A preparation method of a carbon-coated aluminum foil current collector applied to a negative electrode-free sodium battery

By using a layered coating method with aqueous sodium alginate and ammonium bicarbonate pore-forming agent, combined with electrochemical etching of micro-pit arrays, an all-inorganic carbon-coated aluminum foil current collector was prepared. This solved the fatigue fracture problem caused by organic binders in carbon-coated aluminum foil current collectors in negative electrode-free sodium-ion batteries, achieving efficient absorption of dynamic stress and long-cycle stability.

CN123162121APending Publication Date: 2026-11-24FOSHAN DAWEI TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611449062.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-17
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

In existing technologies, carbon-coated aluminum foil current collectors in negative electrode sodium-ion batteries suffer from fatigue fracture and creep problems due to reliance on organic elastic binders. This cannot effectively absorb the dynamic stress of repeated deposition/peeling of metallic sodium, leading to the termination of battery cycle life. Furthermore, existing industrial alternatives are difficult to achieve.

Method used

Aqueous sodium alginate was used as a temporary binder. A gradient distribution of all-inorganic carbon coating was constructed by layering differentiated ammonium bicarbonate pore-forming agents. A strong interfacial bond between the coating and aluminum foil was achieved by electrochemical etching of a micro-pit array and mechanical interlocking with the carbon matrix, replacing organic elastic binders.

Benefits of technology

This technology enables inorganic carbon coatings to absorb dynamic stress while maintaining structural flexibility, avoiding the swelling, deterioration, and fatigue fracture of organic binders. It also improves the bonding strength between the coating and aluminum foil, enhances the long-cycle stability of the battery, and reduces raw material costs and environmental risks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

This application discloses a method for preparing carbon-coated aluminum foil current collectors for use in sodium-ion batteries without negative electrodes, relating to the field of current collector material preparation technology for sodium-ion batteries. The method includes: ultrasonically cleaning the aluminum foil followed by constant-current anodic etching with phosphoric acid solution to form a micro-pit array; preparing a slurry using sodium alginate aqueous solution, and adding ammonium bicarbonate as a pore-forming agent to prepare a bottom layer slurry and a top layer slurry; coating the bottom layer slurry onto the etched aluminum foil surface, pre-drying it to a semi-solid state, and then coating it with the top layer slurry; heating to decompose ammonium bicarbonate to create pores and then drying; performing a three-stage carbonization treatment under inert gas protection to convert sodium alginate into an amorphous carbon matrix; acid washing to remove sodium salts generated in situ during carbonization; and finally, light roll forming. This method obtains a fully inorganic carbon coating with a porosity gradient distribution along the thickness direction, absorbing the dynamic stress of repeated sodium deposition / peeling through structural flexibility, and achieving a strong bond between the coating and the aluminum foil through the mechanical interlocking of the micro-pit array and the carbon matrix.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of current collector material preparation technology for sodium-ion batteries, specifically a method for preparing a gradient porous carbon-coated aluminum foil current collector for use in negative electrode-free sodium-ion batteries. Background Technology

[0002] Electrodeless sodium-ion batteries do not have metallic sodium pre-placed on the negative electrode side during assembly. During the first charge, sodium ions are released from the positive electrode and directly deposited as metallic sodium on the surface of the negative electrode current collector. During discharge, the metallic sodium dissolves out and returns to the positive electrode, exhibiting the potential for high energy density and low cost. In this operating mode, the carbon coating on the surface of the negative electrode current collector directly bears the periodic dynamic volume change stress generated by the repeated deposition / peeling of metallic sodium. Whether the carbon coating can maintain its structural integrity and firmly bond with the aluminum foil during long-term cycling directly determines the cycle life of the electrodeless sodium-ion battery.

[0003] In the prior art, the preparation of carbon-coated aluminum foil current collectors generally adopts the process route of preparing a slurry with an elastic polymer binder (such as PVDF-HFP) in NMP organic solvent and then coating it on the surface of aluminum foil. Representative technical solutions include the conductive carbon black / carbon nanotube hybrid coating solution disclosed in CN102832392A and the thin-layer conductive coating solution disclosed in CN113451546B.

[0004] The mechanism by which the above scheme absorbs dynamic stress essentially relies on the chemical elasticity of the organic binder itself. The binder exists permanently in the coating in the form of an organic polymer. The coating has a uniform structure in the thickness direction. The bond between the coating and the aluminum foil depends entirely on the physical adsorption of the binder on the smooth foil surface.

[0005] However, organic binders inevitably swell and deteriorate under long-term immersion in electrolyte, leading to fatigue fracture and creep under cyclic stress. Their elastic absorption capacity continuously decreases with increasing cycle count. Once the binder performance deteriorates, the coating-aluminum foil interface, maintained solely by physical adsorption, rapidly fails, causing the coating to peel off and ending the battery's cycle life. Although the PECVD ultrathin carbon coating method reported in the literature can obtain binder-free carbon coatings, it requires expensive vacuum and plasma equipment, and the process of large-area uniform coating is difficult to scale up, making it unsuitable as an industrial alternative.

[0006] Therefore, the core technical problem that urgently needs to be solved in this field is: how to get rid of the dependence on organic elastic binders and their material elastic stress absorption mechanism, and to prepare carbon-coated aluminum foil current collectors that rely on the coating structure itself to absorb the dynamic stress of repeated deposition / peeling of metallic sodium and form a strong interface bond with aluminum foil, so as to ensure the long-cycle stability of negative electrode sodium-ion batteries. Summary of the Invention

[0007] To address the aforementioned technical problems, this application provides a method for preparing a carbon-coated aluminum foil current collector for use in sodium-free negative electrode current collectors. The technical concept is as follows: water-based sodium alginate is used as a temporary binder instead of an organic elastic binder and is carbonized into an amorphous carbon matrix. A fully inorganic carbon coating with a gradient porosity along the thickness direction is constructed by layering and coating with ammonium bicarbonate pore-forming agents of varying contents. The coating relies on structural flexibility rather than the elasticity of the binder material to absorb the dynamic stress caused by repeated deposition / peeling of metallic sodium. A strong interfacial bond between the coating and the aluminum foil is achieved through the mechanical interlocking of the micro-pit array etched on the aluminum foil surface and the carbon matrix.

[0008] The preparation method includes the following steps: Step (1) Aluminum foil pretreatment: The aluminum foil is ultrasonically cleaned sequentially in acetone and anhydrous ethanol, dried at 40-60℃, and then placed in a 1-10wt% phosphoric acid solution with the aluminum foil as the anode and the inert electrode as the cathode, at a current density of 5-50mA / cm. 2 The aluminum foil is etched under constant current for 10-120 seconds to form a micro-pit array on the surface. After etching, it is rinsed with deionized water until neutral and dried at 40-60℃ for later use. Step (2) Preparation of sodium alginate solution: Add sodium alginate powder to deionized water and stir at 200-600 rpm for 30-120 min at 20-30℃ to prepare a sodium alginate aqueous solution with a mass concentration of 1-5wt%. Step (3) Carbon slurry preparation: Add conductive carbon material to deionized water and disperse it at high speed of 3000-10000 rpm for 10-30 min. Add the sodium alginate aqueous solution obtained in step (2) and mix and stir at 500-1500 rpm for 20-60 min. Then add ammonium bicarbonate powder at 0-15℃ and stir rapidly at 500-1500 rpm for 10-30 min. Perform low-temperature vacuum degassing to prepare bottom slurry and surface slurry respectively. The mass ratio of conductive carbon material to sodium alginate is (5-15):1. Based on the sum of the mass of conductive carbon material and sodium alginate as 100 parts by mass, the amount of ammonium bicarbonate added in the bottom slurry is 5-25 parts by mass, and the amount of ammonium bicarbonate added in the surface slurry is 30-70 parts by mass. Step (4) Layered coating: The bottom layer slurry is coated onto the surface of the aluminum foil treated in step (1) using a doctor blade coating method to form a bottom layer wet film. After pre-drying at 25-35℃ for 5-20 minutes until the surface of the bottom layer wet film is semi-solid, the top layer slurry is then coated onto the bottom layer using a doctor blade coating method to form a top layer wet film. Step (5) Decomposition and drying of pore-forming agent: Place the coated aluminum foil in a ventilated oven and raise the temperature from room temperature to 50-70℃ at a rate of 0.5-2℃ / min and keep it at that temperature for 30-90min to completely decompose the ammonium bicarbonate. Then continue to raise the temperature to 80-120℃ and keep it at that temperature for 30-60min until the coating is completely dry. Step (6) Step-by-step carbonization: Place the dried carbon-coated aluminum foil in a tube furnace and perform a three-stage carbonization process at a heating rate of 1-5℃ / min under the protection of high-purity inert gas: the first stage is to heat to 200-300℃ and hold for 30-90min, the second stage is to heat to 350-500℃ and hold for 30-120min, and the third stage is to heat to 550-640℃ and hold for 30-120min; after carbonization, cool the furnace to room temperature under an inert atmosphere. Step (7) Pickling and drying: Immerse the carbonized and cooled aluminum foil in a hydrochloric acid solution with a concentration of 0.1-1 mol / L, pickle at 20-40℃ for 10-60 min, take it out and rinse with deionized water until the washing solution is neutral, and then vacuum dry at 60-80℃ for 2-8 h. Step (8) Roll forming: The dried carbon-coated aluminum foil is lightly rolled and formed with a rolling pressure of 0.5-5 N / mm.

[0009] Preferably, the thickness of the aluminum foil in step (1) is 10-30 μm; the specific operation of the ultrasonic cleaning is as follows: first, immerse the aluminum foil in acetone and clean it with an ultrasonic power of 100-300W for 5-15 minutes, then take it out and immerse it in anhydrous ethanol and clean it with an ultrasonic power of 100-300W for 5-15 minutes.

[0010] Preferably, the phosphoric acid solution in step (1) has a mass concentration of 2-5 wt% and an etching current density of 10-30 mA / cm². 2 The etching time is 30-90 seconds, and the temperature of the phosphoric acid solution is controlled at 20-35℃ during the etching process.

[0011] Preferably, the sodium alginate aqueous solution in step (2) has a mass concentration of 2-4 wt%, a stirring speed of 300-500 rpm, and a stirring time of 45-90 min.

[0012] Preferably, the conductive carbon material in step (3) is selected from nano-sized conductive carbon black, carbon nanotubes, or a mixture of nano-sized conductive carbon black and carbon nanotubes; when the conductive carbon material is a mixture of nano-sized conductive carbon black and carbon nanotubes, the mass ratio of nano-sized conductive carbon black to carbon nanotubes is (3-9):1; the mass ratio of the conductive carbon material to sodium alginate is (7-12):1.

[0013] Preferably, in step (3), based on a total mass of 100 parts by mass of conductive carbon material and sodium alginate, the amount of ammonium bicarbonate added to the bottom slurry is 8-18 parts by mass, and the amount of ammonium bicarbonate added to the surface slurry is 35-55 parts by mass; the slurry temperature is controlled at 0-10℃ during the addition and stirring of ammonium bicarbonate.

[0014] Preferably, in step (4), the gap between the blade coating of the bottom wet film is 30-80 μm, and the gap between the blade coating of the top wet film is 50-120 μm; the pre-drying temperature is 28-33℃, and the pre-drying time is 8-15 min.

[0015] Preferably, in step (5), the holding temperature during the ammonium bicarbonate decomposition stage is 55-65℃ and the holding time is 45-75min; the temperature during the complete drying stage is 90-110℃ and the drying time is 35-50min; and the heating rate is 0.8-1.5℃ / min.

[0016] Preferably, the high-purity inert gas in step (6) is high-purity argon or high-purity nitrogen, with a gas flow rate of 50-200 mL / min; a heating rate of 1-3℃ / min; a first-stage temperature of 220-280℃ and a holding time of 45-75 min; a second-stage temperature of 380-450℃ and a holding time of 45-90 min; and a third-stage temperature of 580-640℃ and a holding time of 45-90 min.

[0017] Preferably, the concentration of the hydrochloric acid solution in step (7) is 0.2-0.5 mol / L, the pickling temperature is 25-35℃, the pickling time is 15-40 min, the vacuum drying temperature is 65-75℃, and the vacuum drying time is 3-6 h.

[0018] In the above preparation method, sodium alginate acts as an aqueous temporary binder in the slurry and wet film stages to maintain the film-forming properties and interlayer bonding of the coating. During the stepped heating carbonization process, the first stage (200-300℃) dehydrates sodium alginate and initially crosslinks and shapes it; the second stage (350-500℃) is the main pyrolysis and weight loss stage of sodium alginate, where pyrolysis gas escapes smoothly through the macroporous channels reserved by the decomposition of ammonium bicarbonate, avoiding bubbling and cracking of the coating; the third stage (550-640℃) further condenses the carbon skeleton, improving the conductivity and structural strength of the coating. During the carbonization process, the sodium element in sodium alginate is converted in situ into sodium salt, mainly sodium carbonate, and dispersed in the carbon matrix. The hydrochloric acid washing in step (7) dissolves and removes the sodium salt, leaving additional micropores in the carbon matrix. The sodium salt thus acts as a pore-forming template, which is also the way to realize the pore-forming template function in the triple function of sodium alginate temporary binder → carbon source → pore-forming template.

[0019] It should be noted that the upper limit of the carbonization temperature in the third stage is set at 640℃ because the solidus temperature of battery-grade aluminum foil (purity ≥99.3%) is approximately 644-646℃. Maintaining a safety margin between the upper limit of the carbonization temperature and the solidus temperature can prevent the aluminum foil from undergoing initial melting at grain boundaries and high-temperature softening instability. During the carbonization process, the temperature control accuracy of the tube furnace should ensure that the actual temperature inside the furnace does not exceed the set temperature by 3℃. That is, when operating at the upper limit of 640℃, the actual temperature inside the furnace should not exceed 643℃, which is still lower than the lower limit of the solidus temperature. In addition, during the pickling process, the uncoated surface of the aluminum foil is directly exposed to the hydrochloric acid solution. It is advisable to operate at a lower hydrochloric acid concentration and a shorter pickling time, or to apply a protective film to the uncoated surface to avoid over-corrosion of the aluminum substrate.

[0020] In summary, the preparation method of this application has the following beneficial technical effects: 1. Sodium alginate can completely replace special elastic polymer binders (such as PVDF-HFP). Sodium alginate is abundant, inexpensive, and has good batch stability, which significantly reduces raw material costs and incoming material testing costs.

[0021] 2. The entire process uses an aqueous system, completely replacing NMP organic solvent with deionized water, eliminating occupational health risks and environmental emissions from organic solvents at the source, saving investment and operating costs for solvent recovery equipment, and reducing drying energy consumption.

[0022] 3. By layering and coating a slurry with a differentiated ammonium bicarbonate content and then carbonizing it, a carbon coating with a porosity gradient distribution along the thickness direction is obtained (a dense layer near the aluminum foil and a loose layer away from the aluminum foil). This allows the coating to physically absorb the dynamic stress generated by repeated deposition / peeling of metallic sodium through structural flexibility, and this structural function does not decrease with the increase of the number of cycles.

[0023] 4. Electrochemical micro-etching creates a micro-pit array on the aluminum foil surface. After carbonization, the carbon matrix fills the micro-pits to form a mechanically interlocked interface bond. The coating peel strength is significantly higher than that of existing methods that rely on physical adsorption of adhesives, and there is no polymer creep failure problem.

[0024] 5. Sodium alginate is carbonized into an amorphous carbon matrix. Sodium salts such as sodium carbonate generated in situ from sodium elements in sodium alginate during the carbonization process are removed by acid washing in step (7) and additional micropores are left in the carbon matrix. The final product is an all-inorganic carbon coating system that does not contain organic polymer components, thus eliminating the risk of swelling and deterioration of organic binders and fatigue fracture under electrolyte immersion.

[0025] 6. The continuous carbon skeleton formed by carbonization provides a continuous pathway for electron conduction throughout the coating thickness direction. The coating resistance is lower than that of traditional carbon coatings containing organic binders, which helps to reduce the nucleation overpotential of sodium deposition and promote uniform deposition.

[0026] 7. Sodium alginate achieves a triple functional transformation from temporary binder to carbon source to pore-forming template throughout the entire process, while ammonium bicarbonate realizes a functional chain from pore-forming agent to macropore channel to pyrolysis gas channel, demonstrating a highly efficient design that uses one material for multiple purposes.

[0027] 8. All equipment required for the entire process (electrochemical etching tank, blade coating machine, ventilated drying oven, tubular carbonization furnace, pickling tank) are mature industrial equipment. The viscosity control window of the water-based slurry is wide, which is conducive to the uniform control of large-area coating and has good industrialization feasibility. Detailed Implementation

[0028] The present application will be further described in detail below with reference to specific embodiments. The following embodiments are for illustrative purposes only and do not constitute a limitation on the scope of protection of the present application.

[0029] Raw material description The raw materials used in all embodiments of this application are commercially available products, specifically as follows: the aluminum foil is battery-grade aluminum foil (purity ≥99.3%); acetone and anhydrous ethanol are both analytical grade; phosphoric acid is analytical grade, diluted with deionized water to the required concentration before use; sodium alginate is food-grade or industrial-grade, with a viscosity grade of 200-500 mPa·s (1% aqueous solution, 25℃); and nano-sized conductive carbon black is SuperP or equivalent (particle size 30-50 nm, BET specific surface area ≥60 m²). 2 / g); the carbon nanotubes are multi-walled carbon nanotubes (outer diameter 8-15nm, length 5-15μm); ammonium bicarbonate is analytical grade (particle size passed through a 100-mesh sieve); hydrochloric acid is analytical grade and should be diluted with deionized water to the required concentration before use; high-purity argon and high-purity nitrogen have a purity ≥99.999%; the resistivity of deionized water is ≥18MΩ·cm. The inert electrodes are graphite plates or platinum sheets.

[0030] Example 1 Step (1) Aluminum foil pretreatment: Cut 20μm thick aluminum foil to 5cm×10cm, immerse it in acetone and clean it with 200W ultrasonic power for 10min, then immerse it in anhydrous ethanol and clean it with 200W ultrasonic power for 10min, and dry it at 50℃ for 30min. Use the cleaned aluminum foil as the anode and the graphite plate as the cathode, immerse it in a 3wt% phosphoric acid solution at 25℃, and apply a current density of 20mA / cm. 2 Constant current anodic etching for 60 seconds. After etching, remove the aluminum foil, rinse it 5 times with deionized water until the washing solution is neutral, and dry it at 50°C for 30 minutes for later use.

[0031] Step (2) Preparation of sodium alginate solution: Weigh 1.50g of sodium alginate powder and add it to 48.50g of deionized water. Stir continuously at 400rpm for 60min at 25℃ to obtain 50.00g of homogeneous and transparent sodium alginate aqueous solution with a mass concentration of 3wt%.

[0032] Step (3) Preparation of carbon slurry: Bottom slurry: Weigh 4.38g of conductive carbon black and 0.62g of carbon nanotubes (mass ratio 7:1, total 5.00g) and add them to 25.00g of deionized water. Disperse the mixture at 6000rpm for 20min. Add 16.67g of sodium alginate aqueous solution obtained in step (2) (containing 0.50g of sodium alginate, with a mass ratio of conductive carbon material to sodium alginate of 10:1). Mix and stir at 1000rpm for 40min. Cool the slurry to 5℃ and add 0.66g of ammonium bicarbonate powder (based on 100 parts by mass of the sum of conductive carbon material and sodium alginate 5.50g, ammonium bicarbonate is 12 parts by mass). Stir rapidly at 1000rpm for 20min and then degas under vacuum at 5℃ for 15min.

[0033] Surface slurry: Prepare carbon suspension and mix using the same method as the bottom slurry (5.00g conductive carbon material, 25.00g deionized water, 16.67g sodium alginate aqueous solution). After cooling to 5°C, add 2.48g ammonium bicarbonate powder (45 parts by weight), stir rapidly at 1000rpm for 20min, and degas under vacuum at 5°C for 15min.

[0034] Step (4) Layered coating: Apply the bottom layer slurry to the aluminum foil surface treated in step (1) with a doctor blade gap of 50 μm, and pre-dry at 30°C for 10 min until the bottom layer surface is semi-solid. Then apply the top layer slurry on top of the bottom layer with a doctor blade gap of 80 μm.

[0035] Step (5) Decomposition and drying of pore-forming agent: Place the coated aluminum foil in a ventilated oven and heat it from room temperature to 60°C at a rate of 1°C / min and keep it at that temperature for 60 min to completely decompose the ammonium bicarbonate. Then continue to heat it to 100°C at a rate of 1°C / min and keep it at that temperature for 45 min until the coating is completely dry.

[0036] Step (6) Stepwise carbonization: Transfer the dried carbon-coated aluminum foil to a tube furnace, introduce high-purity argon gas (flow rate 100 mL / min), and perform a three-stage carbonization process at a heating rate of 2℃ / min: the first stage is to heat to 250℃ and hold for 60 min, the second stage is to heat to 420℃ and hold for 60 min, and the third stage is to heat to 600℃ and hold for 60 min. After carbonization, cool the furnace to room temperature under an argon atmosphere.

[0037] Step (7) Pickling and drying: Immerse the carbonized and cooled aluminum foil in a 0.3 mol / L hydrochloric acid solution and pickle at 30°C for 30 min. After taking it out, rinse it with deionized water until the washing solution is neutral and then vacuum dry it at 70°C for 4 h.

[0038] Step (8) Roll forming: The dried carbon-coated aluminum foil is lightly rolled and shaped with a rolling pressure of 2 N / mm. It is then cut to the battery design dimensions to obtain the carbon-coated aluminum foil current collector.

[0039] Example 2 Step (1) Aluminum foil pretreatment: Cut 10μm thick aluminum foil to 5cm×10cm, first immerse it in acetone and clean it with 100W ultrasonic power for 5min, then immerse it in anhydrous ethanol and clean it with 100W ultrasonic power for 5min, and dry it at 40℃ for 30min. Using aluminum foil as the anode and graphite plate as the cathode, immerse it in 1wt% phosphoric acid solution (solution temperature 20℃) at 5mA / cm 2 Constant current anodic etching for 10 seconds. After etching, rinse with deionized water until neutral, and dry at 40°C for 30 minutes.

[0040] Step (2) Preparation of sodium alginate solution: Weigh 2.50g of sodium alginate and add it to 247.50g of deionized water. Stir at 200rpm for 30min at 20℃ to obtain 250.00g of 1wt% sodium alginate aqueous solution.

[0041] Step (3) Preparation of carbon slurry: Bottom slurry: Weigh 5.00g of conductive carbon black and add it to 25.00g of deionized water. Disperse the carbon material at 3000rpm for 10min. Add 100.00g of sodium alginate aqueous solution (containing 1.00g of sodium alginate, with a carbon material to sodium alginate mass ratio of 5:1). Mix and stir at 500rpm for 20min. Cool to 0℃ (ice bath). Add 0.30g of ammonium bicarbonate (5 parts by mass). Stir at 500rpm for 10min. Degas under vacuum at 0℃ for 10min.

[0042] Surface slurry: Prepared in the same way (5.00g conductive carbon black, 25.00g deionized water, 100.00g sodium alginate aqueous solution), cooled to 0℃, then added 1.80g ammonium bicarbonate (30 parts by weight), stirred at 500rpm for 10min, and vacuum degassed at 0℃ for 10min.

[0043] Step (4) Layered coating: Apply the bottom layer slurry with a doctor blade gap of 30 μm, pre-dry at 25°C for 5 min to semi-solid, and apply the top layer slurry with a doctor blade gap of 50 μm.

[0044] Step (5) Decomposition and drying of pore-forming agent: Heat to 50℃ at 0.5℃ / min and keep warm for 30min, then continue to heat to 80℃ and keep warm for 30min.

[0045] Step (6) Stepwise heating carbonization: High-purity argon gas (flow rate 50 mL / min) is introduced into the tube furnace, and the temperature is increased at 1℃ / min: the first stage is held at 200℃ for 30 min, the second stage is held at 350℃ for 30 min, and the third stage is held at 550℃ for 30 min. The furnace is then cooled to room temperature.

[0046] Step (7) Pickling and drying: Immerse in 0.1 mol / L hydrochloric acid, pickle at 20°C for 10 min, wash with water until neutral, and vacuum dry at 60°C for 2 h.

[0047] Step (8) Roll forming: Roll forming line pressure 0.5N / mm. Cut to obtain the product.

[0048] Example 3 Step (1) Aluminum foil pretreatment: Take an aluminum foil with a thickness of 30 μm, first clean it in acetone with 300 W ultrasonication for 15 min, then clean it in anhydrous ethanol with 300 W ultrasonication for 15 min, and dry it at 60℃ for 30 min. Immerse the aluminum foil as the anode in a 10 wt% phosphoric acid solution (solution temperature 35℃), and apply an ultrasonic wave at 50 mA / cm². 2 Constant current etching for 120 seconds. Rinse with water until neutral, then dry at 60°C for 30 minutes.

[0049] Step (2) Weigh 5.00g of sodium alginate and add it to 95.00g of deionized water. Stir at 600rpm for 120min at 30℃ to obtain 100.00g of 5wt% sodium alginate aqueous solution.

[0050] Step (3) Bottom layer slurry: Weigh 5.00g of carbon nanotubes and add them to 25.00g of deionized water, and disperse them by shearing at 10000rpm for 30min; add 6.67g of sodium alginate aqueous solution (containing 0.33g of sodium alginate, with a carbon material to sodium alginate mass ratio of 15:1), and mix and stir at 1500rpm for 60min; cool to 15℃, add 1.33g of ammonium bicarbonate (25 parts by mass), stir at 1500rpm for 30min, and degas under vacuum at 15℃ for 15min. Surface layer slurry: Prepare the carbon suspension and mix using the same method, cool to 15℃, add 3.73g of ammonium bicarbonate (70 parts by mass), stir at 1500rpm for 30min, and degas under vacuum for 15min.

[0051] Step (4) Coat the bottom layer with a blade gap of 80 μm, pre-dry at 35°C for 20 min to semi-solid, and coat the top layer with a blade gap of 120 μm.

[0052] Step (5) Heat to 70℃ at 2℃ / min and hold for 90min, then continue heating to 120℃ and hold for 60min.

[0053] Step (6) High-purity nitrogen gas (flow rate 200 mL / min) is introduced into the tubular furnace, and the temperature is increased at 5℃ / min: the first stage is held at 300℃ for 90 min, the second stage is held at 500℃ for 120 min, and the third stage is held at 640℃ for 120 min. The furnace is then cooled.

[0054] Step (7) Immerse in 1 mol / L hydrochloric acid, acid wash at 40°C for 60 min, wash with water until neutral, and vacuum dry at 80°C for 8 h.

[0055] Step (8) Roller pressure 5 N / mm. Cut to obtain the product.

[0056] Example 4 Step (1) Take a 15μm thick aluminum foil, clean it with acetone at 150W for 8 min, then clean it with anhydrous ethanol at 150W for 8 min, and dry it at 45℃ for 30 min. Immerse the aluminum foil as the anode in a 2wt% phosphoric acid solution (solution temperature 22℃), and so on at 10mA / cm 2 Etch at constant current for 30 seconds. Rinse with water until neutral, then dry at 45°C for 30 minutes.

[0057] Step (2) Weigh 2.00g of sodium alginate and add it to 98.00g of deionized water. Stir at 300rpm for 45min at 22℃ to obtain 100.00g of 2wt% sodium alginate aqueous solution.

[0058] Step (3) Bottom layer slurry: Weigh 3.75g of conductive carbon black and 1.25g of carbon nanotubes (mass ratio 3:1, total 5.00g) and add them to 25.00g of deionized water. Shear and disperse at 5000rpm for 15min. Add 35.71g of sodium alginate aqueous solution (containing 0.71g of sodium alginate, carbon material to sodium alginate mass ratio 7:1) and mix and stir at 800rpm for 30min. Cool to 5℃, add 0.46g of ammonium bicarbonate (8 parts by mass), stir at 800rpm for 15min, and vacuum degas at 5℃ for 10min. Surface layer slurry: Prepared in the same way and cooled to 5℃, add 2.00g of ammonium bicarbonate (35 parts by mass), stir at 800rpm for 15min, and vacuum degas for 10min.

[0059] Step (4) Coat the bottom layer with a doctor blade gap of 40 μm, pre-dry at 28°C for 8 min to semi-solid, and coat the top layer with a doctor blade gap of 60 μm.

[0060] Step (5) Heat to 55℃ at 0.8℃ / min and hold for 45 min, then continue heating to 90℃ and hold for 35 min.

[0061] Step (6) High-purity argon gas (flow rate 50 mL / min) is introduced into the tubular furnace, and the temperature is increased at 1℃ / min: the first stage is held at 220℃ for 45 min, the second stage is held at 380℃ for 45 min, and the third stage is held at 580℃ for 45 min. The furnace is then cooled.

[0062] Step (7) Immerse in 0.2 mol / L hydrochloric acid, acid wash at 25°C for 15 min, wash with water until neutral, and vacuum dry at 65°C for 3 h.

[0063] Step (8) Roller pressing pressure 1N / mm. Cut to obtain the product.

[0064] Example 5 Step (1) Take a 25μm thick aluminum foil, clean it with acetone at 250W for 12 min, then clean it with anhydrous ethanol at 250W for 12 min, and dry it at 55℃ for 30 min. Immerse the aluminum foil as the anode in a 5wt% phosphoric acid solution (solution temperature 35℃), and apply an ultrasonic pulse at 30mA / cm. 2 Constant current etching for 90 seconds. Rinse with water until neutral, then dry at 55°C for 30 minutes.

[0065] Step (2) Weigh 1.00g of sodium alginate and add it to 24.00g of deionized water. Stir at 500rpm for 90min at 28℃ to obtain 25.00g of 4wt% sodium alginate aqueous solution.

[0066] Step (3) Bottom layer slurry: Weigh 4.50g of conductive carbon black and 0.50g of carbon nanotubes (mass ratio 9:1, total 5.00g) and add them to 25.00g of deionized water. Shear and disperse at 8000rpm for 25min. Add 10.42g of sodium alginate aqueous solution (containing 0.42g of sodium alginate, carbon material to sodium alginate mass ratio 12:1) and mix and stir at 1200rpm for 50min. Cool to 10℃, add 0.98g of ammonium bicarbonate (18 parts by mass), stir at 1200rpm for 25min, and vacuum degas at 10℃ for 15min. Surface layer slurry: Prepared in the same way and cooled to 10℃, add 2.98g of ammonium bicarbonate (55 parts by mass), stir at 1200rpm for 25min, and vacuum degas for 15min.

[0067] Step (4) Coat the bottom layer with a blade gap of 70 μm, pre-dry at 33°C for 15 min to semi-solid, and coat the top layer with a blade gap of 100 μm.

[0068] Step (5) Increase the temperature to 65℃ at 1.5℃ / min and hold for 75min, then continue to increase the temperature to 110℃ and hold for 50min.

[0069] Step (6) High-purity nitrogen gas (flow rate 200 mL / min) is introduced into the tubular furnace, and the temperature is increased at 3℃ / min: the first stage is held at 280℃ for 75 min, the second stage is held at 450℃ for 90 min, and the third stage is held at 640℃ for 90 min. The furnace is then cooled.

[0070] Step (7) Immerse in 0.5 mol / L hydrochloric acid, acid wash at 35°C for 40 min, wash with water until neutral, and vacuum dry at 75°C for 6 h.

[0071] Step (8) Roller pressure 3N / mm. Cut to obtain the product.

[0072] Example 6 Step (1) Take a 20μm thick aluminum foil, and clean it with 200W ultrasonication in acetone and anhydrous ethanol for 10 min each, then dry it at 50℃ for 30 min. Immerse the aluminum foil as the anode in a 4wt% phosphoric acid solution (solution temperature 28℃) at 15mA / cm 2 Etch at constant current for 45 seconds. Rinse with water until neutral, then dry at 50°C for 30 minutes.

[0073] Step (2) Weigh 1.50g of sodium alginate and add it to 58.50g of deionized water. Stir at 350rpm for 50min at 24℃ to obtain 60.00g of 2.5wt% sodium alginate aqueous solution.

[0074] Step (3) Bottom layer slurry: Weigh 5.00g of conductive carbon black and add it to 25.00g of deionized water, and shear and disperse at 5000rpm for 15min; add 25.00g of sodium alginate aqueous solution (containing 0.63g of sodium alginate, with a carbon material to sodium alginate mass ratio of 8:1), and mix and stir at 800rpm for 30min; cool to 5℃, add 0.56g of ammonium bicarbonate (10 parts by mass), stir at 800rpm for 15min, and vacuum degas at 5℃ for 10min. Surface layer slurry: Prepared in the same way and cooled to 5℃, add 2.25g of ammonium bicarbonate (40 parts by mass), stir at 800rpm for 15min, and vacuum degas for 10min.

[0075] Step (4) Coat the bottom layer with a doctor blade gap of 45 μm, pre-dry at 28°C for 10 min to semi-solid, and coat the top layer with a doctor blade gap of 75 μm.

[0076] Step (5) Increase the temperature to 58℃ at 1℃ / min and hold for 50min, then continue to increase the temperature to 95℃ and hold for 40min.

[0077] Step (6) High-purity argon gas (flow rate 100 mL / min) is introduced into the tubular furnace, and the temperature is increased at 2℃ / min: the first stage is held at 240℃ for 50 min, the second stage is held at 400℃ for 60 min, and the third stage is held at 610℃ for 70 min. The furnace is then cooled.

[0078] Step (7) Immerse in 0.3 mol / L hydrochloric acid, acid wash at 28°C for 25 min, wash with water until neutral, and vacuum dry at 68°C for 4 h.

[0079] Step (8) Roller pressure 1.5 N / mm. Cut to obtain the product.

[0080] Example 7 Step (1) Take a 20μm thick aluminum foil and clean it with 200W ultrasonication in acetone and anhydrous ethanol for 10 min each, then dry it at 50℃ for 30 min. Immerse the aluminum foil as the anode in a 6wt% phosphoric acid solution (solution temperature 30℃) at 25mA / cm 2 Etch at constant current for 75 seconds. Rinse with water until neutral, then dry at 50°C for 30 minutes.

[0081] Step (2) Weigh 3.50g of sodium alginate and add it to 96.50g of deionized water. Stir at 450rpm for 75min at 26℃ to obtain 100.00g of 3.5wt% sodium alginate aqueous solution.

[0082] Step (3) Bottom layer slurry: Weigh 5.00g of carbon nanotubes and add them to 25.00g of deionized water, and shear and disperse at 7000rpm for 20min; add 15.88g of sodium alginate aqueous solution (containing 0.56g of sodium alginate, with a carbon material to sodium alginate mass ratio of 9:1), and mix and stir at 1000rpm for 40min; cool to 8℃, add 0.83g of ammonium bicarbonate (15 parts by mass), stir at 1000rpm for 20min, and degas under vacuum at 8℃ for 15min. Surface layer slurry: Prepared in the same way and cooled to 8℃, add 2.78g of ammonium bicarbonate (50 parts by mass), stir at 1000rpm for 20min, and degas under vacuum for 15min.

[0083] Step (4) Coat the bottom layer with a doctor blade gap of 60 μm, pre-dry at 30°C for 12 min to semi-solid, and coat the top layer with a doctor blade gap of 90 μm.

[0084] Step (5) Increase the temperature to 62℃ at 1.2℃ / min and hold for 60min, then continue to increase the temperature to 105℃ and hold for 45min.

[0085] Step (6) High-purity nitrogen gas (flow rate 120 mL / min) is introduced into the tubular furnace, and the temperature is increased at 2℃ / min: the first stage is held at 260℃ for 55 min, the second stage is held at 430℃ for 70 min, and the third stage is held at 620℃ for 80 min. The furnace is then cooled.

[0086] Step (7) Immerse in 0.4 mol / L hydrochloric acid, acid wash at 30°C for 35 min, wash with water until neutral, and vacuum dry at 72°C for 5 h.

[0087] Step (8) Roller pressure 2N / mm. Cut to obtain the product.

[0088] Example 8 Step (1) Take a 12μm thick aluminum foil and clean it with 150W ultrasonic in acetone and anhydrous ethanol for 8 min each, then dry it at 45℃ for 30 min. Immerse the aluminum foil as the anode in a 2wt% phosphoric acid solution (solution temperature 22℃) at 8mA / cm 2 Etch at constant current for 50 seconds. Rinse with water until neutral, then dry at 45°C for 30 minutes.

[0089] Step (2) Weigh 2.00g of sodium alginate and add it to 131.33g of deionized water. Stir at 250rpm for 80min at 22℃ to obtain 133.33g of 1.5wt% sodium alginate aqueous solution.

[0090] Step (3) Bottom layer slurry: Weigh 4.17g of conductive carbon black and 0.83g of carbon nanotubes (mass ratio 5:1, total 5.00g) and add them to 25.00g of deionized water. Shear and disperse at 4000rpm for 15min. Add 55.56g of sodium alginate aqueous solution (containing 0.83g of sodium alginate, carbon material to sodium alginate mass ratio 6:1) and mix and stir at 700rpm for 35min. Cool to 3℃, add 0.41g of ammonium bicarbonate (7 parts by mass), stir at 700rpm for 15min, and vacuum degas at 3℃ for 10min. Surface layer slurry: Prepared in the same way and cooled to 3℃, add 1.87g of ammonium bicarbonate (32 parts by mass), stir at 700rpm for 15min, and vacuum degas for 10min.

[0091] Step (4) Coat the bottom layer with a doctor blade gap of 35 μm, pre-dry at 27°C for 8 min to semi-solid, and coat the top layer with a doctor blade gap of 55 μm.

[0092] Step (5) Heat to 55℃ at 0.8℃ / min and hold for 50 min, then continue heating to 85℃ and hold for 35 min.

[0093] Step (6): High-purity argon gas (flow rate 80 mL / min) is introduced into the tubular furnace, and the temperature is increased at 1.5℃ / min: the first stage is held at 230℃ for 65 min, the second stage is held at 390℃ for 75 min, and the third stage is held at 590℃ for 75 min. The furnace is then cooled.

[0094] Step (7) Immerse in 0.2 mol / L hydrochloric acid, acid wash at 25°C for 20 min, wash with water until neutral, and vacuum dry at 65°C for 3 h.

[0095] Step (8) Roller pressing pressure 1N / mm. Cut to obtain the product.

[0096] Example 9 Step (1) Take an 18μm thick aluminum foil, and clean it with 250W ultrasonic in acetone and anhydrous ethanol for 12 min each, then dry it at 55℃ for 30 min. Immerse the aluminum foil as the anode in an 8wt% phosphoric acid solution (solution temperature 32℃), and apply an ultrasonic pulse at 40mA / cm. 2 Etch at constant current for 100 seconds. Rinse with water until neutral, then dry at 55°C for 30 minutes.

[0097] Step (2) Weigh 4.50g of sodium alginate and add it to 95.50g of deionized water. Stir at 550rpm for 100min at 28℃ to obtain 100.00g of 4.5wt% sodium alginate aqueous solution.

[0098] Step (3) Bottom layer slurry: Weigh 4.44g of conductive carbon black and 0.56g of carbon nanotubes (mass ratio 8:1, total 5.00g) and add them to 25.00g of deionized water. Shear and disperse at 9000rpm for 25min. Add 7.94g of sodium alginate aqueous solution (containing 0.36g of sodium alginate, carbon material to sodium alginate mass ratio 14:1) and mix and stir at 1300rpm for 50min. Cool to 12℃, add 1.18g of ammonium bicarbonate (22 parts by mass), stir at 1300rpm for 25min, and vacuum degas at 12℃ for 15min. Surface layer slurry: Prepared in the same way and cooled to 12℃, add 3.48g of ammonium bicarbonate (65 parts by mass), stir at 1300rpm for 25min, and vacuum degas for 15min.

[0099] Step (4) Coat the bottom layer with a blade gap of 75 μm, pre-dry at 33°C for 15 min to semi-solid, and coat the top layer with a blade gap of 110 μm.

[0100] Step (5) Heat to 68℃ at 1.8℃ / min and hold for 80 min, then continue heating to 115℃ and hold for 55 min.

[0101] Step (6) High-purity nitrogen gas (flow rate 180 mL / min) is introduced into the tubular furnace, and the temperature is increased at 4℃ / min: the first stage is held at 290℃ for 40 min, the second stage is held at 480℃ for 100 min, and the third stage is held at 640℃ for 100 min. The furnace is then cooled.

[0102] Step (7) Immerse in 0.8 mol / L hydrochloric acid, acid wash at 38°C for 50 min, wash with water until neutral, and vacuum dry at 78°C for 7 h.

[0103] Step (8) Roller pressure 4N / mm. Cut to obtain the product.

[0104] Comparative Example 1 (without electrochemical etching step) The process conditions and formulation amounts of this comparative example are exactly the same as those of Example 1. The only difference is that the electrochemical etching operation is omitted in step (1). That is, the aluminum foil is directly dried after ultrasonic cleaning with acetone and anhydrous ethanol (without anodic etching), and the surface of the aluminum foil remains in its original smooth state. All operating parameters and raw material amounts in subsequent steps (2) to (8) are the same as those in Example 1.

[0105] Comparative Example 2 (coating with no gradient structure, i.e. uniform porosity) The process conditions and aluminum foil pretreatment of this comparative example are exactly the same as those of Example 1 (including the electrochemical etching step). The only difference is that in step (3), the bottom slurry and the top slurry use the same amount of ammonium bicarbonate, which is 28 parts by weight (the middle value between 12 parts by weight for the bottom layer and 45 parts by weight for the top layer in Example 1). Specifically, 1.54 g of ammonium bicarbonate is added to both the bottom slurry and the top slurry. The type and amount of carbon material, the amount of sodium alginate, and all operating parameters in steps (4) to (8) are the same as those in Example 1.

[0106] Comparative Example 3 (Traditional PVDF-HFP / NMP system, i.e., without carbonization treatment) This comparative example uses a traditional elastic polymer binder and organic solvent system to prepare carbon-coated aluminum foil, without electrochemical etching or carbonization. The specific procedures are as follows: Aluminum foil pretreatment: Take a 20μm thick aluminum foil, clean it with 200W ultrasonic in acetone and anhydrous ethanol for 10 min each, and dry it at 50℃ for 30 min (without electrochemical etching).

[0107] Slurry preparation: Weigh 0.63g of PVDF-HFP and dissolve it in 9.37g of NMP (PVDF-HFP concentration 6.3wt%). Stir at 500rpm for 120min at 50℃ until completely dissolved. Separately, add 4.38g of conductive carbon black and 0.62g of carbon nanotubes (mass ratio 7:1, total 5.00g) to 8.00g of NMP and disperse at 6000rpm for 20min using high-speed shearing. Mix the PVDF-HFP solution with the carbon dispersion and stir at 1000rpm for 60min. Degas under vacuum at room temperature for 30min.

[0108] Coating and drying: The slurry was uniformly coated onto the surface of the aluminum foil with a doctor blade gap of 80 μm (single-layer coating, not multi-layer coating), and vacuum dried at 120℃ for 2 h.

[0109] Roll forming: Roll forming line pressure 10N / mm. Cutting to obtain the product.

[0110] This comparative example does not involve ammonium bicarbonate pore-forming, carbonization, or acid washing steps; the PVDF-HFP in the coating exists permanently in the form of an organic polymer.

[0111] Performance testing methods: The following performance tests were performed on the carbon-coated aluminum foil current collectors prepared in Examples 1-9 and Comparative Examples 1-3: (1) Coating peel strength test: The 180° peel method was used. Standard 3M tape (25mm wide) was pasted on the coating surface and peeled at a rate of 50mm / min at 180°. The average peel force during the stable peeling stage was recorded and converted into peel strength per unit width (N / m). Each sample was tested 3 times and the average value was taken.

[0112] (2) Coating Resistance Test: The coating resistance of the carbon-coated aluminum foil through the thickness direction was measured using the DC voltage drop method. The carbon-coated aluminum foil was cut into 14mm diameter circular pieces and placed between two gold-plated planar electrodes. A 10mA DC current was applied under a constant pressure of 1.0MPa, and the voltage drop between the two electrodes was measured. After subtracting the background resistance of the blank fixture, the coating resistance per unit area (mΩ·cm) was calculated. 2 The coating resistance comprehensively reflects both the bulk resistance of the carbon coating and the interfacial contact resistance between the coating and the aluminum foil. Five parallel samples were tested for each sample, and the average value was taken.

[0113] (3) Half-cell coulombic efficiency and cycle stability tests: CR2032 coin cells were assembled in an argon glove box using 12mm diameter discs of carbon-coated aluminum foil as the working electrode and sodium metal sheets as the counter and reference electrodes. The electrolyte was 1 mol / L NaPF6 dissolved in EC:DEC (1:1, volume ratio) with 5 vol% FEC added. Test conditions: 1 mA / cm². 2 A current density of 1 mAh / cm² was deposited on the working electrode. 2 Sodium metal was then stripped at the same current density until the voltage reached 1.0V (cutoff). The coulombic efficiency was the ratio of the stripping capacity to the deposition capacity in that cycle. The coulombic efficiency of the first cycle and the average coulombic efficiency of the first 50 cycles were recorded. Considering that the coulombic efficiency was low in the first few cycles due to the consumption of active sodium by SEI film formation, the cycle life criterion was calculated from the 10th cycle onwards: the cycle life was defined as the number of cycles when the coulombic efficiency dropped below 99.0% for three consecutive cycles, and the number of cycles was recorded.

[0114] (4) Cross-sectional morphology observation: Cut the carbon-coated aluminum foil along the cross-sectional direction and observe the coating cross-section using a scanning electron microscope (SEM) to confirm the porosity difference between the bottom of the coating (the side closer to the aluminum foil) and the top of the coating (the side farther from the aluminum foil).

[0115] (5) Coating integrity check after long cycle: After 300 charge-discharge cycles, the battery was disassembled (in an argon glove box), and the surface condition of the carbon-coated aluminum foil was observed using SEM and optical microscope. The coating was recorded to see if peeling, cracking or delamination occurred.

[0116] The performance test results are shown in Table 1 below: Table 1: Performance Test Results Based on the above data, the analysis is as follows: (1) Overall performance of Examples 1-9 Examples 1-9 successfully prepared all-inorganic carbonaceous coated aluminum foil current collectors with a gradient porous structure. Cross-sectional SEM images of all examples confirmed a gradient porosity distribution characterized by a dense bottom and a loose top in the coating. All coatings remained intact after 300 cycles, without peeling or debonding. Peel strength ranged from 35-55 N / m, and coating resistivity ranged from 10-22 mΩ·cm. 2 The first-cycle coulomb efficiency ranges from 98.1% to 99.3%, the average coulomb efficiency for the first 50 cycles ranges from 99.35% to 99.78%, and the cycle life ranges from 250 to 460 cycles.

[0117] Among them, Example 4 (using the preferred process parameter range) has the best overall performance, with a peel strength of 55 N / m and a coating resistance of 10 mΩ·cm. 2 The first-cycle coulombic efficiency was 99.3%, and the cycle life was 460 cycles. Example 1 (intermediate parameters) showed good performance. Example 2 (lower limit parameters) had relatively lower peel strength and cycle life due to lower etching strength and lower carbonization temperature, but still met the usage requirements.

[0118] (2) Effect of Comparative Example 1 - No Electrochemical Etching Step The coating resistance of Comparative Example 1 (12 mΩ·cm) 2 The initial coulombic efficiency (99.0%) of Comparative Example 1 was comparable to that of Example 1, indicating that the etching step had no significant impact on the conductivity and initial electrochemical performance of the coating itself. However, the peel strength of Comparative Example 1 was only 18 N / m, significantly lower than the 52 N / m of Example 1, a decrease of 65%. After 120 cycles, the coulombic efficiency of Comparative Example 1 dropped below 99.0%, and after 300 cycles, the coating showed localized peeling (edge ​​lifting). This indicates that the micro-pit array formed by electrochemical etching is crucial for improving the adhesion between the coating and the aluminum foil and for long-term cycling stability.

[0119] (3) Effect on Example 2 - No Gradient Structure The only difference between Comparative Example 2 and Example 1 is that the bottom and top slurries used the same amount of ammonium bicarbonate (28 parts by mass each), resulting in a coating with a uniform porosity structure. The peel strength of Comparative Example 2 (51 N / m) was comparable to that of Example 1 (due to the continued electrochemical etching and carbonization treatment), but its cycle life was only 200 cycles, significantly lower than the 420 cycles of Example 1. Cracks were visible on the coating surface after 300 cycles. The coulombic efficiency of the first cycle (98.5%) and the average coulombic efficiency of the first 50 cycles (99.42%) were both lower than those of Example 1. This indicates that the stress buffering function of the gradient porous structure plays a crucial role in long-term cycling stability, and the uniform porosity coating cannot effectively absorb the dynamic stress during cycling.

[0120] (4) Comparison of Example 3 - Traditional PVDF-HFP / NMP system Comparative Example 3 uses a conventional approach with PVDF-HFP elastic polymer binder and NMP organic solvent, without electrochemical etching, gradient pore formation, or carbonization. The peel strength of Comparative Example 3 is only 22 N / m (compared to 52 N / m in Example 1), and the coating resistance is 28 mΩ·cm. 2 (Example 1 is 12mΩ·cm) 2 The initial coulombic efficiency was 98.0% (99.2% in Example 1), but the cycle life was only 150 cycles (420 cycles in Example 1), and the coating edges showed significant peeling after 300 cycles. The high coating resistance was due to the presence of organic binders between the conductive carbon particles, which increased the interfacial impedance. This indicates that the overall process scheme of this application is significantly superior to the traditional elastic polymer binder scheme in terms of coating adhesion, conductivity, electrochemical efficiency, and cycle life.

Claims

1. A method for preparing a carbon-coated aluminum foil current collector for use in sodium-ion batteries without negative electrodes, characterized in that, Includes the following steps: Step (1) After ultrasonically cleaning and drying the aluminum foil, the aluminum foil is used as the anode and the inert electrode is used as the cathode. The aluminum foil is placed in a phosphoric acid solution with a mass concentration of 1-10wt% for constant current anodic etching to form a micro-pit array on the surface of the aluminum foil. The aluminum foil is then rinsed until neutral and dried. Step (2) Dissolve sodium alginate powder in deionized water to prepare an aqueous solution of sodium alginate with a mass concentration of 1-5 wt%. Step (3) The conductive carbon material is added to deionized water and dispersed by high-speed shearing. The sodium alginate aqueous solution obtained in step (2) is added and mixed and stirred. Then, ammonium bicarbonate powder is added at 0-15℃ and stirred and vacuum degassed to prepare bottom slurry and surface slurry respectively. The mass ratio of the conductive carbon material to sodium alginate is (5-15):

1. Based on the sum of the mass of conductive carbon material and sodium alginate as 100 parts by mass, the amount of ammonium bicarbonate added in the bottom slurry is 5-25 parts by mass, and the amount of ammonium bicarbonate added in the surface slurry is 30-70 parts by mass. Step (4) The bottom layer slurry is coated onto the surface of the aluminum foil treated in step (1) to form a bottom layer wet film. After pre-drying at 25-35°C until the surface of the bottom layer wet film is semi-solid, the top layer slurry is coated onto the bottom layer to form a top layer wet film. Step (5) Heat the coated aluminum foil to 50-70℃ and keep it at that temperature to completely decompose the ammonium bicarbonate. Continue to heat it to 80-120℃ and keep it at that temperature until the coating is completely dry. Step (6) The dried carbon-coated aluminum foil is carbonized in three stages under the protection of high-purity inert gas: the first stage is heated to 200-300℃ and held, the second stage is heated to 350-500℃ and held, the third stage is heated to 550-640℃ and held, and then cooled to room temperature in the furnace. Step (7) Immerse the carbon-coated aluminum foil in hydrochloric acid solution to remove the sodium salt generated in situ during carbonization, rinse with deionized water until neutral and dry. Step (8) involves lightly rolling the carbon-coated aluminum foil with a rolling pressure of 0.5-5 N / mm to obtain the coated aluminum foil current collector.

2. The preparation method according to claim 1, characterized in that, The thickness of the aluminum foil in step (1) is 10-30 μm; the specific operation of the ultrasonic cleaning is as follows: first, immerse the aluminum foil in acetone and clean it with an ultrasonic power of 100-300W for 5-15 minutes, then take it out and immerse it in anhydrous ethanol and clean it with an ultrasonic power of 100-300W for 5-15 minutes.

3. The preparation method according to claim 1, characterized in that, The phosphoric acid solution in step (1) has a mass concentration of 2-5 wt% and an etching current density of 10-30 mA / cm. 2 The etching time is 30-90 seconds, and the temperature of the phosphoric acid solution is controlled at 20-35℃ during the etching process.

4. The preparation method according to claim 1, characterized in that, The sodium alginate aqueous solution in step (2) has a mass concentration of 2-4 wt%, a stirring speed of 300-500 rpm, and a stirring time of 45-90 min.

5. The preparation method according to claim 1, characterized in that, The conductive carbon material mentioned in step (3) is selected from nano-sized conductive carbon black, carbon nanotubes, or a mixture of nano-sized conductive carbon black and carbon nanotubes; when the conductive carbon material is a mixture of nano-sized conductive carbon black and carbon nanotubes, the mass ratio of nano-sized conductive carbon black to carbon nanotubes is (3-9):1; the mass ratio of the conductive carbon material to sodium alginate is (7-12):

1.

6. The preparation method according to claim 1, characterized in that, In step (3), based on a total mass of conductive carbon material and sodium alginate of 100 parts by mass, the amount of ammonium bicarbonate added to the bottom slurry is 8-18 parts by mass, and the amount of ammonium bicarbonate added to the surface slurry is 35-55 parts by mass; the slurry temperature is controlled at 0-10℃ during the addition and stirring of ammonium bicarbonate.

7. The preparation method according to claim 1, characterized in that, In step (4), the gap between the blade coating of the bottom wet film is 30-80 μm, and the gap between the blade coating of the top wet film is 50-120 μm; the pre-drying temperature is 28-33℃, and the pre-drying time is 8-15 min.

8. The preparation method according to claim 1, characterized in that, In step (5), the holding temperature during the ammonium bicarbonate decomposition stage is 55-65℃ and the holding time is 45-75min; the temperature during the complete drying stage is 90-110℃ and the drying time is 35-50min; the heating rate is 0.8-1.5℃ / min.

9. The preparation method according to claim 1, characterized in that, The high-purity inert gas mentioned in step (6) is high-purity argon or high-purity nitrogen, with a gas flow rate of 50-200 mL / min; the heating rate is 1-3℃ / min; the first stage temperature is 220-280℃, and the holding time is 45-75 min; the second stage temperature is 380-450℃, and the holding time is 45-90 min; the third stage temperature is 580-640℃, and the holding time is 45-90 min.

10. The preparation method according to claim 1, characterized in that, The concentration of the hydrochloric acid solution in step (7) is 0.2-0.5 mol / L, the pickling temperature is 25-35℃, and the pickling time is 15-40 min; the vacuum drying temperature is 65-75℃, and the vacuum drying time is 3-6 h.

Citation Information

Patent Citations

  • Current collector carbon coated aluminum foil and its preparation method

    CN102832392A

  • Sodium metal batteries, electrochemical devices

    CN113451546B