Negative electrode sheet, method for manufacturing the same, and lithium battery cell
By synergistically designing a gradient porous self-supporting carbon current collector, a lithiophilic modified layer, and an artificial SEI layer at the interface, the problems of lithium dendrite growth and volume expansion were solved, improving the cycle stability and safety of lithium batteries while reducing production costs.
Patent Information
- Application Number
- CN202611319991.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2026-06-16
- Filing Date
- 2026-08-28
- Publication Date
- 2026-11-24
AI Technical Summary
Traditional lithium metal batteries use copper foil as the current collector, which has problems such as lithium dendrite growth, short cycle life, poor safety and high resource dependence. In addition, the high density of copper foil reduces the energy density of the battery.
By employing a gradient porous self-supporting carbon current collector, combined with a lithiophilic modified layer, an artificial SEI layer at the interface, and a carbon framework confinement design, a multi-structure, multi-component, and multi-interface synergistic mechanism is formed to optimize the overall performance of lithium metal batteries.
It effectively inhibits lithium dendrite growth, alleviates volume expansion, reduces interface impedance, improves the cycle stability and safety of lithium battery cells, reduces production costs, and increases energy density.
Smart Images

Figure CN123162138A_ABST
Abstract
Description
Technical Field
[0001] This application belongs to the field of lithium battery technology, specifically relating to a negative electrode sheet and its preparation method, and a lithium battery cell.
[0002] Cross-references to related applications This application claims priority to Chinese patent application 202610873226.5, filed on June 16, 2026, entitled “Negative electrode sheet and preparation method thereof, lithium battery cell”, the entire contents of which are incorporated herein by reference. Background Technology
[0003] Lithium metal batteries have become a core development direction in fields such as electric vehicles, portable electronic devices, and energy storage power stations due to the high theoretical specific capacity and low redox potential of lithium metal.
[0004] However, traditional lithium metal batteries typically use copper foil as the current collector, which presents a significant technical bottleneck. Copper foil has a dense planar structure with a low specific surface area, making it prone to forming needle-like dendrites during lithium metal deposition. This can lead to internal short circuits, shortened cycle life, and severely restrict safety.
[0005] Furthermore, global copper reserves are limited and highly dependent on imports, making its cost significantly susceptible to fluctuations in the international market. Additionally, the high density of copper foil reduces battery energy density. The lithium metal-electrolyte interface reacts violently, and the naturally formed SEI layer, composed of components such as Li₂CO₃ and LiOH, suffers from high impedance, poor stability, and susceptibility to cracking, exacerbating lithium dendrite growth and volume expansion. The lack of effective physical constraints during lithium metal deposition leads to increased volume change rates, causing electrode structure collapse and active material shedding, further deteriorating battery cycle stability. Summary of the Invention
[0006] To address the aforementioned issues, this application provides a negative electrode sheet, its preparation method, and a lithium battery cell. The negative electrode sheet of this application employs a four-pronged synergistic design—gradient porous self-supporting carbon current collector replacing copper foil, lithiophilic modification, artificial SEI at the interface, and carbon framework confinement—to suppress lithium dendrite formation, alleviate lithium volume expansion during cycling, reduce interfacial impedance, and thereby improve the cycle stability and safety of the lithium battery cell.
[0007] In a first aspect, a negative electrode sheet includes: a porous self-supporting carbon current collector comprising carbon nanotubes, graphene, and a binder, wherein the porosity of the porous self-supporting carbon current collector near the tab is 50%–65%, and the porosity of the porous self-supporting current collector away from the tab is 70%–85%. A lithiophilic modification layer, at least partially located on the outer surface of the porous self-supporting carbon current collector and / or on the surface of the pore inner wall of the porous self-supporting carbon current collector, the lithiophilic modification layer comprising one or more of nitrogen-doped carbon materials, phosphorus-doped carbon materials, silver nanoparticles, and zinc nanoparticles, wherein the mass ratio of the lithiophilic modification layer to the porous self-supporting carbon current collector is 0.05:1 to 0.15:1. An interfacial artificial SEI layer, at least partially located on the surface of the lithiophilic modification layer, the interfacial artificial SEI layer comprising lithium nitride, lithium fluoride, and lithium phosphate. Lithium metal, at least partially located on the surface of the artificial SEI layer at the interface and / or in the pores of the porous self-supporting current collector, is packaged in the negative electrode with a lithium metal encapsulation amount of 10 mAh / cm². 2 ~150 mAh / cm 2 .
[0008] According to the embodiments of this application, the negative electrode sheet of this application relies on the synergistic effect of multiple structures, multiple components, and multiple interfaces to comprehensively optimize the overall performance of lithium metal batteries. The porous self-supporting carbon current collector itself has the advantage of being lightweight, which can effectively optimize the overall energy density of the battery. Its unique three-dimensional interconnected porous structure and gradient pore design form a structural synergistic effect, which can not only ensure the efficient and rapid conduction of electrons, but also provide sufficient lithium storage space for the lithium deposition process, effectively mitigating the volume expansion problem generated during battery charge and discharge cycles, and consolidating the foundation for battery structural stability.
[0009] Furthermore, when the mass ratio of the lithiophilic modified layer to the porous self-supporting carbon current collector is 0.05:1 to 0.15:1, the lithiophilic active component and the excellent lithiophilic interface properties form a functional synergy. The lithiophilic active component can effectively reduce the lithium-ion nucleation barrier, guide lithium metal to be uniformly deposited in the pores of the carbon framework, and inhibit the initiation and growth of lithium dendrites from the root. At the same time, the excellent lithiophilic interface can significantly enhance the interfacial bonding strength between lithium metal and the porous self-supporting carbon current collector, improve the compatibility and stability of the two-phase interface, and avoid performance degradation caused by interfacial desorption.
[0010] Furthermore, the artificial SEI modification layer and the carbon skeleton form an interface protection and transport synergy. The interface artificial SEI layer of this application has low impedance characteristics. Combined with the refined grain structure and high-density grain boundary system, it can construct an efficient lithium-ion transport pathway, significantly improving ion conduction efficiency. At the same time, this SEI layer has excellent mechanical strength and chemical stability. It can act as a protective barrier to isolate the electrolyte from direct contact with lithium metal, suppress side reactions, reduce the formation of by-products, optimize the internal reaction environment of the battery, and work synergistically with the substrate structure to ensure the efficient and stable operation of the battery.
[0011] Furthermore, the spatial confinement effect of the carbon skeleton and the interfacial composite properties create a synergistic effect of structural stability. The three-dimensional carbon skeleton of the porous self-supporting carbon current collector can construct a stable physical constraint system, effectively limiting the disordered growth of lithium metal and improving the volume deformation problem during battery charging and discharging. At the same time, the carbon skeleton and lithium metal can achieve close bonding and composite, reducing the problem of active material shedding. The synergistic effect of multiple structures significantly improves the structural integrity and operational stability of the battery during long-term cycling.
[0012] In some optional embodiments, the porous self-supporting carbon current collector satisfies at least one of the following: (1) the thickness of the porous self-supporting carbon current collector is 10 μm to 50 μm. (2) the porosity of the porous self-supporting carbon current collector is gradient-distributed along the thickness direction. (3) the areal density of the porous self-supporting carbon current collector is 1 mg / cm³. 2 ~3 mg / cm 2 (4) The conductivity of the porous self-supporting carbon current collector is ≥1000 S / m. (5) The diameter of the carbon nanotube is 10 nm~20 nm, and the aspect ratio is 50~100. (6) The number of graphene layers is 3~5. (7) The softening point of the binder is 80℃~100℃. (8) The mass ratio of carbon nanotubes, graphene and binder is (2.4~3.6):(1.6~2.4):(4~6), which can be selected as 3:2:5. (9) The binder includes one or more of phenolic resin, epoxy resin, polyimide resin, furan resin and urea-formaldehyde resin; or the polymer binder includes one or more of polyvinylidene fluoride, polytetrafluoroethylene, styrene-butadiene rubber, carboxymethyl cellulose, polyacrylic acid, sodium alginate and polyethylene oxide.
[0013] In some alternative embodiments, the lithiophilic modified layer satisfies at least one of the following: (1) the lithiophilic contact angle of the lithiophilic modified layer is ≤30°. (2) the particle size of the silver nanoparticles is 5 nm to 10 nm. (3) the particle size of the zinc nanoparticles is 5 nm to 10 nm. (4) based on the total atomic weight of the nitrogen-doped carbon material, the atomic percentage of nitrogen is 5 at.% to 10 at.%. (5) based on the total atomic weight of the phosphorus-doped nitrogen material, the atomic percentage of phosphorus is 3 at.% to 8 at.%.
[0014] In some alternative embodiments, the negative electrode sheet satisfies at least one of the following: (1) the thickness of the interfacial artificial SEI layer is 10 nm to 50 nm. (2) the impedance of the interfacial artificial SEI layer is 30 Ω to 80 Ω. (3) the grain size of the interfacial artificial SEI layer is 10 nm to 18 nm. (4) the ionic conductivity of the interfacial artificial SEI layer is ≥1×10⁻⁶. -4S / cm; (5) The fracture strength of the artificial SEI layer at the interface is ≥20 MPa. (6) The metallic lithium and the porous self-supporting carbon current collector form a composite structure. (7) The purity of metallic lithium is ≥99.9%. (8) The volume change rate of the porous self-supporting carbon current collector after encapsulation of lithium is ≤50%.
[0015] Secondly, embodiments of this application provide a method for preparing a negative electrode sheet, comprising: Carbon nanotubes, graphene, and binder are mixed in a first predetermined mass ratio to obtain a composite material. A pore-forming agent accounting for 30% to 60% of the total mass of the composite material is added. The mixture is ball-milled using a first solvent as the dispersion medium and ultrasonically dispersed to obtain a uniform slurry. The uniform slurry is then coated into a film, dried, and calcined under a protective atmosphere to remove the pore-forming agent, resulting in a porous self-supporting carbon current collector.
[0016] The porous self-supporting current collector can be modified by nitrogen doping or phosphorus doping using vapor deposition, or by depositing silver nanoparticles or zinc nanoparticles using chemical plating to obtain a porous self-supporting carbon current collector with a lithium-affinity modified layer.
[0017] A diluent containing lithium nitrate, ammonium fluoride, and phosphoric acid was prepared and coated onto the surface of a porous self-supporting carbon current collector with a lithiophilic modified layer under a protective atmosphere. After the solvent evaporated at room temperature, the current collector was allowed to stand under a protective atmosphere to form a porous self-supporting carbon current collector with an artificial SEI layer and a lithiophilic modified layer.
[0018] Using a porous self-supporting carbon current collector with an artificial SEI layer and a lithiophilic modification layer as the cathode and a lithium metal plate as the sacrificial anode, lithium metal is deposited onto the porous self-supporting carbon current collector with the artificial SEI layer and lithiophilic modification layer using an electrodeposition process until the lithium metal encapsulation amount reaches 10 mAh / cm³. 2 ~150 mAh / cm 2 Thus, the negative electrode sheet of the first aspect is obtained.
[0019] According to the embodiments of this application, the preparation process of the negative electrode sheet provided in this application is compatible with the existing mature battery production system. It can achieve continuous and large-scale mass production by relying on roll-to-roll electrodeposition technology, which can effectively reduce production costs compared with traditional copper foil current collectors. At the same time, carbon-based raw materials are widely available and have a stable supply, without dependence on imported resources. With multiple synergistic advantages in performance, process and cost, it has outstanding industrial application value and promotion prospects.
[0020] In some optional embodiments, carbon nanotubes, graphene, and a binder are mixed in a first predetermined mass ratio to obtain a composite material. A pore-forming agent accounting for 30% to 60% of the total mass of the composite material is added. The mixture is ball-milled using a first solvent as a dispersion medium, and then ultrasonically dispersed to obtain a uniform slurry. The uniform slurry is then coated into a film, dried, and calcined under a protective atmosphere to remove the pore-forming agent, resulting in a porous self-supporting carbon current collector. A composite material is obtained by mixing carbon nanotubes, graphene, and phenolic resin in a predetermined mass ratio. Polymethyl methacrylate (PMMA) microspheres, accounting for 30%–60% of the total mass of the composite material, are added. Using ethanol as the dispersion medium, the mixture is ball-milled at 300–500 r / min for 2–4 h, followed by ultrasonic dispersion for 30 min to obtain a uniform slurry. The uniform slurry is then coated onto a film and dried at 120℃ for 2 h, followed by calcination at 800℃–1200℃ for 3 h under an argon atmosphere. The PMMA microspheres are then removed to obtain a porous, self-supporting carbon current collector. Optionally, the particle size of the PMMA microspheres is gradient-distributed along the tab extension direction, with the particle size of PMMA microspheres near the tab side being 3 μm–5 μm and the particle size of PMMA microspheres away from the tab side being 1 μm–3 μm. μm; the heating rate of calcination is 5℃ / min, and optionally, the mass ratio of carbon nanotubes, graphene and phenolic resin is 3:(1.6~2.4):(4~6), or optionally 3:2:5.
[0021] In some optional embodiments, the porous self-supporting current collector is modified by nitrogen doping or phosphorus doping using a vapor deposition method, or by depositing silver nanoparticles or zinc nanoparticles on the porous self-supporting current collector using a chemical plating method to obtain a porous self-supporting carbon current collector with a lithiophilic modified layer, including the following steps: The porous self-supporting current collector is modified by nitrogen doping or phosphorus doping using vapor deposition at 500℃~700℃ for 2h~4h, or by chemical plating at 50℃~80℃ for 30min~120min to form silver nanoparticles or zinc nanoparticles, thus obtaining a porous self-supporting carbon current collector with a lithiophilic modified layer. Optionally, the nitrogen-containing gas used in the vapor deposition method is a mixture of ammonia and nitrogen, and the phosphorus source gas is trimethylphosphine; the concentration of silver ions in the plating solution used in the chemical plating method is 0.05mol / L~0.2mol / L, and the concentration of zinc ions is 0.1mol / L~0.3mol / L. Further optionally, the nitrogen-containing gas used in the vapor deposition method is a mixture of ammonia and nitrogen with a volume ratio of 1:1~1:4, and can be selected as a mixture of ammonia and nitrogen with a volume ratio of 1:4.
[0022] In some optional embodiments, the steps of preparing a diluent containing lithium nitrate, ammonium fluoride, and phosphoric acid, coating it onto the surface of a porous self-supporting carbon current collector with a lithiophilic modified layer under a protective atmosphere, evaporating the solvent at room temperature, and then allowing it to stand under a protective atmosphere to form a porous self-supporting carbon current collector with an artificial SEI layer and a lithiophilic modified layer include: A modification solution containing lithium nitrate, ammonium fluoride, and phosphoric acid with a concentration of 0.1 mol / L to 0.5 mol / L was prepared using ethanol as the solvent. The solution was prepared under argon protection using a nozzle pressure of 0.3 MPa to 0.5 MPa and a flow rate of 0.5 mL / cm². 2 ~2 mL / cm 2 The coating is applied to the surface of a porous self-supporting carbon current collector with a lithiophilic modified layer. After the solvent evaporates at room temperature, the mixture is left to stand at 100℃~150℃ in a nitrogen atmosphere for 2h~4h to form a porous self-supporting carbon current collector with an artificial SEI layer and a lithiophilic modified layer. Optionally, the molar ratio of lithium nitrate, ammonium fluoride and phosphate in the modification solution is (1.5~2.5):(0.75~1.25):(0.75~1.25), and more preferably 2:1:1.
[0023] In some optional embodiments, a porous self-supporting carbon current collector with an artificial SEI layer and a lithiophilic modification layer is used as the cathode, and a lithium metal plate is used as the sacrificial anode. Lithium metal is deposited onto the porous self-supporting carbon current collector with the artificial SEI layer and lithiophilic modification layer using an electrodeposition process until the lithium metal encapsulation amount reaches 10 mAh / cm³. 2 ~150 mAh / cm 2 The steps to obtain the negative electrode sheet include: Using a porous, self-supporting carbon current collector with an artificial SEI layer and a lithiophilic modified layer as the cathode and a lithium metal plate as the sacrificial anode, a roll-to-roll electrodeposition process was employed in an EC / DMC electrolyte containing 5% fluoroethylene carbonate and 1 mol / L LiPF6, with the electrodeposition current controlled at 0.05 mA / cm². 2 ~4 mA / cm 2 Winding speed 0.08 m 2 / min~5 m 2 The deposition rate was 1 h / min, and the deposition time was 1 h to 12 h until the lithium metal encapsulation amount reached 10 mAh / cm³. 2 ~150 mAh / cm 2 This yields the negative electrode sheet.
[0024] Thirdly, embodiments of this application provide a lithium battery cell, including a negative electrode sheet of the first aspect and / or a negative electrode sheet prepared by the preparation method of the second aspect. Optionally, the lithium battery cell is a solid-state battery cell, and the solid-state battery cell has a capacity retention rate of ≥82% and a coulombic efficiency of ≥98.8% after 300 cycles at a rate of 0.3 C. Attached Figure Description
[0025] The accompanying drawings, which form part of this application, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an undue limitation of the invention. In the drawings: Figure 1 This is a schematic diagram of the negative electrode structure provided in an embodiment of the present invention.
[0026] Figure 2 This is a charge-discharge curve of the all-solid-state battery assembled with the negative electrode in Example 1 and Comparative Example 1 of the present invention, under the conditions of Experiment 1, on the 10th cycle.
[0027] Figure 3 The graph shows the cycle performance of the all-solid-state battery assembled with the negative electrode in Example 1 and Comparative Example 1 of this invention under the conditions of Experiment Example 1.
[0028] The above figures include the following reference numerals: 1. Porous self-supporting carbon current collector. 2. Lithophilic modified layer. 3. Artificial SEI layer at the interface. 4. Metallic lithium encapsulated within the pores of the carbon framework. Detailed Implementation
[0029] To make the purpose, technical solution, and beneficial technical effects of this application clearer, the following detailed description is provided in conjunction with embodiments. It should be understood that the embodiments described in this specification are merely for explaining this application and are not intended to limit it.
[0030] For simplicity, this application only explicitly discloses some numerical ranges. However, any lower limit can be combined with any upper limit to form a range not explicitly stated; and any lower limit can be combined with other lower limits to form a range not explicitly stated, just as any upper limit can be combined with any other upper limit to form a range not explicitly stated. Furthermore, although not explicitly stated, every point or individual value between the endpoints of the range is included within that range. Therefore, each point or individual value can be used as its own lower or upper limit and combined with any other point or individual value or with other lower or upper limits to form a range not explicitly stated.
[0031] In the description of this application, it should be noted that, unless otherwise stated, "above" and "below" include the stated number, and "multiple" in "one or more" means two or more.
[0032] The foregoing description of this application is not intended to describe every disclosed implementation or method. Instead, the following description provides more specific examples of exemplary embodiments. Throughout the application, guidance is provided through a series of embodiments that can be used in various combinations. The examples listed are representative only and should not be construed as exhaustive.
[0033] Lithium metal batteries, due to the ultra-high theoretical specific capacity of lithium metal (3860 mAh / g) and low redox potential of -3.04 V (vs. standard hydrogen electrode), have become a core development direction in fields such as electric vehicles, portable electronic devices, and energy storage power stations. However, traditional lithium metal batteries use copper foil as the current collector, which presents a significant technical bottleneck. Copper foil has a dense planar structure with a specific surface area of only 0.1~0.5 m². 2 Lithium metal deposition easily forms needle-like dendrites, leading to internal short circuits and shortened cycle life, severely restricting battery safety. Global copper resources are limited and highly dependent on imports, with costs significantly affected by international market fluctuations. Furthermore, copper foil has a high density of 8.96 g / cm³. 3 This significantly reduces battery energy density. The reaction between lithium metal and electrolyte is intense, and the naturally formed SEI layer, composed of components such as Li2CO3 and LiOH, suffers from high impedance, poor stability, and susceptibility to cracking, exacerbating lithium dendrite growth and volume expansion. The lack of effective physical constraints during lithium metal deposition leads to volume changes exceeding 300%, causing electrode structure collapse and active material shedding, further deteriorating battery cycle stability.
[0034] In existing technologies, although some studies have attempted to replace copper foil with porous carbon materials or titanium foil, there are significant drawbacks: porous carbon materials have an inert surface, a lithium-affinity contact angle ≥90°, and uneven lithium-ion deposition; titanium foil has a conductivity only 30% that of copper (approximately 3.5 × 10⁻⁶). 4 Furthermore, the welding process is complex and costly, and single interface modification or physical confinement strategies cannot simultaneously solve the three core problems of dendrite growth, volume expansion, and interface stability. In addition, some technologies employ a "lithium-first composite followed by molding" process, which suffers from poor wettability between lithium and the carbon framework and uneven composite formation. Therefore, developing a novel current collector with high conductivity, excellent lithium affinity, and strong structural stability, along with a "multi-dimensional" synergistic stabilization mechanism, is crucial for the industrialization of lithium metal batteries.
[0035] To address the aforementioned issues, this application provides a negative electrode sheet, its preparation method, and a lithium battery cell. The negative electrode sheet of this application employs a four-pronged synergistic design—gradient porous self-supporting carbon current collector replacing copper foil, lithiophilic modification, artificial SEI at the interface, and carbon framework confinement—to suppress lithium dendrite formation, alleviate lithium volume expansion during cycling, reduce interfacial impedance, and thereby improve the cycle stability and safety of the lithium battery cell.
[0036] Negative electrode sheet This application provides a negative electrode sheet; please refer to [link / reference]. Figure 1 ,include: Porous self-supporting carbon current collectors include carbon nanotubes, graphene, and binders. The porosity of the porous self-supporting carbon current collectors near the tab is 50% to 65%, and the porosity of the porous self-supporting current collectors away from the tab is 70% to 85%.
[0037] The lithiophilic modified layer is located at least partially on the outer surface of the porous self-supporting carbon current collector and / or on the surface of the pore inner wall of the porous self-supporting carbon current collector. The lithiophilic modified layer includes one or more of nitrogen-doped carbon materials, phosphorus-doped carbon materials, silver nanoparticles and zinc nanoparticles. The mass ratio of the lithiophilic modified layer to the porous self-supporting carbon current collector is 0.05:1 to 0.15:1.
[0038] An artificial SEI layer is located at least partially on the surface of a lithiophilic modified layer. The artificial SEI layer includes lithium nitride, lithium fluoride, and lithium phosphate.
[0039] Lithium metal, at least partially located on the surface of the artificial SEI layer at the interface and / or in the pores of the porous self-supporting current collector, is packaged in the negative electrode with a lithium metal encapsulation amount of 10 mAh / cm². 2 ~150 mAh / cm 2 .
[0040] As an example, the porosity of the porous self-supporting carbon current collector near the tab can be 50%, 52%, 55%, 58%, 60%, 62%, 65%, or any combination of the above values. The porosity of the porous self-supporting current collector away from the tab can be 70%, 72%, 75%, 78%, 80%, 82%, 85%, or any combination of the above values.
[0041] As an example, the mass ratio of the lithiophilic modified layer to the porous self-supporting carbon current collector can be 0.05:1, 0.06:1, 0.07:1, 0.08:1, 0.09:1, 0.1:1, 0.11:1, 0.12:1, 0.13:1, 0.14:1, 0.15:1, or any range of the above values.
[0042] As an example, the package size of lithium metal can be 10 mAh / cm³.2 20 mAh / cm 2 50 mAh / cm 2 80 mAh / cm 2 100 mAh / cm 2 120 mAh / cm 2 150 mAh / cm 2 or a range consisting of any of the above values.
[0043] According to embodiments of this application, the negative electrode sheet utilizes a multi-structure, multi-component, and multi-interface mechanism to comprehensively optimize the overall performance of lithium metal batteries. The porous self-supporting carbon current collector possesses excellent lightweight and low-density characteristics, with a density of 1.5~2.0 g / cm³. 3 Compared to traditional copper foil, its density is significantly reduced, by more than 78%, which can significantly improve the overall energy density of the battery from the carrier level. Its three-dimensional interconnected porous structure and gradient pore design form a highly efficient structural synergy effect. On the one hand, it can ensure the rapid and smooth conduction of electrons, consolidating the foundation of the battery's conductivity; on the other hand, it can provide sufficient lithium storage space for the lithium metal deposition process, effectively buffering and mitigating the volume expansion problem that occurs during battery charging and discharging, and stabilizing the overall structural stability of the battery.
[0044] Furthermore, when the mass ratio of the lithiophilic modified layer to the porous self-supporting carbon current collector is 0.05:1 to 0.15:1, the lithiophilic active component and the excellent lithiophilic interface properties form a functional synergy, fundamentally solving core problems such as lithium dendrite growth and weak interfacial bonding. The lithiophilic active component built into the material can effectively reduce the lithium-ion nucleation barrier, precisely induce the uniform deposition of lithium metal inside the carbon framework pores, and completely eliminate the initial inducing factors for lithium dendrite initiation and growth. At the same time, the material has excellent lithiophilic wetting properties, with a lithiophilic contact angle as low as 30° and below, which can significantly enhance the interfacial bonding force between lithium metal and the porous self-supporting carbon current collector, improve the adhesion, compatibility and structural stability of the two-phase interface, and effectively avoid battery performance degradation caused by interface desorption and peeling.
[0045] Furthermore, the artificial SEI modification layer and the carbon skeleton form a dual synergy of interface protection and ion transport, significantly optimizing the internal reaction and conduction system of the battery. The interface artificial SEI layer of this application possesses ultra-low impedance characteristics, with an impedance as low as 30~80Ω, while the grain size is precisely controlled within 10~18 nm. Its unique high-density grain boundary structure can construct high-speed transport channels for lithium ions, increasing ion conductivity by more than 50% and effectively improving the overall lithium-ion transport efficiency. Simultaneously, this SEI layer exhibits outstanding mechanical strength and excellent chemical stability, serving as a dense protective barrier to effectively prevent direct contact and reaction between the electrolyte and lithium metal, suppressing internal side reactions, reducing by-product accumulation, purifying the internal reaction environment of the battery, and synergistically ensuring the long-term efficient and stable operation of the battery with the carbon substrate structure.
[0046] Furthermore, the spatial confinement effect of the carbon skeleton and the interfacial composite properties create a synergistic effect of structural stability. The three-dimensional carbon skeleton of the porous self-supporting carbon current collector can construct a stable physical constraint system, effectively limiting the disordered growth of lithium metal and improving the volume deformation problem during battery charging and discharging. At the same time, the carbon skeleton and lithium metal can achieve close bonding and composite, reducing the problem of active material shedding. The synergistic effect of multiple structures significantly improves the structural integrity and operational stability of the battery during long-term cycling.
[0047] In some embodiments, the thickness of the porous self-supporting carbon current collector is 10 μm to 50 μm. For example, it can be 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, or any combination of the above values. This can match the lithium deposition capacity, reduce the problems of longer conductive paths, increased internal resistance, and material redundancy caused by excessive thickness, and at the same time reduce the defects such as insufficient structural strength and weakened confinement ability caused by insufficient thickness, thus achieving the optimal match between structural stability and electrochemical performance.
[0048] In some embodiments, the porosity of the porous self-supporting carbon current collector exhibits a gradient distribution along the thickness direction. Utilizing the differentiated characteristics of the gradient pore structure, functional zones can be formed in different thickness regions of the current collector: areas with fewer pores effectively enhance the overall mechanical strength and structural stability of the framework, suppressing structural collapse under long-term cycling; areas with more pores provide ample lithium storage space and ion diffusion channels, significantly accelerating lithium-ion transport kinetics and adapting to the demands of large-capacity lithium deposition.
[0049] In some embodiments, the areal density of the porous self-supporting carbon current collector is 1 mg / cm³. 2 ~3 mg / cm 2 For example, it could be 1 mg / cm³. 2 1.5 mg / cm 2 2 mg / cm 2 2.5 mg / cm 2 3 mg / cm2 or a range consisting of any of the above values.
[0050] In some embodiments, the conductivity of the porous self-supporting carbon current collector is ≥1000 S / m. For example, it can be 1000 S / m, 1200 S / m, 1400 S / m, 1600 S / m, 1800 S / m, 2000 S / m, or any range of the above values.
[0051] In some embodiments, the carbon nanotubes have a diameter of 10 nm to 20 nm and an aspect ratio of 50 to 100. For example, the diameter of the carbon nanotubes can be 10 nm, 12 nm, 14 nm, 16 nm, 18 nm, 20 nm, or any combination thereof. The aspect ratio of the carbon nanotubes can be 50, 60, 70, 80, 90, 100, or any combination thereof. When the diameter and aspect ratio of the carbon nanotubes meet the requirements of this application, a multi-scale structural synergistic optimization effect can be achieved. A suitable diameter can regulate the internal pore configuration, reduce the problem of skeletal strength reduction caused by excessively large pores or ion blockage caused by excessively small pores, and improve the connectivity and stability of pore channels; a controllable aspect ratio can build a continuously interwoven conductive network, optimize electron transport paths, and avoid network loosening and breakage or structural stacking densification defects caused by aspect ratio imbalance. Meanwhile, the optimized carbon nanotube microstructure can be further adapted to the thickness gradient pore structure, uniformly construct multi-level mass transfer channels, alleviate stress concentration during lithium deposition, synergistically suppress structural collapse and volume distortion, improve the overall flexibility and load stability of the framework, enhance the bonding and composite effect between lithium metal and carbon framework, and further avoid the problem of active material shedding from the microstructure level.
[0052] In some embodiments, the number of graphene layers is 3 to 5. For example, it can be 3, 4, or 5 layers. When the number of graphene layers is 3 to 5, the graphene sheet structure can uniformly coat the carbon skeleton and carbon nanotube conductive network, further improving the overall conductivity continuity and interface flatness, optimizing the uniform migration path of lithium ions, weakening the phenomenon of local current density concentration, and helping to suppress the heterogeneous nucleation and disordered growth of lithium dendrites at the interface level. At the same time, the regular graphene sheets can enhance the overall toughness and structural deformation resistance of the carbon skeleton, disperse the interface stress during the lithium deposition process, match the structural advantages of gradient porosity, further stabilize the overall electrode structure, effectively alleviate the volume distortion and structural loosening problems during long-term cycling, and significantly improve the electrode structural integrity and cycle durability.
[0053] In some embodiments, the softening point of the binder is 80°C to 100°C. For example, it can be 80°C, 85°C, 90°C, 95°C, 100°C, or any combination of the above values. This allows for the sustainable anchoring of the multi-level structure of graphene, carbon nanotubes, and the carbon framework, maintaining the integrity and overall structure of the electrode, ensuring that the conductive network and mass transfer channels are not damaged during long-term thermal cycling and mechanical deformation, and synergistically improving the cycle stability and operational reliability of the battery.
[0054] In some embodiments, the mass ratio of carbon nanotubes, graphene, and binder is (2.4~3.6):(1.6~2.4):(4~6). For example, it can be 2.4:1.6:4, 2.4:2.4:4, 2.4:1.6:6, 2.4:2.6:6, 3.6:1.6:4, 3.6:2.4:4, 3.6:1.6:6, 3.6:2.6:6, or any range of the above values. Optionally, the mass ratio of carbon nanotubes, graphene, and binder is 3:2:5.
[0055] In some embodiments, the adhesive includes one or more of phenolic resin, epoxy resin, polyimide resin, furan resin, and urea-formaldehyde resin; or the polymer adhesive includes one or more of polyvinylidene fluoride, polytetrafluoroethylene, styrene-butadiene rubber, carboxymethyl cellulose, polyacrylic acid, sodium alginate, and polyethylene oxide.
[0056] In some embodiments, the lithiophilic contact angle of the lithiophilic modified layer is ≤30°.
[0057] In some embodiments, the particle size of the silver nanoparticles is 5 nm to 10 nm. For example, it can be 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, 10 nm, or any combination of the above values.
[0058] In some embodiments, the particle size of the zinc nanoparticles is 5 nm to 10 nm. For example, it can be 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, 10 nm, or any combination of the above values.
[0059] In the above embodiments, when the particle size of silver nanoparticles is 5 nm to 10 nm and / or the particle size of zinc nanoparticles is 5 nm to 10 nm, multi-dimensional synergistic optimization of interfacial conductivity, lithiophilicity, and structural uniformity can be further achieved. Uniformly sized and appropriately sized metal nanoparticles can be uniformly loaded onto the interface of the carbon framework, carbon nanotubes, and graphene composite, effectively filling interfacial defects and conductive gaps in carbon-based materials, constructing continuous and dense highly conductive pathways, significantly reducing interfacial contact resistance, and improving electron transport efficiency and overall electrode conductivity. If the nanoparticle size is too large, particle agglomeration and uneven loading are likely to occur, causing an imbalance in the interfacial current density distribution, inducing local lithium dendrite growth, and simultaneously blocking microscopic pore channels, hindering lithium-ion diffusion. If the particle size is too small, particle migration and detachment are likely to occur, making it difficult to maintain a long-term stable modification effect.
[0060] In some embodiments, the atomic percentage of nitrogen is 5 at.% to 10 at.% based on the total atomic weight of the nitrogen-doped carbon material. For example, it can be 5 at.%, 6 at.%, 7 at.%, 8 at.%, 9 at.%, 10 at.%, or any range of the above values. A suitable nitrogen doping amount can stably construct abundant nitrogen-containing active sites on the carbon framework surface, effectively optimize the electron distribution on the carbon material surface, significantly improve the intrinsic lithiophilicity and surface adsorption capacity of the carbon matrix, homogenize the interfacial lithium-ion flux, and inhibit the heterogeneous growth of lithium dendrites at the chemical interface level. Too low a nitrogen content will result in an insufficient number of active sites, weak lithiophilic modification effect, and inability to effectively improve lithium-ion deposition behavior. Too high a nitrogen content, on the other hand, can easily lead to excessive enrichment of structural defects, causing a decrease in the structural stability of the carbon matrix, a decrease in conductivity, and inducing structural degradation during cycling.
[0061] In some embodiments, the atomic percentage of phosphorus is 3 at.% to 8 at.% based on the total atomic weight of the phosphorus-doped nitrogen material. For example, it can be 3 at.%, 4 at.%, 5 at.%, 6 at.%, 7 at.%, 8 at.%, or any range of the above values. When the atomic percentage of phosphorus is 3 at.% to 8 at.%, the introduction of phosphorus atoms can widen the interlayer spacing, optimize the surface charge distribution, reduce the lithium-ion migration barrier, and accelerate interfacial ion conduction. At the same time, appropriate phosphorus doping can synergistically construct a multi-element active interface with the nitrogen-doped system, further reducing the lithium-ion nucleation barrier. If the phosphorus doping amount is too low, it is difficult to achieve the effects of interface modification and kinetic optimization; excessive phosphorus doping can easily generate dopant agglomeration defects, introduce a large number of inert impurity sites, destroy the integrity of the carbon skeleton, increase interfacial impedance, and thus deteriorate the battery cycle and rate performance.
[0062] In some embodiments, the thickness of the artificial SEI layer at the interface is 10 nm to 50 nm. For example, it can be 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, or any combination of the above values. When the thickness of the artificial SEI layer at the interface is 10 nm to 50 nm, it can effectively isolate the direct contact between the lithium metal anode and the electrolyte, effectively suppress the continuous decomposition of the electrolyte and the generation of by-products, and avoid the problem of anode corrosion failure; it can also ensure the rapid penetration and transport of lithium ions, and avoid the obstruction of ion transport at the interface. If the thickness of the artificial SEI layer at the interface is too thin, the integrity of the film layer is insufficient, and microscopic pores and defects are likely to exist, which cannot form an effective shielding protection. The electrolyte can easily penetrate and erode the anode, and it is difficult to suppress side reactions and dendrite growth. If the thickness is too thick, it will significantly increase the interface impedance, prolong the lithium ion migration path, reduce the ion conduction efficiency, and deteriorate the rate performance and kinetic characteristics of the battery. At the same time, the excessively thick film layer lacks flexibility and cannot adapt to the volume deformation of the lithium deposition process, which can easily cause cracking and peeling, resulting in repeated interface damage and reconstruction, and aggravating the battery capacity decay.
[0063] In some embodiments, the impedance of the artificial SEI layer at the interface is 30 Ω to 80 Ω. For example, it can be 30 Ω, 40 Ω, 50 Ω, 60 Ω, 70 Ω, 80 Ω, or any range of the above values.
[0064] In some embodiments, the grain size of the artificial SEI layer at the interface is 10 nm to 18 nm. For example, it can be 10 nm, 11 nm, 12 nm, 13 nm, 14 nm, 15 nm, 16 nm, 17 nm, 18 nm, or any range of the above values.
[0065] In some embodiments, the ionic conductivity of the artificial SEI layer at the interface is ≥1×10⁻⁶. -4 S / cm. For example, it can be 1×10 -4 S / cm, 1.2×10 -4 S / cm, 1.4×10 -4 S / cm, 1.6×10 -4 S / cm, 1.8×10 -4 S / cm, 1×10 -3 S / cm, or any range of the above values.
[0066] In some embodiments, the fracture strength of the artificial SEI layer at the interface is ≥20 MPa. As an example, it can be 20 MPa, 22 MPa, 24 MPa, 26 MPa, 28 MPa, 30 MPa, or any range of the above values.
[0067] In some embodiments, lithium metal and a porous self-supporting carbon current collector form a composite structure.
[0068] In some embodiments, the purity of lithium metal is ≥99.9%.
[0069] In some embodiments, the volume change rate of the porous self-supporting carbon current collector after lithium encapsulation is ≤50%. For example, it can be 40%, 42%, 44%, 46%, 48%, 50%, or any range of the above values.
[0070] Preparation method of negative electrode sheet This application provides a method for preparing a negative electrode sheet, comprising: In step S100, carbon nanotubes, graphene, and binder are mixed in a first predetermined mass ratio to obtain a composite material. A pore-forming agent accounting for 30% to 60% of the total mass of the composite material is added. The mixture is ball-milled using a first solvent as the dispersion medium and ultrasonically dispersed to obtain a uniform slurry. The uniform slurry is then coated into a film, dried, and calcined under a protective atmosphere to remove the pore-forming agent, thus obtaining a porous self-supporting carbon current collector.
[0071] Step S200: The porous self-supporting current collector is modified by nitrogen doping or phosphorus doping using vapor deposition, or by depositing silver nanoparticles or zinc nanoparticles using chemical plating to obtain a porous self-supporting carbon current collector with a lithiophilic modification layer.
[0072] In step S300, a diluent containing lithium nitrate, ammonium fluoride, and phosphoric acid is prepared and coated onto the surface of a porous self-supporting carbon current collector with a lithiophilic modified layer under a protective atmosphere. After the solvent evaporates at room temperature, the current collector is allowed to stand under a protective atmosphere to form a porous self-supporting carbon current collector with an artificial SEI layer and a lithiophilic modified layer.
[0073] In step S400, using a porous self-supporting carbon current collector with an artificial SEI layer and a lithiophilic modification layer as the cathode and a lithium metal plate as the sacrificial anode, lithium metal is deposited onto the porous self-supporting carbon current collector with the artificial SEI layer and the lithiophilic modification layer using an electrodeposition process until the lithium metal encapsulation amount reaches 10 mAh / cm³. 2 ~150 mAh / cm 2 The aforementioned negative electrode sheet is obtained.
[0074] As an example, the pore-forming agent accounts for 30%, 35%, 40%, 45%, 50%, 55%, 60% of the total mass of the composite material, or any of the above values.
[0075] As an example, the lithium metal encapsulation amount (also known as lithium deposition amount) can be 10 mAh / cm³. 2 20 mAh / cm 2 50mAh / cm 2 80 mAh / cm 2100 mAh / cm 2 120 mAh / cm 2 150 mAh / cm 2 Or a range of any of the above values. Optionally, the lithium metal package weight can be 20 mAh / cm³. 2 ~100 mAh / cm 2 More alternatively, the lithium metal package capacity can be 50 mAh / cm³. 2 ~80 mAh / cm 2 .
[0076] According to the embodiments of this application, the preparation process of the negative electrode sheet provided in this application is compatible with the existing mature battery production system. It can achieve continuous and large-scale mass production by relying on roll-to-roll electrodeposition technology, which can effectively reduce production costs compared with traditional copper foil current collectors. At the same time, carbon-based raw materials are widely available and have a stable supply, without dependence on imported resources. With multiple synergistic advantages in performance, process and cost, it has outstanding industrial application value and promotion prospects.
[0077] In some embodiments, step S100 includes: mixing carbon nanotubes, graphene, and phenolic resin in a predetermined mass ratio to obtain a composite material; adding polymethyl methacrylate microspheres accounting for 30% to 60% of the total mass of the composite material; using ethanol as the dispersion medium; ball milling at a speed of 300 to 500 r / min for 2 to 4 h; ultrasonically dispersing for 30 min to obtain a uniform slurry; coating the uniform slurry into a film; drying at 120°C for 2 h; calcining at 800°C to 1200°C for 3 h under an argon atmosphere; removing the polymethyl methacrylate microspheres; and obtaining a porous self-supporting carbon current collector.
[0078] In some embodiments, the particle size of the polymethyl methacrylate microspheres is gradient-distributed along the tab extension direction, with the particle size of the polymethyl methacrylate microspheres near the tab side being 3 μm to 5 μm and the particle size of the polymethyl methacrylate microspheres away from the tab side being 1 μm to 3 μm; the calcination heating rate is 5 °C / min.
[0079] In some embodiments, the mass ratio of carbon nanotubes, graphene, and phenolic resin is (2.4~3.6):(1.6~2.4):(4~6). For example, it can be 2.4:1.6:4, 2.4:2.4:4, 2.4:1.6:6, 2.4:2.6:6, 3.6:1.6:4, 3.6:2.4:4, 3.6:1.6:6, 3.6:2.6:6, or any range of the above values. Optionally, the mass ratio of carbon nanotubes, graphene, and binder is 3:2:5.
[0080] In some embodiments, step S200 includes: performing nitrogen doping or phosphorus doping modification on the porous self-supporting current collector by vapor deposition at 500°C to 700°C for 2 to 4 hours, or depositing silver nanoparticles or zinc nanoparticles on the porous self-supporting current collector by chemical plating at 50°C to 80°C for 30 to 120 minutes, to obtain a porous self-supporting carbon current collector with a lithiophilic modification layer.
[0081] In some embodiments, the nitrogen-containing gas used in the vapor deposition method is a mixture of ammonia and nitrogen, and the phosphorus source gas is trimethylphosphine.
[0082] In some embodiments, the concentration of silver ions in the plating solution used in the chemical plating method is 0.05 mol / L to 0.2 mol / L, and the concentration of zinc ions is 0.1 mol / L to 0.3 mol / L. For example, it can be 0.1 mol / L, 0.15 mol / L, 0.2 mol / L, 0.25 mol / L, 0.3 mol / L, or any range of the above values.
[0083] In some embodiments, the nitrogen-containing gas used in the vapor deposition method is a mixture of ammonia and nitrogen in a volume ratio of 1:1 to 1:4. As an example, the volume ratio of ammonia to nitrogen can be 1:1, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5, 1:4, or any range of the above values. Optionally, the nitrogen-containing gas used in the vapor deposition method is a mixture of ammonia and nitrogen in a volume ratio of 1:4.
[0084] In some embodiments, step S300 includes: preparing a modification solution containing lithium nitrate, ammonium fluoride, and phosphoric acid at a concentration of 0.1 mol / L to 0.5 mol / L, with ethanol as the solvent, and applying it under argon protection at a nozzle pressure of 0.3 MPa to 0.5 MPa and a flow rate of 0.5 mL / cm². 2 ~2 mL / cm 2 The coating is applied to the surface of a porous self-supporting carbon current collector with a lithiophilic modified layer. After the solvent evaporates at room temperature, the mixture is left to stand for 2 to 4 hours at 100°C to 150°C under a nitrogen atmosphere to form a porous self-supporting carbon current collector with an artificial SEI layer and a lithiophilic modified layer.
[0085] In some embodiments, the molar ratio of lithium nitrate, ammonium fluoride, and phosphate in the modification solution is (1.5~2.5):(0.75~1.25):(0.75~1.25). As an example, it can be 1.5:0.75:0.75, 1.5:1.25:0.75, 1.5:0.75:1.25, 1.5:1.25:1.25, 2.5:0.75:0.75, 2.5:1.25:0.75, 2.5:0.75:1.25, 2.5:1.25:1.25, or any range of the above values. Optionally, the molar ratio of lithium nitrate, ammonium fluoride, and phosphate in the modification solution is 2:1:1.
[0086] In some embodiments, step S400 includes: using a porous self-supporting carbon current collector with an interfacial artificial SEI layer and a lithiophilic modified layer as the cathode and a lithium metal plate as the sacrificial anode, in an EC / DMC electrolyte containing 5% fluoroethylene carbonate and 1 mol / L LiPF6, employing a roll-to-roll electrodeposition process, and controlling the electrodeposition current at 0.05 mA / cm². 2 ~4 mA / cm 2 Winding speed 0.08 m 2 / min~5 m 2 The deposition rate was 1 h / min, and the deposition time was 1 h to 12 h until the lithium metal encapsulation amount reached 10 mAh / cm³. 2 ~150 mAh / cm 2 This yields the negative electrode sheet.
[0087] lithium battery cell This application provides a lithium battery cell, including the negative electrode sheet described above and / or the negative electrode sheet prepared by the above preparation method.
[0088] In some embodiments, the lithium battery cell is a solid-state battery cell, and the solid-state battery cell has a capacity retention of ≥82% and a coulombic efficiency of ≥98.8% after 300 cycles at a 0.3 C rate.
[0089] In some embodiments, a lithium battery cell includes a positive electrode, a negative electrode, and a solid electrolyte layer, wherein the solid electrolyte layer includes a solid electrolyte.
[0090] In some embodiments, the solid electrolyte includes a sulfide solid electrolyte.
[0091] In some embodiments, the sulfide solid electrolyte may include Li 6+m+l P 1-m M m S 5-n+l N n Y 1-l The material, with the molecular formula Li 10±δ Ge1-g G g P 2-q Q q S 12-w W w Materials, Li 4-v Ge 1-v P v One or more of the following materials are included: S4, Li2S-P2S5, Li2S-SiS2, Li2S-GeS2, Li2S-MeS-P2S5, and LiGeGaS, where 0 ≤ m < 1, 0 ≤ n < 1, -1 < l < 1; M includes one or more elements of Ge, Si, Sn, Al, Zr, and Sb; N includes one or more elements of O, Se, and Te; Y includes one or more elements of Cl, Br, and I, where 0 ≤ δ < 1, 0 ≤ g ≤ 1, 0 ≤ q ≤ 2, 0 ≤ w < 1; G includes one or two elements of Si and Sn; Q includes Sb; W includes one or more elements of O, Se, Te, Cl, Br, and I, where 0 < v < 1; and Me includes one or more elements of Si, Ge, Sn, and Al.
[0092] As an example, sulfide solid electrolytes may include, but are not limited to, Li6PS5Cl (LPSCl), Li6PS5Br, Thio-LISICON (Li 3.25 Ge 0.25 P 0.75 S4), Li2S-P2S5-LiCl, Li2S-SiS2, LiI-Li2S-SiS2, LiI-Li2S-P2S5, LiI-Li2S-P2O5, LiI-Li3PO4-P2 S5, Li2S-P2S5, Li3PS4, LiI-Li2S-B2S3, Li3PO4-Li2S-Si2S, Li3PO4-Li2S-SiS2, LiPO4-Li2S-SiS, Li 10 GeP2S 12 Li 9.54 Si 1.74 P 1.44 S 11.7 Cl 0.3 and Li7P3S 11 One or more of them.
[0093] In some embodiments, the solid electrolyte may also include one or more of oxide solid electrolytes, halide solid electrolytes, and organic solid electrolytes.
[0094] In some embodiments, halide solid electrolytes may include those with the molecular formula Li 6-aA a+ X6 is one or more of the following materials, wherein a is the valence of the A ion, a is 3 or 4, A includes one or more of Ga, In, Sc, Y, lanthanides, Sb, Bi, Ti, Zr, and Hf, and X includes one or more of the following halogens.
[0095] As an example, halide solid electrolytes may include, but are not limited to, one or more of Li3YCl6, Li3YBr6, Li3ErCl6, Li3InCl6, and Li3InBr6.
[0096] In some embodiments, the oxide solid electrolyte may include, but is not limited to, one or more of NASICON-type solid electrolyte, LISICON-type solid electrolyte, perovskite-type solid electrolyte, and garnet-type solid electrolyte.
[0097] As an example, oxide solid electrolytes may include, but are not limited to, Li5La3Ti2O 12 Li7La3Zr2O 12 Li4Ti5O 12 Li 14 Zn(GeO4)4, LiTi2(PO4)3, Li 1+x Al x Ti 2-x (PO4)3, Li 1+y Al y Ge 2-y One or more of (PO4)3, 0 < x < 2, 0 < y < 2.
[0098] Oxide-based solid electrolytes exhibit high safety in air and have a 10 -3 S / cm to 10 -4 The lithium-ion conductivity (S / cm) is lower than that of sulfide-based solid electrolytes, but relatively higher. Furthermore, oxide-based solid electrolytes exhibit high electrochemical safety and mechanical strength. However, oxide-based solid electrolytes have high oxidation voltages. Additionally, solid electrolytes have high grain boundary resistance, making it difficult to form a contact interface between the electrode and electrolyte, requiring high-temperature heat treatment processes of 1000 kJ or higher, and are difficult to scale up. In the embodiments of this application, the oxide-based solid electrolyte can be any known oxide material used in the field of lithium batteries. In the embodiments of this application, the oxide-based solid electrolyte includes perovskite solid electrolytes, sodium superionic conductor solid electrolytes (NASICON), lithium superionic conductor solid electrolytes (LISICON), and lithium lanthanum zirconium oxide solid electrolytes (LLZO).
[0099] Organic solid electrolytes (OSEs) are a type of solid electrolyte. OSEs can readily form electrode interfaces and minimize dendrite growth, thus ensuring stable reactions between OSEs and lithium metal. The disadvantages of OSEs are their relatively low lithium-ion conductivity and the fact that they typically require high-temperature operation. In this embodiment, the OSE comprises polyethylene oxide (PEO).
[0100] The thickness of the electrolyte layer can be selected differently depending on the properties of the desired solid-state battery cell. Specifically, in some embodiments, the thickness of the electrolyte layer can be from 0.1 μm to 1000 μm; in other embodiments, the thickness of the electrolyte layer can be from 1 μm to 500 μm; in still other embodiments, the thickness of the electrolyte layer can be from 20 μm to 30 μm; this application does not limit it in this regard.
[0101] In some embodiments, the positive electrode includes a positive current collector and a positive electrode film layer located on at least one side of the positive current collector, the positive electrode film layer including a positive electrode active material.
[0102] As an example, the positive current collector has two surfaces opposite each other in its own thickness direction, and the positive electrode film layer is disposed on either or both of the two opposite surfaces of the positive current collector.
[0103] In some embodiments, the positive electrode active material may include one or more of lithium phosphate and layered lithium transition metal oxides.
[0104] Lithium-containing phosphates may include one or more of lithium iron phosphate, lithium manganese phosphate, lithium manganese iron phosphate, and their respective modified compounds.
[0105] Examples of layered lithium-containing transition metal oxides may include one or more of lithium cobalt oxides, lithium nickel oxides, lithium manganese oxides, lithium nickel cobalt oxides, lithium manganese cobalt oxides, lithium nickel manganese oxides, lithium nickel cobalt manganese oxides, lithium nickel cobalt aluminum oxides, and their respective modified compounds.
[0106] In some embodiments, the layered lithium-containing transition metal oxide may include Ni. The molar amount of Ni may account for more than 70% of the total molar amount of transition metal elements in the layered lithium-containing transition metal oxide; optionally, the molar amount of Ni may account for more than 80% of the total molar amount of transition metal elements in the layered lithium-containing transition metal oxide; more preferably, the molar amount of Ni may account for more than 90% of the total molar amount of transition metal elements in the layered lithium-containing transition metal oxide.
[0107] The higher the Ni content in layered lithium-containing transition metal oxides, the higher the energy density of the battery cell.
[0108] In some embodiments, layered lithium-containing transition metal oxides may include Li a Ni b Co c M d O e A f Wherein, 0 < a ≤ 1.2; 0.8 ≤ b < 1; 0 < c < 1; 0 < d < 1; b + c + d = 1; 1 ≤ e ≤ 2; 0 ≤ f ≤ 1; M includes, but is not limited to, one or more of Mn, Al, Zr, Zn, Cu, Cr, Mg, Fe, V, Ti, and B; A includes, but is not limited to, one or more of N, F, S, and Cl. This can further improve the energy density of individual battery cells.
[0109] In some embodiments, as an example, layered lithium-containing transition metal oxides may include, but are not limited to, LiNi. 0.8 Co 0.1 Mn 0.1 O2, LiNi 0.8 Co 0.15 Al 0.05 O2, LiNi 0.9 Co 0.06 Mn 0.04 O2, LiNi 0.92 Co 0.06 Mn 0.02 O2, LiNi 0.96 Co 0.02 Mn 0.02 O2, LiNi 0.96 Co 0.02 Mn 0.02 O2N 0.02 One or more of them.
[0110] During the charging and discharging process of a battery cell, Li undergoes insertion / extraction and consumption, resulting in varying molar Li content at different discharge states. In the examples of positive electrode active materials in this application, the molar Li content refers to the initial state of the material, i.e., the state before feeding. After charge-discharge cycles, the molar Li content may change when the positive electrode active material is applied to the battery cell.
[0111] In the examples of positive electrode active materials in this application, the molar content of O is only a theoretical value. Oxygen release from the crystal lattice will cause the molar content of O to change, and the actual molar content of O will fluctuate.
[0112] The modified compounds for the above-mentioned positive electrode active materials can be obtained by doping and / or surface coating of the positive electrode active materials.
[0113] In some embodiments, the positive electrode film layer may optionally include a binder. As an example, the binder may include one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), PVDF-tetrafluoroethylene-propylene terpolymer, PVDF-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorinated acrylate resins.
[0114] In some embodiments, the adhesive has a weight percentage of 0.5% or greater in the positive electrode film layer, which is beneficial for obtaining good adhesion performance.
[0115] In some embodiments, the positive electrode film layer further includes a conductive agent. As an example, the conductive agent may include one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0116] In some embodiments, the positive electrode film layer further includes a solid electrolyte.
[0117] Solid electrolytes may include any one or more of the solid electrolytes provided in the embodiments of this application.
[0118] In some embodiments, based on the total mass of the positive electrode film, the mass percentage of solid electrolyte in the positive electrode film can be 5%-35%, for example, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, 33%, 34%, 35%, or any range of the above values, and can be selected as 10%-32%.
[0119] In some embodiments, the current collector serving as the positive electrode may also be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material substrate and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector can be made by forming a metal material, such as aluminum, aluminum alloy, copper, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, on the polymer material substrate. The polymer material substrate may include polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), and other substrates.
[0120] In some embodiments, the thickness of the positive current collector is from 4 μm to 20 μm. It is optionally from 6 μm to 18 μm, and more preferably from 8 μm to 16 μm.
[0121] In some embodiments, the positive electrode may not require an additional positive current collector; for example, the stainless steel sheet of the mold battery can be directly used as the positive current collector.
[0122] The positive electrode can be prepared by either a dry process or a wet process.
[0123] Example The following examples describe the disclosure of this invention in more detail. These examples are merely illustrative, as various modifications and variations will be apparent to those skilled in the art within the scope of this disclosure. Unless otherwise stated, all parts, percentages, and ratios reported in the following examples are based on mass, and all reagents used in the examples are commercially available or synthesized by conventional methods and can be used directly without further processing. The instruments used in the examples are also commercially available.
[0124] Example 1 A negative electrode sheet is prepared by the following method: S100, carbon nanotubes (aspect ratio of 200, tube diameter of 5 to 12 nm), graphene (4 layers), and phenolic resin were weighed in a mass ratio of 3:2:5. Polymethyl methacrylate (PMMA) microspheres, accounting for 40% of the total mass of the composite material, were added. The PMMA microspheres were distributed in a gradient along the tab extension direction, with the microspheres near the tab having a particle size of 3 μm to 5 μm and the microspheres away from the tab having a particle size of 1 μm to 3 μm. The mixture was ultrasonically dispersed for 30 min to obtain a uniform slurry. A coating thickness of 50 μm was applied, dried at 120℃ for 2 h, and calcined at 1000℃ for 3 h under an argon atmosphere to obtain a porous self-supporting carbon current collector with a porosity gradient of 55% (near the tab) to 75% (away from the tab), a thickness of 30 μm, and an areal density of 2 mg / cm³. 2 Its electrical conductivity is 1200 S / m.
[0125] S200, the above-mentioned porous self-supporting carbon current collector is placed in a tube furnace, and a mixture of ammonia and nitrogen (volume ratio 1:4) is introduced and kept at 600℃ for 3 h to achieve nitrogen doping modification. The porous self-supporting carbon current collector with a lithiophilic modified layer has a nitrogen content of 8 at.% and a lithiophilic contact angle of 25°. The mass ratio of the lithiophilic modified layer to the porous self-supporting carbon current collector is 0.1:1.
[0126] S300, prepare a 0.3 mol / L modification solution (lithium nitrate: ammonium fluoride: phosphoric acid = 2:1:1, solvent is ethanol), and spray at a rate of 1 mL / cm under argon protection. 2After the solvent evaporates at room temperature, the mixture is allowed to stand for 3 h under a nitrogen atmosphere at 120°C to form a porous self-supporting carbon current collector with an artificial SEI layer and a lithiophilic modified layer. The thickness of the artificial SEI layer is 30 nm, the impedance is 50 Ω, and the grain size is 15 nm. The S400 electrodeposition method employed roll-to-roll electrodeposition with a 1 mol / L LiPF6 EC / DMC solution as the electrolyte and an electrodeposition current of 0.5 mA / cm². 2 Winding speed 0.5 m 2 / min, lithium deposition rate 50 mAh / cm³ 2 This yields the negative electrode sheet.
[0127] Example 2 The difference between Example 2 and Example 1 is that in step S200, the porous self-supporting carbon current collector is placed in a tube furnace, and chemical silver plating is performed for 60 min. The silver nanoparticle loading is 10% of the mass of the porous self-supporting carbon current collector, and the particle size is 5-10 nm. The remaining preparation methods and parameters are the same as in Example 1, and a negative electrode sheet is prepared.
[0128] Example 3 The difference between Example 3 and Example 1 is that in step S300, a 0.25 mol / L modification solution is prepared (the molar ratio of lithium nitrate, ammonium fluoride, and phosphoric acid is 2:1:1, and the solvent is ethanol); under argon protection, the modification solution is first introduced at a rate of 0.8 mL / cm². 2 A coating of a certain amount was applied to the surface of the porous self-supporting carbon current collector with a lithiophilic modified layer. After standing at room temperature for 10 min to evaporate some of the solvent, it was then left to stand at 120°C under a nitrogen atmosphere for 3 h to form an artificial SEI layer with a thickness of 15 nm to 20 nm, an impedance of 35 Ω to 45 Ω, and a grain size of 12 nm to 15 nm. The remaining preparation methods and parameters were the same as in Example 1, and the negative electrode sheet was prepared.
[0129] Example 4 The difference between Example 4 and Example 1 is that in step S400, "roll-to-roll" electrodeposition is used, the electrolyte is a 1 mol / L LiPF6 EC / DMC solution, and the electrodeposition current is 1 mA / cm. 2 Winding speed 0.5 m 2 / min, lithium deposition rate 80 mAh / cm³ 2 The remaining preparation methods and parameters are the same as in Example 1, and a negative electrode sheet is obtained.
[0130] Example 5 The difference between Example 5 and Example 1 is that in step S400, "roll-to-roll" electrodeposition is used, the electrolyte is a 1 mol / L LiPF6 EC / DMC solution, and the electrodeposition current is 1 mA / cm. 2 Winding speed 0.5 m 2 / min, lithium deposition rate 20 mAh / cm 2 The remaining preparation methods and parameters are the same as in Example 1, and a negative electrode sheet is obtained.
[0131] Example 6 The difference between Example 6 and Example 1 is that in step S400, "roll-to-roll" electrodeposition is used, the electrolyte is a 1 mol / L LiPF6 EC / DMC solution, and the electrodeposition current is 1 mA / cm. 2 Winding speed 0.5 m 2 / min, lithium deposition rate 100 mAh / cm³ 2 The remaining preparation methods and parameters are the same as in Example 1, and a negative electrode sheet is obtained.
[0132] Example 7 The difference between Example 7 and Example 1 is that, in S100, carbon nanotubes (aspect ratio of 100, tube diameter of 20 nm), graphene (2 layers), and phenolic resin were weighed in a mass ratio of 3:2:5. Polymethyl methacrylate microspheres (particle size 1-3 μm) accounting for 40% of the total mass of the composite material were added, and the mixture was ultrasonically dispersed for 30 min to obtain a uniform slurry. The slurry was coated to a thickness of 50 μm, dried at 120℃ for 2 h, and calcined at 1000℃ for 3 h under an argon atmosphere to obtain a porous self-supporting carbon current collector with a porosity gradient of 55% (near the tab side) to 75% (far from the tab side), a thickness of 30 μm, and a surface density of 2 mg / cm³. 2 The conductivity is 1200 S / m. The remaining preparation methods and parameters are the same as in Example 1, resulting in a negative electrode sheet.
[0133] Example 8 The difference between Example 8 and Example 1 is that, in S100, carbon nanotubes (aspect ratio of 200, tube diameter of 5 to 12 nm), graphene (4 layers), and phenolic resin were weighed in a mass ratio of 3:2:5. Polymethyl methacrylate microspheres (particle size 1-3 μm) accounting for 60% of the total mass of the composite material were added, and the mixture was ultrasonically dispersed for 30 min to obtain a uniform slurry. The slurry was coated to a thickness of 50 μm, dried at 120℃ for 2 h, and calcined at 1000℃ for 3 h under an argon atmosphere to obtain a porous self-supporting carbon current collector with a porosity gradient of 65% (near the tab side) to 85% (far from the tab side), a thickness of 30 μm, and an areal density of 1.5 mg / cm³. 2The conductivity is 800 S / m. The remaining preparation methods and parameters are the same as in Example 1, resulting in a negative electrode sheet.
[0134] Example 9 The difference between Example 9 and Example 1 is that, in S100, carbon nanotubes (aspect ratio of 200, diameter of 5-12 nm), graphene (4 layers), and phenolic resin were weighed in a mass ratio of 3:2:5. Polymethyl methacrylate microspheres (particle size 1-3 μm) accounting for 30% of the total mass of the composite material were added, and the mixture was ultrasonically dispersed for 30 min to obtain a uniform slurry. The slurry was coated to a thickness of 50 μm, dried at 120℃ for 2 h, and calcined at 1000℃ for 3 h under an argon atmosphere to obtain a porous self-supporting carbon current collector with a porosity gradient of 45% (near the tab side) to 65% (far from the tab side), a thickness of 30 μm, and an areal density of 2.5 mg / cm³. 2 The conductivity is 1500 S / m. The remaining preparation methods and parameters are the same as in Example 1, resulting in a negative electrode sheet.
[0135] Comparative Example 1 Comparative Example 1 is similar to Example 1, except that steps S200 and S300 were not performed. The rest of the preparation methods and parameters are the same as those in Example 1, and a negative electrode sheet is prepared.
[0136] Comparative Example 2 Comparative Example 2 is similar to Example 1, except that step S300 was not performed. The rest of the preparation methods and parameters are the same as those in Example 1, and a negative electrode sheet is prepared.
[0137] Comparative Example 3 Comparative Example 3 is similar to Example 1, except that in step S100, carbon nanotubes, graphene, and phenolic resin are weighed in a mass ratio of 3:2:5, and polymethyl methacrylate microspheres accounting for 40% of the total mass of the composite material are added. The polymethyl methacrylate microspheres have a uniform particle size of 2 μm to 3 μm. The mixture is ultrasonically dispersed for 30 min to obtain a uniform slurry. The coating thickness is 50 μm, and the mixture is dried at 120℃ for 2 h and calcined at 1000℃ for 3 h under an argon atmosphere to obtain a porous self-supporting carbon current collector with uniform porosity. The porosity of the porous self-supporting carbon current collector is basically the same along the thickness direction. The remaining preparation methods and parameters are the same as in Example 1, and a negative electrode sheet is prepared.
[0138] Comparative Example 4 The difference between Comparative Example 4 and Example 1 is that in step S400, a "roll-to-roll" electrodeposition is used, the electrolyte is a 1 mol / L LiPF6 EC / DMC solution, and the electrodeposition current is 1 mA / cm. 2 Winding speed 0.5 m 2 / min, lithium deposition rate 5 mAh / cm³ 2 The remaining preparation methods and parameters are the same as in Example 1, and a negative electrode sheet is obtained.
[0139] Performance testing The negative electrodes prepared in each embodiment and each comparative example were respectively compared with NCM9-based sulfide positive electrodes (2.4 mAh / cm³). 2 LPSC electrolyte matching was used to assemble all-solid-state mold batteries at an operating voltage of 2.8-4.3 V. The performance of individual battery cells was tested using the following methods, and the specific results are detailed in Table 1.
[0140] First-cycle discharge specific capacity of a single battery cell: At 25°C, the assembled solid-state lithium metal battery cell is charged to 4.3V at a current density of 0.3C, and then discharged to 2.8V at a current density of 0.3C. The discharge capacity C0 of the solid-state lithium metal battery cell is recorded. The ratio of the first-cycle discharge capacity C0 of the solid-state lithium metal battery cell to the weight of the positive electrode active material is taken as the first-cycle discharge specific capacity (mAh / g) of the solid-state lithium metal battery cell.
[0141] The first charge-discharge efficiency of a single battery cell: At 25°C, the assembled solid-state lithium metal battery cell is charged to 4.3V at a current density of 0.1C, and the charging capacity of the solid-state lithium metal battery cell is recorded as D0. Then, it is discharged to 2.8V at a current density of 0.1C. The battery cell is subjected to two charge-discharge cycles in the same manner. Then, it is charged to 4.3V at a current density of 0.3C, and then discharged to 2.8V at a current density of 0.3C. The discharge capacity of the solid-state lithium metal battery cell is recorded as C1. The first charge-discharge efficiency (%) of the solid-state lithium metal battery cell is C1 / D0×100%.
[0142] Cycle capacity retention of solid-state lithium metal battery cells: At 25°C, the assembled solid-state lithium metal battery cells are charged to 4.3V at a current density of 0.1C, and the charging capacity of the solid-state lithium metal battery cells is recorded as D0. Then, they are discharged to 2.8V at a current density of 0.1C. The battery cells are subjected to two charge-discharge cycles in the above manner. Then, they are charged to 4.3V at a current density of 0.3C, and then discharged to 2.8V at a current density of 0.3C. This cycle is repeated, and the number of cycles of the solid-state lithium metal battery cells when the discharge capacity is 80% is recorded.
[0143] Table 1 From Table 1 and Figure 2 , Figure 3The data shows that, compared with the comparative example, the all-solid-state battery assembled from the negative electrode material prepared in the example has better cycle stability and safety, indicating that the negative electrode prepared by the method of the present invention can improve the cycle performance and safety performance of the battery.
[0144] The above description is merely a specific embodiment of this application, but the scope of protection of this application is not limited thereto. Any person skilled in the art can easily conceive of various equivalent modifications or substitutions within the technical scope disclosed in this application, and these modifications or substitutions should all be included within the scope of protection of this application. Therefore, the scope of protection of this application should be determined by the scope of the claims.
Claims
1. A negative electrode sheet, characterized in that, include: A porous self-supporting carbon current collector, comprising carbon nanotubes, graphene, and a binder, wherein the porosity of the porous self-supporting carbon current collector near the tab is 50% to 65%, and the porosity of the porous self-supporting current collector away from the tab is 70% to 85%. A lithiophilic modified layer is located at least partially on the outer surface of the porous self-supporting carbon current collector and / or on the surface of the pore inner wall of the porous self-supporting carbon current collector. The lithiophilic modified layer comprises one or more of nitrogen-doped carbon materials, phosphorus-doped carbon materials, silver nanoparticles, and zinc nanoparticles. The mass ratio of the lithiophilic modified layer to the porous self-supporting carbon current collector is 0.05:1 to 0.15:
1. An artificial SEI layer is located at least partially on the surface of the lithiophilic modified layer, and the artificial SEI layer comprises lithium nitride, lithium fluoride, and lithium phosphate. as well as, Lithium metal, at least partially located on the surface of the artificial SEI layer at the interface and / or in the pores of the porous self-supporting current collector, is present in the negative electrode sheet, with an encapsulation amount of 10 mAh / cm³. 2 ~150 mAh / cm 2 .
2. The negative electrode sheet according to claim 1, characterized in that, The porous self-supporting carbon current collector satisfies at least one of the following: (1) The thickness of the porous self-supporting carbon current collector is 10 μm to 50 μm; (2) The porosity of the porous self-supporting carbon current collector is distributed in a gradient along the thickness direction; (3) The areal density of the porous self-supporting carbon current collector is 1 mg / cm³. 2 ~3 mg / cm 2 ; (4) The conductivity of the porous self-supporting carbon current collector is ≥1000 S / m; (5) The diameter of the carbon nanotubes is 10 nm to 20 nm and the aspect ratio is 50 to 100; (6) The graphene has 3 to 5 layers; (7) The softening point of the adhesive is 80℃~100℃; (8) The mass ratio of the carbon nanotubes, the graphene and the binder is (2.4~3.6):(1.6~2.4):(4~6), and can be selected as 3:2:5; (9) The adhesive includes one or more of phenolic resin, epoxy resin, polyimide resin, furan resin, and urea-formaldehyde resin; or the polymer adhesive includes one or more of polyvinylidene fluoride, polytetrafluoroethylene, styrene-butadiene rubber, carboxymethyl cellulose, polyacrylic acid, sodium alginate, and polyethylene oxide.
3. The negative electrode sheet according to claim 1, characterized in that, The lithiophilic modified layer satisfies at least one of the following: (1) The lithiophilic contact angle of the lithiophilic modified layer is ≤30°; (2) The particle size of the silver nanoparticles is 5 nm to 10 nm; (3) The particle size of the zinc nanoparticles is 5 nm to 10 nm; (4) Based on the total atomic weight of the nitrogen-doped carbon material, the atomic percentage of nitrogen is 5 at.% to 10 at.%; (5) Based on the total atomic weight of the phosphorus-doped nitrogen material, the atomic percentage of phosphorus is 3 at.% to 8 at.%.
4. The negative electrode sheet according to claim 1, characterized in that, The negative electrode sheet satisfies at least one of the following: (1) The thickness of the artificial SEI layer at the interface is 10 nm to 50 nm; (2) The impedance of the artificial SEI layer at the interface is 30 Ω~80 Ω; (3) The grain size of the artificial SEI layer at the interface is 10 nm to 18 nm; (4) The ionic conductivity of the artificial SEI layer at the interface is ≥1×10 -4 S / cm; (5) The fracture strength of the artificial SEI layer at the interface is ≥20 MPa; (6) The metallic lithium and the porous self-supporting carbon current collector form a composite structure; (7) The purity of the lithium metal is ≥99.9%; (8) The volume change rate of the porous self-supporting carbon current collector after lithium encapsulation is ≤50%.
5. A method for preparing a negative electrode sheet, characterized in that, include: Carbon nanotubes, graphene, and binder are mixed in a first predetermined mass ratio to obtain a composite material. A pore-forming agent accounting for 30% to 60% of the total mass of the composite material is added. The mixture is ball-milled using a first solvent as the dispersion medium and then ultrasonically dispersed to obtain a uniform slurry. The uniform slurry is then coated into a film, dried, and calcined under a protective atmosphere to remove the pore-forming agent, thereby obtaining the porous self-supporting carbon current collector. The porous self-supporting current collector is modified by nitrogen doping or phosphorus doping using vapor deposition, or by depositing silver nanoparticles or zinc nanoparticles using chemical plating to obtain a porous self-supporting carbon current collector with a lithium-affinity modified layer. A diluent containing lithium nitrate, ammonium fluoride, and phosphoric acid was prepared and coated onto the surface of the porous self-supporting carbon current collector with a lithium-philic modified layer under a protective atmosphere. After the solvent evaporated at room temperature, the current collector was allowed to stand under a protective atmosphere to form a porous self-supporting carbon current collector with an artificial SEI layer and a lithium-philic modified layer. Using the porous self-supporting carbon current collector with an artificial SEI layer and a lithiophilic modification layer as the cathode and lithium metal as the sacrificial anode, lithium metal is deposited onto the porous self-supporting carbon current collector with the artificial SEI layer and lithiophilic modification layer using an electrodeposition process until the lithium metal encapsulation amount reaches 10 mAh / cm³. 2 ~150mAh / cm 2 The negative electrode sheet according to any one of claims 1 to 4 is obtained.
6. The preparation method according to claim 5, characterized in that, The steps of mixing carbon nanotubes, graphene, and a binder according to a first predetermined mass ratio to obtain a composite material, adding a pore-forming agent accounting for 30% to 60% of the total mass of the composite material, ball milling with a first solvent as the dispersion medium, ultrasonic dispersion to obtain a uniform slurry, coating the uniform slurry into a film, drying, and calcining under a protective atmosphere to remove the pore-forming agent, and obtaining the porous self-supporting carbon current collector include: A composite material is obtained by mixing carbon nanotubes, graphene, and phenolic resin in a predetermined mass ratio. Polymethyl methacrylate (PMMA) microspheres, accounting for 30%–60% of the total mass of the composite material, are added. The mixture is then ball-milled at 300–500 r / min for 2–4 h using ethanol as the dispersion medium, followed by ultrasonic dispersion for 30 min to obtain a uniform slurry. This uniform slurry is then coated onto a film, dried at 120°C for 2 h, and calcined at 800°C–1200°C for 3 h under an argon atmosphere. The PMMA microspheres are then removed to obtain the porous self-supporting carbon current collector. Optionally, the PMMA microspheres exhibit a gradient distribution along the tab extension direction, with the PMMA microspheres near the tab having a particle size of 3 μm–5 μm and the PMMA microspheres away from the tab having a particle size of 1 μm–3 μm. μm; the heating rate of the calcination is 5℃ / min, and optionally, the mass ratio of carbon nanotubes, graphene and phenolic resin is 3:(1.6~2.4):(4~6), or optionally 3:2:
5.
7. The preparation method according to claim 5, characterized in that, The steps of modifying the porous self-supporting current collector with nitrogen doping or phosphorus doping by vapor deposition, or depositing silver nanoparticles or zinc nanoparticles by chemical plating, to obtain a porous self-supporting carbon current collector with a lithiophilic modified layer include: The porous self-supporting current collector is modified by nitrogen doping or phosphorus doping using a vapor phase deposition method at 500℃~700℃ for 2h~4h, or by chemical plating at 50℃~80℃ for 30min~120min to form silver nanoparticles or zinc nanoparticles, thus obtaining a porous self-supporting carbon current collector with a lithiophilic modified layer. Optionally, the nitrogen-containing gas used in the vapor phase deposition method is a mixture of ammonia and nitrogen, and the phosphorus source gas is trimethylphosphine; the concentration of silver ions in the plating solution used in the chemical plating method is 0.05mol / L~0.2mol / L, and the concentration of zinc ions is 0.1mol / L~0.3mol / L. Further optionally, the nitrogen-containing gas used in the vapor phase deposition method is a mixture of ammonia and nitrogen with a volume ratio of 1:1~1:4, and can be selected as a mixture of ammonia and nitrogen with a volume ratio of 1:
4.
8. The preparation method according to claim 5, characterized in that, The steps of preparing a diluent containing lithium nitrate, ammonium fluoride, and phosphoric acid, coating it onto the surface of the porous self-supporting carbon current collector with a lithiophilic modified layer under a protective atmosphere, evaporating the solvent at room temperature, and then allowing it to stand under a protective atmosphere to form a porous self-supporting carbon current collector with an artificial SEI layer and a lithiophilic modified layer include: A modification solution containing lithium nitrate, ammonium fluoride, and phosphoric acid with a concentration of 0.1 mol / L to 0.5 mol / L was prepared using ethanol as the solvent. The solution was prepared under argon protection using a nozzle pressure of 0.3 MPa to 0.5 MPa and a flow rate of 0.5 mL / cm². 2 ~2 mL / cm 2 The coating is applied to the surface of a porous self-supporting carbon current collector with a lithiophilic modified layer. After the solvent evaporates at room temperature, the mixture is left to stand at 100℃~150℃ in a nitrogen atmosphere for 2h~4h to form a porous self-supporting carbon current collector with an artificial SEI layer and a lithiophilic modified layer. Optionally, the molar ratio of lithium nitrate, ammonium fluoride and phosphate in the modification solution is (1.5~2.5):(0.75~1.25)~(0.75~1.25), and more preferably 2:1:
1.
9. The preparation method according to claim 5, characterized in that, The process involves using a porous self-supporting carbon current collector with an artificial SEI layer and a lithiophilic modification layer as the cathode and a lithium metal plate as the sacrificial anode. Lithium metal is deposited onto the porous self-supporting carbon current collector using an electrodeposition process until the lithium metal encapsulation amount reaches 10 mAh / cm³. 2 ~150 mAh / cm 2 The steps for obtaining the negative electrode sheet include: Using a porous, self-supporting carbon current collector with an artificial SEI layer and a lithiophilic modified layer as the cathode and a lithium metal plate as the sacrificial anode, a roll-to-roll electrodeposition process was employed in an EC / DMC electrolyte containing 5% fluoroethylene carbonate and 1 mol / L LiPF6, with the electrodeposition current controlled at 0.05 mA / cm². 2 ~4 mA / cm 2 Winding speed 0.08 m 2 / min~5 m 2 The deposition rate was 1 h / min, and the deposition time was 1 h to 12 h until the lithium metal encapsulation amount reached 10 mAh / cm³. 2 ~150 mAh / cm 2 The negative electrode sheet is obtained.
10. A lithium battery cell, characterized in that, The negative electrode sheet includes the negative electrode sheet according to any one of claims 1 to 4 and / or the negative electrode sheet prepared by the preparation method according to any one of claims 5 to 9. Optionally, the lithium battery cell is a solid-state battery cell, and the solid-state battery cell has a capacity retention rate of ≥82% and a coulombic efficiency of ≥98.8% after 300 cycles at a 0.3 C rate.