-0.10 mm, the wrapping tension is 8-12 N, the overlap rate is 25%-30%, and it is low temperature set at 60-80℃ after wrapping. S6. After the stranded conductor (3) is wound with the corona-resistant and uniformly pressed inner layer (4), it is simultaneously extruded in a two-stage co-extrusion die head using cross-linked ethylene-tetrafluoroethylene copolymer to form a double-layer insulation layer (5). The temperature gradient of the extruder is controlled at 220-290℃. The extrusion pressure of the inner insulation (51) is 22-26MPa, and the extrusion pressure of the outer insulation (52) is 27-31MPa. The thickness of the inner insulation (51) is 0.50-0.60mm, and the thickness of the outer insulation (52) is 0.50-0.60mm. The total thickness of the double insulation is 1.0-1.2mm. After extrusion, the cable enters the cold water bath for constant temperature shaping. Before extruding the double-layer insulation layer (5), the raw material particles of the cross-linked ethylene-tetrafluoroethylene copolymer were dried in hot air at 80°C for 4 hours, and the moisture content was controlled to not exceed 0.02%. S7. The shaped cable is uniformly transported to the electron beam irradiation channel for irradiation crosslinking. The nitrogen protective atmosphere of the electron beam irradiation channel is maintained. The basic crosslinking dose of 60-90kGy is applied in the first stage. In the second stage, a supplementary crosslinking dose of 30-60 kGy is applied, and the total crosslinking dose of the first and second stages is stabilized at 100-130 kGy. S8. The outer surface of the cable with cross-linked double insulation layer (5) is cleaned and dust removed, and conductive graphite emulsion is evenly coated. Then, it is dried and cured in a constant temperature environment of 100-120℃ to form a conductive uniform pressure coating. Outside the conductive uniform pressure coating, a metal braided layer is formed by weaving silver-plated copper wire, with a braiding coverage of 35%-40%. After forming, a composite shielding layer of conductive uniform pressure coating and metal braided layer is obtained (6). S9. The outer side of the composite shielding layer (6) is covered with a weather-resistant sheath (7) made of modified polyether ether ketone material using a single screw precision extrusion unit, with a thickness of 0.3-0.5mm, forming a complete conductor.
5. The manufacturing process for high-voltage conductors for aerospace applications according to claim 1, characterized in that: Before silver plating the stranded conductor (3) in step S1, the stranded conductor (3) is mechanically polished as a whole to remove surface burrs and protrusions; The polished stranded conductor (3) is cleaned with an organic solvent to remove surface impurities; After degreasing, the stranded conductor (3) is placed in a low-temperature annealing environment of 120-140℃ to eliminate residual stress and stabilize the size of the stranded conductor (3).
6. The manufacturing process for high-voltage conductors for aerospace applications according to claim 1, characterized in that: The diameter of the single wire in the stranded conductor (3) is 0.08-0.12 mm; The twisting pitch multiple is 8-16, and the compression coefficient is 0.92-0.95; The silver plating solution contains a silver cyanide complex, free potassium cyanide, and potassium carbonate; Silver concentration 30-45 g / L, free potassium cyanide 30-38 g / L, potassium carbonate 45-60 g / L; During the silver plating stage, the stranded conductor (3) serves as the cathode, with a cathode current density of 0.5-3 A / dm. 2 ; During the electropolishing stage, the stranded conductor (3) serves as the anode, with an anode current density of 0.5-3 A / dm³. 2 Silver plating uses a voltage of 2.5-3.5V, and electrolytic polishing uses a voltage of 2.5-3.5V. During the silver plating and electropolishing processes, the electrolyte is circulated and stirred at a speed of 100-400 RPM.
7. The manufacturing process for high-voltage conductors for aerospace applications according to claim 1, characterized in that: Electropolishing employs a two-stage gradient current density. First stage coarse polishing section: Anode current density is 1.5-3 A / dm² 2 The duration is 10-60 seconds; Second stage of fine polishing: Anode current density gradually decreases to 0.5-1.5 A / dm³ 2 The duration is 30-180 seconds.
8. The manufacturing process for high-voltage conductors for aerospace applications according to claim 1, characterized in that: The outer wall of the glass tube (11) is provided with scale lines along its length, and the scale lines are located between the clamp (2) at the inlet and the clamp (2) at the outlet of the glass tube (11). When a local luminous spot appears on the fluorescent layer (12) of the glass tube (11), the location of the defect point on the stranded conductor (3) is determined according to the scale line corresponding to the luminous spot.
9. The manufacturing process for high-voltage conductors for aerospace applications according to claim 8, characterized in that: The glass tube (11) was placed in a dark room for testing. At least three cameras are arranged circumferentially along the glass tube (11), and the signal output terminals of the cameras are connected to the microprocessor system; At least three scale lines are arranged around the circumference of the glass tube (11), and at least one scale line is provided at the position of a camera facing the glass tube (11); The semi-transparent conductive metal layer (13) is transparent to the light emitted by the fluorescent layer (12), and the camera captures images of the light-emitting points of the fluorescent layer (12) through the semi-transparent conductive metal layer (13); The microprocessor system determines the position of the light-emitting point by using the scale lines on the outer wall of the glass tube (11) based on the position of the camera that receives the light-emitting signal.
10. The manufacturing process for high-voltage conductors for aerospace applications according to claim 9, characterized in that: The clamps (2) at the inlet and outlet are rotatable clamps (2); The rotatable chuck (2) is connected to a rotary drive mechanism, which is equipped with a control switch. The signal input terminal of the control switch is connected to the control signal output terminal of the microprocessor system. The microprocessor system controls the rotation drive mechanism to drive the stranded conductor (3) to rotate according to the position of the local light-emitting point detected by the camera, so that the local light-emitting point is aligned with a set scale line, and controls the rotation drive mechanism to stop. The microprocessor system determines the position of the defect point on the stranded conductor (3) based on the position of the local light-emitting point captured by the camera on the scale line.