A kind of water removal process of prussian blue positive electrode sheet
By combining negative pressure hot rolling and vacuum hot drying processes, the problems of incomplete water removal and material layer shrinkage in Prussian blue cathode sheets have been solved, achieving low water content, less shrinkage and high peeling force, thereby improving battery performance and reducing manufacturing costs.
Patent Information
- Application Number
- CN202510665459.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-22
- Publication Date
- 2026-11-24
AI Technical Summary
Existing drying methods for Prussian blue cathode sheets suffer from incomplete water removal, secondary water reabsorption, and material layer shrinkage, leading to decreased battery performance and increased manufacturing costs.
The process combines negative pressure hot rolling and vacuum hot drying. First, the material is initially dehydrated by negative pressure hot rolling, and then it is deeply dehydrated by vacuum hot drying. The negative pressure hot rolling conditions are 1~15 kPa and the rolling pressure is 10~60 MPa. The vacuum hot drying conditions are 0.01~1 kPa and 140~200℃, in order to reduce material layer shrinkage and improve peel strength.
This technology achieves low water content, minimal shrinkage, and high peel strength in Prussian blue cathode sheets, improving battery cycle capacity retention and cycle performance while reducing energy consumption and equipment usage time.
Abstract
Description
Technical Field
[0001] This invention relates to the field of battery electrode dehydration technology, and in particular to a dehydration process for Prussian blue positive electrode sheets. Background Technology
[0002] Prussian blue cathode materials possess advantages such as high capacity, low cost, and good conductivity, making them promising candidates for electrochemical energy storage. However, the high moisture content in Prussian blue cathode sheets can significantly impact battery performance. Therefore, the removal of moisture from Prussian blue cathode sheets has attracted considerable attention.
[0003] Based on the form in which water molecules exist, the water in Prussian blue cathode materials can be classified into coordinated water, interstitial water, and adsorbed water. Current technologies often use forced-air drying ovens and / or vacuum drying ovens under high temperature and long-term conditions to remove adsorbed, interstitial, and coordinated water from the cathode material. However, forced-air drying ovens and / or vacuum drying ovens have poor water removal efficiency and can lead to secondary water reabsorption.
[0004] In the prior art, for example, Chinese patent application publication number CN118016821 A discloses a baking method for Prussian blue cathode sheets. This method uses a stepped temperature baking process to bake the prepared Prussian blue cathode sheets to remove water, overcoming the problems of low baking efficiency and incomplete water removal. However, simply increasing the temperature to remove water from the cathode material can easily lead to shrinkage of the cathode material layer, reducing the peeling force of the cathode material layer.
[0005] In addition, since the drying temperature reaches the conditions for the removal of moisture from the material, the water is directly removed from the material without any other treatment, which can easily lead to the generation of gaps and defects in the Prussian blue cathode material layer. These gaps and defects can cause the problem of secondary reabsorption of moisture. Therefore, the cathode sheet dried by this patent method needs to provide assembly environment conditions with a lower dew point to avoid secondary reabsorption of moisture in the cathode material during the cell assembly process, which leads to a significant increase in the cell manufacturing cost.
[0006] In view of this, it is necessary to further improve the existing dehydration process for Prussian blue cathode materials to prevent the material layer shrinkage and secondary reabsorption problems that exist in the dehydration process of directly heating and dehydrating without other treatment. Summary of the Invention
[0007] To address the aforementioned technical problems, this invention provides a dehydration process for Prussian blue cathode sheets.
[0008] The specific technical solution of this invention is as follows: On one hand, the present invention provides a dehydration process for Prussian blue cathode sheets, comprising the following steps: Step S1: Apply negative pressure hot rolling to the coated Prussian blue positive electrode sheet; Step S2: Vacuum heat drying of the Prussian blue cathode sheet after negative pressure hot rolling; Wherein: the ambient pressure of the negative pressure hot roller is 1~15kPa and the roller pressure is 10~60MPa.
[0009] The aforementioned dehydration process occurs after the Prussian blue-based material coating. This invention adds a negative pressure hot rolling step to initially dehydrate the positive electrode sheet, followed by deep dehydration through vacuum thermal drying, ultimately achieving complete removal of moisture from the Prussian blue-based positive electrode sheet. The resulting Prussian blue-based positive electrode sheet, in addition to its low water content, also exhibits advantages such as minimal shrinkage of the positive electrode material layer and high peel strength.
[0010] Specifically, the advantage of the dehydration process of this invention stems from the negative pressure hot rolling process in step S1. During this stage, most of the adsorbed and interstitial water in the positive electrode sheet is removed, and the connections between different materials are strengthened, enhancing adhesion. In this stage, after the adsorbed and interstitial water are removed from the material structure, the crystal volume of the positive electrode material decreases. Under rolling conditions, the material contact state can be improved, mitigating the shrinkage and weakened material contact problems during subsequent deep dehydration.
[0011] Preferably, the ambient temperature of the negative pressure hot roller press is 100~150℃. The ambient temperature of the negative pressure hot roller press can be understood as the temperature inside the roller press and the roller body, that is, the working ambient temperature of the roller press.
[0012] The negative pressure hot rolling stage is carried out at a relatively low temperature range, 100~150℃. Excessively high temperatures cause moisture to be removed too quickly, and the compacting effect of the rolling process cannot quickly fill the gaps originally occupied by water molecules. This ultimately leads to gaps and defects in the positive electrode material layer, which can cause secondary moisture reabsorption. Lower temperatures result in low dehydration efficiency, leading to a higher moisture content in the positive electrode sheet during the subsequent vacuum heat drying process. Under vacuum and high temperature, a large number of water molecules are released from the positive electrode sheet, causing shrinkage of the positive electrode material layer and consequently, low peel strength.
[0013] Preferably, the duration of the negative pressure hot roller pressing is 10-15 meters per minute, measured by the electrode speed of the roller press.
[0014] Preferably, the ambient pressure for vacuum heat drying is 0.01~1 kPa.
[0015] Preferably, the ambient temperature for vacuum heat drying is 140~200℃.
[0016] Since most of the adsorbed and interstitial water in the positive electrode sheet has been removed during the negative pressure hot rolling stage, the temperature can be appropriately increased during the vacuum drying stage with minimal volume shrinkage. Increasing the temperature is beneficial for the removal of coordination water in Prussian blue-based materials.
[0017] Preferably, the vacuum heat drying process takes 4 to 12 hours.
[0018] The introduction of the negative pressure hot roller pressing stage can significantly reduce the dehydration time of the vacuum drying section and reduce the damage to the electrode structure caused by the high temperature of vacuum drying.
[0019] On the other hand, the present invention provides a sodium-ion battery, including a positive electrode and a negative electrode, wherein the preparation process of the positive electrode includes the above-mentioned dehydration process.
[0020] The Prussian blue cathode sheet obtained by the above-mentioned dehydration process of the present invention has the advantages of low water content, small shrinkage of cathode material layer and large peeling force. When used as the cathode of sodium-ion battery, the battery performance is excellent, specifically reflected in excellent cycle capacity retention and excellent cycle performance.
[0021] Compared with the prior art, the present invention has the following technical effects: (1) The present invention adds a negative pressure hot roller pressing step to preliminarily remove water from the positive electrode sheet, and then performs deep water removal through vacuum hot drying, so as to finally remove water from the Prussian blue positive electrode sheet. In addition to low water content, the Prussian blue positive electrode sheet obtained by water removal also has the advantages of small shrinkage of the positive electrode material layer and large peeling force.
[0022] (2) The water removal process provided by the present invention can significantly improve the water removal efficiency of Prussian blue cathode sheets and reduce energy consumption.
[0023] (3) The dehydration process provided by the present invention can reduce the usage time of vacuum drying equipment and reduce equipment investment. Detailed Implementation
[0024] The present invention will be further described below with reference to embodiments. Those skilled in the art will be able to implement the present invention based on these descriptions. Furthermore, the embodiments of the present invention described below are generally only some, not all, of the embodiments of the present invention. Therefore, all other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort should fall within the scope of protection of the present invention.
[0025] In this embodiment of the invention, the Prussian blue cathode slurry formulation is as follows: Prussian blue cathode powder: PVDF: conductive carbon = 90:5:5 (mass ratio).
[0026] Example 1 A dewatering process for Prussian blue cathode plates includes the following steps: (1) Prussian blue positive electrode slurry is coated on the current collector to obtain a positive electrode sheet. The positive electrode sheet is subjected to negative pressure hot rolling under the conditions of ambient pressure of 5 kPa, rolling temperature of 120℃ and rolling pressure of 30 MPa. The electrode sheet speed of the rolling press is 12 m / min.
[0027] (2) Place the positive electrode sheet in a vacuum device with a pressure of 0.5 kPa and a temperature of 180°C and vacuum dry for 8 hours.
[0028] Example 2 A dewatering process for Prussian blue cathode plates includes the following steps: (1) Prussian blue positive electrode slurry is coated on the current collector to obtain a positive electrode sheet. The positive electrode sheet is subjected to negative pressure hot rolling under the conditions of ambient pressure of 10 kPa, rolling temperature of 100℃ and rolling pressure of 10 MPa. The electrode sheet speed of the rolling press is 12 m / min.
[0029] (2) Place the positive electrode sheet in a vacuum device with a pressure of 1 kPa and a temperature of 140°C and vacuum dry for 4 hours.
[0030] Example 3 A dewatering process for Prussian blue cathode plates includes the following steps: (1) Prussian blue positive electrode slurry is coated on the current collector to obtain a positive electrode sheet. The positive electrode sheet is subjected to negative pressure hot rolling under the conditions of ambient pressure of 1 kPa, rolling temperature of 150℃ and rolling pressure of 50 MPa. The electrode sheet speed of the rolling press is 12 m / min.
[0031] (2) Place the positive electrode sheet in a vacuum device with a pressure of 0.1 kPa and a temperature of 200°C and vacuum dry for 12 hours.
[0032] Example 4 A dewatering process for Prussian blue cathode plates includes the following steps: (1) Prussian blue positive electrode slurry is coated on the current collector to obtain a positive electrode sheet. The positive electrode sheet is subjected to negative pressure hot rolling under the conditions of ambient pressure of 5 kPa, rolling temperature of 120℃ and rolling pressure of 10 MPa. The electrode sheet speed of the rolling press is 12 m / min.
[0033] (2) Place the positive electrode sheet in a vacuum device with a pressure of 0.5 kPa and a temperature of 180°C and vacuum dry for 8 hours.
[0034] Example 5 A dewatering process for Prussian blue cathode plates includes the following steps: (1) Prussian blue positive electrode slurry is coated on the current collector to obtain a positive electrode sheet. The positive electrode sheet is subjected to negative pressure hot rolling under the conditions of ambient pressure of 5 kPa, rolling temperature of 120℃ and rolling pressure of 50 MPa. The electrode sheet speed of the rolling press is 12 m / min.
[0035] (2) Place the positive electrode sheet in a vacuum device with a pressure of 0.5 kPa and a temperature of 180°C and vacuum dry for 8 hours.
[0036] Comparative Example 1 A dehydration process for a Prussian blue cathode sheet differs from that in Example 1 in that the environmental pressure in step (1) is 0.5 kPa. The other steps are the same as in Example 1.
[0037] Comparative Example 2 A dehydration process for a Prussian blue cathode sheet differs from that in Example 1 in that the environmental pressure in step (1) is 20 kPa. The other steps are the same as in Example 1.
[0038] Comparative Example 3 A dehydration process for a Prussian blue cathode sheet differs from that in Example 1 in that step (1) does not involve rolling. The other steps are the same as in Example 1.
[0039] This comparative example is conducted according to the following steps: (1) Prussian blue-based positive electrode slurry is coated on the current collector to obtain a positive electrode sheet. The positive electrode sheet is placed in a roller press and subjected to negative pressure heat treatment under an ambient pressure of 5 kPa and a temperature of 120°C. The roller press pressure is set to 0 MPa and the electrode sheet speed is set to 12 m / min to maintain the same processing time as step (1) of Example 1.
[0040] (2) Place the positive electrode sheet in a vacuum device with a pressure of 0.5 kPa and a temperature of 180°C and vacuum dry for 8 hours.
[0041] Comparative Example 4 A dehydration process for a Prussian blue cathode sheet differs from that in Example 1 in that the rolling pressure in step (1) is 5 MPa. The other steps are the same as in Example 1.
[0042] Comparative Example 5 A dehydration process for a Prussian blue cathode sheet differs from that in Example 1 in that the rolling pressure in step (1) is 70 MPa. The other steps are the same as in Example 1.
[0043] Comparative Example 6 A dehydration process for a Prussian blue cathode sheet differs from that in Example 1 in that the rolling temperature in step (1) is 90°C. The other steps are the same as in Example 1.
[0044] Comparative Example 7 A dehydration process for a Prussian blue cathode sheet differs from that in Example 1 in that the rolling temperature in step (1) is 180°C. The other steps are the same as in Example 1.
[0045] Performance Characterization After the dehydration processes of Examples 1 to 5 and Comparative Examples 1 to 7, the obtained positive electrode sheets were immediately tested for water content. Additionally, the positive electrode sheets obtained above were exposed to a -20°C dew point environment for 72 hours, and their water content was tested again. The water content was tested using the Karl Fischer method at 250°C. The results are shown in Table 1. Shrinkage rate refers to the rate of change in thickness of the electrode sheet after vacuum baking following negative pressure hot rolling. The test results are shown in Table 1.
[0046] Furthermore, the positive electrode obtained above was subjected to a peel strength test. The peel strength test method was as follows: the peel strength was quantitatively determined using the 180° peel method. The free end of the electrode was folded 180°, and the free end of the electrode and the test plate were clamped on the upper and lower clamps respectively. The electrode was continuously peeled using a tensile testing machine in the same environment until the electrode and the coating were completely separated. The peel strength value was directly read. The test results are shown in Table 1.
[0047] Table 1. Test results of electrode characteristics in the examples and comparative examples Group The water content of the electrode after dehydration is ppm Water content (ppm) after exposure to dew point at -20℃ for 72 hours Shrinkage rate % Peel force (N / m) Example 1 1200 3200 2.1% 25 Example 2 1800 3300 2.2% 22 Example 3 600 4000 1.8% 19 Example 4 1500 3000 2.4% 23 Example 5 1000 3400 1.9% 18 Comparative Example 1 900 3600 2.0% 15 Comparative Example 2 3500 3000 2.5% 12 Comparative Example 3 2500 4500 5.5% 5 Comparative Example 4 2200 4000 4.5% 10 Comparative Example 5 1000 3600 1.8% 12 Comparative Example 6 5000 3500 3.5% 8 Comparative Example 7 800 5000 2.0% 11 The data in Table 1 show that: Characterization data from Examples 1 to 5 show that the present invention performs preliminary dehydration of the positive electrode sheet by adding a negative pressure hot roller pressing step, and then performs deep dehydration by vacuum hot drying, ultimately achieving the removal of moisture from the Prussian blue positive electrode sheet. The Prussian blue positive electrode sheet obtained by this dehydration has the advantages of low water content, low reabsorption, low shrinkage rate, and high peeling force, and the secondary reabsorption of moisture is low.
[0048] Comparative analysis of Example 1 and Comparative Examples 1 and 2 shows that setting the environmental pressure of the negative pressure hot rolling process to 0.5 kPa and 20 kPa, respectively, in Comparative Examples 1 and 2 significantly reduced the peeling force. This indicates that the environmental pressure during the negative pressure hot rolling stage has a significant impact on the water removal performance of the positive electrode sheet.
[0049] Comparative analysis of Example 1 with Comparative Examples 3, 4, and 5 shows that when the rolling pressure of the negative pressure hot roller was set to 0 MPa, 5 MPa, and 70 MPa respectively in Comparative Examples 3 and 4, the shrinkage rate of the positive electrode sheet was significantly increased and the peeling force was significantly reduced. This indicates that no rolling or low rolling pressure results in low electrode sheet peeling force. The positive electrode sheet peeling force obtained in Comparative Example 5 was also low, indicating that excessive rolling pressure will actually decrease the electrode sheet peeling force.
[0050] Comparative analysis of Example 1 with Comparative Examples 6 and 7 shows that when the rolling temperatures of negative pressure hot rolling in Comparative Examples 6 and 7 were set to 90℃ and 180℃ respectively, the moisture content of Comparative Example 6 increased significantly, the shrinkage rate increased significantly, and the peel force decreased significantly. Comparative Example 7 showed a high reabsorption of moisture. The possible reasons for this are: during the negative pressure hot rolling stage, excessively high temperatures lead to excessive moisture removal, making the electrode more prone to reabsorption; if moisture is removed too quickly, the contact between materials within the electrode weakens, resulting in low peel force. Conversely, excessively low temperatures result in slow and insufficient moisture removal, failing to enhance the contact between materials within the electrode, leading to higher total moisture content and lower peel force.
[0051] Unless otherwise specified, the raw materials and equipment used in this invention are all commonly used in the field; unless otherwise specified, the methods used in this invention are all conventional methods in the field.
[0052] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Any simple modifications, alterations, and equivalent transformations made to the above embodiments based on the technical essence of the present invention shall still fall within the protection scope of the present invention.
Claims
1. A dewatering process for Prussian blue-based positive electrode sheets, characterized in that: Includes the following steps: Step S1: Apply negative pressure hot rolling to the coated Prussian blue positive electrode sheet; Step S2: Vacuum heat drying of the Prussian blue cathode sheet after negative pressure hot rolling; Wherein: the ambient pressure of the negative pressure hot roller is 1~15kPa and the roller pressure is 10~60MPa.
2. The dehydration process for a Prussian blue cathode as described in claim 1, characterized in that: The ambient temperature of the negative pressure hot roller is 100~150℃.
3. The dehydration process for a Prussian blue cathode as described in claim 1, characterized in that: The duration of the negative pressure hot roller pressing is measured by the electrode speed of the roller press, which is 10-15 meters per minute.
4. The dehydration process for a Prussian blue cathode as described in claim 1, characterized in that: The ambient pressure for vacuum heat drying is 0.01~1 kPa.
5. The dehydration process for a Prussian blue cathode as described in claim 1, characterized in that: The ambient temperature for vacuum heat drying is 140~200℃.
6. The dehydration process for a Prussian blue cathode as described in claim 1, characterized in that: The vacuum heat drying process takes 4 to 12 hours.
7. A Prussian blue-based positive electrode, characterized in that: The Prussian blue cathode sheet is obtained using any one of the dehydration processes described in claims 1-6.
8. A sodium-ion battery, characterized in that: Includes the Prussian blue cathode material as described in claim 7.
Citation Information
Patent Citations
Baking method of Prussian blue positive plate
CN118016821A