High-silicon-content negative electrode, preparation method and application thereof
By optimizing the preparation process and material ratio of the negative electrode slurry, a three-dimensional network structure is formed, which solves the problem of breakage caused by volume changes during charging and discharging of high silicon content negative electrode materials, and improves the cycle life and performance stability of lithium-ion batteries.
Patent Information
- Application Number
- CN202510670963.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-23
- Publication Date
- 2026-11-24
AI Technical Summary
In existing technologies, the problems of electrode demolding and short cycle life caused by silicon volume expansion in high-silicon-content anode materials have not been effectively solved.
A dry slurry process was used to prepare the anode slurry, which used materials such as graphite, silicon carbide, single-walled carbon nanotubes, conductive carbon black SP powder, polyacrylic acid, sodium carboxymethyl cellulose, and styrene-butadiene rubber. By optimizing the binder ratio and stepwise stirring process, a three-dimensional network structure was formed to adapt to the large volume changes of the silicon anode during lithiation/delithiation.
The cycle life and performance stability of the negative electrode have been improved. The prepared high silicon content negative electrode has a cycle life of ≥500 cycles and a capacity retention rate of ≥80%, which effectively alleviates the problem of negative electrode breakage and demolding caused by silicon volume change.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention belongs to the field of lithium-ion battery technology, specifically relating to a high-silicon-content anode, its preparation method, and its application. Background Technology
[0002] With the rapid development of lithium-ion batteries, people have increasingly higher requirements for their energy density and safety performance. Graphite remains the primary anode material for lithium-ion batteries, and improving energy density is crucial. Therefore, silicon-based anodes are generally used in conjunction with graphite to enhance energy density. However, silicon expands by more than 300% in volume during complete lithium-ionization, leading to high internal stress and potential electrode compression. This can cause cracks at the silicon anode material interface, even resulting in pulverization or loss of contact with the current collector, causing the active material to detach from the electrode. This significantly reduces cycle life, resulting in silicon-doped batteries currently containing approximately 10% silicon in the anode active material. Chinese patent (CN111697194 A) focuses on the stability of silicon-carbon slurry, addressing the sedimentation and powdering issues of traditional silicon-carbon slurry by adjusting the sodium carboxymethyl cellulose substitution degree (DS = 0.8–1.0) and the styrene-butadiene rubber ratio. The silicon content is not specified (the slurry formulation contains 36%–40% silicon-carbon graphite). The Chinese patent (CN 118448586 A) optimizes fast-charging performance through a double-layer heterogeneous structure (layered coating of slurry A / B), with a low silicon content (silicon-carbon content of 8%–10% in slurry A), but does not address the volume expansion problem associated with high silicon content. Therefore, the problems of electrode demolding and short cycle life caused by silicon volume expansion (over 300%) in high-silicon-content anode materials have not been effectively solved. Summary of the Invention
[0003] Based on the above problems, the negative electrode sheet prepared by the present invention can effectively solve the problem of negative electrode breakage and demolding caused by large silicon volume change during charging and discharging when the silicon content is high, and effectively improve the cycle life and performance stability of the battery.
[0004] The first inventive point provided by this invention is: a method for preparing a high-silicon-content negative electrode, wherein the negative electrode comprises a current collector copper foil and negative electrode active materials located on both sides of the current collector copper foil, comprising the following steps:
[0005] 1) The negative electrode active material is prepared into a negative electrode slurry using a dry slurry process in a certain proportion. The negative electrode slurry is uniformly coated on both sides of the negative electrode current collector copper foil by a single-layer coating method. The solvent is removed by baking to obtain the electrode roll.
[0006] 2) The electrode roll is then subjected to one and two rolling processes, and then die-cut and baked to obtain the high silicon content negative electrode.
[0007] Further, the negative electrode active material mentioned in step 1) includes graphite, silicon carbide, single-walled carbon nanotubes, conductive carbon black SP powder, polyacrylic acid, sodium carboxymethyl cellulose and styrene-butadiene rubber, deionized water, and N-methylpyrrolidone (NMP).
[0008] Further, the mass ratio of graphite, silicon carbide, single-walled carbon nanotubes, conductive carbon black SP powder, polyacrylic acid, sodium carboxymethyl cellulose, styrene-butadiene rubber, deionized water, and N-methylpyrrolidone NMP is (24.9~28.7):(9.5~13.4):(0.02~0.04):(0.2~0.4):(1~1.2):(0.1~0.3):(0.2~0.4):(58~62):(1~1.2).
[0009] Furthermore, the dry slurry mixing process includes:
[0010] S1: Weigh the following materials according to the mass ratio: graphite, silicon carbide, single-walled carbon nanotubes, conductive carbon black SP powder, polyacrylic acid, sodium carboxymethyl cellulose, styrene-butadiene rubber, deionized water, and N-methylpyrrolidone (NMP).
[0011] S2: Add silicon carbide, graphite, conductive carbon black SP powder, and sodium carboxymethyl cellulose to a planetary mixer and stir at low speed without vacuum for 20-30 minutes according to parameter a.
[0012] S3: Add single-walled carbon nanotubes to the slurry in step S2, and then weigh 10-20% of the total weight of the required deionized water and 50-60% of the total weight of the required polyacrylic acid and add them to the slurry in step S2 respectively. Use a planetary mixer to stir at medium speed without vacuum for 50-60 minutes according to parameter b.
[0013] S4: Weigh 40-50% of the total weight of the required deionized water and 40-50% of the total weight of the required polyacrylic acid and add them to the slurry in step S3. Use a planetary mixer to stir at high speed under vacuum for 60-90 minutes according to parameter c.
[0014] S5: Weigh 30-50% of the total weight of the required deionized water and the total weight of the required N-methylpyrrolidone (NMP) and add them to the slurry in step S4. Use a planetary mixer to stir at high speed under vacuum for 60-90 minutes according to parameter d.
[0015] S6: Weigh the required styrene-butadiene rubber and add it to the slurry prepared in step S5. Use a planetary mixer to vacuum stir at low speed for 20-30 minutes according to parameter e to obtain a silicon-carbon anode slurry for lithium-ion batteries with a solid content of 38-42%.
[0016] Preferably, parameter a is: revolution 10-20 rpm, rotation 1000-1500 rpm;
[0017] The parameter b is: revolution 20-30 rpm, rotation 2000-2500 rpm;
[0018] The parameter c is: revolution 20-30 rpm, rotation 2500-3000 rpm;
[0019] The parameter d is: revolution 20-30 rpm, rotation 2500-3000 rpm;
[0020] The parameter e is: revolution 20-30 rpm, rotation 500-1000 rpm.
[0021] Furthermore, the areal density of the negative electrode active material layer described in step 1) is 95–105 g / m². 2 Preferably, it is 103 g / m 2 The slurry is filtered using a 180-220 mesh capsule filter before coating.
[0022] Furthermore, the compaction ratio of the first rolling operation in step 2) is 1.35–1.4 g / cm³. 3 The secondary roller compaction ratio is 1.52–1.62 g / cm³. 3 The baking temperature is 80-100℃.
[0023] The second inventive point of this invention is: a high silicon content negative electrode, prepared by the method described above, wherein the silicon content of the negative electrode is 25% to 35%; the cycle life of the negative electrode is ≥500 cycles, and the capacity retention rate is ≥80%.
[0024] The third inventive point of this invention is: a lithium-ion battery comprising the high silicon content negative electrode described above.
[0025] Compared with the prior art, the advantages of the present invention are:
[0026] This invention employs a suitable ratio of negative electrode active materials and a unique preparation process. Several negative electrode active materials synergistically form a three-dimensional network structure, effectively adsorbing and coating silicon-carbon, graphite, and conductive carbon black (SP) particles. This effectively accommodates the large volume changes of the silicon negative electrode during lithiation / delithiation, allowing the negative electrode to adhere well to the copper current collector. This effectively alleviates the problem of negative electrode breakage and demolding caused by large silicon volume changes during charge and discharge, improving the battery's cycle life and performance stability. This invention is simple to operate, low in cost, and easy to industrialize, thus promoting the development of silicon-carbon and high-energy-density lithium-ion battery industries. Specific implementation methods
[0027] To make the objectives, technical solutions, and advantages of this application clearer, a more detailed description is provided below. However, it should be understood that the description herein is merely for explaining this application and is not intended to limit its scope.
[0028] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application belongs. The terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the scope of this application. All reagents and instruments used herein are commercially available, and the characterization methods involved can be found in relevant descriptions in the prior art, and will not be repeated here.
[0029] To further understand this application, the following detailed description is provided in conjunction with the preferred embodiments.
[0030] Example 1
[0031] This embodiment provides a method for preparing a high-silicon-content negative electrode, wherein the negative electrode comprises a current collector copper foil and a negative electrode active material layer located on both sides of the current collector copper foil, characterized by comprising the following steps:
[0032] 1) The negative electrode active material is prepared into a negative electrode slurry using a dry slurry process in a certain proportion. The negative electrode slurry is uniformly coated on both sides of the negative electrode current collector copper foil by a single-layer coating method. The solvent is removed by baking to obtain the electrode roll.
[0033] 2) The electrode roll is then subjected to one and two rolling processes, and then die-cut and baked to obtain the high silicon content negative electrode.
[0034] As a further preferred embodiment, the negative electrode active material in step 1) is graphite, silicon carbide, single-walled carbon nanotubes, SP powder, polyacrylic acid, sodium carboxymethyl cellulose, styrene-butadiene rubber, deionized water, and N-methylpyrrolidone (NMP).
[0035] Preferably, the mass ratio of graphite, silicon carbide, single-walled carbon nanotubes, conductive carbon black SP powder, polyacrylic acid, sodium carboxymethyl cellulose, styrene-butadiene rubber, deionized water, and N-methylpyrrolidone (NMP) is (24.9–28.7):(9.5–13.4):(0.02–0.04):(0.2–0.4):(1–1.2):(0.1–0.3):(0.2–0.4):(58–62):(1–1.2).
[0036] More preferably, the negative electrode slurry is prepared from graphite, silicon carbide, single-walled carbon nanotubes, SP powder, polyacrylic acid, sodium carboxymethyl cellulose, styrene-butadiene rubber, deionized water, and N-methylpyrrolidone (NMP) in a mass ratio of 27:11.8:0.03:0.3:1.1:0.2:0.245:60:1.1.
[0037] The graphite is preferably fast-charging artificial graphite.
[0038] This invention optimizes the binder ratio and adds a chain-like polymeric aqueous binder: polyacrylic acid, which can effectively adapt to the large volume changes of the silicon anode during lithiumation / delithiation. It works synergistically with styrene-butadiene rubber and sodium carboxymethyl cellulose through different mechanisms, enhancing the cohesion, stability, and adhesion between the anode material and the current collector of the battery slurry. The prepared electrode is not easy to detach from the film and has good flexibility, improving processing performance, stabilizing the SEI film, and effectively extending the cycle life of the battery.
[0039] As a further preferred embodiment, the dry slurry mixing process includes:
[0040] S1: Weigh the following materials according to the mass ratio: graphite, silicon carbide, single-walled carbon nanotubes, conductive carbon black SP powder, polyacrylic acid, sodium carboxymethyl cellulose, styrene-butadiene rubber, deionized water, and N-methylpyrrolidone (NMP).
[0041] S2: Add silicon carbide, graphite, conductive carbon black SP powder, and sodium carboxymethyl cellulose to a planetary mixer and stir at low speed without vacuum for 20-30 minutes according to parameter a.
[0042] S3: Add single-walled carbon nanotubes to the slurry in step S2, and then weigh 10-20% of the total weight of the required deionized water and 50-60% of the total weight of the required polyacrylic acid and add them to the slurry in step S2 respectively. Use a planetary mixer to stir at medium speed without vacuum for 50-60 minutes according to parameter b.
[0043] S4: Weigh 40-50% of the total weight of the required deionized water and 40-50% of the total weight of the required polyacrylic acid and add them to the slurry in step S3. Use a planetary mixer to stir at high speed under vacuum for 60-90 minutes according to parameter c.
[0044] S5: Weigh 30-50% of the total weight of the required deionized water and the total weight of the required N-methylpyrrolidone (NMP) and add them to the slurry in step S4. Use a planetary mixer to stir at high speed under vacuum for 60-90 minutes according to parameter d.
[0045] S6: Weigh the required styrene-butadiene rubber and add it to the slurry prepared in step S5. Use a planetary mixer to vacuum stir at low speed for 20-30 minutes according to parameter e to obtain a silicon-carbon anode slurry for lithium-ion batteries with a solid content of 38-42%.
[0046] Preferably,
[0047] The parameter 'a' is: revolution 10-20 rpm, rotation 1000-1500 rpm.
[0048] The parameter b is: revolution 20-30 rpm, rotation 2000-2500 rpm.
[0049] The parameter c is: revolution 20-30 rpm, rotation 2500-3000 rpm.
[0050] The parameter d is: revolution 20-30 rpm, rotation 2500-3000 rpm.
[0051] The parameter e is: revolution 20-30 rpm, rotation 500-1000 rpm.
[0052] As a further preferred embodiment, the silicon-carbon has a capacity of 1750–1850 mAh / g @ 0.8V; the graphite is fast-charging graphite with a capacity of 348–352 mAh / g and a specific surface area ≤ 3.00 m². 2 / g.
[0053] As a further preferred embodiment, the viscosity of the negative electrode slurry is 4500-7000 MPa.
[0054] As a further preferred embodiment, the double-sided areal density of the negative electrode active material layer in step 1) is 95-105 g / m². 2 Preferably, it is 103 g / m 2 .
[0055] As a further preferred embodiment, the slurry described in step 1) is filtered using a 180-220 mesh capsule filter before coating.
[0056] As a further preferred embodiment, the compaction ratio of the first rolling in step 2) is 1.35–1.4 g / cm³. 3 The secondary roller compaction ratio is 1.52–1.62 g / cm³. 3 .
[0057] As a further preferred embodiment, the baking temperature is 80–100°C.
[0058] Example 2
[0059] According to the preparation method of Example 1, this example provides a high silicon content anode, which is prepared by the method described above, and the silicon content of the anode is 25% to 35%.
[0060] Preferably, the negative electrode has a cycle life of ≥500 cycles and a capacity retention rate of ≥80%.
[0061] This embodiment also provides a lithium-ion battery comprising the high-silicon-content negative electrode described above.
[0062] The positive electrode of a lithium-ion battery is a conventional material that is readily available on the market.
[0063] Example 3
[0064] This embodiment describes the content of the above embodiment in detail, sets up experimental cases and comparative examples, conducts relevant performance tests and effect data, as follows:
[0065] Experimental Example 1
[0066] A high-silicon-content negative electrode, comprising a copper foil and negative electrode active material layers located on both sides of the copper foil, is prepared as follows:
[0067] 1) The negative electrode slurry containing negative electrode active material is prepared using a dry slurry mixing process, as shown in the following steps:
[0068] S1: Weigh the negative electrode active material according to the following mass ratio: 27g graphite, 11.8g silicon carbide, 0.03g single-walled carbon nanotubes, 0.3g conductive carbon black SP powder, 1.1g polyacrylic acid, 0.2g sodium carboxymethyl cellulose, 0.245g styrene-butadiene rubber, 60g deionized water, and 1.1g N-methylpyrrolidone (NMP).
[0069] S2: Add 11.8g of silicon carbide, 27g of fast-charging artificial graphite, 0.3g of conductive carbon black SP powder, and 0.2g of sodium carboxymethyl cellulose to a planetary mixer, and stir at a low speed of 10 rpm for 20 minutes without vacuuming, according to parameter a.
[0070] S3: Add 0.03g of single-walled carbon nanotubes to the slurry in step S2, then weigh 6g of deionized water and 0.61g of polyacrylic acid and add them to the slurry in step S2 respectively. Use a planetary mixer to stir at a medium speed of 20 rpm for revolution and 2000 rpm for rotation without vacuum for 50 minutes according to parameter b.
[0071] S4: Weigh 27g of deionized water and 0.49g of the required polyacrylic acid and add them to the slurry in step S3. Use a planetary mixer to perform high-speed vacuum mixing for 60 minutes at parameters c: 20 rpm for revolution and 2500 rpm for rotation.
[0072] S5: Weigh 27g of the required deionized water and 1.1g of N-methylpyrrolidone (NMP) and add them to the slurry from step S4. Use a planetary mixer to stir at high speed under vacuum for 60 minutes according to parameter d, with the planetary mixer revolving at 20 rpm and rotating at 2500 rpm.
[0073] S6: Weigh 0.245g of styrene-butadiene rubber and add it to the slurry prepared in step S5. Use a planetary mixer to perform low-speed vacuum stirring for 20min at parameter e, with an orbital rotation of 20rpm and a rotation of 500rpm, to obtain a silicon-carbon anode slurry for lithium-ion batteries with a solid content of 40%.
[0074] The negative electrode slurry was filtered using a 200-mesh capsule filter.
[0075] The filtered negative electrode slurry was coated in a single layer at a concentration of 103 g / m³. 2 Double-sided surface density coating is applied to both sides of the negative electrode current collector copper foil, and the solvent is removed by baking at 90°C to obtain the electrode roll;
[0076] 2) The electrode roll is then subjected to a first roll pressing and a second roll pressing. The compaction ratio of the first roll pressing is 1.38 g / cm3, and the compaction ratio of the second roll pressing is 1.6 g / cm3. Then it is die-cut and baked at 90°C to obtain the high silicon content negative electrode, wherein the silicon content is 30%.
[0077] Experimental Example 2
[0078] A high-silicon-content negative electrode, comprising a copper foil and negative electrode active material layers located on both sides of the copper foil, is prepared as follows:
[0079] 1) The negative electrode slurry containing negative electrode active material is prepared using a dry slurry mixing process, as shown in the following steps:
[0080] S1: Weigh the negative electrode active material according to the following mass ratio: 66g graphite, 28.8g silicon carbide, 0.073g single-walled carbon nanotubes, 0.73g conductive carbon black SP powder, 2.58g polyacrylic acid, 0.48g sodium carboxymethyl cellulose, 0.56g styrene-butadiene rubber, 147g deionized water, and 2.58g N-methylpyrrolidone (NMP). Set aside.
[0081] S2: Add 29g of silicon carbon, 66g of fast-charging artificial graphite, 0.73g of SP powder, and 0.48g of sodium carboxymethyl cellulose to a planetary mixer, and mix at a low speed of 20 rpm for revolution and 1500 rpm for rotation without vacuum for 30 minutes according to parameter a.
[0082] S3: Add 0.073g of single-walled carbon nanotubes to the slurry in step S2, weigh out 14.7g of the required deionized water and 1.38g of the required polyacrylic acid and add them to the slurry in step S2 respectively. Use a planetary mixer to stir at a medium speed of 30rpm and 2500rpm without vacuum for 60min according to parameter b.
[0083] S4: Weigh 66.15g of the required deionized water and 1.2g of the required polyacrylic acid and add them to the slurry in step S3. Use a planetary mixer and stir at high speed and vacuum for 90 minutes according to parameter c: 30 rpm revolution and 3000 rpm rotation.
[0084] S5: Weigh 66.15g of the required deionized water and 2.58g of N-methylpyrrolidone (NMP) and add them to the slurry from step S2. Use a planetary mixer to perform high-speed vacuum mixing for 90 minutes at parameters d: 20 rpm revolution and 2500 rpm rotation.
[0085] S6: Weigh 0.56g of styrene-butadiene rubber and add it to the slurry prepared in step S5. Use a planetary mixer to perform low-speed vacuum stirring for 300min at parameters e, with the planetary mixer revolving at 30rpm and rotating at 1000rpm, to obtain a silicon-carbon anode slurry for lithium-ion batteries with a solid content of 39%.
[0086] The negative electrode slurry was filtered using a 200-mesh capsule filter.
[0087] The filtered negative electrode slurry was coated in a single layer at a concentration of 104 g / m³. 2 Double-sided surface density coating is applied to both sides of the negative electrode current collector copper foil, and the solvent is removed by baking at 100°C to obtain the electrode roll;
[0088] 2) The electrode roll is then subjected to a first roll pressing and a second roll pressing. The compaction ratio of the first roll pressing is 1.39 g / cm3, and the compaction ratio of the second roll pressing is 1.59 g / cm3. Then it is die-cut and baked at 100°C to obtain the high silicon content negative electrode, wherein the silicon content is 30%.
[0089] Experimental Example 3
[0090] A high-silicon-content negative electrode: The difference between this experimental example and Experimental Example 1 is that in step 1), the following components are present: 66g graphite, 28.8g silicon carbide, 0.073g single-walled carbon nanotubes, 0.73g conductive carbon black SP powder, 2.78g polyacrylic acid (60% of the total weight of polyacrylic acid is added in step S3 and 40% of the total weight of polyacrylic acid is added in step S4), 0.48g sodium carboxymethyl cellulose, 0.66g styrene-butadiene rubber, 147g deionized water (20% of the total weight of deionized water in step S3, 40% of the total weight of deionized water in step S4, and 40% of the total weight of deionized water in step S5), and 2.78g N-methylpyrrolidone (NMP). The formulation of this product is different from that of Experimental Example 1.
[0091] The remaining preparation methods and parameters were consistent with those in Example 1. The prepared high-silicon-content anode had a silicon content of 30%.
[0092] Test Example 4
[0093] A high-silicon-content negative electrode: The difference between this experimental example and Experimental Example 1 is that in step 1), the following components are present: 70.15g graphite, 24.65g silicon carbide, 0.073g single-walled carbon nanotubes, 0.73g conductive carbon black SP powder, 2.68g polyacrylic acid (of which 55% of the total weight of polyacrylic acid is added in step S3 and 45% of the total weight of polyacrylic acid is added in step S4), 0.48g sodium carboxymethyl cellulose, 0.6g styrene-butadiene rubber, 147g deionized water, and 2.68g N-methylpyrrolidone (NMP). The formulation of this product is different from that of Experimental Example 1.
[0094] The remaining preparation methods and parameters were consistent with those in Example 1. The prepared high-silicon-content anode had a silicon content of 26%.
[0095] Experimental Example 5
[0096] A high-silicon-content negative electrode: The difference between this experimental example and Experimental Example 1 is that in step 1), the following components are present: 62.56g graphite, 32.23g silicon carbide, 0.073g single-walled carbon nanotubes, 0.73g conductive carbon black SP powder, 2.68g polyacrylic acid (of which 55% of the total weight of polyacrylic acid is added in step S3 and 45% of the total weight of polyacrylic acid is added in step S4), 0.48g sodium carboxymethyl cellulose, 0.6g styrene-butadiene rubber, 147g deionized water, and 2.68g N-methylpyrrolidone (NMP). The formulation of this product is different from that of Experimental Example 1.
[0097] The remaining preparation methods and parameters were consistent with those in Example 1. The prepared high-silicon-content anode had a silicon content of 34%.
[0098] Comparative Example 1
[0099] A silicon-containing negative electrode, comprising a copper foil and negative electrode active material layers located on both sides of the copper foil, wherein the specific preparation method is as follows:
[0100] The negative electrode slurry containing negative electrode active material is prepared using a wet slurry mixing process, as shown in the following steps:
[0101] The negative electrode active materials include: 66g graphite, 28.8g silicon carbide, 0.073g single-walled carbon nanotubes, 0.73g conductive carbon black SP powder, 2.58g polyacrylic acid, 0.48g sodium carboxymethyl cellulose, 0.56g styrene-butadiene rubber, 147g deionized water, and 2.58g N-methylpyrrolidone (NMP).
[0102] S1: Weigh 0.48g of sodium carboxymethyl cellulose and 28g of the required deionized water, add them to a planetary mixer, and stir at low speed vacuum for 150min according to the parameters of revolution at 10rpm and rotation at 1000rpm.
[0103] S2: Weigh 0.73g of SP powder and 87g of the required deionized water and add them to the planetary mixer. Set the parameters to 10rpm for revolution and 1000rpm for rotation at low speed and without vacuum for 30 minutes.
[0104] S3: Add 28.8g of silicon carbon, 66g of fast-charging artificial graphite, and 0.073g of silicon carbon single-walled carbon nanotubes to the slurry in step S2. Set the planetary mixer to 20 rpm for revolution and 2000 rpm for rotation. Mix at medium speed without vacuum for 60 minutes.
[0105] S4: Weigh 30g of the required deionized water and 2.58g of the required polyacrylic acid and add them to the slurry in step S3. Set the planetary mixer to 20rpm for revolution and 2500rpm for rotation and high-speed vacuum mixing for 120min.
[0106] S5: Weigh 30g of the required deionized water and 2.58g of N-methylpyrrolidone (NMP) and add them to the slurry in step S4. Set the planetary mixer to 20 rpm for revolution and 2500 rpm for rotation and high-speed vacuum mixing for 60 minutes.
[0107] S6: Weigh 0.56g of styrene-butadiene rubber and add it to the slurry prepared in step S5. Set the planetary mixer to 20rpm for revolution and 500rpm for rotation and low-speed vacuum stirring for 20min to obtain a silicon-carbon anode slurry for lithium-ion batteries with a solid content of 40%.
[0108] The remaining steps are the same as in Example 2, and the silicon-containing anode prepared has a silicon content of 30%.
[0109] Comparative Example 2
[0110] A silicon-containing negative electrode, comprising a copper foil and negative electrode active material layers located on both sides of the copper foil, wherein the specific preparation method is as follows:
[0111] The negative electrode slurry containing negative electrode active material is prepared using a dry slurry mixing process, as shown in the following steps:
[0112] The negative electrode active materials include: 66g graphite, 28.8g silicon carbide, 0.073g single-walled carbon nanotubes, 0.73g conductive carbon black SP powder, 2.08g polyacrylic acid (of which 45% of the total weight of polyacrylic acid is added in step S3 and 55% of the total weight of polyacrylic acid is added in step S4), 0.28g sodium carboxymethyl cellulose, 0.36g styrene-butadiene rubber, 147g deionized water, and 2.58g N-methylpyrrolidone (NMP). Other steps are the same as in Experimental Example 2.
[0113] The prepared silicon-containing anode has a silicon content of 30%.
[0114] Comparative Example 3
[0115] A silicon-containing negative electrode, comprising a copper foil and negative electrode active material layers located on both sides of the copper foil, wherein the specific preparation method is as follows:
[0116] The negative electrode slurry containing negative electrode active material is prepared using a dry slurry mixing process, as shown in the following steps:
[0117] The negative electrode active materials include: 66g graphite, 28.8g silicon carbide, 0.073g single-walled carbon nanotubes, 0.73g conductive carbon black SP powder, 3.38g polyacrylic acid (of which 55% of the total weight of polyacrylic acid is added in step S3 and 45% of the total weight of polyacrylic acid is added in step S4), 1.18g sodium carboxymethyl cellulose, 0.76g styrene-butadiene rubber, 147g deionized water, and 2.58g N-methylpyrrolidone (NMP). Other steps are the same as in Experimental Example 2.
[0118] The prepared silicon-containing anode has a silicon content of 30%.
[0119] Comparative Example 4
[0120] A silicon-containing negative electrode, comprising a copper foil and negative electrode active material layers located on both sides of the copper foil, wherein the specific preparation method is as follows:
[0121] The negative electrode slurry containing negative electrode active material is prepared using a dry slurry mixing process, as shown in the following steps:
[0122] The negative electrode active materials include: 73g graphite, 21.8g silicon carbide, 0.073g single-walled carbon nanotubes, 0.73g conductive carbon black SP powder, 2.58g polyacrylic acid (of which 55% of the total weight of polyacrylic acid is added in step S3 and 45% of the total weight of polyacrylic acid is added in step S4), 0.48g sodium carboxymethyl cellulose, 0.56g styrene-butadiene rubber, 147g deionized water, and 2.58g N-methylpyrrolidone (NMP). Other steps are the same as in Experimental Example 2.
[0123] The prepared silicon-containing anode has a silicon content of 23%.
[0124] Comparative Example 5
[0125] A silicon-containing negative electrode, comprising a copper foil and negative electrode active material layers located on both sides of the copper foil, wherein the specific preparation method is as follows:
[0126] The negative electrode slurry containing negative electrode active material is prepared using a dry slurry mixing process, as shown in the following steps:
[0127] The negative electrode active materials include: 60.7g graphite, 34.1g silicon carbide, 0.073g single-walled carbon nanotubes, 0.73g conductive carbon black SP powder, 2.58g polyacrylic acid (of which 55% of the total weight of polyacrylic acid is added in step S3 and 45% of the total weight of polyacrylic acid is added in step S4), 0.48g sodium carboxymethyl cellulose, 0.56g styrene-butadiene rubber, 147g deionized water, and 2.58g N-methylpyrrolidone (NMP). Other steps are the same as in Experimental Example 2.
[0128] The prepared silicon-containing anode has a silicon content of 36%.
[0129] Example 4
[0130] The silicon-carbon anode slurry prepared in Examples 1-5 and Comparative Examples 1-5 was coated, rolled, and sheeted to obtain anode sheets. Then, it was stacked with the cathode sheets, packaged, injected with electrolyte, formed, degassed, capacity tested, and shaped to obtain lithium-ion batteries.
[0131] All the above experimental examples and comparative examples used 4.2V NCM cathode materials, and the resulting lithium-ion battery cells were model 10674172 (10.6mm*74mm*172mm) with a nominal capacity of 28Ah.
[0132] The performance test results of the prepared lithium-ion batteries are shown in Table 1.
[0133] Table 1: Comparison of relevant performance indicators of lithium-ion batteries manufactured in the embodiments and comparative examples of the present invention
[0134]
[0135] Analysis of Table 1 shows that the test capacity of Example 2 is similar to that of Comparative Examples 1-3. However, Example 2 showed no powder shedding on the electrode, while Comparative Example 1 showed slight powder shedding. This indicates that Example 2, through dry slurry mixing and step-by-step addition of binder, significantly alleviated the active material shedding caused by silicon volume expansion, thus extending the cycle life. Comparative Example 2, due to the lack of strict binder addition, suffered from insufficient slurry cohesion, resulting in severe powder shedding on the electrode and cracks in the cell, making it unable to complete the cycle test. Example 2, by optimizing the binder (polyacrylic acid + CMC + SBR) content and using a step-by-step vacuum stirring process, formed a three-dimensional network structure, enhancing the electrode flexibility, and employed two rolling processes (1.39 / 1.59 g / cm³). 3 The electrode density is more uniform. Comparative Example 3 had a capacity retention of only 79.56%. The excessively high binder content (polyacrylic acid + CMC + SBR) in Comparative Example 3 resulted in poor electrode flexibility and conductivity, affecting lithium-ion transport kinetics. Comparative Example 4 had a silicon content of only 23%, lower than the silicon content of this application, with a capacity retention of 82.85%, but a breakdown capacity of 27.52 Ah. This indicates that while low silicon content can alleviate volume expansion, it sacrifices energy density and cannot meet high capacity requirements. Comparative Example 5 had a silicon content as high as 36%, leading to severe electrode powder shedding and cell cracking, making testing impossible. The silicon content exceeded the range of this application, proving that when the silicon content is too high, the existing binder system cannot adapt to drastic volume expansion.
[0136] Therefore, other methods of mixing the paste alone, or changes in the material ratio, cannot achieve the performance of the examples. This indicates that the present invention uses a suitable ratio of negative electrode active materials and a special preparation process. Furthermore, the several negative electrode active materials work together to form a three-dimensional network structure, which effectively adsorbs and coats silicon carbon, graphite, and conductive carbon black SP particles. This can effectively adapt to the large volume change of the silicon negative electrode during lithiation / delithiation, allowing the negative electrode to adhere well to the copper current collector. This effectively alleviates the problem of negative electrode breakage and demolding caused by large silicon volume changes during charging and discharging, and improves the cycle life and performance stability of the battery.
[0137] The above description is merely a preferred embodiment of this application and is not intended to limit this application. Any modifications, equivalent substitutions, or improvements made within the spirit and principles of this application should be included within the protection scope of this application.
Claims
1. A method for preparing a high-silicon-content negative electrode, wherein the negative electrode comprises a current collector copper foil and negative electrode active materials located on both sides of the current collector copper foil, characterized in that, Includes the following steps: 1) The negative electrode active material is prepared into a negative electrode slurry using a dry slurry process in a certain proportion. The negative electrode slurry is uniformly coated on both sides of the negative electrode current collector copper foil by a single-layer coating method. The solvent is removed by baking to obtain the electrode roll. 2) The electrode roll is then subjected to one and two rolling processes, and then die-cut and baked to obtain the high silicon content negative electrode.
2. The preparation method according to claim 1, characterized in that, The negative electrode active material mentioned in step 1) includes graphite, silicon carbide, single-walled carbon nanotubes, conductive carbon black SP powder, polyacrylic acid, sodium carboxymethyl cellulose and styrene-butadiene rubber, deionized water, and N-methylpyrrolidone (NMP).
3. The preparation method according to claim 2, characterized in that, The mass ratio of graphite, silicon carbide, single-walled carbon nanotubes, conductive carbon black SP powder, polyacrylic acid, sodium carboxymethyl cellulose, styrene-butadiene rubber, deionized water, and N-methylpyrrolidone (NMP) is (24.9–28.7):(9.5–13.4):(0.02–0.04):(0.2–0.4):(1–1.2):(0.1–0.3):(0.2–0.4):(58–62):(1–1.2).
4. The preparation method according to claim 3, characterized in that, The dry slurry mixing process includes: S1: Weigh the following materials according to the mass ratio: graphite, silicon carbide, single-walled carbon nanotubes, conductive carbon black SP powder, polyacrylic acid, sodium carboxymethyl cellulose, styrene-butadiene rubber, deionized water, and N-methylpyrrolidone (NMP). S2: Add silicon carbide, graphite, conductive carbon black SP powder, and sodium carboxymethyl cellulose to a planetary mixer and stir at low speed without vacuum for 20-30 minutes according to parameter a. S3: Add single-walled carbon nanotubes to the slurry in step S2, and then weigh 10-20% of the total weight of the required deionized water and 50-60% of the total weight of the required polyacrylic acid and add them to the slurry in step S2 respectively. Use a planetary mixer to stir at medium speed without vacuum for 50-60 minutes according to parameter b. S4: Weigh 40-50% of the total weight of the required deionized water and 40-50% of the total weight of the required polyacrylic acid and add them to the slurry in step S3. Use a planetary mixer to stir at high speed under vacuum for 60-90 minutes according to parameter c. S5: Weigh 30-50% of the total weight of the required deionized water and the total weight of the required N-methylpyrrolidone (NMP) and add them to the slurry in step S4. Use a planetary mixer to stir at high speed under vacuum for 60-90 minutes according to parameter d. S6: Weigh the required styrene-butadiene rubber and add it to the slurry prepared in step S5. Use a planetary mixer to vacuum stir at low speed for 20-30 minutes according to parameter e to obtain a silicon-carbon anode slurry for lithium-ion batteries with a solid content of 38-42%.
5. The preparation method according to claim 4, characterized in that, The parameter 'a' is: revolution 10-20 rpm, rotation 1000-1500 rpm; The parameter b is: revolution 20-30 rpm, rotation 2000-2500 rpm; The parameter c is: revolution 20-30 rpm, rotation 2500-3000 rpm; The parameter d is: revolution 20-30 rpm, rotation 2500-3000 rpm; The parameter e is: revolution 20-30 rpm, rotation 500-1000 rpm.
6. The preparation method according to claim 1, characterized in that, The negative electrode active material layer described in step 1) has a double-sided surface density of 95–105 g / m². 2 Preferably, it is 103 g / m 2 .
7. The preparation method according to claim 1, characterized in that, The slurry described in step 1) is filtered using a 180-220 mesh capsule filter before coating.
8. The preparation method according to claim 1, characterized in that, In step 2), the compaction ratio of the first rolling operation is 1.35–1.4 g / cm³. 3 The secondary roller compaction ratio is 1.52–1.62 g / cm³. 3 The baking temperature is 80-100℃.
9. A high-silicon-content negative electrode, characterized in that, The anode is prepared by the method according to any one of claims 1 to 8, wherein the silicon content is 25% to 35%; the cycle life of the anode is ≥500 cycles, and the capacity retention is ≥80%.
10. A lithium-ion battery, characterized in that, It includes the high silicon content negative electrode as described in claim 9.
Citation Information
Patent Citations
Preparation method of silicon-carbon negative electrode slurry and lithium ion battery thereof
CN111697194A
Negative electrode and preparation method thereof
CN118448586A