A battery cell, a battery device, and an electric device
By employing a layered coating negative electrode design in lithium-ion batteries and utilizing large-particle-size binders to enhance the adhesion of silicon-based materials, the volume expansion problem of silicon-based materials during fast charging is solved, thereby improving the battery's cycle performance and fast charging capability.
Patent Information
- Application Number
- CN202510665269.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-22
- Publication Date
- 2026-11-24
AI Technical Summary
Silicon-based anode materials experience severe volume expansion during the fast charging process of lithium-ion batteries, leading to accelerated degradation of battery cell lifespan and cracking of casing welds, thus affecting the battery's fast charging cycle capacity retention rate.
The negative electrode sheet adopts a layered coating design. The first negative electrode active layer and the second negative electrode active layer contain graphite material and silicon-based material, respectively. The second negative electrode active layer has a high silicon content and uses a second binder with an average particle size of 0.3μm~0.7μm to enhance adhesion and cohesion and reduce expansion force.
It improves the cycle performance of individual battery cells under fast charging conditions, reduces the full-charge rebound of the negative electrode, and enhances the battery's fast charging capability and energy density.
Smart Images

Figure CN123162136A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of battery technology, and in particular to a battery cell, a battery device, and an electrical device. Background Technology
[0002] With the development and advancement of lithium-ion batteries, increasingly higher requirements are being placed on their energy density and safety performance. Silicon-based anodes, due to their high theoretical specific capacity, are considered one of the ideal choices for high-energy-density rechargeable batteries.
[0003] During the charging and discharging process of a battery, silicon-based materials will undergo significant volume expansion, which can lead to accelerated degradation of the battery cell's lifespan and even cracking of the casing welds. In particular, under fast charging conditions, the volume expansion of silicon-based materials is aggravated, which will cause the battery cell's fast charging cycle capacity retention rate to decay even faster. Summary of the Invention
[0004] To improve the cycle performance of a battery cell under fast charging conditions, this application provides a battery cell, a battery device, and an electrical device.
[0005] The first aspect of this application provides a battery cell including a negative electrode sheet, the negative electrode sheet including a negative current collector and a negative active layer disposed on at least one side of the negative current collector, the negative active layer including a first negative active layer and a second negative active layer, the first negative active layer being located between the negative current collector and the second negative active layer, the negative active layer including a negative active material, the negative active material including a graphite material and a silicon-based material, the silicon element mass content in the second negative active layer being greater than the silicon element mass content in the first negative active layer, and the ratio of the silicon element mass in the second negative active layer to the silicon element mass in the negative active layer being greater than or equal to 50%, the second negative active layer further including a second binder, the average particle size of the second binder being in the range of 0.3 μm to 0.7 μm.
[0006] This application employs a first and second negative electrode active layer to layer silicon-based and graphite materials. The second negative electrode active layer, located further away from the negative electrode current collector, contains a higher proportion of silicon-based material. During charging, the silicon-based material expands due to lithium insertion, and shrinks in volume after delithiation during discharging. A second binder with an average particle size ranging from 0.3 μm to 0.7 μm is used in the second negative electrode active layer. The larger particle size of this second binder makes it less prone to floating after slurry coating, resulting in more uniform dispersion within the second negative electrode active layer. Furthermore, the larger particle size provides stronger adhesion and binding to the silicon-based material in the second negative electrode active layer, improving its cohesion and adhesion, reducing its expansion force, and thus minimizing the rebound during full charge of the negative electrode sheet in fast charging, thereby improving the cycle performance of the battery cell under fast charging conditions. Moreover, the increased silicon-based material in the second negative electrode active layer reduces the lithium-ion diffusion path, further enhancing the fast-charging capability of the battery cell.
[0007] In any embodiment of the first aspect, the first negative electrode active layer further includes a first binder, and the first binder and the second binder satisfy at least one of the following conditions:
[0008] (1) The average particle size of the second binder is greater than or equal to the average particle size of the first binder;
[0009] (2) The weight-average molecular weight of the second adhesive is greater than or equal to the weight-average molecular weight of the first adhesive;
[0010] (3) The mass content of the second binder in the second negative electrode active layer is more than 1.5 times the mass content of the first binder in the first negative electrode active layer; optionally, the mass content of the second binder in the second negative electrode active layer is more than 2 times the mass content of the first binder in the first negative electrode active layer.
[0011] In any embodiment of the first aspect, the average particle size of the first binder is in the range of 0.01 μm to 0.6 μm. When the average particle size of the first binder is smaller than the average particle size of the second binder and is within the above range, the first binder sufficiently fills the gaps in the negative electrode active material of the first negative electrode active layer, bonding the negative electrode active material therein, reducing the interfacial resistance between the negative electrode active materials, and improving the kinetic performance of the battery cell.
[0012] In any embodiment of the first aspect, the weight-average molecular weight of the second adhesive is 2 × 10⁻⁶. 5 ~5×10 5 Within the range, and / or, the weight-average molecular weight of the first adhesive is 1 × 10⁻⁶. 5 ~2×10 5Within the specified range. By controlling the above-mentioned weight-average molecular weight, the first binder and the second binder can each exert their bonding and binding effects on the negative electrode active material, while also facilitating the efficient and uniform dispersion of the binder in the slurry during preparation.
[0013] In any embodiment of the first aspect, the first binder has a mass content of 0.5% to 3% in the first negative electrode active layer, and / or the second binder has a mass content of 1.5% to 7% in the second negative electrode active layer.
[0014] In any embodiment of the first aspect, the first adhesive and the second adhesive each independently contain hydrophilic groups; optionally, the hydrophilic groups include at least one of sulfonic acid groups, phosphate groups, hydroxyl groups, carboxyl groups, amide groups, amino groups, aldehyde groups, carbonyl groups, cyano groups, and acid anhydrides; optionally, the first adhesive and the second adhesive each independently include one or more of polystyrene-butadiene copolymers and their modifications, polystyrene-acrylates and their modifications, polyacrylate copolymers and their modifications, butadiene-acrylonitrile copolymers and their modifications, polytetrafluoroethylene and its modifications, polyvinylidene fluoride and its modifications, styrene-butadiene rubber (SBR), and acrylonitrile-butadiene-styrene copolymer (ABS).
[0015] In any embodiment of the first aspect, the silicon content in the second negative electrode active layer is 10% to 70% by mass.
[0016] In any embodiment of the first aspect, the ratio of the mass content of the second binder to the mass content of silicon in the second negative electrode active layer is 0.07 to 0.35. This allows for adjustment of the amount of the second binder based on the mass content of silicon, thereby minimizing the expansion force of the second negative electrode active layer while avoiding excessive introduction of the second binder.
[0017] In any embodiment of the first aspect, the silicon content in the first negative electrode active layer is 0% to 20% by mass.
[0018] In any embodiment of the first aspect, the thickness ratio of the first negative electrode active layer to the second negative electrode active layer is 9:1 to 1:9, and the thickness of the first negative electrode active layer is 20-200 μm.
[0019] In any embodiment of the first aspect, the silicon-based material includes one or more of elemental silicon, silicon-carbon composite materials, or silicon-oxygen composites.
[0020] In any embodiment of the first aspect, the mass content of silicon element in the silicon-based material is 30%-70%.
[0021] In any embodiment of the first aspect, the silicon-based material includes a silicon-carbon composite material, which satisfies one or more of the following characteristics:
[0022] (1) The silicon-carbon composite material includes porous carbon and crystalline silicon located in the pores and on the surface of the porous carbon, and optionally, the porous carbon is hard carbon;
[0023] (2) The silicon-carbon composite material also includes a carbon-containing coating layer, which is located on the surface of porous carbon and / or crystalline silicon;
[0024] (3) The average particle size of the silicon-carbon composite material is 2μm-15μm, and can be selected as 7μm-11μm;
[0025] (4) The powder resistivity of silicon-carbon composite material at 8 MPa is 4 Ω·cm - 17 Ω·cm;
[0026] (5) The BET specific surface area of the silicon-carbon composite material is 1.0 m². 2 / g - 6.7 m 2 / g.
[0027] In any embodiment of the first aspect, the negative electrode active layer further includes a conductive agent, which includes one or more of carbon black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0028] In any embodiment of the first aspect, the mass content of the conductive agent in the first negative electrode active layer is 0.05%-1%, and the mass content of the conductive agent in the second negative electrode active layer is 0.05%-2%. Since the first negative electrode active layer uses graphite as the main negative electrode active material, it has good conductivity. This allows it to meet the conductivity requirements under fast charging conditions even with a relatively low conductive agent content, thus allowing for an appropriate increase in the graphite material content to improve the energy density of this layer. Using a relatively large amount of conductive agent in the second negative electrode active layer helps improve its conductivity, thereby contributing to improved charging capability.
[0029] In any embodiment of the first aspect, the conductive agent in the second negative electrode active layer includes carbon black and carbon nanotubes, wherein the mass ratio of carbon black to carbon nanotubes is 6:4-9:1, and optionally 8:2-8.5:1.5.
[0030] In any embodiment of the first aspect, the graphite material includes a first graphite material and a second graphite material, the first graphite material is disposed in the first negative electrode active layer, and the second graphite material is disposed in the second negative electrode active layer, wherein the first graphite material and the second graphite material satisfy at least one of the following conditions:
[0031] (1) The average particle size of the second graphite material is lower than that of the first graphite material;
[0032] (2) The tap density of the second graphite material is greater than that of the first graphite material;
[0033] (3) The first graphite material and the second graphite material are each independently selected from at least one of artificial graphite and natural graphite; optionally, the first graphite material includes natural graphite and the second graphite material includes artificial graphite. The above-mentioned small particle size and / or low tap density second graphite material shortens the ion transport path in the second negative electrode active layer, thereby improving the dynamic performance of the battery cell and taking into account high energy density.
[0034] In any embodiment of the first aspect, the negative electrode sheet includes a base coating layer disposed between the negative electrode current collector and the negative electrode active layer, and the base coating layer includes a base coating conductive agent and a base coating binder.
[0035] In any embodiment of the first aspect, the battery cell further includes a positive electrode sheet, the positive electrode sheet including a positive current collector and a positive active layer disposed on at least one side of the positive current collector, the positive active layer including a positive active material, the positive active material including a nickel-containing lithium transition metal oxide or a lithium phosphate.
[0036] In any embodiment of the first aspect, the nickel-containing lithium transition metal oxide includes lithium-containing nickel-cobalt-manganese oxide and lithium-containing nickel-cobalt-aluminum oxide.
[0037] In any embodiment of the first aspect, the nickel-containing nickel-cobalt-manganese oxide includes the compound Li a Ni b Co c Mn d M e O 2-f M includes one or more elements selected from Al, Fe, Ti, Mg, Zr, Cr, Ga, Cu, Zn, Nb, and B.
[0038] a can be any value in the range of 0.7-1.1, and can be any value in the range of 0.8-1.1;
[0039] b can be any value in the range of 0.45-0.97, and can be any value in the range of 0.8-0.97, and can be further selected as any value in the range of 0.85-0.95;
[0040] c can be any value in the range of 0.02-0.25, and can be any value in the range of 0.02-0.2;
[0041] d can be any value in the range of 0.05-0.5, and can be any value in the range of 0.05-0.48;
[0042] e can be any value in the range of 0 to 0.2, and can be any value in the range of 0.001 to 0.2;
[0043] f is any value in the range of 0-0.3, and can be any value in the range of 0-0.2.
[0044] In any embodiment of the first aspect, the positive electrode active material includes primary particles and / or secondary particles, and optionally, based on the total cross-sectional area of the positive electrode active material, the cross-sectional area of the primary particles accounts for more than 30%.
[0045] The second aspect of this application provides a battery device comprising a battery cell provided in any of the embodiments of the first aspect described above.
[0046] The third aspect of this application provides an electrical device, including a battery cell provided in any embodiment of the first aspect and a battery device provided in any embodiment of the second aspect, wherein the battery cell or the battery device is used to store or provide electrical energy. Attached Figure Description
[0047] To more clearly illustrate the technical solutions of the embodiments of this application, the drawings used in the embodiments of this application will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on the drawings without creative effort.
[0048] Figure 1 This is a schematic diagram of a battery cell according to one embodiment of this application.
[0049] Figure 2 yes Figure 1 An exploded view of a battery cell according to one embodiment of this application is shown.
[0050] Figure 3 This is a schematic diagram of a battery module according to one embodiment of this application.
[0051] Figure 4 This is a schematic diagram of a battery pack according to one embodiment of this application.
[0052] Figure 5 yes Figure 4 An exploded view of a battery pack according to one embodiment of this application is shown.
[0053] Figure 6 This is a schematic diagram of an electrical device that uses a secondary battery as a power source according to one embodiment of this application.
[0054] The accompanying drawings are not drawn to scale.
[0055] Explanation of reference numerals in the attached figures:
[0056] 1 Battery pack; 2 Upper housing; 3 Lower housing; 4 Battery module; 5 Battery cell; 51 Casing; 52 Electrode assembly; 53 End cap. Detailed Implementation
[0057] The embodiments of this application will be described in further detail below with reference to the accompanying drawings and examples. The detailed description of the following embodiments and the accompanying drawings are used to illustrate the principles of this application by way of example, but should not be used to limit the scope of this application, that is, this application is not limited to the described embodiments.
[0058] The following detailed description, with appropriate reference to the accompanying drawings, specifically discloses embodiments of the battery cell, battery device, and power-consuming device of this application. However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repetitive descriptions of practically identical structures may be omitted. This is to avoid unnecessarily lengthy descriptions and to facilitate understanding by those skilled in the art. Furthermore, the accompanying drawings and the following description are provided to enable those skilled in the art to fully understand this application and are not intended to limit the subject matter of the claims.
[0059] The "range" disclosed in this application is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a specific parameter, it is expected that ranges of 60-110 and 80-120 are also included. Furthermore, if minimum range values of 1 and 2 are listed, and if maximum range values of 3, 4, and 5 are listed, then the following ranges are all expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this application, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0-5" have been listed in this article; "0-5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is stated as an integer ≥2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0060] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions.
[0061] Unless otherwise specified, all technical features and optional technical features of this application may be combined to form new technical solutions.
[0062] Unless otherwise specified, all steps in this application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the mention that the method may also include step (c) indicates that step (c) may be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.
[0063] Unless otherwise specified, the terms "comprising" and "including" as used in this application are open-ended. For example, "comprising" and "including" may mean that other components not listed may also be included or contained.
[0064] Unless otherwise specified, the term "or" is inclusive in this application. For example, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0065] [Battery cell]
[0066] In this embodiment of the application, the battery cell can be a secondary battery, which refers to a battery cell that can be recharged to activate the active materials and continue to be used after the battery cell has been discharged.
[0067] The battery cell can be a lithium-ion battery, sodium-ion battery, sodium-lithium-ion battery, lithium metal battery, sodium metal battery, lithium-sulfur battery, magnesium-ion battery, nickel-metal hydride battery, nickel-cadmium battery, lead-acid battery, etc., and the embodiments of this application are not limited to this.
[0068] Typically, a battery cell includes a positive electrode, a negative electrode, a separator, and an electrolyte. During charging and discharging, active ions (such as lithium ions) repeatedly insert and extract between the positive and negative electrodes. The separator, located between the positive and negative electrodes, primarily prevents short circuits while allowing active ions to pass through. The electrolyte, also located between the positive and negative electrodes, mainly conducts the active ions.
[0069] As analyzed in the background section of this application, during fast charging, the volume expansion of silicon-based materials is more severe, leading to a significant decrease in the fast charging cycle capacity retention rate of individual battery cells. To address this issue, one embodiment of this application provides a negative electrode sheet, which includes a negative current collector and a negative active layer disposed on at least one side of the negative current collector. The negative active layer includes a first negative active layer and a second negative active layer, with the first negative active layer located between the negative current collector and the second negative active layer. The negative active layer includes a negative active material, which includes graphite material and silicon-based material. The silicon content in the second negative active layer is greater than that in the first negative active layer, and the ratio of the mass of silicon in the second negative active layer to the mass of silicon in the negative active layer is greater than or equal to 50%. The second negative active layer also includes a second binder, the average particle size of which is in the range of 0.3 μm to 0.7 μm.
[0070] This application employs a first and second negative electrode active layer to layer silicon-based and graphite materials. The second negative electrode active layer, located further away from the negative electrode current collector, contains a higher proportion of silicon-based material. During charging, the silicon-based material expands due to lithium insertion, and shrinks in volume after delithiation during discharging. A second binder with an average particle size ranging from 0.3 μm to 0.7 μm is used in the second negative electrode active layer. The larger particle size of this second binder makes it less prone to floating after slurry coating, resulting in more uniform dispersion within the second negative electrode active layer. Furthermore, the larger particle size provides stronger adhesion and binding to the silicon-based material in the second negative electrode active layer, improving its cohesion and adhesion, reducing its expansion force, and thus minimizing the rebound during full charge of the negative electrode sheet in fast charging, thereby improving the cycle performance of the battery cell under fast charging conditions. Moreover, the increased silicon-based material in the second negative electrode active layer reduces the lithium-ion diffusion path, further enhancing the fast-charging capability of the battery cell.
[0071] The test method for the average particle size of the second binder mentioned above is as follows:
[0072] After discharging the battery cell to 0% SOC, disassemble the negative electrode sheet and scrape off the powder of the second negative electrode active layer. Using deionized water or ethanol as the dispersion medium, take 10-20 mg of the second negative electrode active layer powder, add 5-10 mL of dispersant, and sonicate for 10-30 minutes (power recommended ≤100 W) until the slurry is in a uniform suspension, a light-colored dispersion is visible to the naked eye, and there is no sediment. This is the sample to be tested. Dilute the sample to a transmittance of 0.1-1 mg / mL. Calibrate the DLS instrument using standard particles (such as polystyrene microspheres), and test the diluted sample using a dynamic light scattering instrument. Repeat the test 5 times and take the average value as the average particle size.
[0073] The method for determining the ratio of the mass of silicon in the second negative electrode active layer to the mass of silicon in the negative electrode active layer is as follows:
[0074] For any region of the negative electrode sheet, the second negative electrode active layer is separated by a scraping method, and the mass of the second negative electrode active layer is weighed and recorded as M2; the first negative electrode active layer below the scraped second negative electrode active layer is collected, and the mass of the first negative electrode active layer is weighed and recorded as M1; the coating weight ratio of the first negative electrode active layer and the second negative electrode active layer is calculated based on this weight as s = M2 / M1.
[0075] Weigh out m2 grams of the second negative electrode material and use ICP-OES to test the silicon content in m2 grams of the second negative electrode material, denoted as W2; weigh out m1 grams of the first negative electrode material (m1=m2 / s) and use ICP-OES to test the silicon content in m1 grams of the first negative electrode material, denoted as W1. Therefore, calculate the ratio of the mass of silicon in the second negative electrode active layer to the mass of silicon in the negative electrode active layer: = m2×W2 / (m1×W1+m2×W2).
[0076] In some embodiments, the ratio of the mass of silicon in the second negative electrode active layer to the mass of silicon in the negative electrode active layer is greater than or equal to 60%, 70%, 80%, or 90%, or even 100%.
[0077] In some embodiments, the average particle size of the second binder is greater than or equal to the average particle size of the first binder.
[0078] The method for testing the average particle size of the first binder is the same as described above.
[0079] When the average particle size of the second binder is greater than that of the first binder, the second binder achieves stronger bonding and binding of the silicon-based material in the second negative electrode active layer.
[0080] In some embodiments, the average particle size of the first binder is in the range of 0.01 μm to 0.6 μm, such as 0.01 μm, 0.05 μm, 0.1 μm, 0.2 μm, 0.3 μm, 0.4 μm, 0.5 μm, or 0.6 μm, or any combination of two of the above values. When the average particle size of the first binder is smaller than the average particle size of the second binder and is within the above range, the first binder sufficiently fills the gaps in the negative electrode active material of the first negative electrode active layer, bonding the negative electrode active material therein, reducing the interfacial resistance between the negative electrode active materials, and improving the kinetic performance of the battery cell.
[0081] In some embodiments, the weight-average molecular weight of the second binder is greater than or equal to that of the first binder. When the weight-average molecular weight of the second binder is greater than that of the first binder, the second binder achieves stronger adhesion and confinement of the silicon-based material in the second negative electrode active layer.
[0082] In some embodiments, the weight-average molecular weight of the second adhesive is 2 × 10⁻⁶. 5 ~5×10 5 Within the range, and / or, the weight-average molecular weight of the first adhesive is 1 × 10⁻⁶. 5 ~2×10 5 Within the specified range. By controlling the above-mentioned weight-average molecular weight, the first binder and the second binder can each exert their bonding and binding effects on the negative electrode active material, while also facilitating the efficient and uniform dispersion of the binder in the slurry during preparation.
[0083] In some embodiments, the mass content of the second binder in the second negative electrode active layer is more than 1.5 times the mass content of the first binder in the first negative electrode active layer; alternatively, the mass content of the second binder in the second negative electrode active layer is more than 2 times the mass content of the first binder in the first negative electrode active layer.
[0084] In some implementations, controlling the use of a higher mass content of the second binder in the second negative electrode active layer can achieve more thorough bonding and binding of the silicon-based material in the second negative electrode active layer, thereby further reducing the full-charge rebound of the negative electrode sheet during fast charging and better improving the cycle performance of the battery cell under fast charging conditions.
[0085] In some embodiments, the first binder has a mass content of 0.5% to 3% in the first negative electrode active layer, such as 0.5%, 1%, 1.5%, 2%, 2.5%, or 3%, or within any two of the above values; and / or, the second binder has a mass content of 1.5% to 7% in the second negative electrode active layer, such as 1.5%, 2.0%, 2.5%, 3.0%, 3.5%, 4.0%, 4.5%, 5.0%, 5.5%, 6.0%, 6.5%, or 7.0%, or within any two of the above values.
[0086] The first and second binders used in this application can be selected from conventional lithium battery negative electrode binders. In some embodiments, the first and second binders each independently contain hydrophilic groups. Optionally, the hydrophilic groups include at least one of sulfonic acid groups, phosphate groups, hydroxyl groups, carboxyl groups, amide groups, amino groups, aldehyde groups, carbonyl groups, cyano groups, and acid anhydrides. By including at least one of sulfonic acid groups, phosphate groups, hydroxyl groups, carboxyl groups, amide groups, amino groups, aldehyde groups, carbonyl groups, cyano groups, and acid anhydrides in the binder, these hydrophilic groups can improve the interaction force between the binder and the silicon-based material and the graphite material, thereby effectively controlling the floatation of the binder during the electrode coating and drying process, promoting the uniform residence of the binder in the gaps of the silicon-based material, and thus more effectively improving the cohesion of the negative electrode.
[0087] In some embodiments, the first adhesive and the second adhesive each independently comprise one or more of the following: polystyrene-butadiene copolymer and its modifications, polystyrene-acrylate and its modifications, polyacrylate copolymer and its modifications, polyurethane copolymer and its modifications, butadiene-acrylonitrile copolymer and its modifications, polytetrafluoroethylene and its modifications, polyvinylidene fluoride and its modifications, styrene-butadiene rubber (SBR), and acrylonitrile-butadiene-styrene copolymer (ABS). The aforementioned substances exhibit good adhesion, which helps to further improve the adhesion between the negative electrode active material and the negative electrode current collector.
[0088] In some embodiments, due to the difference in the negative electrode active materials of the first negative electrode active layer and the second negative electrode active layer, a more suitable binder can be selected from the above binder substances. For example, since graphite is the main active material in the first negative electrode active layer, graphite has less expansion but a relatively lower specific capacity than silicon. Therefore, in order to improve the energy density of the first negative electrode active layer while achieving sufficient bonding of the first negative electrode active material, the first binder is selected from any one or more of styrene-butadiene rubber (SBR), styrene-butadiene block copolymer (SBS), acrylonitrile-butadiene-styrene copolymer (ABS), polyurethane (PU), and polytetrafluoroethylene (PTEE). For example, since the second negative electrode active layer uses silicon-based materials as the main active material, in order to suppress the expansion of silicon and achieve more stable adhesion, the second adhesive is selected from any one or more of the following: polystyrene-butadiene copolymer and its modified products, polystyrene-acrylate and its modified products, polyacrylate copolymer and its modified products, polyurethane copolymer and its modified products, butadiene-acrylonitrile copolymer and its modified products, polytetrafluoroethylene and its modified products, and polyvinylidene fluoride and its modified products.
[0089] In this application, most or all of the silicon-based material in the negative electrode active material is dispersed in the second negative electrode active layer. In some embodiments, the silicon content in the second negative electrode active layer is 10% to 70% by mass, for example, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, or 75%, or any combination of the above values. In some embodiments, the silicon content in the first negative electrode active layer is 0% to 20% by mass. It should be noted that when both the first and second negative electrode active layers include graphite and silicon-based materials, the graphite materials in the first and second negative electrode active layers can be the same or different, and the silicon-based materials can be the same or different. In some embodiments, the ratio of the mass content of the second binder to the mass content of silicon in the second negative electrode active layer is 0.07 to 0.35, for example, 0.07, 0.075, 0.1, 0.125, 0.15, 0.2, 0.25, 0.3, or 0.35, or any combination of the above values. This allows for adjustment of the amount of the second binder based on the mass content of silicon, thereby minimizing the expansion force of the second negative electrode active layer while avoiding excessive introduction of the second binder.
[0090] To improve the charging capability of a single battery cell while achieving the highest possible energy density, in some embodiments, the thickness ratio of the first negative electrode active layer to the second negative electrode active layer is 9:1 to 1:9, such as 9:1, 8:2, 7:3, 6:4, 5:5, 4:6, 3:7, 2:8, or 9:1, or any two of the above values. The thickness of the first negative electrode active layer is 20-200 μm, such as 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, 120 μm, 150 μm, 170 μm, or 200 μm, or any two of the above values. This allows the second negative electrode active layer to significantly improve charging capability and maximize the energy density of the single battery cell.
[0091] In some embodiments, the silicon-based material includes one or more of elemental silicon, silicon-carbon composites, or silicon-oxygen compounds.
[0092] In some embodiments, the silicon-oxygen compound includes at least one of unpre-lithium silicon-oxygen compound, pre-lithium silicon-oxygen compound, unpre-magnesium silicon-oxygen compound, and pre-magnesium silicon-oxygen compound.
[0093] In some embodiments, the mass content of silicon in the silicon-based material is independently 30%-70%, for example, 30%, 40%, 50%, 50%, 60% or 70%, or within any two of the above values.
[0094] In this application, the method for testing the silicon content in silicon-based materials can be a method known in the art. As an example, the following method can be used for testing: a certain amount of silicon-based material is taken, and the mass of silicon element is obtained by inductively coupled plasma optical emission spectrometry (ICP-OES). The mass percentage of silicon element can then be calculated.
[0095] In some implementations, the silicon-based material includes silicon-carbon composite materials.
[0096] The silicon-carbon composite of this application can be prepared using conventional silicon-carbon composites or conventional preparation methods, such as depositing nano-silicon materials on porous carbon by chemical vapor deposition, and further carbon coating, such as using amorphous carbon coating.
[0097] By controlling the silicon content, silicon can be fully dispersed in the pores of the silicon-carbon composite. The carbon-containing porous material forms a supporting structure and pores to mitigate the expansion of silicon material caused by lithium intercalation during charging. The supporting effect of the carbon-containing porous material creates pores within the silicon-carbon composite, allowing the large influx of lithium ions during charging to fill the entire second negative electrode active layer and smoothly enter the first negative electrode active layer. This enables the silicon and porous carbon materials along the entire thickness of the second negative electrode active layer to fully and rapidly intercalate lithium, while the second negative electrode active layer also quickly enters the lithium intercalation state. Therefore, while achieving fast charging, this mitigates the concentration polarization of lithium ions in the upper layers, thereby suppressing the risks of shortened battery cell cycle life and reduced safety caused by lithium ion concentration polarization.
[0098] In some embodiments, the silicon-carbon composite material satisfies one or more of the following characteristics:
[0099] (1) The silicon-carbon composite material includes porous carbon and crystalline silicon located in the pores and on the surface of the porous carbon, and optionally, the porous carbon is hard carbon;
[0100] (2) The silicon-carbon composite material also includes a carbon-containing coating layer, which is located on the surface of porous carbon and / or crystalline silicon;
[0101] (3) The average particle size of the silicon-carbon composite material is 2μm-15μm, and can be selected as 7μm-11μm;
[0102] (4) The powder resistivity of silicon-carbon composite material at 8 MPa is 4 Ω·cm - 17 Ω·cm;
[0103] (5) The BET specific surface area of the silicon-carbon composite material is 1.0 m². 2 / g - 6.7 m 2 / g.
[0104] In some embodiments, the silicon-carbon composite material comprises porous carbon and silicon-containing materials dispersed in the pores of the porous carbon. The porous carbon, acting as a carrier for the silicon-containing material, provides support for the material while simultaneously offering expansion space within the pores, effectively mitigating stress compression caused by expansion during charging. Especially when the silicon-containing material has a nanometer-scale particle size, it exhibits higher specific capacity and is better dispersed within the pores of the porous carbon, allowing for more efficient utilization of the carbon's pore-buffering effect on expansion.
[0105] In some embodiments, the porous carbon may optionally be hard carbon. When the porous carbon is hard carbon, it has stronger support, a more stable pore structure, and is harder, thus providing better porosity for the negative electrode active layer, providing a smoother path for active ion transport, and improving the charging capability of the battery cell.
[0106] In some embodiments, the silicon-containing material includes at least one of elemental silicon, silicon oxides, silicon nitrides, and silicon alloys. In some embodiments, the silicon-containing material includes crystalline silicon, thereby further improving the structural stability of the silicon-containing material and the energy density of the battery cell.
[0107] In some embodiments, the silicon-carbon composite material further includes a carbon-containing coating layer that coats the surface of the core. This enhances the conductivity of the silicon-carbon composite, reduces the internal impedance of the battery cell, and effectively reduces the probability of direct contact between the silicon-containing material in the porous carbon channels and the external environment, thereby improving the chemical stability of the silicon-carbon composite. The negative electrode active layer also includes a conductive agent, which may be one or more of carbon black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers, or a mixture thereof.
[0108] In addition to providing structural support and buffering for the expansion of silicon-containing materials, the pores in silicon-carbon composite materials also form between the particles. To further improve the flow of lithium ions through the intraparticle and interparticle pores, in some embodiments, the average particle size of the silicon-carbon composite material is 2 μm-15 μm. Optionally, the average particle size of the silicon-carbon composite material is 7 μm-11 μm, or 5 μm-10 μm. This creates a particle size distribution between the average particle size of the silicon-carbon composite material and the graphite material, thus facilitating the use of interparticle gaps to increase the compaction of the negative electrode active layer, thereby further improving the energy density of the battery cell.
[0109] The average particle size of the aforementioned silicon-carbon composite material can be tested using equipment and methods known in the art. For example, a scanning electron microscope (e.g., ZEISS Sigma 300) can be used, referring to JY / T010-1996, to obtain a scanning electron microscope (SEM) image of the negative electrode sheet. As an example, the test can be performed as follows: Randomly select a test sample of length × width = 50 mm × 100 mm on the negative electrode sheet. Randomly select multiple test areas (e.g., 5 areas) within the test sample, and at a certain magnification (e.g., 1000x when measuring silicon-carbon composite materials), read the particle size of each silicon-carbon composite material particle in each test area (i.e., take the distance between the two farthest points on the silicon-carbon composite material particle as the particle size). Count the number and particle size values of silicon-carbon composite materials in each test area, and take the arithmetic mean of the silicon-carbon composite material particles in each test area, which is the average particle size of the silicon-carbon composite material particles in the test sample. To ensure the accuracy of the test results, multiple test samples (e.g., 10) can be taken and the above test can be repeated. The average value of each test sample can be taken as the final test result.
[0110] In some embodiments, the powder resistivity of the silicon-carbon composite material at 8 MPa is 4 Ω·cm - 17 Ω·cm. This control of powder resistivity improves the conductivity of the silicon-carbon composite, thereby increasing the charging rate of the battery cell.
[0111] In this application, the powder resistivity of silicon-carbon composite materials can be determined using methods known in the art. As an example, a four-probe method can be used, where two probes apply voltage and the other two probes measure current. The powder resistivity can be calculated by measuring the resistance value. Models of four-probe semiconductor powder resistivity testers include the ST-2722.
[0112] In some embodiments, the BET specific surface area of the silicon-carbon composite material is 1.0 m² / g - 6.7 m² / g.
[0113] In this application, the method for testing the BET specific surface area of silicon-carbon composite materials can be a method known in the art. As an example, referring to GB / T 19587-2017, the nitrogen adsorption specific surface area analysis method can be used. The sample tube containing the silicon-carbon composite material sample is immersed in liquid nitrogen at -196℃, and the amount of nitrogen adsorbed on the surface of the solid sample at different pressures of 0.05-0.30 MPa is measured. Based on the BET multilayer adsorption theory and calculation formula, the monolayer adsorption amount of the sample is obtained, and thus the BET specific surface area is obtained. This test can be performed using a Tri-Star 3020 specific surface area and pore size analyzer from Micromeritics, USA.
[0114] In some embodiments, the negative electrode active layer further includes a conductive agent, which includes one or more of carbon black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0115] In some embodiments, the mass content of the conductive agent in the first negative electrode active layer is 0.05%-1%, such as 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, or 1%, or within any two of the above values. The mass content of the conductive agent in the second negative electrode active layer is 0.05%-2%, such as 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.2%, 1.5%, 1.8%, or 2%, or within any two of the above values. Since graphite material is used as the main body of the negative electrode active material in the first negative electrode active layer, it has good conductivity. It can meet the conductivity requirements under fast charging conditions even with a relatively low conductive agent content, thereby appropriately increasing the graphite material content to improve the energy density of this layer. Using a relatively large amount of conductive agent in the second negative electrode active layer is beneficial to improving the conductivity of the second negative electrode active layer, thereby helping to improve the charging capability.
[0116] In some embodiments, the conductive agent in the second negative electrode active layer includes carbon black and carbon nanotubes, with the mass ratio of carbon black to carbon nanotubes being 6:4 to 9:1, optionally 8:2 to 8.5:1.5.
[0117] Carbon nanotubes exhibit better electrical conductivity than carbon black, thus they can be used to improve the poor intrinsic conductivity of silicon materials. Furthermore, the linear nature of carbon nanotubes can restrain the expansion of silicon-carbon composite materials and also play a role in controlling the elongation of the negative electrode sheet.
[0118] During repeated charge-discharge cycles, the cohesive force between the negative electrode active layer and the negative electrode current collector is affected by repeated stress compression. This can lead to powder shedding or even delamination after long cycles. In some embodiments, the negative electrode sheet also includes a base coating layer, which is disposed between the negative electrode current collector and the negative electrode active layer. The base coating layer includes a base conductive agent and a base adhesive. The base coating layer increases the adhesion between the negative electrode active layer and the negative electrode current collector, further extending the cycle life of the battery cell.
[0119] In some embodiments, the graphite material includes a first graphite material and a second graphite material, wherein the first graphite material is disposed in a first negative electrode active layer, and the second graphite material is disposed in a second negative electrode active layer, and the first graphite material and the second graphite material satisfy at least one of the following conditions:
[0120] (1) The average particle size of the second graphite material is lower than that of the first graphite material;
[0121] (2) The tap density of the second graphite material is greater than that of the first graphite material;
[0122] (3) The first graphite material and the second graphite material are each independently selected from at least one of artificial graphite and natural graphite; optionally, the first graphite material includes natural graphite and the second graphite material includes artificial graphite. The above-mentioned small particle size and / or low tap density second graphite material shortens the ion transport path in the second negative electrode active layer, thereby improving the dynamic performance of the battery cell and taking into account high energy density.
[0123] The average particle size of the first and second graphite materials was tested using the same method as the average particle size test method for the silicon-carbon composite material.
[0124] The test methods for the tap density of the first and second graphite materials are as follows:
[0125] Pretreatment: Obtain the powder sample to be tested, take a 25mL graduated cylinder with known mass, put 21-24mL of powder sample into it and weigh it, then seal the graduated cylinder with sealing film.
[0126] Test: A graduated cylinder containing powder is fixed to a mechanical vibration device. The motor drives the device to vibrate vertically up and down, gradually compacting the powder. Vibration stops after a set number of vibrations, and the volume of the graduated cylinder is read. The density of the compacted powder is calculated by dividing mass by volume. Amplitude: 3.0 ± 0.1 mm, Vibration frequency: 250 ± 15 times / min, Number of vibrations: 5000.
[0127] In some embodiments, the primer coating has one or more of the following characteristics:
[0128] The primer conductive agent includes carbon black, which reduces the cost of conductivity;
[0129] The primer binder includes polyvinylidene fluoride, which increases the adhesion between the primer layer and the negative electrode current collector;
[0130] The adhesive content in the primer layer is 40%-60% by mass, such as 40%, 45%, 50%, 55% or 60%, or any two of the above values, to achieve better adhesion while reducing the influence of the adhesive on the conductivity between the negative electrode current collector and the negative electrode active layer.
[0131] The thickness of the base coating is 0.2 μm - 2 μm, for example, 0.2 μm, 0.3 μm, 0.4 μm, 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, 1.0 μm, 1.2 μm, 1.5 μm, 1.7 μm or 2.0 μm, or any two of the above values, to control the impact of the base coating on the energy density of the battery cell as much as possible.
[0132] As an example, the negative electrode current collector can be a metal foil, a conductive polymer material, a carbon material, or a composite current collector. For example, as a metal foil, pure metals, alloys, or surface-treated metals can be used, including but not limited to stainless steel, copper, aluminum, nickel, titanium, or silver. The composite current collector may include a polymer material substrate and a metal layer. The composite current collector can be formed by forming a metal material (copper, copper alloys, nickel, nickel alloys, titanium, titanium alloys, silver, and silver alloys, etc.) on a polymer material substrate (such as a substrate of polypropylene, polyethylene terephthalate, polybutylene terephthalate, polystyrene, polyethylene, etc.).
[0133] [Positive electrode plate]
[0134] A single battery cell typically also includes a positive electrode sheet, which includes a positive current collector and a positive active layer disposed on at least one side of the positive current collector. The positive active layer includes a positive active material.
[0135] As an example, the positive current collector has two surfaces opposite each other in its own thickness direction, and the positive electrode film layer is disposed on either or both of the two opposite surfaces of the positive current collector.
[0136] As an example, the positive current collector can be a metal foil, a conductive polymer material, a carbon material, or a composite current collector. For example, as a metal foil, pure metals, alloys, or surface-treated metals can be used, including but not limited to stainless steel, copper, aluminum, nickel, titanium, or silver. The composite current collector may include a polymer material base layer and a metal layer. The composite current collector can be formed by forming a metal material (aluminum, aluminum alloys, nickel, nickel alloys, titanium, titanium alloys, silver, and silver alloys, etc.) on a polymer material substrate (such as a substrate of polypropylene, polyethylene terephthalate, polybutylene terephthalate, polystyrene, polyethylene, etc.).
[0137] In some embodiments, the positive electrode active material may be a known positive electrode active material for batteries. As an example, the positive electrode active material may include at least one of the following materials: lithium-containing phosphates with an olivine structure, lithium transition metal oxides, and their respective modified compounds. However, this application is not limited to these materials, and other conventional materials that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Examples of lithium transition metal oxides include, but are not limited to, lithium cobalt oxides (such as LiCoO2), lithium nickel oxides (such as LiNiO2), lithium manganese oxides (such as LiMnO2, LiMn2O4), lithium nickel cobalt oxides, lithium manganese cobalt oxides, lithium nickel manganese oxides, and lithium nickel cobalt manganese oxides. Examples of lithium-containing phosphates with an olivine structure include, but are not limited to, at least one of lithium iron phosphate (such as LiFePO4 (also referred to as LFP)), lithium iron phosphate and carbon composites, lithium manganese phosphate (such as LiMnPO4), lithium manganese phosphate and carbon composites, lithium manganese iron phosphate, and lithium manganese iron phosphate and carbon composites.
[0138] In some embodiments, the positive electrode active material includes a nickel-containing lithium transition metal oxide or a lithium-containing phosphate.
[0139] As an example, nickel-containing lithium transition metal oxides include lithium-containing nickel-cobalt-manganese oxides and lithium-containing nickel-cobalt-aluminum oxides.
[0140] In some embodiments, lithium-containing nickel-cobalt-manganese oxides include the compound Li a Ni b Co c Mn d M e O 2-f Wherein, M includes one or more elements selected from Al, Fe, Ti, Mg, Zr, Cr, Ga, Cu, Zn, Nb, and B; a is any value in the range of 0.7-1.1, and can be selected as any value in the range of 0.8-1.1; b is any value in the range of 0.45-0.97, and can be selected as any value in the range of 0.8-0.97, and can be further selected as any value in the range of 0.85-0.95; c is any value in the range of 0.02-0.25, and can be selected as any value in the range of 0.02-0.2; d is any value in the range of 0.05-0.5, and can be selected as any value in the range of 0.05-0.48; e is any value in the range of 0-0.2, and can be selected as any value in the range of 0.001-0.2; f is any value in the range of 0-0.3, and can be selected as any value in the range of 0-0.2.
[0141] As an example, lithium-containing nickel-cobalt-manganese oxides include LiNi 1 / 3 Co1 / 3 Mn 1 / 3 O2 (also known as NCM333), LiNi 0.5 Co 0.2 Mn 0.3 O2 (also known as NCM523), LiNi 0.5 Co 0.25 Mn 0.25 O2 (also known as NCM211), LiNi 0.6 Co 0.2 Mn 0.2 O2 (also known as NCM622), LiNi 0.8 Co 0.1 Mn 0.1 O2 (also known as NCM811), LiNi 0.85 Co 0.15 Mn 0.05 O2, LiNi 0.9 Co 0.05 Mn 0.05 One or more of O2 and its modified compounds.
[0142] In some embodiments, the positive electrode active material includes primary particles and / or secondary particles. Optionally, based on the total cross-sectional area of the positive electrode active material, the cross-sectional area of the primary particles accounts for more than 30%. Primary particles have better structural stability and are therefore more suitable for fast charging conditions.
[0143] In some embodiments, the positive electrode film layer may optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), PVDF-tetrafluoroethylene-propylene terpolymer, PVDF-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorinated acrylate resin.
[0144] In some embodiments, the positive electrode film may optionally include a conductive agent. As an example, the conductive agent may include at least one selected from superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0145] In some embodiments, the positive electrode sheet can be prepared by dispersing the above-mentioned components for preparing the positive electrode sheet, such as positive active material, conductive agent, binder and any other components, in a solvent (e.g., N-methylpyrrolidone) to form a positive electrode slurry; coating the positive electrode slurry onto the positive electrode current collector, and then obtaining the positive electrode sheet after drying, cold pressing and other processes.
[0146] [Electrolytes]
[0147] In some embodiments, the battery cell also includes an electrolyte, which acts as a conductor of ions between the positive and negative electrodes. This application does not impose specific limitations on the type of electrolyte; it can be selected according to requirements. The electrolyte can be liquid, gel, or solid.
[0148] Liquid electrolytes include electrolyte salts and solvents.
[0149] In some embodiments, the electrolyte salt may be selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalate borate, lithium dioxalate borate, lithium difluorodioxalate phosphate, and lithium tetrafluorooxalate phosphate.
[0150] In some embodiments, the solvent may be selected from at least one of ethylene carbonate, propylene carbonate, methyl ethyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, butyl carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, sulfolane, dimethyl sulfone, methyl ethyl sulfone, and diethyl sulfone. The solvent may also be an ether solvent. Ether solvents may include one or more of ethylene glycol dimethyl ether, ethylene glycol diethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, 1,3-dioxolane, tetrahydrofuran, methyl tetrahydrofuran, diphenyl ether, and crown ethers.
[0151] In some embodiments, the electrolyte may optionally include additives. For example, additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain properties of the battery cell, such as additives that improve the overcharge / fast charge performance of the battery cell, additives that improve the high-temperature performance of the battery cell, and additives that improve the low-temperature performance of the battery cell.
[0152] The gel electrolyte includes a polymer as a backbone network and can be used in conjunction with an ionic liquid-lithium salt.
[0153] Solid electrolytes include polymer solid electrolytes, inorganic solid electrolytes, and composite solid electrolytes.
[0154] As an example, the polymers of polymeric solid electrolytes may include polyethers (polyoxyethylene), polysiloxanes, polycarbonates, polyacrylonitrile, polyvinylidene fluoride, polymethyl methacrylate, monoionic polymers, polyionic liquids, cellulose, etc.
[0155] As an example, inorganic solid electrolytes can be one or more of the following: oxide solid electrolytes (crystalline perovskite, sodium superconducting ion conductor, garnet, amorphous LiPON thin film), sulfide solid electrolytes (crystalline lithium superconducting ion conductor (lithium germanium phosphorus sulfide, silver sulfide germanium ore), amorphous sulfides), halide solid electrolytes, nitride solid electrolytes, and hydride solid electrolytes.
[0156] As an example, composite solid electrolytes are formed by adding inorganic solid electrolyte fillers to polymer solid electrolytes.
[0157] [Isolation Component]
[0158] In some embodiments, the electrode assembly further includes an isolator disposed between the positive and negative electrodes.
[0159] In some embodiments, the separator is a separator membrane. This application does not impose any particular limitation on the type of separator membrane; any known porous separator membrane with good chemical and mechanical stability can be selected.
[0160] As an example, the main material of the separator can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene, polyvinylidene fluoride, and ceramic. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation. The separator can be a single component located between the positive and negative electrodes, or it can be attached to the surfaces of the positive and negative electrodes. An inorganic particle coating, an organic particle coating, or an organic / inorganic composite coating can also be applied to the surface of the separator.
[0161] In some embodiments, the separator is a solid electrolyte. The solid electrolyte is disposed between the positive and negative electrodes, serving both to transport ions and to isolate the positive and negative electrodes.
[0162] [Electrode Assembly]
[0163] The electrode assembly can be a wound structure, a stacked structure, or a hybrid structure of wound and stacked.
[0164] In some embodiments, the electrode assembly is a wound structure. The positive electrode and the negative electrode are wound into a wound structure.
[0165] In some implementations, the electrode assembly is a stacked structure.
[0166] As an example, multiple positive and negative electrode plates can be set, and multiple positive and multiple negative electrode plates can be stacked alternately.
[0167] As an example, multiple positive electrode sheets can be set, and negative electrode sheets are folded to form multiple stacked folded segments, with a positive electrode sheet sandwiched between adjacent folded segments.
[0168] As an example, both the positive and negative electrode sheets are folded to form multiple stacked folded segments.
[0169] As an example, multiple separators can be provided, each positioned between any adjacent positive or negative electrode plates.
[0170] As an example, the separator can be continuously arranged between any adjacent positive or negative electrode plates by folding or rolling.
[0171] In some embodiments, the electrode assembly can be cylindrical, flat, or polygonal, etc.
[0172] In some embodiments, the electrode assembly is provided with tabs that allow current to be drawn from the electrode assembly. The tabs include a positive tab and a negative tab.
[0173] shell
[0174] In some embodiments, the battery cell may include a casing. The casing may be a steel casing, an aluminum casing, a plastic casing (such as a polypropylene casing), a composite metal casing (such as a copper-aluminum composite casing), or an aluminum-plastic film, etc. In some embodiments, the casing may be a sealed structure or a non-sealed structure. As an example, when the casing is a non-sealed structure, the casing serves to protect the electrode assembly, and a sealing bag is included between the casing and the electrode assembly to encapsulate the electrode assembly and electrolyte. Specifically, the sealing bag may be a bag-shaped insulating component or an aluminum-plastic film. When the casing is a sealed structure, it is used to encapsulate components such as the electrode assembly and electrolyte.
[0175] As an example, the battery cell can be a cylindrical battery cell, a prismatic battery cell, a pouch battery cell, or a battery cell of other shapes. Prismatic battery cells include prismatic battery cells, blade-shaped battery cells, and multi-prismatic batteries, such as hexagonal prismatic batteries. This application does not have any particular limitations.
[0176] In some embodiments, the housing includes an end cap and a housing, the housing having an opening, and the end cap covering the opening. The housing may have one or more openings. The end cap may also have one or more.
[0177] Figure 1 The example shown is a square-structured battery cell 5.
[0178] In some implementations, refer to Figure 2The outer packaging may include a housing 51 and an end cap 53. The housing 51 may include a base plate and side plates connected to the base plate, the base plate and side plates forming a receiving cavity. The housing 51 has an opening communicating with the receiving cavity, and the end cap 53 can be placed over the opening to close the receiving cavity. The positive electrode, negative electrode, and separator can be formed into an electrode assembly 52 by a winding process or a stacking process. The electrode assembly 52 is encapsulated within the receiving cavity. Electrolyte is immersed in the electrode assembly 52. The number of electrode assemblies 52 contained in a single battery cell 5 can be one or more, which can be selected by those skilled in the art according to specific practical needs.
[0179] electrode terminals
[0180] In some embodiments, at least one electrode terminal is provided on the housing, and the electrode terminal is electrically connected to the tab. The electrode terminal can be directly connected to the tab, or it can be indirectly connected to the tab through a current collector. The electrode terminal can be provided on the end cap or on the housing.
[0181] Pressure relief mechanism
[0182] In some embodiments, a pressure relief mechanism is provided on the casing. The pressure relief mechanism is used to release the internal gas of the battery cell.
[0183] As an example, the internal pressure or temperature of a battery cell is actuated to release the internal pressure or temperature when it reaches a predetermined threshold. When the internal pressure or temperature of the battery cell reaches the predetermined threshold, the pressure relief mechanism is activated or a weak structure in the pressure relief mechanism is broken, thereby forming an opening or channel for the internal pressure or temperature to be released. The threshold design varies depending on the design requirements. The threshold may depend on the materials of one or more of the positive electrode, negative electrode, electrolyte, and separator in the battery cell.
[0184] As an example, the pressure relief mechanism can be integrally molded with the housing.
[0185] As an example, the pressure relief mechanism can also be separately installed and connected to the housing.
[0186] The term "actuation" as used in this application refers to the activation or actuation of the pressure relief mechanism to a certain state, thereby releasing the internal pressure and temperature of the battery cell. The actions of the pressure relief mechanism may include, but are not limited to: movement of components within the mechanism to form an exhaust channel, rupture, breakage, tearing, or opening of at least a portion of the mechanism, etc. When the pressure relief mechanism is activated, the high-temperature, high-pressure substances inside the battery cell are discharged as waste from the activated portion. This method allows for pressure and temperature relief of the battery cell under controllable pressure or temperature, thereby preventing potentially more serious accidents.
[0187] In some embodiments, when the housing is a non-sealed structure, the pressure relief mechanism can be configured as a through hole for venting gas inside the battery cell.
[0188] The emissions from battery cells mentioned in this application include, but are not limited to: electrolyte, dissolved or split positive and negative electrode plates, fragments of separators, high-temperature and high-pressure gases generated by the reaction, flames, etc.
[0189] The battery apparatus mentioned in the embodiments of this application may include one or more battery cell assemblies for providing voltage and capacity. A battery cell assembly may include multiple battery cells connected in series, parallel, or mixed connections via a busbar.
[0190] In some embodiments, a battery cell assembly is typically formed by arranging multiple battery cells.
[0191] As an example, a battery cell assembly can be a battery module, which is formed by arranging and fixing multiple battery cells together to form an independent module. As another example, a battery module can be formed by bundling multiple battery cells together with cable ties.
[0192] Figure 3 This is battery module 4 as an example. (See reference...) Figure 3 In the battery module 4, multiple battery cells 5 can be arranged sequentially along the length of the battery module 4. Of course, they can also be arranged in any other way. Furthermore, these multiple secondary battery cells 5 can be fixed in place using fasteners.
[0193] Optionally, the battery module 4 may also include a housing with a receiving space in which multiple battery cells 5 are received.
[0194] In some embodiments, the battery device may be a battery pack, which includes a housing and one or more individual battery cells housed within the housing.
[0195] As an example, the battery cell assembly can be a battery module, which can be housed in a housing by fixing the battery module in the housing.
[0196] As an example, battery cell assemblies can also be housed in a housing by directly fixing multiple battery cells to the housing.
[0197] As an example, the enclosure may include a first enclosure and a second enclosure. The first enclosure and the second enclosure are fastened together to form a closed space inside the enclosure to house the individual battery cells. Here, "closed" refers to covering or closing, and can be either sealed or unsealed. The first enclosure may be a top cover or a bottom plate.
[0198] As an example, the enclosure may include a top cover, a frame, and a bottom plate. The top cover and bottom plate are connected to the frame, creating an enclosed space inside the enclosure to house the individual battery cells. Figure 4 and Figure 5 This is battery pack 1 as an example. (See reference...) Figure 4 and Figure 5 The battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box includes an upper body 2 and a lower body 3, with the upper body 2 covering the lower body 3 to form a closed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.
[0199] In some embodiments, the housing may be part of the vehicle's chassis structure. For example, a portion of the housing may be at least a part of the vehicle's floor, or a portion of the housing may be at least a part of the vehicle's crossbeams and longitudinal beams.
[0200] The technical solutions described in the embodiments of this application are applicable to various electrical devices that use individual battery cells, such as mobile phones, portable devices, laptops, electric vehicles, electric toys, power tools, vehicles, ships, and spacecraft. For example, spacecraft include airplanes, rockets, space shuttles, and spacecraft.
[0201] As the electrical device, a single secondary battery cell, a battery module, or a battery pack can be selected according to its usage requirements.
[0202] Figure 6 This is an example of an electrical device. The device could be a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of the secondary battery for this device, a battery pack or battery module can be used.
[0203] [Example]
[0204] The following describes embodiments of this application. The embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in this field or according to the product instructions. Reagents or instruments used, unless otherwise specified, are all conventional products that can be obtained commercially.
[0205] Example 1
[0206] Positive electrode sheet:
[0207] Positive electrode active material LiNi 0.9 Co 0.05 Mn 0.05 O2, conductive agent acetylene black, and binder polyvinylidene fluoride were added to NMP solvent in a mass ratio of 97:2:1 and stirred evenly to prepare a positive electrode slurry. This slurry was then uniformly coated onto a 13μm thick aluminum foil, with an areal density of 300mg / 1540.25mm². 2 After drying, the material is cold-pressed and then die-cut to a width of 100mm to produce lithium-ion battery positive electrode sheets.
[0208] Negative electrode plate:
[0209] Preparation of the first negative electrode slurry: The first graphite material, SP conductive carbon black, sodium carboxymethyl cellulose, and styrene-butadiene rubber (Dv50 approximately 0.25 μm, weight-average molecular weight approximately 150,000) were thoroughly mixed in an appropriate amount of deionized water at a mass ratio of 97:1:1:1 to form the first negative electrode slurry. The first graphite material had an average particle size of 15 μm and a tap density of 1.4 g / cm³. 3 Natural graphite;
[0210] Preparation of the second negative electrode slurry: Active material formed by mixing second graphite material and silicon-based silicon-carbon composite material, SP conductive carbon black, carbon nanotubes, sodium carboxymethyl cellulose, and styrene-acrylate emulsion (Dv50 approximately 0.6 μm, weight-average molecular weight approximately 300,000) were mixed uniformly at a mass ratio of 95:1:0.5:0.5:3, and then an appropriate amount of deionized water was added to form the second negative electrode slurry. The second graphite material has an average particle size of 9 μm and a tap density of 1.9 g / cm³. 3 The artificial graphite, the second silicon-carbon composite material includes porous hard carbon and silicon-containing materials located in the pores and on the surface of the porous carbon. Some of the silicon-containing materials are crystalline silicon. Its Dv50 particle size is 9 μm, its BET specific surface area is about 2 m² / g, the mass ratio of silicon element is 50%, and the powder resistivity is 8 Ω·cm. The mass ratio of the second graphite material to the silicon-carbon composite material is 60:40.
[0211] Preparation of primer slurry: The primer conductive agent SP conductive carbon black and the primer binder polyvinylidene fluoride (PVDF) are mixed at a mass ratio of 8:2 to prepare the primer slurry.
[0212] A base coating slurry is applied to the copper foil of the negative electrode current collector and dried to form a base coating with a thickness of 0.5 μm. A dual-cavity coating device is used to simultaneously apply the first negative electrode slurry and the second negative electrode slurry to the surface of the current collector copper foil with the base coating. After drying, cold pressing and slitting, the negative electrode sheet of Example 1 is obtained. The first negative electrode slurry forms the first negative electrode active layer and the second negative electrode slurry forms the second negative electrode active layer. The thickness ratio of the two is 5:5.
[0213] Separating membrane:
[0214] A separation membrane was obtained by coating a 3μm thick alumina coating onto a polyethylene base membrane.
[0215] Electrolyte:
[0216] LiPF6 was dissolved in a solvent with a volume ratio of DMC:DEC:EC of 1:1:1 to obtain a lithium-ion battery electrolyte with a LiPF6 concentration of 1 mol / L.
[0217] Assembly:
[0218] The positive electrode, negative electrode, and separator are wound together, and then the casing is assembled. After electrolyte injection, the battery undergoes formation and other processes to obtain the battery. The formation process of the battery is as follows: first, it is charged at 0.02C to 3.0V, then at 0.1C to 3.4V, and finally at 0.2C to 3.9V.
[0219] test
[0220] Average particle size test of upper and lower adhesive layers:
[0221] After discharging the battery cell to 0% SOC, disassemble it, remove the negative electrode sheet, and scrape off the powder to obtain the negative electrode material. Using deionized water or ethanol as the dispersion medium, take 10-20 mg of the negative electrode powder, add 5-10 mL of dispersant, and sonicate for 10-30 minutes (power recommended ≤100 W) until the slurry is in a uniform suspension, a light-colored dispersion is visible to the naked eye, and there is no sediment, thus obtaining the sample to be tested. Dilute the sample to a transmittance of 0.1-1 mg / mL. Calibrate the DLS instrument using standard particles (such as polystyrene microspheres), and test the diluted sample using a dynamic light scattering instrument. Repeat the test 5 times, and take the average value as the average particle size.
[0222] Electrode cohesion test:
[0223] After discharging the battery cells to 0% SOC, disassemble them. Cut the anode electrode into a 2cm*20cm rectangular sheet. Attach 20mm*160mm double-sided adhesive tape to the negative electrode active layer of the rectangular sheet. Attach the other side of the tape to a 30mm*200mm steel plate. Then, use a 2kg constant pressure roller to roll back and forth three times along the slide rail. Peel the sheet in a tensile testing machine. After the test, record the average peel force of the peel curve. Multiply this peel force by 50 to obtain the cohesive force.
[0224] Battery cycle capacity retention:
[0225] At 25℃, the battery cells were charged at 5C to 30% SOC, 4C to 40% SOC, 3.5C to 50% SOC, constant current to 50% SOC, 3.2C to 60% SOC, 2.8C to 70% SOC, 2.5C to 80% SOC, and 0.5C to 4.25V. Constant voltage charging was then continued to 0.04C. After resting for 30 minutes, the cells were discharged at 0.5C to 2.5V, and the discharge capacity of the first cycle was tested. This cycle was repeated for a total of 100 cycles. The discharge capacity of the last cycle was then tested. The cycle capacity retention rate was obtained by dividing the discharge capacity of the last cycle by the discharge capacity of the first cycle.
[0226] Methods for testing the charging time of individual battery cells:
[0227] At 25°C, the battery cell was charged to 3.8V at a constant current of 0.33C, then charged to 0.05C at a constant voltage. After standing for 5 minutes, it was discharged to 2.0V at a constant current of 0.33C, and its actual capacity was recorded as C0.
[0228] The battery cells were sequentially charged at constant current rates of 1.0C0, 1.3C0, 1.5C0, 1.8C0, 2.0C0, 2.3C0, 2.5C0, and 3.0C0 to a negative electrode cutoff potential of 3.8V or 0V (whichever comes first). After each charge was completed, the cells were discharged to 2.0V at 1C0. The negative electrode potentials corresponding to the state of charge (SOC) of 10%, 20%, 30%, 40%, 50%, 60%, 70%, and 80% were recorded at different charging rates. Charging rate-negative electrode potential curves were plotted for different SOC states. Linear fitting was performed to obtain the charging rate corresponding to a negative electrode potential of 0V for each SOC state. This charging rate represents the charging window for that SOC state, denoted as C10%SOC, C20%SOC, C30%SOC, C40%SOC, C50%SOC, C60%SOC, C70%SOC, and C80%SOC. The charging time T (assuming no lithium plating in the battery cell) from 10% SOC to 80% SOC was calculated using the following formula, in minutes.
[0229] T=(0.1 / C10%SOC+0.1 / C20%SOC+0.1 / C30%SOC+0.1 / C40%SOC+0.1 / C50%SOC+0.1 / C60%SOC+0.1 / C70%SOC+0.1 / C80%SOC)×60.
[0230] The test results are recorded in Table 1.
[0231] Example 2
[0232] The difference from Example 1 is that the styrene-acrylate emulsion used in the second negative electrode slurry has a Dv50 of approximately 0.4 μm and a weight-average molecular weight of approximately 200,000; otherwise, it is the same as in Example 1. Example 3
[0233] The difference from Example 1 is that the styrene-acrylate emulsion used in the second negative electrode slurry has a Dv50 of about 0.75 μm and a weight-average molecular weight of about 500,000, while the rest is the same as in Example 1.
[0234] Example 4
[0235] The difference from Example 1 is that the mass ratio of the first graphite material, silicon-carbon composite material (the same as the silicon-carbon composite material in Example 1), SP conductive carbon black, sodium carboxymethyl cellulose, and styrene-butadiene rubber (Dv50 is about 0.25 μm, weight-average molecular weight is about 150,000) in the first negative electrode slurry is 60:37:1:1:1, and the rest is the same as in Example 1, so that the mass ratio of silicon element in the second negative electrode active layer to the mass ratio of silicon element in the negative electrode active layer is about 50%.
[0236] Comparative Example 1
[0237] The difference from Example 1 is that the styrene-acrylate emulsion used in the second negative electrode slurry has a Dv50 of about 0.12 μm and a weight-average molecular weight of about 70,000, while the rest is the same as in Example 1.
[0238] Comparative Example 2
[0239] The difference from Example 1 is that the styrene-acrylate emulsion used in the second negative electrode slurry has a Dv50 of about 1.1 μm and a weight-average molecular weight of about 800,000, while the rest is the same as in Example 1.
[0240] Table 1
[0241] Average particle size of the second binder / μm Cohesion N / m Capacity retention rate / % Charging time / min Example 1 0.5 160 97 8.7 Example 2 0.3 120 92 10.2 Example 3 0.7 130 90 8.7 Example 4 0.7 135 92 9.9 Comparative Example 1 0.1 90 88 15.8 Comparative Example 2 1.0 100 89 13.1
[0242] According to the data comparison of the embodiments and comparative examples in Table 1, it can be seen that when the average particle size of the second binder in the upper second negative electrode active layer is less than 0.3 μm or greater than 0.7 μm, the cohesion of the negative electrode active layer will be significantly reduced, the cycle capacity retention rate of the battery cell will be reduced, and the charging time will be prolonged.
[0243] Examples 5 and 6 investigate the effects of the particle size and weight-average molecular weight of the first binder on the performance of the battery cells.
[0244] The difference between Example 5 and Example 1 is that the styrene-butadiene rubber used in the first negative electrode slurry has a Dv50 particle size of about 0.01 μm and a weight-average molecular weight of about 100,000, while the rest is the same as in Example 1.
[0245] The difference between Example 6 and Example 1 is that the styrene-butadiene rubber used in the first negative electrode slurry has a Dv50 particle size of about 0.6 μm and a weight-average molecular weight of about 200,000, while the rest is the same as in Example 1.
[0246] The test results are recorded in Table 2.
[0247] Table 2
[0248] Average particle size of the first binder / μm Cohesion N / m Capacity retention rate / % Charging time / min Example 1 0.2 160 97 8.7 Example 5 0.01 150 94 12.2 Example 6 0.6 130 92 10.1
[0249] The data comparison in Table 2 shows that when the average particle size of the first binder decreases to 0.01 μm, although the effect on cohesion is small, it leads to a longer charging time. This may be because the adhesion to the graphite material decreases, resulting in an increase in the interparticle resistance and a longer lithium ion insertion rate in the lower layer. When the average particle size of the first binder increases to 0.6 μm, the particle size is too large to fill the gaps between the graphite particles well. The cohesion of the active layer decreases significantly compared to Example 1, and the charging time is also prolonged.
[0250] The following examines the effects of binder dosage and type on the performance of individual battery cells.
[0251] Example 7
[0252] The difference from Example 1 is that the mass ratio of each component in the first negative electrode slurry is adjusted. Specifically, the mass ratio of the first graphite material, SP conductive carbon black, sodium carboxymethyl cellulose, and styrene-butadiene rubber is 97.5:1:1:0.5, while the rest is the same as in Example 1.
[0253] Example 8
[0254] The difference from Example 1 is that the mass ratio of each component in the first negative electrode slurry is adjusted. Specifically, the mass ratio of the first graphite material, SP conductive carbon black, sodium carboxymethyl cellulose, and styrene-butadiene rubber is 95:1:1:3, while the rest is the same as in Example 1.
[0255] Example 9
[0256] The difference from Example 1 is that the mass ratio of each component in the second negative electrode slurry is adjusted. Specifically, the mass ratio of the active material formed by mixing the second graphite material and the silicon-based silicon-carbon composite material, SP conductive carbon black, carbon nanotubes, sodium carboxymethyl cellulose, and styrene-acrylate emulsion is 96.5:1:0.5:0.5:1.5.
[0257] Example 10
[0258] The difference from Example 1 is that the mass ratio of each component in the second negative electrode slurry is adjusted, specifically the mass ratio of the second graphite material, silicon-carbon composite material, SP conductive carbon black, carbon nanotubes, sodium carboxymethyl cellulose, and styrene-acrylate emulsion is 53:38:1:0.5:0.5:7.
[0259] Example 11
[0260] The difference from Example 1 is that a polyurethane copolymer binder was used instead of the styrene-butadiene rubber in Example 1. This polyurethane copolymer has a Dv50 of approximately 0.65 μm and a weight-average molecular weight of approximately 200,000, and its average particle size in the first negative electrode active layer was measured to be approximately 0.6 μm. The rest is the same as in Example 1.
[0261] Example 12
[0262] The difference from Example 1 is that an acrylonitrile-butadiene-styrene copolymer was used instead of the styrene-acrylate emulsion in Example 1. The acrylonitrile-butadiene-styrene copolymer has a Dv50 of approximately 0.65 μm and a weight-average molecular weight of approximately 350,000, and its average particle size in the first negative electrode active layer was measured to be approximately 0.6 μm. The rest is the same as in Example 1.
[0263] The test results are recorded in Table 3.
[0264] Table 3
[0265] Cohesion N / m Capacity retention rate / % Charging time / min Example 1 160 97 8.7 Example 7 125 90 11.2 Example 8 130 92 12.4 Example 9 130 90 10.3 Example 10 155 92 11.5 Example 11 120 93 10.9 Example 12 130 92 11.1
[0266] A comparison of the data from Examples 1, 7, and 8 shows that increasing the content of the first binder in the first negative electrode active layer, or increasing the content of the second binder in the second negative electrode active layer, can increase the cohesion of the electrode to a certain extent. However, this also leads to difficulties in slurry processing, the binder is prone to demulsification, the active material is unevenly dispersed, resulting in the binder's inability to fully exert its effect, and the electrode becomes brittle. Therefore, the cohesion of Examples 8 and 10 is not as strong as that of Example 1. Furthermore, the increased binder content reduces the proportion of active material, leading to a longer charging time.
[0267] Examples 13 to 15 investigate the effect of silicon content in the second negative electrode active layer on the performance of the battery cell.
[0268] Example 13
[0269] The difference from Example 1 is that the styrene-acrylate emulsion used has a Dv50 of approximately 0.5 μm and a weight-average molecular weight of approximately 270,000. The silicon-carbon composite material used includes porous hard carbon and silicon-containing materials located in the pores and on the surface of the porous carbon. Some of the silicon-containing materials are crystalline silicon with a Dv50 particle size of 9 μm, a BET specific surface area of approximately 2.2 m² / g, a silicon element mass ratio of 30%, and a powder resistivity of 4 Ω·cm. The mass ratio of the second graphite material, silicon-carbon composite material, SP conductive carbon black, carbon nanotubes, sodium carboxymethyl cellulose, and styrene-acrylate emulsion is 57.6:38:1:0.5:0.5:2.4, resulting in a silicon element mass content of approximately 11% in the second negative electrode active layer. The rest is the same as in Example 1.
[0270] Example 14
[0271] The difference from Example 1 is that the styrene-acrylate emulsion used has a Dv50 of approximately 0.7 μm and a weight-average molecular weight of approximately 400,000. The silicon-carbon composite material used includes porous hard carbon and silicon-containing materials located in the pores and on the surface of the porous carbon. Some of the silicon-containing materials are crystalline silicon with a Dv50 particle size of 9 μm, a BET specific surface area of approximately 2.2 m² / g, a silicon element mass ratio of 70%, and a powder resistivity of 17 Ω·cm. The mass ratio of the second graphite material, silicon-carbon composite material, SP conductive carbon black, carbon nanotubes, sodium carboxymethyl cellulose, and styrene-acrylate emulsion is 5756.5:38:1:0.5:0.5:3.5, resulting in a silicon element mass content of approximately 27% in the second negative electrode active layer. The rest is the same as in Example 1.
[0272] Example 15
[0273] The difference from Example 1 is that the styrene-acrylate emulsion used has a Dv50 of approximately 0.7 μm and a weight-average molecular weight of approximately 400,000. The silicon-carbon composite material used includes porous hard carbon and silicon-containing materials located in the pores and on the surface of the porous carbon. Some of the silicon-containing materials are crystalline silicon with a Dv50 particle size of 9 μm, a BET specific surface area of approximately 2.2 m² / g, a silicon element mass ratio of 70%, and a powder resistivity of 17 Ω·cm. The mass ratio of silicon-carbon composite material, SP conductive carbon black, carbon nanotubes, sodium carboxymethyl cellulose, and styrene-acrylate emulsion is 91:1:0.5:0.5:7, resulting in a silicon element mass content of approximately 64% in the second negative electrode active layer. The rest is the same as in Example 1.
[0274] The test results are recorded in Table 4.
[0275] Table 4
[0276] Average particle size of the second binder / μm Cohesion N / m Capacity retention rate / % Charging time / min Example 1 0.5 160 97 8.7 Example 13 0.4 130 93 13.2 Example 14 0.6 110 87 13.2 Example 15 0.6 125 89 10.1
[0277] In Examples 14 and 15, the increased silicon content led to a deterioration in cycling performance compared to Example 1. However, although Example 15 had a higher silicon content, it used more of the second binder than Example 14, resulting in better overall performance.
[0278] Examples 16 to 18 investigate the effect of conductive agents on the performance of battery cells.
[0279] Example 16
[0280] The only difference from Example 1 is that the mass ratio of the first graphite material, SP conductive carbon black, sodium carboxymethyl cellulose, and styrene-butadiene rubber in the first negative electrode slurry is adjusted to 97.5:1:1:0.5. Everything else is the same as in Example 1.
[0281] Example 17
[0282] The only difference from Example 1 is that the mass ratio of the active material formed by mixing the second graphite material and the silicon-based silicon-carbon composite material in the second negative electrode slurry, SP conductive carbon black, carbon nanotubes, sodium carboxymethyl cellulose, and styrene-acrylate emulsion is adjusted to 94.5:1.6:0.4:0.5:3. Everything else is the same as in Example 1.
[0283] Example 18
[0284] The only difference from Example 1 is that the mass ratio of the active material formed by mixing the second graphite material and the silicon-based silicon-carbon composite material in the second negative electrode slurry, SP conductive carbon black, carbon nanotubes, sodium carboxymethyl cellulose, and styrene-acrylate emulsion is adjusted to 95.5:0.85:0.15:0.5:3. Everything else is the same as in Example 1.
[0285] The test results are recorded in Table 5.
[0286] Table 5
[0287] Cohesion N / m Capacity retention rate / % Charging time / min Example 1 160 97 8.7 Example 16 135 92 10.1 Example 17 155 94 9.1 Example 18 140 90 10.7
[0288] The comparison of Examples 1, 16 to 18 shows that increasing the carbon nanotube content in the conductive agent helps to shorten the charging time.
[0289] Although this application has been described with reference to preferred embodiments, various modifications can be made thereto and components can be replaced with equivalents without departing from the scope of this application. In particular, the technical features mentioned in the various embodiments can be combined in any manner, provided there is no structural conflict. This application is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.
Claims
1. A battery cell, comprising a negative electrode sheet, the negative electrode sheet comprising a negative current collector and a negative active layer disposed on at least one side of the negative current collector, the negative active layer comprising a first negative active layer and a second negative active layer, the first negative active layer being located between the negative current collector and the second negative active layer. The negative electrode active layer includes a negative electrode active material, which includes graphite material and silicon-based material. The silicon content in the second negative electrode active layer is greater than the silicon content in the first negative electrode active layer, and the ratio of the silicon mass in the second negative electrode active layer to the silicon mass in the first negative electrode active layer is greater than or equal to 50%. The second negative electrode active layer further includes a second binder, the average particle size of which is in the range of 0.3 μm to 0.7 μm.
2. The battery cell according to claim 1, wherein, The first negative electrode active layer further includes a first binder, and the first binder and the second binder satisfy at least one of the following conditions: (1) The average particle size of the second adhesive is greater than or equal to the average particle size of the first adhesive; (2) The weight-average molecular weight of the second adhesive is greater than or equal to the weight-average molecular weight of the first adhesive; (3) The mass content of the second adhesive in the second negative electrode active layer is more than 1.5 times the mass content of the first adhesive in the first negative electrode active layer; optionally, the mass content of the second adhesive in the second negative electrode active layer is more than 2 times the mass content of the first adhesive in the first negative electrode active layer.
3. The battery cell according to claim 2, wherein, The average particle size of the first adhesive is in the range of 0.01 μm to 0.6 μm.
4. The battery cell according to claim 2 or 3, wherein, The weight-average molecular weight of the second adhesive is 2 × 10⁻⁶. 5 ~5×10 5 Within the range, and / or, the weight-average molecular weight of the first adhesive is 1 × 10⁻⁶. 5 ~2×10 5 Within the range.
5. The battery cell according to any one of claims 2 to 4, wherein, The first binder has a mass content of 0.5% to 3% in the first negative electrode active layer, and / or the second binder has a mass content of 1.5% to 7% in the second negative electrode active layer.
6. The battery cell according to any one of claims 2 to 5, wherein, The first adhesive and the second adhesive each independently contain hydrophilic groups; optionally, the hydrophilic groups include at least one of sulfonic acid groups, phosphate groups, hydroxyl groups, carboxyl groups, amide groups, amino groups, aldehyde groups, carbonyl groups, cyano groups, and acid anhydrides; optionally, the first adhesive and the second adhesive each independently include one or more of polystyrene-butadiene copolymers and their modifications, polystyrene-acrylates and their modifications, polyacrylate copolymers and their modifications, butadiene-acrylonitrile copolymers and their modifications, polytetrafluoroethylene and its modifications, polyvinylidene fluoride and its modifications, styrene-butadiene rubber (SBR), and acrylonitrile-butadiene-styrene copolymer (ABS).
7. The battery cell according to any one of claims 1 to 6, wherein, The silicon content in the second negative electrode active layer is 10% to 70% by mass.
8. The battery cell according to any one of claims 1 to 7, wherein, In the second negative electrode active layer, the ratio of the mass content of the second binder to the mass content of silicon is 0.07~0.
35.
9. The battery cell according to any one of claims 1 to 8, wherein, The silicon content in the first negative electrode active layer is 0%~20% by mass.
10. The battery cell according to any one of claims 1 to 9, wherein, The thickness ratio of the first negative electrode active layer to the second negative electrode active layer is 9:1 to 1:9, and the thickness of the first negative electrode active layer is 20-200 μm.
11. The battery cell according to any one of claims 1 to 10, wherein, The silicon-based material includes one or more of elemental silicon, silicon-carbon composite materials, or silicon-oxygen composites.
12. The battery cell according to any one of claims 1 to 11, wherein, The silicon-based material contains 30%-70% silicon by mass.
13. The battery cell according to any one of claims 1 to 12, wherein, The silicon-based material includes a silicon-carbon composite material, which satisfies one or more of the following characteristics: (1) The silicon-carbon composite material includes porous carbon and crystalline silicon located in the pores and surface of the porous carbon. Optionally, the porous carbon is hard carbon. (2) The silicon-carbon composite material further includes a carbon-containing coating layer, which is located on the surface of the porous carbon and / or the crystalline silicon; (3) The average particle size of the silicon-carbon composite material is 2μm-15μm, and can be selected as 7μm-11μm; (4) The powder resistivity of the silicon-carbon composite material at 8 MPa is 4 Ω·cm - 17 Ω·cm; (5) The BET specific surface area of the silicon-carbon composite material is 1.0 m². 2 / g - 6.7 m 2 / g.
14. The battery cell according to any one of claims 1 to 13, wherein, The negative electrode active layer also includes a conductive agent, which includes one or more of carbon black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
15. The battery cell according to claim 14, wherein, The mass content of the conductive agent in the first negative electrode active layer is 0.05%-1%, and the mass content of the conductive agent in the second negative electrode active layer is 0.05%-2%.
16. The battery cell according to claim 14 or 15, wherein, The conductive agent in the second negative electrode active layer includes carbon black and carbon nanotubes, and the mass ratio of carbon black to carbon nanotubes is 6:4-9:1, which can be selected as 8:2-8.5:1.
5.
17. The battery cell according to any one of claims 1 to 16, wherein, The graphite material includes a first graphite material and a second graphite material, wherein the first graphite material is disposed in the first negative electrode active layer, and the second graphite material is disposed in the second negative electrode active layer, and the first graphite material and the second graphite material satisfy at least one of the following conditions: (1) The average particle size of the second graphite material is lower than that of the first graphite material; (2) The tap density of the second graphite material is greater than that of the first graphite material; (3) The first graphite material and the second graphite material are each independently selected from at least one of artificial graphite and natural graphite; optionally, the first graphite material includes natural graphite and the second graphite includes artificial graphite.
18. The battery cell according to any one of claims 1 to 17, wherein, The negative electrode sheet includes a base coating layer disposed between the negative current collector and the negative active layer. The base coating layer includes a base conductive agent and a base binder.
19. The battery cell according to any one of claims 1 to 18, wherein, The battery cell further includes a positive electrode sheet, which includes a positive current collector and a positive active layer disposed on at least one side of the positive current collector. The positive active layer includes a positive active material, which includes a nickel-containing lithium transition metal oxide or a lithium phosphate.
20. The battery cell according to claim 19, wherein, The nickel-containing lithium transition metal oxides include lithium-containing nickel-cobalt-manganese oxides and lithium-containing nickel-cobalt-aluminum oxides.
21. The battery cell according to claim 19 or 20, wherein, The nickel-containing nickel-cobalt-manganese oxide includes the compound Li a Ni b Co c Mn d M e O 2-f Wherein, M includes one or more elements selected from Al, Fe, Ti, Mg, Zr, Cr, Ga, Cu, Zn, Nb, and B; The value of 'a' can be any value in the range of 0.7-1.1, and can be selected as any value in the range of 0.8-1.
1. The value of b is any value in the range of 0.45-0.97, and can be selected as any value in the range of 0.8-0.97, and can be further selected as any value in the range of 0.85-0.95; The value of c is any value in the range of 0.02-0.25, and can be selected as any value in the range of 0.02-0.2; The value of d is any value in the range of 0.05-0.5, and can be selected as any value in the range of 0.05-0.48; The value of e is any value in the range of 0 to 0.2, and can be selected as any value in the range of 0.001 to 0.2; f can be any value in the range of 0-0.3, and can be selected as any value in the range of 0-0.
2.
22. The battery cell according to any one of claims 19 to 21, wherein, The positive electrode active material includes primary particles and / or secondary particles. Optionally, based on the total cross-sectional area of the positive electrode active material, the cross-sectional area of the primary particles accounts for more than 30%.
23. A battery device comprising a battery cell according to any one of claims 1 to 22.
24. An electrical device comprising a battery cell according to any one of claims 1 to 22, or a battery device according to claim 23, wherein the battery cell or the battery device is used to store or provide electrical energy.