A method for preparing an NFPP polyanion sodium-ion battery negative electrode slurry

By optimizing the ratio of hard carbon, SP, SBR, and CMC and using deionized water, a high-performance sodium-ion battery anode slurry was prepared, solving the performance problems of sodium-ion batteries under high-rate charge-discharge and low-temperature environments, and realizing the preparation of sodium-ion battery anode slurry at low cost and large scale.

CN123162145APending Publication Date: 2026-11-24四川星空钠电电池有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611427482.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-15
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing sodium-ion batteries suffer from performance degradation at high-rate charge and discharge rates and in low-temperature environments, as well as insufficient safety performance and high manufacturing costs, making it difficult to meet the needs of large-scale energy storage and low-speed electric vehicles.

Method used

By using hard carbon as the active material, SP as the conductive agent, SBR as the binder, and CMC as the thickener, and by optimizing the proportions and synergistic effects of each component, a sodium-ion battery anode slurry with excellent electrochemical and processing properties was prepared. Deionized water was used as the solvent to simplify the preparation process.

Benefits of technology

It improves the initial coulombic efficiency and reversible capacity of sodium-ion batteries, enhances the conductivity and rate performance of the negative electrode, optimizes the dispersion uniformity and rheological properties of the slurry, strengthens the peel strength and cycle stability of the electrode, and reduces production costs, making it suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123162145A_ABST
    Figure CN123162145A_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing NFPP polyanionic sodium-ion battery negative electrode slurry, belonging to the field of sodium-ion battery manufacturing. The method includes: dissolving CMC with a portion of deionized water to obtain a CMC solution; adding SP and hard carbon to the CMC solution and stirring until homogeneous; adding SBR and the remaining deionized water and continuing stirring; and coating the slurry onto the surface of a current collector after vacuum degassing, followed by drying and rolling to obtain the final product. This invention, through the synergistic compounding of hard carbon, SP, SBR, and CMC, gives the negative electrode slurry excellent flowability, dispersion stability, and coating performance, with a viscosity reaching 4865 mPa·s and a fineness of 10 μm. The resulting battery cell capacity closely matches the design value, with a 0.5C capacity test temperature difference of only 3.3℃, ​​and good electrochemical reaction uniformity, making it suitable for large-scale energy storage, low-speed electric vehicles, and other sodium-ion battery applications.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of sodium-ion battery manufacturing, and specifically to a method for preparing NFPP polyanion sodium-ion battery anode slurry. Background Technology

[0002] With the global energy structure shifting towards cleaner and lower-carbon energy, new energy storage technologies and electric vehicles have developed rapidly, creating an increasingly urgent demand for high-performance, low-cost, and highly safe sodium-ion batteries. Lithium-ion batteries, with their high energy density and long cycle life, have been widely used in various fields. However, the limited and uneven distribution of lithium resources, coupled with significant price fluctuations, severely restricts their further promotion in cost-sensitive areas such as large-scale energy storage and low-speed electric vehicles. Sodium-ion batteries, on the other hand, benefit from abundant sodium resources (sodium's abundance in the Earth's crust is approximately 2.36%, far exceeding lithium's 0.0065%) and widespread and even global distribution, free from geopolitical constraints imposed by specific countries and regions. This means that the supply of raw materials for sodium-ion batteries is intrinsically secure. Furthermore, they share similar working principles and electrochemical characteristics with lithium-ion batteries, while exhibiting unique advantages in low-temperature performance, rate performance, and cost control. Therefore, sodium-ion batteries are considered a highly promising alternative energy storage technology for large-scale energy storage, low-speed electric vehicles, and portable electronic devices, and have become a research hotspot in the new energy field in recent years.

[0003] Specifically, existing lithium-ion batteries have the following main shortcomings: Under high-rate charge / discharge, low-temperature, or high-temperature extreme conditions, the charge / discharge efficiency of lithium batteries drops significantly, severely impacting performance, and their safety performance is lower than that of sodium-ion batteries. Sodium-ion batteries, on the other hand, exhibit excellent performance in low-temperature environments, maintaining over 90% of their room-temperature capacity at -20°C, with some systems still maintaining considerable charge / discharge capacity even at extreme temperatures of -40°C. In contrast, lithium batteries typically retain only 60%–70% of their capacity at the same low temperatures and pose a serious safety hazard related to lithium plating.

[0004] Therefore, this patent aims to provide a safe, reliable, high-performance, and low-cost anode formulation design for sodium-ion batteries. It seeks to comprehensively address the performance shortcomings of existing sodium-ion battery anode materials through innovative material formulation design, fully leveraging the resource, cost, and safety advantages of sodium-ion batteries. Based on this, the present invention provides a method for preparing NFPP polyanionic sodium-ion battery anode slurry. Summary of the Invention

[0005] The purpose of this invention is to overcome the above-mentioned defects of the prior art and provide an NFPP polyanionic sodium-ion battery negative electrode slurry and its preparation method, so as to improve the initial coulombic efficiency and reversible capacity of sodium-ion batteries; improve the conductivity and rate performance of the negative electrode sheet; optimize the dispersion uniformity and rheological properties of the slurry, improve the coating quality and electrode sheet consistency; enhance the peel strength and cycle stability of the electrode sheet; simplify the preparation process, reduce production costs, and be suitable for large-scale industrial production.

[0006] This invention uses hard carbon as the active material, SP as the conductive agent, SBR and CMC as the binder system, and deionized water as the solvent. By optimizing the ratio and synergistic effect between the components, a sodium-ion battery negative electrode slurry with excellent electrochemical and processing performance is prepared, achieving excellent technical results. Hard carbon, as the negative electrode active material of sodium-ion batteries, has a disordered layered structure with a large interlayer spacing (>0.37nm), which is conducive to the insertion and extraction of sodium ions, providing high reversible capacity and good cycle stability. SP (superconducting carbon black), as a conductive agent, has a high specific surface area and a good conductive network structure, which can form an effective electron transport channel between active material particles, reduce electrode polarization, and improve rate performance. SBR (styrene-butadiene rubber latex), as a binder, has excellent elasticity and bonding strength, which can firmly bond the active material and conductive agent to the current collector surface. At the same time, its flexibility can effectively buffer the stress generated by the change in electrode volume during charging and discharging. CMC (sodium carboxymethyl cellulose), as a thickener and dispersant, can adjust the slurry viscosity, improve the rheological properties and stability of the slurry, prevent the active material from settling, and ensure coating uniformity. Deionized water, as a solvent, is environmentally friendly and pollution-free, and has good compatibility with SBR and CMC, which facilitates the preparation and coating of the slurry. This invention achieves excellent levels in key process parameters such as fluidity, viscosity, fineness, and solid content of the negative electrode slurry through the rational combination and synergistic effect of each component, and endows the battery cell with excellent capacity performance and temperature uniformity.

[0007] Based on the above findings, the present invention provides the following technical solution: This invention provides a method for preparing an NFPP polyanionic sodium-ion battery negative electrode slurry, comprising the following raw materials by weight (based on dry powder): 93-96.5 parts hard carbon, 1-2 parts SP, 2-3 parts SBR, and 0.8-1.5 parts CMC. Deionized water is weighed, and the total amount of deionized water added is controlled to ensure that the solid content of the final negative electrode slurry is 45%-50%. The preparation method includes the following steps: S1. Weigh out the hard carbon, SP, SBR, CMC and deionized water according to the weight ratio; S2. Mix CMC with some deionized water and stir until completely dissolved to obtain CMC adhesive solution; S3. Add SP to the CMC adhesive solution, stir evenly, then add hard carbon and continue stirring to obtain a mixed slurry; S4. Add SBR and remaining deionized water to the mixed slurry, stir evenly, and obtain sodium-ion battery negative electrode slurry. S5. After vacuum degassing, the negative electrode slurry is coated onto the surface of the current collector, dried, and rolled to obtain the negative electrode sheet.

[0008] In some embodiments of the present invention, the hard carbon has a D50 particle size of 3-8 μm and a specific surface area of ​​3-8 m². 2 / g, with an interlayer spacing d002 of 0.37-0.40nm.

[0009] In some embodiments of the present invention, the carbonization temperature of the hard carbon is 1000-1400°C, and the carbonization time is 2-6 hours.

[0010] In some embodiments of the present invention, the specific surface area of ​​the SP is 60-80 m². 2 / g, DBP absorption value is 150-200ml / 100g.

[0011] In some embodiments of the present invention, the SBR has a glass transition temperature of -5°C to -15°C, based on its effective solids content.

[0012] In some embodiments of the present invention, the degree of substitution of the CMC is 0.7-1.0, and the viscosity of the 2% aqueous solution is 2000-5000 mPa·s.

[0013] In some embodiments of the present invention, the stirring speed in step S2 is 800-1500 rpm and the stirring time is 60-120 minutes.

[0014] In some embodiments of the present invention, the stirring speed in step S3 is 1000-2000 rpm and the stirring time is 120-180 minutes.

[0015] In some embodiments of the present invention, the stirring speed in step S4 is 500-1000 rpm and the stirring time is 30-60 minutes.

[0016] In some embodiments of the present invention, the vacuum degree of the vacuum degassing process in step S5 is -0.08MPa to -0.10MPa, and the degassing time is 10-30 minutes.

[0017] The beneficial effects of this invention are as follows: First, this invention achieves optimal synergistic effects among active materials, conductive agents, and binders by optimizing the ratio of hard carbon, SP, SBR, and CMC. Hard carbon, as the active material, provides sodium-ion storage capacity; SP constructs an efficient electron conduction network; SBR provides excellent binding properties and flexibility; and CMC regulates the rheological properties of the slurry and assists in dispersion. The synergistic effect of these four components enables the negative electrode sheet to simultaneously possess high active material loading, good electronic conductivity and ion transport channels, excellent structural stability, and processing performance, thereby significantly improving the initial coulombic efficiency, reversible capacity, and cycle stability of sodium-ion batteries.

[0018] Secondly, this invention significantly improves the coating performance of the slurry by precisely controlling key process parameters such as solid content, viscosity, and fineness. The slurry viscosity is controlled within the range of 4000-6000 mPa·s, exhibiting good fluidity and leveling properties, minimizing defects such as scratches, bubbles, and uneven thickness during coating. A fineness of ≤15 μm ensures sufficient dispersion of all components, avoiding the adverse effects of large particle agglomerates on coating quality and electrochemical performance. A solid content of 45%-50% ensures coating efficiency and electrode density while avoiding the stability degradation caused by excessively high solid content. Field verification showed that the negative electrode slurry prepared according to the formula of this invention exhibits good fluidity, with a viscosity of 4865 mPa·s measured by a viscometer, a fineness of 10 μm, and a solid content of 47%, all of which meet the qualified standards.

[0019] Third, the negative electrode slurry prepared in this invention exhibits excellent electrochemical performance when applied to sodium-ion battery cells. After a capacity testing process involving constant current and constant voltage charging to 3.6V at 0.5C and constant current discharging to 1.5V at 0.5C, the battery capacity closely matches the design value, indicating that the formulation of this invention has good capacity designability and batch consistency. Simultaneously, the temperature curve during the capacity testing process shows that the cell temperature difference at 0.5C at room temperature is only 3.3℃, ​​indicating good uniformity of the electrochemical reaction inside the electrode, uniform current density distribution, and no obvious local overheating phenomenon, further verifying the superiority of the slurry formulation of this invention in terms of conductivity and mass transfer uniformity.

[0020] Fourth, this invention uses deionized water as a solvent, avoiding the use of organic solvents, and has significant advantages in terms of environmental friendliness, safety, and low cost. Compared with organic solvent systems, the aqueous slurry preparation process does not require expensive solvent recovery equipment, is environmentally friendly, has high operational safety, and deionized water is widely available and inexpensive, which can significantly reduce battery manufacturing costs. Furthermore, SBR and CMC are both commonly used binders in aqueous systems and have good compatibility with deionized water. The slurry preparation process is simple and controllable, making it suitable for large-scale industrial production.

[0021] Fifth, the preparation process of this invention is simple, the operating conditions are mild, and it does not require complex equipment or stringent process parameter control. The steps of preparing the CMC adhesive, dispersing SP and hard carbon, and adding SBR are all conventional stirring operations. Vacuum degassing treatment effectively removes air bubbles from the slurry, ensuring coating quality. The entire preparation process can be completed at room temperature, with low energy consumption and a short cycle time, which helps to reduce production costs and improve production efficiency.

[0022] Sixth, the formulation of this invention contains a high proportion of hard carbon (93%-96.5%), ensuring that the electrode has a high active material loading and volumetric energy density. Simultaneously, an appropriate amount of SP (1%-2%) constructs a highly efficient conductive network, ensuring electron conductivity while avoiding the dilution effect of excessive conductive agents on energy density. The amounts of SBR (2%-3%) and CMC (0.8%-1.5%) are precisely optimized, ensuring sufficient bonding strength and slurry stability while avoiding the adverse effects of excessive binders on electrode ion conduction and rate performance. The precise matching of the amounts of each component achieves an optimal balance in the overall performance of the electrode. Attached Figure Description

[0023] Figure 1 A photograph of the NFPP polyanion sodium-ion battery negative electrode slurry prepared according to an embodiment of the present invention; Figure 2 The 0.5C capacity test curve of the sodium-ion battery cell prepared in the embodiment of the present invention; Figure 3 The diagram shows the capacity testing temperature curve of the sodium-ion battery cell prepared according to an embodiment of the present invention. Detailed Implementation

[0024] The present invention will be further described in detail below with reference to embodiments and comparative examples. Where specific experimental steps or conditions are not specified in the embodiments, they can be performed according to the conventional experimental steps or conditions described in the literature in this field. Reagents or instruments used, unless otherwise specified, are all commercially available conventional reagent products.

[0025] Hard carbon (D50 particle size 5μm, specific surface area 5m²) 2 / g, interlayer spacing d002=0.38nm), purchased from Kuraray Corporation, Japan; SP (superconducting carbon black, specific surface area 68m²) 2 / g, DBP absorption value 180ml / 100g), brand name Super P TM -Li, purchased from the Swiss company Temico; SBR (styrene-butadiene rubber latex, solid content 48%, glass transition temperature -10℃), purchased from Zeon Corporation, Japan; CMC (sodium carboxymethyl cellulose, degree of substitution 0.85, viscosity of 2% aqueous solution 3500 mPa·s), purchased from Ashland Corporation, USA.

[0026] The cell assembly method of this invention involves the following steps: The prepared negative electrode sheet is cut into φ14mm round pieces. NFPP is used as the positive electrode active material (matching the negative electrode of this invention), mixed with SP and PVDF at a mass ratio of 8:1:1. NMP is used as the solvent to prepare the positive electrode slurry, which is then coated onto aluminum foil, dried, rolled, and cut into φ12mm positive electrode sheets. Glass fiber filter paper (Whatman GF / D) is used as the separator. A mixed solvent of 1M NaPF6 dissolved in ethylene carbonate (EC) and diethyl carbonate (DEC) (volume ratio 1:1) with 2% fluoroethylene carbonate (FEC) is added as the electrolyte. The CR2032 coin cell is assembled in an argon glove box. The assembly sequence is: negative electrode shell → positive electrode sheet → electrolyte → separator → electrolyte → negative electrode sheet → gasket → spring sheet → positive electrode shell. After sealing, the assembly is allowed to stand for 12 hours before testing.

[0027] Example 1 This embodiment provides a method for preparing NFPP polyanionic sodium-ion battery negative electrode slurry, including the following steps: Weigh the raw materials according to the following parts by weight: 95 parts hard carbon, 1.5 parts SP, 2.5 parts SBR (based on dry solid effective components), and 1.0 part CMC. Weigh deionized water and control the total amount of deionized water added so that the solid content of the final negative electrode slurry is 47%.

[0028] S1. Weigh out the hard carbon, SP, SBR, CMC and deionized water according to the weight ratio; S2. Mix CMC with half the weight of deionized water and stir at 1000 rpm for 90 minutes until completely dissolved to obtain CMC adhesive solution. S3. Add SP to the CMC adhesive solution, stir at 1500 rpm for 30 minutes, add hard carbon, and continue stirring for 120 minutes to obtain a mixed slurry; S4. Add SBR and remaining deionized water to the mixed slurry, and stir at 800 rpm for 45 minutes to obtain sodium-ion battery negative electrode slurry. S5. After the negative electrode slurry is subjected to vacuum degassing treatment at -0.09MPa for 20 minutes, it is coated on the surface of the aluminum foil current collector, dried, and rolled to obtain the negative electrode sheet.

[0029] Example 2 This embodiment provides a method for preparing NFPP polyanionic sodium-ion battery negative electrode slurry, including the following steps: Weigh the raw materials according to the following parts by weight: 93 parts hard carbon, 2 parts SP, 3 parts SBR (based on dry solid effective components), and 1.5 parts CMC. Weigh deionized water and control the total amount of deionized water added so that the solid content of the final negative electrode slurry is 48%.

[0030] S1. Weigh out the hard carbon, SP, SBR, CMC and deionized water according to the weight ratio; S2. Mix CMC with half the weight of deionized water and stir at 800 rpm for 120 minutes until completely dissolved to obtain CMC adhesive solution. S3. Add SP to the CMC adhesive solution and stir at 1000 rpm for 40 minutes. Add hard carbon and continue stirring for 180 minutes to obtain a mixed slurry. S4. Add SBR and remaining deionized water to the mixed slurry, and stir at 500 rpm for 60 minutes to obtain sodium-ion battery negative electrode slurry. S5. After the negative electrode slurry is subjected to vacuum degassing treatment at -0.08MPa for 30 minutes, it is coated on the surface of the aluminum foil current collector, dried, and rolled to obtain the negative electrode sheet.

[0031] Example 3 This embodiment provides a method for preparing NFPP polyanionic sodium-ion battery negative electrode slurry, including the following steps: Weigh the raw materials according to the following parts by weight: 96.5 parts hard carbon, 1 part SP, 2 parts SBR (based on dry solid effective components), and 0.8 parts CMC. Weigh deionized water and control the total amount of deionized water added so that the solid content of the final negative electrode slurry is 46%.

[0032] S1. Weigh out the hard carbon, SP, SBR, CMC and deionized water according to the weight ratio; S2. Mix CMC with half the weight of deionized water and stir at 1500 rpm for 60 minutes until completely dissolved to obtain CMC adhesive solution. S3. Add SP to the CMC adhesive solution, stir at 2000 rpm for 20 minutes, add hard carbon, and continue stirring for 120 minutes to obtain a mixed slurry; S4. Add SBR and remaining deionized water to the mixed slurry, and stir at 1000 rpm for 30 minutes to obtain sodium-ion battery negative electrode slurry. S5. After the negative electrode slurry is subjected to vacuum degassing treatment at -0.10MPa for 10 minutes, it is coated on the surface of the aluminum foil current collector, dried, and rolled to obtain the negative electrode sheet.

[0033] Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that the amounts of hard carbon, SP, SBR, and CMC exceed the preferred range. Specifically, each raw material is weighed according to the following weight percentages: 90 parts hard carbon, 3 parts SP, 4 parts SBR (based on dry solid effective components), and 2 parts CMC. Deionized water is also weighed, and the total amount of deionized water is controlled so that the solid content of the final negative electrode slurry is 47%. The remaining steps are the same as in Example 1.

[0034] Comparative Example 2 The difference between Comparative Example 2 and Example 1 is that the D50 particle size of the hard carbon used is 12 μm, and the specific surface area is 1.5 m². 2 / g, the proportions of the remaining raw materials and the preparation steps are exactly the same as in Example 1.

[0035] Comparative Example 3 The difference between Comparative Example 3 and Example 1 is that the glass transition temperature of the SBR emulsion used is -25°C, while the other raw material ratios and preparation steps are exactly the same as in Example 1.

[0036] Comparative Example 4 The difference between Comparative Example 4 and Example 1 is that the degree of substitution of CMC used is 0.5, the viscosity of the 2% aqueous solution is 1500 mPa·s, and the other raw material ratios and preparation steps are exactly the same as those in Example 1.

[0037] Test case The negative electrode slurry and battery cell prepared by the methods of Examples 1-3 and Comparative Examples 1-4 were compared and tested: (1) Viscosity: Tested using a rotational viscometer in accordance with GB / T 10247-2008 standard; (2) Fineness: The fineness was tested using a scraper fineness tester in accordance with GB / T 1724-2019 standard; (3) Solid content: Tested using the oven drying method according to GB / T 1725-2007 standard; (4) Electrochemical performance test: The sample was charged to 3.6V using a constant current and constant voltage at 0.5C (cutoff current 0.02C), allowed to stand for 5 minutes, and then discharged to 1.5V using a constant current at 0.5C. The discharge capacity was recorded. Subsequently, the sample was charged to 3.0V using a constant current at 0.5C, and the charging capacity was recorded. The temperature change during the capacity gradation process was also recorded. Five parallel samples were tested for each example and comparative example, and the average value was taken as the final result.

[0038] The test results are shown in Table 1.

[0039] Table 1: Overall performance test results of each embodiment and comparative example

[0040] Figure 1This is a photograph of the NFPP polyanionic sodium-ion battery negative electrode slurry prepared in Example 1 of this invention. As can be seen from the image, the slurry is a uniform, black, viscous liquid with a smooth, particle-free surface, and no obvious bubbles or agglomerates, indicating that the components are well dispersed in the slurry. The slurry exhibits good flowability in a container, forming a continuous streamline when poured without interruption or adhesion to the walls, indicating excellent rheological properties suitable for subsequent coating processes.

[0041] Figure 2 This is a 0.5C capacity testing curve of the sodium-ion battery cell prepared in Example 1 of this invention. As can be seen from the figure, both the charging and discharging curves are smooth and complete, without obvious plateau fluctuations or abnormal inflection points, indicating that the electrochemical reactions of the electrodes are stable and reversible during charging and discharging. The charging capacity and discharging capacity are close, the initial coulombic efficiency is high, and the irreversible capacity loss is small. The discharge plateau voltage is stable, indicating a low degree of electrode polarization, unobstructed electron conduction and ion transport channels, and that the synergistic effect between the components is fully utilized.

[0042] Figure 3 This is a temperature profile of the sodium-ion battery cell prepared in Example 1 of this invention. As can be seen from the figure, the cell temperature remained stable throughout the entire capacity testing process, with the difference between the highest and lowest temperatures being only 3.3℃. This indicates a uniform current density distribution within the cell and no localized overheating. The uniform temperature distribution demonstrates, on the one hand, that the amount of conductive agent SP added to the slurry formulation of this invention is reasonable, enabling the construction of a uniform conductive network within the electrode; on the other hand, it also indicates good bonding and dispersion of SBR and CMC, resulting in a uniform electrode structure that is conducive to the uniform conduction of electrochemical reactions. Good temperature uniformity is of great significance for ensuring battery safety and cycle life.

[0043] As shown in Table 1, the viscosity, fineness, and solid content of the slurry in Examples 1-3 of this invention are all within the preferred range. The slurry has good fluidity, uniform dispersion, and excellent coating performance. The cell capacity is highly consistent with the design value, the capacity difference is small, and the electrochemical performance is excellent. In contrast, Comparative Example 1 has an excessively low proportion of active material and an excessively high proportion of conductive agent and binder, resulting in excessively high slurry viscosity and coarse fineness. This makes it prone to defects during coating. At the same time, the reduced active material content leads to a significant decrease in capacity and a significant increase in temperature difference, indicating that exceeding the preferred range of component ratios will seriously damage the slurry processing performance and battery performance. In Comparative Example 2, the hard carbon particle size is too large and the specific surface area is too small, which reduces the sodium ion insertion and extraction kinetics and reactive sites, resulting in a decrease in capacity and an increase in temperature difference. Comparative Example 3 uses SBR with an excessively low glass transition temperature, resulting in insufficient bonding strength, poor electrode structure stability, and deterioration of both capacity and temperature difference. In Comparative Example 4, the CMC substitution degree is too low, weakening the thickening and dispersion effects, reducing slurry stability, decreasing capacity, and increasing temperature difference. The above comparison fully demonstrates that the various physical properties of hard carbon, SBR, and CMC must be within the preferred range of this invention in order to form the best synergistic effect with each component. Changing any key parameter alone will significantly degrade the slurry performance and electrochemical performance.

[0044] In summary, this invention successfully prepared a sodium-ion battery anode slurry with excellent electrochemical performance, good processing performance, and high consistency through the systematic synergy of hard carbon, SP, SBR, CMC, and deionized water. The various technical features support each other and synergistically enhance each other, achieving technical effects that cannot be achieved by a single component or simple combination. It has significant technological progress and broad application prospects.

[0045] This specific embodiment is merely an explanation of the present invention and is not intended to limit the invention. After reading this specification, those skilled in the art can make modifications to this embodiment without contributing any inventive step, but such modifications are protected by patent law as long as they are within the scope of the claims of the present invention.

Claims

1. A method for preparing an NFPP polyanionic sodium-ion battery negative electrode slurry, characterized in that, The raw materials for preparation, based on dry powder mass, include the following parts by weight: 93-96.5 parts hard carbon, 1-2 parts SP, 2-3 parts SBR, and 0.8-1.5 parts CMC; It also includes deionized water, the total amount of which results in a final negative electrode slurry with a solid content of 45%-50%; the preparation method includes the following steps: S1. Weigh out the hard carbon, SP, SBR, CMC and deionized water according to the weight ratio; S2. Mix CMC with some deionized water and stir until completely dissolved to obtain CMC adhesive solution; S3. Add SP to the CMC adhesive solution, stir evenly, then add hard carbon and continue stirring to obtain a mixed slurry; S4. Add SBR and remaining deionized water to the mixed slurry, stir evenly, and obtain sodium-ion battery negative electrode slurry. S5. After vacuum degassing, the negative electrode slurry is coated onto the surface of the current collector, dried, and rolled to obtain the negative electrode sheet.

2. The method for preparing an NFPP polyanionic sodium-ion battery negative electrode slurry according to claim 1, characterized in that, The hard carbon has a D50 particle size of 3-8 μm and a specific surface area of ​​3-8 m². 2 / g, with an interlayer spacing d002 of 0.37-0.40nm.

3. The method for preparing an NFPP polyanionic sodium-ion battery negative electrode slurry according to claim 1, characterized in that, The hard carbon is carbonized at a temperature of 1000-1400℃ for 2-6 hours.

4. The method for preparing an NFPP polyanionic sodium-ion battery negative electrode slurry according to claim 1, characterized in that, The specific surface area of ​​the SP is 60-80m². 2 / g, DBP absorption value is 150-200ml / 100g.

5. The method for preparing an NFPP polyanionic sodium-ion battery negative electrode slurry according to claim 1, characterized in that, The SBR is based on its effective solids content, and the glass transition temperature of the SBR emulsion is -5°C to -15°C.

6. The method for preparing an NFPP polyanionic sodium-ion battery negative electrode slurry according to claim 1, characterized in that, The CMC has a degree of substitution of 0.7-1.0 and a viscosity of 2% aqueous solution of 2000-5000 mPa·s.

7. The method for preparing an NFPP polyanionic sodium-ion battery negative electrode slurry according to claim 1, characterized in that, The stirring speed in step S2 is 800-1500 rpm, and the stirring time is 60-120 minutes.

8. The method for preparing an NFPP polyanionic sodium-ion battery negative electrode slurry according to claim 1, characterized in that, The stirring speed in step S3 is 1000-2000 rpm, and the stirring time is 120-180 minutes.

9. The method for preparing an NFPP polyanionic sodium-ion battery negative electrode slurry according to claim 1, characterized in that, The stirring speed in step S4 is 500-1000 rpm, and the stirring time is 30-60 minutes.

10. The method for preparing an NFPP polyanionic sodium-ion battery negative electrode slurry according to claim 1, characterized in that, The vacuum degree of the vacuum degassing process in step S5 is -0.08MPa to -0.10MPa, and the degassing time is 10-30 minutes.