Bi / cnt composite functionalized zinc channel array electrode and preparation method and application thereof

By constructing a zinc trench array electrode with a Bi/CNT composite functional layer on the zinc substrate surface, the problems of zinc anode dendrite growth and hydrogen evolution side reaction are solved, achieving uniform zinc deposition and long-term electrode stability, which is suitable for large-scale energy storage systems.

CN123162148APending Publication Date: 2026-11-24TIANFU JIANGXI LAB
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611192441.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-07
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

In aqueous zinc metal batteries, uneven deposition of zinc ions in the zinc anode leads to dendrite growth and hydrogen evolution side reactions, affecting the battery's cycle life and stability.

Method used

Bi/CNT composite functionalized zinc trench array electrodes were fabricated by constructing a regular trench array on the surface of a zinc substrate and coating it with a Bi/CNT composite paste to form a Bi/CNT composite functional layer. By combining the high hydrogen evolution overpotential of bismuth nanosheets and the three-dimensional conductive network of carbon nanotubes, uniform zinc deposition and side reaction suppression were achieved.

Benefits of technology

It effectively suppresses dendrite growth and hydrogen evolution side reactions, ensures a dense and uniform zinc deposition layer, improves the structural integrity and interface stability of the electrode, extends battery cycle life, and is suitable for large-scale energy storage systems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123162148A_ABST
    Figure CN123162148A_ABST
Patent Text Reader

Abstract

This application provides a Bi / CNT composite functionalized zinc trench array electrode, its preparation method, and its application, belonging to the field of electrochemical energy storage technology. The method includes: constructing a trench array structure on the surface of a zinc substrate to provide a regular physical confinement space for newly generated zinc metal deposition during electrochemical cycling of the Bi / CNT / Zn composite electrode, thus confining the zinc deposition behavior within the trenches and preventing disordered lateral growth of zinc on the substrate surface; bismuth nanosheets in the Bi / CNT composite functional layer provide a high density of zinc-loving nucleation sites, inducing preferential nucleation and orderly deposition of zinc ions within the trenches; simultaneously, the inherently high hydrogen evolution overpotential of bismuth endows the Bi / CNT composite functional layer with the ability to suppress hydrogen evolution side reactions; a three-dimensional conductive network constructed from carbon nanotubes runs through the interior of the composite functional layer, ensuring rapid electron transport during the electrode reaction process, making it suitable for large-scale energy storage systems.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of electrochemical energy storage technology, specifically relating to a Bi / CNT composite functionalized zinc trench array electrode, its preparation method, and its application. Background Technology

[0002] Aqueous zinc-metal batteries have become an ideal choice for large-scale energy storage systems due to their high safety, environmental friendliness, and low cost. However, zinc anodes face significant bottlenecks in practical applications, such as severe dendrite growth and persistent parasitic side reactions (e.g., hydrogen evolution reaction, interfacial corrosion, and passivation), which severely limit the battery's cycle life. The root cause lies in the uneven deposition of zinc ions during charging and discharging, leading to localized electric field distortion, which in turn triggers rampant dendrite growth and even punctures the separator. Simultaneously, the free water molecules released during the desolvation of hydrated zinc ions can induce hydrogen evolution and interfacial corrosion. Therefore, enhancing the interfacial stability of the zinc anode in electrochemical reactions and effectively controlling deposition behavior are crucial for improving the overall performance of aqueous zinc-metal batteries.

[0003] Currently, modification strategies for zinc anodes mainly focus on constructing artificial interface layers or designing three-dimensional structural substrates. While these methods alleviate adverse side reactions to some extent by physically isolating water molecules or reducing local current density through a three-dimensional framework, they also have significant limitations. Therefore, there is an urgent need to develop a composite functionalized zinc anode that achieves uniform zinc deposition and suppresses dendrite growth and hydrogen evolution side reactions through the synergistic effect of a spatially confined structure and a zinc-loving conductive functional layer. Summary of the Invention

[0004] The present invention aims to solve at least one of the technical problems existing in the prior art or related art.

[0005] Therefore, a first aspect of the present invention provides a method for preparing a Bi / CNT composite functionalized zinc trench array electrode.

[0006] A second aspect of the present invention provides a Bi / CNT composite functionalized zinc trench array electrode.

[0007] In view of this, a method for fabricating a Bi / CNT composite functionalized zinc trench array electrode is proposed according to a first aspect of the embodiments of this application, comprising: Preparation of zinc substrates with trench array structures; Bismuth salts and carbon nanotubes were mixed in a liquid phase system to obtain a mixture. A reducing agent is added to the mixture to reduce bismuth ions to metallic bismuth, thereby obtaining Bi / CNT composite powder; Bi / CNT composite powder was redispersed in an organic solvent to obtain Bi / CNT composite slurry; Bi / CNT composite paste is coated onto the surface of the trench array structure, allowing the Bi / CNT composite paste to flow into the trenches. After drying, a Bi / CNT / Zn composite electrode is obtained.

[0008] In one feasible implementation, the preparation of a zinc substrate having a trench array structure includes the following steps: Zinc foil is rolled using a stainless steel mesh roller to create a regular groove array structure on the surface of the zinc foil. After cleaning with anhydrous ethanol, it is vacuum dried to obtain a zinc substrate. The trenches in the trench array structure have a width of 50μm to 60μm and a depth of 30μm to 40μm.

[0009] In one feasible implementation, the vacuum drying temperature is 60°C and the vacuum drying time is 2h to 4h.

[0010] In one feasible implementation, bismuth salt and carbon nanotubes are mixed in a liquid phase system to obtain a mixture, comprising the steps of: Dissolve bismuth nitrate pentahydrate in deionized water, add an appropriate amount of nitric acid to inhibit hydrolysis, and stir until homogeneous to obtain a bismuth salt solution. Hydroxylated multi-walled carbon nanotubes were added to a bismuth salt solution, stirred uniformly, and ultrasonically dispersed to obtain a mixture. The ultrasonic power for ultrasonic dispersion treatment is 400W to 600W.

[0011] In one feasible implementation, the concentration of bismuth nitrate pentahydrate is 5 mmol to 7 mmol to optimize the matching relationship between bismuth loading and zinc nucleation barrier.

[0012] In one feasible embodiment, a reducing agent is added to the mixture to reduce bismuth ions to metallic bismuth, obtaining Bi / CNT composite powder, comprising the steps of: Add sodium borohydride solution to the mixture, and Bi 3+ Reduced to metallic Bi nanoparticles; After the reaction was completed, the precipitate was centrifuged, washed thoroughly with deionized water and dried to obtain Bi / CNT composite powder; The centrifugation speed is 6000 rpm to 10000 rpm.

[0013] In one feasible embodiment, 5 mL of a 3 mol / L sodium borohydride aqueous solution is injected into the mixture, and the reduction reaction is carried out for 8 min to 10 min.

[0014] In one feasible embodiment, a Bi / CNT composite paste is coated onto the surface of a trench array structure, allowing the Bi / CNT composite paste to flow into the trenches. After drying, a Bi / CNT / Zn composite electrode is obtained, comprising the following steps: Bi / CNT composite slurry was coated on the surface of the trench array structure, and the Bi / CNT composite slurry flowed into the trench. The slurry was dried under vacuum at 60°C for 6 to 8 hours, and the loading of bismuth metal was controlled to be 80 wt% to 90 wt% to obtain the Bi / CNT / Zn composite electrode.

[0015] According to a second aspect of the embodiments of this application, a Bi / CNT composite functionalized zinc trench array electrode is provided, which is prepared by the preparation method of Bi / CNT composite functionalized zinc trench array electrode of any of the above-described technical solutions. The Bi / CNT composite functionalized zinc trench array electrode includes: Zinc substrate; A trench array structure is disposed on at least one surface of a zinc substrate; Bi / CNT composite functional layer, the Bi / CNT composite functional layer fills the trenches of the trench array structure and covers the surface of the zinc substrate; The Bi / CNT composite functional layer includes carbon nanotubes and bismuth nanosheets loaded on the surface of carbon nanotubes. The bismuth nanosheets are oriented with (012) crystal planes, and the bismuth nanosheets and carbon nanotubes form a three-dimensional conductive network.

[0016] According to a third aspect of the embodiments of this application, an aqueous zinc-iodine battery is provided, comprising a negative electrode, a positive electrode, a separator, and an electrolyte. The negative electrode is prepared by any of the above-described technical solutions using the Bi / CNT composite functionalized zinc trench array electrode preparation method.

[0017] The present application discloses a Bi / CNT composite functionalized zinc trench array electrode, its preparation method, and its application. Compared with the prior art, the advantages are as follows: In the preparation method of Bi / CNT (bismuth / carbon nanotube) composite functionalized zinc trench array electrode provided in the embodiments of this application, Bi / CNT composite slurry is coated on the surface of a zinc substrate with a regular trench array and the slurry is allowed to flow fully into the trench. After drying, a Bi / CNT / Zn (bismuth / carbon nanotube / zinc) composite electrode in which the Bi / CNT composite functional layer and the trench array structure are tightly bonded is obtained. By constructing a trench array structure on the zinc substrate surface, a regular physical confinement space is provided for the newly generated zinc metal deposition during the electrochemical cycling of the Bi / CNT / Zn composite electrode, constraining the zinc deposition behavior during electrochemical cycling within the trenches and avoiding the disordered lateral growth of zinc on the substrate surface. The bismuth nanosheets in the Bi / CNT composite functional layer provide a high density of zinc-loving nucleation sites, which can induce preferential nucleation and orderly deposition of zinc ions within the trenches. At the same time, the inherently high hydrogen evolution overpotential of bismuth endows the Bi / CNT composite functional layer with the ability to suppress hydrogen evolution side reactions. The three-dimensional conductive network constructed by carbon nanotubes runs through the interior of the composite functional layer, ensuring the rapid transport of electrons during the electrode reaction process. In the fabricated composite electrode, the Bi / CNT composite functional layer forms a tight bond with the inner wall of the trench, ensuring that the composite functional layer is not easily peeled off during long-term cycling. The physical confinement effect of the trench and the chemical guiding effect of the bismuth nanosheets work synergistically to effectively constrain the zinc deposition within the trench, resulting in a dense and uniform deposition layer, thus avoiding the short-circuit risk caused by dendrite protrusion. Simultaneously, the high hydrogen evolution overpotential of bismuth and the composite layer weaken the interfacial water activity, maintaining the stability of the electrode / electrolyte interface and effectively suppressing side reactions such as hydrogen evolution and corrosion. The structural integrity of the Bi / CNT composite functional layer, the dense and uniform zinc deposition layer, and the chemical stability of the reaction interface collectively ensure the overall reliability of the Bi / CNT / Zn composite electrode during long-term electrochemical cycling, providing a high-performance negative electrode solution for the practical application of aqueous zinc-based batteries, suitable for large-scale energy storage systems.

[0018] This application provides a zinc anode based on Bi / CNT composite material and trench array regulation. Through the dual regulation mechanism of spatial structure confinement and zinc-loving multifunctional coating, the adsorption energy of water molecules is weakened (-0.14eV), which effectively suppresses water-induced hydrogen evolution side reaction and interface corrosion.

[0019] The Bi / CNT coating prepared in this application exhibits extremely low hydrogen evolution overpotential and excellent charge transfer capability (charge transfer resistance as low as 20.1 Ω in the high-frequency region), enabling it to guide zinc preferential growth along the thermodynamically favorable (002) crystal plane at 1.0 mA·cm⁻¹. -2 The nucleation overpotential at the current density is only 5.8 mV.

[0020] The Bi / CNT / Zn composite electrode prepared in this application operates at 1 mA·cm⁻¹. -2 / 1mAh·cm -2 Under these conditions, the symmetrical cell can cycle stably for over 3000 hours with a voltage polarization of only 22 mV. A full cell assembled with an I2 / NC cathode can achieve this at 5 A·g... -1 After 20,000 cycles at high current density, the capacity retention rate is as high as 87.7%, and the coulombic efficiency is close to the ideal 99.7%. Attached Figure Description

[0021] Various other advantages and benefits will become apparent to those skilled in the art upon reading the following detailed description of preferred embodiments. The accompanying drawings are for illustrative purposes only and are not intended to limit the scope of this application. Furthermore, the same reference numerals denote the same parts throughout the drawings. In the drawings: Figure 1 A schematic flowchart illustrating the steps of a method for fabricating a Bi / CNT composite functionalized zinc trench array electrode according to an embodiment of this application; Figure 2 A schematic structural diagram of a Bi / CNT composite functionalized zinc trench array electrode according to an embodiment of this application; Figure 3 These are comparison images of the X-ray diffraction patterns of the products prepared in Examples 1-3 of this application; Figure 4 Scanning electron microscope image and corresponding elemental distribution energy spectrum of the Bi / CNT / Zn composite electrode surface prepared in Example 1 of this application; Figure 5 The AC impedance spectra of each group of symmetrical cells in Example 6 of this application and their values ​​at 1 mA·cm⁻¹ -2 Comparison of long-cycle performance at current density; Figure 6 This is a comparison diagram of the surface morphology evolution of electrodes prepared in Examples 1 and 5 of this application at different deposition times; Figure 7 For the zinc-iodine full cell constructed based on the electrodes prepared in Examples 1 and 5 of this application, at 1 A·g -1 Comparison curves of long-cycle performance under current density. Detailed Implementation

[0022] In the description of this application, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "upper", "lower", "front", "rear", "left", "right", "vertical", "horizontal", "top", "bottom", "inner", "outer", "clockwise", "counterclockwise", etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are used only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this application.

[0023] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of that feature. In the description of this application, "multiple" means two or more, unless otherwise explicitly specified.

[0024] In this application, unless otherwise expressly specified and limited, the terms "installation," "connection," "linking," and "fixing," etc., should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; and they can refer to the internal connection between two components. Those skilled in the art can understand the specific meaning of the above terms in this application according to the specific circumstances.

[0025] The preferred embodiments of this application are described below with reference to the accompanying drawings. It should be understood that the preferred embodiments described herein are for illustration and explanation only and are not intended to limit this application.

[0026] like Figure 1 As shown, according to a first aspect of the embodiments of this application, a method for fabricating a Bi / CNT composite functionalized zinc trench array electrode is proposed, comprising: Step 100: Prepare a zinc substrate with a trench array structure; Step 200: Mix bismuth salt and carbon nanotubes in a liquid phase system to obtain a mixed solution; Step 300: Add a reducing agent to the mixture to reduce bismuth ions to metallic bismuth and obtain Bi / CNT composite powder; Step 400: Redisperse the Bi / CNT composite powder in an organic solvent to obtain a Bi / CNT composite slurry; Step 500: Coat the surface of the trench array structure with Bi / CNT composite paste, allowing the Bi / CNT composite paste to flow into the trenches. After drying, obtain the Bi / CNT / Zn composite electrode.

[0027] In the preparation method of Bi / CNT (bismuth / carbon nanotube) composite functionalized zinc trench array electrode provided in the embodiments of this application, Bi / CNT composite slurry is coated on the surface of a zinc substrate with a regular trench array and the slurry is allowed to flow fully into the trench. After drying, a Bi / CNT / Zn (bismuth / carbon nanotube / zinc) composite electrode in which the Bi / CNT composite functional layer and the trench array structure are tightly bonded is obtained. By constructing a trench array structure on the zinc substrate surface, a regular physical confinement space is provided for the newly generated zinc metal deposition during the electrochemical cycling of the Bi / CNT / Zn composite electrode, constraining the zinc deposition behavior during electrochemical cycling within the trenches and avoiding the disordered lateral growth of zinc on the substrate surface. The bismuth nanosheets in the Bi / CNT composite functional layer provide a high density of zinc-loving nucleation sites, which can induce preferential nucleation and orderly deposition of zinc ions within the trenches. At the same time, the inherently high hydrogen evolution overpotential of bismuth endows the Bi / CNT composite functional layer with the ability to suppress hydrogen evolution side reactions. The three-dimensional conductive network constructed by carbon nanotubes runs through the interior of the composite functional layer, ensuring the rapid transport of electrons during the electrode reaction process. In the fabricated composite electrode, the Bi / CNT composite functional layer forms a tight bond with the inner wall of the trench, ensuring that the composite functional layer is not easily peeled off during long-term cycling. The physical confinement effect of the trench and the chemical guiding effect of the bismuth nanosheets work synergistically to effectively constrain the zinc deposition within the trench, resulting in a dense and uniform deposition layer, thus avoiding the short-circuit risk caused by dendrite protrusion. Simultaneously, the high hydrogen evolution overpotential of bismuth and the composite layer weaken the interfacial water activity, maintaining the stability of the electrode / electrolyte interface and effectively suppressing side reactions such as hydrogen evolution and corrosion. The structural integrity of the Bi / CNT composite functional layer, the dense and uniform zinc deposition layer, and the chemical stability of the reaction interface collectively ensure the overall reliability of the Bi / CNT / Zn composite electrode during long-term electrochemical cycling, providing a high-performance negative electrode solution for the practical application of aqueous zinc-based batteries, suitable for large-scale energy storage systems.

[0028] The inventors discovered that existing two-dimensional thin-film coatings are prone to stress concentration due to zinc volume fluctuations during long-term cycling, leading to interfacial layer peeling or cracking. While traditional three-dimensional porous frameworks can disperse the electric field, they lack in-situ zinc-loving guiding sites, causing zinc ions to still easily deposit randomly at the top or outer edges of the pores, making it difficult to simultaneously achieve efficient ion transport kinetics and long-term mechanical stability. The synergistic engineering of spatial structure confinement and zinc-loving multifunctional coatings is an effective way to solve the above problems. Bismuth (Bi), a semi-metallic compound, not only significantly suppresses hydrogen evolution side reactions due to its inherently high hydrogen evolution overpotential, but also interacts strongly with zinc (Zn), providing abundant zinc-loving sites for uniform nucleation of zinc ions. The three-dimensional conductive carbon nanotube (CNT) network provides a rapid charge transfer channel and significantly enhances the mechanical toughness of the interfacial layer. Through the excellent zinc affinity of Bi and the rapid charge transport capability of the CNT three-dimensional conductive network, combined with the physical confinement effect of the trench array structure, the zinc nucleation energy barrier is effectively reduced, inducing uniform zinc deposition, while significantly suppressing dendrite growth and hydrogen evolution side reactions. This application combines a Bi / CNT composite system with a trench array zinc substrate having regular physical microchannels, enabling spatial confinement at the microscale. This topology can homogenize local ion flux, making full use of the trench space to guide Zn during charging. 2+ The zinc is preferentially reduced to zinc metal inside the trench (rather than on the top or sidewalls), and the zinc deposition is dense and uniform without dendrite formation. Simultaneously, the high hydrogen evolution overpotential of bismuth in the Bi / CNT composite functional layer effectively weakens the adsorption activity of water molecules, suppressing hydrogen evolution side reactions and interfacial corrosion. The synergistic effect of these two factors ensures the structural integrity and interfacial stability of the electrode during long-term cycling.

[0029] like Figure 2 As shown, in one feasible embodiment, the preparation of a zinc substrate with a trench array structure includes the following steps: Zinc foil is rolled using a 60-mesh stainless steel mesh roller to create a regular groove array structure on the surface of the zinc foil. After cleaning with anhydrous ethanol, it is vacuum dried to obtain a zinc substrate. The trenches in the trench array structure have a width of 50μm to 60μm and a depth of 30μm to 40μm.

[0030] In this technical solution, zinc foil is pre-treated by rolling with a 60-mesh stainless steel mesh roller, followed by cleaning with anhydrous ethanol and vacuum drying. This results in a zinc substrate with a clean surface and regular trench array, with a trench width of 50μm to 60μm and a depth of 30μm to 40μm, providing a structural basis for subsequent slurry coating. The trench array structure has a regular micron-level physical confinement space, which can constrain the subsequent zinc deposition behavior within the trenches, avoiding disordered lateral growth of zinc on the substrate surface. The trench structure also increases the specific surface area of ​​the zinc substrate, which helps to reduce the local current density, further homogenize the zinc ion flux, and avoid preferential dendrite nucleation caused by the tip effect. At the same time, the inner wall of the trench provides sufficient anchoring area for the subsequent filling of Bi / CNT slurry, ensuring that the Bi / CNT functional layer formed after drying can be tightly bonded to the zinc substrate, avoiding interface layer peeling or cracking caused by zinc volume fluctuations during long-term cycling.

[0031] In one feasible implementation, the vacuum drying temperature is 60°C and the vacuum drying time is 2h to 4h.

[0032] In this technical solution, by controlling the vacuum drying temperature at 60℃ and the drying time at 2h to 4h, the residual ethanol cleaning solvent on the zinc substrate surface is effectively removed under mild conditions. The drying temperature of 60℃ can quickly evaporate the residual solvent while avoiding oxidation or abnormal grain growth on the zinc substrate surface that may be caused by excessively high temperatures. The drying time of 2h to 4h ensures that the residual solvent inside the zinc substrate and deep in the trenches is fully removed, ensuring the cleanliness and chemical activity of the zinc substrate surface. This provides a clean and chemically active interface for the subsequent formation of a strong bond between the Bi / CNT composite slurry and the zinc substrate, ensuring the bonding strength and long-term cycling stability between the functional layer and the substrate in the prepared composite electrode.

[0033] In one feasible implementation, bismuth salt and carbon nanotubes are mixed in a liquid phase system to obtain a mixture, comprising the steps of: Dissolve bismuth nitrate pentahydrate in deionized water, add an appropriate amount of nitric acid to inhibit hydrolysis, and stir until homogeneous to obtain a bismuth salt solution. Hydroxylated multi-walled carbon nanotubes were added to a bismuth salt solution, stirred uniformly, and ultrasonically dispersed to obtain a mixture. The ultrasonic power for ultrasonic dispersion treatment is 400W to 600W.

[0034] In this technical solution, bismuth nitrate pentahydrate is dissolved in deionized water and an appropriate amount of nitric acid is added dropwise to inhibit Bi. 3+ Hydrolysis, combined with high-power ultrasonic dispersion treatment of 400W~600W, achieved Bi 3+ Uniform mixing of salt and hydroxylated multi-walled carbon nanotubes in a liquid phase system. The addition of nitric acid inhibited the Bi...3+ Hydrolysis and precipitation in aqueous solution ensures the stability of bismuth ion concentration in the solution, providing a homogeneous reaction system for subsequent reduction reactions; the oxygen-containing functional groups on the surface of hydroxylated multi-walled carbon nanotubes can react with Bi in the solution. 3+ Coordination or electrostatic adsorption occurs, providing preferential nucleation sites for the uniform anchoring of Bi nanoparticles; high-power ultrasound of 400W–600W not only promotes the full dispersion of carbon nanotubes in the liquid phase, overcoming the technical challenge of easy aggregation of carbon nanotubes, but also enables Bi... 3+ It can be uniformly adsorbed on the surface of carbon nanotubes, ensuring the uniform composite of the two components at the microscale in the final Bi / CNT composite product.

[0035] In one feasible implementation, the concentration of bismuth nitrate pentahydrate is 5 mmol to 7 mmol to optimize the matching relationship between bismuth loading and zinc nucleation barrier.

[0036] In this technical solution, the matching relationship between bismuth loading and zinc nucleation barrier is optimized by controlling the concentration of bismuth pentahydrate nitrate within the range of 5 mmol to 7 mmol. Controlling the concentration of bismuth pentahydrate nitrate within the range of 5 mmol to 7 mmol ensures a balance between the density of zinc-loving sites and the integrity of the conductive network in the Bi / CNT composite coating, thereby effectively inducing the deposition of newly generated zinc metal along the thermodynamically favorable (002) crystal plane orientation during electrochemical cycling.

[0037] It should be noted that if the bismuth salt concentration is below 5 mmol, the loading of bismuth nanosheets in the Bi / CNT composite coating is insufficient, making it difficult to provide enough zinc-loving sites to guide the uniform nucleation of zinc. Zinc still tends to deposit randomly on the exposed zinc substrate surface. If the bismuth salt concentration is above 7 mmol, the insulating bismuth component in the Bi / CNT composite coating is excessive, which may hinder the charge transfer efficiency of the three-dimensional conductive network to some extent, and instead increase the polarization of the electrode.

[0038] In one feasible embodiment, a reducing agent is added to the mixture to reduce bismuth ions to metallic bismuth, obtaining Bi / CNT composite powder, comprising the steps of: Add sodium borohydride solution to the mixture, and Bi 3+ Reduced to metallic Bi nanoparticles; After the reaction was completed, the precipitate was centrifuged, washed thoroughly with deionized water and dried to obtain Bi / CNT composite powder; The centrifugation speed is 6000 rpm to 10000 rpm.

[0039] In this technical solution, sodium borohydride, as a strong reducing agent, can rapidly reduce Bi at room temperature. 3+The reduction to zero-valent bismuth was carried out under mild conditions and with a controllable reaction rate. High-speed centrifugation effectively removed reaction byproducts and unreacted impurity ions, resulting in a pure and uniformly sized Bi / CNT composite powder, thus avoiding the adverse effects of impurities on the subsequent electrochemical performance of the electrode. The prepared Bi nanosheets were uniformly anchored to the surface of carbon nanotubes with a (012) crystal plane orientation, constructing a continuous three-dimensional conductive network. The interface between the Bi nanosheets and carbon nanotubes in the Bi / CNT composite powder was strong, and the active sites were fully exposed, providing high-quality functional materials for subsequent slurry coating and composite electrode construction. This ensured the rapid charge transfer capability of the composite electrode and provided abundant zinc ion adsorption sites.

[0040] In one feasible embodiment, 5 mL of a 3 mol / L sodium borohydride aqueous solution is injected into the mixture, and the reduction reaction is carried out for 8 min to 10 min.

[0041] In this technical solution, by injecting 5 mL of a 3 mol / L sodium borohydride aqueous solution into the mixture and controlling the reduction reaction time to be 8 min to 10 min, the prepared metallic Bi nanoparticles have uniform particle size and no excessive growth. They can be uniformly anchored on the surface of carbon nanotubes with (012) crystal plane orientation, avoiding Bi nanoparticles caused by insufficient reduction. 3+ The agglomeration and growth of nanoparticles caused by excessive residual or reduction time ensures the uniform dispersion and structural consistency of active components in the Bi / CNT composite functional layer.

[0042] In one feasible embodiment, a Bi / CNT composite paste is coated onto the surface of a trench array structure, allowing the Bi / CNT composite paste to flow into the trenches. After drying, a Bi / CNT / Zn composite electrode is obtained, comprising the following steps: Bi / CNT composite slurry was coated on the surface of the trench array structure, and the Bi / CNT composite slurry flowed into the trench. The slurry was dried under vacuum at 60°C for 6 to 8 hours, and the loading of bismuth metal was controlled to be 80 wt% to 90 wt% to obtain the Bi / CNT / Zn composite electrode.

[0043] In this technical solution, a composite electrode in which the Bi / CNT composite functional layer is uniformly and densely filled inside the trench is prepared by uniformly coating the surface of the trench array with Bi / CNT composite slurry and controlling the bismuth loading to 80wt%–90wt%, followed by vacuum drying at 60℃ for 6–8 hours. The 80wt%–90wt% loading range ensures sufficient supply of Bi zinc-affinity sites to effectively reduce nucleation overpotential, while avoiding excessive bismuth from covering and blocking the three-dimensional conductive network of carbon nanotubes. This ensures that the Bi / CNT composite functional layer possesses both excellent zinc affinity and efficient charge transfer capability. At the same time, a tightly bonded interface is formed between the composite functional layer and the inner wall of the trench, constructing a continuous, high-strength interface protective layer with rapid charge transfer capability. This effectively avoids interface peeling or cracking caused by zinc volume fluctuations during long-term cycling, ensuring the structural integrity and interface stability of the electrode during ultra-long cycling.

[0044] like Figure 2 As shown, according to the second aspect of this application, a Bi / CNT composite functionalized zinc trench array electrode is proposed, which is prepared by the preparation method of Bi / CNT composite functionalized zinc trench array electrode of any of the above technical solutions. The Bi / CNT composite functionalized zinc trench array electrode includes: a zinc substrate, a trench array structure and a Bi / CNT composite functional layer; the trench array structure is disposed on at least one surface of the zinc substrate; the Bi / CNT composite functional layer fills the trenches of the trench array structure and covers the surface of the zinc substrate; the Bi / CNT composite functional layer includes carbon nanotubes and bismuth nanosheets loaded on the surface of carbon nanotubes, the bismuth nanosheets are (012) crystal plane oriented, and the bismuth nanosheets and carbon nanotubes form a three-dimensional conductive network.

[0045] The Bi / CNT composite functionalized zinc trench array electrode provided in this application has a periodic trench physical confinement structure and a Bi / CNT zinc-loving conductive functional layer. Through the synergistic effect of spatial confinement engineering and the zinc-loving interface, precise control of zinc deposition behavior is achieved. The periodic trench array on the zinc substrate surface constitutes a regular physical confinement space at the microscale, effectively constraining the zinc deposition process and preventing the disordered lateral spread of zinc on the substrate surface. Simultaneously, the presence of the trench array increases the effective surface area of ​​the electrode, helping to disperse local ion concentration and suppressing dendrite preferential nucleation caused by the tip effect. The Bi / CNT composite functional layer on the inner wall of the trench provides sufficient adhesion area, ensuring a tight bond between the Bi / CNT composite functional layer and the zinc substrate, avoiding interface layer peeling or cracking caused by zinc volume fluctuations during long-term cycling. In the Bi / CNT composite functional layer, Bi nanosheets are uniformly anchored to the carbon nanotube surface with a (012) crystal plane orientation, forming a three-dimensional conductive network with a high specific surface area. The specific crystal orientation of Bi nanosheets enables them to serve as preferential nucleation sites, strongly adsorbing zinc ions and effectively reducing the nucleation overpotential of zinc. This guides zinc ions to preferentially deposit at high density from bottom to top within the trenches. Simultaneously, the inherently high hydrogen evolution overpotential of bismuth endows the composite layer with excellent hydrogen evolution suppression capabilities, effectively weakening the adsorption activity of water molecules on the electrode surface and reducing the risk of water-induced hydrogen evolution side reactions and interfacial corrosion. The three-dimensional conductive network constructed by carbon nanotubes ensures rapid electron transport within the Bi / CNT composite functional layer, effectively reducing the charge transfer impedance of the electrode and guaranteeing charge transfer efficiency during the electrode reaction process. The composite structure formed by physical confinement, high-density zinc-loving nucleation sites provided by bismuth nanosheets, chemical guidance, and a three-dimensional conductive network constructed by carbon nanotubes effectively confines the zinc deposition behavior in the electrode within the trench, thereby ensuring a dense and uniform deposition layer without dendrite protrusion. At the same time, the electrode / electrolyte interface remains stable, and side reactions such as hydrogen evolution and corrosion are significantly suppressed. This ensures the structural integrity and interfacial stability of the electrode during long-term electrochemical cycling, providing a high-performance anode solution with excellent durability for aqueous zinc-based batteries.

[0046] The Bi / CNT composite functionalized zinc trench array electrode provided in this application embodiment is prepared by the preparation method of Bi / CNT composite functionalized zinc trench array electrode of any of the above technical solutions. Therefore, the Bi / CNT composite functionalized zinc trench array electrode has all the beneficial effects of the preparation method of Bi / CNT composite functionalized zinc trench array electrode of the above technical solutions, and will not be elaborated here.

[0047] According to a third aspect of this application, an aqueous zinc-iodine battery is proposed, comprising a negative electrode, a positive electrode, a separator, and an electrolyte, wherein the negative electrode is prepared by any of the above-mentioned technical solutions using the preparation method of Bi / CNT composite functionalized zinc trench array electrode.

[0048] The aqueous zinc-iodine battery provided in this application embodiment has all the beneficial effects of the Bi / CNT composite functionalized zinc trench array electrode preparation method of the above-mentioned technical solutions because the negative electrode of the aqueous zinc-iodine battery is prepared by the preparation method of the Bi / CNT composite functionalized zinc trench array electrode of any of the above-mentioned technical solutions, and will not be elaborated here.

[0049] Example 1 (Best Solution): This embodiment provides a Bi / CNT composite functionalized zinc trench array electrode and its preparation method: Weigh 2.91g of bismuth nitrate crystals and dissolve them in 20mL of deionized water. Add a few drops of nitric acid to inhibit hydrolysis and stir until homogeneous to obtain a bismuth salt solution. 0.1 g of hydroxylated multi-walled carbon nanotubes were added to a bismuth salt solution and ultrasonically dispersed to obtain a uniform mixture. Add 5 mL of 3 mol / L NaBH4 solution to the mixture, and then add Bi... 3+ The reaction product was reduced to metallic Bi; the product was centrifuged, washed thoroughly with deionized water, and then dried at 60°C to obtain Bi / CNT composite powder. A groove array zinc foil with a groove width of approximately 60 μm and a depth of approximately 40 μm was prepared by rolling a pure zinc foil surface with a 60-mesh stainless steel roller. Bi / CNT composite powder was ultrasonically dispersed in anhydrous ethanol to form a Bi / CNT composite slurry. The Bi / CNT composite slurry was uniformly coated and filled into the surface grooves of the groove array zinc foil by brushing. It was then vacuum dried at 60°C and cut into 10 mm diameter discs to obtain the Bi / CNT / Zn composite electrode.

[0050] Example 2: This embodiment provides a comparative electrode lacking a CNT conductive network and its preparation method: Weigh 2.91g of bismuth nitrate crystals and dissolve them in 20mL of deionized water. Add a few drops of nitric acid to inhibit hydrolysis and stir until homogeneous to obtain a bismuth salt solution. Add 5 mL of 3 mol / L NaBH4 solution directly to Bi 3+ Reduced to metallic Bi; centrifuge the reaction product, wash thoroughly with deionized water, dry at 60°C and disperse in anhydrous ethanol to form pure Bi slurry; A groove array zinc foil with a groove width of approximately 60 μm and a depth of approximately 40 μm was prepared by rolling a pure zinc foil surface with a 60-mesh stainless steel roller. Pure Bi slurry was brushed onto the surface of grooved zinc foil pretreated with a 60-mesh stainless steel roller, dried under vacuum at 60°C, and then cut to obtain Bi / Zn electrodes.

[0051] Example 3: This embodiment provides a comparative electrode lacking zinc-loving Bi sites and its preparation method: Weigh 0.1g of hydroxylated multi-walled carbon nanotubes and ultrasonically disperse them in anhydrous ethanol to form a pure CNT slurry; Pure CNT slurry was brushed onto the surface of grooved array zinc foil pretreated with a 60-mesh stainless steel roller, dried under vacuum at 60°C, and then cut to obtain a CNT / Zn (carbon nanotube / zinc) electrode.

[0052] Example 4: This embodiment provides a comparative electrode with only a physical trench structure and its preparation method: A groove array zinc foil with a groove width of approximately 60 μm and a depth of approximately 40 μm was prepared by rolling a pure zinc foil surface with a 60-mesh stainless steel roller. The zinc foil is not coated with any composite materials and is directly cut into 10mm diameter discs to obtain MeshZn electrodes.

[0053] Example 5: This embodiment provides a blank control electrode: Commercially available pure zinc foil, without any mechanical rolling or surface coating, is directly cut into the appropriate size to serve as BareZn (raw zinc) electrodes.

[0054] Example 6: Using the optimal electrode prepared in Example 1 and the comparative electrodes prepared in Examples 2-5 as negative electrode materials, zinc symmetric cells and zinc-iodine full cells were prepared, respectively. The specific steps are as follows: Symmetrical battery assembly: In the CR2032 button cell case, the negative electrode case, the electrode to be tested prepared above (such as Bi / CNT / Zn), the Whatman glass fiber diaphragm, the same electrode to be tested, the gasket, the spring and the positive electrode case are placed in sequence. 120 μL of 2 mol / L ZnSO4 aqueous solution is added as electrolyte and then sealed and pressed. Full battery assembly: Preparation of I2 / NC composite cathode: Iodine and nitrogen-doped porous carbon were mixed in a certain proportion and heated at 90℃ for 4 hours. Then, acetylene black and PVDF (polyvinylidene fluoride) were mixed in a mass ratio of 7:2:1. The mixture was prepared into a slurry using NMP (N-methylpyrrolidone) as a solvent and coated onto titanium foil. The foil was cut into pieces with a diameter of 10 mm and a surface loading of 2.3 mg / cm². -2 The negative electrode shell, the negative electrode to be tested, the separator, the I2 / NC composite positive electrode, the gasket, the spring sheet, and the positive electrode shell are placed in sequence in the battery case. 120 μL of 2 mol / L ZnSO4 (zinc sulfate) electrolyte is added, and the battery is sealed and crimped to assemble a full cell for electrochemical testing.

[0055] The test results are as follows: The products obtained in Examples 1-3 were characterized by XRD, and the results are as follows: Figure 3 As shown, Examples 2 and 3 exhibit characteristic diffraction peaks of pure metallic bismuth and carbon nanotubes, respectively; Example 1 contains characteristic peaks of both and no impurity phase was detected, indicating that Bi nanosheets and CNT (carbon nanotube) matrix have been successfully and uniformly composited.

[0056] Figure 4 Scanning electron microscopy and EDS spectroscopy showed that the Bi / CNT composite material prepared in Example 1 was uniformly and densely filled in a groove about 60 μm wide, with C and Bi elements having a highly consistent distribution, thus constructing a continuous and high-strength interface structure.

[0057] like Figure 5 As shown, at 1 mA·cm -2 1mAh·cm -2 Under the test conditions, the symmetric cell constructed from the Bi / CNT / Zn composite electrode prepared in Example 1 exhibited excellent cycle stability, capable of stable cycling for over 3000 hours without short circuit, and the voltage polarization remained at an extremely low level (approximately 22 mV). In contrast, the comparative electrode, lacking the synergistic protection of the Bi / CNT coating and trench structure, experienced severe voltage fluctuations and short circuit failure within 500 hours of cycling, demonstrating the crucial role of the Bi / CNT composite structure in suppressing dendrites and maintaining interface stability.

[0058] Figure 6 The morphology of the electrode surface at different deposition times was observed. The results showed that, compared with the uncontrolled dendrite growth on the surface of Example 5 (BareZn), Example 1 (Bi / CNT / Zn) successfully guided the uniform deposition of zinc from bottom to top in the trench without dendrite protrusion.

[0059] Figure 7 The results of long-cycle performance tests for the zinc-iodine full cell assembled in Example 6 are as follows: The full cell based on the Bi / CNT / Zn electrode prepared in Example 1 at 1 A·g -1After undergoing 30,000 cycles at a current density, the specific capacity remained at 132.1 mAh·g. -1 .

[0060] It will be readily understood by those skilled in the art that the above embodiments can be freely combined and superimposed without conflict.

[0061] The above are merely preferred embodiments of this application and are not intended to limit this application. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of this application should be included within the protection scope of this application. The above are merely preferred embodiments of this application. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the technical principles of this application, and these improvements and modifications should also be considered within the protection scope of this application.

Claims

1. A method for preparing a Bi / CNT composite functionalized zinc trench array electrode, characterized in that, The method for preparing the Bi / CNT composite functionalized zinc trench array electrode includes: Preparation of zinc substrates with trench array structures; Bismuth salts and carbon nanotubes were mixed in a liquid phase system to obtain a mixture. A reducing agent is added to the mixture to reduce bismuth ions to metallic bismuth, thereby obtaining Bi / CNT composite powder; The Bi / CNT composite powder was redispersed in an organic solvent to obtain a Bi / CNT composite slurry; The Bi / CNT composite slurry is coated onto the surface of the trench array structure, allowing the Bi / CNT composite slurry to flow into the trenches. After drying, a Bi / CNT / Zn composite electrode is obtained.

2. The method for preparing a Bi / CNT composite functionalized zinc trench array electrode according to claim 1, characterized in that, The preparation of the zinc substrate with the trench array structure includes the following steps: The zinc foil is rolled using a stainless steel mesh roller to construct a regular groove array structure on the surface of the zinc foil. After cleaning with anhydrous ethanol, it is vacuum dried to obtain the zinc substrate. The trenches in the trench array structure have a width of 50μm to 60μm and a depth of 30μm to 40μm.

3. The method for preparing a Bi / CNT composite functionalized zinc trench array electrode according to claim 2, characterized in that, The vacuum drying temperature is 60°C, and the vacuum drying time is 2 to 4 hours.

4. The method for preparing a Bi / CNT composite functionalized zinc trench array electrode according to claim 1, characterized in that, The method of mixing bismuth salt and carbon nanotubes in a liquid phase system to obtain a mixed solution includes the following steps: Dissolve bismuth nitrate pentahydrate in deionized water, add an appropriate amount of nitric acid to inhibit hydrolysis, and stir until homogeneous to obtain a bismuth salt solution. Hydroxylated multi-walled carbon nanotubes were added to the bismuth salt solution, and the mixture was stirred uniformly and ultrasonically dispersed to obtain the mixture. The ultrasonic power of the ultrasonic dispersion process is 400W to 600W.

5. The method for preparing a Bi / CNT composite functionalized zinc trench array electrode according to claim 4, characterized in that, The concentration of bismuth nitrate pentahydrate was 5 mmol to 7 mmol to optimize the matching relationship between bismuth loading and zinc nucleation barrier.

6. The method for preparing a Bi / CNT composite functionalized zinc trench array electrode according to claim 4, characterized in that, The method of adding a reducing agent to the mixture to reduce bismuth ions to metallic bismuth and obtain Bi / CNT composite powder includes the following steps: Add sodium borohydride solution to the mixture, and Bi 3+ Reduced to metallic Bi nanoparticles; After the reaction was completed, the precipitate was centrifuged, washed thoroughly with deionized water and dried to obtain the Bi / CNT composite powder. The centrifugation speed is 6000 rpm to 10000 rpm.

7. The method for preparing a Bi / CNT composite functionalized zinc trench array electrode according to claim 6, characterized in that, Add 5 mL of a 3 mol / L sodium borohydride aqueous solution to the mixture and allow the reduction reaction to proceed for 8 to 10 minutes.

8. The method for preparing a Bi / CNT composite functionalized zinc trench array electrode according to claim 1, characterized in that, The method of coating the Bi / CNT composite slurry onto the surface of the trench array structure, allowing the Bi / CNT composite slurry to flow into the trenches, and then drying it to obtain a Bi / CNT / Zn composite electrode includes the following steps: The Bi / CNT composite slurry is coated on the surface of the trench array structure, and the Bi / CNT composite slurry flows into the trench. It is dried under vacuum at 60°C for 6 to 8 hours, and the loading of metallic bismuth is controlled to be 80 wt% to 90 wt%, to obtain the Bi / CNT / Zn composite electrode.

9. A Bi / CNT composite functionalized zinc trench array electrode, characterized in that, The Bi / CNT composite functionalized zinc trench array electrode is prepared by the method described in any one of claims 1 to 8, wherein the Bi / CNT composite functionalized zinc trench array electrode comprises: Zinc substrate; A trench array structure, wherein the trench array structure is disposed on at least one surface of the zinc substrate; Bi / CNT composite functional layer, wherein the Bi / CNT composite functional layer fills the trenches of the trench array structure and covers the surface of the zinc substrate; The Bi / CNT composite functional layer includes carbon nanotubes and bismuth nanosheets loaded on the surface of the carbon nanotubes. The bismuth nanosheets are oriented with (012) crystal planes, and the bismuth nanosheets and the carbon nanotubes form a three-dimensional conductive network.

10. An aqueous zinc-iodine battery, comprising a negative electrode, a positive electrode, a separator, and an electrolyte, characterized in that, The negative electrode is prepared by the method for preparing Bi / CNT composite functionalized zinc trench array electrode according to any one of claims 1 to 8.