Secondary battery and electric device

By employing a three-layer structured negative electrode in a secondary battery, and utilizing the elastic modulus of the interface buffer layer and the lithium-ion binder, the volume change problem of silicon-based negative electrode materials during charge and discharge processes was solved, achieving battery performance with low expansion rate, high energy density, and long cycle life.

CN123162129APending Publication Date: 2026-11-24SOUTH CHINA UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611290929.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-24
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing technologies struggle to simultaneously achieve low expansion rate, high energy density, and long cycle life in rechargeable batteries. Volume changes in silicon-based anode materials during lithium insertion and extraction lead to structural collapse and SEI film rupture, affecting battery performance.

Method used

The negative electrode adopts a three-layer structure, including a negative current collector, a first active material layer, an interface buffer layer, and a second active material layer. The interface buffer layer is composed of a lithium-based binder and has an elastic modulus of 0.1 GPa-2 GPa, providing ion transport channels and stress buffering functions, and ensuring stable bonding at the interface.

Benefits of technology

It reduces battery volume expansion, enhances structural stability and interfacial bonding strength, improves battery cycle performance, reduces energy density loss, and extends cycle life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123162129A_ABST
    Figure CN123162129A_ABST
Patent Text Reader

Abstract

This application relates to the field of battery technology, and in particular discloses a secondary battery and an electrical device. The interface buffer layer of this application is located between two active material layers containing silicon-carbon anode material. It has a lithium-based binder, providing a stable interface while offering efficient ion transport channels to reduce energy density loss. Furthermore, its elastic modulus is 0.1 GPa–2 GPa, enabling it to act as a stress buffer interface, dissipating the dynamic stress caused by the upper and lower active material layers during cycling, reducing battery volume expansion, and enhancing the structural stability and interfacial bonding strength of the upper and lower layers during charge and discharge processes, thereby improving the battery's cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of battery technology, and in particular to a secondary battery and an electrical device. Background Technology

[0002] With the rapid development of electric vehicles, portable electronic devices, and large-scale energy storage systems, the market is placing increasingly higher demands on the energy density, cycle life, and safety of secondary batteries such as lithium-ion batteries. Silicon (Si)-based materials, especially nano-silicon-carbon composites, are considered the most promising next-generation anode materials due to their extremely high theoretical specific capacity (pure silicon can reach 4200 mAh / g), which can significantly improve the overall energy density of batteries.

[0003] However, silicon materials undergo dramatic volume expansion and contraction during lithium insertion and extraction. This inherent defect triggers a series of cascading problems at the electrode scale: First, repeated volume changes cause silicon particles to fracture and pulverize, resulting in loss of electrical contact, active material failure, and rapid capacity decay. Second, intense stress damages the solid electrolyte interphase (SEI) film covering the surface of the active material, causing the SEI film to continuously fracture and reconstruct, continuously consuming electrolyte and active lithium, reducing coulombic efficiency and exacerbating capacity decay. Third, enormous stress can directly cause the entire active material layer to peel off from the copper foil current collector, leading to complete electrode structure collapse and a sharp deterioration in battery performance. These problems severely hinder the commercialization and large-scale application of silicon-carbon anodes.

[0004] To address these challenges, existing technologies primarily focus on modifying the materials themselves. For example, silicon-carbon composites and coatings utilize the conductivity and mechanical buffering properties of carbon materials to stabilize the structure, or film-forming additives are added to the electrolyte to form a more robust SEI film. These methods improve the cycle performance of silicon-carbon anodes to some extent, but they typically come at the cost of sacrificing electrode tap density, initial efficiency, or increasing the proportion of inactive materials. It is difficult to achieve a fundamental balance between maintaining high energy density and achieving long cycle life in rechargeable batteries. Summary of the Invention

[0005] The purpose of this application is to solve the technical problem that it is difficult to simultaneously achieve low expansion rate, high energy density and fast and long cycle life in the prior art of secondary batteries. The application proposes a secondary battery and electrical device. The secondary battery of this application can simultaneously have low expansion rate, high energy density and long cycle life.

[0006] To achieve the above objectives, a first aspect of this application provides a secondary battery, including a negative electrode, said negative electrode comprising: Negative electrode current collector; A first active material layer is disposed on at least one side of the negative electrode current collector, and the first active material layer comprises a first silicon-carbon negative electrode material; An interface buffer layer is disposed on the side of the first active material layer away from the negative electrode current collector. The interface buffer layer contains a first lithiation binder, and the elastic modulus of the buffer layer is 0.1 GPa-2 GPa. A second active material layer is disposed on the side of the buffer layer away from the negative electrode current collector, and the second active material layer contains a second silicon-carbon negative electrode material.

[0007] As an embodiment of this application, the peel strength between the interface buffer layer and the first active material layer is 8N / m-25N / m.

[0008] As an embodiment of this application, the interface buffer layer has a lithium-ion conductivity of 1×10⁻⁶ at 25°C. -5 -8×10 -4 S / cm.

[0009] As an embodiment of this application, the areal density of the interface buffer layer is 3g / 1540.25mm. 2 -10g / 1540.25mm 2 .

[0010] As an embodiment of this application, the thickness of the interface buffer layer accounts for 1%-10% of the total thickness of the first active material layer, the interface buffer layer and the second active material layer.

[0011] As an embodiment of this application, the first active material layer and / or the second active material layer further include the first lithiation binder.

[0012] As an embodiment of this application, the first active material layer and the second active material layer include the first lithiated binder, satisfying the following relationship: m2>m3≥m1, where m1 is the mass percentage of the first lithiated binder in the first active material layer, m2 is the mass percentage of the first lithiated binder in the interface buffer layer, and m3 is the mass percentage of the first lithiated binder in the second active material layer.

[0013] As an embodiment of this application, the first lithium-ion adhesive includes at least one of lithium-ion polyacrylic acid (PAALi) and lithium carboxymethyl cellulose (CMC-Li).

[0014] As an embodiment of this application, the interface buffer layer further includes a second adhesive, which includes at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), carboxymethyl cellulose (CMC), sodium alginate (SA), polyvinylidene fluoride (PVDF), polyimide (PI), and polypyrrole copolymer.

[0015] As an embodiment of this application, the average particle size of the first silicon-carbon anode material is larger than the average particle size of the second silicon-carbon anode material.

[0016] As an embodiment of this application, the first active material layer includes a first graphite, the second active material layer includes a second graphite, the first graphite includes spherical graphite, and the second graphite includes flake graphite.

[0017] As an embodiment of this application, the interface buffer layer further includes a conductive agent, which includes at least one of zero-dimensional conductive agents, one-dimensional conductive agents, and two-dimensional conductive agents.

[0018] As an embodiment of this application, the average particle size of the first silicon-carbon anode material is 15μm-25μm.

[0019] As an embodiment of this application, the average particle size of the second silicon-carbon anode material is 5μm-15μm.

[0020] As an embodiment of this application, the secondary battery satisfies the following relationship: n2 > n1, where n1 is the mass percentage of the first silicon-carbon anode material in the first active material layer, and n2 is the mass percentage of the second silicon-carbon anode material in the second active material layer.

[0021] As an embodiment of this application, the secondary battery satisfies the following relationship: P1 > P2, where P1 is the porosity of the first active material layer and P2 is the porosity of the second active material layer.

[0022] As an embodiment of this application, the secondary battery satisfies: k = [(d1×P1) / (d2×P2)]×(n1 / n2), 0.1≤k≤1; where d1 is the thickness of the first active material layer in μm; d2 is the thickness of the second active material layer in μm; P1 is the porosity of the first active material layer; P2 is the porosity of the second active material layer; n1 is the mass percentage of the first silicon-carbon anode material in the first active material layer; and n2 is the mass percentage of the second silicon-carbon anode material in the second active material layer.

[0023] On the other hand, this application also provides an electrical device comprising the aforementioned secondary battery.

[0024] Compared with the prior art, the beneficial effects of this application are as follows: The interface buffer layer of this application is located between two active material layers containing silicon-carbon anode material. It has a lithium binder, which can provide a high-efficiency ion transport channel while having the basic function of bonding and stabilizing the interface, thus reducing the loss of energy density. Moreover, its elastic modulus is 0.1GPa-2GPa, which enables it to act as a stress buffer interface to dissipate the dynamic stress of the upper and lower active material layers during cycling, reduce the volume expansion of the battery, and enhance the structural stability and interface bonding strength of the upper and lower layers during the charging and discharging process, so as to improve the cycle performance of the battery. Attached Figure Description

[0025] Figure 1 This is a schematic diagram of the structure of the first active material layer, the interface buffer layer, and the second active material layer on one side of the negative electrode current collector in the negative electrode sheet of this application; Figure description: 1. Negative electrode current collector, 2. First active material layer, 3. Interface buffer layer, 4. Second active material layer. Detailed Implementation

[0026] To make the objectives, technical solutions, and advantages of the embodiments of this application clearer, the technical solutions in the embodiments of this application will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of this application, not all embodiments. Based on the embodiments in this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.

[0027] In this application, the technical features described in an open-ended manner include both closed technical solutions consisting of the listed features and open technical solutions that include the listed features.

[0028] In this application, numerical ranges are referred to as continuous unless otherwise specified, and include the minimum and maximum values ​​of the range, as well as every value between the minimum and maximum values. Furthermore, when the range refers to integers, it includes every integer between the minimum and maximum values ​​of the range. Additionally, when multiple ranges are provided to describe a feature or characteristic, the ranges may be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges to which they are incorporated.

[0029] This application discloses a secondary battery, including a negative electrode, said negative electrode comprising: Negative electrode current collector; A first active material layer is disposed on at least one side of the negative electrode current collector, and the first active material layer comprises a first silicon-carbon negative electrode material; An interface buffer layer is disposed on the side of the first active material layer away from the negative electrode current collector. The interface buffer layer contains a first lithiation binder, and the elastic modulus of the buffer layer is 0.1 GPa-2 GPa. A second active material layer is disposed on the side of the buffer layer away from the negative electrode current collector, and the second active material layer contains a second silicon-carbon negative electrode material.

[0030] The interface buffer layer of this application is located between two active material layers containing silicon-carbon anode material. It has a lithium-based binder, which not only has the basic function of bonding and stabilizing the interface, but also provides a highly efficient ion transport channel to reduce energy density loss. Moreover, its elastic modulus is 0.1GPa-2GPa, which enables it to act as a stress buffer interface to dissipate the dynamic stress caused by the upper and lower active material layers during cycling, reduce the volume expansion of the battery, and enhance the structural stability and interfacial bonding strength of the upper and lower layers during charge and discharge, so as to improve the cycle performance of the battery.

[0031] The interface buffer layer comprises a first lithiated binder, which inherently possesses basic adhesive properties. Furthermore, the lithium ions pre-loaded on its molecular chains provide an additional lithium source for SEI film construction during the initial charge-discharge process. Simultaneously, it exhibits higher ionic conductivity than the untreated binder, enabling the construction of an additional ionic conductive network within the active layer to form efficient ion transport channels, thus ensuring the interface buffer layer retains good ion transport capabilities. The buffer layer has an elastic modulus of 0.1 GPa-2 GPa. This relatively low elastic modulus allows the interface buffer layer to effectively absorb mechanical energy through its own elastic deformation when subjected to volume expansion stress from the silicon-carbon anode material, reducing stress transmission to the current collector interface, thereby lowering the battery's expansion rate and improving the electrode's structural stability. Therefore, the interface buffer layer of this application, in addition to its adhesive function of bonding two active material layers, simultaneously undertakes the functions of ion transport and stress buffering.

[0032] In one embodiment, the elastic modulus of the buffer layer is 0.1 GPa-2 GPa, specifically 0.1 GPa, 0.24 GPa, 0.37 GPa, 0.51 GPa, 0.64 GPa, 0.78 GPa, 0.91 GPa, 1.05 GPa, 1.19 GPa, 1.32 GPa, 1.46 GPa, 1.59 GPa, 1.73 GPa, 1.86 GPa, 2.0 GPa, or any range between any two of the above points.

[0033] The elastic modulus of the interface buffer layer was tested using nanoindentation, including the following steps: 1. Sample preparation: A three-layer slot extrusion coating machine was used to coat the first negative electrode slurry on both sides of a 4.5 μm thick copper foil, obtaining a wet film of the first active material layer. Immediately afterward, an interface buffer layer slurry was coated onto this wet film, resulting in a wet film of the interface buffer layer. Subsequently, the second negative electrode slurry was immediately coated, obtaining a wet film of the second active material layer. The coated electrode sheets were dried at 80°C to form a stable porous structure, followed by drying and rolling (compacted density 1.6 g / cm³). 3 After that, the unrolled electrode is immersed in deionized water. Taking advantage of the weak adhesion between the copper foil and the coating, the multi-layer coating is carefully peeled off completely from the copper foil surface. Subsequently, the interface buffer layer is separated from the three-layer composite coating by mechanical peeling (or cryogenic ultrathin sectioning) to obtain an independent interface buffer layer film with the same thickness as in the electrode (approximately 1-5 μm).

[0034] 2. Testing Method: Nanoindentation was performed using a Berkovich diamond indenter. Tests were conducted at room temperature (25°C) in continuous stiffness measurement (CSM) mode. The indentation depth was controlled to be within 10% of the interfacial buffer layer thickness (typically <200 nm) to eliminate substrate effects. The preset indentation strain rate was 0.05 s⁻¹. -1 At a frequency of 45Hz, a continuous load-displacement curve (Ph curve) was obtained.

[0035] 3. Data Processing: The elastic modulus (E) was calculated using the Oliver-Pharr method from the slope at the top of the unloading curve in the load-displacement curve. The Poisson's ratio ν of the tested buffer layer involved in the calculation was taken as 0.3, and the average value of stable elastic modulus data within the indentation depth range of 100-200 nm was taken as the elastic modulus of the interface buffer layer.

[0036] In one embodiment, the peel strength between the interface buffer layer and the first active material layer is 8 N / m-25 N / m, specifically 8 N / m, 9.2 N / m, 10.4 N / m, 11.6 N / m, 12.9 N / m, 14.1 N / m, 15.3 N / m, 16.5 N / m, 17.7 N / m, 18.9 N / m, 20.1 N / m, 21.3 N / m, 22.5 N / m, 23.7 N / m, 25 N / m, or any range between any two of the above points.

[0037] The peel strength between the interface buffer layer and the first active material layer is within the above-mentioned range, indicating that the interface buffer layer and the first active material layer have good adhesive strength. This adhesive strength originates from the strong hydrogen bonding between the groups on the adhesive molecular chain and the surface of the active material layer, which can effectively prevent interlayer separation during charge-discharge cycles.

[0038] Peel strength was tested using a 180° peel test. 1. Sample preparation: A three-layer slot extrusion coating machine was used to coat the first negative electrode slurry on both sides of a 4.5 μm thick copper foil, obtaining a wet film of the first active material layer. Immediately afterward, an interface buffer layer slurry was coated onto this wet film, resulting in a wet film of the interface buffer layer. The coated sheet was then dried at 80°C to form a stable pore structure and rolled to a compaction density of 1.6 g / cm³. 3 A first active material layer and an interface buffer layer were formed on the copper foil. The sheet was cut into rectangular strips 150mm long and 25mm wide. 3M double-sided tape (or tape of equivalent tack) was used to smoothly attach the strips to the surface of the interface buffer layer, and a 2kg roller was used to roll the strips back and forth three times to ensure a tight bond.

[0039] 2. Testing Method: A 180° peel test was conducted using a universal testing machine (referencing standard GB / T 2790-1995). One end of the copper foil and the other end of the adhesive tape of the sample were clamped in the upper and lower fixtures of the testing machine, ensuring a constant peel angle of 180°. Peeling was performed at a constant rate of 50 mm / min, and the peel force-displacement curve was recorded.

[0040] 3. Data Processing: The average value is taken in the stable section of the peel force-displacement curve, and the peel strength (N / m) is calculated as: average peel force (N) / sample width (m). In this application, this value reflects the bonding strength between the interface buffer layer and the first active material layer.

[0041] In one embodiment, the lithium-ion conductivity of the interface buffer layer at 25°C is 1×10⁻⁶. -5 S / cm-8×10 - 4 S / cm, specifically it can be 1.0 × 10 -5 S / cm, 4.5×10 -5 S / cm, 8.0×10 -5 S / cm, 1.15×10 -4 S / cm, 1.5×10 -4 S / cm, 1.85×10 -4 S / cm, 2.2×10 -4 S / cm, 2.55×10 -4 S / cm, 2.9×10 -4 S / cm, 3.25×10 -4 S / cm, 3.6×10 -4 S / cm, 3.95×10 -4 S / cm, 4.3×10-4 S / cm, 4.65×10 -4 S / cm, 5.0×10 -4 S / cm, 5.2×10 -4 S / cm, 5.5×10 -4 S / cm, 5.8×10 -4 S / cm, 6.1×10 -4 S / cm, 6.4×10 -4 S / cm, 6.7×10 -4 S / cm, 7.0×10 -4 S / cm, 7.3×10 -4 S / cm, 7.6×10 -4 S / cm, 7.9×10 -4 S / cm, 8.0×10 -4 S / cm, or the range between any two of the above points.

[0042] The interface buffer layer has a lithium-ion conductivity within the range mentioned above, indicating that it has good ion transport function. This is because the interface buffer layer has a lithiumized binder, and the lithium ions pre-loaded on its molecular chain can provide an additional lithium source to participate in the construction of the SEI film during the first charge and discharge process. At the same time, it has an ionic conductivity higher than that of the untreated binder, which can build an additional ion-conducting network inside the active layer to form an efficient ion transport channel.

[0043] The lithium-ion conductivity of the interface buffer layer at 25℃ was tested using the AC impedance method as follows: 1. Sample preparation: The interface buffer layer slurry was separately coated onto the release film and vacuum dried at 80°C for 12 hours to obtain a self-supporting film with uniform thickness (approximately 100-200 μm) and a smooth surface. The film was then cut into circular pieces with a diameter of 19 mm in an argon-filled glove box (H2O < 0.1 ppm, O2 < 0.1 ppm).

[0044] 2. Battery assembly: Using the blocking electrode method, the above-mentioned membrane is sandwiched between two polished stainless steel (SS) gaskets in a glove box to assemble a “SS|interface buffer layer membrane|SS” symmetrical blocking cell.

[0045] 3. Testing Method: After the assembled battery was placed in a 25°C constant temperature chamber for 2 hours, it was connected to an electrochemical workstation for AC impedance (EIS) testing. The test conditions were: frequency range 0.1Hz to 1MHz, AC disturbance voltage amplitude 5mV.

[0046] 4. Data Processing: The intersection of the high-frequency region and the real axis in the Nyquist plot is the bulk impedance Rb. The ionic conductivity (σ) is calculated using the following formula: σ=L / (Rb×A), Where L is the film thickness (cm) and A is the area of ​​the stainless steel electrode (cm²). 2 Rb is the body impedance (Ω).

[0047] In one embodiment, the areal density of the interface buffer layer is 3g / 1540.25mm. 2 -10g / 1540.25mm 2 Specifically, it can be 3.00g / 1540.25mm. 2 3.37g / 1540.25mm 2 3.74g / 1540.25mm 2 4.11g / 1540.25mm 2 4.47g / 1540.25mm 2 4.84g / 1540.25mm 2 5.21g / 1540.25mm 2 5.58g / 1540.25mm 2 5.95g / 1540.25mm 2 6.32g / 1540.25mm 2 6.68g / 1540.25mm 2 7.05g / 1540.25mm 2 7.42g / 1540.25mm 2 7.79g / 1540.25mm 2 8.16g / 1540.25mm 2 8.53, 8.89g / 1540.25mm 2 9.26g / 1540.25mm 2 9.63g / 1540.25mm 2 10.00g / 1540.25mm 2 The areal density range, or any two points mentioned above, precisely balances buffering, bonding, and ion conduction functions. It ensures the formation of a continuous and effective interfacial buffer layer, sufficiently suppressing electrode expansion and guaranteeing interlayer adhesion strength; while avoiding excessive sacrifice of battery volumetric energy density and significant extension of ion transport paths due to an excessively thick interfacial buffer layer. Within this range, efficient release of interfacial stress and rapid lithium-ion pathways can be achieved, thereby maximizing the capacity of active materials and extending cycle life while reducing expansion rate.

[0048] Testing the areal density of the interface buffer layer: Take a copper foil of known area (S1) and weigh it (M1). Coat the copper foil with only an interface buffer layer slurry. After drying under the same conditions, obtain a sheet with an interface buffer layer coated on one side. Cut a sample sheet with area S2 and weigh it to obtain the total mass (M2). The areal density (ρ) of the interface buffer layer per unit area is: ρ = (M2 – M1 × S2 / S1) / S2. Repeat this measurement with 3-5 samples and take the average value to obtain the areal density of the interface buffer layer (unit: g / 1540.25mm²). 2 ).

[0049] In one embodiment, the first lithium-based adhesive comprises at least one of lithium-based polyacrylic acid (PAALi) and lithium carboxymethyl cellulose (CMC-Li). Lithium-based polyacrylic acid (PAALi) is a partial lithium salt of polyacrylic acid (PAA), and its molecular chain contains both unneutralized carboxylic acid groups (-COOH) and ionized carboxylic acid groups (-COO-Li). + This endows PAALi with multiple functions: (a) bonding: the -COOH group can form strong hydrogen bonds with oxygen-containing functional groups on the surface of the current collector coating or active particles, providing interfacial adhesion; (b) ion conduction: -COO-Li + (c) Film-forming properties: As a polymer, PAALi itself possesses film-forming ability, forming a continuous and uniform film layer at the interface. Therefore, in the interfacial buffer layer, PAALi can simultaneously perform the dual functions of "ion transport" and "adhesion". Lithium carboxymethyl cellulose (CMC-Li) also contains lithium ions and has conductive properties, and it is also a good binder, similarly performing the dual functions of "ion transport" and "adhesion".

[0050] In one embodiment, the PAALi is obtained by partial pre-lithiation of PAA, more specifically by neutralizing some of the -COOH groups in PAA with LiOH, with the degree of neutralization controlled at 40%~70%. This retains sufficient free carboxyl groups to maintain good adhesion to the current collector and active particles, while providing additional lithium-ion hopping sites through the ionized carboxylate groups (-COO⁻Li⁺). The pre-loaded lithium ions in PAALi can participate in the stable construction of the SEI film during the first charge, reducing irreversible capacity loss and improving the first coulombic efficiency.

[0051] In one embodiment, the interface buffer layer further includes a second adhesive, the second adhesive comprising at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), carboxymethyl cellulose (CMC), sodium alginate (SA), polyvinylidene fluoride (PVDF), polyimide (PI), and polypyrrole copolymer.

[0052] The interface buffer layer also includes a second adhesive to further improve the interlayer bonding strength, and the second adhesive can increase the flexibility and elasticity of the interface buffer layer to further adapt to the interlayer dynamic strain during the charging and discharging process.

[0053] In one embodiment, the second adhesive in the interface buffer layer has a mass percentage content of 2%-5%, specifically 2.0%, 2.21%, 2.43%, 2.64%, 2.86%, 3.07%, 3.29%, 3.50%, 3.71%, 3.93%, 4.14%, 4.36%, 4.57%, 4.79%, 5.0%, or any two of the above points.

[0054] In one embodiment, the interface buffer layer further includes a conductive agent, which includes at least one of a zero-dimensional conductive agent, a one-dimensional conductive agent, and a two-dimensional conductive agent.

[0055] One-dimensional conductive carbon materials, such as carbon nanotubes (CNTs) and volumetric carbon fibers (VGCF), offer the advantage of forming highly efficient conductive networks with low addition amounts. Their high aspect ratio also provides a degree of fiber toughening, better adapting to the buffering and high transport effects of interfacial buffer layers. Zero-dimensional (conductive carbon black), two-dimensional (graphene), or hybrid dimensional conductive agents can further enhance the conductivity of interfacial buffer layers. Three-dimensional materials, such as three-dimensional flake graphite and spherical graphite, also improve the conductivity of interfacial buffer layers.

[0056] In one embodiment, the conductive agent in the interface buffer layer has a mass percentage content of 80%-90%, specifically 80.0%, 80.7%, 81.4%, 82.1%, 82.9%, 83.6%, 84.3%, 85.0%, 85.7%, 86.4%, 87.1%, 87.9%, 88.6%, 89.3%, 90.0%, or any range between any two of the above points.

[0057] In one embodiment, the thickness of the interface buffer layer accounts for 1%-10% of the total thickness of the first active material layer, the interface buffer layer, and the second active material layer. Specifically, it can be 1%, 1.5%, 2.0%, 2.5%, 3.0%, 3.5%, 4.0%, 4.5%, 5.0%, 5.5%, 6.0%, 6.5%, 7.0%, 7.5%, 8.0%, 8.5%, 9.0%, 9.5%, 10.0%, or a range between any two of the above points.

[0058] This thickness ratio ensures that the interface buffer layer has sufficient space to form a continuous and dense network structure, so as to exert its strong adhesion and volume expansion stress buffering function for the upper and lower active material layers. At the same time, this ratio effectively limits the proportion of the interface buffer layer in the overall electrode thickness, avoiding excessive sacrifice of the active material layer loading due to excessive buffer layer thickness. Thus, while reducing the electrode expansion rate and maintaining excellent interface stability, it maximizes the volumetric energy density and long-term cycle performance of the battery.

[0059] In one embodiment, the thickness of the interface buffer layer is 1μm-5μm, specifically 1.0μm, 1.29μm, 1.57μm, 1.86μm, 2.14μm, 2.43μm, 2.71μm, 3.00μm, 3.29μm, 3.57μm, 3.86μm, 4.14μm, 4.43μm, 4.71μm, 5.0μm, or any range between any two of the above points.

[0060] In one embodiment, the thickness d1 of the first active material layer is 10μm-30μm, specifically it can be 10.0μm, 11.4μm, 12.9μm, 14.3μm, 15.7μm, 17.1μm, 18.6μm, 20.0μm, 21.4μm, 22.9μm, 24.3μm, 25.7μm, 27.1μm, 28.6μm, 30.0μm, or any range between any two of the above points.

[0061] In one embodiment, the thickness d2 of the second active material layer is 10μm-30μm, specifically it can be 10.0μm, 11.4μm, 12.9μm, 14.3μm, 15.7μm, 17.1μm, 18.6μm, 20.0μm, 21.4μm, 22.9μm, 24.3μm, 25.7μm, 27.1μm, 28.6μm, 30.0μm, or any range between any two of the above points.

[0062] In one embodiment, the first active material layer and / or the second active material layer further include the first lithiation binder.

[0063] Introducing a first lithiation binder into the active material layer creates an additional lithium-ion conduction network within it, further improving the ion transport efficiency of the active material layer to enhance the battery's energy density and cycle performance.

[0064] In one embodiment, the first active material layer and the second active material layer include the first lithiated binder, satisfying the following relationship: m2 > m3 ≥ m1, where m1 is the mass percentage of the first lithiated binder in the first active material layer, m2 is the mass percentage of the first lithiated binder in the interface buffer layer, and m3 is the mass percentage of the first lithiated binder in the second active material layer.

[0065] The content of the first lithiation binder in the three layers varies in a gradient. The highest content (m2) in the interface buffer layer ensures excellent bonding strength and ion transport efficiency, effectively buffering expansion stress. The second active material layer has a higher m3, which maintains good interfacial bonding while building a denser ion-conducting network, ensuring sufficient ion supply for the high-capacity layer during rapid charge and discharge. The pre-lithiation characteristics of PAALi allow the pre-loaded lithium ions on the molecular chain to participate in the formation of the SEI film during the first charge, which helps to form a stable interface phase rich in LiF, thereby reducing irreversible capacity loss and maintaining high energy density. The lowest m1 in the first active material layer maximizes the proportion of active material. The three layers work together to achieve simultaneous improvement in expansion suppression and cycle performance without sacrificing energy density.

[0066] In one embodiment, m2 is 5%-15%, specifically it can be 5.0%, 5.7%, 6.4%, 7.1%, 7.9%, 8.6%, 9.3%, 10.0%, 10.7%, 11.4%, 12.1%, 12.9%, 13.6%, 14.3%, 15.0%, or a range between any two of the above points.

[0067] In one embodiment, m1 is 0%-2%, which can specifically be 0.0%, 0.14%, 0.29%, 0.43%, 0.57%, 0.71%, 0.86%, 1.00%, 1.14%, 1.29%, 1.43%, 1.57%, 1.71%, 1.86%, 2.0%, or a range between any two of the above points.

[0068] In one embodiment, m3 is 0%-3%, which can specifically be 0.0%, 0.21%, 0.43%, 0.64%, 0.86%, 1.07%, 1.29%, 1.50%, 1.71%, 1.93%, 2.14%, 2.36%, 2.57%, 2.79%, 3.0%, or a range between any two of the above points.

[0069] In one embodiment, the average particle size of the first silicon-carbon anode material is greater than the average particle size of the second silicon-carbon anode material.

[0070] The first active material layer uses silicon-carbon anode material with a larger particle size, which can form more inter-particle pores after rolling and enhance the buffering capacity against silicon volume expansion. The second active material layer uses material with a smaller particle size, which can provide a higher specific surface area and compaction density, which is beneficial to improving capacity and rate performance. At the same time, the absolute volume expansion of individual particles is smaller, and the local damage to the surrounding conductive network is less.

[0071] In one embodiment, the average particle size of the first silicon-carbon anode material is 15μm-25μm, specifically 15.0μm, 15.7μm, 16.4μm, 17.1μm, 17.9μm, 18.6μm, 19.3μm, 20.0μm, 20.7μm, 21.4μm, 22.1μm, 22.9μm, 23.6μm, 24.3μm, 25.0μm, or any two of the above-mentioned values.

[0072] In one embodiment, the average particle size of the second silicon-carbon anode material is 5μm-15μm, specifically 5.0μm, 5.7μm, 6.4μm, 7.1μm, 7.9μm, 8.6μm, 9.3μm, 10.0μm, 10.7μm, 11.4μm, 12.1μm, 12.9μm, 13.6μm, 14.3μm, 15.0μm, or any range between any two of the above.

[0073] The average particle size Dv50 of the first and second silicon-carbon anode materials stripped from the anode sheet was measured using a laser particle size analyzer and used as its average particle size.

[0074] In one embodiment, the secondary battery satisfies the following relationship: n2 > n1, where n1 is the mass percentage of the first silicon-carbon anode material in the first active material layer, and n2 is the mass percentage of the second silicon-carbon anode material in the second active material layer.

[0075] During charging, the high-silicon-content second active material layer provides high capacity, but its silicon material undergoes significant volume expansion. The lower low-silicon-content layer has a small expansion rate, forming a mechanical buffer layer that effectively absorbs and buffers the stress generated by the expansion of the second active material layer, preventing stress from directly acting on the current collector interface and avoiding delamination between the active material layer and the current collector. The intermediate interface buffer layer, with its highly conductive network and highly viscoelastic first lithiation binder, provides an efficient channel for the rapid transport of lithium ions between the upper and lower layers. Furthermore, as a stress buffer interface, it effectively dissipates and absorbs shear stress caused by the difference in expansion rates between the upper and lower layers, preventing interlayer separation. Simultaneously, during discharge, the first active material layer releases stored stress, maintaining the stability of the overall electrode structure.

[0076] In one embodiment, the first active material layer and the second active material layer further include a negative electrode conductive agent.

[0077] This application does not impose any particular restrictions on the selection of the negative electrode conductive agent; conventional negative electrode conductive agents in the art can be used. For example, the negative electrode conductive agent may be graphite, acetylene black, graphene, carbon nanotubes (CNTs), etc.

[0078] In one embodiment, the first active material layer includes a first graphite, the second active material layer includes a second graphite, the first graphite includes spherical graphite, and the second graphite includes flake graphite.

[0079] The uniform stacking of spherical graphite can form a stable porous framework, enhancing the mechanical stability of the first active material layer; the flake graphite has better flexibility and interlayer slippage ability, which can better adapt to the drastic volume changes of the high-silicon content layer of the second active material layer and reduce electrical contact failure between active particles.

[0080] In one embodiment, the secondary battery satisfies the following relationship: P1 > P2, where P1 is the porosity of the first active material layer and P2 is the porosity of the second active material layer.

[0081] The high porosity of the first active material layer provides additional buffer space for silicon expansion, which is suitable for effectively releasing stored stress during discharge and maintaining the stability of the overall electrode structure.

[0082] In one embodiment, the secondary battery satisfies: k = [(d1×P1) / (d2×P2)]×(n1 / n2), 0.1≤k≤1; where d1 is the thickness of the first active material layer in μm; d2 is the thickness of the second active material layer in μm; P1 is the porosity of the first active material layer; P2 is the porosity of the second active material layer; n1 is the mass percentage of the first silicon-carbon anode material in the first active material layer; n2 is the mass percentage of the second silicon-carbon anode material in the second active material layer; and k is the balance factor.

[0083] The physical meaning of the above relationship is that when the silicon-carbon content of the first active material layer is low and the expansion is small (i.e., n1 / n2 is small), the effective buffer space (d1×P1) of the first active material layer needs to be increased accordingly to match the larger expansion requirements of the second active material layer. By adjusting the value of k, an adjustable balance can be achieved between buffering capacity and volumetric energy density, ensuring the optimal balance of electrochemical and mechanical performance within a limited electrode volume.

[0084] In one embodiment, n1 is 1.5%-2.5%, specifically it can be 1.50%, 1.57%, 1.64%, 1.71%, 1.79%, 1.86%, 1.93%, 2.00%, 2.07%, 2.14%, 2.21%, 2.29%, 2.36%, 2.43%, 2.50%, or any range between any two of the above points.

[0085] In one embodiment, n2 is 7%-9%, specifically it can be 7.00%, 7.14%, 7.29%, 7.43%, 7.57%, 7.71%, 7.86%, 8.00%, 8.14%, 8.29%, 8.43%, 8.57%, 8.71%, 8.86%, 9.00%, or a range between any two of the above points.

[0086] In one embodiment, P1 is 25%-30%, which can specifically be 25.00%, 25.36%, 25.71%, 26.07%, 26.43%, 26.79%, 27.14%, 27.50%, 27.86%, 28.21%, 28.57%, 28.93%, 29.29%, 29.64%, 30.00%, or a range between any two of the above points.

[0087] In one embodiment, P2 is 20%-25%, specifically it can be 20.00%, 20.36%, 20.71%, 21.07%, 21.43%, 21.79%, 22.14%, 22.50%, 22.86%, 23.21%, 23.57%, 23.93%, 24.29%, 24.64%, 25.00%, or a range between any two of the above points.

[0088] The method for testing the porosity of the first and second active material layers is as follows: 1. Sample preparation: The first or second active material layer is obtained by peeling it off from the negative electrode. The first (or second) active material layer is cut into 2cm × 2cm sample pieces. The apparent volume V of the sample pieces is accurately measured. apparent ( = area × thickness) and mass m.

[0089] 2. Testing Method: The true density ρ of the sample is determined using either mercury intrusion porosimetry or a true density meter (helium displacement method). true Simultaneously, based on the formulation and component densities, its theoretical density ρ is calculated using a weighted average. theory .

[0090] 3. Data Processing: The formula for calculating porosity (P) is: P = (V apparent - m / ρ true ) / V apparent ×100%; Or simplified to: P = (1-ρ apparent / ρ true )×100%; Where m is the mass of the first active material layer (or the second active material layer), ρ apparent The apparent density is given. In one embodiment, the first and second active material layers further include a second binder.

[0091] In one embodiment, the first active material layer includes styrene-butadiene rubber, satisfying the following formula 1: n3 = 0.3% + 0.25 × n1%, where n3 is the mass percentage of styrene-butadiene rubber in the first active material layer, and n1 is the mass percentage of silicon-carbon anode material in the first active material layer.

[0092] In one embodiment, the first active material layer comprises polyacrylic acid, satisfying the following formula 2: n5 = 0.7% + 0.45 × n1%, where n5 is the mass percentage of polyacrylic acid in the first active material layer and n1 is the mass percentage of silicon-carbon anode material in the first active material layer.

[0093] In one embodiment, the second active material layer includes styrene-butadiene rubber, satisfying the following formula 3: n4 = 0.3% + 0.25 × n2%, where n4 is the mass percentage of styrene-butadiene rubber in the second active material layer, and n2 is the mass percentage of silicon-carbon anode material in the second active material layer.

[0094] In one embodiment, the second active material layer comprises polyacrylic acid, satisfying the following formula 4: n6 = 0.7% + 0.45 × n2%, where n6 is the mass percentage of polyacrylic acid in the second active material layer and n2 is the mass percentage of silicon-carbon anode material in the second active material layer.

[0095] In one embodiment, the first active material layer satisfies the following formula 5: m1 = 0.05% × n1 + 0.5%, where n7 is the mass percentage of the first lithiation binder in the first active material layer, and m1 is the mass percentage of the silicon-carbon anode material in the first active material layer.

[0096] In one embodiment, the second active material layer satisfies the following formula 6: m3 = 0.05% × n2 + 0.5%, where m3 is the mass percentage of the first lithiation binder in the second active material layer, and n2 is the mass percentage of the silicon-carbon anode material in the second active material layer.

[0097] The first active material layer and the second active material layer include a first lithiation binder and a second binder. More specifically, the second binder includes styrene-butadiene rubber and / or polyacrylic acid. When Equations 1 to 6 are satisfied, the bonding strength, flexibility and ionic conductivity of each binder system are dynamically matched with the change of silicon content, so as to achieve a balance between the electrochemical performance and mechanical stability of the battery.

[0098] In one embodiment, the secondary battery includes a positive electrode sheet, the positive electrode sheet including a positive current collector and a positive active material layer disposed on at least one surface of the positive current collector; the positive active material layer includes a positive active material, a positive binder and a positive conductive agent.

[0099] This application does not impose any particular restrictions on the selection of the positive electrode active material; conventional positive electrode active materials in the art can be used. For example, the positive electrode active material may be lithium iron phosphate, lithium manganese iron phosphate, lithium cobalt oxide, lithium nickel cobalt manganese oxide, etc.

[0100] This application does not impose any particular restrictions on the selection of the positive electrode binder; conventional positive electrode binders in the art can be used. For example, the positive electrode binder may be polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), sodium polyacrylate (PAANa), carboxymethyl cellulose (CMC), styrene-butadiene rubber (SBR), etc.

[0101] This application does not impose any particular restrictions on the selection of the positive electrode conductive agent; conventional positive electrode conductive agents in the art can be used. For example, the positive electrode conductive agent may be graphite, acetylene black, SuperP, carbon nanotubes, graphene, etc.

[0102] In one embodiment, the secondary battery further includes an electrolyte comprising an organic solvent and a lithium salt.

[0103] This application does not impose any particular restrictions on the selection of organic solvents; conventional organic solvents in the art can be used. For example, the organic solvent may be ethylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, etc.

[0104] This application does not impose any particular restrictions on the selection of lithium salts, and conventional lithium salts in the art can be used. For example, the lithium salt may be lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethylsulfonyl)imide, etc.

[0105] In one embodiment, the method for preparing the secondary battery includes the following steps: (1) Preparation of positive electrode sheet: The positive active material, positive conductive agent and positive binder are mixed and added to a solvent to obtain a positive slurry. The positive slurry is coated on at least one surface of the positive current collector, and then dried, rolled, slit and cut to obtain a positive electrode sheet. (2) Preparation of negative electrode sheet: The raw materials of the first active material layer, the second active material layer and the interface buffer layer are mixed with solvent evenly to obtain the first negative electrode slurry, the second negative electrode slurry and the interface buffer layer slurry respectively; the first negative electrode slurry, the interface buffer layer slurry and the second negative electrode slurry are coated on at least one surface of the negative electrode current collector in sequence, and then dried, rolled, slit and cut to obtain the negative electrode sheet; (3) Preparation of electrolyte: Lithium salt and additives are added to an organic solvent to obtain an electrolyte; (4) Preparation of secondary battery: The positive electrode, negative electrode, separator and other components are assembled and then subjected to processes such as winding, hot pressing, super welding, core assembly, casing, baking, liquid injection, high temperature immersion, formation, aging, sealing and capacity testing to obtain secondary battery.

[0106] In one embodiment, in step (1), the solvent includes N-methylpyrrolidone.

[0107] In one embodiment, in step (2), the solvent includes water.

[0108] On the other hand, this application also provides an electrical device comprising the aforementioned secondary battery.

[0109] For example, the aforementioned electrical equipment may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but are not limited thereto.

[0110] Example 1 This application provides a secondary battery, the preparation method of which includes the following steps: (1) Preparation of PAALi: It was prepared by partially neutralizing polyacrylic acid (PAA) and lithium hydroxide (LiOH) in an aqueous solution, with the degree of neutralization controlled at 50% (the mass ratio of PAA to LiOH is approximately 100:29), to obtain an aqueous solution with a PAALi solid content of 15 wt%.

[0111] (2) Preparation of negative electrode sheet: The raw materials for the first active material layer, interface buffer layer, and second active material layer of the negative electrode sheet, as listed in Table 1-2, were respectively mixed with deionized water to obtain a first negative electrode slurry, an interface buffer layer slurry, and a second negative electrode slurry, each with a solid content of 50 wt%. If CMC is present in the raw materials, it must be pre-dissolved in deionized water to form a gel before mixing with other raw materials. PAA and SBR were added in emulsion form during the later stages of mixing. PAALi was added as a 15 wt% aqueous solution before the addition of PAA to ensure uniform dispersion in the slurry system.

[0112] A three-layer slot extrusion coating machine was used to coat the first negative electrode slurry on both sides of a 4.5 μm thick copper foil, obtaining a wet film of the first active material layer. Immediately afterward, an interface buffer layer slurry was coated onto this wet film, obtaining a wet film of the interface buffer layer. Subsequently, the second negative electrode slurry was immediately coated, obtaining a wet film of the second active material layer, while maintaining the surface density of the first and second active material layers at 66 g / 1540.25 mm². 2 The areal density of the interface buffer layer is controlled at 4g / 1540.25mm. 2 The coated electrode is dried at 80°C for a specified time to form a stable porous structure, resulting in an unrolled electrode.

[0113] Then roll-press to a compaction density of 1.6 g / cm³. 3 The negative electrode sheet is obtained by slitting and cutting. A schematic diagram of the first active material layer, interface buffer layer, and second active material layer on one side of the negative electrode current collector in this negative electrode sheet is shown below. Figure 1 As shown.

[0114] (2) Preparation of the positive electrode sheet: The positive electrode active material (lithium iron phosphate), positive electrode conductive agent (carbon black), and positive electrode binder (PVDF) were mixed in a weight ratio of 97:0.7:2.3. Then, N-methylpyrrolidone (NMP) was added and thoroughly mixed to obtain a positive electrode slurry with a solid content of 65%. The positive electrode slurry was then coated on both sides of a 15μm thick carbon-coated aluminum foil (with a single-sided carbon layer thickness of 1μm), with a coating weight of 199g / m². 2 After coating, the electrode is dried, rolled, slit and cut to obtain the positive electrode.

[0115] (3) Preparation of electrolyte: Ethylene carbonate, ethyl methyl carbonate, and dimethyl carbonate were mixed in a mass ratio of 1:1:1, then lithium hexafluorophosphate was added, and after thorough mixing, vinylene carbonate was added as an additive. Based on the mass of the electrolyte, the mass content of lithium hexafluorophosphate was 12%, and the mass content of vinylene carbonate was 0.5%. (4) Preparation of secondary batteries: The positive electrode, negative electrode, separator (polyethylene film) and other battery components are assembled and then processed through shaping, baking, packaging, liquid injection, formation and capacity testing to obtain a secondary battery.

[0116] Example 2-3 This application provides a secondary battery. The difference between the preparation method of the secondary battery and that of Example 1 is that the content of the first silicon carbide material n1 and the content of spherical graphite in the first active material layer are changed, as shown in the parameters in Tables 1-3.

[0117] Examples 4-5 This application provides a secondary battery. The difference between the preparation method of the secondary battery and that of Example 1 is that the average particle size of the first silicon-carbon material is changed to achieve the parameters in Tables 1-3.

[0118] Examples 6-8 This application provides a secondary battery. The difference between the preparation method of the secondary battery and that of Example 1 is that the content of PAALi (m1) and PAA in the first active material layer is changed to achieve the parameters in Tables 1-3.

[0119] Examples 9-10 This application provides a secondary battery. The difference between the preparation method of the secondary battery and that of Example 1 is that the amount of coating of the first negative electrode slurry is adjusted and the thickness d1 of the first active material layer is changed to achieve the parameters in Table 1-3.

[0120] Examples 11-14 This application provides a secondary battery. The difference between the preparation method of the secondary battery and that of Example 1 is that the content of PAALi (m2) and the content of carbon nanotubes in the interface buffer layer are changed to achieve the parameters in Tables 1-3.

[0121] Example 15 This application provides a secondary battery. The difference between the preparation method of the secondary battery and that of Example 1 is that the PAALi in the interface buffer layer is replaced with an equal amount of CMCLi to achieve the parameters in Tables 1-3; and the preparation method of CMCLi in this embodiment is as follows: Sodium carboxymethyl cellulose (CMC-Na) was dissolved in deionized water to prepare a 5 wt% solution. An excess of 1 M hydrochloric acid (HCl) solution was added, and the solution was acidified by stirring at room temperature for 4 hours to convert the -COONa groups to -COOH. The acidified CMC solution was then placed in a dialysis bag (molecular weight cutoff 10000 Da) and dialyzed in deionized water for 72 hours to remove Na⁺ and Cl⁻ ions. Subsequently, 1 M lithium hydroxide (LiOH) solution was slowly added dropwise to the dialyzed solution to adjust the pH to 7-8, allowing the -COOH groups to react equimolarly to form -COOLi. Finally, the neutralized solution was concentrated by rotary evaporation at 60 °C and freeze-dried to obtain powdered CMC-Li.

[0122] Example 16 This application provides a secondary battery. The difference between the preparation method of the secondary battery and that of Example 1 is that SBR is not added to the interface buffer layer, and the content of PAALi m2 is 10%, so as to achieve the parameters in Table 1-3.

[0123] Example 17 This application provides a secondary battery. The difference between the preparation method of the secondary battery and that of Example 1 is that the SBR in the interface buffer layer is replaced with CMC in equal amounts to achieve the parameters in Table 1-3.

[0124] Examples 18-21 This application provides a secondary battery. The difference between the preparation method of the secondary battery and that of Example 1 is that the type of conductive agent in the first active material layer, the interface buffer layer, or the second active material layer is changed to achieve the parameters in Tables 1-3.

[0125] Examples 22-23 This application provides a secondary battery. The difference between the preparation method of the secondary battery and that of Example 1 is that the coating amount of the interface buffer layer slurry is adjusted and the areal density of the interface buffer layer is changed to achieve the parameters in Tables 1-3.

[0126] Examples 24-25 This application provides a secondary battery. The difference between the preparation method of the secondary battery and that of Example 1 is that the coating amount of the interface buffer layer slurry is adjusted and the thickness of the interface buffer layer is changed to achieve the parameters in Table 1-3.

[0127] Examples 26-28 This application provides a secondary battery. The difference between the preparation method of the secondary battery and that of Example 1 is that the average particle size of the second silicon-carbon material is changed to achieve the parameters in Tables 1-3.

[0128] Examples 29-30 This application provides a secondary battery. The difference between the preparation method of the secondary battery and that of Example 1 is that the content of the second silicon-carbon material n2 and the content of flake graphite in the second active material layer are changed to achieve the parameters in Tables 1-3.

[0129] Examples 31-32 This application provides a secondary battery. The difference between the preparation method of the secondary battery and that of Example 1 is that the content of PAALi (m3) and PAA in the second active material layer is changed to achieve the parameters in Tables 1-3.

[0130] Examples 33-34 This application provides a secondary battery. The difference between the preparation method of the secondary battery and that of Example 1 is that the amount of coating of the second negative electrode slurry is adjusted and the thickness d2 of the second active material layer is changed to achieve the parameters in Tables 1-3.

[0131] Comparative Example 1 This application provides a secondary battery in a comparative example. The difference between the preparation method of the secondary battery and that of Example 1 is that no interface buffer layer is prepared to achieve the parameters in Tables 1-3.

[0132] Comparative Example 2 This application provides a secondary battery in a comparative example. The difference between the preparation method of the secondary battery and that of Example 1 is that the PAALi in the interface buffer layer is replaced by an equal amount of PAA to achieve the parameters in Tables 1-3.

[0133] Comparative Example 3 This application provides a secondary battery in a comparative example. The difference between the preparation method of the secondary battery and that of Example 1 is that the first active material layer is not prepared, and the thickness of the second active material layer is 54 μm, that is, the first active material layer is missing, so as to achieve the parameters in Table 1-3.

[0134] Comparative Example 4 This application provides a secondary battery in a comparative example. The difference between the preparation method of the secondary battery and that of Example 1 is that a second active material layer is not prepared, and the thickness of the first active material layer is 54 μm, that is, the second active material layer is missing, so as to achieve the parameters in Table 1-3.

[0135] Unless otherwise specified, all raw materials used in this application are existing materials. The first and second silicon-carbon materials with different average particle sizes in the examples and comparative examples can both be obtained using conventional methods. Both types of silicon-carbon materials are granular or spherical, and the silicon content in the first and second silicon-carbon materials is 10 wt.% and 15 wt.%, respectively. The flake graphite in the examples and comparative examples has an average particle size of 15 μm, and the spherical graphite has an average particle size of 20 μm.

[0136] The performance testing of secondary batteries includes the following: First Coulomb efficiency test: In a 25°C constant temperature chamber, the secondary batteries prepared in the examples and comparative examples were charged at a constant current of 1C to 3.65V, then charged at a constant voltage until the current <0.05C, and allowed to stand for 5 minutes. They were then discharged at 1C to 2.5V. The initial charge capacity was C. charge The initial discharge capacity is C. discharge Therefore, the initial Coulomb efficiency ICE = C. discharge / C charge ×100%.

[0137] Cyclic performance test: In constant temperature chambers at 25℃ and 45℃, the capacitor is charged at a constant current of 4C to 3.65V, then charged at a constant voltage of 3.65V until the current is less than 0.05C. After resting for 5 minutes, it is discharged at a current of 1C to 2.5V. This constitutes one cycle. The discharge capacity C1 of the first cycle and the discharge capacity C of the 500th cycle are recorded. 500 Capacity retention rate at 500th lap = C 500 / C1×100%.

[0138] Volume expansion rate test: At 25℃, the center thickness of the fresh battery at 50% state of charge (SOC) is first measured with a micrometer and recorded as T0. Then, the above-mentioned cyclic test is performed. After 2000 cycles, the center thickness of the battery in a fully discharged state is measured and recorded as T1. The volume expansion rate is approximately (T1-T0) / T0×100%.

[0139] In Tables 1-3 below, the content of each component is expressed as a percentage by mass.

[0140] Table 1 Table 2 Table 3 Table 4 As can be seen from the above Examples 1-34 and Comparative Examples 1-4, the negative electrode sheet of the secondary battery of this application has a three-layer structure of a first active material layer, an interface buffer layer and a second active material layer, and the interface buffer layer contains a lithium-based binder, which enables the secondary battery to achieve high energy density, cycle stability and low volume expansion.

Claims

1. A secondary battery characterized by comprising: Includes a negative electrode sheet, wherein the negative electrode sheet comprises: Negative electrode current collector; A first active material layer is disposed on at least one side of the negative electrode current collector, and the first active material layer comprises a first silicon-carbon negative electrode material; An interface buffer layer is disposed on the side of the first active material layer away from the negative electrode current collector. The interface buffer layer contains a first lithiation binder, and the elastic modulus of the buffer layer is 0.1 GPa-2 GPa. A second active material layer is disposed on the side of the buffer layer away from the negative electrode current collector, and the second active material layer contains a second silicon-carbon negative electrode material.

2. The secondary battery according to claim 1, characterized by The peel strength between the interface buffer layer and the first active material layer is 8N / m-25N / m; and / or the interfacial buffer layer has a lithium ion conductivity of 1 x 10 -5 -8 x 10 -4 S / cm at 25 °C. and / or the areal density of the interface buffer layer is 3 g / 15 40.25 mm 2 - 10 g / 15 40.25 mm 2 .

3. The secondary battery according to claim 1, characterized by The thickness of the interface buffer layer accounts for 1%-10% of the total thickness of the first active material layer, the interface buffer layer, and the second active material layer.

4. The secondary battery according to claim 1, characterized by The first active material layer and / or the second active material layer further include the first lithium binder.

5. The secondary battery according to claim 4, characterized by The first active material layer and the second active material layer include the first lithiated binder, satisfying the following relationship: m2>m3≥m1, where m1 is the mass percentage of the first lithiated binder in the first active material layer, m2 is the mass percentage of the first lithiated binder in the interface buffer layer, and m3 is the mass percentage of the first lithiated binder in the second active material layer.

6. The secondary battery according to claim 1, characterized by At least one of the following AD conditions must be met: A. The first lithium-ionized adhesive includes at least one of lithium-ionized polyacrylic acid and lithium carboxymethyl cellulose; B. The interface buffer layer further includes a second adhesive, which includes at least one of styrene-butadiene rubber, polyacrylic acid, carboxymethyl cellulose, sodium alginate, polyvinylidene fluoride, polyimide, and polypyrrole copolymer. C. The average particle size of the first silicon-carbon anode material is greater than the average particle size of the second silicon-carbon anode material. D. The first active material layer includes a first graphite, and the second active material layer includes a second graphite. The first graphite includes spherical graphite, and the second graphite includes flake graphite.

7. The secondary battery according to claim 6, characterized by The interface buffer layer further includes a conductive agent, which includes at least one of zero-dimensional conductive agents, one-dimensional conductive agents, and two-dimensional conductive agents.

8. The secondary battery according to claim 6, characterized by The average particle size of the first silicon-carbon anode material is 15μm-25μm, and the average particle size of the second silicon-carbon anode material is 5μm-15μm.

9. The secondary battery according to claim 1, characterized by The following relationship is satisfied: n2 > n1, where n1 is the mass percentage of the first silicon-carbon anode material in the first active material layer, and n2 is the mass percentage of the second silicon-carbon anode material in the second active material layer.

10. The secondary battery according to claim 1, characterized by The following relationship must be satisfied: P1 > P2, where, P1 is the porosity of the first active material layer, and P2 is the porosity of the second active material layer.

11. The secondary battery according to claim 1, characterized by satisfy: k=[(d1×P1) / (d2×P2)]×(n1 / n2), 0.1≤k≤1; Wherein, d1 is the thickness of the first active material layer in μm; d2 is the thickness of the second active material layer in μm; P1 is the porosity of the first active material layer; P2 is the porosity of the second active material layer; n1 is the mass percentage of the first silicon-carbon anode material in the first active material layer; and n2 is the mass percentage of the second silicon-carbon anode material in the second active material layer.

12. An electrical device, characterized by It includes the secondary battery as described in any one of claims 1-11.