Secondary battery and electric device

CN123162149APending Publication Date: 2026-11-24CATL (JIANGSU) NEW ENERGY TECHNOLOGY CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510622999.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-14
Publication Date
2026-11-24

Smart Images

  • Figure CN123162149A_ABST
    Figure CN123162149A_ABST
Patent Text Reader

Abstract

This application belongs to the field of battery technology, specifically disclosing a secondary battery and an electrical device. The secondary battery includes a positive electrode, a negative electrode, and a separator disposed between the positive and negative electrodes. The positive electrode includes positive electrode particles, which include lithium manganese iron phosphate. The lithium manganese iron phosphate comprises secondary particles composed of multiple primary particles, and the positive electrode particles include nanocrystalline lithium metal salts located at at least a portion of the interfaces between the primary particles. The nanocrystalline lithium metal salts include lithium, oxalic group elements, and other elements. The other elements include any two or more of phosphorus, aluminum, titanium, zirconium, hafnium, niobium, tantalum, tin, scandium, germanium, and lanthanides. This secondary battery possesses stable electrochemical performance, such as long cycle life and good high-temperature storage performance, while improving the specific capacity of the positive electrode active material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of batteries, specifically to a secondary battery and an electrical device. Background Technology

[0002] Secondary batteries are widely used in various consumer electronics and electric vehicles due to their outstanding characteristics such as light weight, no pollution, and no memory effect. Among them, lithium-ion batteries have a very wide range of applications in portable electronic devices and electric vehicles.

[0003] As the application of rechargeable batteries becomes more and more widespread, the requirements for battery performance are also becoming higher and higher. Summary of the Invention

[0004] In view of the above problems, this application provides a secondary battery and an electrical device, which has stable electrochemical performance, such as long cycle life and good high-temperature storage performance, based on improving the specific capacity of the positive electrode active material.

[0005] In a first aspect, this application provides a secondary battery, which includes a positive electrode, a negative electrode, and a separator disposed between the positive electrode and the negative electrode.

[0006] The positive electrode includes positive electrode particles, which include lithium manganese iron phosphate, which includes secondary particles composed of a plurality of primary particles, and the positive electrode particles include nanocrystalline lithium metal salt, which is located at at least a portion of the interface between the primary particles.

[0007] The aforementioned nanocrystalline metallic lithium salts include lithium, oxalic group elements, and other elements, including any two or more of phosphorus, aluminum, titanium, zirconium, hafnium, niobium, tantalum, tin, scandium, germanium, and lanthanides.

[0008] The nanocrystalline lithium metal salt of this application has the function of conducting lithium ions. It is located at at least part of the interface of the primary particles of lithium manganese iron phosphate. By constructing a robust and unobstructed lithium ion transport pathway, it facilitates the effective utilization of the specific capacity of the positive electrode active material and enables the secondary battery to have stable electrochemical performance, such as long cycle life and good high-temperature storage performance.

[0009] In some embodiments, based on the total mass of the cathode particles, the mass percentage content of the nanocrystalline lithium metal salt located between the primary particles is 0.3% to 20%.

[0010] and / or;

[0011] The volumetric particle size distribution Dv50 of the aforementioned nanocrystalline lithium metal salt located between the primary particles is 1 nm to 200 nm.

[0012] In some embodiments, the cathode particles have a coating layer disposed on at least a portion of the surface of the lithium manganese iron phosphate, the coating layer comprising a nanocrystalline lithium metal salt.

[0013] In these embodiments, this application discloses that the nanocrystalline lithium salt in the coating layer is beneficial for further improving the ionic conductivity of the cathode particles, enabling lithium ions to quickly reach the surface of the cathode particles, facilitating lithium ion insertion and extraction, and promoting the utilization of the specific capacity of the cathode active material. Simultaneously, the amorphous carbon in this application is beneficial for improving electronic conductivity, thereby facilitating electron conduction.

[0014] In some embodiments, the thickness of the coating layer is 1 nm to 500 nm;

[0015] and / or;

[0016] The aforementioned coating layer comprises shaped carbon and / or amorphous carbon, wherein the mass ratio between the mass of shaped carbon and / or amorphous carbon and the mass of nanocrystalline lithium metal salt in the coating layer is (0.025–50):1.

[0017] In these embodiments, this application discloses that the nanocrystalline lithium metal salt in the coating layer is beneficial for further improving the ionic conductivity of the cathode particles, enabling lithium ions to quickly reach the surface of the cathode particles, which is conducive to the insertion and extraction of lithium ions and facilitates the utilization of the specific capacity of the cathode active material. At the same time, the amorphous carbon and shaped carbon in this application are beneficial for improving electronic conductivity, thereby facilitating electron conduction.

[0018] In this application, nanocrystalline lithium metal salts together with a certain amount of amorphous carbon and / or morphological carbon form a structurally stable coating layer. This coating layer provides good physical isolation between lithium manganese iron phosphate and nanocrystalline lithium metal salts in the cathode particles and the external electrolyte, which is beneficial to improving the structural stability of lithium manganese iron phosphate and nanocrystalline lithium metal salts, and improving the cycle life and high-temperature storage performance of the battery.

[0019] In some embodiments, the volumetric particle size distribution Dv50 of the nanocrystalline lithium metal salt in the above-mentioned coating layer is 1 nm to 500 nm.

[0020] In this application, the particle size of the nanocrystalline lithium metal salt located between the aforementioned primary particles is less than or equal to the particle size of the nanocrystalline lithium metal salt in the coating layer.

[0021] In some embodiments,

[0022] The aforementioned nanocrystalline lithium metal salts include compounds represented by Chemical Formula I and Chemical Formula II, or Li 10 Ge 0.8 Al 0.2 P2S11.6 Se 0.3 One or more of the following:

[0023] Li 7-x La3Zr 2-x A x O 12 Chemical formula I,

[0024] Where A includes any one or more of the elements Ta, Nb, Sn, Hf, Sc, and Ge, and 0 ≤ x ≤ 0.75;

[0025] Li 3a La 0.66-a TiO3 chemical formula II

[0026] Where 0 < a ≤ 0.16.

[0027] This application selects nanocrystalline lithium metal salts with the above-mentioned chemical formula. These lithium salts have good ionic conductivity, and some of the nanocrystalline lithium metal salts are located at at least part of the interface between the primary particles of lithium manganese iron phosphate, which is conducive to building a strong and smooth lithium-ion transport pathway and improving the conductivity and structural stability of lithium manganese iron phosphate.

[0028] In some embodiments, the volumetric particle size distribution Dv50 of the above-mentioned lithium manganese iron phosphate primary particles is 10 nm to 2 μm;

[0029] and / or;

[0030] The volumetric particle size distribution (Dv50) of the aforementioned secondary lithium manganese iron phosphate particles is 100 nm to 50 μm.

[0031] and / or;

[0032] The chemical formula of the above-mentioned lithium manganese iron phosphate is Li b Fe c Mn d M 1-c-d PO4;

[0033] Wherein, M represents the doping element at the manganese and iron sites, and the doping element at the manganese and iron sites includes any one or more of Al, Cu, Mg, Zn, Ni, Ti, V, Zr, Co, Ga, Sn, Sb, and Nb.

[0034] b ranges from 0.9 to 1.1;

[0035] c ranges from 0.001 to 0.999;

[0036] d ranges from 0.001 to 0.999;

[0037] 1-cd is between 0 and 0.1.

[0038] In some embodiments, the volumetric particle size distribution Dv50 of the above-mentioned positive electrode particles is:

[0039] 0.2μm~17μm.

[0040] and / or;

[0041] The compacted density of the above-mentioned positive electrode particles under a force of 30,000 N is 2.0 g / cm³. 3 ~2.6g / cm 3 .

[0042] and / or;

[0043] The above-mentioned positive electrode particles have an electronic conductivity of 1×10⁻⁶ at 25°C. -12 S / cm~1×10 -3 S / cm.

[0044] In some embodiments, the ion diffusion coefficient of the above-mentioned secondary battery at 25°C is 1×10⁻⁶. -11 cm 2 / s~1×10 -4 cm 2 / s.

[0045] In some embodiments, the mass percentage content of the above-mentioned positive electrode particles is 95% to 99% based on the total mass of the film layer on one side of the positive electrode sheet;

[0046] The aforementioned positive electrode sheet includes a conductive agent, which includes one or more of graphite, carbon black, carbon dots, acetylene black, graphene, carbon nanotubes, and carbon nanofibers.

[0047] A second aspect of this application is to provide an electrical device comprising the secondary battery described in the first aspect.

[0048] The above description is only an overview of the technical solution of this application. In order to better understand the technical means of this application and to implement it in accordance with the contents of the specification, and to make the above and other objects, features and advantages of this application more obvious and understandable, the following are specific embodiments of this application. Attached Figure Description

[0049] Various other advantages and benefits will become apparent to those skilled in the art upon reading the following detailed description of preferred embodiments. The accompanying drawings are for illustrative purposes only and are not intended to limit the scope of this application. Furthermore, the same reference numerals denote the same parts throughout the drawings. In the drawings:

[0050] Figure 1 This is a schematic diagram of the battery structure of some embodiments of this application;

[0051] Figure 2 This is an exploded structural diagram of a battery according to some embodiments of this application;

[0052] Figure 3 This is a schematic diagram of the vehicle structure according to some embodiments of this application;

[0053] Figure 4 This is a schematic diagram of the battery pack structure according to some embodiments of this application;

[0054] Figure 5 This is a schematic diagram of the structure of the positive electrode particles in some embodiments of this application;

[0055] The reference numerals in the detailed embodiments are as follows:

[0056] 10000, vehicles;

[0057] 1000, Battery; 2000, Controller; 3000, Motor;

[0058] 100. Battery cell;

[0059] 200. Box body; 210. First part; 220. Second part;

[0060] 10. Secondary batteries;

[0061] 101. Housing; 102. Electrode assembly; 103. Cover plate;

[0062] 11. Positive electrode particles;

[0063] 111. Primary particles; 112. Secondary particles; 113. Nanocrystalline lithium metal salts; 114. Amorphous carbon. Detailed Implementation

[0064] The following detailed description, with appropriate reference to the accompanying drawings, discloses embodiments of the positive electrode, secondary battery, battery pack, and power-consuming device of this application. However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repetitive descriptions of practically identical structures may be omitted. This is to avoid unnecessarily lengthy descriptions and to facilitate understanding by those skilled in the art. Furthermore, the accompanying drawings and the following description are provided for the purpose of enabling those skilled in the art to fully understand this application and are not intended to limit the subject matter of the claims.

[0065] The "range" disclosed in this application is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60–120 and 80–110 are listed for a specific parameter, it is also expected that ranges of 60–110 and 80–120 are also included. Furthermore, if minimum range values ​​of 1 and 2 are listed, and if maximum range values ​​of 3, 4, and 5 are listed, then the following ranges are all expected: 1–3, 1–4, 1–5, 2–3, 2–4, and 2–5. In this application, unless otherwise stated, the numerical range "a–b" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0~5" indicates that all real numbers between "0~5" have been listed in this article; "0~5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is stated as an integer ≥2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0066] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions.

[0067] Unless otherwise specified, all technical features and optional technical features of this application may be combined to form new technical solutions.

[0068] Unless otherwise specified, all steps in this application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the mention that the method may also include step (c) indicates that step (c) may be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.

[0069] Unless otherwise specified, the terms "comprising" and "including" as used in this application can be open-ended or closed-ended. For example, "comprising" and "including" can mean that other components not listed may also be included, or that only the listed components may be included.

[0070] Unless otherwise specified, the term "or" is inclusive in this application. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, the condition "A or B" is satisfied by any of the following conditions: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0071] Unless otherwise specified, in this application, the terms "first," "second," etc., are used only to distinguish different objects and should not be construed as indicating or implying relative importance or implicitly specifying the number, specific order, or primary and secondary relationship of the indicated technical features.

[0072] Unless otherwise specified, in this application, the term "multiple" means two or more (including two), similarly, "multiple sets" means two or more (including two sets), and "multiple pieces" means two or more (including two pieces).

[0073] Unless otherwise specified, the technical terms "center," "longitudinal," "lateral," "length," "width," "thickness," "upper," "lower," "front," "rear," "left," "right," "vertical," "horizontal," "top," "bottom," "inner," "outer," "clockwise," "counterclockwise," "axial," "radial," and "circumferential" indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are used only for the convenience of describing the embodiments of this application and simplifying the description, and are not intended to indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on the embodiments of this application.

[0074] Secondary batteries

[0075] In this application embodiment, a secondary battery refers to a battery cell that can be recharged after the battery cell has been discharged, allowing the active materials to be activated and the battery cell to continue to be used.

[0076] The secondary battery can be a lithium-ion battery, sodium-ion battery, sodium-lithium-ion battery, lithium metal battery, sodium metal battery, lithium-sulfur battery, magnesium-ion battery, nickel-metal hydride battery, nickel-cadmium battery, lead-acid battery, etc., and the embodiments of this application are not limited to this.

[0077] Electrode assembly

[0078] A secondary battery typically includes an electrode assembly. This assembly comprises a positive electrode, a negative electrode, and a separator, with the separator positioned between the positive and negative electrodes. During the charging and discharging process of a secondary battery, active ions (such as lithium ions) repeatedly insert and extract between the positive and negative electrodes. The separator, positioned between the positive and negative electrodes, prevents short circuits while allowing active ions to pass through.

[0079] Battery device

[0080] The battery apparatus mentioned in the embodiments of this application may include one or more battery cell assemblies for providing voltage and capacity. A battery cell assembly may include multiple battery cells connected in series, parallel, or mixed connections via a busbar.

[0081] In some embodiments, a battery cell assembly is typically formed by arranging multiple battery cells.

[0082] As an example, a battery cell assembly can be a battery module, which is formed by arranging and fixing multiple battery cells together to form an independent module. As another example, a battery module can be formed by bundling multiple battery cells together with cable ties.

[0083] In some embodiments, the battery device may be a battery pack, which includes a housing and one or more individual battery cells housed within the housing.

[0084] As an example, the battery cell assembly can be a battery module, which can be housed in a housing by fixing the battery module in the housing.

[0085] As an example, battery cell assemblies can also be housed in a housing by directly fixing multiple battery cells to the housing.

[0086] As an example, the enclosure may include a first enclosure and a second enclosure. The first enclosure and the second enclosure are fastened together to form a closed space inside the enclosure to house the individual battery cells. Here, "closed" refers to covering or closing, and can be either sealed or unsealed. The first enclosure may be a top cover or a bottom plate.

[0087] As an example, the enclosure may include a top cover, a frame, and a bottom plate. The top cover and bottom plate are connected to the frame, creating an enclosed space inside the enclosure to house the individual battery cells.

[0088] In some embodiments, the housing may be part of the vehicle's chassis structure. For example, a portion of the housing may be at least a part of the vehicle's floor, or a portion of the housing may be at least a part of the vehicle's crossbeams and longitudinal beams.

[0089] The battery cell of this application may include an outer packaging. This outer packaging can be used to encapsulate the electrode assembly and electrolyte composed of the aforementioned battery cell. The outer packaging of the battery cell can be a rigid shell, such as a hard plastic shell, aluminum shell, steel shell, etc. The outer packaging of the battery cell can also be a flexible package, such as a pouch-type flexible package. The material of the flexible package can be plastic, including but not limited to polypropylene, polybutylene terephthalate, and polybutylene succinate.

[0090] This application does not impose any particular limitation on the shape of the battery; it can be cylindrical, square, or any other arbitrary shape. For example, Figure 1 This is an example of a square-structured secondary battery 10.

[0091] According to some embodiments of this application, reference is made to Figure 2 The outer packaging may include a housing 101 and a cover plate 103. The housing 101 may include a bottom plate and side plates connected to the bottom plate, the bottom plate and side plates forming a receiving cavity. The housing 101 has an opening communicating with the receiving cavity, and the cover plate 103 can be placed over the opening to close the receiving cavity. The positive electrode, negative electrode, and separator may be formed into an electrode assembly 102 by a winding process or a stacking process. The electrode assembly 102 is encapsulated within the receiving cavity. Electrolyte is immersed in the electrode assembly 102. The secondary battery 10 may contain one or more electrode assemblies 102, which can be selected by those skilled in the art according to specific practical needs.

[0092] The electrode assembly 102 provided in this application is beneficial to improving the performance of a battery cell when applied in a battery cell. The battery cell can be used as a power source for an electrical device or as an energy storage unit for an electrical device. The electrical device is used in the power field, such as mobile devices (e.g., mobile phones, laptops, etc.), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but is not limited to the above fields.

[0093] For ease of explanation, some embodiments of this application are illustrated using a vehicle as an example of an electrical device.

[0094] Please refer to Figure 3 , Figure 3This is a schematic diagram of the structure of a vehicle 10000 provided in some embodiments of this application. The vehicle 10000 can be a gasoline-powered vehicle, a natural gas-powered vehicle, or a new energy vehicle. New energy vehicles can be pure electric vehicles, hybrid electric vehicles, or range-extended electric vehicles, etc. A battery 1000 is disposed inside the vehicle 10000, and the battery 10000 can be located at the bottom, front, or rear of the vehicle 10000. The battery 10000 can be used to power the vehicle 10000; for example, the battery 10000 can serve as the operating power source for the vehicle 10000. The vehicle 10000 may also include a controller 2000 and a motor 3000. The controller 2000 is used to control the battery 10000 to supply power to the motor 3000, for example, to meet the power needs of the vehicle 10000 during startup, navigation, and driving.

[0095] In some embodiments of this application, the battery 1000 can not only serve as the operating power source for the vehicle 10000, but also as the driving power source for the vehicle 10000, replacing or partially replacing fuel or natural gas to provide driving power for the vehicle 10000.

[0096] Please refer to Figure 4 , Figure 4 This is an exploded view of a battery 1000 provided in some embodiments of this application. The battery 1000 includes a housing 200 and a battery cell 100. A conventional battery cell includes a primary battery or a secondary battery. This application specifically protects a secondary battery 10. The battery cell 100 is housed within the housing 200. The housing 200 provides space for the battery cell 100, and the housing 200 can adopt various structures.

[0097] In some embodiments, the housing 200 may include a first portion 210 and a second portion 220, which overlap each other, and together define a receiving space for accommodating the battery cell 100. The second portion 220 may be a hollow structure with one open end, and the first portion 210 may be a plate-like structure, with the first portion 210 covering the open side of the second portion 220 so that the first portion 210 and the second portion 220 together define the receiving space; alternatively, the first portion 210 and the second portion 220 may both be hollow structures with one open side, with the open side of the first portion 210 covering the open side of the second portion 220. Of course, the housing 200 formed by the first portion 210 and the second portion 220 may be of various shapes, such as a cylinder, a cuboid, etc.

[0098] In battery 1000, there can be multiple battery cells 100, which can be connected in series, parallel, or in a mixed manner. A mixed connection means that multiple battery cells 100 are connected in both series and parallel configurations. Multiple battery cells 100 can be directly connected in series, parallel, or in a mixed manner, and then the entire assembly of the multiple battery cells 100 is housed within housing 200. Alternatively, battery 1000 can also be composed of multiple battery cells 100 first connected in series, parallel, or in a mixed manner to form battery modules, and then these modules are connected in series, parallel, or in a mixed manner to form a whole, which is also housed within housing 200. Battery 1000 may also include other structures; for example, it may include a busbar component for electrical connection between the multiple battery cells 100.

[0099] Secondary batteries

[0100] Secondary batteries, due to their advantages such as high energy density, long cycle life, and safety and reliability, have been widely used in various products. Lithium manganese iron phosphate (LFP), as an upgraded version of lithium iron phosphate, was developed to further improve energy density while retaining the safety and cycle life advantages of phosphate batteries. However, LFP is essentially an insulator, exhibiting low conductivity and manganese leaching that leads to suboptimal capacity, stability, and cycle performance.

[0101] To alleviate the aforementioned problems, related technologies have disclosed the doping of lithium manganese iron phosphate with oxide solid-state crystalline electrolyte materials that have lithium-ion conduction capabilities, such as doping in the coating layer of lithium manganese iron phosphate. However, these methods still suffer from the technical drawback of not achieving ideal improvement results.

[0102] In view of this, this application discloses a secondary battery, which includes a positive electrode, a negative electrode, and a separator disposed between the positive electrode and the negative electrode.

[0103] The aforementioned positive electrode sheet includes positive electrode particles, which include lithium manganese iron phosphate, which includes secondary particles composed of multiple primary particles, and the positive electrode particles include nanocrystalline lithium metal salt, which is located at at least a portion of the interface between the primary particles.

[0104] The aforementioned nanocrystalline metallic lithium salts include lithium, oxalic group elements, and other elements, including any two or more of phosphorus, aluminum, titanium, zirconium, hafnium, niobium, tantalum, tin, scandium, germanium, and lanthanides.

[0105] The cathode particles in this application contain positive electrode active materials.

[0106] The primary particles in this application refer to individual fine crystals that have not agglomerated and are the most basic unit in the positive electrode active material.

[0107] The secondary particles in this application refer to larger particles formed by the aggregation of two or more primary particles.

[0108] The method for determining the primary and secondary particles in this application includes obtaining a cross-sectional scanning electron microscope (SEM) image of the cathode particles and analyzing the cross-sectional scanning electron microscope (SEM) image to obtain the primary and secondary particles of lithium manganese iron phosphate, as well as the nanocrystalline metallic lithium salt located at at least part of the interface between the primary particles. The method of obtaining cross-sectional scanning electron microscope (SEM) images of the above-mentioned positive electrode particles from the secondary battery in this application includes: placing the battery cell in a 1.0 mol / L sodium hydroxide aqueous solution at room temperature for discharge treatment; after discharge is completed, manually disassembling to obtain the positive electrode sheet; cutting the positive electrode sheet into 6 mm × 6 mm sizes; preparing the cross-section of the positive electrode sheet using a cross-section polisher (e.g., JEOL IB-09010CP argon ion cross-section polisher); then, referring to JY / T010-1996, scanning the longitudinal cross-section of the positive electrode sheet using a scanning electron microscope (e.g., ZEISS Sigma 300 scanning electron microscope); and searching for suitable cross-sectional scanning electron microscope (SEM) images of the secondary particles in these longitudinal cross-sections.

[0109] The nanocrystalline lithium metal salt of this application is a nanocrystalline electrolyte composed of lithium, oxalic group elements and other metal elements, wherein the oxalic group elements include any one or more of oxygen, sulfur, selenium and tellurium.

[0110] The nanocrystalline lithium metal salts of this application may also contain phosphorus group elements, such as, but not limited to, phosphorus.

[0111] The nanocrystalline lithium salt of this application exhibits high ionic conductivity, and it is located at at least part of the interface between primary lithium manganese iron phosphate particles, which is conducive to building a robust and unobstructed lithium-ion transport pathway, thereby improving the conductivity and structural stability of lithium manganese iron phosphate.

[0112] The determination of each constituent element in the nanocrystalline lithium metal salt of this application includes any method conventional in the art, such as energy-dispersive X-ray spectroscopy. Specifically, the cathode particles are first obtained, and the specific steps are as follows:

[0113] (1) The battery cell is placed in a 1.0 mol / L sodium hydroxide aqueous solution at room temperature for discharge treatment. After discharge, the positive electrode is manually disassembled to obtain the positive electrode sheet. The positive electrode sheet is broken into fragments. The fragments are subjected to low-temperature pyrolysis to remove the electrolyte, and then subjected to high-temperature pyrolysis to remove the binder and other substances to obtain a fully pyrolyzed positive electrode sheet. The fully pyrolyzed positive electrode sheet is further crushed using a morphology control device to control the morphology of the crushed particles, and aluminum foil particles and positive electrode particles with different morphologies are obtained. Further sieving yields the positive electrode particles.

[0114] (2) The composition of nanocrystalline lithium metal salt in cathode particles is analyzed by using, for example, an energy dispersive X-ray spectroscopy (EDS) model ISC150 coupled with a transmission electron microscope (TEM) model ZEISS. Specifically, point analysis is performed by detecting the chemical composition at the interface between primary particles in the material using EDS; surface analysis is performed by scanning the electron beam as it moves across the sample surface and recording the intensity of characteristic X-rays at different locations to generate an elemental distribution map; surface analysis is performed by collecting characteristic X-rays with a detector and converting them into electrical signals, which are then processed by a multichannel pulse height analyzer. By detecting the energy distribution of these X-rays, the types of elements in the sample can be determined. By measuring the intensity of characteristic X-rays and comparing them with known standard samples, a semi-quantitative analysis of elemental content can be achieved.

[0115] Therefore, the secondary battery provided in this application facilitates the effective utilization of the specific capacity of the positive electrode active material by constructing a robust and unobstructed lithium-ion transport pathway inside the battery, and enables the secondary battery to have stable electrochemical performance, such as long cycle life and good high-temperature storage performance.

[0116] In some embodiments, based on the total mass of the cathode particles, the mass percentage content of the nanocrystalline lithium metal salt located between the primary particles is 0.3% to 20%.

[0117] As described above, this application can use energy-dispersive X-ray spectroscopy combined with TEM to achieve semi-quantitative analysis of the elemental content of nanocrystalline lithium metal salts, and further determine the content of nanocrystalline lithium metal salts located between the primary particles, and obtain it according to the calculation formula: mass of nanocrystalline lithium metal salts located between primary particles / total mass of cathode particles × 100%.

[0118] This application selects to control the mass percentage content of nanocrystalline lithium metal salt between primary particles to a certain range so as not to affect the continued growth of primary particles, while ensuring sufficient and effective physical contact between primary particles and nanocrystalline lithium metal salt, so as to facilitate the construction of a robust and unobstructed lithium-ion transport pathway.

[0119] In these embodiments, this application discloses that, based on the total mass of the aforementioned positive electrode particles, the mass percentage content of the nanocrystalline lithium metal salt located between the aforementioned primary particles is 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, and 2.5%. The percentage is 10%, 3.0%, 3.5%, 4.0%, 4.5%, 4.9%, 5.0%, 5.5%, 6.0%, 6.3%, 6.5%, 7.0%, 7.5%, 8.0%, 8.5%, 9.0%, 9.5%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, or 20%, or any combination thereof.

[0120] In some embodiments, the volumetric particle size distribution Dv50 of the nanocrystalline lithium metal salt located between the primary particles is 1 nm to 200 nm.

[0121] In this application, Dv50 refers to the particle size distribution where 50% of the volume of particles larger than Dv50 are equal to 50% of the volume of particles smaller than Dv50. It is also known as the median diameter or median particle size and is typically used to represent the average particle size. The volumetric particle size distribution Dv50 of the aforementioned nanocrystalline lithium metal salt located between the primary particles in this application can be determined using any method conventional in the art, such as a combination of transmission electron microscopy and laser diffraction particle size analysis.

[0122] In this application, the nanocrystalline lithium metal salt is composed of nanoscale crystalline particles, which is beneficial for further enhancing the physical contact between the primary particles and the nanocrystalline lithium metal salt.

[0123] In these embodiments, this application discloses that the volumetric particle size distribution Dv50 of the aforementioned nanocrystalline metallic lithium salt located between the aforementioned primary particles is any one of 1nm, 2nm, 3nm, 3.4nm, 4nm, 5nm, 6nm, 7nm, 8nm, 9nm, 9.5nm, 9.6nm, 10nm, 11.2nm, 13.1nm, 14.2nm, 15nm, 19.1nm, 20nm, 25nm, 30nm, 35nm, 40nm, 45nm, 49.5nm, 50nm, 55nm, 60nm, 65nm, 70nm, 75nm, 80nm, 85nm, 90nm, 95nm, 100nm, 110nm, 120nm, 130nm, 140nm, 150nm, 160nm, 170nm, 180nm, 190nm, and 200nm, or any one of both of the above ranges.

[0124] In some embodiments, the cathode particles have a coating layer disposed on at least a portion of the surface of the lithium manganese iron phosphate, the coating layer comprising a nanocrystalline lithium metal salt.

[0125] In these embodiments, this application discloses that the nanocrystalline lithium metal salt in the coating layer is beneficial for further improving the ionic conductivity of the cathode particles, enabling lithium ions to quickly reach the surface of the cathode particles, which is conducive to the insertion and extraction of lithium ions and facilitates the utilization of the specific capacity of the cathode active material. At the same time, the amorphous carbon and shaped carbon in this application are beneficial for improving electronic conductivity, thereby facilitating electron conduction.

[0126] In some embodiments, the thickness of the coating layer is 1 nm to 500 nm.

[0127] In this application, the thickness of the coating layer on the outside of the cathode particle can be obtained by obtaining a cross-sectional scanning electron microscope (SEM) image of the cathode particle and analyzing and measuring the cross-sectional scanning electron microscope (SEM) image.

[0128] In these embodiments, this application discloses that the thickness of the coating layer is any one of 1nm, 2nm, 3nm, 4nm, 5nm, 6nm, 7nm, 8nm, 9nm, 10nm, 15nm, 20nm, 25nm, 30nm, 35nm, 40nm, 45nm, 50nm, 55nm, 60nm, 70nm, 75nm, 80nm, 85nm, 90nm, 95nm, 100nm, 200nm, 300nm, 400nm, and 500nm, or any one of both of the above ranges.

[0129] In some embodiments, the coating layer comprises shaped carbon and / or amorphous carbon, wherein the mass ratio of shaped carbon and / or amorphous carbon to nanocrystalline lithium salt in the coating layer is (0.025–50):1.

[0130] like Figure 5 The positive electrode particle 11 includes secondary particles 112 formed by the aggregation of primary particles 111. The secondary particles 112 are partially cut, and there is a nanocrystalline lithium metal salt 113 at part of the interface of the primary particles 111. The nanocrystalline lithium metal salt 113 is in close contact with the primary particles 111. At the same time, nanocrystalline lithium metal salt 113 is also formed on the outer surface of the secondary particles 112. The nanocrystalline lithium metal salt 113 at this position, together with amorphous carbon 114, constitutes the coating layer of the secondary particles 112. The coating layer of this application also contains shaped carbon, which is not directly shown in the accompanying drawings.

[0131] In this application, nanocrystalline lithium metal salts together with a certain amount of amorphous carbon and / or morphological carbon form a structurally stable coating layer. This coating layer provides good physical isolation between lithium manganese iron phosphate and nanocrystalline lithium metal salts in the cathode particles and the external electrolyte, which is beneficial to improving the structural stability of lithium manganese iron phosphate and nanocrystalline lithium metal salts, and improving the cycle life and high-temperature storage performance of the battery.

[0132] This application discloses in these embodiments that the mass ratio between the mass of shaped carbon and / or amorphous carbon and the mass of nanocrystalline lithium metal salt in the coating layer is 0.025:1, 0.03:1, 0.04:1, 0.05:1, 0.06:1, 0.07:1, 0.08:1, 0.09:1, 0.1:1, 0.2:1, 0.3:1, 0.4:1, 0.5:1, 0.6: 1. Any one of the following: 0.7:1, 0.8:1, 0.9:1, 1:1, 2:1, 5:1, 8:1, 10:1, 12:1, 15:1, 18:1, 20:1, 22:1, 25:1, 28:1, 30:1, 32:1, 35:1, 38:1, 40:1, 42:1, 45:1, 48:1, 50:1, or any one of the ranges of the above two.

[0133] In some embodiments, the volumetric particle size distribution Dv50 of the nanocrystalline lithium metal salt in the above-mentioned coating layer is 1 nm to 500 nm.

[0134] This application discloses in these embodiments that the volumetric particle size distribution Dv50 of the nanocrystalline lithium metal salt in the coating layer is 1nm, 2nm, 3nm, 4nm, 5nm, 6nm, 7nm, 8nm, 9nm, 10nm, 11nm, 12nm, 13nm, 14nm, 15nm, 16nm, 17nm, 18nm, 19nm, 20nm, 21nm, 22nm, 23nm, 24nm, 25nm, 26nm, 27nm, 28nm, and 29nm. Any one of the following: 30nm, 31nm, 32nm, 33nm, 34nm, 35nm, 36nm, 37nm, 38nm, 39nm, 40nm, 41nm, 42nm, 43nm, 44nm, 45nm, 46nm, 47nm, 48nm, 49nm, 50nm, 51nm, 52nm, 53nm, 100nm, 200nm, 300nm, 400nm, 500nm, or any one of the above two ranges.

[0135] In some embodiments, the above-mentioned nanocrystalline lithium metal salt includes compounds illustrated by Chemical Formula I and Chemical Formula II, or Li 10 Ge 0.8 Al 0.2 P2S11.6 Se 0.3 One or more of the following:

[0136] Li 7-x La3Zr 2-x A x O 12 Chemical formula I,

[0137] Where A includes any one or more of the elements Ta, Nb, Sn, Hf, Sc, and Ge, and 0 ≤ x ≤ 0.75;

[0138] Li 3a La 0.66-a TiO3 chemical formula II

[0139] Where 0 < a ≤ 0.16.

[0140] In some embodiments, the compound represented by Chemical Formula I is a garnet-type lithium metal salt. Garnet-type lithium metal salts possess high ionic conductivity and good electrochemical stability, but they also suffer from high hardness and fragility. This application selects to nano-size the garnet-type lithium metal salt and form it between the primary particles of lithium manganese iron phosphate. This also helps to improve the structural stability of the garnet-type lithium metal salt and enhances the conductivity of lithium manganese iron phosphate by improving the physical contact between the garnet-type lithium metal salt and the lithium manganese iron phosphate.

[0141] In the chemical formula of the garnet-type lithium metal salt of this application, x includes any one of 0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.75 or any one of the above two ranges.

[0142] This application discloses, in these embodiments, that the garnet-type lithium metal salt includes Li7La3Zr2O. 12 Li 6.4 La3Ta 0.6 Zr 1.4 O 12 Li 6.5 La3Ta 0.5 Zr 1.5 O 12 and Li 6.6 La3Ta 0.4 Zr 1.6 O 12 Any one or more of the following.

[0143] In some embodiments, the compound Li, as illustrated by the specific chemical formula above, 10 Ge 0.8 Al 0.2 P2S 11.6 Se 0.3It is a lithium superionic conductor (LISICON) type lithium metal salt, which also has high ionic conductivity and good electrochemical stability.

[0144] In some embodiments, the compound indicated by the above chemical formula II is a perovskite-type lithium metal salt, which also possesses high ionic conductivity and good electrochemical stability.

[0145] In this application, the chemical formula of the perovskite-type lithium metal salt includes 'a', which comprises any one of 0.10, 0.11, 0.12, 0.13, 0.14, 0.15, and 0.16, or any one of both ranges. This application discloses in these embodiments that the perovskite-type lithium metal salt includes Li. 0.5 La 0.5 TiO3.

[0146] This application selects nanocrystalline lithium metal salts with the above-mentioned chemical formula. These lithium salts have good ionic conductivity, and some of the nanocrystalline lithium metal salts are located at at least part of the interface between the primary particles of lithium manganese iron phosphate, which is conducive to building a strong and smooth lithium-ion transport pathway and improving the conductivity and structural stability of lithium manganese iron phosphate.

[0147] In some embodiments of this application, a portion of nanocrystalline lithium metal salt is located on the surface of lithium manganese iron phosphate secondary particles to form a coating layer for lithium manganese iron phosphate. The nanocrystalline lithium metal salt in the coating layer is beneficial for further improving the ionic conductivity of the cathode particles, enabling lithium ions to quickly reach the surface of the cathode particles, which is conducive to the insertion and extraction of lithium ions and facilitates the utilization of the specific capacity of the cathode active material.

[0148] In some embodiments of this application, a portion of the nanocrystalline lithium metal salt is selected and located together with amorphous carbon and / or shaped carbon on the surface of the lithium manganese iron phosphate secondary particles to form a coating layer for the lithium manganese iron phosphate. This coating layer provides excellent physical isolation between the lithium manganese iron phosphate and nanocrystalline lithium metal salt within the cathode particles and the external electrolyte, which is beneficial for improving the structural stability of the lithium manganese iron phosphate and nanocrystalline lithium metal salt, and for improving the cycle life and high-temperature storage performance of the battery.

[0149] In some embodiments, the volumetric particle size distribution Dv50 of the above-mentioned lithium manganese iron phosphate primary particles is 10 nm to 2 μm.

[0150] As described above, this application discloses the method of obtaining cross-sectional scanning electron microscope (SEM) images of cathode particles and analyzing these SEM images to determine the primary and secondary particles of lithium manganese iron phosphate. The volumetric particle size distribution Dv50 is the average particle size. In some embodiments, the volumetric particle size distribution Dv50 of the aforementioned lithium manganese iron phosphate secondary particles is...

[0151] 100nm~50μm.

[0152] The volumetric particle size distribution Dv50 of the lithium manganese iron phosphate secondary particles in this application refers not only to the particle size of the secondary particles determined by obtaining and analyzing the cross-sectional scanning electron microscope (SEM) images of the cathode particles, but also to the particle size of the lithium manganese iron phosphate secondary particles formed during the preparation process.

[0153] In these embodiments, this application discloses that the volumetric particle size distribution Dv50 of primary lithium manganese iron phosphate particles is any one of 10nm, 20nm, 30nm, 40nm, 50nm, 60nm, 63nm, 70nm, 80nm, 90nm, 100nm, 200nm, 300nm, 380nm, 390nm, 400nm, 413nm, 420nm, 430nm, 450nm, 500nm, 600nm, 603nm, 700nm, 800nm, 900nm, 1μm, 1.5μm, 2μm or any one of the above two ranges.

[0154] This application discloses in these embodiments the volumetric particle size distribution Dv50 of lithium manganese iron phosphate secondary particles as 100nm, 200nm, 300nm, 400nm, 500nm, 600nm, 700nm, 800nm, 900nm, 1μm, 2μm, 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, 11μm, 12μm, 13μm, 14μm, 15μm, 16μm, 17μm, 18μm, 19μm, 2 The value is any one of the following: 0μm, 21μm, 22μm, 23μm, 24μm, 25μm, 26μm, 27μm, 28μm, 29μm, 30μm, 31μm, 32μm, 33μm, 34μm, 35μm, 36μm, 37μm, 38μm, 39μm, 40μm, 41μm, 42μm, 43μm, 44μm, 45μm, 46μm, 47μm, 48μm, 49μm, 50μm, or any one of the above two ranges.

[0155] In some embodiments, the chemical formula of the above-mentioned lithium manganese iron phosphate is Li b Fe c Mn d M 1-c-d PO4;

[0156] Wherein, M represents the doping element at the manganese site and the iron site, and the doping element at the manganese site and the iron site includes any one or more of Al, Cu, Mg, Zn, Ni, Ti, V, Zr, Co, Ga, Sn, Sb and Nb.

[0157] b ranges from 0.9 to 1.1;

[0158] c ranges from 0.001 to 0.999;

[0159] d ranges from 0.001 to 0.999;

[0160] 1-cd is between 0 and 0.1.

[0161] The lithium manganese iron phosphate of this application can be purchased through commercial channels, and the elemental composition of the purchased products is already labeled. Furthermore, the components of the positive electrode active material of this application can also be detected by chemical analysis methods commonly used in the art, including but not limited to: complexation titration, precipitation gravimetric method, redox method, differential method, inductively coupled plasma atomic emission spectrometry (ICP-AES), and atomic absorption spectrometry. Among these, ICP-AES and atomic absorption spectrometry are convenient and efficient, and their mechanisms are as follows:

[0162] Plasma emission spectroscopy is an analytical method that uses a high-temperature excitation source generated by plasma as the excitation source for atomic emission spectra. Different elements produce different characteristic spectra. These characteristic spectra are projected onto a grating in a spectrometer through a lens. By controlling a motor to rotate the grating, a transmission mechanism accurately positions the intensity of the characteristic spectral lines of the element to be measured at the exit slit after spectral dispersion. A photomultiplier tube converts this spectral intensity into an electric current. After further circuit processing and conversion, the data is processed by a computer to obtain the analytical results.

[0163] Atomic absorption spectrometry (AAS), also known as atomic absorption spectrophotometry, is an analytical method based on the absorption of characteristic radiation (spectral lines) emitted by atomic vapors of the same type of atom. The analytical process involves irradiating the sample solution with atomized and atomized atomic vapors of the sample solution using characteristic radiation emitted by the same type of atom. The gaseous ground-state atoms of the analyte in the vapor absorb the characteristic radiation lines emitted from the light source. Different elements exhibit selective absorption of these characteristic radiation lines, and the concentration of the analyte in the sample is determined by the degree of radiation attenuation.

[0164] In these embodiments, this application discloses that the chemical formula of lithium manganese iron phosphate has b as any one of 0.90, 0.91, 0.92, 0.93, 0.94, 0.95, 0.96, 0.97, 0.98, 0.99, 1.0, 1.01, 1.02, 1.03, 1.04, 1.05, 1.06, 1.07, 1.08, 1.09, 1.1 or any one of the above two ranges.

[0165] In these embodiments, this application discloses that the chemical formula of lithium manganese iron phosphate has c as any one of 0.001, 0.01, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 0.99, 0.999 or any one of the above ranges.

[0166] In these embodiments, this application discloses that d is any one of 0.001, 0.01, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 0.99, 0.999 or any one of the ranges of the above two values.

[0167] In some embodiments, the volumetric particle size distribution Dv50 of the above-mentioned positive electrode particles is 0.2 μm to 15 μm.

[0168] The meaning and measurement method of the volumetric particle size distribution Dv50 of the cathode particles in this application are the same as those described above, and will not be repeated here. Furthermore, in these embodiments, this application discloses that the volumetric particle size distribution Dv50 of the cathode particles is any one of 0.2μm, 0.3μm, 0.4μm, 0.5μm, 0.6μm, 0.7μm, 0.8μm, 0.9μm, 1.0μm, 2.0μm, 3.0μm, 4.0μm, 5.0μm, 6.0μm, 7.0μm, 8.0μm, 9.0μm, 10.0μm, 11.0μm, 12.0μm, 13.0μm, 14.0μm, 15.0μm, 16.0μm, and 17.0μm, or any one of the above two ranges.

[0169] In some embodiments, the compaction density of the above-mentioned positive electrode particles under a force of 30000N is 2.0 g / cm³. 3 ~2.6g / cm 3 .

[0170] The compaction density described in this application encompasses any concept conventional in the art, and can be obtained using instruments or methods known in the art, such as limiting the cold pressing pressure to 30000N and calculating it according to the method in GB / T 24533-2009. For example, it can be measured using an electronic pressure testing instrument (e.g., UTM7305). Specifically, a specific amount M of the powder sample to be tested is placed on a dedicated mold (with a bottom area of ​​S0), and different pressures are set. Each pressure is maintained for 30 seconds, then released. After 10 seconds, the thickness H0 of the powder compressed under that pressure is read on the device. The compaction density under that pressure is calculated, and the compaction density of the positive electrode particles under that pressure is equal to M / (H0×S0).

[0171] This application discloses in these embodiments that the compaction density of the positive electrode particles under an action of 30000N is 2.0 g / cm³. 3 2.1g / cm 3 2.2g / cm 3 2.3g / cm 3 2.4g / cm 3 2.5g / cm 3 2.6g / cm 3 It can be any one of the above or any one of the range values ​​of any two of the above.

[0172] In some embodiments, the ion diffusion coefficient of the above-mentioned secondary battery at 25°C is 1×10⁻⁶. -11 cm 2 / s~1×10 -4 cm 2 / s.

[0173] The ion diffusion coefficient of this application is used to characterize the lithium ion transport capability in a secondary battery. The specific test method can adopt any conventional measurement method in the art, which will be described in detail in the following embodiments.

[0174] In these embodiments, this application discloses that the ion diffusion coefficient of the aforementioned secondary battery at 25°C is 1×10⁻⁶. - 11 cm 2 / s, 1×10 -10 cm 2 / s, 1×10 -9 cm 2 / s, 1×10 -8 cm 2 / s, 1×10 -7 cm 2 / s, 1×10 -6 cm 2 / s, 1×10 - 5 cm 2 / s, 1×10 -4 cm 2 Any one of / s or any one of the ranges of the above two.

[0175] In some embodiments, the electronic conductivity of the above-mentioned positive electrode particles at 25°C is 1×10⁻⁶. -12 S / cm~1×10 - 3 S / cm.

[0176] The electronic conductivity of this application is used to characterize the conductivity of the positive electrode particles in a secondary battery. Specific testing methods can employ any conventional measurement techniques in the art, which will be detailed in subsequent embodiments.

[0177] In these embodiments, this application discloses that the electronic conductivity of the above-mentioned positive electrode particles at 25°C is 1×10⁻⁶. -12 S / cm, 1×10 -11 S / cm, 1×10 -10 S / cm, 1×10 -9 S / cm, 1×10 -8 S / cm, 1×10 -7 S / cm, 1×10 -6 S / cm, 1×10 -5 S / cm, 1×10 -4 S / cm, 1×10 -3 Any of the values ​​in S / cm or any of the values ​​within the range of either of the above two.

[0178] In some embodiments, the mass percentage content of the above-mentioned positive electrode particles is 95% to 99% based on the total mass of the film layer on one side of the positive electrode sheet;

[0179] The aforementioned positive electrode sheet includes a conductive agent, which includes one or more of graphite, carbon black, carbon dots, acetylene black, graphene, carbon nanotubes, and carbon nanofibers.

[0180] In these embodiments, this application discloses that, based on the total mass of the single-sided film layer of the positive electrode sheet, the mass percentage content of the positive electrode particles is any one of 95%, 96%, 97%, 98%, 99%, or any one of the ranges of both of the above.

[0181] The positive electrode sheet of this application includes a positive electrode film layer containing positive electrode particles as positive electrode active material, and the conductive agents listed above, as well as a binder. The binder may include, but is not limited to, one or more of the following: polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), terpolymer of PVDF-tetrafluoroethylene-propylene, terpolymer of PVDF-hexafluoropropylene-tetrafluoroethylene, terpolymer of tetrafluoroethylene-hexafluoropropylene, fluorinated acrylate resin, styrene-butadiene rubber, polyacrylic acid, sodium polyacrylate, polyacrylamide, polyvinyl alcohol, sodium alginate, polymethacrylic acid, carboxymethyl chitosan, etc.

[0182] The method of forming the positive electrode film layer in this application includes mixing the above-mentioned raw materials with a solvent (such as N-methylpyrrolidone) in a certain mass ratio to form a positive electrode slurry, uniformly coating the positive electrode slurry on both sides of the positive electrode current collector, controlling the coating weight on one side, and after drying, compacting it to a certain compaction density using a cold press to obtain a positive electrode sheet containing the positive electrode film layer.

[0183] [Negative electrode plate]

[0184] The negative electrode sheet includes a negative current collector and a negative electrode film layer located on at least one surface of the negative current collector. The negative electrode film layer includes a negative electrode active material, a conductive agent, a binder, and a dispersant. The negative electrode film layer of this application may be located on one or both sides of the negative current collector. The following discussion of the negative electrode film layer in this application is based on the assumption that it is located on both sides of the negative current collector.

[0185] The negative electrode active material in this application includes carbonaceous materials, which include one or more combinations of artificial graphite, natural graphite, soft carbon, and hard carbon. Among them, artificial graphite, natural graphite, soft carbon, and hard carbon include any form of material conventional in the art, and include any manufacturer and model conventional in the art. Meanwhile, the negative electrode active material may also include silicon-based materials, which include one or two of silicon-oxygen materials or silicon-carbon materials. In addition, the negative electrode active material may also include silicon-carbon composites, Li-Sn alloys, Li-Sn-O alloys, Sn, SnO, SnO2, TiO2-Li4Ti5O 12 Li-Al alloys are used. However, this application is not limited to these materials; other conventional materials that can be used as negative electrode active materials for lithium-ion batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.

[0186] The conductive agents in this application include any type conventional in the art, such as graphite, superconducting carbon, carbon black (e.g., acetylene black, Ketjen black, Super P, etc.), carbon dots, carbon nanotubes, graphene, and carbon nanofibers, or a combination of two or more of these. The dispersants in this application also include any type conventional in the art, such as cellulose and its salts, specifically including, but not limited to, methylcellulose, carboxymethylcellulose, hydroxyethylcellulose, sodium carboxymethylcellulose, lithium carboxymethylcellulose, etc. The binders in this application include one or more of styrene-butadiene rubber (SBR), water-soluble unsaturated resin SR-1B, waterborne acrylic resins (e.g., polyacrylic acid PAA, polymethacrylic acid PMAA, sodium polyacrylate PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), and carboxymethyl chitosan (CMCS). Other optional additives may include thickeners (e.g., sodium carboxymethylcellulose CMC-Na), PTC thermistor materials, etc.

[0187] The negative electrode current collector in this application includes, but is not limited to, metal foil or composite current collector. The metal foil may be a copper foil, and the composite current collector may include a polymer material substrate and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector can be formed by forming a metal material, such as copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, on a polymer material substrate such as polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.

[0188] The positive electrode film layer of this application is formed by coating, for example, dissolving the components including the negative electrode active material and other components into water to form a negative electrode slurry, coating the negative electrode slurry onto the two surfaces of the current collector, and obtaining the positive electrode film layer after drying and cold pressing.

[0189] [Electrolytes]

[0190] In the field of batteries, the electrolyte can be selected from at least one of solid electrolytes, gel electrolytes, and liquid electrolytes (i.e., electrolyte solutions). The secondary battery of this application uses a liquid electrolyte, i.e., an electrolyte solution.

[0191] Some embodiments of this application disclose an electrolyte comprising an electrolyte salt and an organic solvent. The electrolyte salt includes any type conventional in the art, such as, but not limited to, inorganic metal salts, such as RClO4, RAsF6, RPF6, RBF4, RSbF6, RSO3F, RN(FSO2)2, etc.; fluorinated organometallic salts, such as RCF3SO3, RN(FSO2)(CF3SO2), RN(CF3SO2)2, RN(C2F5SO2)2, cyclic 1,3-hexafluoropropanedisulfonylimide lithium / sodium, cyclic 1,2-tetrafluoroethanedisulfonylimide lithium / sodium, RN(CF3SO2)(C4F5SO2)2, etc. Lithium ions include lithium ions such as 9SO2, RC(CF3SO2)3, RPF4(CF3)2, RPF4(C2F5)2, RPF4(CF3SO2)2, RPF4(C2F5SO2)2, RBF2(CF3)2, RBF2(C2F5)2, RBF2(CF3SO2)2, and RBF2(C2F5SO2)2; as well as metal salts containing dicarboxylic acid complexes, such as lithium bis(oxalate)borate, lithium difluorooxalate borate, lithium tri(oxalate)phosphate, lithium difluorobis(oxalate)phosphate, and lithium tetrafluoro(oxalate)phosphate. Here, both the metal and R represent one or two combinations of lithium ions.

[0192] According to some embodiments of this application, the concentration of the electrolyte salt in the electrolyte is 0.1 mol / L to 4 mol / L. In these embodiments, this application discloses that the concentration of the electrolyte salt is any one of 0.1 mol / L, 0.2 mol / L, 0.3 mol / L, 0.4 mol / L, 0.5 mol / L, 0.6 mol / L, 0.7 mol / L, 0.8 mol / L, 0.9 mol / L, 1 mol / L, 1.2 mol / L, 1.5 mol / L, 1.8 mol / L, 2 mol / L, 2.2 mol / L, 2.5 mol / L, 2.8 mol / L, 3 mol / L, 3.2 mol / L, 3.5 mol / L, 3.8 mol / L, and 4 mol / L, or any one of the above ranges.

[0193] According to some embodiments of this application, the organic solvent comprises one or two of carbonates, carboxylic esters, nitrile solvents, and sulfone solvents. The carboxylic esters comprise one or more of ethyl acetate (EA), methyl acetate (MA), ethyl propionate (EP), propyl acetate (PA), methyl propionate (MP), methyl butyrate (MB), ethyl butyrate (EB), and 1,4-butyrolactone (GBL). The carbonates comprise one or more of ethylene carbonate (EC), propylene carbonate (PC), vinylene carbonate, dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl ethyl carbonate (EMC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butyl carbonate (BC), and fluoroethylene carbonate (FEC). The nitrile solvents comprise one or more of acetonitrile (AN), glutaronitrile (GLN), and adiponitrile (ADN). Sulfone solvents include at least one or a combination of two of sulfolane (SF), dimethyl sulfone (MSM), ethyl sulfone (EMS), and diethyl sulfone (ESE).

[0194] According to some embodiments of this application, the electrolyte further comprises a film-forming stabilizer, which includes a positive electrode film-forming stabilizer and a negative electrode film-forming stabilizer. The positive electrode film-forming stabilizer comprises carbonate additives and / or sulfate additives. The carbonate additives include one or more of vinylene carbonate (VC), fluoroethylene carbonate (FEC), difluoroethylene carbonate (DFEC), vinyl ethylene carbonate (VEC), and dioctyl carbonate (CC). The sulfate additives include cyclic sulfonate additives and / or sulfated hydrocarbon ester additives; further, the cyclic sulfonate additives include one or more of 1,3-propanesulfonate lactone (PS), propenesulfonate lactone (PES), and 3-fluoro-1,3-propanesulfonate lactone (FPS); the sulfated hydrocarbon ester additives include one or more of vinyl sulfate (DTD), diethyl sulfate (DES), and dimethyl sulfate (DMS). The negative electrode film-forming stabilizer includes one or more of boron lithium salts, phosphorus-containing lithium salts, and sulfur-containing lithium salts; boron-containing lithium salts include one or more of lithium tetrafluoroborate (LiBF4), lithium bis(oxalate)borate (LiBOB), and lithium bis(oxalate)borate (LiDFOB); phosphorus-containing lithium salts include one or more of lithium difluorophosphate (LiPO2F2), lithium fluorophosphate (Li2PO3F), and lithium phosphate (Li3PO4). Sulfur-containing lithium salts include one or more of lithium fluorosulfonate (LiFSO3), lithium sulfate (Li2SO4), and lithium aminosulfonate (LiSO3NH2).

[0195] [Isolation Component]

[0196] In some embodiments, the secondary battery further includes a separator. This application does not impose any particular limitation on the type of separator; any known porous membrane with good chemical and mechanical stability can be selected.

[0197] In some embodiments, the separator includes a substrate material layer and a coating disposed on the surface of the substrate material layer; the substrate material layer includes one or more of polyethylene, polypropylene, poly(p-phenylene terephthalamide), polyethylene terephthalate, polytetrafluoroethylene, polyacrylonitrile, polyimide, and polyamide; the coating includes a ceramic coating and / or a polymer coating. The substrate material layer has good lithium-ion permeability, which is beneficial to lithium-ion migration; the coating disposed on the surface of the substrate material layer can further improve the mechanical properties of the separator. Optionally, the ceramic particles in the ceramic coating include one or more of SiO2, Al2O3, AlOOH, CaO, TiO2, MgO, ZnO, ZrO2, Mg(OH)2, and BaSO4. Optionally, the polymer material of the polymer coating includes one or more of polyethylene (PE), polypropylene (PP), poly(p-phenylene terephthalamide) (PPTA), polyethylene terephthalate (PET), polytetrafluoroethylene (PTFE), polyacrylonitrile (PAN), polyimide (PI), and polyamide (PA). The polymer coating can be made of the same or different material as the substrate material layer, and the thicknesses of the polymer coating and the substrate material layer can be different. Optionally, the thickness of the polymer coating is less than the thickness of the substrate material layer.

[0198] In other embodiments, the material of the separator can be selected from at least one of glass fiber, nonwoven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.

[0199] The secondary battery of this application will be described in detail below with reference to specific embodiments.

[0200] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods.

[0201] Unless otherwise specified, all materials and reagents used in the following examples are commercially available.

[0202] This application may employ conventional inorganic chemistry techniques within the art. In the following examples, efforts have been made to ensure the accuracy of the figures used (including quantities, temperatures, reaction times, etc.), but some experimental errors and biases should be considered. Temperatures (in degrees Celsius) used in the following examples are expressed in °C, and pressures are at or near atmospheric pressure. All reagents were purchased from AR-grade suppliers, and all reactions were carried out under argon protection. Unless otherwise stated, all reagents were obtained commercially.

[0203] [Preparation of positive electrode particles]

[0204] This application discloses a method for preparing positive electrode particles in some embodiments, and the specific preparation process is as follows:

[0205] Preparation of lithium manganese iron phosphate precursor: Lithium source, phosphorus source, manganese source and iron source are dispersed in a first solvent and subjected to precipitation reaction to obtain precipitate. The precipitate is washed, filtered, ball-milled, dried and crushed to obtain dry powder. The above dry powder is placed in an inert atmosphere and the sintering temperature is controlled at 450℃~550℃ to obtain lithium manganese iron phosphate precursor.

[0206] Preparation of cathode particles: Take the reaction raw materials used to prepare nanocrystalline lithium metal salt and disperse them with the above-mentioned lithium manganese iron phosphate precursor in a second solvent, mix them evenly and dry them. In an inert atmosphere, control the sintering temperature to be 750℃~890℃ to obtain cathode particles.

[0207] The specific types of raw materials used in this application to prepare lithium manganese iron phosphate precursors include any conventional methods in the art. For example, lithium sources include, but are not limited to, any one or more of lithium carbonate, lithium hydroxide, lithium dihydrogen phosphate, or lithium acetate; iron sources include, but are not limited to, any one or more of iron oxide, iron sulfate, iron oxalate, and iron phosphate; manganese sources include, but are not limited to, any one or more of manganese tetroxide, manganese carbonate, manganese acetate, manganese pyrophosphate, manganese oxalate, manganese oxide, and manganese sulfate; and phosphorus sources include, but are not limited to, any one or more of ammonium dihydrogen phosphate, lithium dihydrogen phosphate, lithium monohydrogen phosphate, lithium phosphate, pyrophosphate, and ammonium phosphate.

[0208] The specific types of raw materials used in this application for preparing nanocrystalline lithium metal salts include any conventional methods in the art. For example, if the nanocrystalline lithium metal salt is a garnet-type lithium metal salt, then the lithium source used to prepare the garnet-type lithium metal salt includes any one or more of lithium carbonate, lithium hydroxide, lithium dihydrogen phosphate, or lithium acetate; the lanthanum (La) source includes La2O3, the zirconium (Zr) source includes ZrO2, and the tantalum (Ta) source includes Ta2O5.

[0209] This application discloses another method for preparing positive electrode particles in some embodiments. The difference between this method and the above-mentioned method is that a nanocrystalline lithium metal salt precursor is prepared. Specifically, the reactants used to prepare the nanocrystalline lithium metal salt are dispersed in a third solvent and then precipitated and dried to obtain a powder containing microcrystals or amorphous shapes.

[0210] The above-mentioned nanocrystalline lithium metal salt precursor and the above-mentioned lithium manganese iron phosphate precursor are then dispersed in a second solvent, mixed, dried, and sintered to obtain positive electrode particles.

[0211] In some embodiments, this application also discloses adding a carbon source during the preparation of cathode particles to generate a coating layer with shaped carbon and / or amorphous carbon.

[0212] In these embodiments, the carbon source disclosed in this application includes any material conventional in the art, such as PVA, sucrose, PEG, glucose, citric acid, graphene, etc.

[0213] In these embodiments, this application discloses that the first solvent, the second solvent, and the third solvent are each independently selected from deionized water or an organic solvent, such as ethanol.

[0214] Preparation Example 1-1

[0215] Li7La3Zr2O was prepared 12 Doped lithium manganese iron phosphate (LiFe) 0.4 Mn 0.6 The specific preparation steps for PO4 positive electrode particles are as follows:

[0216] Preparation of lithium manganese iron phosphate precursor: 766g LiOH, 3325g NH4H2PO4, 2899g MnSO4, and 1945g FeSO4 were added to 14kg of pure water. After the resulting mixed solution was stirred and reacted, the precipitate was washed, filtered, ball-milled, dried, and crushed to obtain a dry powder. The dry powder was then placed in a nitrogen atmosphere sintering furnace and sintered at 500℃ for 3 hours to obtain the lithium manganese iron phosphate precursor.

[0217] Preparation of cathode particles: The lithium manganese iron phosphate precursor obtained above, 1 kg glucose, 54.3 g LiOH, 158.3 g La2O3 and 79.8 g ZrO2 were added to ethanol, ground in a sand mill for 2 h and then filtered through a 400 mesh sieve. Citric acid was added to the mixed slurry for complexation. After filtration, the mixture was dried in a fluidized bed to obtain a dry powder. The powder was then sintered in a nitrogen atmosphere furnace at 800℃ for 6 h, cooled and removed, and crushed until it could completely pass through an 800 mesh sieve to obtain cathode particles.

[0218] Among them, based on the total mass of the cathode particles, the nanocrystalline lithium metal salt (Li7La3Zr2O) located between the primary particles... 12 The mass percentage content of the coating is 5%, and the thickness of the coating layer is 20 nm; the mass of shaped carbon and / or amorphous carbon in the coating layer is equal to that of the nanocrystalline lithium metal salt (Li7La3Zr2O). 12 The mass ratio between the masses is 2:1, and the particle size Dv50 of the nanocrystalline lithium metal salt in the coating layer is 10 nm.

[0219] This application discloses a method for measuring the coating thickness in this embodiment. The electrode sheet before cold pressing is cut into 6cm x 6cm samples using scissors, and then polished using an IB-19500CP ion section polisher to obtain a polished sample with a cut surface. The sample is then tested using a ZEISS sigma 300 instrument according to standard JY / T010-1996. Ten different locations are randomly selected from the above test samples for testing, and the average value is taken. The method for measuring the coating thickness in the following preparation examples is the same as in this preparation example, and will not be repeated here.

[0220] Preparation Examples 1-2

[0221] Li7La3Zr2O was prepared 12 Doped lithium manganese iron phosphate (LiFe) 0.4 Mn 0.6 The difference between this preparation example and the preparation example 1 above is that in the preparation of the positive electrode particles: nanocrystalline lithium metal salt (Li7La3Zr2O) is first prepared. 12 Precursor: Specifically, 54.3g LiOH, 158.3g La2O3 and 79.8g ZrO2 were added to ethanol, and after precipitation, drying and sintering, a powder containing microcrystals or amorphous shape was obtained.

[0222] Then, the nanocrystalline lithium metal salt (Li7La3Zr2O) prepared above is... 12 The precursor, lithium manganese iron phosphate precursor prepared in Example 1-1 above, was added to ethanol with 1 kg of glucose. After grinding in a sand mill for 2 hours, it was filtered through a 400-mesh sieve. The mixed slurry was filtered and then dried in a fluidized bed to obtain a dry powder. It was placed in a nitrogen atmosphere furnace at 800°C for 6 hours, cooled down and removed, and crushed until it could completely pass through an 800-mesh sieve to obtain positive electrode particles.

[0223] Among them, based on the total mass of the cathode particles, the nanocrystalline lithium metal salt (Li7La3Zr2O) located between the primary particles... 12 The mass percentage content of the coating is 5%, and the thickness of the coating layer is 25 nm; the mass of shaped carbon and / or amorphous carbon in the coating layer is related to the mass of the nanocrystalline lithium metal salt (Li7La3Zr2O). 12 The mass ratio between the two masses is 2:1.

[0224] Preparation Examples 1-3

[0225] Li7La3Zr2O was prepared 12 Doped lithium manganese iron phosphate (LiFe) 0.4 Mn 0.6 PO4) positive electrode particles. This preparation example differs from Preparation Example 1-1 in that the amount of each raw material added is adjusted to:

[0226] Among them, based on the total mass of the cathode particles, the nanocrystalline lithium metal salt (Li7La3Zr2O) located between the primary particles... 12 The mass percentage content of the coating is 20%, and the thickness of the coating layer is 500 nm; the mass of shaped carbon and / or amorphous carbon in the coating layer is equal to that of the nanocrystalline lithium metal salt (Li7La3Zr2O). 12 The mass ratio between them is 0.03:1.

[0227] Preparation Examples 1-4

[0228] Li7La3Zr2O was prepared 12 Doped lithium manganese iron phosphate (LiFe) 0.4 Mn 0.6 PO4) positive electrode particles. This preparation example differs from Preparation Example 1-1 in that the amount of each raw material added is adjusted to:

[0229] Among them, based on the total mass of the cathode particles, the nanocrystalline lithium metal salt (Li7La3Zr2O) located between the primary particles... 12 The mass percentage content of the coating is 0.3%, and the thickness of the coating layer is 1 nm; the coating layer contains shaped carbon and / or amorphous carbon and nanocrystalline lithium metal salt (Li7La3Zr2O) 12 The mass ratio between them is 50:1.

[0230] Preparation Examples 1-5

[0231] Li5La3Ta2O was prepared 12 Doped lithium manganese iron phosphate (LiFe) 0.4 Mn 0.6 The positive electrode particles prepared in this example differ from those prepared in Example 1 above in that the lithium manganese iron phosphate precursor, 1 kg glucose, 38.8 g LiOH, 158.3 g La2O3, and 143.1 g Ta2O5 prepared above are added to ethanol; otherwise, they are the same as those prepared in Example 1.

[0232] Among them, based on the total mass of the cathode particles, the nanocrystalline lithium metal salt (Li5La3Ta2O) located between the primary particles... 12 The mass percentage content of the coating is 5%, and the thickness of the coating layer is 20 nm; the coating layer contains amorphous carbon and nanocrystalline lithium salt (Li5La3Ta2O) 12 The mass ratio between them is 1:2.

[0233] Preparation Examples 1-6

[0234] Li7La3Zr2O was prepared 12 Lithium manganese iron phosphate (LiFe) doped with nickel 0.39 Mn0.58 Ni 0.03 The positive electrode particles (PO4) differ from Preparation Example 1 above in that 110g of nickel phosphate is added during the preparation of the lithium manganese iron phosphate precursor. Otherwise, they remain the same as in Preparation Example 1-1. The lithium manganese iron phosphate obtained in this example has the chemical formula LiFe. 0.39 Mn 0.58 Ni 0.03 PO4, based on the total mass of the cathode particles, refers to the nanocrystalline metallic lithium salt (Li7La3Zr2O) located between the primary particles. 12 The mass percentage content of the coating layer is 4.9%, and the thickness of the coating layer is 20 nm; the mass of shaped carbon and / or amorphous carbon in the coating layer is related to the mass of the nanocrystalline lithium metal salt (Li7La3Zr2O). 12 The mass ratio between the two masses is 2:1.

[0235] Preparation Example 2

[0236] LISICON-type lithium metal salts (Li) were prepared 10 Ge 0.8 Al 0.2 P2S 11.6 Se 0.3 Lithium manganese iron phosphate (LiFe) doped 0.4 Mn 0.6 The difference between this preparation example and the preparation example 1-1 above is that:

[0237] Preparation of cathode particles: The lithium manganese iron phosphate precursor obtained in Preparation Example 1-1, 1 kg of glucose, 147.0 g of Li2S, 142.3 g of P2S5, 70.0 g of GeS2, and 8.8 g of Al2Se3 were added to ethanol, ground in a sand mill for 2 hours, and then filtered through a 400-mesh sieve. Citric acid was added to the mixed slurry for complexation. After filtration, the mixture was dried in a fluidized bed to obtain a dry powder. The powder was then sintered in a nitrogen atmosphere furnace at 800°C for 6 hours, cooled down, and crushed until it could completely pass through an 800-mesh sieve to obtain cathode particles.

[0238] Among them, based on the total mass of the cathode particles, the nanocrystalline lithium metal salt (Li) located between the primary particles... 10 Ge 0.8 Al 0.2 P2S 11.6 Se 0.3 The mass percentage content of ) is 6.3%, and the thickness of the coating layer is 25 nm; the mass of shaped carbon and / or amorphous carbon in the coating layer is related to the mass of nanocrystalline lithium metal salt (Li 10 Ge 0.8 Al 0.2 P2S 11.6 Se 0.3The mass ratio between the two masses is 2:1.

[0239] Preparation Example 3

[0240] Perovskite-type lithium metal salts (Li) were prepared 0.5 La 0.5 TiO3-doped lithium manganese iron phosphate (LiFe) 0.4 Mn 0.6 PO4) positive electrode particles,

[0241] The difference between this preparation example and the above-mentioned preparation example 1-1 is as follows: For the preparation of cathode particles: the prepared lithium manganese iron phosphate precursor, 1 kg glucose, 217.8 g tetrabutyl titanate, 11.8 g lithium carbonate, and 52.1 g La₂O₃ were added to ethanol, ground in a sand mill for 2 hours, and then filtered through a 400-mesh sieve. Citric acid was added to the mixed slurry for complexation. After filtration, the mixture was dried in a fluidized bed to obtain a dry powder, which was then sintered in a nitrogen atmosphere furnace at 800°C for 6 hours. After cooling, the powder was removed and crushed until it completely passed through an 800-mesh sieve to obtain cathode particles. Among these, based on the total mass of the cathode particles, the nanocrystalline lithium metal salt (Li₂O₃) located between the primary particles... 0.5 La 0.5 The TiO3 content is 5% by mass, and the coating thickness is 25 nm; the mass of shaped carbon and / or amorphous carbon in the coating is related to the mass of nanocrystalline lithium salt (Li). 0.5 La 0.5 The mass ratio between TiO3 is 2:1.

[0242] [Materials Performance Testing]

[0243] The performance of the cathode particles prepared in Preparation Examples 1-1 to 1-6, Preparation Example 2 and Preparation Example 3 were characterized as follows:

[0244] (1) Volumetric particle size distribution Dv50 test:

[0245] The particle size distribution of each particle was obtained with reference to the standard GB / T19077-2016, and the particle size was determined by laser diffraction particle size analysis.

[0246] Among them, the Dv50 of nanocrystalline lithium metal salt located between primary particles, the Dv50 of nanocrystalline lithium metal salt located in the coating layer, and the Dv50 of primary particles and cathode particles of lithium manganese iron phosphate are shown in Table 1-1.

[0247] Table 1-1

[0248]

[0249]

[0250] (2) Test of compaction density and electronic conductivity of positive electrode particles under 30000N pressure: Table 1-3 are obtained.

[0251] Test method for compacted density of powder at 30000N:

[0252] The calculation method is based on GB / T 24533-2009. For example, it can be measured using an electronic pressure testing instrument (e.g., UTM7305). A specific amount M of the powder sample to be tested is placed on a special mold (bottom area S0), and different pressures are set. Each pressure is maintained for 30 seconds, then released. After 10 seconds, the thickness H0 of the powder compressed under that pressure is read on the device. The compaction density under that pressure is calculated, and the compaction density of the positive electrode particles under that pressure is equal to M / (H0×S0).

[0253] Methods for testing the electronic conductivity of positive electrode powder particles:

[0254] As described in GB / T30835-2014, the above-mentioned positive electrode particle sample powder is pressed into a cylindrical sample using a pressing mold with a known pressing area. The resistance of the cylindrical sample is tested using an electrochemical workstation. Specifically, the prepared cylindrical sample is fixed in a three-electrode mold, and an AC impedance test is performed using an electrochemical workstation with an amplitude of 5mV and a frequency of 1000Hz. The absolute value of the reading on the horizontal axis of the electrochemical workstation test result is the resistivity R, in ohms (Ω). The conductivity γ (Siemens per centimeter, S / cm) is then obtained according to the formula: conductivity γ = h / S × R.

[0255] In the above formula, h refers to the tableting height in centimeters (cm), and S refers to the area of ​​the tableting mold in square centimeters (cm²). 2 ).

[0256] The compacted density and electronic conductivity of the powders obtained using the above measurement methods are shown in Table 1-2.

[0257] Table 1-2

[0258]

[0259]

[0260] (3) The ionic conductivity of the secondary battery at 25℃ was tested. The specific test process included:

[0261] The cathode particles of the above preparation examples were fabricated into secondary batteries according to the design method described in the following examples;

[0262] The Li was studied using the galvanostatic intermittent titration (GITT) method. +Diffusion coefficient in the electrode. GITT curve and corresponding lithium-ion diffusion coefficient (D). Li+ In the GITT study, the battery was charged and discharged at a current density of 0.1C, followed by a 1-hour open-circuit step to allow it to relax back to equilibrium. This process was continued until the charge (or discharge) voltage reached 4.3V (2V). Li can be calculated using the equations outlined by Weppner and Huggins. + The diffusion coefficient. If a sufficiently small current is applied over a short time interval, and the coulometric titration curve can be considered linear over the compositional range involved in this step, the D of the electrode material... Li+ It can be calculated using the formula:

[0263]

[0264] Where m B V M and M B denoted by , respectively, the active mass load; , respectively, the volume and molar mass; S is the surface area of ​​the electrode; τ is the duration of the constant current pulse; and ΔEτ is the total voltage change during the current pulse. s It refers to the change in steady-state voltage during constant current titration.

[0265] Table 1-3 were obtained according to the above measurement method.

[0266] Table 1-3

[0267]

[0268] Example 1-1

[0269] A secondary battery is provided, comprising a positive electrode, a separator, and a negative electrode stacked sequentially, and an electrolyte.

[0270] Preparation of positive electrode sheet:

[0271] The positive electrode particles, conductive carbon black, carbon nanotubes, and PVDF prepared in Example 1-1 were mixed together in a ratio of 96.5:2:0.5:1. After adding N-methylpyrrolidone solvent and stirring, a positive electrode slurry with a solid content of 60% was formed. This slurry was coated onto both surfaces of the positive electrode current collector aluminum foil and dried using a multi-section oven at sequential temperatures of 120℃ / 100℃ / 90℃. The resulting positive electrode sheet was then compacted using a cold press, yielding a compacted density of 2.7 g / cm³. 3 The positive electrode sheet has a single-sided coating weight of 0.34g / 1540.25mm. 2 .

[0272] Preparation of negative electrode sheet:

[0273] Artificial graphite, conductive carbon black, sodium carboxymethyl cellulose stabilizer, and SBR binder were dispersed in deionized water at a mass ratio of 96.2:1.8:1.2:0.8 to form a negative electrode slurry. This slurry was then uniformly coated onto both sides of the copper foil used as the negative electrode current collector. The foil was dried in a nine-section oven at sequential temperatures of 100℃ / 100℃ / 95℃ / 85℃ / 85℃ / 80℃ / 80℃ / 80℃ / 60℃. Finally, the foil was compacted using a cold press to achieve a single-sided coating weight of 0.15g / 1540.25mm. 2 .

[0274] Preparation of electrolyte:

[0275] In an argon atmosphere glove box (H2O < 0.1 ppm, O2 < 0.1 ppm), non-aqueous organic solvents ethylene carbonate and ethyl methyl carbonate are mixed at a volume ratio of 3:7 to obtain a first solvent. Ethyl acetate and propyl acetate are mixed at a volume ratio of 2:1 to obtain a second solvent. The first and second solvents are mixed in a certain amount to form a non-aqueous solvent. Lithium hexafluorophosphate is added to the non-aqueous solvent, followed by film-forming stabilizers (lithium fluorosulfonate and lithium difluorophosphate) to prepare an electrolyte with a lithium hexafluorophosphate concentration of 12.5%. The amount of film-forming stabilizer added is 0.01 wt% (based on the total mass of the electrolyte).

[0276] Provide isolation components:

[0277] Polypropylene film with a thickness of 12µm is used as the separator.

[0278] Preparation of secondary batteries:

[0279] The positive electrode, separator, and negative electrode are stacked in sequence, with the separator acting as a separator between the positive and negative electrodes. Three copper wires are added for the electrodes, and the tabs are welded together to form a stacked bare cell. The stacked bare cell is placed in an outer packaging shell, dried, and then injected with electrolyte. After vacuum sealing, settling, formation, and shaping, a lithium-ion battery is obtained.

[0280] Examples 1-2 to 1-6 provide a secondary battery, as detailed below:

[0281] Examples 1-2

[0282] A secondary battery is provided, which differs from Example 1-1 in that the positive electrode particles of Preparation Example 1-1 are replaced with the positive electrode particles of Preparation Example 1-2, while all other aspects remain the same as Example 1-1.

[0283] Examples 1-3

[0284] A secondary battery is provided, which differs from Example 1-1 in that the positive electrode particles of Preparation Example 1-1 are replaced with the positive electrode particles of Preparation Example 1-3, while all other aspects remain the same as Example 1-1.

[0285] Examples 1-4

[0286] A secondary battery is provided, which differs from Example 1-1 in that the positive electrode particles of Preparation Example 1-1 are replaced with the positive electrode particles of Preparation Example 1-4, while all other aspects remain the same as Example 1-1.

[0287] Examples 1-5

[0288] A secondary battery is provided, which differs from Example 1-1 in that the positive electrode particles of Preparation Example 1-1 are replaced with the positive electrode particles of Preparation Example 1-5, while all other aspects remain the same as Example 1-1.

[0289] Examples 1-6

[0290] A secondary battery is provided, which differs from Example 1-1 in that the positive electrode particles of Preparation Example 1-1 are replaced with the positive electrode particles of Preparation Example 1-6, while all other aspects remain the same as Example 1-1.

[0291] Examples 2 and 3 provide a secondary battery, as detailed below:

[0292] Example 2

[0293] A secondary battery is provided, which differs from Example 1-1 in that the positive electrode particles of Preparation Example 1-1 are replaced with the positive electrode particles of Preparation Example 2, while all other aspects remain the same as Example 1-1.

[0294] Example 3

[0295] A secondary battery is provided, which differs from Example 1-1 in that the positive electrode particles of Preparation Example 1-1 are replaced with the positive electrode particles of Preparation Example 3, while all other aspects remain the same as Example 1-1.

[0296] Comparative Example 1

[0297] A secondary battery is provided, wherein the positive electrode particles are lithium manganese iron phosphate. In the preparation of the positive electrode particles, the aforementioned lithium manganese iron phosphate precursor is added to 1 kg of glucose in ethanol, ground in a sand mill for 2 hours, and then filtered through a 400-mesh sieve. Citric acid is added to the mixed slurry for complexation, and after filtration, the mixture is dried in a fluidized bed to obtain a dry powder. This powder is then sintered in a nitrogen atmosphere furnace at 800°C for 6 hours, cooled, and crushed until it completely passes through an 800-mesh sieve to obtain the positive electrode particles. Other aspects remain the same as in Examples 1-1.

[0298] Comparative Example 2

[0299] A secondary battery is provided, wherein the positive electrode particles of the secondary battery are lithium manganese iron phosphate, and the coating layer of lithium manganese iron phosphate contains nanocrystalline metallic lithium salt.

[0300] The specific preparation process is as follows:

[0301] Preparation of lithium manganese iron phosphate particles: 1 kg of glucose, 766 g of LiOH, 3325 g of NH4H2PO4, 2899 g of MnSO4, and 1945 g of FeSO4 were added to 14 kg of solvent. After the resulting mixed solution was stirred and reacted, the precipitate was washed, filtered, ball-milled, dried, and crushed to obtain a dry powder. The dry powder was then placed in a nitrogen atmosphere sintering furnace and sintered at 800℃ for 6 h to obtain the lithium manganese iron phosphate precursor.

[0302] Further preparation of nanocrystalline lithium metal salt (Li7La3Zr2O) 12 Materials: Specifically, 54.3g LiOH, 158.3g La2O3 and 79.8g ZrO2 were added to a solvent, and nanocrystalline lithium salts were obtained by precipitation, drying and sintering (900℃, 8h).

[0303] The two materials were mixed evenly in a solvent, filtered, dried, sintered (800℃, 6h), cooled and removed, and crushed until they completely passed through an 800-mesh sieve to obtain positive electrode particles.

[0304] [Battery parameter test]

[0305] ① Discharge specific capacity corresponding to 1C: At 25℃, the batteries corresponding to the examples and comparative examples were charged to 3.65V at a constant current of 1 / 3*C, then charged to a current of 0.05C at a constant voltage of 3.65V. After resting for 5 minutes, they were discharged to 2.5V at 1C. The discharge capacity Q1 was recorded. The discharge specific capacity = discharge capacity Q1 / mass of positive electrode active material.

[0306] 1C corresponds to the following charging capacity:

[0307] At 25°C, the batteries corresponding to the examples and comparative examples were charged to 3.65V with a constant current of 1 / 3*C, and then charged to 0.05C with a constant voltage of 3.65V. The charging capacity Q2 was recorded. Then, the charging capacity = charging capacity Q2 / mass of positive electrode active material.

[0308] ② Battery capacity retention test after 2000 cycles at 25℃:

[0309] Using the Shenzhen Xinwei Battery Testing System, at 25℃, the batteries corresponding to the examples and comparative examples were charged to 3.65V at a constant current of 1 / 3*C, then charged to a constant voltage of 3.65V until the current was 0.05C. After resting for 5 minutes, they were discharged to 2.5V at 1C. The discharge capacity Q1 was recorded. The battery was cycled 2000 times under the above charge-discharge conditions. The discharge capacity on the 2000th cycle was Q1'. Therefore, the capacity retention rate = Q1' / Q1 × 100%.

[0310] ③ Battery storage performance test at 60℃: The batteries corresponding to the examples and comparative examples were placed in a 60℃ constant temperature furnace. Every 7 days, they were taken out and charged and discharged at a 1C rate. Specifically, they were charged at a constant current of 1 / 3*C to 3.65V, then charged at a constant voltage of 3.65V to a current of 0.05C, rested for 5 minutes, and then discharged at 1C to 2.5V. The discharge capacity Q1 was recorded. Then, they were charged at a constant current of 1 / 3*C to 3.65V, and then charged at a constant voltage of 3.65V to a current of 0.05C. They were then placed back in the 60℃ constant temperature furnace. After another 7 days, the above operation was repeated. This process was repeated for 420 days to obtain the final measured discharge capacity Q1``. The capacity retention rate is calculated as Q1`` / Q1×100%.

[0311] The specific test results of each embodiment and comparative battery obtained according to the above test method are shown in Table 2 below:

[0312] Table 2

[0313]

[0314] As can be seen from the embodiments in Table 2 and Comparative Example 1, the design provided in this application is beneficial to improving the cycle life and storage performance of the battery. Further comparison of the embodiments, Comparative Example 1, and Comparative Example 2 shows that by generating nanocrystalline metallic lithium salts at at least part of the interfaces between primary lithium manganese iron phosphate particles, it is beneficial to construct a robust and unobstructed lithium-ion transport pathway. This improves the battery's cycle life and storage performance by enhancing the conductivity and structural stability of lithium manganese iron phosphate. Simultaneously, it maximizes the specific capacity of lithium manganese iron phosphate by improving lithium-ion transport capability.

[0315] As can be seen from Examples 1-1, 1-3 and 1-4, compared with the content of nanocrystalline lithium metal salt in the cathode particles, its crystalline particle size is more important for constructing a robust and unobstructed lithium-ion transport pathway, and a suitable particle size is beneficial for constructing a lithium-ion transport pathway.

[0316] As can be seen from Examples 1-1, 2 and 3, different types of nanocrystalline lithium metal salts have different effects on battery performance. The garnet-type lithium metal salt illustrated in Example 1-1 can better utilize the specific capacity of the positive electrode active material and improve the battery's cycle performance and high-temperature storage performance.

[0317] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of this application, and not to limit them. Although this application has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features therein. These modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of this application, and they should all be covered within the scope of the claims and specification of this application. In particular, as long as there is no structural conflict, the various technical features mentioned in the embodiments can be combined in any way. This application is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.

Claims

1. A secondary battery, characterized in that: Includes a positive electrode, a negative electrode, and a separator disposed between the positive electrode and the negative electrode; The positive electrode sheet includes positive electrode particles, the positive electrode particles include lithium manganese iron phosphate, the lithium manganese iron phosphate includes secondary particles composed of multiple primary particles, and the positive electrode particles include nanocrystalline lithium metal salt, the nanocrystalline lithium metal salt being located at at least a portion of the interface between the primary particles; The nanocrystalline lithium metal salt includes lithium, oxalic group elements and other elements, wherein the other elements include any two or more of phosphorus, aluminum, titanium, zirconium, hafnium, niobium, tantalum, tin, scandium, germanium and lanthanides.

2. The secondary battery according to claim 1, characterized in that: Based on the total mass of the cathode particles, the mass percentage content of the nanocrystalline metallic lithium salt located between the primary particles is 0.3% to 20%. and / or; The volumetric particle size distribution Dv50 of the nanocrystalline lithium metal salt located between the primary particles is 1 nm to 200 nm.

3. The secondary battery according to any one of claims 1 to 2, characterized in that: The positive electrode particles have a coating layer disposed on at least a portion of the surface of the lithium manganese iron phosphate, and the coating layer comprises a nanocrystalline metallic lithium salt.

4. The secondary battery according to claim 3, characterized in that: The thickness of the coating layer is 1 nm to 500 nm; and / or; The coating layer comprises shaped carbon and / or amorphous carbon, wherein the mass ratio between the mass of the shaped carbon and / or amorphous carbon and the mass of the nanocrystalline lithium metal salt in the coating layer is (0.025~50):

1. and / or; The volumetric particle size distribution Dv50 of the nanocrystalline lithium metal salt in the coating layer is 1 nm to 500 nm.

5. The secondary battery according to any one of claims 1 to 4, characterized in that: The nanocrystalline lithium metal salt includes compounds illustrated by Chemical Formula I and Chemical Formula II, or Li 10 Ge 0.8 Al 0.2 P2S 11.6 Se 0.3 One or more of the following: Li 7-x La3Zr 2-x A x O 12 Chemical Formula I, Where A includes any one or more of the elements Ta, Nb, Sn, Hf, Sc, and Ge, and 0 ≤ x ≤ 0.75; Li 3a La 0.66-a TiO3 chemical formula II, Where 0 < a ≤ 0.

16.

6. The secondary battery according to any one of claims 1 to 5, characterized in that: The chemical formula of the lithium manganese iron phosphate is Li b Fe c Mn d M 1-c-d PO4; Wherein, M represents the doping element at the manganese and iron sites, and the doping element at the manganese and iron sites includes any one or more of Al, Cu, Mg, Zn, Ni, Ti, V, Zr, Co, Ga, Sn, Sb, and Nb. b ranges from 0.9 to 1.1; c ranges from 0.001 to 0.999; d ranges from 0.001 to 0.999; 1-cd is between 0 and 0.

1.

7. The secondary battery according to any one of claims 1 to 6, characterized in that: The volumetric particle size distribution Dv50 of the positive electrode particles is 0.2 μm to 17 μm; and / or; The compacted density of the positive electrode particles under a force of 30,000 N is 2.0 g / cm³. 3 ~2.6g / cm 3 ; and / or; The positive electrode particles have an electronic conductivity of 1×10⁻⁶ at 25°C. -12 S / cm~1×10 -3 S / cm.

8. The secondary battery according to any one of claims 1 to 7, characterized in that: The secondary battery has an ion diffusion coefficient of 1×10⁻⁶ at 25°C. -11 cm 2 / s~1×10 -4 cm 2 / s.

9. The secondary battery according to any one of claims 1 to 8, characterized in that: Based on the total mass of the single-sided film layer of the positive electrode sheet, the mass percentage content of the positive electrode particles is 95% to 99%. The positive electrode sheet includes a conductive agent, which includes one or more of graphite, carbon black, carbon dots, acetylene black, graphene, carbon nanotubes, and carbon nanofibers.