A sodium sub-primary battery anode and a preparation method thereof and a sodium sulfinyl chloride primary battery

By employing a multi-step evaporation pore-forming and three-dimensional network structure preparation method, the problem that existing porous carbon cathodes are not suitable for sodium thionyl chloride primary batteries has been solved, thereby improving the discharge performance and mechanical strength of sodium thionyl chloride primary batteries.

CN123162117APending Publication Date: 2026-11-24HCB BATTERY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611301093.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-26
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing porous carbon cathode materials are not suitable for sodium thionyl chloride primary batteries, resulting in insufficient discharge platform and discharge efficiency. It is necessary to develop carbon cathode materials that are more suitable for sodium thionyl chloride primary batteries.

Method used

A multi-step evaporation pore-forming method was adopted to prepare porous carbon cathodes with different particle sizes by evaporating different solvents and decomposing pore-forming agents, thereby increasing the proportion of large-pore size and enhancing mechanical strength and structural stability through a three-dimensional network structure.

Benefits of technology

It significantly improves the current load capacity and electrolyte penetration efficiency of sodium submersible primary batteries, and enhances the battery's discharge performance and mechanical strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123162117A_ABST
    Figure CN123162117A_ABST
Patent Text Reader

Abstract

This application provides a sodium thionyl chloride primary battery cathode and its preparation method, as well as a sodium thionyl chloride primary battery. The preparation method includes the following steps: mixing carbon material and an alcohol solvent to obtain a first slurry; mixing the first slurry with an aqueous solution of an inorganic pore-forming agent to obtain a second slurry; mixing a binder solution with the second slurry to obtain a wet material; pressing the wet material into a blank to obtain a green body; drying the green body and then heat-treating it to obtain the sodium thionyl chloride primary battery cathode, wherein the drying includes at least two stages of drying treatment. The preparation method of this application adopts a multi-step evaporation pore-forming approach. Through the evaporation of different solvents and the decomposition of the pore-forming agent, the resulting porous carbon cathode contains pores of different particle sizes and increases the proportion of large-diameter pores, making it suitable for the discharge of sodium thionyl chloride primary batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of sodium thionyl chloride primary battery technology, and relates to a sodium thionyl chloride primary battery positive electrode, its preparation method, and a sodium thionyl chloride primary battery. Background Technology

[0002] Lithium-thionyl chloride (LTC) batteries are primary lithium batteries that use thionyl chloride as the electrolyte solvent and cathode active material, and metallic lithium as the anode active material. Initially, LTC batteries were primarily used in the aerospace and military fields; later, with the maturation and development of manufacturing processes, they gradually found applications in the civilian sector. LTC batteries currently boast the highest energy density and widest operating temperature range among commercially available batteries. Today, LTC batteries are widely used in various smart meters such as electricity meters, water meters, and gas meters, and are also increasingly applied and developed in transportation, security, and the Internet of Things (IoT). With the expansion of applications, higher demands are being placed on the manufacturing cost of LTC batteries. Due to the rising costs of metallic lithium and lithium salt electrolytes, researchers are seeking alternatives to LTC batteries, such as sodium thionyl chloride (NSC) primary batteries.

[0003] Since sodium is far more abundant on Earth than lithium, and the cost of both metallic sodium and sodium salts is significantly lower than that of lithium metal and lithium salts, sodium thionyl chloride (NSCLC) primary batteries have a market application. In existing technologies, metallic sodium is modified to prepare composite sodium sheets, which facilitates the machining of metallic sodium and improves its long-term storage stability in dry environments. This makes the use of metallic sodium as the anode active material in the manufacture of NSCLC primary batteries a feasible process.

[0004] In comparison, lithium metal loses electrons more easily, and lithium is also lighter. Therefore, the voltage of a lithium thionyl chloride primary battery is 0.327V higher than that of a sodium thionyl chloride battery, and its energy density is also estimated to be more than 50% higher. To make sodium thionyl chloride primary batteries practically applicable, their discharge plateau and discharge efficiency must be improved, which places demands on the manufacturing of the positive electrode for sodium thionyl chloride primary batteries.

[0005] Porous carbon cathodes serve the same purpose in both lithium-ion and sodium-ion batteries, primarily utilizing their internal pores to adsorb and store the electrolyte. Simultaneously, the large specific surface area provided by these pores promotes catalytic reactions, and the products of the chemical reaction are stored within these pores. Therefore, porous carbon cathodes directly influence several key factors affecting the battery's discharge performance throughout its entire lifespan, including the chemical reaction rate, electrolyte adsorption and diffusion, and reaction product storage. The electrolyte solute in sodium thionyl chloride (NSC) primary batteries is sodium tetrachloroaluminate. Sodium ions act as charge carriers, resulting in an electrolyte viscosity higher than that of lithium-ion battery electrolytes. Furthermore, sodium ions are larger than lithium ions, and their reaction product, sodium chloride, is more likely to crystallize into large particles than lithium chloride. Therefore, the porous carbon cathodes commonly used in lithium-ion batteries are not well-suited for NSC primary batteries. To enable the practical application of NSC primary batteries, a more suitable method for preparing a carbon cathode is needed. Summary of the Invention

[0006] The purpose of this application is to provide a sodium thionyl chloride primary battery cathode and its preparation method, as well as a sodium thionyl chloride primary battery. The preparation method adopts a multi-step evaporation pore-forming approach, which creates pores by evaporating different solvents and decomposing pore-forming agents, resulting in a porous carbon cathode with pores of different particle sizes inside, and increasing the proportion of large-diameter pores, which is suitable for the discharge of sodium thionyl chloride primary batteries.

[0007] To achieve the purpose of this application, the following technical solution is adopted:

[0008] In a first aspect, this application provides a method for preparing a sodium sub-primary battery cathode, the method comprising the following steps:

[0009] (1) The carbon material and the alcohol solvent are mixed to obtain the first slurry;

[0010] (2) The first slurry from step (1) is mixed with an aqueous solution of an inorganic pore-forming agent to obtain a second slurry;

[0011] (3) Mix the adhesive solution with the second slurry from step (2) to obtain a wet material;

[0012] (4) Press the wet material described in step (3) to obtain a blank, dry the blank first, and then heat treat it to obtain the sodium submersible primary battery positive electrode;

[0013] The drying process in step (4) includes at least two drying stages.

[0014] This application considers the higher viscosity of sodium ion primary battery electrolytes and the larger radius of sodium ions compared to lithium ions, which places higher demands on the pore structure of the positive electrode and the wettability of the electrolyte. First, carbon materials and alcohol solvents are mixed, then with an aqueous solution of an inorganic pore-forming agent, and finally with a binder solution. This results in a wet mixture containing evaporable alcohol solvents and water, as well as decomposable inorganic pore-forming agents. During the multi-stage drying process, the alcohol solvents and water evaporate, leaving pores, while the inorganic pore-forming agents decompose, leaving pores as well. This results in pores of different particle sizes within the positive electrode of the sodium ion primary battery, increasing the proportion of large-pore size. Therefore, by controlling the multi-stage pore distribution, this application effectively reduces interfacial impedance and improves the electrolyte penetration efficiency within the positive electrode, thereby significantly improving the battery's current load capacity. Furthermore, the binder is fibrousized through heat treatment after drying, forming a three-dimensional network structure. The gas escape channels generated by the decomposition of the inorganic pore-forming agent and the network skeleton formed by the fiberization of the binder work synergistically to further enhance the mechanical strength and structural stability of the positive electrode material.

[0015] In some embodiments, the drying in step (4) includes a first drying, a second drying, and a third drying performed sequentially (the temperature of the third drying is ≥ the temperature of the second drying > the temperature of the first drying).

[0016] In some embodiments, the temperature of the first drying is 55°C to 65°C, for example, 55°C, 58°C, 60°C, 62°C or 65°C, and the time is 7h to 9h, for example, 7h, 7.5h, 8h, 8.5h or 9h, but not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0017] In some embodiments, the temperature of the second drying is 100°C to 115°C, for example, 100°C, 105°C, 110°C or 115°C, and the time is 3h to 5h, for example, 3h, 3.5h, 4h, 4.5h or 5h, but not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0018] In some embodiments, the temperature of the third drying is 115°C to 125°C, for example, 115°C, 118°C, 120°C, 122°C or 125°C, and the time is 1h to 3h, for example, 1h, 1.5h, 2h, 2.5h or 3h, but not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0019] This application first uses a low-temperature drying process at 55℃~65℃ to remove alcohol solvents, then raises the temperature to 100℃~115℃ to remove moisture and decompose the inorganic pore-forming agent, increasing porosity. Finally, it uses a drying process at 115℃~125℃ to completely volatilize the decomposition products. Therefore, this application forms multiple pores in the positive electrode through three-stage drying. If only one or two stages of drying are performed, such as skipping the first stage of low-temperature drying at 55℃~65℃ and proceeding directly to subsequent drying, the alcohol solvents may not be removed during the low-temperature drying, potentially causing alcohol solvent combustion and posing a safety risk. The second stage... Drying at 00℃~115℃ is to completely remove moisture. Simultaneously, this temperature causes ammonium acetate to decompose, generating gas and creating larger pores in the positive electrode. If the second drying stage is skipped and the process proceeds directly from the first to the third stage, the ammonium acetate, not having decomposed below 120℃, may produce byproducts that are difficult to remove, leading to impurities. Conversely, without the third drying stage at 115℃~125℃, the decomposition products of ammonium acetate cannot be completely removed and may remain in the positive electrode, affecting subsequent fiberization processes or even entering the battery as impurities that impact battery performance. Therefore, each of the three drying stages has an irreplaceable function. Furthermore, because different drying temperatures remove different solvents or generate different gases from the positive electrode, the resulting pore sizes also vary. This process results in a diverse pore size distribution in the positive electrode, which is beneficial for battery discharge performance.

[0020] In some embodiments, the temperature of the heat treatment in step (4) is 260°C to 280°C, for example, 260°C, 265°C, 270°C, 275°C or 280°C, and the time is 15 min to 30 min, for example, 15 min, 18 min, 20 min, 22 min, 25 min, 28 min or 30 min, but not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0021] In some embodiments, the pressing pressure in step (4) is 2kPa to 6kPa, for example, it can be 2kPa, 3kPa, 4kPa, 5kPa or 6kPa, and the holding time is 10s to 20s, for example, it can be 10s, 12s, 14s, 15s, 16s, 18s or 20s, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0022] In some embodiments, the carbon material in step (1) includes acetylene black, multi-walled carbon nanotubes, and conductive carbon black.

[0023] In some embodiments, the carbon material is obtained by stirring acetylene black, multi-walled carbon nanotubes, and conductive carbon black at a stirring rate of 120 r / min to 240 r / min (e.g., 120 r / min, 150 r / min, 200 r / min, or 240 r / min) for 30 min to 60 min (e.g., 30 min, 40 min, 50 min, or 60 min).

[0024] In some embodiments, in the carbon material of step (1), the mass percentage of acetylene black is 60wt% to 80wt%, for example, it can be 60wt%, 65wt%, 70wt%, 75wt% or 80wt%, the mass percentage of multi-walled carbon nanotubes is 2wt% to 5wt%, for example, it can be 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt%, 4.5wt% or 5wt%, and the mass percentage of conductive carbon black is 20wt% to 35wt%, for example, it can be 20wt%, 22wt%, 25wt%, 28wt%, 30wt%, 32wt% or 35wt%, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0025] In some embodiments, the specific surface area of ​​the acetylene black is 60 m². 2 / g~80m 2 / g, for example, could be 60m 2 / g、65m 2 / g、70m 2 / g、75m 2 / g or 80m 2 / g, the specific surface area of ​​multi-walled carbon nanotubes is 200m². 2 / g~300m 2 / g, for example, could be 200m 2 / g、220m 2 / g、250m 2 / g、280m 2 / g or 300m 2 / g, the specific surface area of ​​the conductive carbon black is 60m². 2 / g~80m 2 / g, for example, could be 60m 2 / g、65m 2 / g、70m 2 / g、75m 2 / g or 80m 2 / g, but not limited to the listed values, other unlisted values ​​within the range also apply.

[0026] In some embodiments, the stirring rate for mixing the carbon material and the alcohol solvent in step (1) is 120 r / min to 240 r / min, for example, it can be 120 r / min, 140 r / min, 160 r / min, 180 r / min, 200 r / min, 220 r / min or 240 r / min, and the stirring time is 10 min to 30 min, for example, it can be 10 min, 12 min, 15 min, 18 min, 20 min, 25 min or 30 min, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0027] In some embodiments, the mass of the alcohol solvent in step (1) is 2 to 3 times the mass of the carbon material, for example, it can be 2 times, 2.2 times, 2.5 times, 2.8 times or 3 times, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0028] In some embodiments, the alcohol solvent in step (1) includes isopropanol and / or anhydrous ethanol.

[0029] In some embodiments, the mass concentration of the inorganic pore-forming agent aqueous solution in step (2) is 2wt% to 5wt%, for example, it can be 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt%, 4.5wt% or 5wt%, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0030] In some embodiments, the inorganic pore-forming agent in the inorganic pore-forming agent aqueous solution in step (2) includes ammonium acetate (with a purity higher than 98%).

[0031] In some embodiments, the mass of the inorganic pore-forming agent aqueous solution in step (2) is 1 to 2 times the mass of the carbon material, for example, it can be 1, 1.2, 1.5, 1.8 or 2 times, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0032] The mass of the inorganic pore-forming agent aqueous solution relative to the carbon material affects the pore-forming effect, thereby affecting the porosity in the cathode. Preferably, the mass of the inorganic pore-forming agent aqueous solution is 1 to 2 times the mass of the carbon material. This ensures a suitable multi-level pore structure in the cathode while avoiding an excessive proportion of large-diameter pores in the cathode due to excessive inorganic pore-forming agent, which would lead to a decrease in the specific surface area of ​​the cathode, a decrease in the reduction reaction capacity of the catalyst during discharge, and a reduction in the discharge performance of the battery.

[0033] In some embodiments, the stirring rate for mixing the first slurry with the inorganic pore-forming agent aqueous solution in step (1) is 60 r / min to 180 r / min, for example, it can be 60 r / min, 80 r / min, 100 r / min, 120 r / min, 140 r / min, 160 r / min or 180 r / min, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0034] In some embodiments, the adhesive in the adhesive solution of step (3) includes polytetrafluoroethylene.

[0035] In some embodiments, the mass of the binder in the binder solution in step (3) is 5wt% to 10wt% of the mass of the carbon material, for example, it can be 5wt%, 6wt%, 7wt%, 8wt%, 9wt% or 10wt%, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0036] In some embodiments, the solid content of the adhesive solution in step (3) is 1wt% to 4wt%, for example, it can be 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, 3.5wt% or 4wt%, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0037] In some embodiments, the method for preparing the adhesive solution in step (3) includes adding deionized water to the adhesive emulsion for dilution to obtain the adhesive solution. The amount of deionized water added is 2.5 to 4.5 times the mass of the carbon material, for example, it can be 2.5 times, 3 times, 3.5 times, 4 times or 4.5 times, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0038] In some embodiments, the stirring rate for mixing the adhesive solution with the second slurry in step (2) is 60 r / min to 180 r / min, for example, 60 r / min, 80 r / min, 100 r / min, 120 r / min, 140 r / min, 160 r / min or 180 r / min, and the stirring time is 8 min to 15 min, for example, 8 min, 9 min, 10 min, 11 min, 12 min, 13 min, 14 min or 15 min, but not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0039] Secondly, this application provides a sodium sub-primary battery positive electrode, which is prepared by the preparation method described in the first aspect.

[0040] Thirdly, this application provides a sodium thionyl chloride primary battery, the sodium thionyl chloride primary battery comprising the sodium primary battery positive electrode as described in the second aspect.

[0041] In some embodiments, the sodium thionyl chloride primary battery includes a casing, a sodium metal negative electrode, a separator, a positive electrode core, and a positive electrode blank, wherein the positive electrode blank is the sodium thionyl chloride primary battery positive electrode as described in the second aspect.

[0042] The sodium metal negative electrode is located between the outer shell and the separator, the separator is located between the sodium metal negative electrode and the positive electrode blank, the positive electrode blank includes a reserved space, and the positive electrode core fills the reserved space in the positive electrode blank;

[0043] The cross-section of the positive electrode preform is flower-shaped, and there is a reserved space between the positive electrode preform and the separator.

[0044] The specially designed positive electrode preform structure of this application makes it easier for the electrolyte to flow inside the battery. The products generated during the discharge process will fill the inside of the positive electrode, causing the positive electrode volume to expand. The special reserved space provides a place for the positive electrode to expand, so that the gaps will not be blocked by the discharge products prematurely due to space constraints, thereby avoiding voltage drop and capacity decay caused by pore closure.

[0045] The positive electrode core described in this application is a metal current collector inserted into the positive electrode blank.

[0046] Compared with the prior art, this application has the following advantages:

[0047] This application first mixes carbon materials and alcohol solvents, then mixes them with an aqueous solution of an inorganic pore-forming agent, and finally mixes them with a binder solution. This results in a wet mixture containing evaporable alcohol solvents and water, as well as decomposable inorganic pore-forming agents. During drying, the alcohol solvents and water evaporate, leaving pores, while the inorganic pore-forming agent decomposes, leaving pores as well. This creates pores of varying particle sizes within the cathode of a sodium-ion battery, increasing the proportion of large-diameter pores. By controlling the multi-level pore distribution, interfacial impedance is effectively reduced, and the electrolyte permeation efficiency within the cathode is improved, thus significantly enhancing the battery's current load capacity. Furthermore, after drying, heat treatment causes the binder to become fibrous, forming a three-dimensional network structure. The gas escape channels generated by the decomposition of the inorganic pore-forming agent and the network skeleton formed by the fibrous binder work synergistically to further enhance the mechanical strength and structural stability of the cathode material. Attached Figure Description

[0048] Figure 1 This is a flowchart of the preparation method described in Example 1 of this application.

[0049] Figure 2 This is a cross-sectional schematic diagram of the sodium thionyl chloride primary battery described in this application.

[0050] Figure 3 The figures show the room temperature discharge curves of the battery prepared using the positive electrode obtained in Example 1 of this application and the battery prepared using the positive electrode obtained in Comparative Example 1.

[0051] Among them, 1-shell, 2-sodium metal negative electrode, 3-diaphragm, 4-reserved space, 5-positive electrode blank, 6-positive electrode core. Detailed Implementation

[0052] The technical solution of this application will be further described below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely to help understand this application and should not be regarded as specific limitations on this application.

[0053] Example 1

[0054] This embodiment provides a method for preparing a sodium sub-primary battery cathode, the flowchart of which is shown below. Figure 1 As shown, it includes the following steps:

[0055] (1) Acetylene black, multi-walled carbon nanotubes and conductive carbon black were stirred and mixed at a stirring speed of 180 r / min for 50 min to obtain carbon material. In the carbon material, the mass percentage of acetylene black was 65 wt%, the mass percentage of multi-walled carbon nanotubes was 5 wt%, and the mass percentage of conductive carbon black was 30 wt%.

[0056] The specific surface area of ​​the acetylene carbon black is 72 m². 2 / g, the specific surface area of ​​multi-walled carbon nanotubes is 215m². 2 / g, the specific surface area of ​​the conductive carbon black is 65m². 2 / g;

[0057] (2) The carbon material described in step (1) and isopropanol are stirred and mixed at a stirring rate of 180 r / min for 15 min to obtain the first slurry, wherein the mass of the isopropanol is 2.4 times the mass of the carbon material described in step (1);

[0058] (3) Dissolve ammonium acetate in deionized water and stir until homogeneous to prepare an ammonium acetate solution with a mass concentration of 3.03 wt%.

[0059] (4) Add the ammonium acetate solution from step (3) to the first slurry from step (2) and stir evenly at a stirring rate of 120 r / min to obtain the second slurry, wherein the amount of ammonium acetate solution added is 1.65 times the mass of the carbon material from step (1);

[0060] (5) Add deionized water to the polytetrafluoroethylene emulsion with a solid content of 60% to dilute it and obtain an adhesive solution. Mix the adhesive solution with the second slurry in step (4) at a stirring rate of 120 r / min for 10 min to obtain a wet material.

[0061] The mass of polytetrafluoroethylene solid added is 6% of the mass of the carbon material in step (1), and the amount of deionized water added during dilution is 3.6 times the mass of the carbon material in step (1).

[0062] (6) Place the wet material described in step (5) into the mold and hold it under pressure of 3 kPa for 16 seconds to obtain the blank;

[0063] (7) The blank obtained in step (6) is first dried at 60°C for 8 hours, then dried at 100°C for 4 hours, and then dried at 120°C for 2 hours to obtain the dried material;

[0064] (8) Heat-treat the dried material in step (7) at 275°C for 18 min to obtain the sodium sub-primary battery positive electrode.

[0065] Example 2

[0066] This embodiment provides a method for preparing a sodium sub-primary battery cathode, the method comprising the following steps:

[0067] (1) Acetylene black, multi-walled carbon nanotubes and conductive carbon black were stirred and mixed at a stirring speed of 240 r / min for 30 min to obtain carbon material. In the carbon material, the mass percentage of acetylene black was 78 wt%, the mass percentage of multi-walled carbon nanotubes was 2 wt%, and the mass percentage of conductive carbon black was 20 wt%.

[0068] The specific surface area of ​​the acetylene carbon black is 80 m². 2 / g, the specific surface area of ​​multi-walled carbon nanotubes is 200m². 2 / g, the specific surface area of ​​the conductive carbon black is 60m². 2 / g;

[0069] (2) The carbon material described in step (1) and isopropanol are stirred and mixed at a stirring rate of 120 r / min for 30 min to obtain the first slurry, wherein the mass of the isopropanol is 3 times the mass of the carbon material described in step (1);

[0070] (3) Dissolve ammonium acetate in deionized water, stir well, and prepare an ammonium acetate solution with a mass concentration of 2wt%;

[0071] (4) Add the ammonium acetate solution from step (3) to the first slurry from step (2) and stir evenly at a stirring rate of 180 r / min to obtain the second slurry, wherein the amount of ammonium acetate solution added is twice the mass of the carbon material from step (1);

[0072] (5) Add deionized water to the polytetrafluoroethylene emulsion with a solid content of 60% to dilute it and obtain an adhesive solution. Mix the adhesive solution with the second slurry in step (4) at a stirring rate of 180 r / min for 8 min to obtain a wet material.

[0073] The mass of polytetrafluoroethylene solid added is 10% of the mass of the carbon material in step (1), and the amount of deionized water added during dilution is 4.5 times the mass of the carbon material in step (1).

[0074] (6) Place the wet material described in step (5) into the mold and hold it under a pressure of 2 kPa for 20 seconds to obtain the blank;

[0075] (7) The blank obtained in step (6) is first dried at 55°C for 9 hours, then dried at 115°C for 3 hours, and then dried at 125°C for 1 hour to obtain the dried material;

[0076] (8) Heat-treat the dried material in step (7) at 260°C for 30 min to obtain the sodium sub-primary battery positive electrode.

[0077] Example 3

[0078] This embodiment provides a method for preparing a sodium sub-primary battery cathode, the method comprising the following steps:

[0079] (1) Acetylene black, multi-walled carbon nanotubes and conductive carbon black were stirred and mixed at a stirring speed of 120 r / min for 60 min to obtain carbon material. In the carbon material, the mass percentage of acetylene black was 70 wt%, the mass percentage of multi-walled carbon nanotubes was 4 wt%, and the mass percentage of conductive carbon black was 26 wt%.

[0080] The specific surface area of ​​the acetylene carbon black is 60 m². 2 / g, the specific surface area of ​​multi-walled carbon nanotubes is 300m². 2 / g, the specific surface area of ​​the conductive carbon black is 80m². 2 / g;

[0081] (2) The carbon material described in step (1) and isopropanol are stirred and mixed at a stirring rate of 240 r / min for 10 min to obtain the first slurry, wherein the mass of the isopropanol is twice the mass of the carbon material described in step (1);

[0082] (3) Dissolve ammonium acetate with a purity higher than 98% in deionized water, stir evenly, and prepare an ammonium acetate solution with a mass concentration of 5wt%.

[0083] (4) Add the ammonium acetate solution from step (3) to the first slurry from step (2) and stir evenly at a stirring rate of 60 r / min to obtain the second slurry, wherein the amount of ammonium acetate solution added is 1 times the mass of the carbon material from step (1);

[0084] (5) Add deionized water to the polytetrafluoroethylene emulsion with a solid content of 60% to dilute it and obtain an adhesive solution. Stir the adhesive solution and the second slurry in step (4) at a stirring rate of 60 r / min for 15 min to obtain a wet material.

[0085] The mass of polytetrafluoroethylene solid added is 5% of the mass of the carbon material in step (1), and the amount of deionized water added during dilution is 2.5 times the mass of the carbon material in step (1).

[0086] (6) Place the wet material described in step (5) into the mold and hold it under a pressure of 6 kPa for 10 seconds to obtain the blank;

[0087] (7) The blank obtained in step (6) is first dried at 65°C for 7 hours, then dried at 100°C for 5 hours, and then dried at 115°C for 3 hours to obtain the dried material;

[0088] (8) Heat-treat the dried material in step (7) at 280°C for 15 min to obtain the sodium sub-primary battery positive electrode.

[0089] Example 4

[0090] This embodiment provides a method for preparing a sodium sub-primary battery cathode. Except for step (4), in which the amount of ammonium acetate solution added is 0.5 times the mass of the carbon material in step (1), the preparation method is the same as in Example 1.

[0091] Example 5

[0092] This embodiment provides a method for preparing a sodium sub-basic battery cathode. The method is identical to that in Example 1, except that in step (4), the amount of ammonium acetate solution added is 2.5 times the mass of the carbon material in step (1).

[0093] Example 6

[0094] This embodiment provides a method for preparing a sodium sub-primary battery cathode. Except for step (7), in which the blank is first dried at 60°C for 8 hours and then dried at 105°C for 4 hours, the preparation method is the same as in Example 1.

[0095] Comparative Example 1

[0096] This comparative example provides a method for preparing a sodium sub-primary battery cathode, the method comprising the following steps:

[0097] (1) Acetylene black and conductive carbon black were stirred and mixed at a stirring speed of 180 r / min for 50 min to obtain carbon material, wherein the mass percentage of acetylene black in the carbon material was 85 wt% and the mass percentage of conductive carbon black was 15 wt%;

[0098] The specific surface area of ​​the acetylene carbon black is 72 m². 2 / g, the specific surface area of ​​the conductive carbon black is 65m². 2 / g;

[0099] (2) The carbon material described in step (1) and isopropanol are stirred and mixed at a stirring rate of 180 r / min for 15 min to obtain the first slurry, wherein the mass of the isopropanol is 2.4 times the mass of the carbon material described in step (1);

[0100] (3) Add deionized water to a polytetrafluoroethylene emulsion with a solid content of 60% to dilute it and obtain an adhesive solution. Mix the adhesive solution with the first slurry in step (2) at a stirring rate of 120 r / min for 10 min to obtain a wet material.

[0101] The mass of polytetrafluoroethylene solid added is 8% of the mass of the carbon material in step (1), and the amount of deionized water added during dilution is 4.8 times the mass of the carbon material in step (1).

[0102] (4) The wet material described in step (3) is placed into an extruder to form cylindrical strips with a diameter of 2 mm and a length of 5-15 mm;

[0103] (5) Place the cylindrical strips described in step (4) into a shot blasting machine, adjust the speed of the shot blasting machine to 180 r / min, blast for 60 s, then adjust the speed to 90 r / min, blast for 180 s, and obtain small balls with a diameter of 0.5-2.5 mm.

[0104] (6) The small balls described in step (5) are first dried at 60°C for 8 hours, and then dried at 120°C for 2 hours to obtain the dried material;

[0105] (8) Heat-treat the dried material described in step (7) at 265°C for 15 minutes to obtain the positive electrode of the battery.

[0106] Comparative Example 2

[0107] This comparative example provides a method for preparing a sodium sub-primary battery cathode. Except for step (7), in which the blank is dried at 120°C for 2 hours, the preparation method is the same as in Example 1.

[0108] Comparative Example 3

[0109] This comparative example provides a method for preparing a sodium sub-primary battery cathode. Except for step (7), in which the blank is dried at 100°C for 4 hours, the preparation method is the same as in Example 1.

[0110] The positive electrodes obtained in the above examples and comparative examples were used to prepare a NAER 14250 battery. Specifically, the positive electrode was assembled with metallic sodium and a separator, and an electrolyte prepared from thionyl chloride, sodium chloride, aluminum chloride, and sulfur dioxide was injected. The battery was then sealed. A cross-sectional schematic diagram of the prepared battery is shown below. Figure 2 As shown, it includes a shell 1, a sodium metal negative electrode 2, a separator 3, a positive electrode core 6, and a positive electrode blank 5. The positive electrode core 6 is the positive electrode obtained in the above embodiments and comparative examples. The sodium metal negative electrode 2 is located between the shell 1 and the separator 3. The separator 3 is located between the sodium metal negative electrode 2 and the positive electrode blank 5. The positive electrode blank 5 includes a reserved space 4, and the positive electrode core 6 fills the reserved space 4 in the positive electrode blank 5. The cross-section of the positive electrode blank 5 is flower-shaped, and there is a reserved space 4 between the positive electrode blank 5 and the separator 3.

[0111] The electrochemical performance of the batteries prepared above was tested using the following method: the battery was placed in a discharge device with dynamically adjustable discharge load, and the discharge current was kept constant at 5 ± 0.03 mA during the discharge process. The battery voltage was recorded during the discharge process, and the discharge was stopped when the voltage dropped to 2.0V. The discharge curve showing the change of discharge voltage with discharge time was obtained, and the discharge capacity was calculated. The median voltage when the battery was discharged to half capacity was read. The room temperature discharge curves of the batteries prepared using the positive electrode obtained in Example 1 of this application and the batteries prepared using the positive electrode obtained in Comparative Example 1 are shown below. Figure 3 It can be seen that, from Figure 3 It can be seen that the positive electrode prepared in Example 1 of this application has better discharge performance.

[0112] The electrochemical performance test results are shown in Table 1:

[0113] Table 1

[0114]

[0115] As can be seen from Table 1 above:

[0116] As can be seen from Examples 1-6 and Comparative Example 1, Comparative Example 1 is a method for preparing a mature lithium-ion battery cathode. The preparation method described in this application is more suitable for the discharge of sodium thionyl chloride batteries compared to the mature lithium-ion battery cathode. As can be seen from Examples 1, 6 and Comparative Examples 2-3, this application uses at least two-stage drying, preferably three-stage drying, to construct stable different pore structures, which is beneficial to improving the electrochemical performance of the battery. As can be seen from Examples 1 and 4-5, the amount of inorganic pore-forming agent aqueous solution added in this application affects the pore structure and stability in the cathode, preferably within a specific range.

[0117] The above description is only a specific embodiment of this application, but the protection scope of this application is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in this application fall within the protection and disclosure scope of this application.

Claims

1. A method for preparing a sodium-ion primary battery cathode, characterized in that, The preparation method includes the following steps: (1) The carbon material and the alcohol solvent are mixed to obtain the first slurry; (2) The first slurry from step (1) is mixed with an aqueous solution of an inorganic pore-forming agent to obtain a second slurry; (3) Mix the adhesive solution with the second slurry from step (2) to obtain a wet material; (4) Press the wet material described in step (3) to obtain a blank, dry the blank first, and then heat treat it to obtain the sodium submersible primary battery positive electrode; The drying process in step (4) includes at least two drying stages.

2. The preparation method according to claim 1, characterized in that, The drying process in step (4) includes a first drying, a second drying, and a third drying performed sequentially. The first drying temperature is 55℃~65℃, and the time is 7h~9h; The second drying temperature is 100℃~115℃, and the time is 3h~5h; The third drying process is carried out at a temperature of 115℃~125℃ for 1h~3h.

3. The preparation method according to claim 1 or 2, characterized in that, The heat treatment in step (4) is performed at a temperature of 260℃~280℃ for 15min~30min. And / or, the pressing pressure in step (4) is 2kPa~6kPa, and the holding time is 10s~20s.

4. The preparation method according to claim 1 or 2, characterized in that, The carbon materials mentioned in step (1) include acetylene black, multi-walled carbon nanotubes, and conductive carbon black; In the carbon material described in step (1), the mass percentage of acetylene black is 60wt%~80wt%, the mass percentage of multi-walled carbon nanotubes is 2wt%~5wt%, and the mass percentage of conductive carbon black is 20wt%~35wt%. The specific surface area of ​​the acetylene carbon black is 60 m². 2 / g~80m 2 / g, the specific surface area of ​​multi-walled carbon nanotubes is 200m². 2 / g~300m 2 / g, the specific surface area of ​​the conductive carbon black is 60m². 2 / g~80m 2 / g.

5. The preparation method according to claim 1 or 2, characterized in that, In step (1), the stirring rate for mixing the carbon material and the alcohol solvent is 120 r / min to 240 r / min, and the stirring time is 10 min to 30 min. And / or, the mass of the alcohol solvent in step (1) is 2 to 3 times the mass of the carbon material; And / or, the alcohol solvent in step (1) includes isopropanol and / or anhydrous ethanol.

6. The preparation method according to claim 1 or 2, characterized in that, The mass concentration of the inorganic pore-forming agent aqueous solution in step (2) is 2wt%~5wt%; And / or, the inorganic pore-forming agent in the inorganic pore-forming agent aqueous solution in step (2) includes ammonium acetate; And / or, the mass of the inorganic pore-forming agent aqueous solution in step (2) is 1 to 2 times the mass of the carbon material.

7. The preparation method according to claim 1 or 2, characterized in that, The adhesive in the adhesive solution of step (3) includes polytetrafluoroethylene; And / or, the mass of the binder in the binder solution in step (3) is 5wt%~10wt% of the mass of the carbon material; And / or, the solid content of the adhesive solution in step (3) is 1wt%~4wt%; And / or, the method for preparing the adhesive solution in step (3) includes adding deionized water to the adhesive emulsion for dilution to obtain the adhesive solution, wherein the amount of deionized water added is 2.5 to 4.5 times the mass of the carbon material.

8. A sodium-ion primary battery positive electrode, characterized in that, The sodium submersible primary battery cathode is prepared by the preparation method according to any one of claims 1-7.

9. A sodium thionyl chloride primary battery, characterized in that, The sodium thionyl chloride primary battery includes the sodium thionyl chloride primary battery positive electrode as described in claim 8.

10. The sodium thionyl chloride primary battery according to claim 9, characterized in that, The sodium thionyl chloride primary battery includes a casing, a sodium metal negative electrode, a separator, a positive electrode core, and a positive electrode blank, wherein the positive electrode blank is the sodium thionyl chloride primary battery positive electrode as described in claim 8; The sodium metal negative electrode is located between the outer shell and the separator, the separator is located between the sodium metal negative electrode and the positive electrode blank, the positive electrode blank includes a reserved space, and the positive electrode core fills the reserved space in the positive electrode blank; The cross-section of the positive electrode preform is flower-shaped, and there is a reserved space between the positive electrode preform and the separator.