Three-phase vanadium oxide thermistor layer, preparation method thereof and infrared detection chip
By designing nanocomposite grain boundaries in a three-phase vanadium oxide thermistor layer, the problems of nonlinear distortion and high noise in the resistance response of traditional single-phase vanadium oxide thermistor layers over a wide temperature range are solved, achieving high sensitivity and stability in high-precision infrared imaging.
Patent Information
- Application Number
- CN202611309887.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-27
- Publication Date
- 2026-11-24
AI Technical Summary
Traditional uncooled infrared detectors with a single-phase vanadium oxide thermistor layer suffer from nonlinear distortion of resistance response, low sensitivity, and high noise within a wide temperature range of -40℃ to 120℃, making it difficult to meet the application requirements of high-precision infrared imaging equipment.
A three-phase vanadium oxide thermistor layer, composed of vanadium dioxide, vanadium trioxide and vanadium pentoxide, is deposited by magnetron sputtering and then annealed to form nanocomposite grain boundaries. This process synergistically regulates carrier mobility and noise, achieving stability and high sensitivity with a negative temperature coefficient.
It achieves high resistance-temperature linearity, high TCR and low noise in a wide temperature range of -40℃ to 120℃, and is suitable for high-precision thermal imaging scenarios such as vehicle temperature measurement, security monitoring and industrial high temperature detection.
Smart Images

Figure CN123161992A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of temperature detection technology, and in particular to a three-phase vanadium oxide thermistor layer, its preparation method, and an infrared detection chip. Background Technology
[0002] Traditional uncooled infrared detectors primarily use single-phase vanadium oxide (VO2) as their thermal sensing material. x Or amorphous silicon. Among them, the single component VO x Thin films generally suffer from problems such as low TCR (Temperature Coefficient of Resistance) (absolute value < 2.0% / K), large resistance drift in the high-temperature range, and high 1 / f noise and thermal noise levels. For example, VO2-based thermistors exhibit a severe metal-insulator phase transition effect near 68℃, leading to a step abrupt change in resistance. This results in severe nonlinear distortion of the device's temperature response curve, making it unable to meet the requirement of continuous linear resistance response over a wide temperature range of -40℃ to 120℃. Furthermore, their low detection sensitivity and high noise make them unsuitable for applications requiring high-precision infrared imaging equipment. Summary of the Invention
[0003] Therefore, it is necessary to provide a three-phase vanadium oxide thermistor layer, its preparation method, and an infrared detection chip to improve the continuous resistance response of the three-phase vanadium oxide thermistor layer in a wide temperature range of -40℃ to 120℃, while taking into account both high sensitivity and low noise.
[0004] In a first aspect, this application provides a three-phase vanadium oxide thermistor layer, comprising vanadium dioxide, vanadium trioxide, and vanadium pentoxide. The vanadium trioxide content in the three-phase vanadium oxide thermistor layer is 20% to 60% of the mass of vanadium dioxide; the vanadium pentoxide content in the three-phase vanadium oxide thermistor layer is 30% to 80% of the mass of vanadium dioxide.
[0005] In some embodiments, the three-phase vanadium oxide thermistor layer satisfies at least one of the following conditions:
[0006] (1) The mass percentage of vanadium dioxide in the three-phase vanadium oxide thermistor layer is 40%~65%;
[0007] (2) The ratio between the amount of oxygen and the amount of vanadium in the three-phase vanadium oxide thermistor layer is 1.8 to 2.2.
[0008] (3) The thickness of the three-phase vanadium oxide thermistor layer is 50nm~100nm.
[0009] In some embodiments, the three-phase vanadium oxide thermistor layer also contains doping elements.
[0010] Optionally, the doping element includes at least one of tungsten, aluminum, titanium and chromium.
[0011] Optionally, the mass percentage of doped elements in the three-phase vanadium oxide thermistor layer is 0.5% to 3%.
[0012] Secondly, this application also provides a method for preparing a three-phase vanadium oxide thermistor layer according to the first aspect, comprising the following steps:
[0013] A stack of vanadium trioxide, vanadium dioxide, and vanadium pentoxide layers is deposited and formed. After annealing, a three-phase vanadium oxide thermistor layer containing vanadium dioxide, vanadium trioxide, and vanadium pentoxide is formed.
[0014] In some embodiments, the preparation method satisfies at least one of the following conditions:
[0015] (1) The thickness of the vanadium trioxide layer is 17 nm to 33 nm;
[0016] (2) The thickness of the vanadium dioxide layer is 17 nm to 33 nm;
[0017] (3) The thickness of the vanadium pentoxide layer is 17 nm to 33 nm;
[0018] (4) The annealing temperature is 300℃~450℃, the holding time is 30min~120min, and the vacuum degree is 1×10 - 3 Pa~5×10 -4 Pa.
[0019] In some embodiments, a vanadium trioxide layer is deposited using magnetron sputtering, which includes: introducing argon gas as the working gas and oxygen gas as the reaction gas, and using a vanadium target for magnetron sputtering to form the vanadium trioxide layer.
[0020] Optionally, during the formation of the vanadium trioxide layer by magnetron sputtering, the oxygen flow rate is 2 sccm to 8 sccm.
[0021] Optionally, during the formation of the vanadium trioxide layer by magnetron sputtering, the power of the vanadium target is 1.0kW~2.5kW.
[0022] Optionally, the vanadium target containing dopant elements is used in the process of forming the vanadium trioxide layer by magnetron sputtering. More preferably, the mass percentage of the dopant elements in the vanadium target is 0.5% to 3%.
[0023] In some embodiments, a vanadium dioxide layer is deposited using a magnetron sputtering method, including: introducing argon gas as the working gas and oxygen gas as the reaction gas, and using a vanadium target for magnetron sputtering to form the vanadium dioxide layer.
[0024] Optionally, during the formation of the vanadium dioxide layer by magnetron sputtering, the oxygen flow rate is 10 sccm to 20 sccm.
[0025] Optionally, during the formation of the vanadium dioxide layer by magnetron sputtering, the power of the vanadium target is 1.0kW to 2.5kW.
[0026] Optionally, the vanadium target used in the magnetron sputtering process for forming the vanadium dioxide layer contains doping elements. More preferably, the mass percentage of the doping elements in the vanadium target is 0.5% to 3%.
[0027] In some embodiments, a vanadium pentoxide layer is deposited using magnetron sputtering, which includes: introducing argon gas as the working gas and oxygen gas as the reaction gas, and using a vanadium target for magnetron sputtering to form the vanadium pentoxide layer.
[0028] Optionally, during the formation of the vanadium pentoxide layer by magnetron sputtering, the oxygen flow rate is 25 sccm to 40 sccm.
[0029] Optionally, during the formation of the vanadium pentoxide layer by magnetron sputtering, the power of the vanadium target is 1.0kW to 2.5kW.
[0030] Optionally, the vanadium target containing dopant elements is used in the process of forming the vanadium pentoxide layer by magnetron sputtering. More preferably, the mass percentage of the dopant elements in the vanadium target is 0.5% to 3%.
[0031] Thirdly, this application provides an infrared detection chip, including a thermistor layer. The thermistor layer includes the three-phase vanadium oxide thermistor layer described in the first aspect.
[0032] In some embodiments, the thermal layer includes a plurality of thermal pixel units arranged in an array, and the thermal pixel units include a three-phase vanadium oxide thermistor layer.
[0033] Optionally, the width of the three-phase vanadium oxide thermistor layer is 6μm~9μm;
[0034] Optionally, the gap between adjacent thermal pixel units is 1μm to 2μm.
[0035] Compared with traditional technologies, this application has at least the following beneficial effects:
[0036] This three-phase vanadium oxide thermistor layer employs a ternary mixed crystal phase of vanadium dioxide, vanadium trioxide, and vanadium pentoxide. The interpenetrating grains of the three vanadium oxides form nanocomposite grain boundaries, blocking the continuous grain channels of vanadium dioxide. This counteracts the abrupt metal-insulator phase transition of vanadium dioxide near 68℃ and achieves a negative temperature coefficient, enabling the three-phase vanadium oxide thermistor layer to exhibit linear resistance-temperature response over a wide temperature range of -40℃ to 120℃, with higher testing accuracy and sensitivity. Simultaneously, the vanadium trioxide metal grain boundaries enhance carrier mobility, while the vanadium pentoxide insulating grains confine carrier concentration, synergistically stabilizing the negative temperature coefficient. This allows the TCR of the three-phase vanadium oxide thermistor layer to be stably maintained within the range of -2.8% / K to -3.3% / K, while also balancing the sheet resistance of the thin film and suppressing lattice scattering noise and interface 1 / f noise. Therefore, this three-phase vanadium oxide thermistor layer has high resistance-temperature linearity, high TCR and low noise in a wide temperature range of -40℃ to 120℃, which can meet the needs of high-precision thermal imaging scenarios such as vehicle temperature measurement, security monitoring and industrial high temperature detection. Attached Figure Description
[0037] To more clearly illustrate the technical solutions in the embodiments and examples of this application, and to more completely understand this application and its beneficial effects, the drawings used in the description of the embodiments or examples will be briefly introduced below. Obviously, the drawings described below are merely some embodiments of this application. Those skilled in the art can obtain other drawings based on these drawings without creative effort. It should also be noted that the drawings are all drawn in a simplified form and are only used to conveniently and clearly assist in illustrating this application. The various dimensions of each component shown in the drawings are arbitrarily shown; they may be precise or not drawn to scale. For example, to make the illustration clearer, the dimensions of some components are appropriately exaggerated in the drawings. Unless otherwise specified, the components in the drawings are not drawn to scale. The drawings of this application do not limit each dimension of each component.
[0038] Figure 1 This is a schematic diagram of the infrared detection chip of this application;
[0039] Figure 2 This is a partial schematic diagram of the arrangement of thermal pixel units in the infrared detection chip of this application.
[0040] Among them, 100-integrated circuit substrate; 200-reflective layer; 300-resonant cavity structure layer; 400-thermal insulation structure layer; 500-support layer; 600-thermal layer; 610-thermal pixel unit; 611-three-phase vanadium oxide thermistor layer; 612-pad; 700-dielectric insulating layer; 800-electrode layer; 900-infrared absorption layer. Detailed Implementation
[0041] The present application will be further described in detail below with reference to the embodiments and examples. These embodiments and examples are only for illustrating the present application and are not intended to limit the scope of the present application. The purpose of providing these embodiments and examples is to make the disclosure of the present application more thorough and comprehensive. It should also be understood that the present application can be implemented in many different forms and is not limited to the embodiments and examples described herein. Those skilled in the art can make various modifications or alterations without departing from the spirit of the present application, and the equivalent forms obtained also fall within the protection scope of the present application. In addition, numerous specific details are set forth in the following description to provide a fuller understanding of the present application. It should be understood that the present application can be implemented without one or more of these details.
[0042] In this application, "optionally," "optionally," and "optional" mean that something is optional, that is, it means that it is selected from either "with" or "without." If there are multiple "optional" entries in a technical solution, unless otherwise specified, and there are no contradictions or mutual constraints, each "optional" entry shall be independent.
[0043] In this application, the terms "first aspect," "second aspect," etc., are used for descriptive purposes only and should not be construed as indicating or implying relative importance or quantity, nor should they be construed as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first aspect," "second aspect," etc., serve only as a non-exhaustive enumeration and should be understood not to constitute a closed limitation on quantity.
[0044] In this application, when numerical intervals (i.e., numerical ranges) are mentioned, unless otherwise specified, the distribution of selectable numerical values within the numerical interval is considered continuous, and includes the two endpoints of the numerical interval (i.e., the minimum and maximum values), as well as every numerical value between these two endpoints. Unless otherwise specified, when a numerical interval refers only to integers within that numerical interval, it includes the two endpoint integers of the numerical range, as well as every integer between the two endpoints, which is equivalent to directly listing every integer. When multiple numerical ranges are provided to describe features or characteristics, these numerical ranges can be merged. In other words, unless otherwise specified, the numerical ranges disclosed in this application should be understood to include any and all subranges included therein. The "numerical value" in the numerical interval can be any quantitative value, such as a number, percentage, ratio, etc. The term "numerical interval" can be broadly included to include percentage intervals, ratio intervals, proportion intervals, etc.
[0045] In traditional technologies, the materials used for single-phase vanadium oxide thermistor layers include vanadium dioxide, vanadium trioxide, or vanadium pentoxide. Vanadium dioxide exhibits inherent phase transition defects, undergoing a metal-insulator phase transition near 68℃, causing a sudden change in resistance and resulting in severe nonlinearity in the temperature measurement curve, leading to image distortion over a wide temperature range. Vanadium trioxide has relatively strong metallic properties, resulting in a relatively small absolute TCR value for the film, insufficient temperature response sensitivity, and low imaging contrast under weak infrared radiation. Vanadium pentoxide has relatively high insulation properties, resulting in a high sheet resistance for the film. While this can reduce the signal-to-noise ratio of the readout circuit, it makes it difficult to detect weak infrared signals. Therefore, traditional single-phase vanadium oxide thermistor layers struggle to simultaneously achieve high linearity detection, high TCR, and low noise over a wide temperature range of -40℃ to 120℃.
[0046] The first aspect of this application provides a three-phase vanadium oxide thermistor layer, comprising vanadium dioxide, vanadium trioxide, and vanadium pentoxide. The vanadium trioxide content in the three-phase vanadium oxide thermistor layer is 20% to 60% of the mass of vanadium dioxide; the vanadium pentoxide content in the three-phase vanadium oxide thermistor layer is 30% to 80% of the mass of vanadium dioxide.
[0047] In this three-phase vanadium oxide thermistor layer, vanadium dioxide, vanadium trioxide, and vanadium pentoxide work synergistically. Vanadium dioxide primarily provides the core negative temperature coefficient conductive channel, contributing to the high TCR (thermal response) of the three-phase vanadium oxide thermistor layer. Vanadium trioxide, as a metallic conductive phase, intersperses between vanadium dioxide grains, interrupting the continuous vanadium dioxide crystal phase and offsetting the abrupt phase transition of vanadium dioxide in the metal-insulator phase at 68℃, thus improving the overall carrier mobility of the thin film. Vanadium pentoxide, as an insulating barrier phase, is dispersed and fills the intergranular gaps in the film, regulating the overall sheet resistance of the film and suppressing lattice scattering and interface 1 / f noise. Therefore, the synergistic effect of these three phases achieves high linearity detection, high TCR, and low noise over a wide temperature range of -40℃ to 120℃.
[0048] It should be noted that vanadium dioxide (VO2), as the core material of the thermosensitive material, has an intrinsically high negative TCR and is the main source of temperature resistance changes, determining the basic temperature sensing sensitivity of the device. However, VO2 material alone suffers from a 68℃ phase transition defect. Furthermore, vanadium trioxide (V2O3), as a metallic vanadium oxide, has low resistance conductivity at room temperature (20℃~30℃). Dispersing V2O3 between VO2 grains can disrupt the continuous VO2 grain network, structurally eliminating the resistance step caused by the phase transition, while simultaneously improving the film's conductivity and preventing excessively high overall resistance. Vanadium pentoxide (V2O5), as a wide bandgap insulating phase, fills the grain boundaries of the three-phase composite film, restricting disordered carrier transitions and reducing thermal noise and 1 / f noise; it also finely adjusts the bulk sheet resistance to match the optimal operating impedance range of the infrared readout circuit.
[0049] For example, the mass of vanadium trioxide contained in the three-phase vanadium oxide thermistor layer is 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55% or 60% of the mass of vanadium dioxide.
[0050] The vanadium trioxide (vanadium oxide) content selected above can effectively block the continuous grains of vanadium dioxide, completely suppress its phase transition distortion at 68℃, and also ensure a suitable carrier mobility. If the vanadium trioxide content is relatively low, the insufficient number of metallic phase grains may prevent the complete disruption of the continuous VO2 crystal network, resulting in a significant resistance jump in the three-phase vanadium oxide thermistor layer near 68℃. Furthermore, the linearity of the temperature resistance curve of the three-phase vanadium oxide thermistor layer decreases significantly in the range of -40℃ to 120℃, leading to problems such as temperature tomography distortion in the infrared detection imaging image. If the vanadium trioxide content is relatively high, the higher proportion of the metallic conductive phase may result in a higher overall metallization degree of the three-phase vanadium oxide thermistor layer, leading to a significant decrease in the absolute value of the film's TCR, resulting in insufficient imaging contrast and decreased temperature measurement sensitivity under weak infrared radiation.
[0051] For example, the mass of vanadium pentoxide contained in the three-phase vanadium oxide thermistor layer is 30% to 80% of the mass of vanadium dioxide, for example, it can be 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75% or 80%.
[0052] By selecting the vanadium pentoxide content as described above, the sheet resistance of the film can be precisely controlled to match the readout circuit. It can also fill grain boundaries to suppress carrier scattering, effectively reducing 1 / f noise and thermal noise. If the vanadium pentoxide content is relatively low, insufficient insulating phase may lead to excessively high grain boundary defects and free carrier concentration, resulting in a significant increase in the film's noise amplitude and a deterioration in the circuit's signal-to-noise ratio, making it difficult to identify weak infrared signals. If the vanadium pentoxide content is relatively high, the excessive proportion of insulating phase may significantly reduce the carrier transport pathway, leading to excessively high sheet resistance, causing the resistance signal to exceed the readout circuit's acquisition range and weakening the device response.
[0053] In some embodiments, the vanadium dioxide content in the three-phase vanadium oxide thermistor layer is 40% to 65% by mass, for example, it can be 40%, 45%, 50%, 55%, 60% or 65%.
[0054] In some embodiments, the ratio of the amount of oxygen to the amount of vanadium in the three-phase vanadium oxide thermistor layer is 1.8 to 2.2, for example, 1.80, 1.85, 1.90, 1.95, 2.00, 2.05, 2.10, 2.15, or 2.20. Controlling the oxygen-vanadium ratio in the three-phase vanadium oxide thermistor layer as described above allows the three phases of vanadium dioxide, vanadium trioxide, and vanadium pentoxide to mutually dope each other, offsetting the abrupt phase transition of vanadium dioxide. This further ensures the continuous and consistent temperature-resistance change in the three-phase vanadium oxide thermistor layer and achieves a negative temperature coefficient (TCR), for example, -2.0% / K to -3.5% / K. If the oxygen-vanadium ratio is relatively low, the three-phase vanadium oxide thermistor layer may exhibit characteristics similar to metallic vanadium trioxide, resulting in a smaller absolute TCR value and lower sensitivity. If the ratio of oxygen to vanadium is relatively high, the three-phase vanadium oxide thermistor layer may be biased towards the insulating properties of vanadium pentoxide, resulting in higher overall film resistance and TCR attenuation, leading to increased noise.
[0055] In some embodiments, the thickness of the three-phase vanadium oxide thermistor layer is 50nm~100nm, for example, it can be 50nm, 55nm, 60nm, 65nm, 70nm, 75nm, 80nm, 85nm, 90nm, 95nm or 100nm.
[0056] In some embodiments, the three-phase vanadium oxide thermistor layer further contains a dopant element. This dopant element is used to suppress the growth of single vanadium oxide phase grains and organize vanadium dioxide grains into continuous sheets, thereby maintaining the coexistence of the three phases of vanadium dioxide, vanadium trioxide, and vanadium pentoxide in the film layer.
[0057] Optionally, the doping element includes at least one of tungsten, aluminum, titanium and chromium.
[0058] Optionally, the mass percentage of doped elements in the three-phase vanadium oxide thermistor layer is 0.5% to 3%, for example, it can be 0.5%, 1.0%, 1.5%, 2.0%, 2.5% or 3.0%.
[0059] The second aspect of this application also provides a method for preparing the three-phase vanadium oxide thermistor layer of the first aspect, comprising the following steps:
[0060] A stack of vanadium trioxide, vanadium dioxide, and vanadium pentoxide layers is deposited and formed. After annealing, a three-phase vanadium oxide thermistor layer containing vanadium dioxide, vanadium trioxide, and vanadium pentoxide is formed.
[0061] This preparation method involves annealing a laminate formed by sequentially stacking vanadium trioxide, vanadium dioxide, and vanadium pentoxide layers. During annealing, bidirectional diffusion of vanadium and oxygen atoms occurs within and between the amorphous precursor films of each layer. Vanadium trioxide releases oxygen ions, while vanadium pentoxide receives oxygen ions. The two react at the interlayer interface to generate a large number of nano-vanadium dioxide crystals in situ. Furthermore, during the heat preservation stage of annealing, the three-phase vanadium oxide thermistor layer can be crystallized as a whole, ultimately forming a mixed grain film dominated by crystalline phases, namely, a three-dimensional interlacing of V2O3 metal grains, VO2 thermistor grains, and V2O5 insulating grains.
[0062] It is understandable that during the deposition process to form a stack, the deposition can proceed in either the order of vanadium trioxide, vanadium dioxide, and vanadium pentoxide, or in the order of vanadium pentoxide, vanadium dioxide, and vanadium trioxide.
[0063] In some embodiments, the thickness of the vanadium trioxide layer is 17nm to 33nm, for example, it can be 17nm, 19nm, 21nm, 23nm, 25nm, 27nm, 29nm, 31nm or 33nm.
[0064] In some embodiments, the thickness of the vanadium dioxide layer is 17nm to 33nm, for example, it can be 17nm, 19nm, 21nm, 23nm, 25nm, 27nm, 29nm, 31nm or 33nm.
[0065] In some embodiments, the thickness of the vanadium pentoxide layer is 17nm to 33nm, for example, it can be 17nm, 19nm, 21nm, 23nm, 25nm, 27nm, 29nm, 31nm or 33nm.
[0066] The deposition thicknesses of the vanadium trioxide, vanadium dioxide, and vanadium pentoxide layers are controlled as described above to ensure sufficient diffusion of vanadium and oxygen atoms during annealing, forming a uniform mixture of vanadium dioxide, vanadium trioxide, and vanadium pentoxide grains. If the thickness of any single layer is relatively low, the total amount of precursor materials for the corresponding phase will be insufficient, resulting in too few grains of that component after annealing. This imbalance in the three-phase ratio makes it difficult to achieve the synergistic effect of phase transition suppression, TCR regulation, and noise reduction, leading to poor performance consistency between pixels in infrared detection. Conversely, if the thickness of any single layer is relatively high, the excessive thickness of the single layer may result in excessively long diffusion distances between atoms during annealing, increasing diffusion resistance. This leads to insufficient interlayer redox reactions, resulting in localized enrichment of a single phase, longitudinal layering and segregation, decreased linearity of the temperature resistance curve, large fluctuations in sheet resistance, increased device noise, and uneven brightness in the imaging image.
[0067] In some embodiments, the thickness of the three-phase vanadium oxide thermistor layer is 50nm~100nm, for example, it can be 50nm, 55nm, 60nm, 65nm, 70nm, 75nm, 80nm, 85nm, 90nm, 95nm, or 100nm. Selecting the thickness of the three-phase vanadium oxide thermistor layer as described above can further ensure sufficient diffusion of atoms between vanadium trioxide, vanadium dioxide, and vanadium pentoxide layers during annealing, improve the uniformity of three-phase grain dispersion within the film layer, and simultaneously consider both infrared absorption efficiency and film sheet resistance range, effectively improving the overall thermistor, noise, and linear response performance of the film layer. If the film layer thickness is relatively low, it may lead to insufficient total deposition of the three-layer precursor film during preparation, resulting in a lower total amount of three-phase components after annealing, easy local segregation of grains, large fluctuations in film sheet resistance, and poor performance consistency between pixel units; at the same time, the infrared light absorption is low, and the device detection sensitivity decreases. If the film thickness is relatively high, the atomic diffusion resistance inside the film may increase during annealing, which may lead to uneven phase distribution between the surface and the bottom layer, and local enrichment of a single vanadium oxide phase. Furthermore, it may also cause an increase in the heat capacity of the film, resulting in a slower heating / cooling response of the three-phase vanadium oxide thermistor layer, which may limit the infrared imaging frame rate and introduce greater thermal noise.
[0068] In some embodiments, the annealing temperature is 300℃~450℃, for example, 300℃, 320℃, 340℃, 360℃, 380℃, 400℃, 420℃, 440℃, or 450℃. Controlling the annealing temperature as described above allows for bidirectional diffusion of oxygen ions between vanadium trioxide and vanadium pentoxide, generating nano-vanadium dioxide grains in situ through interfacial redox reactions. This further ensures that the three-phase vanadium oxide thermistor layer contains stably coexisting nano-mixed grains of vanadium dioxide, vanadium trioxide, and vanadium pentoxide. If the annealing temperature is relatively low, insufficient atomic diffusion may prevent the formation of uniformly dispersed nano-mixed grains of vanadium dioxide, vanadium trioxide, and vanadium pentoxide. Furthermore, the film layer will be dominated by amorphous vanadium oxide with fewer crystalline phases, resulting in a lower absolute TCR value, poor thermal resistance linearity, a significant increase in 1 / f noise amplitude, and poor consistency in thermal performance among pixel units in infrared detection. If the annealing temperature is relatively high, vanadium trioxide may be completely oxidized to vanadium pentoxide by the residual oxygen in the cavity, leaving only vanadium pentoxide and vanadium dioxide in the film, or even only a single vanadium pentoxide insulating phase. This may lead to the complete disappearance of the phase change suppression effect and a sharp increase in the sheet resistance of the thin film, resulting in a significant decrease in temperature measurement sensitivity and a significant deterioration in the signal-to-noise ratio of the device.
[0069] In some embodiments, the holding time for annealing is 30 min to 120 min, for example, it can be 30 min, 40 min, 50 min, 60 min, 70 min, 80 min, 90 min, 100 min, 110 min or 120 min.
[0070] In some embodiments, the vacuum degree of the annealing process is 1×10⁻⁶. -3 Pa~5×10 -4 Pa.
[0071] Understandably, to prevent the laminate from being oxidized by oxygen in the environment during transport, the exposure time of the laminate to the air should be reduced, or the transport process should be carried out in a protective atmosphere or vacuum environment to reduce the oxidation of vanadium oxides in the laminate by oxygen in the environment. Optionally, the exposure time of the laminate to air during transport should be less than 5 minutes.
[0072] In some embodiments, a vanadium trioxide layer is deposited using magnetron sputtering, comprising: introducing argon gas as the working gas and oxygen gas as the reactant gas, and using a vanadium target for magnetron sputtering to form the vanadium trioxide layer. For example, the substrate temperature is 25°C to 100°C during the deposition of the vanadium trioxide layer.
[0073] Optionally, during the formation of the vanadium trioxide layer by magnetron sputtering, the oxygen flow rate is 2 sccm to 8 sccm, for example, 2 sccm, 3 sccm, 4 sccm, 5 sccm, 6 sccm, 7 sccm or 8 sccm.
[0074] Optionally, during the formation of the vanadium trioxide layer by magnetron sputtering, the argon gas flow rate is 40 sccm to 55 sccm.
[0075] Optionally, during the formation of the vanadium trioxide layer by magnetron sputtering, the power of the vanadium target is 1.0kW to 2.5kW, for example, 1.0kW, 1.3kW, 1.5kW, 1.7kW, 1.9kW, 2.1kW, 2.3kW or 2.5kW.
[0076] Optionally, the vanadium target containing doping elements is used in the process of forming the vanadium trioxide layer by magnetron sputtering. Further optionally, the mass percentage of the doping elements in the vanadium target is 0.5% to 3%, for example, it can be 0.5%, 1.0%, 1.5%, 2.0%, 2.5% or 3.0%.
[0077] In some embodiments, a vanadium dioxide layer is deposited using magnetron sputtering, comprising: introducing argon gas as the working gas and oxygen gas as the reactant gas, and forming the vanadium dioxide layer using a vanadium target magnetron sputtering. For example, the substrate temperature is 25°C to 100°C during the deposition of the vanadium dioxide layer.
[0078] Optionally, during the formation of the vanadium dioxide layer by magnetron sputtering, the oxygen flow rate is 10 sccm to 20 sccm, for example, it can be 10 sccm, 11 sccm, 12 sccm, 13 sccm, 14 sccm, 15 sccm, 16 sccm, 17 sccm, 18 sccm, 19 sccm or 20 sccm.
[0079] Optionally, during the formation of the vanadium dioxide layer by magnetron sputtering, the argon gas flow rate is 40 sccm to 55 sccm.
[0080] Optionally, during the formation of the vanadium dioxide layer by magnetron sputtering, the power of the vanadium target is 1.0kW to 2.5kW, for example, 1.0kW, 1.3kW, 1.5kW, 1.7kW, 1.9kW, 2.1kW, 2.3kW or 2.5kW.
[0081] Optionally, the vanadium target used in the magnetron sputtering process for forming the vanadium dioxide layer contains doping elements. Further optionally, the mass percentage of the doping elements in the vanadium target is 0.5% to 3%, for example, 0.5%, 1.0%, 1.5%, 2.0%, 2.5%, or 3.0%.
[0082] In some embodiments, a vanadium pentoxide layer is deposited using magnetron sputtering, comprising: introducing argon gas as the working gas and oxygen gas as the reactant gas, and using a vanadium target for magnetron sputtering to form the vanadium pentoxide layer. For example, the substrate temperature is 25°C to 100°C during the deposition of vanadium pentoxide.
[0083] Optionally, during the formation of the vanadium pentoxide layer by magnetron sputtering, the oxygen flow rate is 25 sccm to 40 sccm, for example, 25 sccm, 27 sccm, 29 sccm, 31 sccm, 33 sccm, 35 sccm, 37 sccm, 39 sccm or 40 sccm.
[0084] Optionally, during the formation of vanadium pentoxide by magnetron sputtering, the argon gas flow rate is 40 sccm to 55 sccm.
[0085] Optionally, during the formation of the vanadium pentoxide layer by magnetron sputtering, the power of the vanadium target is 1.0kW to 2.5kW, for example, 1.0kW, 1.3kW, 1.5kW, 1.7kW, 1.9kW, 2.1kW, 2.3kW or 2.5kW.
[0086] Optionally, the vanadium target containing doping elements is used in the process of forming the vanadium pentoxide layer by magnetron sputtering. Further optionally, the mass percentage of the doping elements in the vanadium target is 0.5% to 3%, for example, it can be 0.5%, 1.0%, 1.5%, 2.0%, 2.5% or 3.0%.
[0087] A third aspect of this application provides an infrared detection chip, including a thermistor layer. The thermistor layer includes the three-phase vanadium oxide thermistor layer of the first aspect.
[0088] like Figure 1 As shown, the infrared detection chip includes an integrated circuit substrate 100, and a reflective layer 200, a resonant cavity structure layer 300, a heat insulation structure layer 400, a support layer 500, a thermistor layer 600, a dielectric insulating layer 700, an electrode layer 800, and an infrared absorption layer 900 sequentially stacked on the surface of the integrated circuit substrate 100 along a direction away from the integrated circuit substrate 100. The thermistor layer 600 includes a three-phase vanadium oxide thermistor layer as described in the first aspect.
[0089] This infrared detection chip achieves secondary reflection and absorption of infrared light through a reflective layer and a resonant cavity structure layer. Combined with a heat insulation structure layer, it can effectively isolate heat diffusion, reduce heat loss, and effectively improve the sensitivity of infrared detection.
[0090] The infrared detection chip operates as follows: long-wave infrared radiation is emitted onto the infrared absorption layer, converting light energy into heat energy. This causes a temperature change in the corresponding three-phase vanadium oxide thermistor layer within the thermistor layer, resulting in a synchronous change in resistance value. This resistance change signal is transmitted to the integrated circuit substrate for readout and converted into a voltage signal. An external device then performs pseudo-color mapping processing on the voltage signal to output a visualized thermal imaging image.
[0091] In some embodiments, such as Figure 2 As shown, the thermal layer 600 includes a plurality of thermal pixel units 610 arranged in an array, and each thermal pixel unit 610 includes a three-phase vanadium oxide thermistor layer 611. It can be understood that the pads 612 are used to export the electrical signals of the three-phase vanadium oxide thermistor layer 611.
[0092] Optionally, such as Figure 2 As shown, the width 'a' of the thermal pixel unit is 8μm~10μm, for example, it can be 8.0μm, 8.5μm, 9.0μm, 9.5μm, or 10.0μm. Selecting the width of the thermal pixel unit as above balances infrared photosensitive area and array resolution. If the width of the thermal pixel unit is relatively low, insufficient photosensitive area may lead to reduced infrared energy absorption and decreased device detection sensitivity. If the width of the thermal pixel unit is relatively large, it may result in reduced imaging resolution.
[0093] Optionally, such as Figure 2 As shown, the width 'b' of the three-phase vanadium oxide thermistor layer is 6μm~9μm, for example, it can be 6.0μm, 6.5μm, 7.0μm, 7.5μm, 8.0μm, 8.5μm, or 9.0μm. Selecting the width of the three-phase vanadium oxide thermistor layer as above ensures a sufficient heat-sensitive area and avoids excessive contact with the pads, thus preventing noise introduction. If the width of the three-phase vanadium oxide thermistor layer is relatively low, the heat-sensitive area may be small, resulting in a lower resistance signal amplitude. If the width of the three-phase vanadium oxide thermistor layer is relatively high, the contact area between the three-phase vanadium oxide thermistor layer and the pads on both sides may be large, easily introducing additional contact noise.
[0094] Optionally, such as Figure 2As shown, the gap distance c between adjacent thermal pixel units is 1μm to 2μm, for example, it can be 1.0μm, 1.2μm, 1.4μm, 1.6μm, 1.8μm, or 2.0μm. Selecting the gap distance as above can isolate heat conduction and leakage between adjacent pixels, avoiding thermal crosstalk and electrical crosstalk. If the gap distance is relatively small, heat diffusion and leakage may occur between pixels, resulting in bright and dark crosstalk fringes in the image; if the gap distance is relatively large, it may lead to a significant decrease in the pixel fill factor, resulting in reduced infrared energy utilization and decreased infrared detection sensitivity.
[0095] In some embodiments, such as Figure 2 As shown, the width d of the pad is 2μm~3μm.
[0096] In some embodiments, the integrated circuit substrate includes a substrate layer and a circuit layer disposed on the substrate layer, the circuit layer being connected to a thermal layer to export the detection signal in the thermal layer. For example, it may be a substrate with an integrated ROIC (Readout Integrated Circuit) circuit.
[0097] The reflective layer can reflect unabsorbed light waves back into the infrared absorption layer, thereby improving the light energy utilization rate of the infrared detection chip. In some embodiments, the thickness of the reflective layer can be 80nm to 150nm. For example, the material of the reflective layer can be at least one of aluminum and titanium.
[0098] The resonant cavity structure layer can work in conjunction with the reflective layer to further enhance the reflection of the light wave of the wavelength under test, thereby improving the light energy utilization rate of the infrared detection chip. In some embodiments, the resonant cavity structure layer can be a quarter-wavelength optical resonant cavity to enhance wavelength energy absorption through the Fabry-Perot (FP) interference effect.
[0099] The thermal insulation layer can isolate heat transfer between the support layer and the resonant cavity structure layer, thereby reducing heat loss and improving detection sensitivity. In some embodiments, the thermal insulation layer can employ a microbridge structure to form a vacuum or air-filled thermal insulation cavity to block heat conduction from the support layer to the substrate. In some embodiments, the thickness of the thermal insulation layer can be 200 nm to 500 nm.
[0100] The support layer can serve as a mechanical framework to provide structural support and electrical isolation. In some embodiments, the thickness of the support layer can be 100 nm to 200 nm. For example, the material of the support layer can be silicon nitride.
[0101] The dielectric insulating layer prevents large-area contact between the electrode layer and the thermistor layer. Only a portion of the electrode layer penetrates the dielectric insulating layer to form a stable ohmic contact with the thermistor layer, creating a low-noise conductive path and reducing interface contact noise. In some embodiments, the thickness of the dielectric insulating layer can be 30 nm to 80 nm. For example, the material of the dielectric insulating layer can be silicon nitride.
[0102] The electrode layer is used for electrical connection with the thermistor layer to enable the transmission of detection signals. In some embodiments, the thickness of the electrode layer can be 50 nm to 120 nm. For example, the material of the electrode layer can be at least one of nickel, titanium, and platinum.
[0103] The infrared absorption layer is used to capture infrared light energy and convert it into heat energy, thereby raising the temperature of the thermistor layer to achieve temperature detection. It is understood that a suitable infrared absorption layer material and size can be selected based on the wavelength of the absorbed light. In some embodiments, the thickness of the infrared absorption layer can be 60 nm to 120 nm. For example, the material of the infrared absorption layer can be at least one of silicon nitride, silicon oxide, and carbon nanoparticles.
[0104] The embodiments of this application will be described in detail below with reference to examples. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of this application. For experimental methods in the following embodiments where specific conditions are not specified, please refer to the guidelines given in this application, or follow experimental manuals or conventional conditions in the art, or follow the conditions recommended by the manufacturer, or refer to experimental methods known in the art.
[0105] Example 1
[0106] S1. Using a silicon wafer with a pre-integrated ROIC readout circuit as a substrate, a thin film of Al material is deposited by sputtering process. After photolithography and etching patterning, a reflective layer and bottom electrode pads are formed simultaneously. A 1 / 4 wavelength optical resonant cavity is set on the reflective layer to achieve secondary absorption of incident infrared light from 8μm to 14μm, which greatly improves the infrared energy utilization rate.
[0107] S2. Spin-coat a polyimide sacrificial layer onto the reflective layer, and use photolithography to create through holes for the pier anchor points, reserving cavity space for the subsequent micro-bridge suspended structure to define the heat insulation structure layer.
[0108] S3. Deposit a support layer on the surface of the patterned sacrificial layer. The support layer is made of silicon nitride and has a thickness of 150 nm.
[0109] S4. A thermistor layer is deposited on the surface of the support layer using magnetron sputtering. The thermistor layer includes multiple thermistor pixel units arranged in an array. Each thermistor pixel unit includes a three-phase vanadium oxide thermistor layer and pads disposed at both ends thereon. The width of the pads is 2 μm. The width of the thermistor pixel unit is 10 μm; the width of the three-phase vanadium oxide thermistor layer is 6 μm; and the gap between adjacent thermistor pixel units is 2 μm.
[0110] The deposition method of the three-phase vanadium oxide thermistor layer includes: introducing argon gas as the working gas and oxygen gas as the reactant gas, and forming a vanadium trioxide layer with a thickness of 22 nm by magnetron sputtering on the surface of the support layer using a vanadium target. The temperature of the support layer as the substrate is 40℃, the argon gas flow rate is 48 sccm, the oxygen flow rate is 5 sccm, the power of the vanadium target is 1.8 kW, and the vanadium target contains 1.2% tungsten by mass.
[0111] Argon gas was introduced as the working gas and oxygen gas as the reactant gas. A vanadium dioxide layer with a thickness of 25 nm was formed on the surface of a vanadium oxide layer by magnetron sputtering using a vanadium target. The temperature of the vanadium oxide layer as the substrate was 40 °C, the argon gas flow rate was 48 sccm, the oxygen flow rate was 15 sccm, the power of the vanadium target was 1.8 kW, and the vanadium target contained 1.2% tungsten by mass.
[0112] Argon gas was introduced as the working gas and oxygen gas as the reactant gas. A vanadium pentoxide layer with a thickness of 28 nm was formed on the surface of a vanadium dioxide layer by magnetron sputtering using a vanadium target. The temperature of the vanadium dioxide layer as the substrate was 40 °C, the argon gas flow rate was 48 sccm, the oxygen flow rate was 32 sccm, the power of the vanadium target was 1.8 kW, and the vanadium target contained 1.2% tungsten by mass.
[0113] The above-mentioned vanadium trioxide layer, vanadium dioxide layer and vanadium pentoxide layer stacked in a vacuum of 3×10 - 4 The vanadium oxide thermistor layer was obtained by annealing at 380℃ for 60 min. The vanadium dioxide content in the vanadium oxide thermistor layer was 52%, vanadium trioxide content was 21%, and vanadium pentoxide content was 27%. The ratio of the amount of oxygen to the amount of vanadium in the vanadium oxide thermistor layer was 2.05.
[0114] S5. A dielectric insulating layer, made of silicon nitride and 50 nm thick, is deposited on the surface of the thermistor layer. Then, a dry etching process is used to penetrate the dielectric insulating layer to create electrode contact holes. A metal electrode layer is then deposited and patterned to form a stable ohmic contact between the electrode layer and the thermistor layer. The electrode layer is made of nickel and 80 nm thick.
[0115] S6. An infrared absorption layer is deposited on the surface of the electrode layer. The infrared absorption layer is made of silicon oxide and has a thickness of 90 nm.
[0116] S7. The sacrificial layer is completely removed by oxygen plasma dry etching, while the heat-insulating bridge arms and pier anchor points are retained to connect the bridge deck and the substrate, forming a completely suspended heat-insulating microbridge structure, thus obtaining an infrared detection chip.
[0117] S8. Vacuum sealing and encapsulation of the infrared detection chip isolates moisture and dust, stabilizes the working environment of the infrared detection chip, and improves the long-term stability of the device.
[0118] Example 2
[0119] The infrared detector chip was prepared using essentially the same method as in Example 1, except that in step S4, the thickness of the vanadium trioxide layer was 18 nm, the thickness of the vanadium dioxide layer was 20 nm, and the thickness of the vanadium pentoxide layer was 32 nm. The annealing temperature was 320°C, and the holding time was 100 min.
[0120] In the three-phase vanadium oxide thermistor layer, vanadium dioxide accounts for 44% of the mass, vanadium trioxide accounts for 23% of the mass, and vanadium pentoxide accounts for 33% of the mass. The ratio between the amount of oxygen and the amount of vanadium in the three-phase vanadium oxide thermistor layer is 1.92.
[0121] Example 3
[0122] The infrared detector chip was prepared using essentially the same method as in Example 1, except that in step S4, the thickness of the vanadium trioxide layer was 30 nm, the thickness of the vanadium dioxide layer was 30 nm, and the thickness of the vanadium pentoxide layer was 22 nm. The annealing temperature was 430°C, and the holding time was 30 min.
[0123] In the three-phase vanadium oxide thermistor layer, the mass percentage of vanadium dioxide is 48%, the mass percentage of vanadium trioxide is 26%, and the mass percentage of vanadium pentoxide is 26%. The ratio between the amount of oxygen and the amount of vanadium in the three-phase vanadium oxide thermistor layer is 2.16.
[0124] Example 4
[0125] The infrared detection chip was prepared using a method that was basically the same as in Example 1, except that the annealing temperature in step S4 was 280°C.
[0126] Example 5
[0127] The infrared detection chip was prepared using a method that was basically the same as in Example 1, except that the annealing temperature in step S4 was 470°C.
[0128] Comparative Example 1
[0129] The infrared detection chip was prepared using a method that was basically the same as in Example 1, except that no vanadium dioxide layer was deposited in step S4.
[0130] Comparative Example 2
[0131] The infrared detection chip was prepared using a method that was basically the same as in Example 1, except that no vanadium trioxide layer was deposited in step S4.
[0132] Comparative Example 3
[0133] The infrared detection chip was prepared using a method that was basically the same as in Example 1, except that no vanadium pentoxide layer was deposited in step S4.
[0134] Comparative Example 4
[0135] The infrared detection chip was prepared using a method that was basically the same as in Example 1, except that in step S4, the three-phase vanadium oxide thermistor layer was replaced with a vanadium dioxide layer formed by vanadium dioxide deposition.
[0136] Comparative Example 5
[0137] The infrared detection chip was prepared using a method that was basically the same as in Example 1, except that the thickness of the vanadium dioxide layer in step S4 was 50 nm.
[0138] Comparative Example 6
[0139] The infrared detection chip was prepared using a method that was basically the same as in Example 1, except that the thickness of the vanadium trioxide layer in step S4 was 50 nm.
[0140] Comparative Example 7
[0141] The infrared detection chip was prepared using a method that was basically the same as in Example 1, except that the thickness of the vanadium pentoxide layer in step S4 was 50 nm.
[0142] The infrared detection chips prepared in the above embodiments and comparative examples were subjected to performance testing. The testing methods included:
[0143] TCR Test: The infrared detector chip was placed in a constant temperature chamber and the temperature was gradually increased from -40℃ to 120℃ at a rate of 1℃ / min. Each temperature point was held for 30 minutes to allow the chip to reach thermal equilibrium. The steady-state resistance of the thin film was collected using a semiconductor parameter analyzer in a four-wire system, and the TCR was calculated as TCR = ΔR / (R0×ΔT), where ΔR is the resistance change corresponding to the temperature change, R0 is the steady-state resistance of the three-phase vanadium oxide thermistor layer at 25℃, and ΔT is the temperature change in K.
[0144] Noise test: The 1 / f noise amplitude of the infrared detection chip in the range of 1Hz to 10kHz was tested using a low noise signal analyzer at 30℃.
[0145] Temperature-resistance test over a wide temperature range of -40℃ to 120℃: The resistance values of the infrared detection chip were measured at -40℃, 0℃, 40℃, 80℃, and 120℃. A linear correlation coefficient R was calculated by fitting the resistance values to the temperature. 2 To evaluate linearity.
[0146] The test results are shown in Table 1.
[0147] Table 1
[0148]
[0149] As can be seen from Table 1:
[0150] Compared to Examples 4-5, Example 4 had a relatively low annealing temperature. Due to insufficient driving force for the diffusion of vanadium and oxygen atoms between layers, the proportion of amorphous phase in the film was relatively high, and the three-phase grains were unevenly dispersed, resulting in a decrease in the absolute value of the film's TCR, a deterioration in the linearity of temperature resistance, and a degradation in noise performance. Example 5 had a relatively high annealing temperature. As the residual oxygen in the chamber oxidized and consumed a large amount of the metallic vanadium trioxide phase, the three-phase equilibrium ratio was broken, leaving only vanadium dioxide and vanadium pentoxide phases. The phase transformation suppression effect disappeared, and the linear response of the resistance over a wide temperature range deteriorated.
[0151] Compared with Comparative Examples 1-4, Example 1 shows that, since Comparative Examples 1-3 did not form a blended grain structure of vanadium trioxide, vanadium dioxide, and vanadium pentoxide, the lack of any one phase prevents the synergistic regulation of the metallic phase, the thermosensitive phase, and the insulating phase. Therefore, the abrupt phase transition of VO2 at 68℃ cannot be eliminated, and high TCR sensitivity and low noise performance cannot be simultaneously achieved. The film layer exhibits obvious nonlinear distortion in the temperature measurement curve from -40℃ to 120℃. Comparative Example 4, which uses a pure vanadium dioxide thin film, is also constrained by the phase transition effect, resulting in high noise and poor linear response over a wide temperature range.
[0152] Compared with Comparative Examples 5-7, Example 1 shows that adjusting the thickness of the vanadium trioxide, vanadium dioxide, and vanadium pentoxide layers—that is, adjusting their contents—can precisely balance the proportions of the three phase components, completely suppress the VO2 metal-insulator phase transition, stabilize high TCR, reduce film noise, and achieve excellent pixel unit performance consistency. In Comparative Example 5, the relatively high vanadium dioxide content leads to a large number of continuous vanadium dioxide grain networks in the film due to the excessive proportion of the thermosensitive core phase. This results in the recurrence of the 68°C resistance step abrupt change, temperature discontinuity in wide-temperature imaging, and a significant decrease in the linear correlation coefficient. In Comparative Example 6, the relatively high vanadium trioxide content leads to an excessive metallic conductive phase and a high overall metallization degree in the film, resulting in a significant decrease in the absolute TCR value, insufficient imaging contrast under weak infrared radiation, and decreased temperature sensitivity. In Comparative Example 7, the vanadium pentoxide content is relatively high. Due to the excessively high proportion of the insulating barrier phase, the carrier conduction channels are greatly reduced, resulting in problems such as excessively high sheet resistance of the thin film, weak signal amplitude of the readout circuit, and a significant increase in 1 / f noise and thermal noise.
[0153] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0154] The embodiments described above are merely illustrative of several implementation methods of this application, and while the descriptions are specific and detailed, they should not be construed as limiting the scope of the application. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of this application, and these modifications and improvements all fall within the scope of protection of this application. Therefore, the scope of protection of this application should be determined by the appended claims, and the specification can be used to interpret the content of the claims.
Claims
1. A three-phase vanadium oxide thermistor layer, characterized in that, The three-phase vanadium oxide thermistor layer comprises vanadium dioxide, vanadium trioxide, and vanadium pentoxide; wherein the mass of vanadium trioxide contained in the three-phase vanadium oxide thermistor layer is 20% to 60% of the mass of vanadium dioxide; and the mass of vanadium pentoxide contained in the three-phase vanadium oxide thermistor layer is 30% to 80% of the mass of vanadium dioxide.
2. The three-phase vanadium oxide thermistor layer as described in claim 1, characterized in that, The three-phase vanadium oxide thermistor layer satisfies at least one of the following conditions: (1) The vanadium dioxide content of the three-phase vanadium oxide thermistor layer is 40%~65% by mass; (2) The ratio between the amount of oxygen and the amount of vanadium in the three-phase vanadium oxide thermistor layer is 1.8 to 2.
2. (3) The thickness of the three-phase vanadium oxide thermistor layer is 50nm~100nm.
3. The three-phase vanadium oxide thermistor layer as described in claim 1 or 2, characterized in that, The three-phase vanadium oxide thermistor layer also contains doping elements; Optionally, the doping element includes at least one selected from tungsten, aluminum, titanium, and chromium; Optionally, the mass percentage of the doped element in the three-phase vanadium oxide thermistor layer is 0.5% to 3%.
4. A method for preparing a three-phase vanadium oxide thermistor layer according to any one of claims 1-3, characterized in that, Includes the following steps: A stacked body consisting of vanadium trioxide, vanadium dioxide, and vanadium pentoxide layers is deposited. After annealing the stacked body, a three-phase vanadium oxide thermistor layer containing vanadium dioxide, vanadium trioxide, and vanadium pentoxide is formed.
5. The method for preparing the three-phase vanadium oxide thermistor layer as described in claim 4, characterized in that, The preparation method satisfies at least one of the following conditions: (1) The thickness of the vanadium trioxide layer is 17 nm to 33 nm; (2) The thickness of the vanadium dioxide layer is 17 nm to 33 nm; (3) The thickness of the vanadium pentoxide layer is 17 nm to 33 nm; (4) The annealing temperature is 300℃~450℃, the holding time is 30min~120min, and the vacuum degree is 1×10 - 3 Pa~5×10 -4 Pa.
6. The method for preparing the three-phase vanadium oxide thermistor layer as described in claim 4 or 5, characterized in that, The vanadium trioxide layer is deposited by magnetron sputtering, which includes: introducing argon gas as the working gas and oxygen gas as the reaction gas, and using a vanadium target to form the vanadium trioxide layer by magnetron sputtering. Optionally, during the formation of the vanadium trioxide layer by magnetron sputtering, the oxygen flow rate is 2 sccm to 8 sccm; Optionally, during the formation of the vanadium trioxide layer by magnetron sputtering, the power of the vanadium target is 1.0kW to 2.5kW; Optionally, the vanadium target containing doping elements is used in the process of forming the vanadium trioxide layer by magnetron sputtering; further optionally, the mass percentage of the doping elements in the vanadium target is 0.5% to 3%.
7. The method for preparing the three-phase vanadium oxide thermistor layer as described in claim 4 or 5, characterized in that, The vanadium dioxide layer is deposited by magnetron sputtering, which includes: introducing argon gas as the working gas and oxygen gas as the reaction gas, and using a vanadium target to form the vanadium dioxide layer by magnetron sputtering. Optionally, during the formation of the vanadium dioxide layer by magnetron sputtering, the oxygen flow rate is 10 sccm to 20 sccm; Optionally, during the formation of the vanadium dioxide layer by magnetron sputtering, the power of the vanadium target is 1.0kW to 2.5kW; Optionally, the vanadium target containing doping elements is used in the process of forming the vanadium dioxide layer by magnetron sputtering; further optionally, the mass percentage of the doping elements in the vanadium target is 0.5% to 3%.
8. The method for preparing the three-phase vanadium oxide thermistor layer as described in claim 4 or 5, characterized in that, The vanadium pentoxide layer is deposited by magnetron sputtering, which includes: introducing argon gas as the working gas and oxygen gas as the reaction gas, and using a vanadium target to form the vanadium pentoxide layer by magnetron sputtering. Optionally, during the formation of the vanadium pentoxide layer by magnetron sputtering, the oxygen flow rate is 25 sccm to 40 sccm; Optionally, during the formation of the vanadium pentoxide layer by magnetron sputtering, the power of the vanadium target is 1.0kW to 2.5kW; Optionally, the vanadium target containing doping elements is used in the process of forming the vanadium pentoxide layer by magnetron sputtering; further optionally, the mass percentage of the doping elements in the vanadium target is 0.5% to 3%.
9. An infrared detection chip, characterized in that, It includes a thermistor layer, wherein the thermistor layer comprises the three-phase vanadium oxide thermistor layer according to any one of claims 1-3.
10. The infrared detection chip as described in claim 9, characterized in that, The thermal layer includes multiple thermal pixel units arranged in an array, and each thermal pixel unit includes the three-phase vanadium oxide thermistor layer; Optionally, the width of the three-phase vanadium oxide thermistor layer is 6μm~9μm; Optionally, the gap between adjacent thermal pixel units is 1μm to 2μm.