A surface-reconstructed zinc foil and a preparation method and application thereof

By forming a surface reconstruction layer with a specific crystal orientation on the zinc foil surface, the problems of uneven zinc deposition and dendrite growth in zinc-ion batteries are solved, achieving high cycle stability and high coulombic efficiency in zinc-ion batteries.

CN123162111APending Publication Date: 2026-11-24JIAMUSI UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611384286.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-08
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing zinc-ion batteries suffer from problems such as uneven zinc deposition, severe dendrite growth, interfacial side reactions, and poor cycle stability during the zinc anode process.

Method used

A surface reconstruction layer with a specific crystal orientation was formed on the surface of zinc foil using a urea-assisted heat treatment method to regulate the deposition behavior of zinc ions and prepare surface-reconstructed zinc anode materials.

Benefits of technology

The zinc anode material improves the cycle stability and rate performance of zinc-ion batteries, exhibiting good long-term cycle stability and high coulombic efficiency under high current density and high areal capacity conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123162111A_ABST
    Figure CN123162111A_ABST
Patent Text Reader

Abstract

This invention relates to a surface-reconstructed zinc foil, its preparation method, and its application, belonging to the field of zinc-ion battery technology. The purpose of this invention is to solve the problems of uneven zinc deposition, severe dendrite growth, interfacial side reactions, and poor cycle stability in existing zinc-ion batteries' zinc anodes during cycling. This invention employs a urea-assisted heat treatment method to thermally induce reconstruction on the zinc foil surface, forming a surface-reconstructed layer with specific crystal orientation and compositional characteristics, thus obtaining a surface-reconstructed zinc anode material. This surface-reconstructed zinc anode material is then applied to the anode of a zinc-ion battery to improve zinc deposition behavior and cycle stability. (The last sentence appears to be incomplete and possibly refers to a specific process, "at 1 mA cm⁻¹".) ‑2 Current density and 1mAh cm ‑2 Under the given areal capacity conditions, the Zn||Zn symmetric cell using the ZU-400 surface-reconstructed zinc anode of the present invention can cycle stably for more than 3380 hours, demonstrating good high current density cycling stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of zinc-ion battery technology, specifically relating to a surface-reconstructed zinc foil, its preparation method, and its application. Background Technology

[0002] With the continuous advancement of science and technology and society, various electronic devices and large-scale energy storage systems are developing rapidly, leading to higher demands for safe, efficient, and low-cost rechargeable battery energy storage technologies. Simultaneously, the massive consumption of traditional fossil fuels and increasingly severe environmental problems have made the development of new green energy storage systems a crucial research direction. Lithium-ion batteries, with their high energy density and long cycle life, have been widely used, but issues such as resource costs, the safety of organic electrolytes, and their applicability to large-scale energy storage still limit their further development.

[0003] In recent years, aqueous zinc-ion batteries have attracted widespread attention due to their use of non-flammable aqueous electrolytes and their advantages such as abundant zinc resources, low cost, environmental friendliness, and high theoretical capacity of metallic zinc. Metallic zinc also possesses high volumetric capacity and low redox potential, making it an important choice for the anode material in aqueous zinc-ion batteries. Therefore, the stability of the zinc anode directly affects the cycle life and practical application performance of aqueous zinc-ion batteries.

[0004] However, during repeated deposition / stripping, zinc is prone to uneven nucleation and localized current concentration, leading to the gradual formation of dendrites and porous, loose deposition structures. Simultaneously, side reactions such as hydrogen evolution, corrosion, and the formation of byproducts like basic zinc sulfate easily occur between the aqueous electrolyte and the zinc metal. These unstable interfacial processes mutually reinforce each other, continuously deteriorating the zinc deposition morphology and potentially causing increased battery polarization, loss of active zinc, and internal short circuits, thus severely limiting the cycle life of the zinc metal anode.

[0005] To address the aforementioned issues, current methods typically employ electrolyte modulation, artificial interface layers, three-dimensional current collectors, and surface structure engineering to regulate zinc deposition behavior. While artificial interface layers and complex three-dimensional structures can improve zinc ion transport and current distribution to some extent, they often involve additional material preparation steps and interface construction processes, resulting in complex fabrication techniques and the potential introduction of additional interfacial impedance. Therefore, employing simple, low-cost, and easily scalable methods to directly control the structure and crystal state of the zinc metal surface is of great significance for improving the cycle stability of zinc metal anodes.

[0006] Zinc metal exhibits a variety of crystal orientations, with significant differences in surface energy, atomic arrangement, and interfacial interactions with zinc ions across different crystal planes. Therefore, zinc deposition behavior is closely related to the initial crystal structure of the anode surface. By controlling the crystal structure of the zinc foil surface to form a reconstructed layer with a specific crystal orientation, it is hoped that the adsorption, nucleation, and subsequent growth behavior of zinc ions on the electrode surface can be altered, thereby enabling the control of the zinc deposition process. However, existing zinc anode modification methods rarely achieve in-situ reconstruction of the zinc foil surface crystal structure directly through a simple heat treatment process, and further utilize the reconstructed crystal surface to control the directional deposition of zinc. Summary of the Invention

[0007] The purpose of this invention is to solve the problems of uneven zinc deposition, severe dendrite growth, interfacial side reactions, and poor cycle stability in existing zinc-ion batteries with zinc anodes during cycling. This invention provides a surface-reconstructed zinc foil, its preparation method, and its application. By subjecting the zinc foil to urea-assisted heat treatment, a thermally induced reconstruction layer is constructed on the surface of the zinc foil, thereby regulating the deposition behavior of zinc ions and improving the cycle stability and rate performance of zinc-ion batteries.

[0008] To achieve the above objectives, the present invention adopts the following technical solution:

[0009] This invention employs a urea-assisted heat treatment method to thermally induce reconstruction on the surface of zinc foil, forming a surface reconstruction layer with specific crystal orientation and compositional characteristics on the zinc foil surface, thereby obtaining a surface-reconstructed zinc anode material. This surface-reconstructed zinc anode material is then applied to the anode of a zinc-ion battery to improve zinc deposition behavior and cycle stability. Specifically, the invention includes the following:

[0010] A surface-reconstructed zinc foil includes a metallic zinc foil substrate and a crystal structure reconstruction layer formed on the surface of the metallic zinc foil substrate by heat treatment;

[0011] The crystal structure reconstruction layer has Zn(002) crystal plane as the main crystal orientation.

[0012] A method for preparing a surface-reconstructed zinc foil is specifically carried out according to the following steps:

[0013] 1. The zinc foil is cleaned and dried to remove contaminants from its surface, resulting in pretreated zinc foil.

[0014] 2. Place the pretreated zinc foil in a tube furnace, and then place urea upstream of the zinc foil;

[0015] 3. Under nitrogen atmosphere protection, the tube furnace is heated from room temperature to 300℃~500℃ and held at that temperature to allow thermally induced surface diffusion and recrystallization to occur on the zinc foil surface, promoting the reconstruction of the crystal structure on the zinc foil surface. After the holding period, the foil is naturally cooled to room temperature to obtain a surface-reconstructed zinc foil (named ZU-X, where X is the annealing temperature).

[0016] A surface-reconstructed zinc foil is used directly as the negative electrode in an aqueous zinc-ion battery.

[0017] The principle of this invention:

[0018] This invention discloses a surface-reconstructed zinc foil and its preparation method. By subjecting the zinc foil to urea-assisted heat treatment under a nitrogen atmosphere (urea provides small amounts of O and N elements and maintains a mild reaction environment), thermally induced structural reconstruction occurs on the zinc foil surface, forming a surface-reconstructed layer with a specific crystal orientation. This, in turn, regulates the deposition behavior of zinc ions on the negative electrode surface. This method eliminates the need for complex artificial coatings or three-dimensional structures, simplifies the preparation process, and improves the deposition uniformity and cycle stability of the zinc metal negative electrode.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] I. This invention proposes a method for preparing surface-reconstructed zinc anode materials by inducing in-situ structural reconstruction on the surface of zinc foil through heat treatment; the method uses ordinary zinc foil as a substrate and forms a reconstruction layer on the surface of the zinc foil through urea-assisted heat treatment, without the need to introduce additional complex artificial coatings or three-dimensional structures, and has the characteristics of simple preparation process, convenient operation and easy large-scale implementation;

[0021] II. By controlling the heat treatment temperature, this invention can adjust the degree of reconstruction and crystal structure of the zinc foil surface; among them, ZU-400 obtained by heat treatment at 400℃ has obvious surface reconstruction characteristics and exhibits a surface crystal structure dominated by Zn(002) crystal plane, which is beneficial to control the subsequent zinc nucleation and crystal growth behavior, making zinc deposition more uniform and orderly.

[0022] III. Experimental results show that at 1 mA cm -2 Current density and 1mAh cm -2 Under the given areal capacity conditions, the Zn||Zn symmetric cell using the ZU-400 surface-reconstructed zinc anode of this invention can stably cycle for over 3380 hours, significantly exceeding the cycle life of commercial zinc foil without heat treatment and electrodes obtained at other heat treatment temperatures; at 10 mA cm -2 and 10mAh cm -2 Under conditions of high current density and high areal capacity, ZU-400 can still maintain stable cycling for more than 1000 hours, demonstrating good high current density cycling stability.

[0023] IV. In Zn||Cu half-cells, when using the ZU-400 of this invention as the zinc anode for zinc deposition / stripping tests, the cell can stably cycle for more than 1600 cycles and maintain an average coulombic efficiency of about 99.4%. The Zn||MnO2 full cell assembled with ZU-400 as the anode can stably cycle for more than 2000 cycles, while the full cell using bare zinc as the anode experiences significant failure after about 250 cycles. Attached Figure Description

[0024] Figure 1 Scanning electron microscope images of the ZU-X zinc anode material prepared in Example 1, where a is ZU-300, b is ZU-400, and c is ZU-500;

[0025] Figure 2 The cross-section of the ZU-400 zinc anode material prepared in Example 1 shows the distribution of O and Zn elements.

[0026] Figure 3 X-ray diffraction patterns of the ZU-X zinc anode material prepared in Example 1 and related standard cards;

[0027] Figure 4 To test the Zn||Zn symmetric cell assembled using the ZU-X zinc anode material prepared in Example 1 as the anode of a zinc-ion battery at 1 mA cm⁻¹ -2 Current density, 1mAh cm -2 Long-cycle charge-discharge data under isotope capacity conditions;

[0028] Figure 5 When ZU-X prepared in Example 1 of this invention is used as the negative electrode material of a zinc-ion battery, the symmetric cell operates at 10 mA cm⁻¹. –2 Current density, 10mAh cm -2 Long-cycle charge-discharge data under isotope capacity conditions;

[0029] Figure 6 When ZU-X prepared in Example 1 of this invention is used as the negative electrode material of a zinc-ion battery, the Zn||Cu half-cell exhibits a performance of 1 mA cm⁻¹. –2 Graphs of coulombic efficiency data under current density and 1V cutoff conditions;

[0030] Figure 7 When ZU-400 prepared in Example 1 of this invention is used as the negative electrode material of a zinc-ion battery, the Zn||MnO2 full cell at 1A g –1 Charging and discharging cycle data at current density. Detailed Implementation

[0031] Specific implementation method one: This implementation method is a surface reconstructed zinc foil, including a metallic zinc foil substrate and a crystal structure reconstruction layer formed on the surface of the metallic zinc foil substrate through heat treatment;

[0032] The crystal structure reconstruction layer has Zn(002) crystal plane as the main crystal orientation.

[0033] Specific Implementation Method Two: This implementation method is a method for preparing surface-reconstructed zinc foil, specifically completed according to the following steps:

[0034] 1. The zinc foil is cleaned and dried to remove contaminants from its surface, resulting in pretreated zinc foil.

[0035] 2. Place the pretreated zinc foil in a tube furnace, and then place urea upstream of the zinc foil;

[0036] 3. Under nitrogen atmosphere protection, the tube furnace is heated from room temperature to 300℃~500℃ and held at that temperature to induce thermal diffusion and recrystallization on the zinc foil surface, promoting the reconstruction of the crystal structure on the zinc foil surface. After the holding period, the furnace is naturally cooled to room temperature to obtain the surface-reconstructed zinc foil.

[0037] Specific Implementation Method Three: This implementation method differs from Specific Implementation Method One or Two in that the zinc foil mentioned in step one is high-purity zinc foil with a mass fraction of 99.99% and a thickness of 20 μm. The other steps are the same as in Specific Implementation Method One or Two.

[0038] Specific Implementation Method Four: This implementation method differs from Specific Implementation Methods One to Three in that: in step one, the zinc foil is cleaned sequentially with anhydrous ethanol and deionized water, and then dried at 60°C for 6 hours. The other steps are the same as in Specific Implementation Methods One to Three.

[0039] Specific Implementation Method Five: This implementation method differs from Specific Implementation Methods One through Four in that: in step two, urea is placed 5cm upstream of the zinc foil; the surface area of ​​the zinc foil to the mass ratio of the urea is 1.54cm². 2 1g. The other steps are the same as those in specific implementation methods one to four.

[0040] Specific Implementation Method Six: This implementation method differs from Specific Implementation Methods One through Five in that the purity of the nitrogen gas mentioned in steps Two and Three is not less than 99.9%, and the nitrogen gas flow rate is 100 mL / min. -1 The other steps are the same as those in Specific Implementation Methods One through Five.

[0041] Specific Implementation Method Seven: This implementation method differs from Specific Implementation Methods One through Six in that: the heat preservation time mentioned in step two is 2 hours; the heating rate mentioned in step two is 2°C / min. -1The other steps are the same as those in Specific Implementation Methods One through Six.

[0042] Specific implementation method eight: This implementation method is a surface-reconstructed zinc foil used directly as the negative electrode of an aqueous zinc-ion battery.

[0043] Specific Implementation Method Nine: This implementation method differs from Specific Implementation Methods One to Eight in that the aqueous zinc-ion battery includes a surface-reconstructed zinc foil, a positive electrode, a separator, and an aqueous electrolyte. Other steps are the same as in Specific Implementation Methods One to Eight.

[0044] Specific Implementation Method Ten: This implementation method differs from Specific Implementation Methods One to Nine in that: the positive electrode is manganese dioxide; the diaphragm is glass fiber; and the aqueous electrolyte is a 2 mol / L zinc sulfate solution. Other steps are the same as in Specific Implementation Methods One to Nine.

[0045] The present invention will be further described in detail below with reference to specific embodiments. The raw materials involved in the embodiments, such as zinc foil, urea, nitrogen, zinc salt electrolyte, and manganese dioxide, can all be obtained from commercially available products.

[0046] Example 1: A method for preparing a surface-reconstructed zinc foil, specifically comprising the following steps:

[0047] 1. Cut commercial zinc foil with a thickness of 20μm into circular electrode sheets with a diameter of 14mm. Use anhydrous ethanol for ultrasonic cleaning for 10min to remove stains on the surface of the zinc foil. After cleaning, place it in an oven and dry at 60℃ for 6h to obtain the pretreated zinc foil.

[0048] 2. Place the pretreated zinc foil in a tube furnace, and then place 1g of urea upstream of the zinc foil, keeping the distance between the urea and the zinc foil at 5cm.

[0049] 3. Introduce nitrogen gas into the tubular furnace at a flow rate of 50 mL / min. -1 The tube furnace was heated at 2°C for 2 minutes under a nitrogen atmosphere. -1 The temperature was increased from room temperature to 300℃, 400℃, and 500℃, and held for 2 hours to induce thermally induced surface diffusion and recrystallization on the zinc foil surface, promoting the reconstruction of the crystal structure on the zinc foil surface. After the holding period, the zinc foil was naturally cooled to room temperature under nitrogen atmosphere protection to obtain surface-reconstructed zinc foil, which is the ZU-X zinc anode material (ZU-300, ZU-400, ZU-500).

[0050] The ZU-X zinc anode material prepared in Example 1 was analyzed, and its specific characterization is as follows:

[0051] Figure 1Scanning electron microscope images of the ZU-X zinc anode material prepared in Example 1, where a is ZU-300, b is ZU-400, and c is ZU-500;

[0052] from Figure 1 It can be observed that different surface structures are formed on the zinc foil after heat treatment at different temperatures, indicating that heat treatment can cause interface reconstruction on the zinc foil surface. The changes are small for ZU-300, obvious crystal texture on the surface of ZU-400, and chaotic and complex surface of ZU-500.

[0053] Figure 2 The cross-section of the ZU-400 zinc anode material prepared in Example 1 shows the distribution of O and Zn elements.

[0054] from Figure 2 It can be observed that Zn is mainly distributed in the zinc foil matrix region, while O is mainly distributed in the zinc foil surface region, indicating that an oxygen-containing modified interface layer is formed on the zinc foil surface after heat treatment.

[0055] Figure 3 X-ray diffraction patterns of the ZU-X zinc anode material prepared in Example 1 and related standard cards;

[0056] from Figure 3 It can be observed that ZU-X at different temperatures exhibits characteristic diffraction peaks of Zn metal, and is mainly composed of Zn (002) crystal planes and Zn (004) and ZnO (101) with the same crystal orientation. This indicates that the present invention can regulate the crystal structure of the zinc foil surface through heat treatment and form a modified interface with a specific (002) crystal structure.

[0057] Application Examples:

[0058] The ZU-X zinc anode material prepared in Example 1 was applied to a zinc-ion battery. The specific steps are as follows:

[0059] Using the ZU-400 zinc anode material prepared in Example 1 as the zinc anode, a coin cell was assembled using a glass fiber separator and a 2M zinc sulfate solution as the electrolyte to test its electrochemical performance. Furthermore, a Zn||Zn symmetric cell was assembled using the ZU-X zinc anode material prepared in Example 1 with a 20μm thick zinc foil to test the deposition / stripping cycle stability of zinc; a Zn||Cu half-cell was assembled using the ZU-X zinc anode material with a 20μm thick copper foil to test the coulombic efficiency of zinc; and a Zn||MnO2 full cell was assembled using the ZU-400 zinc anode material with a commercially available manganese dioxide cathode to test its actual battery performance.

[0060] Figure 4To test the Zn||Zn symmetric cell assembled using the ZU-X zinc anode material prepared in Example 1 as the anode of a zinc-ion battery at 1 mA cm⁻¹ -2 Current density, 1mAh cm -2 Long-cycle charge-discharge data under isotope capacity conditions;

[0061] from Figure 4 As can be seen, the ZU-400 zinc anode maintains a stable zinc deposition / stripping process with a cycle time exceeding 3380 hours, while ZU-300, ZU-500, and bare Zn all fail within 500 hours. This indicates that the ZU-400 zinc anode material prepared in this invention possesses excellent long-term cycle stability.

[0062] Figure 5 When ZU-X prepared in Example 1 of this invention is used as the negative electrode material of a zinc-ion battery, the symmetric cell operates at 10 mA cm⁻¹. –2 Current density, 10mAh cm -2 Long-cycle charge-discharge data under isotope capacity conditions;

[0063] from Figure 5 As can be seen, the ZU-400 zinc anode maintains a stable zinc deposition / stripping process under high current density and high areal capacity conditions, with a cycle time exceeding 1000 hours, while ZU-300, ZU-500, and bare Zn all fail within 300 hours. This indicates that the ZU-400 zinc anode material prepared in this invention still exhibits good cycle stability under high current density conditions.

[0064] Figure 6 When ZU-X prepared in Example 1 of this invention is used as the negative electrode material of a zinc-ion battery, the Zn||Cu half-cell exhibits a performance of 1 mA cm⁻¹. –2 Graphs of coulombic efficiency data under current density and 1V cutoff conditions;

[0065] from Figure 6 As can be seen, the ZU-400 zinc anode can stably cycle for more than 1600 cycles while maintaining an average coulombic efficiency of 99.4%, while ZU-300, ZU-500, and bare Zn all fail within 300 cycles. This indicates that the ZU-400 prepared in this invention can improve the reversibility of the zinc deposition / stripping process.

[0066] Figure 7 When ZU-400 prepared in Example 1 of this invention is used as the negative electrode material of a zinc-ion battery, the Zn||MnO2 full cell at 1A g –1 Charging-discharging cycle data at current density;

[0067] from Figure 7As can be seen, the Zn||MnO2 full cell using ZU-400 as the negative electrode can cycle stably for more than 2000 times, indicating that the ZU-400 zinc negative electrode material prepared in this invention can effectively improve the long-term cycle stability of zinc-ion batteries and has good practical application performance.

[0068] In summary, the preparation method of this invention can form a stable modified interface on the zinc foil surface and regulate its surface structure, thereby improving the deposition / stripping behavior of zinc. When the ZU-400 zinc anode material is applied to zinc-ion batteries, it exhibits good cycle stability under different current densities and areal capacities, and can effectively improve the coulombic efficiency of Zn||Cu half-cells and the long-term cycle performance of Zn||MnO2 full cells.

[0069] The above description is merely a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the technical scope disclosed in the present invention, based on the technical solution and inventive concept of the present invention, should be covered within the scope of protection of the present invention.

Claims

1. A surface-reconstructed zinc foil, characterized in that, The surface-reconstructed zinc foil includes a metallic zinc foil substrate and a crystal structure reconstruction layer formed on the surface of the metallic zinc foil substrate through heat treatment; The crystal structure reconstruction layer has Zn(002) crystal plane as the main crystal orientation.

2. The method for preparing a surface-reconstructed zinc foil as described in claim 1, characterized in that, The preparation method described herein is specifically carried out according to the following steps:

1. The zinc foil is cleaned and dried to remove contaminants from its surface, resulting in pretreated zinc foil.

2. Place the pretreated zinc foil in a tube furnace, and then place urea upstream of the zinc foil; 3. Under nitrogen atmosphere protection, the tube furnace is heated from room temperature to 300℃~500℃ and held at that temperature to induce thermal diffusion and recrystallization on the zinc foil surface, promoting the reconstruction of the crystal structure on the zinc foil surface. After the holding period, the furnace is naturally cooled to room temperature to obtain the surface-reconstructed zinc foil.

3. The method for preparing a surface-reconstructed zinc foil according to claim 1, characterized in that, The zinc foil mentioned in step one is high-purity zinc foil with a mass fraction of 99.99% and a thickness of 20μm.

4. The method for preparing a surface-reconstructed zinc foil according to claim 1, characterized in that, In step one, the zinc foil is cleaned with anhydrous ethanol and deionized water in sequence, and then dried at 60°C for 6 hours.

5. The method for preparing a surface-reconstructed zinc foil according to claim 1, characterized in that, In step two, urea is placed 5 cm upstream of the zinc foil; the surface area of ​​the zinc foil to the mass ratio of the urea is 1.54 cm². 2 1g.

6. The method for preparing a surface-reconstructed zinc foil according to claim 1, characterized in that, The nitrogen gas used in steps two and three has a purity of not less than 99.9% and a flow rate of 100 mL / min. -1 .

7. The method for preparing a surface-reconstructed zinc foil according to claim 1, characterized in that, The heat preservation time mentioned in step two is 2 hours; the heating rate mentioned in step two is 2℃·min. -1 .

8. The application of a surface-reconstructed zinc foil as described in claim 1, characterized in that, A surface-reconstructed zinc foil is used directly as the negative electrode in an aqueous zinc-ion battery.

9. The application of a surface-reconstructed zinc foil according to claim 8, characterized in that, The aqueous zinc-ion battery includes a surface-reconstructed zinc foil, a positive electrode, a separator, and an aqueous electrolyte.

10. The application of a surface-reconstructed zinc foil according to claim 9, characterized in that, The positive electrode is manganese dioxide; the diaphragm is glass fiber; and the aqueous electrolyte is a 2 mol / L zinc sulfate solution.