Anode for lithium-ion batteries
By depositing a fluorinated copolymer film on the anode surface of a lithium-ion battery, the problem of dendritic crystal formation is solved, improving the battery's stability and lifespan, making it suitable for lithium-ion rechargeable batteries.
Patent Information
- Application Number
- CN202611479804.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2018-07-27
- Filing Date
- 2019-07-25
- Publication Date
- 2026-11-24
AI Technical Summary
Existing lithium-ion batteries are prone to dendritic crystal formation at high charging/discharging rates, leading to decreased battery performance and safety hazards. Existing protection methods are complex and difficult to implement industrially.
The lithium-ion battery anode employs a fluorinated copolymer film, which comprises a copolymer or ternary copolymer of vinylidene fluoride and trifluoroethylene units. This film is deposited on the surface of the negative electrode active material of the lithium-ion battery to suppress the formation of dendritic crystals.
It effectively suppresses lithium dendrite formation, improves battery stability and lifespan, and is suitable for lithium-ion rechargeable batteries.
Abstract
Description
[0001] This application is a divisional application of the application filed on July 25, 2019, with application number 201980056131.2 and invention title "Anode for Lithium-ion Batteries". Technical Field
[0002] This invention generally relates to the field of energy storage in Li-ion type lithium rechargeable batteries. More specifically, the invention relates to an anode for a Li-ion rechargeable battery, said anode comprising a protective film based on a fluorinated copolymer. The invention also relates to a method for preparing this anode. Finally, the invention relates to a Li-ion rechargeable battery comprising an anode according to the invention. Background Technology
[0003] Common lithium-ion batteries contain a flammable liquid electrolyte based on a solvent and lithium salt. Given the increasing use of this type of battery in consumer electronics (such as computers, tablets, or mobile phones (smartphones)) and in the transportation sector (especially in the case of electric vehicles), improving the safety of these lithium batteries and reducing manufacturing costs have become major challenges. These batteries use a graphite anode, into which Li ions are inserted during charging. The resulting compound is C6Li, which is one Li equivalent per 72 g of graphite.
[0004] It has long been known that replacing graphite with a Li metal anode can achieve a significant increase in energy density, but the main challenge of using anodes made of lithium metal involves the formation of Li dendritic crystals during metal reduction, which can lead to low coulombic efficiency, increased battery volume, accelerated electrolyte decomposition, separator perforation, and therefore short circuits and thermal runaway.
[0005] It is possible to heal deposits by using additives to stabilize the interface, by using agents that act as shields, or by using ceramics to mechanically block growth.
[0006] Stabilization of the Li anode will be advantageous for both solvent / salt paired batteries and solid polymer electrolyte (SPE) batteries, which have no liquid solvent, thus avoiding the use of flammable liquid components as in conventional Li-ion batteries and enabling the production of thinner and potentially more flexible batteries.
[0007] Therefore, Yong-Gun Lee et al. published a paper titled "Dendrically Free Lithium Deposition with Interconnected Microspheres Protected Lithium Metal Anodes" (…). Dendrite-Free Lithium Deposition for Lithium Metal Anodes with Interconnected Microsphere ProtectionA solution is proposed in *Chem. Mater.*, 2017, 29(14), pp. 5906-5914. This literature describes a Li metal anode protected by polystyrene-co-divinylbenzene P (S-DVB) microspheres. These microspheres guide ions toward specific regions and exert mechanical pressure on them during the growth of dendritic crystals.
[0008] The publication "Lithium Metal Anode: Protection Method" by Y. Liu and Y. Cui in Joule, January 2017, pp. 643-650 Lithium Metal Anodes: A Recipe for Protection In another method proposed in [the paper], a protective layer can be formed during battery operation to create an SEI (solid electrolyte interface). This interface is an ionic conductor formed by a mixture of Li₂S₆ and P₂S₅ (denoted as LSPS), which is intercalated to produce unique polymeric species in dimethoxyethane (DME). Additives are reduced on the surface of Li metal, resulting in a dense layer of Li₃PS₄. The amorphous nature of this material is crucial for good protection. The SEI is uniform and compact, with no high defect density.
[0009] Both of the aforementioned methods are complex and difficult to implement. The microspheres must possess high size and cross-linking homogeneity to prevent weak areas where dendritic crystals might exert stress. The structure of Li3PS4 must also be sufficiently controlled to provide optimal protection. This control is not easy. Furthermore, this structure is extremely sensitive to moisture and oxygen, making its handling challenging.
[0010] The disclosure by Ding et al. in the Journal of the American Chemical Society (J. Am. Chem. Soc.) 2013, 135, 4450-4456, entitled "Denial-free Lithium Deposition via Self-Healing Electrostatic Shielding Mechanism" Dendrite-Free Lithium Deposition via Self-Healing Electrostatic Shield Mechanism The paper proposes an electrostatic self-healing mechanism that reduces lithium dendrite formation by using cations, which have a lower reduction probability than Li / Li+ (Rb,Cs). These cations accumulate near the initial Li clusters, creating an electrostatic shield. This shield is detrimental to the growth of new lithium atoms on the existing clusters. This means that the lithium layer has better quality and is smoother. The disadvantages of this method are low coulombic efficiency due to poor SEI (solid-state electrode interface) and the cost and availability of Rb and Cs.
[0011] Another solution used to stabilize the interface with the anode is to cover the electrode with a polymer or solid layer. The disclosure by I.S. Kang et al. in the Journal of Electrochem. Soc. 2014, 161, A53-A57, entitled "Improved Cycle Stability of Lithium Electrodes in Rechargeable Lithium Batteries," is relevant. Improved Cycling Stability of Lithium Electrodes in Rechargeable Lithium Batteries The description refers to the application of a poly(3,4-ethylenedioxythiophene)-co-poly(ethylene glycol) copolymer layer on a Li metal anode.
[0012] Document KR20110082289 describes a Li-ion battery in which a polymer membrane containing lithium powder is placed between an electrode and a separator. The membrane is prepared by applying a solution to the electrode followed by a drying step, in which lithium metal is dispersed in a polymer binder solution. The binder solution is prepared by dissolving at least one of the following polymers in a non-aqueous solvent: fluorine-based polymers, acrylic polymers, SBR (styrene-butadiene) rubber, and polyacrylonitrile-based polymers.
[0013] However, these methods are based on restricting and not altering the inherent behavior of dendritic crystal growth.
[0014] Therefore, there is still a need for an anode for Li-ion rechargeable batteries that is protected by effective means against dendritic crystal formation and is compatible with industrial implementation methods.
[0015] The objective of this invention is therefore to significantly address at least one of the shortcomings of the prior art, particularly at high charge / discharge rates, namely dendritic crystal formation.
[0016] The present invention also aims to provide a method for manufacturing such anodes, wherein the anodes are stabilized by means of deposition of a fluorinated copolymer film. Finally, the present invention aims to provide a Li-ion rechargeable battery comprising a stabilized anode. Summary of the Invention
[0017] This invention primarily relates to a negative electrode (or anode) for a lithium-ion battery, comprising a current collector and a negative electrode active material layer covered with a fluorinated copolymer film. The term "fluorinated copolymer" includes copolymers and terpolymers described below.
[0018] Typically, the membrane comprises at least one of the following copolymers:
[0019] - A copolymer of formula P(VDF-TrFE) containing vinylidene fluoride and trifluoroethylene units, or
[0020] - A copolymer of formula P(VDF-TFE) containing vinylidene fluoride and tetrafluoroethylene units, or
[0021] - Selected from the following fluorinated terpolymers:
[0022] - A terpolymer of formula P(VDF-TrFE-CTFE) containing vinylidene fluoride, trifluoroethylene, and chlorotrifluoroethylene units.
[0023] - A terpolymer of formula P(VDF-TrFE-CTFE) containing vinylidene fluoride, trifluoroethylene, and chlorotrifluoroethylene units.
[0024] - A terpolymer of formula P(VDF-TrFE-HFP) containing vinylidene fluoride, trifluoroethylene, and hexafluoropropylene units.
[0025] - A terpolymer of formula P(VDF-TFE-CFE) containing vinylidene fluoride, tetrafluoroethylene, and 1,1-chlorofluoroethylene units.
[0026] - A terpolymer of formula P(VDF-TFE-CTFE) containing vinylidene fluoride, tetrafluoroethylene, and trichlorotrifluoroethylene units.
[0027] - A terpolymer of formula P(VDF-TFE-HFP) containing vinylidene fluoride, tetrafluoroethylene and hexafluoropropylene units.
[0028] According to various embodiments, the anode includes the following features, which can be combined if desired.
[0029] According to one embodiment, the membrane comprises a blend of P(VDF-TrFE) copolymer and P(VDF-TFE) copolymer.
[0030] According to one embodiment, the membrane comprises a blend of a P(VDF-TrFE) copolymer and one of the aforementioned terpolymers.
[0031] According to one embodiment, the membrane comprises a blend of a P(VDF-TFE) copolymer and one of the aforementioned terpolymers.
[0032] According to one embodiment, the membrane comprises a blend of two terpolymers selected from those listed above.
[0033] The negative electrode active material is an alkali metal. According to one embodiment, the negative electrode active material is lithium.
[0034] According to one embodiment, the membrane has a thickness of 1 to 14 micrometers, preferably 1 to 10 micrometers, and more preferably in the range of 2 to 10 micrometers, including the limit value.
[0035] According to one embodiment, the membrane has a concentration of 1.2 to 2 g / cm³. 3 Density within the range.
[0036] The present invention also relates to a method for manufacturing a negative electrode comprising a layer of negative electrode active material covered with a fluorinated copolymer film as described above. This method includes the step of depositing or forming a fluorinated copolymer film on the surface of the negative electrode active material.
[0037] According to one embodiment, the film is formed via a solvent approach, by evaporating a solvent from a solution of the fluorinated copolymer.
[0038] According to one embodiment, the deposition of the membrane is carried out via a drying process, which involves preparing a fluorinated membrane on a suitable support and transferring this fluorinated membrane onto a negative electrode active material layer.
[0039] Another subject of the present invention is a Li-ion rechargeable battery comprising the negative electrode, the positive electrode and the electrolyte.
[0040] Another subject of this invention is the use of copolymers or blends, said copolymers being selected from the following:
[0041] - A copolymer of formula P(VDF-TrFE) containing vinylidene fluoride and trifluoroethylene units.
[0042] - A P(VDF-TFE) copolymer containing vinylidene fluoride and tetrafluoroethylene units, and
[0043] - Selected from the following fluorinated terpolymers: terpolymer of formula P(VDF-TrFE-CFE) containing vinylidene fluoride, trifluoroethylene, and chlorofluoroethylene units; terpolymer of formula P(VDF-TrFE-CTFE) containing vinylidene fluoride, trifluoroethylene, and chlorotrifluoroethylene units; terpolymer of formula P(VDF-TrFE-HFP) containing vinylidene fluoride, trifluoroethylene, and hexafluoropropylene units; terpolymer of formula P(VDF-TFE-CFE) containing vinylidene fluoride, tetrafluoroethylene, and chlorofluoroethylene units; terpolymer of formula P(VDF-TFE-CTFE) containing vinylidene fluoride, tetrafluoroethylene, and chlorotrifluoroethylene units; and terpolymer of formula P(VDF-TFE-HFP) containing vinylidene fluoride, tetrafluoroethylene, and hexafluoropropylene units.
[0044] The blend is selected from the following: a blend of P(VDF-TrFE) copolymer and P(VDF-TFE) copolymer; a blend of P(VDF-TrFE) copolymer and one of the aforementioned ter copolymers; a blend of P(VDF-TFE) copolymer and one of the aforementioned ter copolymers; and a blend of two of the aforementioned ter copolymers.
[0045] It is used as a film to cover the anode of a lithium-ion battery containing negative electrode active material in order to suppress the formation of lithium dendrites within the negative electrode active material.
[0046] This invention makes it possible to overcome the shortcomings of existing technologies. More particularly, it provides an anode stabilized by the presence of a fluorinated copolymer film deposited on the surface of the negative electrode active material, said film inhibiting the formation of dendritic crystals within the negative electrode active material. It is particularly suitable for manufacturing lithium-ion rechargeable batteries in which the negative electrode active material is lithium. The stability of this electrode improves battery performance and lifespan. Detailed Implementation
[0047] The invention will now be described in more detail and in a non-limiting manner in the following detailed description.
[0048] According to a first aspect, the present invention relates to a negative electrode for a lithium-ion battery, comprising a current collector and a negative electrode active material layer covered with a fluorinated copolymer film. Typically, the film comprises at least one copolymer of formula P(VDF-TrFE) containing vinylidene fluoride and trifluoroethylene units, or a copolymer of formula P(VDF-TFE) containing vinylidene fluoride and tetrafluoroethylene units, or a fluorinated terpolymer selected from: a terpolymer of formula P(VDF-TrFE-CFE) containing vinylidene fluoride, trifluoroethylene, and 1,1-chlorofluoroethylene units; a terpolymer of formula P(VDF-TrFE-CTFE) containing vinylidene fluoride, trifluoroethylene, and chlorotrifluoroethylene units; or a terpolymer containing vinylidene fluoride, trifluoroethylene, and hexafluoropropylene units. The following are considered copolymers: a terpolymer of the formula P(VDF-TrFE-HFP), a terpolymer of the formula P(VDF-TFE-CFE) containing vinylidene fluoride, tetrafluoroethylene and chlorofluoroethylene units, a terpolymer of the formula P(VDF-TFE-CTFE) containing vinylidene fluoride, tetrafluoroethylene and chlorotrifluoroethylene units, a terpolymer of the formula P(VDF-TFE-HFP) containing vinylidene fluoride, tetrafluoroethylene and hexafluoropropylene units, or a blend of one of the copolymers with one of the terpolymers, or a blend of two copolymers or a blend of two terpolymers.
[0049] The negative electrode active material can be an alkali metal, an alkaline earth metal, or an element from the boron group. The negative electrode active material required in this invention is an alkali metal.
[0050] According to various embodiments, the anode includes the following features, which can be combined if desired.
[0051] According to one embodiment, the negative electrode active material is lithium.
[0052] According to one embodiment, the membrane has a thickness (including limits) in the range of 1 to 14 micrometers, preferably 1 to 10 micrometers, and more preferably 2 to 10 micrometers. The thickness of the fluorinated membrane must be limited to avoid interfacial impedance that is detrimental to the power operation of the battery. If the membrane is too thick, lithium diffusion slows down.
[0053] According to one embodiment, the fluorinated membrane has a concentration of 1.2 to 2 g / cm³. 3 Density within the range.
[0054] According to one embodiment, the fluorinated membrane is a porous membrane with a micropore size between 100 nanometers and 1 micrometer.
[0055] The presence of a fluorinated film on the negative electrode active material layer makes it possible to prevent or at least significantly reduce the formation of lithium dendrites. The targeted copolymers or terpolymers are naturally polar: the FE phase (ferroelectric phase for the copolymer) and / or the RFE phase (relaxed ferroelectric phase for the terpolymer), which are similar to the β phase obtained for PVDF under very specific conditions (e.g., by stretching or dissolving the film in a specific solvent and slowly evaporating or adding additives, the solution being incompatible with industrially applicable methods). Without desiring to elaborate on the technical details, the applicant believes that the polarity of the fluorinated film obtained from the described copolymers and terpolymers is sufficient to allow the lithium cations to be oriented in a plane parallel to the collector and the Li metal film, rather than in a vertical direction that would promote dendrite formation.
[0056] This invention is therefore based on the use of fluorinated copolymers or terpolymers or blends thereof, which are in the form of films deposited on the surface of the negative electrode active material. The term "..." Fluoride "This should be understood as meaning a polymer containing -F groups."
[0057] Preferably, the copolymer and ternary copolymer are ferroelectric or relaxor ferroelectric polymers. Ferroelectric copolymers or ternary copolymers exhibit high polarization hysteresis (charge pair in the field of application) (with high coercive magnetic fields (typically about 20 V / µm, or even 50 V / µm)) and high remanent polarization (typically about 60 mC / m). 2 Relaxor ternary copolymers or copolymers have low coercive magnetic fields (typically below 10 V / µm) and low remanent polarization (typically below 20 mC / m). 2 or even no residual polarization, high saturation polarization (typically around 60 mC / m) 2 Or even 70 mC / m 2 ) and the maximum dielectric permittivity that varies with temperature depending on the frequency of the electric field.
[0058] In addition, another advantage is the higher capacitance of copolymers, especially ternary copolymers, which make it possible to obtain more significant polarization and more significant electrolyte dissociation at the lithium interface.
[0059] The copolymers and terpolymers exhibit a relative dielectric permittivity greater than 10 at 23°C and 1 kHz. The maximum dielectric permittivity as a function of temperature is at least 30 or even 40. The relative dielectric permittivity can be measured by dielectric spectroscopy analysis.
[0060] The Curie temperature of the P(VDF-TrFE) copolymer is between 50°C and 140°C. The Curie temperature of the polymer of the present invention can be measured by differential scanning calorimetry or by dielectric spectroscopy.
[0061] According to one embodiment, in the copolymer of formula P(VDF-TrFE), the proportion of trifluoroethylene-derived units is less than 55 mol% and more than 18 mol% relative to the sum of units derived from vinylidene fluoride and trifluoroethylene.
[0062] According to one embodiment, in the copolymer of formula P(VDF-TFE), the proportion of tetrafluoroethylene-derived units is less than 60 mol% and more than 10 mol% relative to the sum of units derived from vinylidene fluoride and tetrafluoroethylene.
[0063] The copolymers and terpolymers of the present invention can be produced using any known method, such as emulsion polymerization, microemulsion polymerization, suspension polymerization, and solution polymerization. For the purposes of terpolymers, the method described in document WO 2010 / 116105 is particularly preferred. This method makes it possible to obtain terpolymers with high molecular weights and suitable structures.
[0064] According to one embodiment, the weight-average molar mass of the terpolymer (also expressed as “molecular weight” (Mw) in the context of this patent application) has a value of 200,000 to 1,500,000 g / mol, preferably 250,000 to 1,000,000 g / mol, and more specifically 300,000 to 700,000 g / mol.
[0065] The latter can be adjusted by modifying certain parameters of the method (e.g., the temperature in the reactor) or by adding a transfer agent.
[0066] Molecular weight distribution was estimated using SEC (size exclusion chromatography) with dimethylformamide (DMF) as the eluent and a set of three columns with increasing porosity. The stationary phase was styrene-DVB gel. Assays were based on refractive index measurements and calibrated using polystyrene standards. Samples were dissolved in DMF at 0.5 g / L and filtered through a 0.45 μm nylon filter.
[0067] The molecular weight can also be evaluated according to ASTM D1238 (ISO 1133) by measuring the melt flow index (MFI) at 230°C with a 10 kg load. The MFI is between 0.1 and 100, preferably between 0.5 and 50, and more specifically between 1 and 10.
[0068] Furthermore, molecular weight can also be characterized by measuring the viscosity of the solution according to standard ISO 1628. Methyl ethyl ketone (MEK) is a preferred solvent for determining the viscosity index of terpolymers.
[0069] More generally, the molar composition of the terpolymer of the present invention can be determined by various means. Conventional methods for elemental analysis of carbon, fluorine, and chlorine or bromine produce two or three independent sets of equations with two independent unknowns (e.g., % VDF and % TrFE, where % Y = 100 - (% VDF + % TrFE)), which makes it possible to explicitly calculate the weight composition of the polymer and infer the molar composition from the weight composition.
[0070] Multi-core processors can also be used (in this example, protons). 1 H) and fluorine ( 19 FT-NMR technology is used to analyze solutions of polymers in appropriately deuterated solvents. NMR spectra are recorded on an FT-NMR spectrometer equipped with multinuclear probes. Specific signals from different monomers are then located in the spectra generated by one or more nuclei. Thus, for example, in proton NMR, the TrFE (CFH=CF2) unit gives a specific signal characteristic of the CFH group (at approximately 5 ppm). The CH2 group of VDF shows the same pattern (a broad, unresolved peak centered at 3 ppm). The relative integral of the two signals gives the relative abundance of the two monomers, i.e., the VDF / TrFE molar ratio.
[0071] The combination of relative integrals of various signals obtained in proton NMR and fluorine NMR produces a set of equations, the analysis of which leads to the determination of the molar concentrations of various monomer units.
[0072] Finally, it is possible to combine elemental analysis (e.g., for heteroatoms of chlorine or bromine) and NMR analysis. Therefore, the content of CTFE or CFE can be determined by measuring the chlorine content using elemental analysis.
[0073] Those skilled in the art will thus gain access to a range of methods or combinations thereof that allow them to determine the composition of the terpolymer of the present invention without ambiguity and with the necessary precision.
[0074] According to one embodiment, the molar ratio of VDF units to TrFE or TFE units in the terpolymer has a value of 85 / 15 to 30 / 70, and preferably 75 / 25 to 40 / 60.
[0075] According to one embodiment, the proportion of units derived from CFE, HFP, or CTFE monomers is 1 to 15 mol% relative to all units of the terpolymer, more preferably 1 to 12 mol%.
[0076] According to one embodiment, the fluorinated copolymer or terpolymer may contain additional units introduced during free radical polymerization, in amounts between 0.1 and 10 mol%, preferably between 0.2 and 8 mol%, and specifically between 0.5 and 5 mol%. These additional units make it possible to improve certain specific properties of the membrane without degrading its electroactive characteristics, such as improving adhesion by introducing functional units of acids, alcohols, glycidyl groups, or phosphonate types (e.g., trifluoromethacrylic acid).
[0077] According to one embodiment, the fluorinated copolymer or terpolymer may be functionalized. That is, chemical modification is performed after the polymerization step to introduce chemical functional groups along the polymer chain, for example, to enable crosslinking of the film with, for example, a terpolymer carrying an azide functional group, or to improve the adhesion of the film to the electrode with, for example, a terpolymer carrying an associative functional group (e.g., imidazoalkyl, triazolyl, triazine, bisureyl, ureidylpyrimidinyl).
[0078] The copolymers of formula P(VDF-TrFE) or P(VDF-TFE) are compatible with the terpolymers listed above that have a Curie temperature different from that of the terpolymers. The term "compatible" should be understood to mean that the blend of the two polymers forms a homogeneous phase with a single glass transition temperature.
[0079] According to one embodiment, when the fluorinated film deposited on the negative electrode active material is formed by a blend of copolymer and terpolymer, these fluorinated films are present in a weight ratio of 50:50 to 1:99, preferably 45:55 to 1:99, and more particularly preferably 40:60 to 5:95.
[0080] According to one embodiment, the membrane further comprises a compatible polymer of the acrylic and / or methacrylic acid type. These polymers have the function of stabilizing the membrane, promoting adhesion, or enabling crosslinking.
[0081] According to a second aspect, the present invention relates to a method for manufacturing a negative electrode comprising a negative electrode active material layer, said negative electrode active material layer being covered with a fluorinated copolymer film as described above. This method includes the step of depositing or forming a fluorinated copolymer film on the surface of said negative electrode active material.
[0082] According to one embodiment, film deposition is performed via a solvent approach. Specifically, if the anode is made of Li metal, the solvent approach involves dissolving the fluorinated copolymer and / or fluorinated terpolymer in a solvent or solvent mixture that does not damage the anode. Specifically, many solvents, including ketones or esters, damage the Li metal via a chemical reaction.
[0083] The copolymers and terpolymers based on vinylidene fluoride and trifluoroethylene are soluble in a variety of solvents. Unlike PVDF homopolymers, they readily crystallize to obtain polar (ferroelectric or relaxor ferroelectric) phases from solution. This makes it possible to produce deposits that suppress dendritic crystal formation simply, quickly, and at low cost.
[0084] The solvents used in this invention are selected from the group consisting of: carbonates, carbamates, nitriles, amides, sulfoxides (e.g., dimethyl sulfoxide), sulfolane, nitromethane, 1,3-dimethyl-2-imidazolidineone, 1,3-dimethyl-3,4,5,6-tetrahydro-2(1,H)-pyrimidinone, 3-methyl-2-oxazolidineone, and mixtures thereof.
[0085] Among nitrile, examples may be mentioned such as acetonitrile, acetone nitrile, propionitrile, methoxypropionitrile, dimethylaminopropionitrile, butyronitrile, isobutyronitrile, valerate, neovalerate, isovaleritrile, glutaronitrile, methoxyglutaronitrile, 2-methylglutaronitrile, 3-methylglutaronitrile, adiponitrile, malononitrile and mixtures thereof.
[0086] Among carbonates, cyclic carbonates may be mentioned, for example, such as ethylene carbonate (EC) (CAS: 96-49-1), propylene carbonate (PC) (CAS: 108-32-7), butyl carbonate (BC) (CAS: 4437-85-8), dimethyl carbonate (DMC) (CAS: 616-38-6), diethyl carbonate (DEC) (CAS: 105-58-8), methyl ethyl carbonate (EMC) (CAS: 623-53-0), diphenyl carbonate (CAS 102-09-0), methyl phenyl carbonate (CAS: 13509-27-8), dipropyl carbonate (DPC) (CAS: 623-96-1), methyl propyl carbonate (MPC) (CAS: 1333-41-1), ethyl propyl carbonate (EPC), and vinylene carbonate (VC) (CAS: 96-96-1). 872-36-6), fluoroethylene carbonate (FEC) (CAS: 114435-02-8), trifluoropropylene carbonate (CAS: 167951-80-6), or mixtures thereof.
[0087] These solvents advantageously have a dielectric constant greater than or equal to 1 in a temperature range between 0 and 100°C, preferably between 10 and 80°C, and advantageously between 15 and 70°C. Dielectric permittivity can be measured using a Sefelec LCR 819 LCR instrument, which allows for the measurement of capacitance proportional to permittivity.
[0088] The step of depositing a solution of copolymers and / or terpolymers and one or more solvents onto the negative electrode active material in the form of a film is followed by a step of evaporating the solvent (drying the film). After drying, according to one embodiment, the film has a thickness of 2 to 14 micrometers, preferably in the range of 2 to 10 micrometers (including limits).
[0089] According to one embodiment, the deposition of the membrane is carried out via a drying process, which involves preparing a fluorinated membrane on a suitable support and transferring this fluorinated membrane onto the negative electrode active material layer. The transfer of the fluorinated membrane is performed by any mechanical method, which may be achieved by means of a roller or by lamination, followed by pressing with a heat supply not exceeding 100°C.
[0090] According to one embodiment, the solution contains a co-crosslinking agent, such as a (meth)acrylic acid monomer that is difunctional or polyfunctional in terms of reactive double bonds; a difunctional or polyfunctional primary amine; a difunctional or polyfunctional compound carrying an azide functional group; an organic peroxide; or a difunctional or polyfunctional allyl compound. After deposition in film form, the method according to the invention comprises the step of crosslinking the film thermally (between 30°C and 200°C, preferably between 50°C and 180°C, and specifically between 60°C and 160°C); or radiatively (preferably with ultraviolet radiation, and specifically with wavelengths between 250 and 405 nm). After crosslinking, the latter is insoluble in some or all of these solvents that can be used to generate the solution, thus giving the crosslinked film a particular advantage because the use of electrolytes is no longer limited by the solubility of the film.
[0091] Another subject of the present invention is a Li-ion rechargeable battery comprising the negative electrode, the positive electrode and the electrolyte.
[0092] Example
[0093] The following examples illustrate the scope of the invention in a non-limiting manner.
[0094] The sample was heated to 100°C and held at this temperature for 3 minutes to eliminate its thermal history. The product was then cooled to -80°C and then heated to 200°C at a rate between 5°C / min and 20°C / min.
[0095] Example 1 (Comparison)
[0096] The button cell assembly includes a Li metal anode, a 25-micron-thick PP separator, and contains 2% PVDF, 5% Ketjen Black, and 93% NMC 111 (LiNi). 0.33 Mn 0.33 Co 0.32 The cathode is O2. The electrolyte is 1 M LiFSI in the form of a mixture of EMC / EC (7 / 3 volume).
[0097] The cycle consists of 300 cycles of charging and discharging between 3 and 4.2 volts at 2°C.
[0098] Example 2
[0099] A P(VDF-TrFE) copolymer solution with a molar composition of 80% VDF and 20% TrFE was prepared in a 3 / 7 volume ratio EC / EMC mixture. Subsequently, an amount of liquid sufficient to obtain a 4-micron film after drying was deposited onto a Li metal foil in a glove box. Relatively rapid evaporation of the copolymer solution was then performed.
[0100] The button cell assembly includes a fluorinated copolymer-treated Li anode, a 25-micron-thick PP separator, and a battery containing 2% PVDF, 5% Ketjen Black, and 93% NMC 111 (LiNi). 0.33 Mn 0.33 Co 0.32 The cathode is O2. The electrolyte is 1 M LiFSI in the form of a mixture of EMC / EC (7 / 3 volume ratio).
[0101] The cycle consists of 300 cycles of charging and discharging between 3 and 4.2 volts at 2°C.
[0102] Example 3
[0103] Two button batteries were removed in a glove box, and the Li anodes were examined by scanning electron microscopy (SEM). The anodes treated with the fluorinated copolymer of Example 2 began to exhibit very few dendritic crystals, which were less than 50 nanometers in size and had a low surface density.
[0104] The untreated anode from Comparative Example 1 has dendritic crystals with a much higher surface density and a length between a few nanometers and about 1 micrometer.
[0105] Example 4
[0106] A P(VDF-TrFE-CTFE) terpolymer solution was prepared in dimethoxyethane. The molar ratio of VDF units to TrFE units was 67%, and the molar ratio of CTFE was 8%. Subsequently, an amount of liquid sufficient to obtain a non-porous 4-micron film after drying was deposited onto a Li metal foil in a glove box. Relatively rapid evaporation of the copolymer solution was then performed.
[0107] The button cell assembly includes a fluorinated terpolymer-treated Li anode, a 25-micron-thick PP separator, and a battery containing 2% PVDF, 5% Ketjen Black, and 93% NMC 111 (LiNi). 0.33 Mn 0.33 Co 0.32 The cathode is O2. The electrolyte is 1 M LiFSI in the form of a mixture of EMC / EC (7 / 3 volume ratio).
[0108] The cycle consists of 100 cycles of charging and discharging between 3 and 4.2 volts at 2°C.
[0109] Example 5
[0110] The button cell from Example 4 was disassembled in a glove box and the Li anode was examined by scanning electron microscopy (SEM). The anode treated with the fluorinated terpolymer of Example 4 began to exhibit very few dendritic crystals, which were smaller than 12-13 nm in size and had a low surface density. The examination showed that the terpolymer appeared to be more effective than the copolymer from Example 2.
[0111] Example 6
[0112] A P(VDF-TrFE) copolymer solution with a molar composition of 80% VDF and 20% TrFE in 1,3-dioxane was prepared. The solution was then deposited onto a glass support and allowed to stand for the time required for solvent removal to complete. The fluorinated copolymer membrane was then separated and mechanically applied to a Li metal strip in a glove box. A pressure of 1 MPa was applied to the assembly at 60°C to obtain a controllable fluorinated membrane-Li anode composite. A button cell assembly was formed with a fluorinated copolymer-treated Li anode, a 25-micron-thick PP separator, and a substrate containing 2% PVDF, 5% Ketjen Black, and 93% NMC 111 (LiNi). 0.33 Mn 0.33 Co 0.32 The cathode was O2. The electrolyte was a 1 M LiFSI in the form of a mixture of EMC / EC (7 / 3 volume ratio). Cycling was performed at 2 °C for 100 cycles of charging and discharging between 3 and 4.2 volts.
[0113] The button battery was removed in a glove box, and the Li anode was examined by scanning electron microscopy (SEM). The treated anode began to exhibit very few dendritic crystals, with a size of less than 50 nanometers and a low surface density.
Claims
1. An anode for a lithium-ion battery comprising a negative electrode active material, said anode being coated with a membrane, said membrane comprising at least one copolymer selected from: - Selected from the following fluorinated terpolymers: terpolymers of formula P(VDF-TrFE-CTFE) containing vinylidene fluoride, trifluoroethylene, and chlorotrifluoroethylene units. The active material of the negative electrode is an alkali metal.
2. The anode according to claim 1, wherein the negative electrode active material is lithium.
3. The anode according to any one of claims 1 and 2, wherein the membrane has a thickness in the range of 1 micrometer to 14 micrometers, preferably 1 micrometer to 10 micrometers, more preferably 2 micrometers to 10 micrometers and including the limit value.
4. The anode according to any one of claims 1 to 3, wherein the membrane has a concentration of 1.2 g / cm³. 3 Up to 2 g / cm 3 Density within the range.
5. The anode according to any one of claims 1 to 4, wherein, When the fluorinated film deposited on the negative electrode active material is formed by a blend of copolymer and terpolymer, these substances are present in a weight ratio of 50:50 to 1:99, preferably 45:55 to 1:99, and more particularly preferably 40:60 to 5:
95.
6. The anode according to any one of claims 1 to 5, wherein the molar ratio of the VDF unit to the TrFE unit in the terpolymer has a value of 85 / 15 to 30 / 70, and preferably 75 / 25 to 40 / 60.
7. The anode according to any one of claims 1 to 6, wherein the proportion of units derived from the CTFE monomer is 1 mol% to 15 mol% relative to all said units of the terpolymer, more preferably 1 mol% to 12 mol%.
8. A method for manufacturing a negative electrode, the negative electrode comprising a layer of negative electrode active material covered with a membrane according to any one of claims 1 to 7, the method comprising the step of depositing the membrane on the surface of the negative electrode active material.
9. The method of claim 8, wherein the deposition of the membrane is carried out via a solvent route.
10. The method of claim 8, comprising the step of dissolving the fluorinated terpolymer in a solvent selected from the group consisting of: carbonates, urethanes, nitriles, amides, sulfoxides (e.g., dimethyl sulfoxide), sulfolane, nitromethane, 1,3-dimethyl-2-imidazolidineone, 1,3-dimethyl-3,4,5,6-tetrahydro-2(1,H)-pyrimidinone, 3-methyl-2-oxazolidineone, and mixtures thereof.
11. The method of claim 8, wherein the deposition of the membrane is carried out via a drying process.
12. A Li-ion rechargeable battery comprising a negative electrode, a positive electrode, and an electrolyte as described in any one of claims 1 to 7.
13. Use of a copolymer, said copolymer being selected from: - Selected from the following fluorinated terpolymers: terpolymers of formula P(VDF-TrFE-CTFE) containing vinylidene fluoride, trifluoroethylene, and chlorotrifluoroethylene units. It is used as a membrane to cover the anode of a lithium-ion battery containing a negative electrode active material in order to suppress the formation of lithium dendrites within the negative electrode active material.
Citation Information
Patent Citations
Method for the production of terpolymers based on VDF, trfe and CFE, or ctfe
WO2010116105A1