Heat-resistant reinforced MPP power protection pipe and preparation method thereof

By setting different sections along the axial direction of the MPP power protection pipe and controlling the continuous change of material composition, the problem of mutual constraint between heat resistance and heat fusion connection performance was solved, and the overall performance of the heat-resistant reinforced MPP power protection pipe was improved.

CN123161990APending Publication Date: 2026-11-24YANGZHOU LITAI PIPE IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611654332.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-26
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

The existing MPP power protection pipes use basically the same material composition along the pipe body axis, which leads to mutual constraints between heat resistance and load-bearing capacity and pipe end heat fusion connection performance, making it difficult to achieve both simultaneously.

Method used

A first pipe end welding section, a first continuous transition section, a heat-resistant bearing section, a second continuous transition section, and a second pipe end welding section are set along the pipe body axis. Different mixtures are transported through independent metering and feeding paths to control the continuous change of the content of heat-resistant reinforcing components and heat-oxygen stabilizers, forming an integral pipe wall.

Benefits of technology

While maintaining the heat resistance and load-bearing capacity of the main body of the pipe, the performance of the hot-melt connection at the pipe end is improved, the impact of direct abrupt changes in material composition on the continuity of axial load is reduced, and the impact of multiple thermal effects on the stability of the hot-melt connection at the pipe end is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123161990A_ABST
    Figure CN123161990A_ABST
Patent Text Reader

Abstract

This invention relates to the field of power cable protection pipe technology, and discloses a heat-resistant reinforced MPP power protection pipe and its manufacturing method. The protection pipe includes a first pipe end welding section, a first continuous transition section, a heat-resistant load-bearing section, a second continuous transition section, and a second pipe end welding section, sequentially arranged and integrally extruded along the pipe body axis. The content of heat-resistant reinforcing components in the first and second pipe end welding sections is lower than that in the heat-resistant load-bearing section. The content of heat-resistant reinforcing components in the first and second continuous transition sections varies continuously along the pipe body axis. During manufacturing, a first mixture and a second mixture are fed to the same extruder through independent metering feed paths. The feed ratio is periodically changed to form a low-reinforcing component strip, which is then cut at the axial midpoint. This maintains the heat-resistant load-bearing performance of the main pipe body while also ensuring the heat-fusion connection performance of the pipe ends.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of power cable protection pipe technology, specifically to a heat-resistant enhanced MPP power protection pipe and its preparation method. Background Technology

[0002] MPP power protection pipes are typically made from polypropylene as the main raw material, produced through modification and extrusion molding, and are mainly used for the protection of power cables. During trenchless construction and underground cable laying, MPP power protection pipes, in addition to bearing the loads from the soil and construction, may also be affected by the heat generated by the cable operation and changes in ambient temperature. Therefore, existing technologies typically improve the heat resistance of the pipes by adding inorganic fillers, fiber reinforcement materials, or other modified components to the polypropylene matrix. Simultaneously, due to the limited length of a single pipe, it is usually necessary to heat-melt the ends of adjacent pipes during construction to form a continuous cable protection channel.

[0003] Existing MPP power protection pipes typically use a basically consistent material composition along the pipe body axis. When the heat resistance of the main body is improved by increasing the content of heat-resistant reinforcing components, the content of heat-resistant reinforcing components in the hot-melt zone at the pipe end also increases simultaneously, which can easily affect the fusion bonding between polypropylene matrices during the hot-melt process. On the other hand, reducing the content of heat-resistant reinforcing components to meet the requirements of hot-melt connection at the pipe end will reduce the heat resistance of the main body. Therefore, existing pipe materials cannot simultaneously achieve both the heat resistance of the main body and the hot-melt connection performance at the pipe end. Summary of the Invention

[0004] To address the shortcomings of existing technologies, this invention provides a heat-resistant reinforced MPP power protection pipe and its preparation method, solving the problem that existing MPP power protection pipes use a basically consistent material composition along the pipe body axis, which leads to a mutual constraint between improving the heat-bearing capacity of the main body and maintaining the heat fusion connection performance of the pipe ends.

[0005] To achieve the above objectives, the present invention provides the following technical solution: A heat-resistant reinforced MPP power protection pipe includes a first pipe end welding section, a first continuous transition section, a heat-resistant load-bearing section, a second continuous transition section, and a second pipe end welding section, which are sequentially arranged along the pipe body axis and integrally extruded. The heat-resistant load-bearing section includes a polypropylene matrix and a heat-resistant reinforcing component dispersed in the polypropylene matrix. The first pipe end fusion section and the second pipe end fusion section both include a polypropylene matrix, and the content of the heat-resistant reinforcing component in the first pipe end fusion section and the second pipe end fusion section is lower than the content of the heat-resistant reinforcing component in the heat-resistant load-bearing section. The content of the heat-resistant reinforcing component is based on 100 parts by weight of the polypropylene matrix at the corresponding position. The content of the heat-resistant reinforcing component in the first continuous transition section increases continuously from the first pipe end fusion section toward the heat-resistant bearing section, and the content of the heat-resistant reinforcing component in the second continuous transition section decreases continuously from the heat-resistant bearing section toward the second pipe end fusion section, so that the first pipe end fusion section, the first continuous transition section, the heat-resistant bearing section, the second continuous transition section and the second pipe end fusion section form an integral pipe wall that continuously changes along the pipe body axis.

[0006] Furthermore, the polypropylene matrix of the heat-resistant load-bearing section is composed of homopolymer polypropylene and block copolymer polypropylene. Based on 100 parts by weight of the polypropylene matrix, the homopolymer polypropylene is 55 to 70 parts by weight, and the block copolymer polypropylene is 30 to 45 parts by weight.

[0007] Furthermore, the heat-resistant reinforcing component includes calcined kaolin and chopped alkali-free glass fiber. Based on 100 parts by weight of the polypropylene matrix in the heat-resistant load-bearing section, the calcined kaolin comprises 8 to 14 parts by weight, and the chopped alkali-free glass fiber comprises 5 to 9 parts by weight.

[0008] Furthermore, the polypropylene matrix of both the first pipe end weld section and the second pipe end weld section is composed of homopolymer polypropylene and block copolymer polypropylene. Based on 100 parts by weight of the polypropylene matrix, the homopolymer polypropylene is 30 to 45 parts by weight and the block copolymer polypropylene is 55 to 70 parts by weight.

[0009] Furthermore, the heat-resistant reinforcing component content in the first pipe end weld section and the second pipe end weld section is 10% to 30% of the heat-resistant reinforcing component content in the heat-resistant bearing section, respectively.

[0010] Furthermore, the content of block copolymer polypropylene in the first continuous transition section decreases continuously from the first pipe end welding section toward the heat-resistant bearing section, and the content of block copolymer polypropylene in the second continuous transition section increases continuously from the heat-resistant bearing section toward the second pipe end welding section.

[0011] Furthermore, the heat-resistant bearing section, the first pipe end welding section, and the second pipe end welding section each contain a heat-oxygen stabilizer. The content of the heat-oxygen stabilizer is based on 100 parts by weight of the polypropylene matrix at the corresponding position. The content of the heat-oxygen stabilizer in the first pipe end welding section and the second pipe end welding section is 1.3 to 2.5 times that in the heat-resistant bearing section.

[0012] Furthermore, the heat-oxidation stabilizer includes hindered phenolic antioxidants and phosphite antioxidants; based on 100 parts by weight of polypropylene matrix in each section, under the condition of satisfying the aforementioned heat-oxidation stabilizer content ratio, the heat-oxidation stabilizer in the heat-resistant bearing section is 0.3 to 0.7 parts by weight, and the heat-oxidation stabilizer in the first pipe end welding section and the second pipe end welding section is 0.6 to 1.2 parts by weight, respectively.

[0013] Furthermore, the axial lengths of the first pipe end welding section and the second pipe end welding section are 80 to 250 mm, respectively, and the axial lengths of the first continuous transition section and the second continuous transition section are 150 to 600 mm, respectively.

[0014] This invention also provides a method for preparing a heat-resistant reinforced MPP power protection tube, comprising: S1, prepare a first mixture and a second mixture respectively. Both the first mixture and the second mixture include a polypropylene matrix. Based on 100 parts by weight of the polypropylene matrix in each mixture, the content of the heat-resistant reinforcing component in the first mixture is higher than the content of the heat-resistant reinforcing component in the second mixture. S2, the first mixture and the second mixture are fed to the same extruder through independent metering and feeding paths, and continuously extruded by the extruder to form a tube; S3, when forming the heat-resistant bearing section, the feeding ratio of the first mixture is higher than that of the second mixture and the feeding ratio is kept stable, so that the content of the heat-resistant reinforcing component in the heat-resistant bearing section remains stable. S4, when a continuous transition section is formed on both sides of the heat-resistant bearing section, the feeding ratio of the first mixture and the second mixture is continuously changed, and a low-reinforcement component band is formed between two adjacent heat-resistant bearing sections. The content of heat-resistant reinforcing component in the low-reinforcement component band is lower than that in the heat-resistant bearing section, so that the content of heat-resistant reinforcing component continuously decreases from the heat-resistant bearing section toward the low-reinforcement component band, and continuously increases from the low-reinforcement component band toward the adjacent heat-resistant bearing section. S5, the feeding ratio of the first mixture and the second mixture is repeatedly changed according to the length cycle of the continuous extrusion of the tube body. The axial middle position of the low-reinforcement component strip is determined as the predetermined cutting position. The continuously extruded tube body is cut at the predetermined cutting position, so that the tube end welding sections of two adjacent heat-resistant reinforced MPP power protection tubes are formed on both sides of the cutting position. Thus, each heat-resistant reinforced MPP power protection tube sequentially forms a first tube end welding section, a first continuous transition section, a heat-resistant bearing section, a second continuous transition section, and a second tube end welding section along the tube body axial direction.

[0015] This invention provides a heat-resistant reinforced MPP power protection tube and its preparation method. It has the following beneficial effects: 1. This invention forms a first pipe end fusion section, a first continuous transition section, a heat-resistant load-bearing section, a second continuous transition section, and a second pipe end fusion section along the axial direction of the heat-resistant reinforced MPP power protection pipe. The heat-resistant reinforced component content in the first and second pipe end fusion sections is lower than that in the heat-resistant load-bearing section. This ensures that the heat-resistant load-bearing section, which bears the main radial load, maintains a high heat-resistant reinforced component content, while the first and second pipe end fusion sections, which require heat fusion connection, use a lower heat-resistant reinforced component content. Thus, while maintaining the heat-resistant load-bearing performance of the main pipe body, the heat fusion connection performance of the pipe ends is also taken into account, solving the problem of mutual constraints between the two types of performance when the entire pipe body is composed of a uniform material.

[0016] 2. This invention causes the content of heat-resistant reinforcing components in the first continuous transition section to increase continuously from the first pipe end fusion section toward the heat-resistant bearing section, and causes the content of heat-resistant reinforcing components in the second continuous transition section to decrease continuously from the heat-resistant bearing section toward the second pipe end fusion section. At the same time, the content of block copolymer polypropylene changes continuously along the corresponding direction, thereby reducing the impact of the direct abrupt change in material composition between the heat-resistant bearing section and the first and second pipe end fusion sections on the continuity of axial bearing capacity.

[0017] 3. The present invention makes the content of heat-oxygen stabilizer in the first pipe end welding section and the second pipe end welding section higher than the content of heat-oxygen stabilizer in the heat-resistant bearing section, so as to correspond to the multiple thermal histories formed by the first pipe end welding section and the second pipe end welding section through extrusion molding and subsequent hot-melt connection, thereby reducing the impact of multiple thermal effects on the stability of the pipe end hot-melt connection.

[0018] 4. The present invention feeds the first and second mixtures to the same extruder through independent metering and feeding paths, and changes the feeding ratio of the first and second mixtures according to the length of continuous extrusion of the tube body. A low-reinforcement component strip is formed between two adjacent heat-resistant bearing sections, and the low-reinforcement component strip is cut at a predetermined cutting position, so that the tube end welding section of two adjacent heat-resistant reinforced MPP power protection tubes is formed on both sides of the cutting position, thereby enabling the formation of an integral tube body with axially differentiated material composition during continuous extrusion. Attached Figure Description

[0019] Figure 1 This is a flowchart illustrating the preparation method of a heat-resistant reinforced MPP power protection tube according to the present invention. Figure 2 The diagram shows a comparison of the high-temperature annular heat compression forces of Examples 1 to 4 and Comparative Examples 1 to 5. Figure 3The figures show a comparison of the tensile strength of the thermofused joints in Examples 1 to 4 and Comparative Examples 1 to 5, and the tensile strength of the thermofused joints after thermo-oxidative aging. Detailed Implementation

[0020] The present invention will be further described in detail below with reference to the accompanying drawings and embodiments.

[0021] In trenchless power cable laying, MPP power protection pipes not only require high heat-bearing capacity, but also, due to the limited length of a single pipe, often need to be connected by heat fusion to form a continuous pipeline on the construction site. During their research on heat-resistant reinforced MPP power protection pipes, the inventors discovered that these two performance requirements place different demands on the pipe material composition. Increasing the content of heat-resistant reinforcing components in the polypropylene matrix improves the pipe's ability to withstand radial loads at higher temperatures. However, when the heat-resistant reinforcing components are also present in the heat-fusion region at the pipe ends, it reduces the conditions for sufficient fusion bonding between the polypropylene matrix components during the heat fusion process, creating a trade-off between improving heat-bearing capacity and maintaining the heat-fusion connection performance at the pipe ends.

[0022] Further research revealed that the main reason for the aforementioned problems lies in the fact that existing MPP power protection pipes typically use a basically consistent material composition along the pipe's axial direction; that is, the main body of the pipe and the pipe ends, which require further heat fusion, use the same material system. When heat-resistant reinforcing components are added to improve the overall heat-bearing capacity of the pipe, the heat-resistant reinforcing components at the pipe ends also increase simultaneously. Conversely, when the heat-resistant reinforcing components are reduced to improve the heat fusion connection performance at the pipe ends, the heat-bearing capacity of the main body of the pipe, which bears the main radial load, decreases. Furthermore, the pipe ends require further thermal action after extrusion molding, resulting in a different thermal history compared to the main body of the pipe.

[0023] Based on the above findings, this invention does not use the same material composition for the entire heat-resistant reinforced MPP power protection pipe. Instead, the heat-resistant reinforced MPP power protection pipe includes a first pipe end welding section, a first continuous transition section, a heat-resistant load-bearing section, a second continuous transition section, and a second pipe end welding section, which are sequentially arranged along the pipe body axis and integrally extruded. The heat-resistant reinforcing component content in the heat-resistant load-bearing section is higher than that in the first and second pipe end welding sections, so that the heat-resistant load-bearing section mainly corresponds to the heat resistance requirements of the pipe body, and the first and second pipe end welding sections mainly correspond to the subsequent hot-melt connection requirements.

[0024] Simultaneously, this invention ensures that the content of the heat-resistant reinforcing component in the first continuous transition section increases continuously from the first pipe end fusion section towards the heat-resistant bearing section, and that the content of the heat-resistant reinforcing component in the second continuous transition section decreases continuously from the heat-resistant bearing section towards the second pipe end fusion section. Correspondingly, the content of block copolymer polypropylene in the first continuous transition section decreases continuously from the first pipe end fusion section towards the heat-resistant bearing section, and the content of block copolymer polypropylene in the second continuous transition section increases continuously from the heat-resistant bearing section towards the second pipe end fusion section. This avoids direct abrupt changes in material composition between the heat-resistant bearing section and the first and second pipe end fusion sections.

[0025] Based on this, the present invention further addresses the need for the first and second pipe end welding sections to undergo multiple thermal histories through extrusion molding and subsequent hot-melt connection. This is achieved by making the content of heat-oxygen stabilizers in the first and second pipe end welding sections higher than that in the heat-resistant bearing section, thus differentiating the thermal histories experienced at different axial positions from the perspective of material composition.

[0026] To enable the aforementioned different axial positions to be integrally formed under continuous production conditions, this invention prepares a first mixture and a second mixture separately. These two mixtures are then fed to the same extruder via independent metering feed paths. By periodically changing the feed ratio of the first and second mixtures as the tube body is continuously extruded, a heat-resistant load-bearing section, a second continuous transition section, a low-reinforcement component strip, a first continuous transition section, and the next heat-resistant load-bearing section are formed sequentially. A predetermined cutting position of the low-reinforcement component strip is used as the cutting position of the continuous tube body, resulting in the formation of a second tube end fusion section and a first tube end fusion section for two adjacent heat-resistant reinforced MPP power protection tubes on either side of the cutting position. The manufacturing process of the heat-resistant reinforced MPP power protection tube of this invention is as follows: Figure 1 As shown. This invention is based on the above research.

[0027] All experimental materials used in the embodiments of this invention can be obtained through conventional commercial channels, and unless otherwise specified, they are all industrial grade, as detailed below: Homopolymer polypropylene: Propylene homopolymer polypropylene granules, CAS No. 9003-07-0; Block copolymer polypropylene: Propylene-ethylene block copolymer polypropylene granules, CAS No. 9010-79-1; Calcined kaolin: English name is Calcined Kaolin, CAS number 92704-41-1; Chopped alkali-free glass fiber: Alkali-free E-glass chopped fiber, industrial grade; Hindered phenolic antioxidants: Antioxidant 1010 is used, chemical name is pentaerythritol tetrakis[β-3,5-di-tert-butyl-4-hydroxyphenylpropionic acid] ester, CAS number 6683-19-8; Phosphite antioxidants: Antioxidant 168 is used, chemical name is tris[2,4-di-tert-butylphenyl] phosphite, CAS number 31570-04-4.

[0028] The thermo-oxidative stabilizer of this invention includes hindered phenolic antioxidants and phosphite antioxidants. Unless otherwise specified, all raw material names in subsequent embodiments will be referred to by the above names.

[0029] In this invention, unless otherwise stated, the content of heat-resistant reinforcing components and the content of heat-oxidative stabilizers are both based on 100 parts by weight of the polypropylene matrix at the corresponding position.

[0030] Example 1 This embodiment provides a heat-resistant reinforced MPP power protection pipe, which includes a first pipe end welding section, a first continuous transition section, a heat-resistant bearing section, a second continuous transition section, and a second pipe end welding section, which are sequentially arranged along the pipe body axis and integrally extruded.

[0031] In this embodiment, the total axial length of the heat-resistant reinforced MPP power protection pipe is 6000 mm. The axial lengths of the first pipe end fusion section and the second pipe end fusion section are 80 mm each, and the axial lengths of the first continuous transition section and the second continuous transition section are 150 mm each. The remaining portion forms a heat-resistant load-bearing section. The first pipe end fusion section, the first continuous transition section, the heat-resistant load-bearing section, the second continuous transition section, and the second pipe end fusion section have the same outer diameter and wall thickness, and are formed into a radially continuous integral pipe wall through continuous extrusion.

[0032] The heat-resistant load-bearing section comprises a polypropylene matrix and heat-resistant reinforcing components dispersed within the polypropylene matrix. Taking 100 parts by weight of the polypropylene matrix in the heat-resistant load-bearing section as an example, the polypropylene matrix consists of 55 parts by weight of homopolymer polypropylene and 45 parts by weight of block copolymer polypropylene; the heat-resistant reinforcing components include 8 parts by weight of calcined kaolin and 5 parts by weight of chopped alkali-free glass fiber, meaning the total amount of heat-resistant reinforcing components in the heat-resistant load-bearing section is 13 parts by weight.

[0033] The heat-resistant load-bearing section also contains 0.3 parts by weight of a heat-oxidation stabilizer, which includes hindered phenolic antioxidants and phosphite antioxidants. In this embodiment, the mass ratio of hindered phenolic antioxidants to phosphite antioxidants is 1:1.

[0034] The polypropylene matrix composition is the same in both the first and second pipe end weld sections. Taking 100 parts by weight of the polypropylene matrix in either the first or second pipe end weld section as an example, the polypropylene matrix consists of 30 parts by weight of homopolymer polypropylene and 70 parts by weight of block copolymer polypropylene.

[0035] The first and second pipe end fusion sections each contain heat-resistant reinforcing components, which are also composed of calcined kaolin and chopped alkali-free glass fibers. The calcined kaolin is 0.8 parts by weight, the chopped alkali-free glass fibers are 0.5 parts by weight, and the total amount of heat-resistant reinforcing components is 1.3 parts by weight, which is 10% of the heat-resistant reinforcing component content in the heat-resistant bearing section.

[0036] The first and second pipe end fusion sections each contain 0.6 parts by weight of a heat-oxidation stabilizer, which includes hindered phenolic antioxidants and phosphite antioxidants, with a mass ratio of 1:1. The heat-oxidation stabilizer content in the first and second pipe end fusion sections is twice that in the heat-resistant bearing section.

[0037] In the preparation process, a first mixture and a second mixture are first prepared separately. The first mixture is formulated according to the composition of the heat-resistant load-bearing section, and the second mixture is formulated according to the composition of the first pipe end welding section and the second pipe end welding section. The corresponding homopolymer polypropylene, block copolymer polypropylene, calcined kaolin, chopped alkali-free glass fiber, and thermo-oxygen stabilizer are mixed evenly and then melt-blended and granulated to obtain the first mixture and the second mixture.

[0038] The first and second mixtures are fed to the same extruder through independent metering feed paths. The temperatures in each zone of the extruder are controlled sequentially within the range of 180 to 210 degrees Celsius according to the material conveying direction, while the die head temperature is controlled within the range of 195 to 210 degrees Celsius. After extrusion, sizing, and cooling, a tube is continuously formed. Unless otherwise specified, the melt blending granulation, extrusion, sizing, and cooling conditions in Examples 2 to 4 and Comparative Examples 1 to 5 are the same as in Example 1.

[0039] When forming the heat-resistant load-bearing section, the first mixture is supplied at a ratio of 100%, and the second mixture is stopped from being supplied, thereby keeping the content of heat-resistant reinforcing components in the heat-resistant load-bearing section stable.

[0040] During continuous extrusion from the heat-resistant bearing section to the second continuous transition section and the second pipe end welding section, the feed ratio of the first mixture is continuously reduced and the feed ratio of the second mixture is continuously increased within an axial length of 150 mm, so that the feed ratio of the first mixture continuously decreases from 100% to 0%, while the feed ratio of the second mixture continuously increases from 0% to 100%. During this process, the content of the heat-resistant reinforcing component in the second continuous transition section continuously decreases from the heat-resistant bearing section towards the second pipe end welding section, while the content of the block copolymer polypropylene continuously increases from the heat-resistant bearing section towards the second pipe end welding section.

[0041] When the feed ratio of the first mixture is reduced to 0% and the feed ratio of the second mixture is increased to 100%, the second mixture is continuously fed to form a low-reinforcement component band on the continuously extruded tube.

[0042] The axial length of the low-reinforcement component strip is set to 160 mm, and the axial midpoint of the low-reinforcement component strip is determined as the predetermined cutting position. After the continuously extruded tube reaches the predetermined cutting position, it is cut so that the 80 mm low-reinforcement component strip on one side of the predetermined cutting position forms the second end fusion section of the previous heat-resistant reinforced MPP power protection tube, and the 80 mm low-reinforcement component strip on the other side of the predetermined cutting position forms the first end fusion section of the next heat-resistant reinforced MPP power protection tube.

[0043] After the low-reinforced component strip corresponding to the cutting position is extruded, the feed ratio of the first mixture is continuously increased and the feed ratio of the second mixture is continuously decreased within a subsequent 150 mm axial length. This process involves continuously increasing the feed ratio of the first mixture from 0% to 100%, and continuously decreasing the feed ratio of the second mixture from 100% to 0%, forming the first continuous transition section of the subsequent heat-resistant reinforced MPP power protection pipe. During this process, the content of the heat-resistant reinforcing component in the first continuous transition section continuously increases from the first pipe end fusion section towards the heat-resistant bearing section, while the content of the block copolymer polypropylene continuously decreases from the first pipe end fusion section towards the heat-resistant bearing section.

[0044] According to the above-mentioned material supply ratio change method, the material supply ratio of the first mixture and the second mixture is repeatedly changed with the length of the continuous extrusion of the tube body as the cycle, so as to continuously produce a heat-resistant reinforced MPP power protection tube that sequentially forms a first tube end welding section, a first continuous transition section, a heat-resistant bearing section, a second continuous transition section and a second tube end welding section along the tube body axis.

[0045] Example 2 This embodiment provides a heat-resistant reinforced MPP power protection pipe, which includes a first pipe end welding section, a first continuous transition section, a heat-resistant bearing section, a second continuous transition section, and a second pipe end welding section, which are sequentially arranged along the pipe body axis and integrally extruded.

[0046] In this embodiment, the total axial length of the heat-resistant reinforced MPP power protection pipe is 9000 mm, the axial lengths of the first pipe end fusion section and the second pipe end fusion section are 250 mm each, the axial lengths of the first continuous transition section and the second continuous transition section are 600 mm each, and the remaining part forms a heat-resistant load-bearing section.

[0047] Based on 100 parts by weight of the polypropylene matrix in the heat-resistant load-bearing section, the polypropylene matrix consists of 70 parts by weight of homopolymer polypropylene and 30 parts by weight of block copolymer polypropylene.

[0048] The heat-resistant reinforcing component includes 14 parts by weight of calcined kaolin and 9 parts by weight of chopped alkali-free glass fiber, and the total amount of the heat-resistant reinforcing component in the heat-resistant load-bearing section is 23 parts by weight.

[0049] The heat-resistant load-bearing section also contains 0.7 parts by weight of a heat-oxidation stabilizer, which includes hindered phenolic antioxidants and phosphite antioxidants. In this embodiment, the mass ratio of hindered phenolic antioxidants to phosphite antioxidants is 2:1.

[0050] Based on 100 parts by weight of the polypropylene matrix in the first or second pipe end fusion section, the polypropylene matrix consists of 45 parts by weight of homopolymer polypropylene and 55 parts by weight of block copolymer polypropylene.

[0051] The heat-resistant reinforcing components in the first and second pipe end welding sections each consist of 4.2 parts by weight of calcined kaolin and 2.7 parts by weight of chopped alkali-free glass fiber. The total amount of heat-resistant reinforcing components is 6.9 parts by weight, which is 30% of the heat-resistant reinforcing component content in the heat-resistant load-bearing section.

[0052] The first pipe end welding section and the second pipe end welding section each contain 1.2 parts by weight of heat and oxygen stabilizer, which includes hindered phenolic antioxidants and phosphite antioxidants, with a mass ratio of hindered phenolic antioxidants to phosphite antioxidants of 2:1.

[0053] During preparation, a first mixture is prepared according to the composition of the heat-resistant bearing section, and a second mixture is prepared according to the composition of the first pipe end welding section and the second pipe end welding section. The first mixture and the second mixture are then transported to the same extruder through independent metering and feeding paths.

[0054] When forming the heat-resistant load-bearing section, the first mixture is supplied at a ratio of 100%, and the second mixture is stopped from being supplied.

[0055] When forming the second continuous transition section, the feed ratio of the first mixture is continuously reduced and the feed ratio of the second mixture is continuously increased within an axial length of 600 mm, so that the feed ratio of the first mixture is continuously reduced from 100% to 0%, and the feed ratio of the second mixture is continuously increased from 0% to 100%. This causes the content of the heat-resistant reinforcing component in the second continuous transition section to continuously decrease from the heat-resistant bearing section towards the second pipe end welding section, while simultaneously causing the content of the block copolymer polypropylene to continuously increase from the heat-resistant bearing section towards the second pipe end welding section.

[0056] Subsequently, the feeding ratio of the second mixture is maintained at 100%, forming a low-reinforced component strip with an axial length of 500 mm. The axial midpoint of this low-reinforced component strip is used as the predetermined cutting position. After cutting along the predetermined cutting position, the 250 mm low-reinforced component strips on both sides of the predetermined cutting position respectively form the second pipe end fusion section and the first pipe end fusion section of two adjacent heat-resistant reinforced MPP power protection pipes.

[0057] Subsequently, within an axial length of 600 mm, the feed ratio of the first mixture is continuously increased from 0% to 100%, while the feed ratio of the second mixture is continuously decreased from 100% to 0%, forming a first continuous transition section. In the first continuous transition section, the content of the heat-resistant reinforcing component continuously increases from the first pipe end welding section towards the heat-resistant bearing section, while the content of the block copolymer polypropylene continuously decreases from the first pipe end welding section towards the heat-resistant bearing section.

[0058] By periodically repeating the process of changing the feeding ratio of the first mixture and the second mixture, a low-reinforcement component strip, a first continuous transition section, a heat-resistant bearing section, a second continuous transition section, and a next low-reinforcement component strip are sequentially formed on the continuously extruded tube. Cutting is then performed at predetermined cutting positions on each low-reinforcement component strip to obtain the heat-resistant reinforced MPP power protection tube of this embodiment.

[0059] Example 3 This embodiment provides a heat-resistant reinforced MPP power protection pipe, which includes a first pipe end welding section, a first continuous transition section, a heat-resistant bearing section, a second continuous transition section, and a second pipe end welding section, which are sequentially arranged along the pipe body axis and integrally extruded.

[0060] The total axial length of the heat-resistant reinforced MPP power protection pipe is 6000 mm. The axial lengths of the first pipe end fusion section and the second pipe end fusion section are 150 mm and 300 mm respectively.

[0061] Based on 100 parts by weight of the polypropylene matrix in the heat-resistant load-bearing section, the polypropylene matrix consists of 62 parts by weight of homopolymer polypropylene and 38 parts by weight of block copolymer polypropylene.

[0062] The heat-resistant reinforcing component in the heat-resistant load-bearing section includes 10 parts by weight of calcined kaolin and 7 parts by weight of chopped alkali-free glass fiber, with a total of 17 parts by weight of heat-resistant reinforcing component.

[0063] The heat-resistant load-bearing section contains 0.5 parts by weight of a heat-oxidation stabilizer, which includes hindered phenolic antioxidants and phosphite antioxidants. In this embodiment, the mass ratio of hindered phenolic antioxidants to phosphite antioxidants is 1:1.

[0064] Based on 100 parts by weight of the polypropylene matrix in the first or second pipe end fusion section, the polypropylene matrix consists of 38 parts by weight of homopolymer polypropylene and 62 parts by weight of block copolymer polypropylene.

[0065] The heat-resistant reinforcing components in the first and second pipe end welding sections each consist of 2 parts by weight of calcined kaolin and 1.4 parts by weight of chopped alkali-free glass fiber. The total amount of heat-resistant reinforcing components is 3.4 parts by weight, which is 20% of the heat-resistant reinforcing component content in the heat-resistant bearing section.

[0066] The first and second pipe end fusion sections each contain 0.65 parts by weight of heat-oxidative stabilizer, and the mass ratio of hindered phenolic antioxidants to phosphite antioxidants in both sections is 1:1. Therefore, the heat-oxidative stabilizer content in the first and second pipe end fusion sections is 1.3 times that in the heat-resistant bearing section.

[0067] The first mixture is prepared according to the composition of the heat-resistant bearing section, and the second mixture is prepared according to the composition of the first pipe end welding section and the second pipe end welding section.

[0068] The first and second mixtures are fed to the same extruder through independent metering feed paths for continuous extrusion. The first mixture is continuously fed when forming the heat-resistant load-bearing section.

[0069] After entering the second continuous transition section from the heat-resistant bearing section, the feeding ratio of the first mixture and the second mixture is continuously adjusted according to the extrusion length within a 300 mm axial length. In this embodiment, the 300 mm second continuous transition section is divided into continuous control intervals along the axial direction, and the metering feeding device continuously reduces the instantaneous feeding rate of the first mixture and continuously increases the instantaneous feeding rate of the second mixture as the extrusion length progresses, in order to avoid abrupt changes in the content of the heat-resistant reinforcing component in the axial direction.

[0070] When the feeding ratio of the second mixture reaches 100%, it is continuously extruded to form a 300 mm low-reinforcement component strip. The low-reinforcement component strip is cut at the axial middle position, so that a second pipe end weld section and a first pipe end weld section of 150 mm are obtained on both sides of the cut position.

[0071] After the cutting position, the feeding ratio of the first mixture is continuously increased from 0% to 100% within an axial length of 300 mm, and the feeding ratio of the second mixture is continuously decreased from 100% to 0%, forming the first continuous transition section.

[0072] Through the above method, the content of heat-resistant reinforcing component in the first pipe end welding section continuously increases from the first continuous transition section to the heat-resistant bearing section, and the content of heat-resistant reinforcing component in the heat-resistant bearing section continuously decreases from the second continuous transition section to the second pipe end welding section. At the same time, the content of block copolymer polypropylene in the first continuous transition section continuously decreases from the first pipe end welding section to the heat-resistant bearing section, and the content of block copolymer polypropylene in the second continuous transition section continuously increases from the heat-resistant bearing section to the second pipe end welding section.

[0073] Example 4 This embodiment provides a heat-resistant enhanced MPP power protection tube.

[0074] The heat-resistant reinforced MPP power protection pipe includes a first pipe end welding section, a first continuous transition section, a heat-resistant load-bearing section, a second continuous transition section, and a second pipe end welding section, which are sequentially arranged and integrally extruded along the pipe body axis.

[0075] The axial lengths of the first pipe end welding section and the second pipe end welding section are 180 mm and 400 mm respectively, and the axial lengths of the first continuous transition section and the second continuous transition section are 400 mm respectively.

[0076] Based on 100 parts by weight of the polypropylene matrix in the heat-resistant load-bearing section, the polypropylene matrix consists of 65 parts by weight of homopolymer polypropylene and 35 parts by weight of block copolymer polypropylene.

[0077] The heat-resistant reinforcing component in the heat-resistant load-bearing section includes 12 parts by weight of calcined kaolin and 8 parts by weight of chopped alkali-free glass fiber, with a total of 20 parts by weight of heat-resistant reinforcing component.

[0078] The heat-resistant load-bearing section contains 0.4 parts by weight of heat-oxidation stabilizer, which includes hindered phenolic antioxidants and phosphite antioxidants.

[0079] Based on 100 parts by weight of the polypropylene matrix in the first or second pipe end fusion section, the polypropylene matrix consists of 40 parts by weight of homopolymer polypropylene and 60 parts by weight of block copolymer polypropylene.

[0080] The heat-resistant reinforcing components in the first pipe end welding section and the second pipe end welding section each include 1.8 parts by weight of calcined kaolin and 1.2 parts by weight of chopped alkali-free glass fiber. The total amount of heat-resistant reinforcing components is 3 parts by weight, which is 15% of the heat-resistant reinforcing component content in the heat-resistant bearing section.

[0081] The first and second pipe-end fusion sections each contain 1 part by weight of a heat-oxidation stabilizer, and the content of the heat-oxidation stabilizer in the first and second pipe-end fusion sections is 2.5 times the content of the heat-oxidation stabilizer in the heat-resistant bearing section. In this embodiment, the mass ratio of hindered phenolic antioxidant and phosphite antioxidant in the heat-resistant bearing section, the first pipe-end fusion section, and the second pipe-end fusion section is 1:1.

[0082] During preparation, a first mixture is prepared according to the composition of the heat-resistant bearing section, and a second mixture is prepared according to the composition of the first pipe end welding section and the second pipe end welding section.

[0083] The first and second mixtures enter independent metering and feeding paths, and then merge according to a set feeding ratio before entering the same extruder. The total feed amount of the first and second mixtures remains stable, and the composition of the continuous extrusion tube at different axial positions is controlled by changing the ratio of the first and second mixtures in the total feed amount.

[0084] When forming the heat-resistant load-bearing section, the first mixture is used for feeding.

[0085] When forming the second continuous transition section, the feeding ratio of the first mixture is continuously reduced within an axial length of 400 mm, while the feeding ratio of the second mixture is simultaneously and continuously increased until it is completely converted to the feeding of the second mixture, thereby forming a second continuous transition section in which the content of heat-resistant reinforcing components continuously decreases and the content of block copolymer polypropylene continuously increases.

[0086] While maintaining the supply of the second mixture, a 360 mm low-reinforcement component strip is continuously formed on the pipe body, and the axial midpoint of this low-reinforcement component strip is designated as the predetermined cutting position. After cutting along the predetermined cutting position, 180 mm low-reinforcement component strips are retained on both sides of the predetermined cutting position, forming the second pipe end fusion section and the first pipe end fusion section of two adjacent heat-resistant reinforced MPP power protection pipes, respectively.

[0087] Subsequently, the feeding ratio of the first mixture is continuously increased within an axial length of 400 mm, while the feeding ratio of the second mixture is continuously decreased simultaneously, forming a first continuous transition section in which the content of heat-resistant reinforcing components continuously increases and the content of block copolymer polypropylene continuously decreases.

[0088] By controlling the feeding ratio of the first mixture and the second mixture to change periodically with the extrusion length, the heat-resistant bearing section, the second continuous transition section, the low-reinforcement component strip, the first continuous transition section and the next heat-resistant bearing section are periodically formed during the continuous production of the tube. By cutting at the predetermined cutting position of each low-reinforcement component strip, each cut heat-resistant reinforced MPP power protection tube forms a first tube end fusion section, a first continuous transition section, a heat-resistant bearing section, a second continuous transition section and a second tube end fusion section.

[0089] Comparative Example 1 This comparative example is used to examine the effect of different material compositions along the axial direction of the pipe.

[0090] Except for the following differences, this comparative example is the same as Example 3: This comparative example does not use the method of changing the feeding ratio of the first mixture and the second mixture with the extrusion length. The first mixture is always used for feeding during the continuous extrusion process, so that the material composition of each position along the axial direction of the tube is the same as that of the heat-resistant bearing section in Example 3.

[0091] Therefore, the tube body of this comparative example comprises a polypropylene matrix consisting of 62 parts by weight of homopolymer polypropylene and 38 parts by weight of block copolymer polypropylene at each position along the axial direction, and includes 10 parts by weight of calcined kaolin, 7 parts by weight of chopped alkali-free glass fiber and 0.5 parts by weight of thermo-oxidative stabilizer.

[0092] This comparative example does not form a first pipe end fusion section and a second pipe end fusion section where the content of heat-resistant reinforcing component is lower than that of the heat-resistant load-bearing section, nor does it form a first continuous transition section and a second continuous transition section where the content of heat-resistant reinforcing component changes continuously along the pipe body axis.

[0093] The remaining raw material processing, extrusion, sizing, and cooling conditions are the same as in Example 3.

[0094] Comparative Example 2 This comparative example is used to examine the effect of using materials with low heat-resistant reinforcing component content to form the entire pipe body.

[0095] Except for the following differences, this comparative example is the same as Example 3: In this comparative example, the second mixture is always used for feeding during the continuous extrusion process, so that the material composition of each position along the axial direction of the tube is the same as that of the first tube end weld section and the second tube end weld section in Example 3.

[0096] Based on 100 parts by weight of polypropylene matrix, the polypropylene matrix consists of 38 parts by weight of homopolymer polypropylene and 62 parts by weight of block copolymer polypropylene; the heat-resistant reinforcing component includes 2 parts by weight of calcined kaolin and 1.4 parts by weight of chopped alkali-free glass fiber, and the total amount of heat-resistant reinforcing component is 3.4 parts by weight; the heat-oxygen stabilizer is 0.65 parts by weight.

[0097] This comparative example does not include a heat-resistant load-bearing section with a higher content of heat-resistant reinforcing components than other parts of the pipe body, nor does it form a first continuous transition section and a second continuous transition section by changing the feeding ratio of the first mixture and the second mixture.

[0098] The remaining raw material processing, extrusion, sizing, and cooling conditions are the same as in Example 3.

[0099] Comparative Example 3 This comparative example is used to examine the effect of continuous changes in material composition in the first and second continuous transition sections.

[0100] Except for the following differences, this comparative example is the same as Example 3: This comparative example still uses the same first and second mixtures as in Example 3, and keeps the material composition of the heat-resistant bearing section, the first pipe end welding section, and the second pipe end welding section unchanged.

[0101] When transitioning from the heat-resistant bearing section to the second pipe end welding section, instead of continuously reducing the feeding ratio of the first mixture and continuously increasing the feeding ratio of the second mixture within the axial length corresponding to the second continuous transition section, the feeding of the first mixture is directly switched to the feeding of the second mixture at the end position of the heat-resistant bearing section.

[0102] When transitioning from the first pipe end welding section to the heat-resistant bearing section, instead of continuously increasing the feeding ratio of the first mixture and continuously decreasing the feeding ratio of the second mixture within the axial length corresponding to the first continuous transition section, the feeding of the second mixture is directly switched to the feeding of the first mixture at the end position of the first pipe end welding section.

[0103] Therefore, in this comparative example, the content of heat-resistant reinforcing component and the content of block copolymer polypropylene change directly between the heat-resistant bearing section and the first pipe end welding section and the second pipe end welding section, without forming a first continuous transition section and a second continuous transition section in which the content of heat-resistant reinforcing component and the content of block copolymer polypropylene change continuously along the pipe body axis.

[0104] The remaining conditions are the same as in Example 3.

[0105] Comparative Example 4 This comparative example is used to examine the effect of higher content of heat-oxidative stabilizer in the first and second pipe end welding sections compared to the heat-resistant bearing section.

[0106] Except for the following differences, this comparative example is the same as Example 3: In this comparative example, the content of heat-oxidative stabilizer in the heat-resistant bearing section, the first pipe end welding section, and the second pipe end welding section was all set to 0.5 parts by weight. The mass ratio of hindered phenolic antioxidant to phosphite antioxidant was maintained at 1:1.

[0107] The composition of the polypropylene matrix, the composition of the heat-resistant reinforcing component, and the content of the heat-resistant reinforcing component in the heat-resistant bearing section remain unchanged; the composition of the polypropylene matrix, the composition of the heat-resistant reinforcing component, and the content of the heat-resistant reinforcing component in the first pipe end welding section and the second pipe end welding section also remain unchanged.

[0108] The feeding ratio of the first mixture to the second mixture, the formation method of the low-reinforcement component strip, and the predetermined cutting position in the first and second continuous transition sections are the same as in Example 3.

[0109] Therefore, the only difference between this comparative example and Example 3 is that the content of heat-oxidative stabilizer in the first pipe end welding section and the second pipe end welding section is not higher than the content of heat-oxidative stabilizer in the heat-resistant bearing section.

[0110] Comparative Example 5 This comparative example is used to examine the effect of the low-reinforcement component band corresponding to the predetermined cutting position.

[0111] Except for the following differences, this comparative example is the same as Example 3: The heat-resistant load-bearing section, the first continuous transition section, the second continuous transition section, and the low-reinforcement component strip with an axial length of 300 mm are formed in the same manner as in Example 3.

[0112] This comparative example does not use the axial midpoint of the low-reinforced component strip as the predetermined cutting position, but instead sets the predetermined cutting position at the axial midpoint of the first continuous transition section adjacent to the low-reinforced component strip.

[0113] After continuous cutting, the tube end on one side of the cutting position includes a low-reinforcement component band and part of the first continuous transition section, while the tube end on the other side of the cutting position is directly located within the first continuous transition section. This prevents the formation of a first tube end fusion section and a second tube end fusion section with the same material composition and axial length on both sides of the cutting position.

[0114] Except for the predetermined cutting position, the composition of the first mixture and the second mixture, the way the feeding ratio changes, the axial length of the low-reinforcement component belt, and the extrusion conditions are all the same as in Example 3.

[0115] Test case To verify the performance of the heat-resistant reinforced MPP power protection pipes obtained in Examples 1 to 4 and Comparative Examples 1 to 5, the high-temperature ring hot compression force, the tensile strength of the hot-melt joint, the tensile strength of the hot-melt joint after thermo-oxidative aging, and the axial tensile strength of the transition area were tested on each group of pipes.

[0116] To ensure the comparability of the test results of each group, the tubes used for the same test item in Examples 1 to 4 and Comparative Examples 1 to 5 have the same outer diameter and wall thickness, and the same sample preparation method and test conditions are used for the same test item.

[0117] I. High-Temperature Ring Plate Hot Compression Force Test Three pipe segments with a length of 300 mm were cut from the corresponding positions of the heat-resistant load-bearing sections of the pipes obtained in Examples 1 to 4 and Comparative Examples 1 to 5, respectively, as samples.

[0118] For Comparative Example 2, since its pipe body did not have a heat-resistant load-bearing section, a pipe section of the same length was cut from the middle of the pipe body as a sample; for Comparative Example 1, since its entire pipe body was made of the same material as the heat-resistant load-bearing section of Example 3, a sample was cut from the middle of the pipe body.

[0119] The sample was placed in a hot air environment at 70±2 degrees Celsius for 2 hours. After removal, the sample was immediately placed horizontally between the upper and lower pressure plates of the pressure testing machine. A load was applied radially along the tube body at a speed of 5±2 mm per minute. When the outer diameter of the sample was compressed to 5% of the initial outer diameter, the corresponding load was recorded. The arithmetic mean of the test results of the three samples was taken as the high-temperature ring heat compression force.

[0120] This test is used to evaluate the ability of the heat-resistant load-bearing section to withstand radial loads under high-temperature conditions.

[0121] II. Tensile Strength Test of Hot-Melt Joints The tubes obtained from Examples 1 to 4 and Comparative Examples 1 to 5 were selected respectively, and hot-melt butt welding was performed under the same specifications, the same hot-melt equipment and the same hot-melt process conditions.

[0122] For Examples 1 to 4, the first end fusion section of a heat-resistant reinforced MPP power protection tube is heat-fused to the second end fusion section of another heat-resistant reinforced MPP power protection tube.

[0123] For Comparative Examples 1 and 2, hot-melt welding was performed directly from the cut end of the pipe body; for Comparative Examples 3 and 4, hot-melt welding was performed using the first and second pipe end welding sections of the corresponding pipe bodies; for Comparative Example 5, hot-melt welding was performed on the ends of two pipe bodies formed in the same cut and located on both sides of the predetermined cut position.

[0124] After the heat-fused joint has completely cooled to room temperature, tensile specimens spanning the heat-fused joint are prepared along the axial direction of the pipe body. Tensile tests are conducted at 23±2 degrees Celsius, and the maximum tensile load before specimen fracture is recorded. The tensile strength of the heat-fused joint is calculated based on the effective cross-sectional area of ​​the specimen. Five parallel specimens are set for each group, and the arithmetic mean is taken as the tensile strength of the heat-fused joint for the corresponding group.

[0125] This test is used to evaluate the effects of different pipe end material compositions and predetermined cutting positions on the performance of pipe end thermofusion connections.

[0126] III. Tensile Strength Test of Thermo-Oxidative Aging Joints Following the same method used for the tensile strength test of hot-melt joints, hot-melt joint samples from Examples 1 to 4 and Comparative Examples 1 to 5 were prepared respectively.

[0127] The hot-melt joint sample was placed in a hot air aging chamber at 110±2 degrees Celsius for 168 hours. After the thermo-oxidative aging was completed, it was taken out and placed in an environment at 23±2 degrees Celsius for 24 hours.

[0128] Subsequently, a tensile test was conducted under the same conditions as the tensile strength test of the heat fusion joint to obtain the tensile strength of the heat fusion joint after thermo-oxidative aging, and the tensile strength retention rate of the heat fusion joint was calculated according to the following formula: Tensile strength retention rate of heat fusion joint = Tensile strength of heat fusion joint after thermo-oxidative aging ÷ Tensile strength of heat fusion joint before thermo-oxidative aging × 100%.

[0129] This test is used to evaluate the ability of the first and second pipe end welded sections to maintain their connection strength after undergoing extrusion molding, hot-melt connection, and subsequent high-temperature environment, and to compare the effect of the content of heat-oxidative stabilizer in the first and second pipe end welded sections on the heat-oxidative stability of the hot-melt joint.

[0130] IV. Axial Tensile Strength Test in Transition Region Longitudinal samples were cut along the axial direction from the tubes obtained in Examples 1 to 4 and Comparative Examples 3 to 5, respectively.

[0131] The specimens in Examples 1 to 4 are centered on the axial middle of the second continuous transition section, so that the specimens cross the material composition change region in the second continuous transition section along the tube axis.

[0132] Since no second continuous transition section is formed in Comparative Example 3, the position where the first mixture supply is directly switched to the second mixture supply between the heat-resistant bearing section and the second pipe end welding section is taken as the center of the sample.

[0133] Comparative Examples 4 and 5 were prepared at the same locations as in Example 3.

[0134] The specimens were subjected to axial tension at 23±2 degrees Celsius. The maximum tensile load was recorded, and the axial tensile strength of the transition region was calculated based on the effective cross-sectional area of ​​the specimen. Five parallel specimens were set up for each group, and the arithmetic mean was taken as the test result.

[0135] Since the tubes of Comparative Example 1 and Comparative Example 2 are composed of a single material along the axial direction and do not form a first continuous transition section and a second continuous transition section, the axial tensile strength test of the transition region is not performed.

[0136] The test results are shown in Table 1.

[0137] Table 1 Performance test results of the examples and comparative examples Group High-temperature ring plate hot compressive force kN The tensile strength of the heat fusion joint (MPa) Tensile strength of thermo-fusion joint after thermo-oxidative aging (MPa) Tensile strength retention rate of heat fusion joints (%) Axial tensile strength of transition region (MPa) Example 1 2.26 27.4 24.6 89.8 27.1 Example 2 2.78 26.6 25.1 94.4 27.8 Example 3 2.52 28.1 26.3 93.6 27.6 Example 4 2.65 27.8 26.6 95.7 27.9 Comparative Example 1 2.49 22.9 20.0 87.3 — Comparative Example 2 1.72 28.4 25.9 91.2 — Comparative Example 3 2.50 27.9 26.0 93.2 23.4 Comparative Example 4 2.51 26.8 21.8 81.3 27.5 Comparative Example 5 2.48 24.7 22.5 91.1 27.3

[0138] Depend on Figure 2 , Figure 3As can be seen from Table 1, the entire pipe body of Comparative Example 1 is made of the same material as the heat-resistant load-bearing section, and its high-temperature ring heat compression force remains at a high level. However, the tensile strength of the heat-fusion joint is lower than that of Examples 1 to 4. This indicates that although increasing the content of heat-resistant reinforcing components in the entire pipe body is beneficial to improving heat-resistant load-bearing performance, it is not beneficial to the heat-fusion connection performance of the pipe ends.

[0139] In Comparative Example 2, the entire pipe body is composed of the same material as the first and second pipe end fusion sections. Its heat-fusion joint exhibits high tensile strength, but the high-temperature ring heat-compression force is significantly reduced. This indicates that reducing the content of heat-resistant reinforcing components throughout the pipe body can meet the requirements of pipe end heat fusion connection, but it is detrimental to the heat-resistant load-bearing performance of the main pipe body. Examples 1 to 4, by respectively setting a first pipe end fusion section, a first continuous transition section, a heat-resistant load-bearing section, a second continuous transition section, and a second pipe end fusion section along the pipe body axial direction, allow for different contents of heat-resistant reinforcing components at the heat-resistant load-bearing section and pipe end positions, thereby addressing different performance requirements for heat-resistant load-bearing and heat fusion connection.

[0140] Comparative Example 3 has the same material composition for the heat-resistant load-bearing section as Example 3, as well as the material composition for the first and second pipe-end fusion sections. However, Comparative Example 3 does not form a first and second continuous transition section where the content of the heat-resistant reinforcing component and the block copolymer polypropylene content continuously varies along the pipe axial direction. Its axial tensile strength in the transition region is lower than that of Example 3. This demonstrates that by making the content of the heat-resistant reinforcing component and the block copolymer polypropylene content in the first and second continuous transition sections continuously vary along the pipe axial direction, the impact of direct transitions between different material composition regions on the continuity of axial load bearing can be reduced.

[0141] Comparative Example 4 only adjusted the content of the thermo-oxidative stabilizer in the first and second pipe end fusion sections to be the same as that in the heat-resistant bearing section. The tensile strength of the heat-fused joint before thermo-oxidative aging was relatively similar to that of Example 3, but after thermo-oxidative aging, the tensile strength retention rate of the heat-fused joint decreased to 81.3%. In Example 3, the content of the thermo-oxidative stabilizer in the first and second pipe end fusion sections was 1.3 times that in the heat-resistant bearing section, and the tensile strength retention rate of the heat-fused joint was 93.6%. This indicates that increasing the content of the thermo-oxidative stabilizer at the corresponding locations, considering the multiple thermal histories formed by extrusion molding and subsequent thermo-fusion connection of the first and second pipe end fusion sections, is beneficial for maintaining the connection strength of the heat-fused joint after exposure to high-temperature environments.

[0142] Comparative Example 5 used the same first and second mixtures and the same feeding ratio variation method as Example 3, but did not use the axial middle position of the low-reinforcement component strip as the predetermined cutting position. This prevented the ends of adjacent pipes from forming complete first and second pipe end weld segments with consistent axial lengths after cutting, resulting in a lower tensile strength of the heat-fusion joint compared to Example 3. This demonstrates that aligning the low-reinforcement component strip with the predetermined cutting position during continuous extrusion, and forming the first and second pipe end weld segments on either side of the predetermined cutting position, is beneficial for ensuring the heat-fusion connection performance of the pipe ends obtained through continuous production.

[0143] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

Claims

1. A heat-resistant reinforced MPP power protection tube, characterized in that, It includes a first pipe end fusion section, a first continuous transition section, a heat-resistant bearing section, a second continuous transition section, and a second pipe end fusion section, which are sequentially arranged along the axial direction of the pipe body and integrally extruded. The heat-resistant load-bearing section includes a polypropylene matrix and a heat-resistant reinforcing component dispersed in the polypropylene matrix. The first pipe end fusion section and the second pipe end fusion section both include a polypropylene matrix, and the content of the heat-resistant reinforcing component in the first pipe end fusion section and the second pipe end fusion section is lower than the content of the heat-resistant reinforcing component in the heat-resistant load-bearing section. The content of the heat-resistant reinforcing component is based on 100 parts by weight of the polypropylene matrix at the corresponding position. The content of the heat-resistant reinforcing component in the first continuous transition section increases continuously from the first pipe end fusion section toward the heat-resistant bearing section, and the content of the heat-resistant reinforcing component in the second continuous transition section decreases continuously from the heat-resistant bearing section toward the second pipe end fusion section, so that the first pipe end fusion section, the first continuous transition section, the heat-resistant bearing section, the second continuous transition section and the second pipe end fusion section form an integral pipe wall that continuously changes along the pipe body axis.

2. The heat-resistant reinforced MPP power protection tube according to claim 1, characterized in that, The polypropylene matrix of the heat-resistant load-bearing section is composed of homopolymer polypropylene and block copolymer polypropylene. Based on 100 parts by weight of the polypropylene matrix, the homopolymer polypropylene is 55 to 70 parts by weight and the block copolymer polypropylene is 30 to 45 parts by weight.

3. The heat-resistant reinforced MPP power protection tube according to claim 2, characterized in that, The heat-resistant reinforcing component includes calcined kaolin and chopped alkali-free glass fiber. Based on 100 parts by weight of the polypropylene matrix in the heat-resistant load-bearing section, the calcined kaolin comprises 8 to 14 parts by weight, and the chopped alkali-free glass fiber comprises 5 to 9 parts by weight.

4. The heat-resistant reinforced MPP power protection tube according to claim 1, characterized in that, The polypropylene matrix of both the first pipe end fusion section and the second pipe end fusion section is composed of homopolymer polypropylene and block copolymer polypropylene. Based on 100 parts by weight of the polypropylene matrix, the homopolymer polypropylene is 30 to 45 parts by weight and the block copolymer polypropylene is 55 to 70 parts by weight.

5. The heat-resistant reinforced MPP power protection tube according to claim 1, characterized in that, The heat-resistant reinforcing component content in the first pipe end fusion section and the second pipe end fusion section is 10% to 30% of the heat-resistant reinforcing component content in the heat-resistant bearing section, respectively.

6. The heat-resistant reinforced MPP power protection tube according to claim 1, characterized in that, In the first continuous transition section, the content of block copolymer polypropylene continuously decreases from the first pipe end welding section toward the heat-resistant bearing section, and in the second continuous transition section, the content of block copolymer polypropylene continuously increases from the heat-resistant bearing section toward the second pipe end welding section.

7. The heat-resistant reinforced MPP power protection tube according to claim 1, characterized in that, The heat-resistant bearing section, the first pipe end welding section, and the second pipe end welding section each contain a heat-oxygen stabilizer. The content of the heat-oxygen stabilizer is based on 100 parts by weight of the polypropylene matrix at the corresponding position. The content of the heat-oxygen stabilizer in the first pipe end welding section and the second pipe end welding section is 1.3 to 2.5 times that in the heat-resistant bearing section.

8. The heat-resistant reinforced MPP power protection tube according to claim 7, characterized in that, The heat-oxidation stabilizer includes hindered phenolic antioxidants and phosphite antioxidants; based on 100 parts by weight of polypropylene matrix in each section, the heat-oxidation stabilizer in the heat-resistant bearing section is 0.3 to 0.7 parts by weight, and the heat-oxidation stabilizers in the first pipe end welding section and the second pipe end welding section are 0.6 to 1.2 parts by weight, respectively.

9. The heat-resistant reinforced MPP power protection tube according to claim 1, characterized in that, The axial lengths of the first pipe end welding section and the second pipe end welding section are 80 to 250 mm, respectively, and the axial lengths of the first continuous transition section and the second continuous transition section are 150 to 600 mm, respectively.

10. A method for preparing a heat-resistant reinforced MPP power protection tube, characterized in that, include: S1, prepare a first mixture and a second mixture respectively. Both the first mixture and the second mixture include a polypropylene matrix. Based on 100 parts by weight of the polypropylene matrix in each mixture, the content of the heat-resistant reinforcing component in the first mixture is higher than the content of the heat-resistant reinforcing component in the second mixture. S2, the first mixture and the second mixture are fed to the same extruder through independent metering and feeding paths, and continuously extruded by the extruder to form a tube; S3, when forming the heat-resistant bearing section, the feeding ratio of the first mixture is higher than that of the second mixture and the feeding ratio is kept stable, so that the content of the heat-resistant reinforcing component in the heat-resistant bearing section remains stable. S4, when a continuous transition section is formed on both sides of the heat-resistant bearing section, the feeding ratio of the first mixture and the second mixture is continuously changed, and a low-reinforcement component band is formed between two adjacent heat-resistant bearing sections. The content of heat-resistant reinforcing component in the low-reinforcement component band is lower than that in the heat-resistant bearing section, so that the content of heat-resistant reinforcing component continuously decreases from the heat-resistant bearing section toward the low-reinforcement component band, and continuously increases from the low-reinforcement component band toward the adjacent heat-resistant bearing section. S5, the feeding ratio of the first mixture and the second mixture is repeatedly changed according to the length cycle of the continuous extrusion of the tube body. The axial middle position of the low-reinforcement component strip is determined as the predetermined cutting position. The continuously extruded tube body is cut at the predetermined cutting position, so that the tube end welding sections of two adjacent heat-resistant reinforced MPP power protection tubes are formed on both sides of the cutting position. Thus, each heat-resistant reinforced MPP power protection tube sequentially forms a first tube end welding section, a first continuous transition section, a heat-resistant bearing section, a second continuous transition section, and a second tube end welding section along the tube body axial direction.