Positive electrode sheet, full-tab lithium ion cylindrical battery, and electric device
By optimizing the active material loading and internal impedance coupling parameters of the positive electrode, the contradiction between capacity and performance of lithium-ion batteries after the height is reduced is resolved, and a synergistic improvement in high capacity and excellent rate rise performance is achieved.
Patent Information
- Application Number
- CN202611207005.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-10
- Publication Date
- 2026-11-24
AI Technical Summary
After the height of lithium-ion batteries is reduced to 65mm, it becomes difficult to simultaneously meet the requirements of a capacity level of around 5Ah, temperature rise control, rate performance, and cycle stability, especially due to the increase in sheet resistance and AC impedance caused by the thickening of the positive electrode active material layer and the lengthening of pore channels.
By optimizing the design of the positive electrode sheet, establishing the active material loading parameter A and the internal impedance coupling parameter B, and coordinating the adaptation of the material area width and single-sided areal density, the total active material mass of the positive electrode is matched, the lithium ion pore transport path is shortened, and the low impedance characteristics of the all-tab structure are complementary, avoiding excessive thickening of the active material layer and excessive impedance.
Within a limited height range, a discharge capacity of 4.9Ah to 5.2Ah was achieved, meeting energy density requirements. At the same time, excellent rate temperature rise performance and cycle stability prevented polarization and excessive temperature rise during high-rate discharge, thus maintaining battery performance.
Smart Images

Figure CN123162128A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of lithium-ion battery technology, specifically to a positive electrode, a full-tab lithium-ion cylindrical battery, and an electrical device. Background Technology
[0002] Currently, with the widespread application of lithium-ion batteries in new energy vehicles, energy storage systems, and portable electronic devices, the requirements for battery miniaturization, energy density, and thermal safety performance are continuously increasing. Among these, increasing electrode loading, optimizing material systems, reducing internal resistance, and improving end current collector structures can all lead to higher battery capacity and better rate performance.
[0003] For 21mm diameter all-tab batteries, the all-tab structure can shorten the current collection path and reduce the tab current collection resistance, thereby improving high-rate discharge capability. However, when the height of the platform battery is reduced from 70mm to 65mm, it is difficult to achieve a capacity level of around 5Ah.
[0004] It should be noted that the information disclosed in the background section above is only used to enhance the understanding of the background of this application, and therefore may include information that does not constitute prior art known to those skilled in the art. Summary of the Invention
[0005] During the development of the embodiments disclosed herein, it was further discovered that due to the reduction in battery height, dimensions such as end assembly space and flattened end face height are strictly constrained. If the battery capacity is maintained by increasing the single-sided areal density of the positive electrode side, it is easy to cause the positive electrode active material layer to thicken, the pore channels to lengthen, and the sheet resistance or AC impedance to increase, thereby generating greater polarization and temperature rise during high-rate discharge, thus affecting some performance aspects of the 21650 model battery.
[0006] To provide a basic understanding of some aspects of the disclosed embodiments, a brief summary is given below. This summary is not intended as a general commentary, nor is it intended to identify key / important components or describe the scope of protection of these embodiments, but rather as a prelude to the detailed description that follows.
[0007] This disclosure provides a positive electrode, a full-tab lithium-ion cylindrical battery, and an electrical device that, while reducing the overall height of the battery, ensures battery capacity, while also taking into account temperature rise control, rate performance, and cycle stability.
[0008] In some embodiments, the positive electrode is applied to a full-tab lithium-ion cylindrical battery, wherein the height of the full-tab lithium-ion cylindrical battery is 63.5mm~66.5mm, its outer diameter is 20.6mm~21.5mm, and its discharge capacity C0 is 4.9Ah~5.2Ah; the positive electrode includes a positive current collector and a positive active material layer disposed on the surface of the positive current collector, and the end of the positive electrode is a full-tab structure, and the positive electrode satisfies the following conditions: A = W² * M, 670 ≤ A ≤ 760; B=W2*M*Z / 1000, 2.0≤B≤5.8; Where A is a parameter characterizing the active material loading in the effective coating area of the positive electrode, W2 is the material area width of the positive electrode sheet in mm, and M is the areal density of the positive electrode active material layer on one side in mg / cm³. 2 B is used to characterize the coupling parameter between the loading of positive electrode active material and internal impedance, and Z is the AC impedance of the positive electrode sheet, in mΩ.
[0009] In some embodiments, the positive electrode sheet also satisfies the following condition: C = W2 / W1, 0.86 ≤ C ≤ 0.95; Where C is used to characterize the ratio of the effective coating area to the electrode width, and W1 is the width of the positive electrode in mm.
[0010] In some embodiments, the width W1 of the positive electrode sheet is 56mm~64mm, and the material area width W2 of the positive electrode sheet is 52mm~58mm.
[0011] In some embodiments, the areal density M of the positive electrode active material layer is 12.3 mg / cm². 2 ~14.1 mg / cm 2 .
[0012] In some embodiments, the AC impedance Z of the positive electrode is 3.0mΩ to 7.5mΩ.
[0013] In some embodiments, the positive electrode sheet also satisfies the following condition: D = P * T / Z, 20 ≤ D ≤ 35; Where D is used to characterize the balance between the densification degree of the positive electrode active material layer and the pore ion transport impedance, and P is the compaction density of the positive electrode sheet, in g / cm³. 3 T represents the thickness of one side of the positive electrode active material layer, in μm.
[0014] In some embodiments, the compaction density P of the positive electrode sheet is 3.42 g / cm³. 3 ~3.66g / cm 3 .
[0015] In some embodiments, the thickness T of the positive electrode active material layer on one side is 36 μm to 42 μm.
[0016] In some embodiments, the all-tab lithium-ion cylindrical battery includes the positive electrode sheet described in the foregoing embodiments.
[0017] In some embodiments, the electrical device includes a multi-tab lithium-ion cylindrical battery as described in the foregoing embodiments.
[0018] The positive electrode sheet, the all-tab lithium-ion cylindrical battery, and the power supply device provided in this disclosure can achieve the following technical effects: By establishing a parameter A to characterize the active material loading in the effective coating area of the positive electrode, the width of the material zone and the areal density on one side are coupled, thereby transforming the load per unit area into the overall load of the entire electrode sheet. This ensures the matching of the total active material content of the positive electrode, guaranteeing a battery discharge capacity of 4.9Ah~5.2Ah, meeting the energy density requirements of the 21650 battery model. Simultaneously, by coupling the width of the material zone with the areal density on one side, excessive thickening of the active material layer can be avoided, shortening the lithium-ion pore transport path and alleviating the pressure of increased AC impedance caused by increased areal density.
[0019] By establishing a coupling parameter B to characterize the relationship between the loading of positive electrode active material and internal impedance, the total loading level of active material is coupled with the internal AC impedance of the electrode to form a quantified coupling matching window. When B is in the range of 2.0 to 5.8, it can be ensured that the internal pore ion transport and electronic conduction capabilities of the positive electrode are at an appropriate level under a given loading: this avoids severe polarization and excessive battery temperature rise during high-rate discharge caused by excessive loading and excessive impedance; it also avoids excessive introduction of conductive agents to reduce impedance, sacrificing the proportion of active material, resulting in loss of discharge capacity and energy density. At the same time, this coupling design complements the low impedance characteristics of the all-tab end face current collection, fully releasing the high current advantage of the all-tab structure and preventing the internal conduction bottleneck of the electrode from offsetting the structural gain of the all-tab.
[0020] Therefore, by adapting the dual parameters A and B together, without increasing the total width of the electrode or encroaching on the assembly space of the end foil, high capacity and excellent rate rise performance can be achieved simultaneously within a limited height dimension simply by optimizing the electrode material area and coating properties.
[0021] The above general description and the description below are exemplary and illustrative only and are not intended to limit this application. Attached Figure Description
[0022] One or more embodiments are illustrated by way of example with reference to the accompanying drawings. These illustrations and drawings do not constitute a limitation on the embodiments. Elements having the same reference numerals in the drawings are shown as similar elements. The drawings are not to be scaled. And wherein: Figure 1 This is a schematic diagram of the structure of a full-tab lithium-ion cylindrical battery provided in an embodiment of this disclosure; Figure 2 This is a schematic diagram of the structure of the winding core provided in the embodiments of this disclosure; Figure 3 This is a schematic diagram of the structure of a full-tab lithium-ion cylindrical battery provided in an embodiment of this disclosure.
[0023] Figure label: 10. Shell; 11. Positive terminal; 12. Negative terminal; 20. Core; 21. Positive electrode sheet; 22. Negative electrode sheet; 23. Diaphragm; 24. Tab area. Detailed Implementation
[0024] To provide a more detailed understanding of the features and technical content of the embodiments of this disclosure, the implementation of the embodiments of this disclosure will be described in detail below with reference to the accompanying drawings. The accompanying drawings are for illustrative purposes only and are not intended to limit the embodiments of this disclosure. In the following technical description, for ease of explanation, several details are used to provide a full understanding of the disclosed embodiments. However, one or more embodiments may still be implemented without these details. In other cases, well-known structures and devices may be simplified in their depiction to simplify the drawings.
[0025] The terms "first," "second," etc., used in the specification, claims, and accompanying drawings of this disclosure are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence. It should be understood that such data can be interchanged where appropriate for the embodiments of this disclosure described herein. Furthermore, the terms "comprising" and "having," and any variations thereof, are intended to cover non-exclusive inclusion.
[0026] In this disclosure, the terms "upper," "lower," "inner," "middle," "outer," "front," and "rear," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. These terms are primarily for better description of the embodiments of this disclosure and their implementations, and are not intended to limit the indicated devices, elements, or components to having a specific orientation, or to require them to be constructed and operated in a specific orientation. Furthermore, some of the aforementioned terms may be used to indicate other meanings besides orientation or positional relationship; for example, the term "upper" may in some cases indicate a dependency or connection relationship. Those skilled in the art can understand the specific meaning of these terms in the embodiments of this disclosure according to the specific circumstances.
[0027] Furthermore, the terms "set up," "connect," and "fix" should be interpreted broadly. For example, "connection" can be a fixed connection, a detachable connection, or an integral structure; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, or it can be an internal connection between two devices, components, or parts. Those skilled in the art can understand the specific meaning of the above terms in the embodiments of this disclosure according to the specific circumstances.
[0028] Unless otherwise stated, the term "multiple" means two or more.
[0029] In this embodiment of the disclosure, the character " / " indicates that the objects before and after it are in an "or" relationship. For example, A / B means: A or B.
[0030] The term "and / or" describes an association between objects, indicating that three relationships can exist. For example, A and / or B means: A or B, or A and B.
[0031] It should be noted that, unless otherwise specified, the embodiments and features described in the present disclosure can be combined with each other.
[0032] This disclosure provides a positive electrode sheet for use in a full-tab lithium-ion cylindrical battery. The full-tab lithium-ion cylindrical battery has a height of 63.5mm to 66.5mm, an outer diameter of 20.6mm to 21.5mm, and a discharge capacity C0 of 4.9Ah to 5.2Ah. The positive electrode sheet includes a positive current collector and a positive active material layer disposed on the surface of the positive current collector. The ends of the positive electrode sheet have a full-tab structure. The positive electrode sheet satisfies the following conditions: A = W² * M, 670 ≤ A ≤ 760; B=W2*M*Z / 1000, 2.0≤B≤5.8; Where A is a parameter characterizing the active material loading in the effective coating area of the positive electrode, W2 is the material area width of the positive electrode sheet in mm, and M is the areal density of the positive electrode active material layer on one side in mg / cm³. 2 B is used to characterize the coupling parameter between the loading of positive electrode active material and internal impedance, and Z is the AC impedance of the positive electrode sheet, in mΩ.
[0033] All of the above formulas are empirical formulas obtained from actual research and development. In the calculation process, you can directly substitute the corresponding values.
[0034] Using the positive electrode sheet provided in this embodiment, by establishing a parameter A to characterize the active material loading amount of the effective coating area of the positive electrode, the material area width and the single-sided areal density are coupled, thereby transforming the unit area load into the overall load of the entire length of the electrode sheet. This ensures the matching of the total active material content of the positive electrode, guaranteeing a battery discharge capacity of 4.9Ah~5.2Ah, meeting the energy density requirements of the 21650 battery model. Simultaneously, by coupling the material area width and the single-sided areal density, excessive thickening of the active material layer can be avoided, shortening the lithium-ion pore transport path and alleviating the pressure of increased AC impedance caused by increased areal density.
[0035] By establishing a coupling parameter B to characterize the relationship between the loading of positive electrode active material and internal impedance, the total loading level of active material is coupled with the internal AC impedance of the electrode to form a quantified coupling matching window. When B is in the range of 2.0 to 5.8, it can be ensured that the internal pore ion transport and electronic conduction capabilities of the positive electrode are at an appropriate level under a given loading: this avoids severe polarization and excessive battery temperature rise during high-rate discharge caused by excessive loading and excessive impedance; it also avoids excessive introduction of conductive agents to reduce impedance, sacrificing the proportion of active material, resulting in loss of discharge capacity and energy density. At the same time, this coupling design complements the low impedance characteristics of the all-tab end face current collection, fully releasing the high current advantage of the all-tab structure and preventing the internal conduction bottleneck of the electrode from offsetting the structural gain of the all-tab.
[0036] Therefore, by adapting the dual parameters A and B together, without increasing the total width of the electrode or encroaching on the assembly space of the end foil, high capacity and excellent rate rise performance can be achieved simultaneously within a limited height dimension simply by optimizing the electrode material area and coating properties.
[0037] In the embodiments of this disclosure, in the active material loading parameter A used to characterize the effective coating area of the positive electrode, the material area of the positive electrode sheet, also known as the effective coating area, refers to the area on the surface of the positive electrode current collector coated with and forming a complete positive electrode active material layer. The current collector in this area is fully covered by the active material layer and is the core functional area of the electrode sheet that provides electrochemical capacity.
[0038] In this embodiment, the AC impedance Z of the positive electrode is obtained through EIS testing of a symmetrical cell. Specifically, the positive electrode, separator, and positive electrode are stacked sequentially to obtain a symmetrical cell, and the test area is 1.5386 cm². 2 Here, when the test areas are different, they can be converted to equivalent test areas.
[0039] In this embodiment of the disclosure, in the coupling parameter B used to characterize the loading of positive electrode active material and internal impedance, when B is 2.0 to 5.8, the capacity loading and transmission impedance are in a balanced range; when B is greater than 5.8, the high loading and high impedance are superimposed, resulting in deterioration of rate performance and temperature rise; when B is less than 2.0, the loading is insufficient, and the discharge capacity cannot meet the requirements.
[0040] In some embodiments, the positive electrode sheet also satisfies the following condition: C = W2 / W1, 0.86 ≤ C ≤ 0.95; Where C is used to characterize the ratio of the effective coating area to the electrode width, and W1 is the width of the positive electrode in mm.
[0041] In this embodiment of the disclosure, the positive electrode sheet has a positive electrode material region and a positive electrode empty foil region located on at least one side of the positive electrode material region, wherein the positive electrode empty foil region is an exposed area of the current collector where no active material is coated, and is used to form a full tab structure to achieve end face current collection.
[0042] In this embodiment of the disclosure, by limiting the ratio of the material area width of the positive electrode sheet to the width of the positive electrode sheet, the empty foil margin requirement of the full tab structure can be adapted, and the material area width can be maximized while ensuring the welding / flattening space of the end full tab.
[0043] In some embodiments, the width W1 of the positive electrode sheet is 56mm~64mm, and the material area width W2 of the positive electrode sheet is 52mm~58mm.
[0044] In some embodiments, the width W1 of the positive electrode sheet is 58mm~62mm, the material area width W2 of the positive electrode sheet is 54mm~56mm, and 0.90≤C≤0.93.
[0045] In some embodiments, the areal density M of the positive electrode active material layer is 12.3 mg / cm². 2 ~14.1 mg / cm 2 .
[0046] In some embodiments, the areal density M of the positive electrode active material layer is 12.7 mg / cm². 2 ~ to 13.7 mg / cm 2 .
[0047] In some embodiments, the AC impedance Z of the positive electrode is 3.0mΩ to 7.5mΩ.
[0048] In some embodiments, the AC impedance Z of the positive electrode is 3.6mΩ to 6.8mΩ.
[0049] In some embodiments, 704 ≤ A ≤ 748.
[0050] In some embodiments, 2.98 ≤ B ≤ 4.57.
[0051] In some embodiments, the positive electrode sheet also satisfies the following condition: D = P * T / Z, 20 ≤ D ≤ 35; Where D is used to characterize the balance between the densification degree of the positive electrode active material layer and the pore ion transport impedance, and P is the compaction density of the positive electrode sheet, in g / cm³. 3 T represents the thickness of one side of the positive electrode active material layer, in μm.
[0052] In this embodiment, the positive electrode active material layer is further optimized by focusing on microscopic mass transfer within the coating, using the balance parameter D between the densification degree and pore ion transport impedance of the positive electrode active material layer. Specifically, the pore structure and ion diffusion path are jointly determined by the compaction density and coating thickness. This allows for a densification level achievable per unit impedance, thereby further balancing the contradiction between increased energy density from high compaction and deterioration of pore mass transfer.
[0053] In some embodiments, the compaction density P of the positive electrode sheet is 3.42 g / cm³. 3 ~3.66g / cm 3 .
[0054] In some embodiments, the compaction density P of the positive electrode sheet is 3.48 g / cm³. 3 ~3.60g / cm 3 .
[0055] In some embodiments, the thickness T of the positive electrode active material layer on one side is 36 μm to 42 μm.
[0056] In some embodiments, the thickness T of the positive electrode active material layer on one side is 37 μm to 40.5 μm.
[0057] In some embodiments, 21.6 ≤ D ≤ 33.2.
[0058] In the embodiments disclosed herein, the above-mentioned parameters such as the single-sided areal density M of the positive electrode active material layer, the single-sided thickness T of the positive electrode active material layer, and the compaction density P of the positive electrode sheet are all average physical property parameters of the positive electrode active material layer within the effective coating area.
[0059] In some embodiments, the positive electrode active material layer includes a positive electrode active material, conductive carbon black, carbon nanotubes and a binder, wherein the mass ratio of conductive carbon black to carbon nanotubes is 8:1 to 25:1.
[0060] In some embodiments, the content of conductive carbon black is 0.8 wt% to 2.2 wt%, the content of carbon nanotubes is 0.05 wt% to 0.25 wt%, and the content of binder is 0.8 wt% to 1.8 wt%, based on the total mass of the solid components of the positive electrode active material layer.
[0061] In this embodiment, conductive carbon black and carbon nanotubes form a composite conductive network. The conductive carbon black primarily provides point contacts between particles, while the carbon nanotubes form long-range bridging channels. Thus, increasing the proportion of carbon nanotubes can reduce sheet resistance and AC impedance; however, an excessively high proportion of carbon nanotubes can increase slurry viscosity and dispersion difficulty, affecting coating uniformity.
[0062] In some embodiments, the positive electrode active material in the positive electrode active material layer includes a layered lithium transition metal oxide with a nickel content of 88 mol% to 92 mol%.
[0063] In some embodiments, the layered lithium transition metal oxide includes single-crystal particles and polycrystalline particles, wherein the mass ratio of single-crystal particles to polycrystalline particles is 15:85 to 35:65.
[0064] In some embodiments, the positive current collector is an aluminum foil, wherein the thickness of the aluminum foil is 10 μm to 14 μm.
[0065] In some embodiments, the sheet resistance R of the positive electrode is 0.05 mΩ / sq to 1.50 mΩ / sq.
[0066] In some embodiments, the sheet resistance R of the positive electrode is 0.08 mΩ / sq to 0.90 mΩ / sq.
[0067] In the above embodiments, A, B, C, and D are all dimensionless characteristic coefficients, meaning they have no physical dimensions. When A, B, C, and D are within a defined range, they can synergistically regulate the impedance distribution of the positive electrode, alleviating the polarization temperature rise problem of the 21650 cylindrical all-tab battery under high-rate discharge, thus balancing discharge capacity and cycle performance.
[0068] This disclosure also provides a fully tabbed lithium-ion cylindrical battery, including the positive electrode sheet described in the foregoing embodiments. The specific structure of the positive electrode sheet is the same as described in the foregoing embodiments. Since the fully tabbed lithium-ion cylindrical battery adopts all the technical solutions of all the foregoing embodiments, it possesses at least all the technical effects brought about by the technical solutions of the foregoing embodiments, and will not be described in detail here.
[0069] In some embodiments, the DC internal resistance (DCR) of the all-tab lithium-ion cylindrical battery of this application is less than or equal to 9.5 mΩ when the state of charge (SOC) is 100% at 25°C.
[0070] In some embodiments, the discharge capacity C0 of the all-tab lithium-ion cylindrical battery of this application is 4.9Ah~5.2Ah when discharged at a discharge rate of 0.2C in an environment of 25°C.
[0071] In some embodiments, the capacity retention Q of the all-tab lithium-ion cylindrical battery of this application under 40A discharge conditions at 25°C is... 40 ≥97.0%, highest surface temperature T 40 ≤67℃.
[0072] Combination Figures 1 to 3 As shown in this embodiment, the core 20 includes a positive electrode 21, a negative electrode 22, and a separator 23. The positive electrode 21 includes a positive current collector and a positive active material layer coated on the positive current collector. The positive current collector has a positive empty foil region, which is not coated with the positive active material layer. The negative electrode 22 includes a negative current collector and a negative active material layer coated on the negative current collector. The negative current collector has a negative empty foil region, which is not coated with the negative active material layer. The positive and negative empty foil regions are flattened to form a tab region 24, which is welded to the current collector to form a fully tab conductive structure.
[0073] In this embodiment, the core 20 is disposed inside the housing 10 and has a central hole. A positive terminal 11 and a negative terminal 12 are disposed on the housing 10. The positive terminal 11 is electrically connected to the positive electrode tab area of the core 20, and the negative terminal 12 is electrically connected to the negative electrode tab area of the core 20.
[0074] Furthermore, embodiments of this disclosure also provide an electrical device, including a full-tab lithium-ion cylindrical battery for providing power as described in this application.
[0075] The present invention will be further explained and illustrated below with reference to embodiments.
[0076] This embodiment 1 provides a fully tabbed lithium-ion cylindrical battery. The positive electrode comprises a 12 μm thick aluminum current collector and a positive electrode active material layer coated on both sides of the aluminum current collector. The positive electrode active material layer, by mass percentage of solid components, comprises 97.25% positive electrode active material, 1.50% conductive carbon black (SP), 0.10% carbon nanotubes (SWCNTs), and 1.15% polyvinylidene fluoride (PVDF). Here, the positive electrode active material is a layered lithium transition metal oxide with a nickel molar fraction of 90%, comprising polycrystalline and single-crystal particles in a mass ratio of 80:20.
[0077] The above components were dispersed in N-methylpyrrolidone to prepare a positive electrode slurry. Specifically, PVDF was first added to N-methylpyrrolidone and stirred at 1200 r / min for 120 min to obtain a binder solution. Then, conductive carbon black and carbon nanotube slurry were added and stirred and dispersed at 1800 r / min for 90 min. Subsequently, the positive electrode active material was added in two batches, and after each addition, the mixture was stirred at 1500 r / min for 60 min and vacuum degassed for 30 min to obtain a positive electrode slurry with a solid content of 71 wt%. The viscosity of the slurry was controlled between 6500 mPa·s and 9000 mPa·s.
[0078] In the coating of the positive electrode slurry, a slit die is used to intermittently coat the positive electrode slurry on both sides of the aluminum foil. The width of the material area of the positive electrode sheet is adjusted by adjusting the opening of the shim of the coating die, and the surface density of the positive electrode active material layer is adjusted by adjusting the coating surface density. After coating, the electrode is dried in a three-stage oven at 80℃, 100℃, and 120℃. After drying, the moisture content of the electrode sheet is no higher than 500ppm.
[0079] In the rolling process, the compaction density of the positive electrode sheet and the single-sided thickness of the positive electrode active material layer are adjusted by regulating the roll gap and rolling pressure. The rolled positive electrode sheet is then slit and formed with tabs to obtain the final positive electrode sheet. The parameters of the positive electrode sheet are as follows: The width of the positive electrode sheet is 60.0 mm, the width of the empty foil area of the positive electrode sheet is 4.0 mm (single-sided empty foil area, which will later be used as the flattening layer of the positive electrode tab), and the width of the material area of the positive electrode sheet is 55.0 mm; the single-sided areal density of the positive electrode active material layer is 13.2 mg / cm³. 2 The thickness of the positive electrode active material layer on one side is 38.5 μm, and the compaction density of the positive electrode sheet is 3.54 g / cm³. 3 The AC impedance of the positive electrode is 4.90 mΩ, and the coin discharge capacity of the positive electrode is 213 mAh / g.
[0080] The corresponding negative electrode sheet, separator, and electrolyte are prepared. The positive electrode sheet, separator, negative electrode sheet, and separator are wound in a stacked order to form a core. After winding, the positive and negative terminals are flattened to form a full-tab end face. The positive current collector is welded to the positive full-tab end face, and the negative current collector is welded to the negative full-tab end face. The negative current collector is also welded to the bottom of the casing. After the core is inserted into the casing, the insulating components and cap assembly are installed, making the cap assembly electrically connected to the positive current collector path, and the cap is sealed by welding. After insulation testing, electrolyte injection, static immersion, formation, aging, and capacity testing, the full-tab lithium-ion cylindrical battery of Example 1 is obtained. The height of this full-tab lithium-ion cylindrical battery is 65.0 mm, and the outer diameter is 21.0 mm.
[0081] Here, the discharge capacity C0 of the all-tab lithium-ion cylindrical battery is 5.03Ah.
[0082] Example 2 Example 2 provides a full-tab lithium-ion cylindrical battery. The difference between this example and Example 1 is that the material area width W2 of the positive electrode is 54.0 mm, and the discharge capacity C0 of the full-tab lithium-ion cylindrical battery is 4.98 Ah. Everything else is the same as in Example 1.
[0083] Example 3 Example 3 provides a full-tab lithium-ion cylindrical battery. The difference between this example and Example 1 is that the material area width W2 of the positive electrode is 56.0 mm, and the discharge capacity C0 of the full-tab lithium-ion cylindrical battery is 5.07 Ah. Everything else is the same as in Example 1.
[0084] Example 4 Example 4 provides a full-tab lithium-ion cylindrical battery. The difference between this example and Example 1 is that the areal density M of the positive electrode active material layer is 12.8 mg / cm². 2 The positive electrode has an AC impedance of 4.70 mΩ, and the discharge capacity C0 of the all-tab lithium-ion cylindrical battery is 4.94 Ah. Everything else is the same as in Example 1.
[0085] Example 5 Example 5 provides a full-tab lithium-ion cylindrical battery. The difference between this example and Example 1 is that the areal density M of the positive electrode active material layer is 13.6 mg / cm². 2 The positive electrode has an AC impedance of 5.20 mΩ, and the discharge capacity C0 of the all-tab lithium-ion cylindrical battery is 5.11 Ah. Everything else is the same as in Example 1.
[0086] Example 6 Example 6 provides a full-tab lithium-ion cylindrical battery. The difference between this example and Example 1 is that the compaction density P of the positive electrode sheet is 3.48 g / cm³. 3 The positive electrode has an AC impedance of 4.75 mΩ, and the discharge capacity C0 of the all-tab lithium-ion cylindrical battery is 5.00 Ah. Everything else is the same as in Example 1.
[0087] Example 7 Example 7 provides a full-tab lithium-ion cylindrical battery. The difference between this example and Example 1 is that the compaction density P of the positive electrode sheet is 3.60 g / cm³. 3 The positive electrode has an AC impedance of 5.35 mΩ, and the discharge capacity C0 of the all-tab lithium-ion cylindrical battery is 5.04 Ah. Everything else is the same as in Example 1.
[0088] Example 8 Example 8 provides a fully tabbed lithium-ion cylindrical battery. The difference between this example and Example 1 is that the conductive carbon black content is 1.44%, the carbon nanotube content is 0.16%, the AC impedance of the positive electrode is 4.10 mΩ, and the discharge capacity C0 of the fully tabbed lithium-ion cylindrical battery is 5.02 Ah. Everything else is the same as in Example 1.
[0089] Example 9 Example 9 provides a fully tabbed lithium-ion cylindrical battery. The difference between this example and Example 1 is that the conductive carbon black content is 1.54%, the carbon nanotube content is 0.06%, the AC impedance of the positive electrode is 6.30 mΩ, and the discharge capacity C0 of the fully tabbed lithium-ion cylindrical battery is 5.01 Ah. Everything else is the same as in Example 1.
[0090] Comparative Example 1 Comparative Example 1 provides a lithium-ion cylindrical battery. The difference between this comparative example and Example 1 is that the material area width W2 of the positive electrode is 50.5 mm, and the discharge capacity C0 of the full-tab lithium-ion cylindrical battery is 4.82 Ah. Everything else is the same as in Example 1.
[0091] Comparative Example 2 Comparative Example 2 provides a full-tab lithium-ion cylindrical battery. The difference between this comparative example and Example 1 is that the areal density M of the positive electrode active material layer is 14.6 mg / cm². 2 The positive electrode has an AC impedance of 7.80 mΩ, and the discharge capacity C0 of the all-tab lithium-ion cylindrical battery is 5.17 Ah. Everything else is the same as in Example 1.
[0092] Comparative Example 3 Comparative Example 3 provides a fully tabbed lithium-ion cylindrical battery. The difference between this comparative example and Example 1 is that the compaction density P of the positive electrode sheet is 3.75 g / cm³.3 The positive electrode has an AC impedance of 8.20 mΩ, and the discharge capacity C0 of the all-tab lithium-ion cylindrical battery is 5.02 Ah. Everything else is the same as in Example 1.
[0093] Comparative Example 4 Comparative Example 4 provides a fully tabbed lithium-ion cylindrical battery. The difference between this comparative example and Example 1 is that carbon nanotubes were not added, the conductive carbon black content is 1.60%, the AC impedance of the positive electrode is 8.60 mΩ, and the discharge capacity C0 of the fully tabbed lithium-ion cylindrical battery is 4.99 Ah. Everything else is the same as in Example 1.
[0094] Comparative Example 5 Comparative Example 5 provides a full-tab lithium-ion cylindrical battery. The difference between this comparative example and Example 1 is that the width W1 of the positive electrode is 64.0 mm, the width W2 of the positive electrode material area is 53.0 mm, and the single-sided areal density M of the positive electrode active material layer is 12.00 mg / cm³. 2 The positive electrode has an AC impedance of 2.60 mΩ, and the discharge capacity C0 of the all-tab lithium-ion cylindrical battery is 4.76 Ah. Everything else is the same as in Example 1.
[0095] Comparative Example 6 Comparative Example 6 provides a fully tabbed lithium-ion cylindrical battery. The difference between this comparative example and Example 1 is that the areal density M of the positive electrode active material layer is 14.20 mg / cm². 2 The positive electrode has an AC impedance of 7.70 mΩ, and the discharge capacity C0 of the all-tab lithium-ion cylindrical battery is 5.12 Ah. Everything else is the same as in Example 1.
[0096] Comparative Example 7 Comparative Example 7 provides a full-tab lithium-ion cylindrical battery. The difference between this comparative example and Example 1 is that the positive electrode active material is replaced with a high-nickel positive electrode material with a 0.1C coin discharge capacity of 188 mAh / g, resulting in a positive electrode coin discharge capacity of 188 mAh / g, a discharge capacity C0 of 4.72 Ah for the full-tab lithium-ion cylindrical battery, and an AC impedance of 5.20 mΩ for the positive electrode. All other aspects are the same as in Example 1.
[0097] The full-tab lithium-ion cylindrical batteries of Examples 1 to 9 and Comparative Examples 1 to 7 were subjected to corresponding tests. Before testing, each full-tab lithium-ion cylindrical battery was placed in an environment of 23°C to 27°C for at least 12 hours to confirm that there was no deformation, leakage, or abnormalities at the ends of the battery. The test was then conducted at an ambient temperature of 25°C.
[0098] In the 0.2C discharge capacity test, three test batteries were used for each sample group. The test batteries were charged at a constant current rate of 1C to 4.20V, then switched to constant voltage charging to the cutoff current of 0.05C, and left to stand for 30 minutes; subsequently, they were discharged at a constant current rate of 0.2C to 2.50V, and the discharge capacity C0 was recorded. The discharge capacity was calculated as the average value of the three test batteries.
[0099] In the surface resistance test of the positive electrode sheet, five positions of the positive electrode sheet after rolling are taken in each group, and a 50mm×50mm sample is cut. The surface resistance R of the positive electrode sheet is tested using a four-probe surface resistance meter or equivalent equipment in an environment with relative humidity ≤30%, and the average value of the five points is taken.
[0100] In the AC impedance test of the positive electrode, each group of positive electrode sheets was used to prepare a symmetrical cell with "positive electrode / separator / positive electrode", and the test area was 1.5386 cm². 2 After standing for 12 hours, EIS testing was performed using an electrochemical workstation with a frequency range of 100kHz to 10mHz and a disturbance voltage of 5mV. The AC impedance Z of the positive electrode was obtained by fitting the equivalent circuit.
[0101] In the DC internal resistance (DCR) test, three test batteries were used in each group. The test batteries were fully charged to 4.20V at 1C and allowed to stand for 60 minutes. With a state of charge (SOC) of 100%, a 40A discharge pulse was applied for 10 seconds, and the voltages before and after the pulse were recorded. 10 DCR=(U0-U 10 ) / I×1000.
[0102] In the 40A rate discharge test, three test batteries were used in each group. The test batteries were fully charged to 4.20V at 1C, allowed to stand for 30 minutes, and then discharged at 1A to 2.50V to obtain the baseline capacity. The same batch of test batteries were then fully charged again, allowed to stand for 30 minutes, and then discharged at 40A to 2.50V or 75℃ as the cutoff point. The rate capacity and the highest surface temperature T were recorded. max Here, the rate capacity retention rate is obtained by comparing the rate capacity with the reference capacity.
[0103] In the 60A boundary test, two test batteries were taken from each group and left to stand for 30 minutes with a state of charge (SOC) of 100%. The batteries were then discharged at 60A to 2.50V or 80℃ as the cutoff point, and the capacity, energy, and highest temperature were recorded.
[0104] In the electrochemical impedance spectroscopy (EIS) test, three test cells were used in each group. The state of charge (SOC) was adjusted to 50%, and the cells were allowed to stand at 25°C for 2 hours before EIS testing. The frequency range was 100 kHz to 10 mHz, and the perturbation voltage was 5 mV. The ohmic impedance R was obtained by fitting the data. s and charge transfer impedance R ct .
[0105] In the cycle performance test, three test batteries were taken in each group, charged to 4.20V at 8A, constant voltage to 0.25A, and left to stand for 10 minutes; discharged to 2.50V or 75℃ at 40A, left to stand for 10 minutes, and cycled for 200 cycles. The cycle capacity retention rate was obtained by comparing the discharge capacity after 200 cycles with the discharge capacity in the first cycle.
[0106] At least one test cell from each group was taken after capacity testing and disassembled under an inert atmosphere. The positive electrode was cleaned with dimethyl carbonate (DMC) and then vacuum dried. The thickness of the electrode was measured by cross-section, and the particle packing, pores, and conductive network distribution were observed by scanning electron microscopy (SEM). The elemental distribution was confirmed by energy dispersive spectroscopy (EDS).
[0107] In the coin cell test, the positive electrode sheet was used to prepare a coin cell for each group, and the negative electrode was a lithium sheet. After standing for 12 hours, the cells were charged and discharged at 0.1C with a voltage range of 3.0V to 4.3V. The initial discharge capacity was recorded.
[0108] After conducting the above tests in Examples 1 to 9 and Comparative Examples 1 to 7, the corresponding data were obtained. The sheet resistance R, discharge capacity C0, A, B, C, D, DC internal resistance DCR, electrochemical impedance spectroscopy (EIS), and highest surface temperature T at 40A rate were measured. 40 40A rate capacity retention rate Q 40 60A rate capacity retention rate Q 60 Cyclic capacity retention rate Q. The relevant data are shown in Table 1.
[0109]
[0110] Table 1 As shown in Table 1, in Examples 1 to 9, when A, B, C, and D are all within the specified range, the discharge capacity C0 is 4.94 Ah to 5.11 Ah, and the capacity retention rate Q at 40A rate is... 40 All are greater than or equal to 97.1%, and the highest surface temperature T at 40A magnification is... 40 At temperatures not exceeding 66.7℃, the cyclic capacity retention rate Q after 200 cycles is greater than or equal to 93.0%.
[0111] In Comparative Examples 1, 5, and 7, the discharge capacity C0 did not reach 4.9 Ah. However, in Comparative Examples 2 to 4 and Comparative Example 6, the DCR significantly increased, and the highest surface temperature T at 40A rate was [not specified]. 40 Increased and decreased cycle capacity retention rate Q.
[0112] In conjunction with Examples 1 to 3, when the material area width W2 of the positive electrode sheet is adjusted from 55.0 mm to 54.0 mm or 56.0 mm, the active material loading parameter A, which is used to characterize the effective coating area of the positive electrode, changes between 713 and 739, which is within a reasonable range, and its various performances are superior.
[0113] In Comparative Example 1, the material area width W2 of the positive electrode is too small. In this case, the effective active material carrying width is insufficient, and even with low sheet resistance and AC impedance, it cannot provide sufficient positive electrode capacity contribution. When the material area width W2 of the positive electrode is too large, the end foil and the current collection space of the full tab are compressed, which easily causes uneven current distribution in the flattened area.
[0114] Based on Examples 1, 4, and 5, as well as Comparative Examples 2, 5, and 6, it can be seen that the areal density M of the positive electrode active material layer determines the positive electrode capacity per unit area. Specifically, when the areal density M of the positive electrode active material layer is low, the AC impedance and maximum surface temperature are better, but the discharge capacity decreases; while when the areal density M of the positive electrode active material layer is high, the discharge capacity increases, but the Li in the thickness direction of the active layer... + The diffusion path becomes longer, leading to an increase in AC impedance and surface resistivity. Therefore, the single-sided surface density M of the positive electrode active material layer is limited to 12.3 mg / cm². 2 Up to 14.1 mg / cm 2 This approach avoids the problems of scaling down and temperature rise caused by simply increasing the areal density.
[0115] Combining Examples 1, 6, and 7 with Comparative Example 3, when the compaction density P of the positive electrode sheet is low, more pores are retained, but the volumetric efficiency is insufficient; when the compaction density P of the positive electrode sheet is high, the interparticle contact is improved, but the pores are compressed, limiting electrolyte wetting and ion transport. Therefore, the compaction density P of the positive electrode sheet is limited to 3.42 g / cm³. 3 ~3.66g / cm 3 It can balance size and capacity with transmission channels.
[0116] Meanwhile, the single-sided thickness T, single-sided areal density M, and compaction density P of the positive electrode sheet jointly determine the space occupied by the positive electrode active material layer. Therefore, if the single-sided thickness T of the positive electrode active material layer is too high, it will lengthen the electron and ion transport paths, increasing the potential gradient and polarization heat at high rates; if the single-sided thickness T of the positive electrode active material layer is too low, the mass of the positive electrode active material will be insufficient. Limiting the single-sided thickness T of the positive electrode active material layer to 36μm~42μm, and further limiting it through parameters B and C, can avoid the imbalance of high loading but low transport in a thick electrode.
[0117] In conjunction with Examples 1, 8, and 9, as well as Comparative Examples 3 and 4, the AC impedance Z and sheet resistance R of the positive electrode are comprehensive reverse detection indicators of the positive electrode conductive network, channel connectivity, and compaction state. Specifically, when the AC impedance Z of the positive electrode is between 3.0 mΩ and 7.5 mΩ, both discharge capacity and rate performance can be balanced. However, when the AC impedance Z of the positive electrode is greater than 7.5 mΩ, the discharge rate (DCR) and temperature rise increase, and the 60A boundary discharge and cycle performance deteriorate. If the AC impedance Z of the positive electrode is too low, but parameter A is not within the specified range, although the rate performance is good, the discharge capacity cannot meet the design requirements.
[0118] The foregoing description and accompanying drawings fully illustrate embodiments of the present disclosure to enable those skilled in the art to practice them. Other embodiments may include structural and other changes. The embodiments represent only possible variations. Individual components and functions are optional unless explicitly required, and the order of operation may vary. Parts and features of some embodiments may be included or substituted for parts and features of other embodiments. Embodiments of the present disclosure are not limited to the structures described above and shown in the accompanying drawings, and various modifications and changes may be made without departing from its scope. The scope of the present disclosure is limited only by the appended claims.
Claims
1. A positive electrode plate, characterized in that, This technology is applied to all-tab lithium-ion cylindrical batteries. The all-tab lithium-ion cylindrical battery has a height of 63.5mm~66.5mm, an outer diameter of 20.6mm~21.5mm, and a discharge capacity C0 of 4.9Ah~5.2Ah. The positive electrode includes a positive current collector and a positive active material layer disposed on the surface of the positive current collector. The end of the positive electrode has an all-tab structure. The positive electrode satisfies the following conditions: A = W² * M, 670 ≤ A ≤ 760; B=W2*M*Z / 1000, 2.0≤B≤5.8; Where A is a parameter characterizing the active material loading in the effective coating area of the positive electrode, W2 is the material area width of the positive electrode sheet in mm, and M is the areal density of the positive electrode active material layer on one side in mg / cm³. 2 B is used to characterize the coupling parameter between the loading of positive electrode active material and internal impedance, and Z is the AC impedance of the positive electrode sheet, in mΩ.
2. The positive electrode sheet according to claim 1, characterized in that, The positive electrode also satisfies the following conditions: C = W2 / W1, 0.86 ≤ C ≤ 0.95; Where C is used to characterize the ratio of the effective coating area to the electrode width, and W1 is the width of the positive electrode in mm.
3. The positive electrode sheet according to claim 2, characterized in that, The width W1 of the positive electrode is 56mm~64mm, and the material area width W2 of the positive electrode is 52mm~58mm.
4. The positive electrode sheet according to claim 3, characterized in that, The areal density M of the positive electrode active material layer is 12.3 mg / cm³. 2 ~14.1 mg / cm 2 .
5. The positive electrode sheet according to claim 4, characterized in that, The AC impedance Z of the positive electrode is 3.0mΩ~7.5mΩ.
6. The positive electrode sheet according to any one of claims 1 to 5, characterized in that, The positive electrode also satisfies the following conditions: D = P * T / Z, 20 ≤ D ≤ 35; Where D is used to characterize the balance between the densification degree of the positive electrode active material layer and the pore ion transport impedance, and P is the compaction density of the positive electrode sheet, in g / cm³. 3 T represents the thickness of one side of the positive electrode active material layer, in μm.
7. The positive electrode sheet according to claim 6, characterized in that, The compaction density P of the positive electrode sheet is 3.42 g / cm³. 3 ~3.66g / cm 3 .
8. The positive electrode sheet according to claim 6, characterized in that, The thickness T of the positive electrode active material layer on one side is 36μm~42μm.
9. A fully tabbed lithium-ion cylindrical battery, characterized in that, Includes the positive electrode sheet as described in any one of claims 1 to 8.
10. An electrical device, characterized in that, Including the all-tab lithium-ion cylindrical battery as described in any one of claims 9.