Negative electrode sheet and battery

CN123162137APending Publication Date: 2026-11-24NANTONG MORLUS TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611667457.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-27
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

[0004]针对现有技术中石墨负极电池在高温工况下无法同时兼顾循环性能以及动力学性能的问题,提供一种负极片及电池

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_3
    Figure SMS_3
  • Figure SMS_4
    Figure SMS_4
  • Figure SMS_5
    Figure SMS_5
Patent Text Reader

Abstract

This invention provides a negative electrode sheet and a battery, comprising a negative electrode current collector and a negative electrode active material layer, wherein the negative electrode active material layer comprises a negative electrode active material, a binder, and a conductive agent; the negative electrode sheet satisfies the following condition: 5≤d×S1 / S2×A sv ×ω2 / ω3≤62; The negative electrode provided by this invention, through the above multi-component synergy, satisfies 5≤d×S1 / S2×A sv Based on ×ω2 / ω3≤62, the transport dynamics of ions and electrons can be further optimized, thereby achieving a better balance between battery cycle performance and dynamic performance under high-temperature conditions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of battery technology, and more particularly to a negative electrode and a battery. Background Technology

[0002] High temperatures accelerate the degradation of graphite anode materials and the interfacial reaction between the anode and the electrolyte, leading to a rapid decline in battery life. By controlling the particle size (large) and specific surface area (small) of graphite, side reactions can be reduced and cycle life improved, but this will increase impedance and reduce kinetic performance.

[0003] High-temperature operating conditions are a key factor limiting the cycle life and overall performance of lithium-ion batteries. On the one hand, high temperatures directly accelerate the structural degradation of the graphite anode material, disrupting the original stable structure of the electrode and causing performance degradation of the anode itself. On the other hand, high temperatures significantly intensify interfacial side reactions between the graphite anode and the electrolyte, exacerbating problems such as interfacial film damage and continuous electrolyte decomposition and consumption. The combined negative effects of these two factors ultimately lead to a rapid decline in the overall cycle life of the battery. To address the battery performance degradation caused by high temperatures, performance optimization can be achieved by adjusting the physical structural parameters of the graphite anode. For example, appropriately increasing the graphite particle size and reducing its specific surface area can effectively reduce the contact area between the anode and the electrolyte, suppress the occurrence of interfacial side reactions, and improve the high-temperature cycle stability and lifespan of the battery. However, this regulation method has a certain impact on other battery performance. Specifically, as the graphite particle size increases and the specific surface area decreases, the ion transport channels of the negative electrode will decrease accordingly and the active sites of interfacial reactions will decrease. This will directly increase the internal impedance of the battery, weaken the charge transfer kinetics of the electrode, and ultimately cause a decline in the battery's kinetic performance. Its performance under conditions such as high-rate charge and discharge will be reduced. Summary of the Invention

[0004] To address the problem that existing graphite anode batteries cannot simultaneously achieve good cycle performance and kinetic performance under high-temperature conditions, a new anode sheet and battery are provided.

[0005] The technical solution adopted by the present invention to solve the above-mentioned technical problems is as follows: On one hand, the present invention provides a negative electrode sheet, including a negative electrode current collector and a negative electrode active material layer, wherein the negative electrode active material layer includes a negative electrode active material, a binder and a conductive agent; The negative electrode sheet meets the following conditions: 5≤d×S1 / S2×A sv ×ω2 / ω3≤62; Wherein, d is the aggregate particle size of the negative electrode active material, in μm; S1 is the specific surface area of ​​the negative electrode active material, in m². 2 / g; S2 is the specific surface area of ​​the conductive agent, in m². 2 / g; A sv The oil absorption value of the conductive agent is expressed in mL / 100g. ω2 represents the mass percentage of the conductive agent, expressed as % . ω3 represents the mass percentage of the adhesive, in percentages (%).

[0006] Optionally, the negative electrode sheet satisfies the following conditions: 6≤d×S1 / S2×A sv ×ω2 / ω3≤50.

[0007] Optionally, based on the total mass of the negative electrode active material layer, the mass percentage ω2 of the conductive agent is 0.5% to 2.5%; and / or, The mass percentage ω3 of the adhesive is 1.5%~4.0%.

[0008] Optionally, the specific surface area S1 of the negative electrode active material is 1.0~1.7 m². 2 / g; and / or, The specific surface area S2 of the conductive agent is 50~250 m². 2 / g.

[0009] Optionally, the oil absorption value A of the conductive agent... sv It is 160~280 mL / 100g.

[0010] Optionally, the aggregate particle size d of the negative electrode active material is 6.0~12.0μm.

[0011] Optionally, the negative electrode active material includes one or more of single particles and secondary particles.

[0012] Optionally, the particle size of the negative electrode active material satisfies the following condition: 7≤d×(D 90 -D 10 ) / D 50 ≤16; Among them, D 10 This refers to the particle size value corresponding to a particle volume percentage of 10% in the negative electrode active material, in μm. D 90 This refers to the particle size value corresponding to a particle volume percentage of 90% in the negative electrode active material, in μm. D 50 This refers to the particle size value corresponding to a particle volume percentage of 50% in the negative electrode active material, expressed in μm.

[0013] Optionally, in the negative electrode active material, D 10 Its thickness is 4~7.5μm; D 50 The thickness is 8~14μm; D 90 It is 15~25μm.

[0014] Optionally, in the negative electrode active material, the mass ratio of single particles to secondary particles is (100:0) to (40:60).

[0015] Optionally, the negative electrode active material includes graphite, with a graphitization degree G of 92% to 95.5%; The limiting compaction density σ of the negative electrode active material is 1.6~1.8 g / cm³. 3 .

[0016] Optionally, the mass percentage ω1 of the negative electrode active material is 93.5% to 98% based on the total mass of the negative electrode active material layer.

[0017] Optionally, in the negative electrode sheet, the loading ε of the negative electrode active material layer on either side of the negative electrode current collector is 80~250 g / m². 2 ; and / or, The bulk density ρ of the negative electrode active material layer on either side of the negative electrode current collector is 1.4~1.65 g / cm³. 3 .

[0018] Optionally, the negative electrode sheet satisfies the following conditions: 135≤ε×ρ≤325.

[0019] Optionally, the peel strength F between the negative electrode current collector and the negative electrode active material layer is 6~100 N / m.

[0020] Optionally, the longitudinal resistivity R of the negative electrode is 0.01~0.2Ω•cm.

[0021] On the other hand, the present invention provides a battery including the aforementioned negative electrode.

[0022] The beneficial effects of this application are as follows: The negative electrode sheet provided in this application includes a negative electrode current collector and a negative electrode active material layer. The negative electrode active material layer includes a negative electrode active material, a binder, and a conductive agent. The negative electrode active material, as the core component, has aggregate particle size and specific surface area that directly affect high-temperature stability and interfacial reactions. Specifically, appropriately increasing its particle size and decreasing its specific surface area can reduce the contact area between the negative electrode and the electrolyte, effectively suppressing material degradation and interfacial side reactions at high temperatures, and improving cycle life. The conductive agent plays a role in conductivity and mass transfer due to its specific surface area, oil absorption value, and addition ratio. A higher specific surface area and oil absorption value are beneficial for forming a continuous conductive network, wetting the electrolyte, and shortening the charge and ion transport paths. Furthermore, based on extensive testing, limiting the appropriate mass ratio of the conductive agent can significantly reduce electrode impedance and optimize kinetic performance. The binder can bond and fix the active material and the conductive agent, maintaining the overall structural integrity of the electrode. Furthermore, through extensive preliminary experiments, it has been verified that when the aggregate particle size d of the negative electrode active material, the specific surface area S1 of the negative electrode active material, the specific surface area S2 of the conductive agent, and the oil absorption value A of the conductive agent are controlled... sv The mass percentage content ω2 of the conductive agent and the mass percentage content ω3 of the binder satisfy 5 ≤ d × S1 / S2 × A sv When ×ω2 / ω3≤62, the transport dynamics of ions and electrons can be further optimized, thereby achieving a better balance between battery cycle performance and dynamic performance under high-temperature conditions. Detailed Implementation

[0023] To make the technical problems solved, the technical solutions, and the beneficial effects of this invention clearer, the invention will be further described in detail below with reference to embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.

[0024] This invention provides a negative electrode sheet, comprising a negative electrode current collector and a negative electrode active material layer, wherein the negative electrode active material layer comprises a negative electrode active material, a binder, and a conductive agent; The negative electrode sheet meets the following conditions: 5≤d×S1 / S2×A sv ×ω2 / ω3≤62; Wherein, d is the aggregate particle size of the negative electrode active material, in μm; S1 is the specific surface area of ​​the negative electrode active material, in m². 2 / g; S2 is the specific surface area of ​​the conductive agent, in m². 2 / g; A sv The oil absorption value of the conductive agent is expressed in mL / 100g. ω2 represents the mass percentage of the conductive agent, expressed as % . ω3 represents the mass percentage of the adhesive, in percentages (%).

[0025] It should be noted that verification revealed that a single parameter in the above relationships cannot simultaneously consider both battery cycle life and kinetic performance. Specifically, increasing the aggregate particle size d of the negative electrode active material can effectively optimize battery cycle life, but it will increase electrode impedance and degrade kinetic performance. Increasing the specific surface area S1 of the negative electrode active material can improve battery kinetic performance, but it will exacerbate interfacial side reactions and cause cycle life degradation. Increasing the specific surface area S2 of the conductive agent can improve electrode conductivity and optimize kinetic performance, but it will disrupt interfacial stability and reduce cycle life. Furthermore, in the S1 / S2 ratio, a larger S1 / S2 ratio indicates poorer electrode conductivity, while a smaller ratio, although exhibiting excellent conductivity, sacrifices cycle life. The oil absorption value A of the conductive agent... sv Improving the electrolyte adsorption and retention capacity of the electrode can enhance ion transport and optimize kinetic performance, but A sv Increasing the percentage of conductive agent (ω2) usually accompanies a decrease in S2, which in turn affects conductivity and kinetic performance. In terms of component ratio, increasing the mass percentage of conductive agent (ω2) can strengthen the electrode conductive network and improve kinetic performance, but an excessively high proportion of conductive agent will affect the battery cycle stability. Increasing the mass percentage of binder (ω3) can enhance the electrode bonding strength and maintain the integrity of the electrode structure, which is beneficial for long cycle performance, but excessive binder will increase electrode impedance and drag down kinetic performance. Among them, the ratio of conductive agent to binder (ω2 / ω3) also has a trade-off. The larger the ω2 / ω3 ratio, the better the conductivity but the worse the cycle life. The smaller the ratio, the better the cycle performance, but the kinetic performance is greatly weakened. If the kinetic performance cannot meet the requirements of rate use, it will indirectly damage the overall life of the battery.

[0026] The negative electrode sheet provided in this application includes a negative electrode current collector and a negative electrode active material layer. The negative electrode active material layer includes a negative electrode active material, a binder, and a conductive agent. The negative electrode active material, as the core component, has aggregate particle size and specific surface area that directly affect high-temperature stability and interfacial reactions. Specifically, appropriately increasing its particle size and decreasing its specific surface area can reduce the contact area between the negative electrode and the electrolyte, effectively suppressing material degradation and interfacial side reactions at high temperatures, and improving cycle life. The conductive agent plays a role in conductivity and mass transfer due to its specific surface area, oil absorption value, and addition ratio. A higher specific surface area and oil absorption value are beneficial for forming a continuous conductive network, wetting the electrolyte, and shortening the charge transport path. Furthermore, based on extensive testing, limiting the appropriate mass ratio of the conductive agent can significantly reduce electrode impedance and optimize kinetic performance. The binder can bond and fix the active material and the conductive agent, maintaining the overall structural integrity of the electrode. Furthermore, through extensive preliminary experiments, it has been verified that when the aggregate particle size d of the negative electrode active material, the specific surface area S1 of the negative electrode active material, the specific surface area S2 of the conductive agent, and the oil absorption value A of the conductive agent are controlled... sv The mass percentage content ω2 of the conductive agent and the mass percentage content ω3 of the binder satisfy 5 ≤ d × S1 / S2 × A sv When ×ω2 / ω3≤62, the transport dynamics of ions and electrons can be further optimized, thereby achieving a better balance between battery cycle performance and dynamic performance under high-temperature conditions.

[0027] In some embodiments, the negative electrode sheet satisfies the following conditions: 6≤d×S1 / S2×A sv ×ω2 / ω3≤50.

[0028] Specifically, compared to the above relationship, this embodiment further optimizes it. When the relationship is further satisfied, it is beneficial to better optimize the cycle performance and dynamic performance of the battery under high temperature conditions.

[0029] In some embodiments, the mass percentage ω2 of the conductive agent is 0.5% to 2.5% based on the total mass of the negative electrode active material layer; and / or, The mass percentage ω3 of the adhesive is 1.5%~4.0%.

[0030] Specifically, by controlling the mass percentage ω2 of the conductive agent to be between 0.5% and 2.5%, a complete and continuous conductive network can be formed, ensuring rapid electron conduction. If the mass percentage of the conductive agent ω2 is less than 0.5%, the proportion of conductive components is insufficient, and a continuous and complete conductive network cannot be formed inside the electrode. Electron transport between particles is hindered, the electrode ohmic impedance increases significantly, and the battery's dynamic performance and rate performance decrease significantly. If the mass percentage of the conductive agent ω2 is greater than 2.5%, the excess conductive agent will significantly increase the overall specific surface area of ​​the negative electrode, expand the contact interface with the electrolyte, exacerbate interfacial side reactions at high temperatures, accelerate material aging and electrolyte consumption, and cause the battery's cycle life to decline rapidly. At the same time, it will also reduce the proportion of active material and decrease the battery's effective capacity.

[0031] The mass percentage of the binder ω3 is controlled within the range of 1.5% to 4.0%, which can fully bond and fix the components, maintain the integrity of the electrode structure and mechanical stability, and meet the requirements of long-term cycle use. If the mass percentage of binder ω3 < 1.5%, the bonding force is insufficient. Under the volume expansion and contraction caused by repeated charging and discharging, the particles are prone to detachment, the electrode peels and delaminates, the electrode structure gradually fails, and the cycle life is directly shortened. If ω3 > 4.0%, the binder itself has poor conductivity. Excessive addition will coat the active particles and conductive sites, block the internal pores of the electrode, hinder electron conduction and lithium ion migration, resulting in increased internal resistance of the electrode, intensified polarization, and serious deterioration of battery dynamics and rate performance.

[0032] Further, the mass percentage content ω2 of the conductive agent includes, but is not limited to, 0.5%, 0.8%, 1.0%, 1.2%, 1.5%, 1.8%, 2.0%, 2.2%, or 2.5%. The mass percentage ω3 of the adhesive is, but is not limited to, 1.5%, 1.8%, 2.0%, 2.2%, 2.5%, 3.0%, 3.5%, 3.8%, or 4.0%.

[0033] The conductive agent includes at least one of carbon black, conductive graphite, carbon fiber, carbon nanotubes, and graphene; The adhesive includes at least one of rubber, polyvinylidene fluoride, polyimide, polyethylene, polypropylene, polyacrylic acid, polytetrafluoroethylene, polyacrylonitrile, polymethyl methacrylate, sodium carboxymethyl cellulose, and polyurethane.

[0034] In some embodiments, the specific surface area S1 of the negative electrode active material is 1.0~1.7 m². 2 / g; and / or, The specific surface area S2 of the conductive agent is 50~250 m². 2 / g.

[0035] Specifically, the specific surface area S1 of the negative electrode active material is limited to 1.0~1.7 m². 2 Within this range, the contact area between graphite and electrolyte can be effectively reduced, inhibiting interfacial side reactions under high-temperature conditions, slowing down material structure deterioration, and improving cycle stability; if the specific surface area S1 of the negative electrode active material is less than 1.0 m², the reaction can be stopped. 2 If the specific surface area S1 of the negative electrode active material is less than 1.7 m² / g, then the material surface has too few active sites, the electrolyte wetting is insufficient, the reaction interface for lithium ion insertion and extraction is insufficient, the ion migration resistance increases, and the battery kinetics and rate performance deteriorate significantly; if the specific surface area S1 of the negative electrode active material is greater than 1.7 m² / g, then the material surface has too few active sites, the electrolyte wetting is insufficient, the reaction interface for lithium ion insertion and extraction is insufficient, the ion migration resistance increases, and the battery kinetics and rate performance deteriorate significantly. 2 / g, the contact area between graphite and electrolyte increases significantly, and the interfacial side reactions and electrolyte decomposition are aggravated under high temperature environment. At the same time, too many by-products are easily generated, which continuously damage the electrode interface structure and cause the battery cycle life to decline rapidly.

[0036] The specific surface area S2 of the conductive agent is limited to 50~250 m².2 Within the range of / g, it can form a multi-dimensional conductive network, increase the charge conduction contact surface, and improve conductivity efficiency; if the specific surface area S2 of the conductive agent is less than 50 m² 2 / g, insufficient effective contact area of ​​the conductive agent makes it difficult to build a continuous multidimensional conductive network, obstructing the electron conduction path between particles, increasing the overall impedance of the electrode, and reducing the charge-discharge kinetic performance; if the specific surface area S2 of the conductive agent is greater than 250 m², 2 / g, the huge specific surface area of ​​the conductive agent will introduce a large number of additional interfaces, which will induce more electrolyte side reactions at high temperatures, accelerate electrolyte loss and interface film degradation, and significantly reduce battery cycle stability.

[0037] The specific surface area S1 of the negative electrode active material includes, but is not limited to, 1.0 m². 2 / g, 1.2 m 2 / g, 1.4 m 2 / g, 1.5 m 2 / g, 1.6 m 2 / g or 1.7 m 2 / g; The specific surface area S2 of the conductive agent includes, but is not limited to, 50 m². 2 / g、60 m 2 / g、80 m 2 / g, 100 m 2 / g、110 m 2 / g、120 m 2 / g, 150 m 2 / g、180 m 2 / g、200 m 2 / g、220 m 2 / g or 250 m 2 / g.

[0038] In some embodiments, the oil absorption value A of the conductive agent sv It is 160~280 mL / 100g.

[0039] Specifically, when the oil absorption value of the conductive agent is limited to the range of 160~280 mL / 100g, the conductive agent has excellent electrolyte adsorption and retention capacity, which can improve the overall wettability of the electrode, ensure the smooth flow of lithium-ion transport channels, and improve rate capability and kinetic performance. When the oil absorption value is within a reasonable range, it can avoid uneven electrolyte distribution and local mass transfer caused by an oil absorption value that is too low (below 160 mL / 100g), and it can also prevent excessive accumulation of electrolyte caused by an oil absorption value that is too high (above 280 mL / 100g), which would aggravate interfacial side reactions at high temperatures, thus achieving a balance between electrolyte retention capacity and cycle stability.

[0040] Furthermore, the oil absorption value A of the conductive agent sv Including but not limited to 160 mL / 100g, 180 mL / 100g, 200 mL / 100g, 220 mL / 100g, 240 mL / 100g, 260 mL / 100g or 280 mL / 100g.

[0041] In some embodiments, the aggregate particle size d of the negative electrode active material is 6.0~12.0 μm.

[0042] Specifically, the aggregate particle size is controlled at 6.0~12.0μm. This aggregate particle size can reduce the overall specific surface area of ​​the material, reduce the contact interface between the electrolyte and graphite under high temperature environment, suppress side reactions and material decay, and extend cycle life. If the aggregate particle size d of the negative electrode active material is too small (less than 6.0 μm), the overall specific surface area of ​​the particles will increase significantly, the contact interface between graphite and electrolyte will increase, the interfacial side reactions will intensify at high temperatures, the electrolyte will continue to decompose, and the interfacial film will be repeatedly damaged and reconstructed, resulting in a rapid decline in battery cycle life. At the same time, the accumulation of fine particles is prone to forming narrow and tortuous pores, which increases the resistance to lithium-ion transport, increases the electrode impedance, and deteriorates the kinetics and rate performance. If the aggregate particle size d of the negative electrode active material is too large (greater than 12.0 μm), the contact points between particles will decrease and the gaps will become larger, the electron conduction path will become longer, and the ohmic impedance of the electrode will increase. Moreover, the internal lithium-ion diffusion distance of large particles increases, the lithium insertion and extraction kinetics will slow down, and the rate performance will decrease significantly. In addition, during the volume deformation process of repeated charge and discharge, the internal stress distribution of large particles is uneven, which can easily lead to particle cracking and pulverization. After long-term cycling, the stability of the electrode structure will deteriorate.

[0043] Furthermore, the aggregate particle size d of the negative electrode active material includes, but is not limited to, 6.0 μm, 7.0 μm, 8.0 μm, 9.0 μm, 10.0 μm, 11.0 μm or 12.0 μm.

[0044] In some embodiments, the negative electrode active material includes one or more of single particles and secondary particles.

[0045] Specifically, the secondary particles are formed by the agglomeration of aggregate particles of different sizes; Secondary particles, with their larger particle size, effectively increase the porosity of the electrode and improve its kinetic performance. However, secondary particles can increase interfacial side reactions and affect cycle life. Therefore, smaller aggregates and single particles are used to fill the gaps between secondary particles to optimize the internal porosity of the electrode, improve particle contact tightness, build a continuous and unobstructed charge transport channel, reduce the internal resistance of the electrode, and improve the conduction efficiency of lithium ions and electrons. Ultimately, this balances electrode structure stability, high-temperature cycle performance, and charge-discharge kinetic performance.

[0046] In some embodiments, the particle size of the negative electrode active material satisfies the following condition: 7≤d×(D 90 -D 10 ) / D 50 ≤16; Among them, D 10 This refers to the particle size value corresponding to a particle volume percentage of 10% in the negative electrode active material, in μm. D 90 This refers to the particle size value corresponding to a particle volume percentage of 90% in the negative electrode active material, in μm. D 50 This refers to the particle size value corresponding to a particle volume percentage of 50% in the negative electrode active material, expressed in μm.

[0047] Specifically, the particle size of the negative electrode active material is further limited to satisfy 7 ≤ d × (D 90 -D 10 ) / D 50 ≤16, This relationship characterizes the width of the particle size distribution of the negative electrode active material. A reasonable particle size distribution is conducive to achieving close packing of particles and optimizing the pore structure of the electrode. This ensures uniform electrolyte penetration and smooth lithium ion migration, improving kinetic performance. At the same time, it avoids uneven local pores and stress concentration caused by excessively wide particle size distribution, slows down particle pulverization and shedding during cycling, and enhances structural stability and cycle life at high temperatures.

[0048] In some embodiments, the negative electrode active material has a D1 ≥ 2.5 μm; D 99 ≤45μm; D1 is the particle size value corresponding to a particle volume percentage of 1% in the negative electrode active material, in μm. D 99 This refers to the particle size value corresponding to a particle volume percentage of 99% in the negative electrode active material, expressed in μm.

[0049] In some embodiments, in the negative electrode active material, D 10 Its thickness is 4~7.5μm; D 50 The thickness is 8~14μm; D 90 It is 15~25μm.

[0050] Specifically, the range of D in this interval 10 D 50 and D 90It can form a gradient of reasonable particle size distribution, with small particles filling the gaps between large particles, optimizing the electrode packing structure and pore system. While improving particle contact tightness, reducing contact resistance, and accelerating ion and electron transport, it controls the overall specific surface area of ​​the material at a reasonable level, effectively suppressing interfacial side reactions at high temperatures and ensuring cycle stability. If D 10 If the particle size is too small (less than 4μm), the high proportion of ultrafine particles will significantly increase the overall specific surface area, exacerbate electrolyte decomposition and side reactions, and impair cycle life; D 10 If the size is too large (greater than 7.5μm), there will be a lack of fine particles to fill the gaps, resulting in high electrode porosity, insufficient particle contact, increased impedance, and deteriorated kinetic performance. D 50 As the median particle size, a smaller value will result in finer overall particles and intensified interfacial reactions, while a larger value will result in coarser overall particles, increased ion diffusion distance, and increased conduction resistance. D 90 When the proportion of large-diameter particles is too small, it is difficult to effectively reduce the overall specific surface area, resulting in decreased high-temperature cycling stability. D 90 If the particles are too large, they are prone to stress concentration during charging and discharging deformation, which can cause the particles to crack and pulverize, damage the electrode structure, and ultimately lead to battery performance degradation.

[0051] Furthermore, the D 10 Including but not limited to 4μm, 5μm, 6μm, 7μm or 7.5μm; The D 50 Including but not limited to 8μm, 9μm, 10μm, 11μm, 12μm, 13μm or 14μm; The D 90 Including but not limited to 15μm, 16μm, 17μm, 18μm, 19μm, 20μm, 21μm, 22μm, 23μm, 24μm or 25μm.

[0052] In some embodiments, the mass ratio of single particles to secondary particles in the negative electrode active material is (100:0) to (40:60).

[0053] In the aforementioned negative electrode active material, the overall specific surface area, packing state, and pore structure of the material can be flexibly controlled by adjusting the ratio of single particles and secondary particles within a limited range. Specifically, when the proportion of single particles is increased, the high-temperature resistance to side reactions and cycle life are improved; while when the proportion of secondary particles is increased, the particle contact and conductive pathway can be optimized, and the kinetic performance can be improved.

[0054] In a preferred embodiment, the mass ratio of single particles to secondary particles is (100:0) to (60:40).

[0055] In some embodiments, the negative electrode active material comprises graphite, with a graphitization degree G of 92% to 95.5%; The graphite used is preferably made from needle coke, and under an optical microscope, the proportion of large sheet structure is 30%~50%, the proportion of fibrous structure is 40%~55%, and the proportion of mosaic structure is 5%~20%.

[0056] The limiting compaction density σ of the negative electrode active material is 1.6~1.8 g / cm³. 3 .

[0057] Specifically, the 92%~95.5% graphitization degree ensures the complete lamellar crystal structure of graphite, excellent electronic conductivity, strong reversibility of lithium-ion insertion and extraction, reduced polarization, and improved kinetic performance. Simultaneously, the crystal structure is stable and can withstand structural changes during high temperatures and long-term cycling; 1.6~1.8 g / cm³ 3 The compaction limit density can improve the energy density of the electrode while ensuring that there is a reasonable amount of porosity inside, taking into account both electrolyte storage and ion transport. It avoids pore collapse and mass transfer obstruction caused by excessive compaction, and also prevents poor particle contact and increased internal resistance caused by excessively low compaction.

[0058] The method for testing the degree of graphitization is as follows: ① Mix silicon powder and graphite in a 2:1 ratio until homogeneous. Weigh 1.2-1.6g of the sample onto the X-ray diffractometer sample stage, ensuring that the sample is flat on the sample stage. ② Test parameters: λ=1.54059Å, angle range 10~80°, step size 0.01°, scanning speed 10° / min; Calculated according to Bragg's equation D (004) : , i 1 = si(311), i 2 = C(004); ③ Calculate the degree of graphitization G according to the formula: The test method for the ultimate compaction density is as follows: ① Place 0.5~2.0g of sample in the sample stage and measure the compaction density under different pressures, with a pressure range of 1T~5T; ② The inflection point of the first derivative curve of the pressure compaction curve is taken as the ultimate compaction density.

[0059] In some embodiments, the mass percentage ω1 of the negative electrode active material is 93.5% to 98% based on the total mass of the negative electrode active material layer.

[0060] Specifically, the 93.5%~98% negative electrode active material ensures that the negative electrode has sufficient lithium storage active sites to guarantee battery capacity output; on the other hand, it reserves a reasonable proportion of conductive agent and binder to maintain the stability of the conductive network and electrode structure.

[0061] In some embodiments, the loading ε of the negative electrode active material layer on either side of the negative electrode current collector is 80~250 g / m². 2 ; and / or, The bulk density ρ of the negative electrode active material layer on either side of the negative electrode current collector is 1.4~1.65 g / cm³. 3 .

[0062] Specifically, 80~250 g / m 2 The loading can be matched to different capacity requirements, with an anode active material layer of 80~250 g / m². 2 A moderate loading rate can shorten the lithium-ion diffusion distance and optimize kinetic performance, while avoiding excessive loading (greater than 250 g / m²). 2 This can lead to cyclic failure due to excessively thick layers.

[0063] 1.4~1.65 g / cm 3 Bulk density can balance electrode density and porosity, which can improve the capacity per unit volume, ensure electrolyte penetration and gas discharge, and improve the overall stability under high temperature conditions.

[0064] In some embodiments, the negative electrode sheet satisfies the following conditions: 135≤ε×ρ≤325.

[0065] Specifically, the parameters of this relation comprehensively define the matching relationship between the loading and volume density of the active material layer. Within the defined range of the relation, the thickness, density, and porosity of the active material layer can achieve the optimal combination, which can ensure high energy storage capacity, maintain unobstructed ion and electron transport channels, and reduce polarization. At the same time, the uniform layer structure can disperse stress under cycling and high-temperature environments, suppress active material shedding and interfacial side reactions, and comprehensively improve the battery cycle life and rate performance.

[0066] In some embodiments, the peel strength F between the negative electrode current collector and the negative electrode active material layer is 6~100 N / m.

[0067] Specifically, a peel strength F of 6~100 N / m between the negative electrode current collector and the negative electrode active material layer ensures a firm bond between the active material layer and the current collector. During the volume expansion and contraction process of high temperature and repeated charging and discharging, it prevents the active material layer from falling off, maintains the integrity of the electrode structure, and ensures long-term cycle stability. It avoids interface detachment and interruption of the conductive circuit caused by excessively low peel strength (below 6 N / m), and reduces the flexibility of the electrode sheet and causes cracking under changing operating conditions due to excessively high peel strength (100 N / m).

[0068] In some embodiments, the longitudinal resistivity R of the negative electrode is 0.01~0.2Ω•cm.

[0069] Specifically, this resistivity range indicates that the conductive network inside the electrode is continuous and has good conductivity, with low electronic conduction resistance, which can significantly reduce ohmic polarization during charging and discharging, and improve the battery's rate performance and dynamic response speed. At the same time, the low and stable longitudinal resistivity of 0.01~0.2Ω•cm can reduce heat generation during current transmission, mitigate the effects of high-temperature environments, further reduce the probability of side reactions, and help improve the battery's high-temperature cycle life.

[0070] Another embodiment of the present invention provides a battery including the aforementioned negative electrode.

[0071] Specifically, the battery includes the negative electrode sheet provided in this application, comprising a negative electrode current collector and a negative electrode active material layer. The negative electrode active material layer comprises a negative electrode active material, a binder, and a conductive agent. The negative electrode active material, as the core component, has its aggregate particle size and specific surface area directly affecting high-temperature stability and interfacial reactions. Specifically, appropriately increasing its particle size and decreasing its specific surface area can reduce the contact area between the negative electrode and the electrolyte, effectively suppressing material degradation and interfacial side reactions at high temperatures, and improving cycle life. The conductive agent plays a role in conductivity and mass transfer due to its specific surface area, oil absorption value, and addition ratio. A higher specific surface area and oil absorption value are beneficial for forming a continuous conductive network, wetting the electrolyte, and shortening the charge transport path. Furthermore, based on extensive testing, limiting the appropriate mass ratio of the conductive agent can significantly reduce electrode impedance and optimize kinetic performance. The binder can bond and fix the active material and the conductive agent, maintaining the overall structural integrity of the electrode. Furthermore, through extensive preliminary experiments, it has been verified that when the aggregate particle size d of the negative electrode active material, the specific surface area S1 of the negative electrode active material, the specific surface area S2 of the conductive agent, and the oil absorption value A of the conductive agent are controlled... sv The mass percentage content ω2 of the conductive agent and the mass percentage content ω3 of the binder satisfy 5 ≤ d × S1 / S2 × A svWhen ×ω2 / ω3≤62, the transport dynamics of ions and electrons can be further optimized, thereby achieving a better balance between battery cycle performance and dynamic performance under high-temperature conditions.

[0072] The present invention will be further illustrated by the following examples.

[0073] Table 1 Continued from Table 1 Table 2 Continued from Table 2 Example 1 This embodiment illustrates a negative electrode sheet and battery disclosed in this invention. The preparation of the negative electrode sheet and battery includes the following steps: Preparation of negative electrode sheet The negative electrode active material (graphite), conductive agent carbon black, binder styrene-butadiene rubber, and sodium carboxymethyl cellulose were thoroughly mixed in deionized water at a weight ratio of 95.4:1.5:1.5:1.6 to obtain the negative electrode slurry. The negative electrode slurry is evenly coated onto copper foil, and after drying, cold pressing, slitting, sheet making, welding tabs, and adhesive bonding, the negative electrode sheet is obtained. Among them, the d / μm and S1 / m of the negative electrode 2 / g、S2 / m 2 / g、A sv / mL / 100g, ω2 / %, ω3 / %, D 10 / μm、D 50 / μm、D 90 / μm、ε g / m 2 ρ g / cm 3 All are recorded in Table 1.

[0074] Preparation of positive electrode sheet The positive electrode active material lithium iron phosphate, conductive agent SP, and binder PVDF were thoroughly mixed in NMP solvent at a weight ratio of 96.5:1.5:2.0 to obtain the positive electrode slurry. The positive electrode slurry is uniformly coated onto aluminum foil, and then the positive electrode sheet is obtained through processes such as drying, cold pressing, slitting, sheet making, welding tabs, and applying adhesive.

[0075] Battery manufacturing The positive electrode, separator, and negative electrode are stacked in sequence to prepare the battery cell; After liquid injection, the battery is encapsulated and formed to obtain a lithium-ion battery.

[0076] Examples 2-35 Examples 2-35 illustrate a negative electrode sheet and battery disclosed in this invention. The preparation of the negative electrode sheet and battery includes most of the operations in Example 1, except that: In Examples 2-35, d / μm and S1 / m 2 / g、S2 / m 2 / g、A sv / mL / 100g, ω2 / %, ω3 / %, D 10 / μm、D 50 / μm、D 90 / μm、ε g / m 2 ρ g / cm 3 d×S1 / S2×A sv ×ω2 / ω3、d×(D 90 -D 10 ) / D 50 Both ε×ρ are based on Table 1.

[0077] Comparative Examples 1-10 Comparative Examples 1-10 illustrate a negative electrode sheet and battery disclosed in this invention. The preparation of the negative electrode sheet and battery includes most of the operations in Example 1, except that: Comparative Examples 1-10: d / μm, S1 / m 2 / g、S2 / m 2 / g、A sv / mL / 100g, ω2 / %, ω3 / %, D 10 / μm、D 50 / μm、D 90 / μm、ε g / m 2 ρ g / cm 3 d×S1 / S2×A sv ×ω2 / ω3、d×(D 90 -D 10 ) / D 50 Both ε×ρ are based on Table 1.

[0078] Performance testing The following performance tests were performed on Examples 1-35 and Comparative Examples 1-10 prepared above: DC impedance DCIR: At 25±2℃, the battery under test is charged to 27% SOC, left to stand for 10 minutes, and the voltage V1 at the end of the stand is recorded. Then, it is charged at a 2C current for 10 seconds, and the voltage V2 at the end of the charge is recorded. The DCIR value is calculated according to the formula DCIR=(V2-V1) / 2C, and the unit is mΩ. Cycle life: The battery under test was placed in a constant temperature environment of 55±2℃. The battery under test was charged to 3.65V at a constant current and constant voltage of 0.5C, and the cutoff current was 0.05C. After resting for 30 minutes, it was discharged to 2.5V at a constant current of 0.5C. The test was repeated in this cycle. The capacity retention rate of the 1000th test was C1000 / C1*100%. Energy density: Record the weight m of the battery under test. Place the battery under test in a constant temperature environment of 25±2℃ and charge it to 3.65V at a constant current and constant voltage of 0.5C. The cutoff current is 0.05C. Let it rest for 30 minutes, and then discharge it to 2.5V at a constant current of 0.5C. Repeat the above steps 3 times and record the average value E of the discharge energy of the 3 times. The energy density is the ratio of E / m, and the unit is Wh / kg.

[0079] The test results are entered into Table 3.

[0080] Table 3 Continued from Table 3 As can be seen from the test results in Table 3, the particle size d of the anode active material aggregate in Examples 1-5 gradually increased (from 6 μm to 12 μm). In terms of performance, the DCIR slowly increased with the increase of aggregate particle size (0.50 to 0.55 mΩ), and the cycle capacity retention rate remained relatively stable at 88.0%~88.30%. The energy density showed a slight decrease. It is speculated that the increase of aggregate particle size d reduces the total specific surface area of ​​the anode active material and reduces the side reactions at the electrolyte interface. Therefore, the high-temperature cycle stability remains basically unchanged. However, the lithium ion diffusion path inside the larger particles becomes longer, the contact points between particles decrease, the ion transport resistance increases, and the DC impedance increases slightly. When the particle size continues to increase to 12 μm, the particle packing voids become larger, the compaction difficulty increases, the proportion of effective active material decreases, and the energy density decreases.

[0081] In Examples 6-9, the specific surface area S1 of the negative electrode active material gradually increases, and correspondingly, the DCIR continuously decreases (from 0.53 to 0.46 mΩ), the high-temperature capacity retention rate decreases slightly, and the energy density gradually increases. It is speculated that the reason is that after the specific surface area S1 increases, there are more lithium intercalation active sites on the surface of the negative electrode active material, the electrolyte wetting is more sufficient, the lithium ion migration resistance is reduced, the utilization efficiency of the conductive network is improved, the impedance is reduced, and the rate and energy density are optimized. However, the larger specific surface area expands the contact interface between the negative electrode active material and the electrolyte, the interface film continues to break down at high temperatures, the electrolyte decomposition side reaction is aggravated, and the long-term cycle capacity shows a certain degree of decay.

[0082] In Examples 10-14, the increase in the specific surface area of ​​the conductive agent and the decrease in the oil absorption value resulted in a continuous decrease in the DCIR (from 0.50 to 0.44 mΩ), a continuous decrease in the high-temperature cycling retention rate, and an increase in the energy density. The presumed reason is that a higher S2 content in the conductive agent makes it easier to form a multidimensional continuous conductive network, providing ample electron conduction channels and continuously reducing the ohmic impedance of the electrode. However, the high specific surface area of ​​the conductive agent introduces a large number of additional interfaces, and simultaneously, due to A... sv The decrease leads to a decline in the electrolyte retention capacity of the electrode, uneven electrolyte distribution, a significant increase in high-temperature side reactions, and a continuous deterioration in cycle life. However, due to the increased porosity of the conductive agent, it can accommodate more electrolyte, resulting in a slight increase in discharge energy. In Example 14, the relationship d×S1 / S2×A of this application is satisfied. sv The lower limit of ×ω2 / ω3 (d×S1 / S2×A) sv (×ω2 / ω3=5), the cycle performance is worse than other embodiments, but still better than the comparative example.

[0083] Examples 15-17 Conductive Agent A sv As the concentration gradually increased from 160 mL / 100g to 280 mL / 100g, the DCIR continuously decreased (from 0.55 to 0.48 mΩ) in the corresponding performance tests, while the high-temperature capacity retention gradually increased, and the energy density also improved. This is because A... sv The higher the electrolyte content, the stronger the adsorption and liquid retention capacity of the conductive agent, the better the permeability of the ion transport channels inside the electrode, the smaller the concentration polarization, and the lower the impedance. Sufficient electrolyte can buffer local liquid deficiency at the interface under high temperature and suppress the concentrated generation of side reactions, thus significantly improving the high-temperature cycling stability. The increase in electrolyte retention also ensures the full insertion and extraction of lithium in the negative electrode active material, so the energy density is optimized simultaneously.

[0084] In Examples 18-21, as the amount of conductive agent added (ω2) gradually increased from 0.5% to 2.5%, the DCIR continuously decreased, the high-temperature capacity retention rate showed a trend of first increasing and then decreasing, and the energy density decreased. When ω2 increased from 0.5% to 1.5%, the conductive network changed from discontinuous to complete and continuous, the impedance decreased significantly, and the cycle performance was optimized simultaneously. After ω2 exceeded 1.5%, the excess conductive agent significantly increased the total specific surface area of ​​the system, the high-temperature side reactions intensified, and the cycle life began to decline. At the same time, the conductive agent squeezed out the proportion of negative electrode active material, the effective lithium storage component of the battery decreased, and the energy density continued to decline.

[0085] In Examples 22-24, the negative electrode active material D 10 As the concentration gradually increases, the DCIR does not change significantly, but it shows an overall increasing trend. The high-temperature capacity retention rate continues to improve due to the increasing concentration of the anode active material D. 10 Represents the proportion of fine particles, and the negative electrode active material D 10Increasing the size means fewer particles of ultrafine negative electrode active material, a lower overall specific surface area, fewer high-temperature interfacial side reactions, and continuously improved cycle stability; however, the lack of fine particles to fill the gaps between large particles reduces the tightness of electrode particle contact, resulting in higher porosity and increased resistance to electron conduction.

[0086] In Examples 25, 26, and 27, d×S1 / S2×A sv With ×ω2 / ω3 between 22 and 27, the high-temperature cycling retention rate remains stable at over 87%. The particle size distribution of Example 28 is too wide, and d×(D 90 -D 10 ) / D 50 =18, exceeding the limit of this application (7≤d×(D)). 90 -D 10 ) / D 50 In the range of ≤16), the DCIR increases significantly to 0.58mΩ, and the capacity retention rate decreases to 84.42%. This is because an excessively wide particle size distribution will cause uneven local porosity of the electrode, concentrated charging and discharging stress, and large particles are prone to cracking and pulverization. At the same time, local electrolyte enrichment exacerbates side reactions, increases impedance, and significantly reduces cycle life.

[0087] In Examples 29-32, the loading ε of the active material layer was increased from 80 to 260 g / m³. 2 ρ is 1.5 g / cm³ 3 As ε×ρ increases from 120 to 390, DCIR continues to increase (from 0.39 to 0.66 mΩ), the high-temperature cycle retention rate continues to decrease, and the energy density continues to increase. Because the lower the loading, the thinner the active layer, the shorter the lithium-ion diffusion distance and the smaller the polarization, resulting in the lowest impedance and the best cycle stability, but less active material per unit area and a lower energy density. As the loading continues to increase, the active layer thickness increases, the longitudinal resistance of ions increases sharply, the internal resistance increases, the electrolyte consumption rate inside the thick layer is inconsistent at high temperatures, the interfacial side reactions are intensified and the cycle life decays rapidly. Higher loading can accommodate more negative electrode active materials, and the overall energy density of the battery continues to increase. In Examples 31 and 32, ε×ρ exceeds the upper limit range of this application, and the cycle performance decay is significantly increased.

[0088] In Examples 33-35, the electrode bulk density ρ gradually increased, ε×ρ increased simultaneously, DCIR continued to increase, high-temperature cycling retention gradually decreased, and energy density increased. This is because the increase in bulk density represents a higher degree of electrode compaction, an increase in the content of negative electrode active material per unit volume, and an increase in energy density. However, excessive compaction will compress the internal pores of the electrode, reduce the electrolyte storage space, narrow the ion transport channels, and increase polarization and internal resistance. Insufficient pores will prevent the electrolyte from being replenished in time after consumption during high-temperature cycling, leading to a continuous deterioration of interfacial side reactions and a decrease in cycle stability.

[0089] Comparative Examples 1-2 and Comparative Example 5: d×S1 / S2×A sv ×ω2 / ω3 are 3, 4, and 3 respectively, all lower than the lower limit value specified in this application. First, the amount of conductive agent added ω2 is too low and the amount of binder ω3 is too small, so the conductive network cannot be formed completely. At the same time, the particle size d of the aggregate of the negative electrode active material is too small and the specific surface area S1 of graphite is too low. The particles are fine and there are few overall reaction interfaces, resulting in insufficient lithium-ion conduction channels. This directly causes the battery DCIR to increase to 0.72~0.68mΩ, and the kinetic performance deteriorates significantly. The fine graphite particles also bring additional interfacial side reactions. Combined with the imbalance of conductive and binder components, the high-temperature cycle capacity retention rate is only 67.90%, 63.40%, and 72.50%, and the energy density is also low. In Comparative Example 3, d×S1 / S2×A sv The value of ×ω2 / ω3 is as high as 187, and in Comparative Example 4, d×S1 / S2×A sv The value of ×ω2 / ω3 is as high as 129, far exceeding the upper limit of this application. Among them, the aggregate particle size d of the negative electrode active material in Comparative Example 3 is too large, S1 is too high, there is excessive conductive agent, and too much binder is added. The aggregate particle size of the ultra-large negative electrode active material has a long internal lithium diffusion path, excessive conductive agent increases side reaction sites, and high binder blocks pores. Similarly, in Comparative Example 4, the aggregate particle size of the negative electrode active material is too large, the proportion of conductive agent is too high, and the oil absorption value is too low. Both of them show an increase in electrode internal resistance, and the electrolyte continues to decompose at high temperature, and the particles are pulverized due to stress concentration during charge and discharge. The cycle capacity retention rate is only 61.21% and 63.40%, and the energy density decreases simultaneously. That is, in Comparative Examples 1 to 5, d×S1 / S2×A sv The ×ω2 / ω3 relationship does not fall within the parameter range defined in this application. Either the coefficient is too low, resulting in the absence of conductive network and obstruction of ion transport, or the coefficient is too high, causing a surge in interfacial side reactions and easy destruction of particle structure. Ultimately, all of them have defects such as increased impedance, significant decrease in high-temperature cycling stability, and poor energy density.

[0090] In comparative examples 5 and 6, d×S1 / S2×A sv A ×ω2 / ω3 value below 5 indicates insufficient conductive pathways, high internal resistance, and high-temperature cycle retention rates of only 72.50% and 73.43%, respectively. In Comparative Example 7, d×S1 / S2×A sv The ×ω2 / ω3 value far exceeds the upper limit of 62, exacerbating side reactions and resulting in a cycle retention rate of only 72.35%. In comparative examples 8-10, although d×S1 / S2×A sv The ×ω2 / ω3 value is within the range of 5 to 62 as defined in this application, but the volume density of the negative electrode active material layer in Comparative Example 8 reaches 2 g / cm³. 3Excessive compaction can clog pores, hindering electrolyte wetting and ion transport, and increasing internal resistance. Comparative Example 9: Conductive agent with a specific surface area of ​​260 m² 2 / g exceeds 50~250m 2 / g upper limit, the amount of binder added is 5%, which is higher than the limit of 4.0%. A large amount of high specific surface area conductive agent induces high temperature side reaction, and excessive binder increases impedance. Comparative Example 10: Active substance loading 270 g / m³ 2 Exceeding 80~250g / m 2 Within the specified range, ε×ρ exceeds the upper limit, resulting in an excessively thick electrode coating, a longer lithium-ion diffusion distance, concentrated charging and discharging stress, increased DC impedance, and a significantly lower high-temperature cycle capacity retention rate compared to the embodiments of this application. Comparing the test results of the above embodiments and comparative examples, it can be seen that the negative electrode provided by this invention, through the synergistic effect of the above multi-components, satisfies 5≤d×S1 / S2×A. sv Based on ×ω2 / ω3≤62, the transport dynamics of ions and electrons can be further optimized, thereby achieving a better balance between battery cycle performance and dynamic performance under high-temperature conditions.

[0091] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A negative electrode sheet, characterized in that, It includes a negative electrode current collector and a negative electrode active material layer, wherein the negative electrode active material layer includes a negative electrode active material, a binder, and a conductive agent; The negative electrode sheet meets the following conditions: 5≤d×S1 / S2×A sv ×ω2 / ω3≤62; Wherein, d is the aggregate particle size of the negative electrode active material, in μm; S1 is the specific surface area of ​​the negative electrode active material, in m². 2 / g; S2 is the specific surface area of ​​the conductive agent, in m². 2 / g; A sv The oil absorption value of the conductive agent is expressed in mL / 100g. ω2 represents the mass percentage of the conductive agent, expressed as % . ω3 represents the mass percentage of the adhesive, in percentages (%).

2. The negative electrode sheet according to claim 1, characterized in that, The negative electrode sheet meets the following conditions: 6≤d×S1 / S2×A sv ×ω2 / ω3≤50。 3. The negative electrode sheet according to claim 1, characterized in that, Based on the total mass of the negative electrode active material layer, the mass percentage ω2 of the conductive agent is 0.5%~2.5%; and / or, The mass percentage ω3 of the adhesive is 1.5%~4.0%.

4. The negative electrode sheet according to claim 1, characterized in that, The specific surface area S1 of the negative electrode active material is 1.0~1.7 m². 2 / g; and / or, The specific surface area S2 of the conductive agent is 50~250 m². 2 / g.

5. The negative electrode sheet according to claim 1, characterized in that, The oil absorption value A of the conductive agent sv It is 160~280 mL / 100g.

6. The negative electrode sheet according to claim 1, characterized in that, The aggregate particle size d of the negative electrode active material is 6.0~12.0μm.

7. The negative electrode sheet according to claim 6, characterized in that, The negative electrode active material includes one or more of single particles and secondary particles.

8. The negative electrode sheet according to claim 7, characterized in that, In the negative electrode active material, the mass ratio of single particles to secondary particles is (100:0) to (40:60).

9. The negative electrode sheet according to claim 7, characterized in that, The particle size of the negative electrode active material satisfies the following condition: 7≤d×(D 90 -D 10 ) / D 50 ≤16; Among them, D 10 This refers to the particle size value corresponding to a particle volume percentage of 10% in the negative electrode active material, in μm. D 90 This refers to the particle size value corresponding to a particle volume percentage of 90% in the negative electrode active material, in μm. D 50 This refers to the particle size value corresponding to a particle volume percentage of 50% in the negative electrode active material, in μm.

10. The negative electrode sheet according to claim 9, characterized in that, In the negative electrode active material, D 10 Its thickness is 4~7.5μm; D 50 The thickness is 8~14μm; D 90 It is 15~25μm.

11. The negative electrode sheet according to claim 1, characterized in that, The negative electrode active material includes graphite, with a graphitization degree G of 92%~95.5%; The limiting compaction density σ of the negative electrode active material is 1.6~1.8 g / cm³. 3 .

12. The negative electrode sheet according to claim 1, characterized in that, Based on the total mass of the negative electrode active material layer, the mass percentage ω1 of the negative electrode active material is 93.5%~98%.

13. The negative electrode sheet according to claim 1, characterized in that, In the negative electrode sheet, the loading ε of the negative electrode active material layer on either side of the negative electrode current collector is 80~250 g / m. 2 ; and / or, The bulk density ρ of the negative electrode active material layer on either side of the negative electrode current collector is 1.4~1.65 g / cm³. 3 .

14. The negative electrode sheet according to claim 13, characterized in that, The negative electrode sheet meets the following conditions: 135≤ε×ρ≤325.

15. The negative electrode sheet according to claim 1, characterized in that, The peel strength F between the negative electrode current collector and the negative electrode active material layer is 6~100 N / m.

16. The negative electrode sheet according to claim 1, characterized in that, The longitudinal resistivity R of the negative electrode is 0.01~0.2Ω•cm.

17. A battery, characterized in that, Includes the negative electrode sheet as described in any one of claims 1 to 16.