Coated dry battery negative electrode sheet, preparation method and lithium ion battery
By introducing a polyoxyethylene coating layer on the surface of the negative electrode active material, the electrical connection between graphite and polytetrafluoroethylene binder is blocked, which solves the problem of easy decomposition of polytetrafluoroethylene in the negative electrode system and improves the initial coulombic efficiency and cycle life of the battery.
Patent Information
- Application Number
- CN202611405515.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-10
- Publication Date
- 2026-11-24
AI Technical Summary
In the prior art, polytetrafluoroethylene (PTFE) as a dry binder is prone to reduction side reactions in the negative electrode system, resulting in severe irreversible capacity loss and limiting the development of high-loading dry electrodes.
By introducing a polyoxyethylene coating layer on the surface of the negative electrode active material, it is used as an electrical isolator to block the direct electrical connection between graphite and polytetrafluoroethylene binder, thereby inhibiting the reduction decomposition reaction.
It significantly improves the battery's initial coulombic efficiency and cycle life, achieving high capacity and long cycle life performance of high-load dry electrode.
Smart Images

Figure REF-OBJ-1789026471460-000001
Abstract
Description
Technical Field
[0001] This invention relates to the field of battery manufacturing technology, and more specifically, to a coated dry-process battery negative electrode, a preparation method thereof, and a lithium-ion battery. Background Technology
[0002] Since the commercialization of lithium-ion batteries, polyvinylidene fluoride (PVDF) has been frequently used as the main binder for electrodes due to its excellent adhesion to metal surfaces and good electrochemical stability. However, the manufacturing of PVDF-based electrodes is essentially a wet process, requiring the use of solvents such as N-methylpyrrolidone (NMP) to convert the electrode components into a homogeneous slurry. NMP's toxicity, high boiling point, and high volatility result in high manufacturing costs and serious environmental pollution problems. More importantly, in the preparation of high-load, thick graphite electrodes, the wet slurry process often leads to uneven distribution and poor contact of conductive additives due to uneven evaporation of NMP solvent along the electrode contour. This, in turn, causes defects such as low utilization of active materials, easy electrode detachment from copper foil, and high internal resistance.
[0003] Compared to PVDF, polytetrafluoroethylene (PTFE) exhibits stronger adhesion to electrode materials due to its hydrogen-free perfluorinated bonds, superior thermal stability, and solvent-free mixing capability, representing a green development trend in high-load dry electrode manufacturing. However, PTFE suffers from severe electrochemical instability in anode systems. At the lithiation potential of graphite, PTFE chains undergo severe reductive decomposition, generating amorphous carbon and lithium fluoride. This severe irreversible capacity loss due to binder decomposition significantly limits the application of PTFE as a dry binder in anode systems. Summary of the Invention
[0004] To address the technical problem that polytetrafluoroethylene (PTFE) is prone to reduction side reactions when used as a dry-process binder in negative electrode systems, resulting in severe irreversible capacity loss, low initial efficiency, and poor cycle life, thus hindering the development of high-load dry-process electrodes, this invention provides a method for preparing a coated dry-process battery negative electrode, the negative electrode obtained by this method, and a lithium-ion battery containing the negative electrode. This invention aims to block the electrochemical decomposition pathway of the binder in the dry-process negative electrode through interface control, thereby achieving both high capacity and long cycle life in high-load dry-process electrodes.
[0005] In a first aspect, the present invention provides a method for preparing a coated dry-process battery negative electrode sheet, characterized by comprising the following steps: S01, the polymer coating material, preferably a polyether polymer, more preferably polyethylene oxide, is dissolved in a polar solvent and stirred to obtain a first mixture; the polar solvent is preferably water, methanol or ethanol, more preferably water; S02, the first mixture is mixed with the negative electrode active material to obtain the second mixture; the negative electrode active material is preferably a carbon-based negative electrode active material, such as natural graphite, artificial graphite or mesophase carbon microspheres, and more preferably graphite; S03, the second mixture is dried and milled to obtain a coated negative electrode active material (preferably a coated graphite negative electrode), and this is used as the third mixture; S04, the third mixture is mixed with a fluoropolymer binder (preferably polytetrafluoroethylene) and a conductive agent (preferably selected from one of carbon nanotubes, conductive carbon black, graphene or an equivalent mixture thereof) and then sheared to obtain a fourth mixture; S05, the fourth mixture is rolled to obtain a dry film; S06, the dry-process membrane is combined with the current collector to obtain the coated dry-process battery negative electrode sheet.
[0006] Further, in step S01, the solid content of the first mixture is 0.5% to 2.0%.
[0007] Further, in step S02, the mass ratio of the polyethylene oxide to the graphite is (0.5~2.0):(98.0~99.5).
[0008] Furthermore, in step S03, the drying temperature is 110℃~130℃.
[0009] Further, in step S04, the mass ratio of the third mixture, the polytetrafluoroethylene, and the conductive agent is (94.0~98.0):(1.0~3.0):(1.0~3.0).
[0010] Furthermore, in step S04, the shearing operation is high-speed shearing; in step S05, the rolling operation is hot rolling.
[0011] Secondly, the present invention provides a coated dry-process battery negative electrode sheet, which is prepared by any of the above-described methods for preparing coated dry-process battery negative electrode sheets; The coated dry-process battery negative electrode includes a current collector and a dry-process film composited on the surface of the current collector; The dry-process membrane comprises a graphite anode, polytetrafluoroethylene (PTFE), and a conductive agent; wherein the graphite anode comprises graphite and a polyoxyethylene coating layer covering the surface of the graphite, and the PTFE and the graphite are electrically isolated by the polyoxyethylene coating layer.
[0012] Furthermore, in the dry-process membrane, the mass ratio of the coated graphite negative electrode, the polytetrafluoroethylene, and the conductive agent is 96:2:2.
[0013] Furthermore, the resistivity of the coated dry-process battery negative electrode is 260 Ω·cm ~ 326 Ω·cm.
[0014] Thirdly, the present invention provides a lithium-ion battery, including any of the coated dry-process battery negative electrode sheets described above.
[0015] The beneficial effects of this invention are that by introducing a polyethylene oxide (PEO) coating layer onto the surface of the negative electrode active material, the direct electrical connection between graphite particles and the polytetrafluoroethylene (PTFE) binder is cleverly interrupted. Since PEO material possesses excellent lithium-ion conductivity, electronic insulation, and superior reduction stability, it acts as an insulating interface, significantly suppressing the reduction decomposition side reactions of PTFE at low potentials (such as the graphite lithiation potential). Through the synergistic effect of the above-mentioned electrical isolation mechanism, this invention effectively alleviates the irreversible capacity loss of the negative electrode caused by binder decomposition, significantly improving the battery's initial coulombic efficiency. This allows the dry-process negative electrode to maintain high load characteristics while exhibiting high capacity and excellent long cycle life. Detailed Implementation
[0016] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to specific embodiments and comparative examples. It should be understood that the specific embodiments described herein are merely illustrative of the invention and are not intended to limit the invention.
[0017] In the following examples and comparative examples, unless otherwise specified, the raw materials and equipment used are commercially available; and unless otherwise specified, the process steps are performed according to conventional parameters in the art or according to the conditions recommended by the instrument and equipment manufacturer.
[0018] Unless otherwise stated, the terms used in this specification have the following meanings: (1) Polyethylene oxide (PEO): refers to a polyether polymer compound containing (-CH2-CH2-O-)n repeating units in the main chain; when used as a coating layer in this invention, its weight-average molecular weight can be conventionally adjusted according to the actual film strength and ion conduction requirements.
[0019] (2) Electrical isolation: refers to blocking the direct electron transfer between two or more specific materials (such as PTFE and graphite in this application) in a spatial physical structure (i.e., electronic insulation), but does not necessarily hinder the transport of ions (such as lithium ions).
[0020] (3) Solid content: refers to the percentage of the mass of the remaining part (solid substance) after drying under specified conditions to the original total mass. It is mainly used to define the dispersion concentration of the polymer in the solvent in this invention.
[0021] (4) High-speed shearing: refers to mechanical mixing methods with a rotation speed generally greater than 1000 rpm. It achieves highly uniform dispersion of powder materials and binders at the micro level by applying strong shearing force, and at the same time stimulates the fibrillation of fluoropolymer binders to form a network structure, rather than simple low-speed physical stirring.
[0022] (5) Hot rolling: refers to the rolling operation performed under heated conditions above room temperature and below the melting point of the binder, which aims to enhance the physical bonding force between dry powders and form a film through thermoplastic deformation.
[0023] Example 1
[0024] This embodiment provides a coated dry-process battery negative electrode sheet and its preparation method, which includes the following complete steps: Step S01: Weigh out the corresponding mass of polyethylene oxide with a weight average molecular weight Mw = 100,000 and dissolve it in deionized water (conductivity ≤ 1 μS / cm). At an ambient temperature of 25 ± 2℃, use a magnetic stirrer to mechanically stir the mixture at a speed of 500 rpm for 30 minutes to obtain a first mixture with a polyethylene oxide solid content of 1.25%.
[0025] In step S02, take 10g of the first mixture obtained above (containing 0.125g of polyethylene oxide), add 9.875g of artificial graphite (median particle size D50=15μm), and use a V-type mixer to continuously mix and stir at a speed of 800 rpm for 1 hour to ensure that the polyethylene oxide and graphite are in full contact, thereby obtaining the second mixture; at this time, the mass ratio of polyethylene oxide to graphite in the system is 1.25:98.75.
[0026] Step S03: Transfer the second mixture to a vacuum drying oven and dry it at 120°C for 2 hours. Set the vacuum environment to an absolute pressure of ≤-0.09MPa. After drying, use a high-energy ball mill to grind it evenly and pass it through a 300-mesh sieve to obtain a coated graphite anode with a polyoxyethylene coating on the surface, and use it as the third mixture.
[0027] Step S04: Weigh the third mixture, polytetrafluoroethylene micro powder (median particle size D50 = 5 μm), and conductive carbon black, and put them into a high-shear mixer at a mass ratio of 96.0:2.0:2.0. Perform high-speed shearing treatment at 3000 rpm for 15 minutes to promote the fibrillation of polytetrafluoroethylene and uniformly mix it with other materials to obtain the fourth mixture.
[0028] Step S05: The fourth mixture is fed into a two-roll hot press for hot rolling operation. The hot rolling temperature is set to 150°C and the rolling pressure is 20MPa. After repeated rolling 6 times, a dry film with uniform thickness and self-supporting properties is obtained.
[0029] Step S06: The dry-process film and an 8μm thick copper foil are fed into a roll forming machine and laminated under a lamination pressure of 15MPa to obtain the coated dry-process battery negative electrode sheet.
[0030] Example 2
[0031] This embodiment provides a coated dry-process battery negative electrode sheet and its preparation method, which includes the following complete steps: Step S01: Weigh out the corresponding mass of polyethylene oxide with a weight average molecular weight Mw = 100,000 and dissolve it in deionized water (conductivity ≤ 1 μS / cm). At an ambient temperature of 25 ± 2℃, use a magnetic stirrer to mechanically stir the mixture at a speed of 500 rpm for 30 minutes to obtain a first mixture with a polyethylene oxide solid content of 0.5%.
[0032] In step S02, take 10g of the first mixture obtained above (containing 0.05g of polyethylene oxide), add 9.95g of artificial graphite (median particle size D50=15μm), and use a V-type mixer to continuously mix and stir at a speed of 800 rpm for 1 hour to ensure that the polyethylene oxide and graphite are in full contact, thereby obtaining the second mixture; at this time, the mass ratio of polyethylene oxide to graphite in the system is 0.5:99.5.
[0033] Step S03: Transfer the second mixture to a vacuum drying oven and dry it at 120°C for 2 hours. Set the vacuum environment to an absolute pressure of ≤-0.09MPa. After drying, use a high-energy ball mill to grind it evenly and pass it through a 300-mesh sieve to obtain a coated graphite anode with a polyoxyethylene coating on the surface, and use it as the third mixture.
[0034] Step S04: Weigh the third mixture, polytetrafluoroethylene micro powder (median particle size D50 = 5 μm), and conductive carbon black, and put them into a high-shear mixer at a mass ratio of 96.0:2.0:2.0. Perform high-speed shearing treatment at 3000 rpm for 15 minutes to promote the fibrillation of polytetrafluoroethylene and uniformly mix it with other materials to obtain the fourth mixture.
[0035] Step S05: The fourth mixture is fed into a two-roll hot press for hot rolling operation. The hot rolling temperature is set to 150°C and the rolling pressure is 20MPa. After repeated rolling 6 times, a dry film with uniform thickness and self-supporting properties is obtained.
[0036] Step S06: The dry-process film and an 8μm thick copper foil are fed into a roll forming machine and laminated under a lamination pressure of 15MPa to obtain the coated dry-process battery negative electrode sheet.
[0037] Example 3
[0038] This embodiment provides a coated dry-process battery negative electrode sheet and its preparation method, which includes the following complete steps: Step S01: Weigh out the corresponding mass of polyethylene oxide with a weight-average molecular weight Mw = 100,000 and dissolve it in deionized water (conductivity ≤ 1 μS / cm). At an ambient temperature of 25 ± 2℃, use a magnetic stirrer to mechanically stir the mixture at a speed of 500 rpm for 30 minutes to obtain a first mixture with a polyethylene oxide solid content of 0.75%.
[0039] In step S02, take 10g of the first mixture obtained above (containing 0.075g of polyethylene oxide), add 9.925g of artificial graphite (median particle size D50=15μm), and use a V-type mixer to continuously mix and stir at a speed of 800 rpm for 1 hour to ensure that the polyethylene oxide and graphite are in full contact, thereby obtaining the second mixture; at this time, the mass ratio of polyethylene oxide to graphite in the system is 0.75:99.25.
[0040] Step S03: Transfer the second mixture to a vacuum drying oven and dry it at 120°C for 2 hours. Set the vacuum environment to an absolute pressure of ≤-0.09MPa. After drying, use a high-energy ball mill to grind it evenly and pass it through a 300-mesh sieve to obtain a coated graphite anode with a polyoxyethylene coating on the surface, and use it as the third mixture.
[0041] Step S04: Weigh the third mixture, polytetrafluoroethylene micro powder (median particle size D50 = 5 μm), and conductive carbon black, and put them into a high-shear mixer at a mass ratio of 96.0:2.0:2.0. Perform high-speed shearing treatment at 3000 rpm for 15 minutes to promote the fibrillation of polytetrafluoroethylene and uniformly mix it with other materials to obtain the fourth mixture.
[0042] Step S05: The fourth mixture is fed into a two-roll hot press for hot rolling operation. The hot rolling temperature is set to 150°C and the rolling pressure is 20MPa. After repeated rolling 6 times, a dry film with uniform thickness and self-supporting properties is obtained.
[0043] Step S06: The dry-process film and an 8μm thick copper foil are fed into a roll forming machine and laminated under a lamination pressure of 15MPa to obtain the coated dry-process battery negative electrode sheet.
[0044] Example 4
[0045] This embodiment provides a coated dry-process battery negative electrode sheet and its preparation method, which includes the following complete steps: Step S01: Weigh out the corresponding mass of polyethylene oxide with a weight average molecular weight Mw = 100,000 and dissolve it in deionized water (conductivity ≤ 1 μS / cm). At an ambient temperature of 25 ± 2℃, use a magnetic stirrer to mechanically stir the mixture at a speed of 500 rpm for 30 minutes to obtain a first mixture with a polyethylene oxide solid content of 1.0%.
[0046] In step S02, take 10g of the first mixture obtained above (containing 0.10g of polyethylene oxide), add 9.90g of artificial graphite (median particle size D50=15μm), and use a V-type mixer to continuously mix and stir at a speed of 800 rpm for 1 hour to ensure that the polyethylene oxide and graphite are in full contact, thereby obtaining the second mixture; at this time, the mass ratio of polyethylene oxide to graphite in the system is 1.0:99.0.
[0047] Step S03: Transfer the second mixture to a vacuum drying oven and dry it at 120°C for 2 hours. Set the vacuum environment to an absolute pressure of ≤-0.09MPa. After drying, use a high-energy ball mill to grind it evenly and pass it through a 300-mesh sieve to obtain a coated graphite anode with a polyoxyethylene coating on the surface, and use it as the third mixture.
[0048] Step S04: Weigh the third mixture, polytetrafluoroethylene micro powder (median particle size D50 = 5 μm), and conductive carbon black, and put them into a high-shear mixer at a mass ratio of 96.0:2.0:2.0. Perform high-speed shearing treatment at 3000 rpm for 15 minutes to promote the fibrillation of polytetrafluoroethylene and uniformly mix it with other materials to obtain the fourth mixture.
[0049] Step S05: The fourth mixture is fed into a two-roll hot press for hot rolling operation. The hot rolling temperature is set to 150°C and the rolling pressure is 20MPa. After repeated rolling 6 times, a dry film with uniform thickness and self-supporting properties is obtained.
[0050] Step S06: The dry-process film and an 8μm thick copper foil are fed into a roll forming machine and laminated under a lamination pressure of 15MPa to obtain the coated dry-process battery negative electrode sheet.
[0051] Example 5
[0052] This embodiment provides a coated dry-process battery negative electrode sheet and its preparation method, which includes the following complete steps: Step S01: Weigh out the corresponding mass of polyethylene oxide with a weight average molecular weight Mw = 100,000 and dissolve it in deionized water (conductivity ≤ 1 μS / cm). At an ambient temperature of 25 ± 2℃, use a magnetic stirrer to mechanically stir the mixture at a speed of 500 rpm for 30 minutes to obtain a first mixture with a polyethylene oxide solid content of 1.5%.
[0053] In step S02, take 10g of the first mixture obtained above (containing 0.15g of polyethylene oxide), add 9.85g of artificial graphite (median particle size D50=15μm), and use a V-type mixer to continuously mix and stir at a speed of 800 rpm for 1 hour to ensure that the polyethylene oxide and graphite are in full contact, thereby obtaining the second mixture; at this time, the mass ratio of polyethylene oxide to graphite in the system is 1.5:98.5.
[0054] Step S03: Transfer the second mixture to a vacuum drying oven and dry it at 120°C for 2 hours. Set the vacuum environment to an absolute pressure of ≤-0.09MPa. After drying, use a high-energy ball mill to grind it evenly and pass it through a 300-mesh sieve to obtain a coated graphite anode with a polyoxyethylene coating on the surface, and use it as the third mixture.
[0055] Step S04: Weigh the third mixture, polytetrafluoroethylene micro powder (median particle size D50 = 5 μm), and conductive carbon black, and put them into a high-shear mixer at a mass ratio of 96.0:2.0:2.0. Perform high-speed shearing treatment at 3000 rpm for 15 minutes to promote the fibrillation of polytetrafluoroethylene and uniformly mix it with other materials to obtain the fourth mixture.
[0056] Step S05: The fourth mixture is fed into a two-roll hot press for hot rolling operation. The hot rolling temperature is set to 150°C and the rolling pressure is 20MPa. After repeated rolling 6 times, a dry film with uniform thickness and self-supporting properties is obtained.
[0057] Step S06: The dry-process film and an 8μm thick copper foil are fed into a roll forming machine and laminated under a lamination pressure of 15MPa to obtain the coated dry-process battery negative electrode sheet.
[0058] Example 6
[0059] This embodiment provides a coated dry-process battery negative electrode sheet and its preparation method, which includes the following complete steps: Step S01: Weigh out the corresponding mass of polyethylene oxide with a weight-average molecular weight Mw = 100,000 and dissolve it in deionized water (conductivity ≤ 1 μS / cm). At an ambient temperature of 25 ± 2℃, use a magnetic stirrer to mechanically stir the mixture at a speed of 500 rpm for 30 minutes to obtain a first mixture with a polyethylene oxide solid content of 1.75%.
[0060] In step S02, take 10g of the first mixture obtained above (containing 0.175g of polyethylene oxide), add 9.825g of artificial graphite (median particle size D50=15μm), and use a V-type mixer to continuously mix and stir at a speed of 800 rpm for 1 hour to ensure that the polyethylene oxide and graphite are in full contact, thereby obtaining the second mixture; at this time, the mass ratio of polyethylene oxide to graphite in the system is 1.75:98.25.
[0061] Step S03: Transfer the second mixture to a vacuum drying oven and dry it at 120°C for 2 hours. Set the vacuum environment to an absolute pressure of ≤-0.09MPa. After drying, use a high-energy ball mill to grind it evenly and pass it through a 300-mesh sieve to obtain a coated graphite anode with a polyoxyethylene coating on the surface, and use it as the third mixture.
[0062] Step S04: Weigh the third mixture, polytetrafluoroethylene micro powder (median particle size D50 = 5 μm), and conductive carbon black, and put them into a high-shear mixer at a mass ratio of 96.0:2.0:2.0. Perform high-speed shearing treatment at 3000 rpm for 15 minutes to promote the fibrillation of polytetrafluoroethylene and uniformly mix it with other materials to obtain the fourth mixture.
[0063] Step S05: The fourth mixture is fed into a two-roll hot press for hot rolling operation. The hot rolling temperature is set to 150°C and the rolling pressure is 20MPa. After repeated rolling 6 times, a dry film with uniform thickness and self-supporting properties is obtained.
[0064] Step S06: The dry-process film and an 8μm thick copper foil are fed into a roll forming machine and laminated under a lamination pressure of 15MPa to obtain the coated dry-process battery negative electrode sheet.
[0065] Example 7
[0066] This embodiment provides a coated dry-process battery negative electrode sheet and its preparation method, which includes the following complete steps: Step S01: Weigh out the corresponding mass of polyethylene oxide with a weight average molecular weight Mw = 100,000 and dissolve it in deionized water (conductivity ≤ 1 μS / cm). At an ambient temperature of 25 ± 2℃, use a magnetic stirrer to mechanically stir the mixture at a speed of 500 rpm for 30 minutes to obtain a first mixture with a polyethylene oxide solid content of 2.0%.
[0067] In step S02, take 10g of the first mixture obtained above (containing 0.20g of polyethylene oxide), add 9.80g of artificial graphite (median particle size D50=15μm), and use a V-type mixer to continuously mix and stir at a speed of 800 rpm for 1 hour to ensure that the polyethylene oxide and graphite are in full contact, thereby obtaining the second mixture; at this time, the mass ratio of polyethylene oxide to graphite in the system is 2.0:98.0.
[0068] Step S03: Transfer the second mixture to a vacuum drying oven and dry it at 120°C for 2 hours. Set the vacuum environment to an absolute pressure of ≤-0.09MPa. After drying, use a high-energy ball mill to grind it evenly and pass it through a 300-mesh sieve to obtain a coated graphite anode with a polyoxyethylene coating on the surface, and use it as the third mixture.
[0069] Step S04: Weigh the third mixture, polytetrafluoroethylene micro powder (median particle size D50 = 5 μm), and conductive carbon black, and put them into a high-shear mixer at a mass ratio of 96.0:2.0:2.0. Perform high-speed shearing treatment at 3000 rpm for 15 minutes to promote the fibrillation of polytetrafluoroethylene and uniformly mix it with other materials to obtain the fourth mixture.
[0070] Step S05: The fourth mixture is fed into a two-roll hot press for hot rolling operation. The hot rolling temperature is set to 150°C and the rolling pressure is 20MPa. After repeated rolling 6 times, a dry film with uniform thickness and self-supporting properties is obtained.
[0071] Step S06: The dry-process film and an 8μm thick copper foil are fed into a roll forming machine and laminated under a lamination pressure of 15MPa to obtain the coated dry-process battery negative electrode sheet.
[0072] Example 8
[0073] This embodiment provides a coated dry-process battery negative electrode sheet and its preparation method, which includes the following complete steps: Step S01: Weigh out the corresponding mass of polyethylene oxide with a weight average molecular weight Mw = 100,000 and dissolve it in deionized water (conductivity ≤ 1 μS / cm). At an ambient temperature of 25 ± 2℃, use a magnetic stirrer to mechanically stir the mixture at a speed of 500 rpm for 30 minutes to obtain a first mixture with a polyethylene oxide solid content of 1.25%.
[0074] In step S02, take 10g of the first mixture obtained above (containing 0.125g of polyethylene oxide), add 9.875g of artificial graphite (median particle size D50=15μm), and use a V-type mixer to continuously mix and stir at a speed of 800 rpm for 1 hour to ensure that the polyethylene oxide and graphite are in full contact, thereby obtaining the second mixture; at this time, the mass ratio of polyethylene oxide to graphite in the system is 1.25:98.75.
[0075] Step S03: Transfer the second mixture to a vacuum drying oven and dry it at 110°C for 2 hours. Set the vacuum environment to an absolute pressure of ≤-0.09MPa. After drying, use a high-energy ball mill to grind it evenly and pass it through a 300-mesh sieve to obtain a coated graphite anode with a polyoxyethylene coating on the surface, and use it as the third mixture.
[0076] Step S04: Weigh the third mixture, polytetrafluoroethylene micro powder (median particle size D50 = 5 μm), and conductive carbon black, and put them into a high-shear mixer at a mass ratio of 96.0:2.0:2.0. Perform high-speed shearing treatment at 3000 rpm for 15 minutes to promote the fibrillation of polytetrafluoroethylene and uniformly mix it with other materials to obtain the fourth mixture.
[0077] Step S05: The fourth mixture is fed into a two-roll hot press for hot rolling operation. The hot rolling temperature is set to 150°C and the rolling pressure is 20MPa. After repeated rolling 6 times, a dry film with uniform thickness and self-supporting properties is obtained.
[0078] Step S06: The dry-process film and an 8μm thick copper foil are fed into a roll forming machine and laminated under a lamination pressure of 15MPa to obtain the coated dry-process battery negative electrode sheet.
[0079] Example 9
[0080] This embodiment provides a coated dry-process battery negative electrode sheet and its preparation method, which includes the following complete steps: Step S01: Weigh out the corresponding mass of polyethylene oxide with a weight average molecular weight Mw = 100,000 and dissolve it in deionized water (conductivity ≤ 1 μS / cm). At an ambient temperature of 25 ± 2℃, use a magnetic stirrer to mechanically stir the mixture at a speed of 500 rpm for 30 minutes to obtain a first mixture with a polyethylene oxide solid content of 1.25%.
[0081] In step S02, take 10g of the first mixture obtained above (containing 0.125g of polyethylene oxide), add 9.875g of artificial graphite (median particle size D50=15μm), and use a V-type mixer to continuously mix and stir at a speed of 800 rpm for 1 hour to ensure that the polyethylene oxide and graphite are in full contact, thereby obtaining the second mixture; at this time, the mass ratio of polyethylene oxide to graphite in the system is 1.25:98.75.
[0082] Step S03: Transfer the second mixture to a vacuum drying oven and dry it at 130°C for 2 hours. Set the vacuum environment to an absolute pressure of ≤-0.09MPa. After drying, use a high-energy ball mill to grind it evenly and pass it through a 300-mesh sieve to obtain a coated graphite anode with a polyoxyethylene coating on the surface, and use it as the third mixture.
[0083] Step S04: Weigh the third mixture, polytetrafluoroethylene micro powder (median particle size D50 = 5 μm), and conductive carbon black, and put them into a high-shear mixer at a mass ratio of 96.0:2.0:2.0. Perform high-speed shearing treatment at 3000 rpm for 15 minutes to promote the fibrillation of polytetrafluoroethylene and uniformly mix it with other materials to obtain the fourth mixture.
[0084] Step S05: The fourth mixture is fed into a two-roll hot press for hot rolling operation. The hot rolling temperature is set to 150°C and the rolling pressure is 20MPa. After repeated rolling 6 times, a dry film with uniform thickness and self-supporting properties is obtained.
[0085] Step S06: The dry-process film and an 8μm thick copper foil are fed into a roll forming machine and laminated under a lamination pressure of 15MPa to obtain the coated dry-process battery negative electrode sheet.
[0086] Example 10
[0087] This embodiment provides a coated dry-process battery negative electrode sheet and its preparation method, which includes the following complete steps: Step S01: Weigh out the corresponding mass of polyethylene oxide with a weight average molecular weight Mw = 100,000 and dissolve it in deionized water (conductivity ≤ 1 μS / cm). At an ambient temperature of 25 ± 2℃, use a magnetic stirrer to mechanically stir the mixture at a speed of 500 rpm for 30 minutes to obtain a first mixture with a polyethylene oxide solid content of 1.25%.
[0088] In step S02, take 10g of the first mixture obtained above (containing 0.125g of polyethylene oxide), add 9.875g of artificial graphite (median particle size D50=15μm), and use a V-type mixer to continuously mix and stir at a speed of 800 rpm for 1 hour to ensure that the polyethylene oxide and graphite are in full contact, thereby obtaining the second mixture; at this time, the mass ratio of polyethylene oxide to graphite in the system is 1.25:98.75.
[0089] Step S03: Transfer the second mixture to a vacuum drying oven and dry it at 120°C for 2 hours. Set the vacuum environment to an absolute pressure of ≤-0.09MPa. After drying, use a high-energy ball mill to grind it evenly and pass it through a 300-mesh sieve to obtain a coated graphite anode with a polyoxyethylene coating on the surface, and use it as the third mixture.
[0090] Step S04: Weigh the third mixture, polytetrafluoroethylene micro powder (median particle size D50 = 5 μm), and conductive carbon black, and put them into a high-shear mixer in a mass ratio of 94.0:3.0:3.0. Perform high-speed shearing treatment at 3000 rpm for 15 minutes to promote the fibrillation of polytetrafluoroethylene and uniformly mix it with other materials to obtain the fourth mixture.
[0091] Step S05: The fourth mixture is fed into a two-roll hot press for hot rolling operation. The hot rolling temperature is set to 150°C and the rolling pressure is 20MPa. After repeated rolling 6 times, a dry film with uniform thickness and self-supporting properties is obtained.
[0092] Step S06: The dry-process film and an 8μm thick copper foil are fed into a roll forming machine and laminated under a lamination pressure of 15MPa to obtain the coated dry-process battery negative electrode sheet.
[0093] Example 11
[0094] This embodiment provides a coated dry-process battery negative electrode sheet and its preparation method, which includes the following complete steps: Step S01: Weigh out the corresponding mass of polyethylene oxide with a weight average molecular weight Mw = 100,000 and dissolve it in deionized water (conductivity ≤ 1 μS / cm). At an ambient temperature of 25 ± 2℃, use a magnetic stirrer to mechanically stir the mixture at a speed of 500 rpm for 30 minutes to obtain a first mixture with a polyethylene oxide solid content of 1.25%.
[0095] In step S02, take 10g of the first mixture obtained above (containing 0.125g of polyethylene oxide), add 9.875g of artificial graphite (median particle size D50=15μm), and use a V-type mixer to continuously mix and stir at a speed of 800 rpm for 1 hour to ensure that the polyethylene oxide and graphite are in full contact, thereby obtaining the second mixture; at this time, the mass ratio of polyethylene oxide to graphite in the system is 1.25:98.75.
[0096] Step S03: Transfer the second mixture to a vacuum drying oven and dry it at 120°C for 2 hours. Set the vacuum environment to an absolute pressure of ≤-0.09MPa. After drying, use a high-energy ball mill to grind it evenly and pass it through a 300-mesh sieve to obtain a coated graphite anode with a polyoxyethylene coating on the surface, and use it as the third mixture.
[0097] Step S04: Weigh the third mixture, polytetrafluoroethylene micro powder (median particle size D50 = 5 μm), and conductive carbon black, and put them into a high-shear mixer at a mass ratio of 98.0:1.0:1.0. Perform high-speed shearing treatment at 3000 rpm for 15 minutes to promote the fibrillation of polytetrafluoroethylene and uniformly mix it with other materials to obtain the fourth mixture.
[0098] Step S05: The fourth mixture is fed into a two-roll hot press for hot rolling operation. The hot rolling temperature is set to 150°C and the rolling pressure is 20MPa. After repeated rolling 6 times, a dry film with uniform thickness and self-supporting properties is obtained.
[0099] Step S06: The dry-process film and an 8μm thick copper foil are fed into a roll forming machine and laminated under a lamination pressure of 15MPa to obtain the coated dry-process battery negative electrode sheet.
[0100] Example 12
[0101] This embodiment provides a coated dry-process battery negative electrode sheet and its preparation method, which includes the following complete steps: Step S01: Weigh out the corresponding mass of polyethylene oxide with a weight average molecular weight Mw = 100,000 and dissolve it in deionized water (conductivity ≤ 1 μS / cm). At an ambient temperature of 25 ± 2℃, use a magnetic stirrer to mechanically stir the mixture at a speed of 500 rpm for 30 minutes to obtain a first mixture with a polyethylene oxide solid content of 1.25%.
[0102] In step S02, take 10g of the first mixture obtained above (containing 0.125g of polyethylene oxide), add 9.875g of artificial graphite (median particle size D50=15μm), and use a V-type mixer to continuously mix and stir at a speed of 800 rpm for 1 hour to ensure that the polyethylene oxide and graphite are in full contact, thereby obtaining the second mixture; at this time, the mass ratio of polyethylene oxide to graphite in the system is 1.25:98.75.
[0103] Step S03: Transfer the second mixture to a vacuum drying oven and dry it at 120°C for 2 hours. Set the vacuum environment to an absolute pressure of ≤-0.09MPa. After drying, use a high-energy ball mill to grind it evenly and pass it through a 300-mesh sieve to obtain a coated graphite anode with a polyoxyethylene coating on the surface, and use it as the third mixture.
[0104] Step S04: Weigh the third mixture, polytetrafluoroethylene micro powder (median particle size D50 = 5 μm), and conductive carbon black, and put them into a high-shear mixer at a mass ratio of 95.0:2.5:2.5. Perform high-speed shearing treatment at 3000 rpm for 15 minutes to promote the fibrillation of polytetrafluoroethylene and uniformly mix it with other materials to obtain the fourth mixture.
[0105] Step S05: The fourth mixture is fed into a two-roll hot press for hot rolling operation. The hot rolling temperature is set to 150°C and the rolling pressure is 20MPa. After repeated rolling 6 times, a dry film with uniform thickness and self-supporting properties is obtained.
[0106] Step S06: The dry-process film and an 8μm thick copper foil are fed into a roll forming machine and laminated under a lamination pressure of 15MPa to obtain the coated dry-process battery negative electrode sheet.
[0107] Example 13
[0108] This embodiment provides a coated dry-process battery negative electrode sheet and its preparation method, which includes the following complete steps: Step S01: Weigh out the corresponding mass of polyethylene oxide with a weight average molecular weight Mw = 100,000 and dissolve it in deionized water (conductivity ≤ 1 μS / cm). At an ambient temperature of 25 ± 2℃, use a magnetic stirrer to mechanically stir the mixture at a speed of 500 rpm for 30 minutes to obtain a first mixture with a polyethylene oxide solid content of 1.25%.
[0109] In step S02, take 10g of the first mixture obtained above (containing 0.125g of polyethylene oxide), add 9.875g of artificial graphite (median particle size D50=15μm), and use a V-type mixer to continuously mix and stir at a speed of 800 rpm for 1 hour to ensure that the polyethylene oxide and graphite are in full contact, thereby obtaining the second mixture; at this time, the mass ratio of polyethylene oxide to graphite in the system is 1.25:98.75.
[0110] Step S03: Transfer the second mixture to a vacuum drying oven and dry it at 120°C for 2 hours. Set the vacuum environment to an absolute pressure of ≤-0.09MPa. After drying, use a high-energy ball mill to grind it evenly and pass it through a 300-mesh sieve to obtain a coated graphite anode with a polyoxyethylene coating on the surface, and use it as the third mixture.
[0111] Step S04: Weigh the third mixture, polytetrafluoroethylene micro powder (median particle size D50 = 5 μm), and conductive carbon black, and put them into a high-shear mixer at a mass ratio of 97.0:1.5:1.5. Perform high-speed shearing treatment at 3000 rpm for 15 minutes to promote the fibrillation of polytetrafluoroethylene and uniformly mix it with other materials to obtain the fourth mixture.
[0112] Step S05: The fourth mixture is fed into a two-roll hot press for hot rolling operation. The hot rolling temperature is set to 150°C and the rolling pressure is 20MPa. After repeated rolling 6 times, a dry film with uniform thickness and self-supporting properties is obtained.
[0113] Step S06: The dry-process film and an 8μm thick copper foil are fed into a roll forming machine and laminated under a lamination pressure of 15MPa to obtain the coated dry-process battery negative electrode sheet.
[0114] Based on the above embodiments, the following comparative examples are set. Comparative Example 1 The preparation method of Comparative Example 1 is basically the same as that of Example 1, except that steps S01 to S03 are omitted, and unprocessed artificial graphite (median particle size D50=15μm), polytetrafluoroethylene micro powder (median particle size D50=5μm) and conductive carbon black are directly mixed in a ratio of 96.0:2.0:2.0, and this mixture is directly used as the fourth mixture in step S04.
[0115] Comparative Example 2 The preparation method of Comparative Example 2 is basically the same as that of Example 1, except that the solid content of polyethylene oxide in step S01 is modified to 0.1%, and the mass ratio of polyethylene oxide to graphite in the system in step S02 is modified to 0.1:99.9 (that is, 10g of the first mixture with a solid content of 0.1% is added to 9.99g of artificial graphite).
[0116] Comparative Example 3 The preparation method of Comparative Example 3 is basically the same as that of Example 1, except that the solid content of polyethylene oxide in step S01 is modified to 3.0%, and the mass ratio of polyethylene oxide to graphite in the system in step S02 is modified to 3.0:97.0 (that is, 10g of the first mixture with a solid content of 3.0% is added to 9.70g of artificial graphite).
[0117] Comparative Example 4 The preparation method of Comparative Example 4 is basically the same as that of Example 1, except that the drying temperature of the vacuum drying oven in step S03 is changed to 80°C.
[0118] Comparative Example 5 The preparation method of Comparative Example 5 is basically the same as that of Example 1, except that the polytetrafluoroethylene micro powder (median particle size D50=5μm) in step S04 is replaced with polyvinylidene fluoride (PVDF) powder.
[0119] Coating uniformity test: The cross-section of the electrode and the surface morphology of the particles were observed using a Hitachi SU8010 scanning electron microscope (SEM) to evaluate the continuity of the polymer layer.
[0120] Electrode resistivity test: The four-probe method was used to measure the electrode resistivity using an ST2253 four-probe resistance tester in accordance with standard GB / T1551-2009.
[0121] Initial Coulombic Efficiency and Cycle Life Tests: The prepared negative electrode sheet was stamped into a disc, and a lithium metal sheet was used as the counter electrode. The discs were then assembled into CR2032 coin cells in an argon-filled glove box. The electrolyte was a 1.0 mol / L LiPF6 EC / DEC (volume ratio 1:1) mixture. The initial coulombic efficiency was obtained using a Xinwei CT-4008 battery testing system, with charge-discharge tests conducted at a 0.1C rate.
[0122] The results of the above tests are shown in Table 1 below.
[0123] Table 1. Physical Performance Test Table for Dry Electrode Sheets
[0124] As shown in Table 1, Examples 1-13 using the "polyethylene oxide coating process" provided in this application exhibited significantly higher initial coulombic efficiencies than the uncoated Comparative Example 1. This strongly demonstrates that by controlling the polyethylene oxide solid content between 0.5% and 2.0% and performing drying coating at 110°C to 130°C, a protective layer that balances "electronic insulation" and "ionic conduction" can be formed on the graphite surface. This coating layer physically blocks direct electron transport between graphite and the polytetrafluoroethylene binder at a microscopic level, successfully suppressing the reduction decomposition side reaction of polytetrafluoroethylene at low potentials, thereby significantly reducing irreversible capacity loss and significantly extending the cycle life of the battery while maintaining the high load characteristics of the dry process.
[0125] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make some modifications or alterations to the above-disclosed technical content to create equivalent embodiments without departing from the scope of the present invention. Any simple modifications, equivalent changes, and alterations made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the scope of the present invention.
Claims
1. A method for preparing a coated dry-process battery negative electrode, characterized in that, Includes the following steps: S01, dissolve polyethylene oxide in a solvent and stir to obtain a first mixture; S02, the first mixture is mixed with graphite to obtain a second mixture; S03, the second mixture is dried and ground to obtain a coated graphite anode, which is then used as the third mixture; S04, the third mixture is mixed with polytetrafluoroethylene and a conductive agent and then sheared to obtain a fourth mixture; S05, the fourth mixture is rolled to obtain a dry film; S06, the dry-process membrane is combined with the current collector to obtain the coated dry-process battery negative electrode sheet.
2. The method for preparing the coated dry-process battery negative electrode sheet according to claim 1, characterized in that, In step S01, the solvent is water; the solid content of the first mixture is 0.5% to 2.0%.
3. The method for preparing the coated dry-process battery negative electrode sheet according to claim 1, characterized in that, In step S02, the mass ratio of the polyethylene oxide to the graphite is (0.5~2.0):(98.0~99.5).
4. The method for preparing the coated dry-process battery negative electrode sheet according to claim 1, characterized in that, In step S03, the drying temperature is 110℃~130℃.
5. The method for preparing the coated dry-process battery negative electrode sheet according to claim 1, characterized in that, In step S04, the mass ratio of the third mixture, the polytetrafluoroethylene and the conductive agent is (94.0~98.0):(1.0~3.0):(1.0~3.0).
6. The method for preparing the coated dry-process battery negative electrode sheet according to claim 1, characterized in that, In step S04, the shearing operation is high-speed shearing; in step S05, the rolling operation is hot rolling.
7. A coated dry-process battery negative electrode sheet, characterized in that, It is prepared by the method for preparing the coated dry-process battery negative electrode sheet as described in any one of claims 1 to 6; The coated dry-process battery negative electrode includes a current collector and a dry-process film composited on the surface of the current collector; The dry-process membrane comprises a graphite anode, polytetrafluoroethylene (PTFE), and a conductive agent; wherein the graphite anode comprises graphite and a polyoxyethylene coating layer covering the surface of the graphite, and the PTFE and the graphite are electrically isolated by the polyoxyethylene coating layer.
8. The coated dry-process battery negative electrode sheet according to claim 7, characterized in that, In the dry-process membrane, the mass ratio of the coated graphite anode, the polytetrafluoroethylene, and the conductive agent is 96:2:
2.
9. The coated dry-process battery negative electrode sheet according to claim 7, characterized in that, The resistivity of the coated dry cell negative electrode is 260 Ω·cm to 326 Ω·cm.
10. A lithium-ion battery, characterized in that, Includes the coated dry-process battery negative electrode sheet as described in any one of claims 7 to 9.