Secondary battery, method for manufacturing the same, and electric device
By forming a polymer coating layer containing benzoxazine rings on the surface of the positive electrode active material, the cationic polymerization reaction constructs a stable network at high temperature, which solves the problem of oxygen release during structural phase transition of nickel-containing ternary positive electrode materials at high temperature, and improves the thermal stability and mechanical strength of the secondary battery.
Patent Information
- Application Number
- CN202510668303.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-22
- Publication Date
- 2026-11-24
AI Technical Summary
Nickel-containing ternary cathode materials undergo structural phase transitions at high temperatures, releasing oxygen and causing electrolyte oxidation and decomposition, which affects the stability of secondary batteries. Existing surface coating methods cannot effectively improve thermal stability.
A polymer coating layer containing benzoxazine rings is formed on the surface of the positive electrode active material. A stable network structure is constructed at high temperature through cationic polymerization to prevent oxygen release and improve thermal stability.
It significantly improves the thermal stability of secondary batteries, reduces the risk of thermal runaway, and the polymer coating absorbs heat and cross-links at high temperatures to form a stable network, preventing oxygen release and improving mechanical strength.
Smart Images

Figure CN123162153A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of battery technology, and in particular to a secondary battery, its preparation method, and an electrical device thereof. Background Technology
[0002] Nickel-containing ternary cathode materials generally suffer from thermal stability issues, which become more pronounced with increasing nickel content. Under high-temperature environments or conditions of battery abuse, these materials undergo structural phase transitions, releasing large amounts of oxygen and triggering severe oxidative decomposition of the electrolyte, thus affecting the stability of the secondary battery.
[0003] Although there are examples of surface coating of nickel-containing ternary cathode materials to reduce direct contact with the electrolyte and thus suppress side reactions, this method does not effectively improve the thermal stability of secondary batteries. Summary of the Invention
[0004] In view of the above problems, this application provides a secondary battery, a method for preparing the same, and an electrical device thereof, with the aim of improving the thermal stability of the secondary battery.
[0005] In a first aspect, this application provides a secondary battery, including a positive electrode sheet, the positive electrode sheet including a positive electrode active material, the positive electrode active material including a core material and a polymer coating layer covering at least a portion of the surface of the core material, the polymer coating layer containing a benzoxazine ring; the core material including one of lithium-containing transition metal oxides.
[0006] In the technical solution of this application embodiment, the polymer coating layer contains a benzoxazine ring. The benzoxazine ring is a heterocycle formed by the fusion of a benzene ring and a six-membered heterocycle containing one nitrogen atom and one oxygen atom. When the battery system temperature rises to 150℃-200℃, the CO bond in the heterocycle gains sufficient energy to undergo heterolytic cleavage, forming an intramolecular ion pair. This ion pair rapidly attacks the phenoxy group adjacent to the benzoxazine ring. The positive ion in the ion pair combines with the carbon atom adjacent to the phenoxy group, giving the carbon atom a positive charge, thereby initiating a cationic polymerization reaction. On the one hand, the cationic polymerization reaction absorbs a large amount of heat, which helps to lower the system temperature. On the other hand, the cationic polymerization reaction causes the molecular chains to grow and cross-link, gradually building a more stable network structure. This network structure has higher stability and mechanical strength, and can act as a physical barrier, preventing the core material from releasing oxygen free radicals and oxygen at high temperatures due to structural instability, thus preventing crosstalk reactions. This further improves the thermal stability of the positive electrode active material and significantly reduces the risk of thermal runaway. Therefore, this application can significantly improve the thermal stability of secondary batteries using lithium-containing transition metal oxides as positive electrode active materials.
[0007] In some embodiments, the polymer coating layer comprises at least one of the compounds shown in formula (I) and formula (II): Formula (I), Equation (II), Wherein, R1 includes at least one of hydrogen atom, alkyl group, aromatic group, and halogen atom, R2 includes at least one of hydrogen atom, alkyl group, and aromatic group, and R includes one of alkylene groups.
[0008] In the technical solutions of this application embodiment, the compounds shown in formula (I) and formula (II) are both 1,3-benzoxazine, which have higher polymerization activity, can undergo ring-opening polymer reaction under heating conditions, and the resulting polymer coating layer has high thermal stability.
[0009] In some embodiments, the polymer coating layer comprises a benzoxazine oligomer, wherein the degree of polymerization n of the benzoxazine oligomer is 2-15.
[0010] In the technical solution of this application embodiment, when the degree of polymerization n of the benzoxazine oligomer is 2-15, the polymer coating layer contains some unpolymerized benzoxazine monomers. Therefore, the oligomer is not completely cross-linked and can be further cross-linked and cured when the battery system temperature rises, thereby absorbing heat and improving the barrier performance of the polymer coating layer.
[0011] In some embodiments, the polymer coating layer further comprises the chain segment represented by formula (III): Formula (III) Wherein, X includes at least one of nitrogen- and / or phosphorus-containing flame-retardant groups.
[0012] In the technical solution of this application embodiment, the introduction of X flame-retardant groups into the polymer coating layer can achieve thermal response crosslinking protection while giving the polymer coating layer flame-retardant properties, thereby further improving the thermal stability of the secondary battery.
[0013] In some embodiments, X includes at least one of melamine group, dicyandiamine group, guanidine salt group, phosphaphenanthrene group, phosphazene group, and nitrogen-containing phosphate group.
[0014] In the technical solution of this application embodiment, melamine groups and dicyandiamine groups can form a dense char layer during combustion, which plays a role in heat insulation and oxygen isolation, thereby preventing further combustion; guanidine salt groups have long-lasting flame retardant properties; phosphaphenanthrene groups can form a stable char layer at high temperatures, while releasing phosphorus-containing free radicals, which can play a flame retardant role in both the gas phase and condensed phase; phosphazene groups can decompose to produce phosphorus-containing and nitrogen-containing gases, which can dilute the concentration of combustible gases, while forming a phosphorus-containing char layer on the material surface, which plays a role in blocking heat and oxygen; nitrogen-containing phosphate esters combine the flame retardant properties of nitrogen and phosphorus, and can play a flame retardant role in both the condensed phase and the gas phase, with high flame retardant efficiency.
[0015] In some embodiments, the thickness of the polymer coating layer is 1 nm-5 nm.
[0016] In the technical solution of this application embodiment, when the thickness of the polymer coating layer is between 1nm and 5nm, it can not only play an effective barrier role, but also reduce the impact on ion conduction.
[0017] In some embodiments, the volume average particle size of the positive electrode active material is 5 μm-20 μm.
[0018] In the technical solution of this application embodiment, when the volume average particle size of the positive electrode active material is between 2μm and 20μm, it is beneficial for lithium ion diffusion.
[0019] Secondly, this application provides a method for preparing a secondary battery, comprising: providing a positive electrode sheet, the positive electrode sheet comprising a positive electrode active material, the positive electrode active material comprising a core material and a polymer coating layer covering at least a portion of the surface of the core material, the polymer coating layer containing a benzoxazine ring, the core material comprising one of lithium-containing transition metal oxides; providing a negative electrode sheet, a separator, and an electrolyte; assembling the positive electrode sheet, the separator, and the negative electrode sheet into an electrode assembly; encapsulating the electrode assembly in an outer packaging; and injecting the electrolyte to obtain a secondary battery.
[0020] In some embodiments, the preparation steps of the positive electrode active material include: providing a polymer coating material containing a benzoxazine ring; dissolving the polymer coating material in an organic solvent to prepare a polymer solution; adding the core material to the polymer solution and stirring evenly, ultrasonically dispersing to form a suspension, and then vacuum evaporating to remove the organic solvent, thereby obtaining the positive electrode active material; or, providing a polymer monomer material containing a benzoxazine ring; dissolving the polymer monomer material in an organic solvent to obtain a monomer solution; adding the core material to the monomer solution and stirring evenly, and then heating to 120℃-150℃ for 6h-10h, thereby obtaining the positive electrode active material after the reaction is completed.
[0021] In the technical solution of this application embodiment, the polymer coating layer formed by the vacuum evaporation solvent method is more uniform and dense, which helps to improve the barrier performance of the polymer coating layer, thereby further reducing side reactions caused by contact with the electrolyte. Furthermore, the vacuum evaporation solvent method can produce nanoscale polymer coating layers. The polymer coating layer is formed by depositing it on the surface of the core material through in-situ polymerization, resulting in a polymer coating layer that is not only dense but also has strong adhesion to the core material.
[0022] In some embodiments, the polymer coating material accounts for 1%-10% of the mass of the polymer solution; the polymer coating material includes at least one of benzoxazine oligomers, wherein the degree of polymerization n of the benzoxazine oligomer is 2-15.
[0023] In the technical solution of this application embodiment, when the mass percentage of the polymer coating material in the polymer solution is between 1% and 10%, it is beneficial to achieve uniform coating, thereby improving the barrier performance of the polymer coating. Furthermore, it can reduce the impact on battery kinetic performance. When the degree of polymerization (n) of the benzoxazine oligomer is 2-15, it contains some unpolymerized benzoxazine monomers; therefore, the oligomer is not fully cross-linked and can be further cross-linked and cured when the battery system temperature increases.
[0024] In some embodiments, the temperature of the vacuum evaporation step is 40°C-60°C, and the vacuum degree is -0.08MPa--0.1MPa.
[0025] In the technical solution of this application embodiment, vacuum evaporation between 40℃ and 60℃ can reduce the phase change or lattice oxygen loss of the core material due to high temperature, and the chemical stability of the polymer coating material can be preserved at this temperature. A vacuum of -0.08MPa to -0.1MPa can significantly reduce the boiling point of the solvent, which helps in solvent removal.
[0026] In some embodiments, the stirring speed of the stirring step is 500 rpm-1500 rpm, and the stirring time is 1 h-3 h; and / or, the ultrasonic frequency of the ultrasonic dispersion step is 20 kHz-100 kHz, and the ultrasonic time is 0.5 h-1 h.
[0027] In the technical solution of this application embodiment, when the stirring parameters and ultrasonic dispersion parameters are within the above range, it helps to obtain a uniform solution, thereby helping to uniformly coat the polymer coating material.
[0028] In some embodiments, the step of providing the polymer coating material includes: providing a polymer monomer material and a flame retardant compound; adding the polymer monomer material and the flame retardant compound to a solvent and stirring to dissolve them to obtain a mixture; heating the mixture to 120°C-150°C and reacting for 6-10 hours; and obtaining the polymer coating material after the reaction is completed.
[0029] In the technical solution of this application embodiment, flame-retardant groups can be introduced into the polymer coating material by mixing and reacting polymer monomer materials with flame-retardant compounds, thereby helping to further improve the thermal stability of secondary batteries.
[0030] In some embodiments, the molar ratio of the polymer monomer material to the flame retardant compound is 1:(0.1-0.5); and / or, the polymer monomer material includes at least one of aromatic amine benzoxazine, aliphatic amine benzoxazine, bisphenol A benzoxazine, bisphenol F benzoxazine, halogen-modified benzoxazine, and olefin-modified benzoxazine; and / or, the flame retardant compound includes at least one of melamine, dicyandiamine, guanidine salt, phosphaphenanthrene, phosphazene, and nitrogen-containing phosphate.
[0031] In the technical solution of this application embodiment, when the molar ratio of polymer monomer and flame retardant compound is between 1:(0.1-0.5), a certain amount of flame retardant groups can be introduced to improve the thermal stability of the secondary battery, and the number of benzoxazine rings in the polymer monomer affected by the introduction of flame retardant groups can be reduced, thereby reducing the impact on thermal response crosslinking.
[0032] Thirdly, this application provides an electrical device, including any of the above-mentioned secondary batteries or secondary batteries prepared by any of the above-mentioned methods.
[0033] The above description is only an overview of the technical solution of this application. In order to better understand the technical means of this application and to implement it in accordance with the contents of the specification, and to make the above and other objects, features and advantages of this application more obvious and understandable, the following are specific embodiments of this application. Attached Figure Description
[0034] Figure 1 This is a schematic diagram of the vehicle structure in some embodiments of this application; Figure 2 This is an exploded structural diagram of the secondary battery in some embodiments of this application; Figure 3 This is a schematic diagram showing the exploded structure of a single battery cell in some embodiments of this application; Figure 4 The above are EDS energy dispersive spectra of the positive electrode active materials in some embodiments of this application. Attached image description: 1000 vehicles; Secondary battery 100, controller 200, motor 300; Box 10, Part 11, Part 2 12; Battery cell 20, end cap 21, housing 22, electrode assembly 23. Detailed Implementation
[0036] The following embodiments are only used to illustrate the technical solutions of this application more clearly, and are therefore only examples and should not be used to limit the scope of protection of this application.
[0037] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains; the terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the application; the terms “comprising” and “having”, and any variations thereof, in the specification, claims, and foregoing description of the drawings are intended to cover non-exclusive inclusion.
[0038] In the description of the embodiments of this application, technical terms such as "first" and "second" are used only to distinguish different objects and should not be construed as indicating or implying relative importance or implicitly specifying the number, specific order, or primary and secondary relationship of the indicated technical features. In the description of the embodiments of this application, "multiple" means two or more, unless otherwise explicitly defined.
[0039] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of this application. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments.
[0040] In the description of the embodiments in this application, the term "and / or" is merely a description of the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, and B existing alone. Additionally, the character " / " in this document generally indicates that the preceding and following related objects have an "or" relationship.
[0041] In the description of the embodiments of this application, the term "multiple" refers to two or more (including two), similarly, "multiple sets" refers to two or more (including two sets), and "multiple pieces" refers to two or more (including two pieces). The term "at least one" refers to one or more.
[0042] During secondary battery cycling, Ni in lithium-containing metal oxide cathode active materials4+ The ions will be reduced to Ni 2 + At the same time, in order to maintain charge neutrality O 2- Oxygen escapes from the crystal lattice due to oxidation. With increasing nickel content in lithium-containing metal oxide cathode active materials, the hybridization of Ni3d and O2p orbitals increases, and the covalent nature of the Ni-O bond increases, further promoting oxygen release. The release of a large amount of oxygen generates more oxygen vacancies, thereby lowering the activation barrier for transition metal cation migration and accelerating the phase transition process from a layered structure to a spinel structure and then to a rock salt phase structure. Oxygen release and structural degradation of lithium-containing metal oxide cathode materials create a vicious cycle, affecting the battery's thermal runaway temperature and leading to decreased battery thermal stability.
[0043] Some embodiments describe techniques for forming a coating layer on the surface of lithium metal oxide cathode active materials. Conventional coating layers typically use thermally stable polymer materials or conductive inorganic particles, which serve two purposes: firstly, as a physical barrier to reduce contact with the electrolyte, and secondly, to extend the oxygen migration path. However, these coating materials can only offer limited protection against external thermal shocks and chemical reactions, thus failing to effectively reduce the risk of battery thermal runaway. It is advisable to consider using materials capable of actively responding within the thermal runaway temperature range of lithium metal oxides to achieve active thermal protection.
[0044] Based on the above considerations, this application provides a secondary battery, wherein the positive electrode active material includes a core material and a polymer coating layer covering at least a portion of the surface of the core material, the polymer coating layer containing a benzoxazine ring; the core material includes one of lithium-containing transition metal oxides.
[0045] In such a secondary battery, when the battery system temperature rises to 150℃-200℃, the CO bond in the heterocyclic ring gains sufficient energy to undergo heterolytic cleavage, forming an intramolecular ion pair. This ion pair rapidly attacks the phenoxy group adjacent to the phenoxy group on the oxazine ring. The positive ion in the ion pair combines with the carbon atom adjacent to the phenoxy group, giving the carbon atom a positive charge and initiating a cationic polymerization reaction. On the one hand, the cationic polymerization reaction absorbs a large amount of heat, which helps to lower the system temperature. On the other hand, the cationic polymerization reaction causes the molecular chains to grow and cross-link, gradually building a more stable network structure. This network structure has higher stability and mechanical strength, and can act as a physical barrier, preventing the core material from releasing oxygen free radicals and oxygen at high temperatures due to structural instability, thus preventing crosstalk reactions. This further improves the thermal stability of the positive electrode active material and significantly reduces the risk of thermal runaway.
[0046] The secondary batteries disclosed in this application can be used, but are not limited to, in electrical devices such as vehicles, ships, or aircraft. A power system for such an electrical device can also be composed of the secondary batteries disclosed in this application.
[0047] This application provides an electrical device that uses a secondary battery as a power source. The secondary battery can be, but is not limited to, mobile phones, tablets, laptops, electric toys, power tools, electric vehicles, electric cars, ships, spacecraft, etc. Electric toys can include stationary or mobile electric toys, such as game consoles, electric car toys, electric ship toys, and electric airplane toys, etc. Spacecraft can include airplanes, rockets, space shuttles, and spacecraft, etc.
[0048] For ease of explanation, the following embodiments will be described using a vehicle 1000 as an example of an electrical device according to an embodiment of this application.
[0049] Reference Figure 1 As shown, vehicle 1000 can be a gasoline-powered vehicle, a natural gas-powered vehicle, or a new energy vehicle. New energy vehicles can be pure electric vehicles, hybrid electric vehicles, or range-extended electric vehicles, etc. A secondary battery 100 is installed inside vehicle 1000, which can be located at the bottom, front, or rear of vehicle 1000. The secondary battery 100 can be used to power vehicle 1000; for example, it can serve as the operating power source for vehicle 1000. Vehicle 1000 may also include a controller 200 and a motor 300. The controller 200 controls the secondary battery 100 to supply power to the motor 300, for example, to meet the power needs of vehicle 1000 during starting, navigation, and driving.
[0050] In some embodiments of this application, the secondary battery 100 can not only serve as the operating power source for the vehicle 1000, but also as the driving power source for the vehicle 1000, replacing or partially replacing fuel or natural gas to provide driving power for the vehicle 1000.
[0051] In some embodiments of this application, the secondary battery 100 may be a single battery cell, a group of battery cells, or a battery pack, see reference. Figure 2As shown, taking a secondary battery 100 as an example, the secondary battery 100 may include a housing 10 and individual battery cells 20, with the individual battery cells 20 housed within the housing 10. The housing 10 provides a space for the individual battery cells 20 and can have various structures. In some embodiments, the housing 10 may include a first portion 11 and a second portion 12, which overlap each other, jointly defining a space for accommodating the individual battery cells 20. The second portion 12 may be a hollow structure with one open end, and the first portion 11 may be a plate-like structure, covering the open side of the second portion 12 so that the first portion 11 and the second portion 12 jointly define the space. Alternatively, both the first portion 11 and the second portion 12 may be hollow structures with one open side, with the open side of the first portion 11 covering the open side of the second portion 12. Of course, the housing 10 formed by the first portion 11 and the second portion 12 can have various shapes, such as a cylinder or a cuboid.
[0052] In the secondary battery 100, there can be multiple battery cells 20, which can be connected in series, parallel, or in a mixed manner. A mixed connection means that multiple battery cells 20 are connected in both series and parallel configurations. Multiple battery cells 20 can be directly connected in series, parallel, or in a mixed manner, and then the entire assembly of the multiple battery cells 20 is housed within the casing 10. Alternatively, the secondary battery 100 can also consist of multiple battery cells 20 first connected in series, parallel, or in a mixed manner to form a battery module, and then these battery modules are connected in series, parallel, or in a mixed manner to form a whole, which is also housed within the casing 10. The secondary battery 100 may also include other structures; for example, it may include a busbar component for electrical connection between the multiple battery cells 20.
[0053] Among them, the battery cell 20 can be in the form of a cylinder, a flat shape, a cuboid, or other shapes.
[0054] refer to Figure 3 As shown, the battery cell 20 refers to the smallest unit that makes up the battery. The battery cell 20 includes an end cap 21, a housing 22, an electrode assembly 23, and other functional components.
[0055] End cap 21 refers to a component that covers the opening of housing 22 to isolate the internal environment of battery cell 20 from the external environment. The shape of end cap 21 can be adapted to the shape of housing 22 to fit it. Optionally, end cap 21 can be made of a material with certain hardness and strength (such as aluminum alloy), so that end cap 21 is not easily deformed under pressure or impact, allowing battery cell 20 to have higher structural strength. Functional components such as electrode terminals can be provided on end cap 21. Electrode terminals can be used for electrical connection with electrode assembly 23 for outputting or inputting electrical energy into battery cell 20. In some embodiments, end cap 21 can also be provided with a pressure relief mechanism for releasing internal pressure when the internal pressure or temperature of battery cell 20 reaches a threshold. The material of end cap 21 can also be various, such as copper, iron, aluminum, stainless steel, aluminum alloy, plastic, etc., and this application embodiment does not impose any special limitations on this. In some embodiments, an insulating element may be provided on the inner side of the end cap 21. The insulating element can be used to isolate the electrical connecting pieces inside the housing 22 from the end cap 21 to reduce the risk of short circuit. For example, the insulating element may be made of plastic, rubber, etc.
[0056] The housing 22 is a component used to cooperate with the end cap 21 to form the internal environment of the battery cell 20. This internal environment can accommodate the electrode assembly 23, electrolyte, and other components. The housing 22 and the end cap 21 can be independent components. An opening can be provided on the housing 22, and the end cap 21 can be used to close the opening to form the internal environment of the battery cell 20. Alternatively, the end cap 21 and the housing 22 can be integrated. Specifically, the end cap 21 and the housing 22 can form a common connecting surface before other components are inserted into the housing. When it is necessary to encapsulate the interior of the housing 22, the end cap 21 closes the housing 22. The housing 22 can be of various shapes and sizes, such as cuboid, cylindrical, hexagonal prism, etc. Specifically, the shape of the housing 22 can be determined according to the specific shape and size of the electrode assembly 23. The material of the housing 22 can be various, such as copper, iron, aluminum, stainless steel, aluminum alloy, plastic, etc. This application embodiment does not impose any special limitations on this.
[0057] Electrode assembly 23 is the component in the battery cell 20 where electrochemical reactions occur. The casing 22 may contain one or more electrode assemblies 23. The electrode assembly 23 is mainly formed by winding or stacking positive and negative electrode sheets, and typically a separator is provided between the positive and negative electrode sheets. The portions of the positive and negative electrode sheets containing active material constitute the main body of the electrode assembly, while the portions without active material each constitute a tab. The positive and negative tabs may be located together at one end of the main body or separately at both ends. During the charging and discharging process of the battery, the positive and negative active materials react with the electrolyte, and the tabs connect to the electrode terminals to form a current loop.
[0058] Of course, in some other embodiments, the secondary battery 100 may also be integrated with the chassis / body.
[0059] According to some embodiments of this application, this application provides a secondary battery, including a positive electrode sheet, the positive electrode sheet including a positive electrode active material, the positive electrode active material including a core material and a polymer coating layer covering at least a portion of the surface of the core material, the polymer coating layer containing a benzoxazine ring; the core material including one of lithium transition metal oxides.
[0060] A polymer coating refers to a thin polymer layer covering at least a portion of the surface of a core material. When a polymer coating is applied to the core material surface, the polymer's macromolecular structure allows it to firmly bond with the core material surface through physical entanglement or chemical bonding, forming a stable coating that maintains its integrity over a long period. Furthermore, the polymer coating can isolate the electrolyte from the positive electrode active material. When metal ions dissolve from the interior of the positive electrode active material, they are trapped by the polymer network of the coating, preventing them from freely diffusing into the electrolyte, thus reducing the dissolution of metal ions.
[0061] The benzoxazine ring refers to a heterocycle formed by the fusion of a benzene ring and an oxazine ring. The oxazine ring is a six-membered heterocycle containing one oxygen atom and one nitrogen atom. Based on the positions of the nitrogen and oxygen atoms, the oxazine ring includes the 1,3-oxazine ring shown in formula (IV) and the 1,4-oxazine ring shown in formula (V). Formula (IV), Formula (V).
[0062] In some embodiments, the detection of benzoxazine rings in the polymer coating layer can be performed by the following method: after disassembling the battery, take the positive electrode sheet, and take a film sample, immerse it in dimethyl carbonate (DMC) solution for cleaning, filtration and separation to obtain the positive electrode active material, and perform infrared testing on it, or combine it with elemental analysis to determine the presence of the positive electrode active material.
[0063] Benzooxazine rings undergo cationic polymerization at high temperatures. The specific reaction mechanism is as follows: the CO bond in the heterocycle gains sufficient energy to undergo heterolytic cleavage, forming an intramolecular ion pair. This ion pair rapidly attacks the phenoxy group on the oxazine ring. The positive ion in the ion pair combines with the carbon atom adjacent to the phenoxy group, giving the carbon atom a positive charge, thus initiating the cationic polymerization reaction. When the battery system temperature rises to 150℃-200℃, the polymer coating layer undergoes cationic polymerization. On the one hand, the cationic polymerization process absorbs a large amount of heat, which helps to lower the system temperature. On the other hand, the cationic polymerization reaction causes the molecular chains to grow and cross-link, gradually building a more stable network structure. This network structure has higher stability and mechanical strength, and can act as a physical barrier, preventing the core material from releasing oxygen free radicals and oxygen due to structural instability at high temperatures, thus preventing crosstalk reactions. This further improves the thermal stability of the positive electrode active material and significantly reduces the risk of thermal runaway. Therefore, this application can significantly improve the thermal stability of secondary batteries using lithium-containing transition metal oxides as positive electrode materials.
[0064] Lithium-containing transition metal oxides refer to composite materials composed of hydroxides or oxides of nickel (Ni), cobalt (Co), and manganese (Mn), typically exhibiting a layered crystal structure. In some embodiments, the molecular formula of the lithium-containing transition metal oxide is lithium nickel cobalt manganese oxide (such as LiNi). 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also known as NCM) 333 LiNi 0.5 Co 0.2 Mn 0.3 O2 (also known as NCM) 523 LiNi 0.5 Co 0.25 Mn 0.25 O2 (also known as NCM) 211 LiNi 0.6 Co 0.2 Mn 0.2 O2 (also known as NCM) 622 LiNi 0.8 Co 0.1 Mn 0.1 O2 (also known as NCM) 811 At least one of the following: ) and its modified compounds.
[0065] According to some embodiments of this application, the polymer coating layer includes at least one of the compounds shown in formula (I) and formula (II): Formula (I), Equation (II), Wherein, R1 includes at least one of hydrogen atom, alkyl group, aromatic group, and halogen atom, R2 includes at least one of hydrogen atom, alkyl group, and aromatic group, and R includes one of alkylene groups.
[0066] In some embodiments, the compounds represented by formula (I) include 1,3-benzoxazine, 3-phenyl-3,4-dihydro-2H-1,3-benzoxazine, 3-benzyl-3,4-dihydro-6-methyl-2H-1,3-benzoxazine, and 3-phenyl-6-chloro-3,4-dihydro-2H-1,3-benzoxazine. The compounds represented by formula (II) include bisphenol A type benzoxazine, bisphenol F type benzoxazine, and MDA type benzoxazine.
[0067] The compounds shown in formulas (I) and (II) are both 1,3-benzoxazine, which have higher polymerization activity, can undergo ring-opening polymer reaction under heating conditions, and the resulting polymer coating has high thermal stability.
[0068] According to some embodiments of this application, the polymer coating layer comprises benzoxazine oligomers, wherein the degree of polymerization n of the benzoxazine oligomers is 2-15.
[0069] Benzooxazine oligomers are intermediate products with low molecular weight and incomplete cross-linking formed during the partial polymerization or prepolymerization of benzooxazine monomers. They retain some solubility and processability, and have the potential to be transformed into highly cross-linked polybenzooxazine.
[0070] A degree of polymerization (n) of benzoxazine oligomers of 2-15 means that the oligomers are polymerized from 2-15 benzoxazine units. The molecular chains of benzoxazine oligomers with a degree of polymerization (n) of 2-15 still have active groups (unreacted oxazine rings) at their ends. Thus, when the battery system temperature rises to between 150℃ and 200℃, the polymer coating layer can be further cross-linked and cured, which can not only absorb some heat, but also form a more stable barrier structure.
[0071] According to some embodiments of this application, the polymer coating layer further contains the chain segment shown in formula (III): Formula (III) Wherein, X includes at least one of nitrogen- and / or phosphorus-containing flame-retardant groups.
[0072] Nitrogen and / or phosphorus-containing flame-retardant groups release non-flammable gases or phosphorus free radicals during combustion. The non-flammable gases can dilute the concentration of oxygen and combustible gases in the combustion zone, making it difficult for combustion to continue. The phosphorus free radicals can react with hydrogen free radicals, hydroxyl free radicals, etc., generated during combustion, converting them into more stable products, thereby interrupting the chain reaction of combustion. In addition, nitrogen and / or phosphorus-containing flame-retardant groups can form a char layer during combustion. This char layer has good heat insulation and oxygen barrier properties, thereby inhibiting combustion.
[0073] The segment shown in formula (III) is obtained by reacting a benzoxazine ring-opening reaction with a compound containing X, thereby introducing flame-retardant groups into the polymer coating layer. The introduction of flame-retardant segments into the polymer coating layer allows it to achieve both thermally responsive crosslinking protection and flame-retardant properties, thus further improving the thermal stability of the secondary battery.
[0074] According to some embodiments of this application, X includes at least one of melamine group, dicyandiamine group, guanidine salt group, phosphaphenanthrene group, phosphazene group, and nitrogen-containing phosphate group.
[0075] In some embodiments, the guanidine salt group includes at least one selected from guanidine carbonate group, guanidine phosphate group, guanidine aminosulfonic acid group, and guanidine condensed phosphate group; the phosphenanthrene group includes 9,10-dihydro-9-oxa-10-phosphenanthrene-10-oxide group (DOPO group), 9,10-dihydro-9 At least one of the following: oxa-10-phosphaphenanthrene-10-sulfide group (DOPS group), 10-(2,5-dihydroxyphenyl)-10-hydro-9-oxa-10-phosphaphenanthrene-10-oxide group (DOPO-HQ group), 6H-dibenzo(c,e)(1,2)oxoglycerophosphate-6-oxide group, and 6,6'-(1,2-ethylenediyl)bis-6H-dibenzo[c,e][1,2]oxoglycerophosphate-6,6'-dioxide group (DiDOPO group); phosphazene group including at least one of hexaphenoxycyclotriphosphazene group and polychlorinated phosphazene group; nitrogen-containing phosphate ester group including at least one of amidourea phosphate group, melamine phosphate group, melamine polyphosphate group, and dimethyl N,N'-1,3-phenylenebis(p-methylphosphoamine) group.
[0076] According to some embodiments of this application, the thickness of the polymer coating layer is 1nm-5nm.
[0077] In some embodiments, the thickness of the polymer coating can be measured using a high-resolution transmission electron microscope (TEM). For example, the thickness of the polymer coating can be 1 nm, 2 nm, 3 nm, 4 nm, or 5 nm. When the thickness of the polymer coating is between 1 nm and 5 nm, it can provide effective barrier properties while reducing the impact on ion conduction.
[0078] According to some embodiments of this application, the volume average particle size of the positive electrode active material is 2μm-20μm.
[0079] Volume average particle size is the average particle size calculated with the particle volume as the weight. Its physical meaning is: assuming all particles are spheres of the same size, the diameter of the sphere is the volume average particle size when the total volume of these spheres equals the total volume of the actual particle system. In some embodiments, the volume average particle size of the positive electrode active material can be tested using image analysis: particle images are acquired using a microscope or imaging device, and particle size is measured using image processing software to statistically analyze the volume distribution.
[0080] For example, the volume average particle size of the positive electrode active material can be 2 μm, 4 μm, 6 μm, 8 μm, 10 μm, 12 μm, 14 μm, 16 μm, 18 μm, or 20 μm. A volume average particle size of 2 μm to 20 μm is beneficial for lithium-ion diffusion.
[0081] According to some embodiments of this application, this application provides a method for preparing a secondary battery, comprising: providing a positive electrode sheet, the positive electrode sheet comprising a positive electrode active material, the positive electrode active material comprising a core material and a polymer coating layer covering at least a portion of the surface of the core material, the polymer coating layer containing a benzoxazine ring, and the core material comprising one of lithium-containing transition metal oxides; providing a negative electrode sheet, a separator, and an electrolyte; assembling the positive electrode sheet, the separator, and the negative electrode sheet into an electrode assembly; encapsulating the electrode assembly in an outer packaging; and injecting an electrolyte to obtain a secondary battery.
[0082] The negative electrode sheet includes a negative electrode active material. When the secondary battery is a lithium-ion battery, the negative electrode active material can be a negative electrode active material known in the art for use in batteries. In some embodiments, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, and lithium titanate, etc. Silicon-based materials may be selected from at least one of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. Tin-based materials may be selected from at least one of elemental tin, tin oxide compounds, and tin alloys. In some embodiments, the negative electrode film layer may also optionally include a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS). In some embodiments, the negative electrode film layer may also optionally include a conductive agent. The conductive agent may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. In some embodiments, the negative electrode film may also optionally include other additives, such as thickeners (e.g., sodium carboxymethyl cellulose (CMC-Na)).
[0083] The separator can be any known porous structure separator with good chemical and mechanical stability. In some embodiments, the separator material can be selected from at least one of glass fiber, nonwoven fabric, polyethylene, polypropylene, and polyvinylidene fluoride.
[0084] The electrolyte comprises an electrolyte and a solvent. When the secondary battery is a lithium-ion battery, the electrolyte salt may be selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalate borate, lithium dioxalate borate, lithium difluorodioxalate phosphate, and lithium tetrafluorooxalate phosphate. The solvent may be selected from at least one of ethylene carbonate, propylene carbonate, methyl ethyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, butyl carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, sulfolane, dimethyl sulfone, methyl ethyl sulfone, and diethyl sulfone.
[0085] The electrode assembly can be a stacked electrode assembly or a wound electrode assembly. The outer packaging can be a rigid shell, such as a hard plastic shell, aluminum shell, or steel shell. The outer packaging can also be a flexible package, such as a pouch. The material of the flexible package can be plastic, and examples of plastics include polypropylene, polybutylene terephthalate, and polybutylene succinate.
[0086] According to some embodiments of this application, the preparation steps of the positive electrode active material include: providing a polymer coating material containing a benzoxazine ring; dissolving the polymer coating material in an organic solvent to prepare a polymer solution; adding a core material to the polymer solution and stirring evenly, ultrasonically dispersing to form a suspension, and then vacuum evaporating to remove the organic solvent, thereby obtaining the positive electrode active material; or, providing a polymer monomer material containing a benzoxazine ring; dissolving the polymer monomer material in an organic solvent to obtain a monomer solution; adding the core material to the monomer solution and stirring evenly, and then heating to 120℃-150℃ for 6h-10h, thereby obtaining the positive electrode active material after the reaction is completed.
[0087] Polymer coating materials refer to polymers containing benzoxazine rings, generally benzoxazine oligomers. Benzoxazine oligomers retain some solubility, which facilitates impregnation of the core material.
[0088] The organic solvent is selected from those capable of dissolving benzoxazine oligomers. In some embodiments, the organic solvent may be at least one of acetone, tetrahydrofuran, N,N-dimethylformamide, dimethyl sulfoxide, toluene, chloroform, and dichloromethane.
[0089] Adding the core material to the polymer solution and stirring and sonicating it are to ensure that the core material is evenly dispersed in the solution, which helps to form a uniform polymer coating layer on the surface of the core material.
[0090] The removal of organic solvents via vacuum evaporation can be performed using a rotary evaporator, a vacuum drying oven, or a spray dryer. A rotary evaporator allows for precise control of temperature and rotation speed, effectively reducing the impact of localized overheating on the core material and polymer coating. A vacuum drying oven can process multiple samples simultaneously and is suitable for materials of different shapes and sizes. A spray dryer offers rapid drying, achieving organic solvent evaporation in a short time.
[0091] The polymer coating layer formed by the vacuum evaporation solvent method is more uniform and dense, which helps to improve the barrier properties of the polymer coating layer, thereby further reducing side reactions caused by contact with the electrolyte. In addition, the vacuum evaporation solvent method can produce nanoscale polymer coating layers.
[0092] The polymer monomer material refers to benzoxazine monomer, and its dissolving solvent may include at least one of acetone, tetrahydrofuran, N,N,dimethylformamide, dimethyl sulfoxide, toluene, chloroform, and dichloromethane.
[0093] For example, the polymerization temperature of the monomer solution can be 120°C, 125°C, 130°C, 135°C, 140°C, 145°C, or 150°C, and the polymerization time can be 6h, 6.5h, 7h, 7.5h, 8h, 8.5h, 9h, 9.5h, or 10h. Reacting the monomer solution under these conditions allows for the deposition of a polymer coating layer on the core material surface via in-situ polymerization. The resulting polymer coating layer is not only dense but also exhibits strong adhesion to the core material.
[0094] According to some embodiments of this application, the polymer coating material accounts for 1%-10% of the mass of the polymer solution.
[0095] For example, the mass percentage of the polymer coating material in the polymer solution can be 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, or 10%. A mass percentage of 1%-10% in the polymer solution is beneficial for achieving uniform coating, thereby improving the barrier properties of the polymer coating. Furthermore, it can reduce the impact on battery kinetic performance.
[0096] According to some embodiments of this application, the temperature of the vacuum evaporation step is 40°C-60°C, and the vacuum degree is -0.08MPa--0.1MPa.
[0097] For example, the temperature of the vacuum evaporation step can be 40°C, 45°C, 50°C, 55°C, or 60°C, and the vacuum level can be -0.08MPa, -0.085MPa, -0.09MPa, -0.095MPa, or -0.1MPa. Vacuum evaporation between 40°C and 60°C can reduce phase transitions or lattice oxygen loss in the core material due to high temperatures, and the chemical stability of the polymer coating material can be preserved at this temperature. A vacuum level of -0.08MPa to -0.1MPa can significantly lower the boiling point of the solvent, facilitating solvent removal.
[0098] According to some embodiments of this application, the stirring speed of the stirring step is 500 rpm-1500 rpm, and the stirring time is 1 h-3 h; and / or, the ultrasonic frequency of the ultrasonic dispersion step is 20 kHz-100 kHz, and the ultrasonic time is 0.5 h-1 h.
[0099] For example, the stirring speed can be 500 rpm, 600 rpm, 700 rpm, 800 rpm, 900 rpm, 1000 rpm, 1100 rpm, 1200 rpm, 1300 rpm, 1400 rpm, or 1500 rpm, and the stirring time can be 1 h, 1.5 h, 2 h, 2.5 h, or 3 h; the ultrasonic frequency can be 20 kHz, 30 kHz, 40 kHz, 50 kHz, 60 kHz, 70 kHz, 80 kHz, 90 kHz, or 100 kHz, and the ultrasonic time can be 0.5 h, 0.6 h, 0.7 h, 0.8 h, 0.9 h, or 1 h. When the stirring parameters and ultrasonic dispersion parameters are within the above ranges, it helps to obtain a homogeneous solution, thereby contributing to the uniform coating of the polymer coating material.
[0100] According to some embodiments of this application, the step of providing a polymer coating material includes: providing a polymer monomer material and a flame retardant compound; adding the polymer monomer material and the flame retardant compound to a solvent and stirring to dissolve them to obtain a mixture; heating the mixture to 120°C-150°C and reacting for 6-10 hours; and obtaining the polymer coating material after the reaction is completed.
[0101] The solvent of the mixture should be capable of dissolving the polymer monomers and flame retardant compounds. In some embodiments, the solvent may be at least one of dioxane, acetone, tetrahydrofuran, N,N-dimethylformamide, dimethyl sulfoxide, toluene, chloroform, and dichloromethane.
[0102] Heating the mixture to 120°C-150°C for 6-10 hours is to open the oxazine ring of the polymer monomer and graft flame-retardant compounds onto it. Exemplarily, the reaction temperature can be 120°C, 125°C, 130°C, 135°C, 140°C, 145°C, or 150°C, and the polymerization time can be 6 hours, 6.5 hours, 7 hours, 7.5 hours, 8 hours, 8.5 hours, 9 hours, 9.5 hours, or 10 hours. By mixing and reacting the polymer monomer with the flame-retardant compound, flame-retardant groups can be introduced into the polymer coating material, thereby contributing to further improvement in the thermal stability of the secondary battery.
[0103] According to some embodiments of this application, the molar ratio of polymer monomer material to flame retardant compound is 1:(0.1-0.5); and / or, the polymer monomer material includes at least one of aromatic amine type benzoxazine, aliphatic amine type benzoxazine, bisphenol A type benzoxazine, bisphenol F type benzoxazine, halogen-modified benzoxazine, and olefin-modified benzoxazine; and / or, the flame retardant compound includes at least one of melamine, dicyandiamine, guanidine salt, phosphonophenanthrene, phosphazene, and nitrogen-containing phosphate ester.
[0104] The polymer monomer refers to a benzoxazine monomer. In some embodiments, the benzoxazine monomer may be at least one of aromatic amine benzoxazine, aliphatic amine benzoxazine, bisphenol A benzoxazine, bisphenol F benzoxazine, halogen-modified benzoxazine, and olefin-modified benzoxazine. Aromatic amine benzoxazine includes at least one of aniline benzoxazine and toluidine benzoxazine. Aliphatic amine benzoxazine includes at least one of cyclohexylaminobenzoxazine and ethylenediamine benzoxazine.
[0105] Flame retardant compounds refer to a class of chemical substances that can prevent or inhibit the combustion of materials. In some embodiments, flame retardant compounds include at least one of melamine, dicyandiamine, guanidine salts, phosphaphenanthrene, phosphazenes, and nitrogen-containing phosphates. Guanidine salt groups include guanidine carbonate, guanidine phosphate, guanidine aminosulfonate, and condensed guanidine phosphate. Phosphaphenanthrene groups include 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, etc. -Oxa-10-phosphaphenanthrene-10-sulfide, 10-(2,5-dihydroxyphenyl)-10-hydro-9-oxa-10-phosphaphenanthrene-10-oxide, 6H-dibenzo(c,e)(1,2)oxoglyceric acid ester-6-oxide and 6,6'-(1,2-ethylenediyl)bis-6H-dibenzo[c,e][1,2]oxoglyceric acid ester-6,6'-dioxide; phosphazenes include hexaphenoxycyclotriphosphazene and polychlorophosphazene; nitrogen-containing phosphates include amidourea phosphate, melamine phosphate, melamine polyphosphate and dimethyl N,N'-1,3-phenylenebis(p-methylphosphoamine).
[0106] For example, the molar ratio of polymer monomer to flame retardant compound can be 1:0.1, 1:0.2, 1:0.3, 1:0.4 or 1:0.5. When the molar ratio of polymer monomer to flame retardant compound is between 1:(0.1-0.5), a certain amount of flame retardant groups can be introduced to improve the thermal stability of the secondary battery, while the number of benzoxazine rings in the polymer monomer affected by the introduction of flame retardant groups can be reduced, thereby reducing the impact on thermal response crosslinking.
[0107] According to some embodiments of this application, this application provides an electrical device including any of the aforementioned secondary batteries.
[0108] Example The following describes embodiments of this application. The embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in this field or according to the product instructions. Reagents or instruments used, unless otherwise specified, are all conventional products that can be obtained commercially.
[0109] Example 1 [Positive electrode active material] Bisphenol A benzoxazine oligomers (n=12, weight-average molecular weight 2800 g / mol) were dissolved in tetrahydrofuran (THF) to prepare a 5% (w / w) polymer solution, wherein the bisphenol A benzoxazine oligomers contained the monomer shown in formula (VI): Formula (VI).
[0110] core material LiNi 0.9 Co 0.05 Mn 0.05 O2 was added to the polymer solution, and the mixture was mechanically stirred at 1000 rpm for 2 hours to ensure uniform mixing. The solution was then sonicated at 50 kHz for 0.5 hours to obtain a homogeneous suspension. The organic solvent was slowly evaporated using a rotary evaporator at 50°C and a vacuum of -0.08 MPa. As the solvent evaporated, bisphenol A benzoxazine oligomers gradually deposited on the surface of the core particles, achieving uniform coating. Finally, the material was dispersed using a vibrating screen, and particles with a diameter (Dv50) of 10 μm were collected and used as the positive electrode active material.
[0111] The prepared positive electrode active material was subjected to energy dispersive spectroscopy (EDS) analysis using a ULTIM MAX65 spectrometer. The EDS plot is shown below. Figure 4 As shown, the core material surface has a 2nm coating layer, and the coating layer is uniform and dense. The coating layer contains nitrogen, indicating that it is coated with bisphenol A benzoxazine oligomer.
[0112] [Positive electrode plate] The positive electrode active material prepared above was mixed with conductive carbon black (Super P) and binder polyvinylidene fluoride (PVDF) in an N-methylpyrrolidone (NMP) solvent at a mass ratio of 96:2.2:1.8 to form a positive electrode slurry. The positive electrode slurry was uniformly coated on both sides of an aluminum foil, and then dried, cold-pressed, and slit to obtain the positive electrode sheet.
[0113] [Negative electrode plate] Artificial graphite (anode active material), styrene-butadiene rubber (SBR) (binder), carbon black (Super P) (conductive agent), and sodium carboxymethyl cellulose (CMC-Na) (plasticizer) are dispersed in deionized water at a mass ratio of 95:3:1:1 and thoroughly stirred to obtain a cathode slurry. The slurry is then uniformly coated on both sides of a copper foil, and subsequently dried, cold-pressed, trimmed, cut, and slit to form a cathode sheet.
[0114] [Isolation membrane] Polypropylene film is used as the separating membrane.
[0115] Electrolyte In an argon-atmospheric glove box (H2O < 0.1 ppm, O2 < 0.1 ppm), ethylene carbonate (EC), diethyl carbonate (DEC), and dimethyl carbonate (DMC) were mixed in a volume ratio of 1:1:1. LiPF6 was then uniformly dissolved in the mixture to obtain the electrolyte. The concentration of LiPF6 in this electrolyte was 1 mol / L.
[0116] [Assembly] A positive electrode, a separator, and a negative electrode are stacked sequentially to form an electrode assembly. The electrode assembly is then placed in a housing, and the secondary battery is produced by top-side sealing, high-temperature baking, liquid injection, and formation.
[0117] Example 2 Unlike Example 1, the polymer solution in this example has a mass fraction of 10%, and the thickness of the polymer coating layer is 5 nm.
[0118] Example 3 Unlike Example 1, the polymer solution in this example has a mass fraction of 1%, and the thickness of the polymer coating layer is 1 nm.
[0119] Example 4 Unlike Example 1, the bisphenol A benzoxazine oligomer of this example contains the monomer shown in formula (VII): Equation (VII).
[0120] In this embodiment, the degree of polymerization of the bisphenol A benzoxazine oligomer is n=11, and the molecular weight is 3300 g / mol with a weight average molecular weight.
[0121] Example 5 Unlike Example 1, the bisphenol A benzoxazine oligomer of this example contains the monomer shown in formula (VIII): Formula (VIII).
[0122] In this embodiment, the degree of polymerization of the bisphenol A benzoxazine oligomer is n=13, and the molecular weight is 2400 g / mol with a weight average molecular weight.
[0123] Example 6 Unlike Example 1, the bisphenol A benzoxazine oligomer of this example contains a monomer represented by formula (VIII): Formula (IX).
[0124] In this embodiment, the degree of polymerization of the bisphenol A benzoxazine oligomer is n=12, and the molecular weight is 2300 g / mol (weight average).
[0125] Example 7 Unlike Example 1, the polymer coating material in this example is a bisphenol A benzoxazine oligomer grafted with melamine groups. The preparation method includes: adding bisphenol A benzoxazine monomer (the monomer shown in Formula VI) and melamine to a reaction vessel at a molar ratio of 1:0.3, adding an appropriate amount of dioxane solvent, and stirring to ensure complete dissolution; then heating the reaction system to 130°C and reacting for 8 hours, allowing the amino group of melamine to attack the more reactive methylene group linked to the benzene ring after ring opening. After the reaction, the polymer coating material is obtained. The polymer density of the prepared polymer coating material is 12, and the weight-average molecular weight is 4300 g / mol.
[0126] Comparative Example 1 Unlike Example 1, the lithium-containing transition metal oxide in this comparative example is not coated.
[0127] Comparative Example 2 Unlike Example 1, the preparation method of the positive electrode active material in this comparative example is as follows: core material LiNi 0.9 Co 0.05 Mn 0.05 O2 was dispersed in a round-bottom flask containing an equal mass of toluene and ultrasonically dispersed for 10 min to ensure uniform dispersion of the core material. Ethylene was added and stirred to dissolve, with a core material to ethylene mass ratio of 95:5. Nitrogen gas was purged for 15 min to remove oxygen from the system, and the temperature was raised to 60°C. After the system temperature stabilized, an initiator at a content of 0.2 wt% of the ethylene mass was slowly added, and the reaction was continued with stirring for 6 h. After the reaction was completed, the product was filtered, washed, and dried to obtain the coated lithium-containing transition metal oxide. The coating thickness was 2 nm.
[0128] Performance testing Testing of the heat generation and thermal runaway initiation temperature of the positive electrode: At room temperature (25°C), the battery was charged to 4.25V at a rate of 0.33C. Then, in an inert glove box, the fully charged battery was disassembled, and the fully charged positive electrode was immersed in dimethyl carbonate solution for 2 hours. After drying, a 5mm diameter electrode sheet was cut using a specific punching tool. The electrode sheet was placed in a crucible specifically designed for differential scanning calorimetry (DSC), and 1.5μL of electrolyte (the electrolyte from Example 1) was added. The crucible was then sealed using a sealing tool and placed in the sample cell of the DSC instrument, ensuring accurate placement and good contact with the instrument's heat transfer components. The sample cell door was then closed. The heating rate was set to 10°C / min, and the temperature range was set from room temperature to 490°C. A nitrogen atmosphere was selected. After ensuring accurate instrument parameter settings, the test program was started, and the peak position, area, and intensity were observed. The area under the curve is integrated using the software built into the differential scanning calorimeter (DSC) to obtain the heat change value of the sample within the range of 25℃-490℃. The heat generation of the electrode is calculated according to the following formula: Heat generation = Heat change value within the temperature range / Electrode mass, in J / ΔT (℃). The thermal runaway temperature refers to the temperature corresponding to the peak in the DSC curve.
[0129] Electrolyte resistance of polymer coating material: Weigh approximately 1g of polymer coating material (A) and place it in a semi-permeable membrane (electrolyte permeable, sample powder impermeable) sample bag. Seal the bag and record the total weight B1. Then, immerse the sample bag in 10g of electrolyte (volume ratio EC:EMC=3:7) at 60℃ for 7 days. After immersion, remove the sample bag, drain, and dry at 120℃ for 12 hours. Weigh the sample bag again, B2. The formula for calculating the sample dissolution rate R is as follows: R=(B1-B2) / A×100%.
[0130] Test Results The test results of Examples 1-7 and Comparative Examples 1-2 are shown in Table 1.
[0131] Table 1 shows the test results of Examples 1-7 and Comparative Examples 1-2.
[0132] As can be seen from Table 1, the heat generated by the positive electrode in the embodiments of this application during the process of increasing from room temperature to 490°C is lower than that of the positive electrode in Comparative Example 1, and the thermal runaway initiation temperature is higher than that of Comparative Example 1. This indicates that the polybenzoxazine coated in this application can absorb some heat through further cross-linking and curing when the system temperature rises, thereby helping to increase the thermal runaway initiation temperature of the battery system.
[0133] Comparing Example 1 and Comparative Example 2, it can be seen that when the polymer coating is polyethylene, the heat generation is 5256 J / Ah and the thermal runaway initiation temperature is 207°C. This indicates that compared with the polyethylene coating, the polybenzoxazine coating of this application can significantly reduce the heat generation and increase the thermal runaway initiation temperature of the battery.
[0134] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of this application, and not to limit them. Although this application has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features therein. These modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of this application, and they should all be covered within the scope of the claims and specification of this application. In particular, as long as there is no structural conflict, the various technical features mentioned in the embodiments can be combined in any way. This application is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.
Claims
1. A secondary battery, comprising a positive electrode sheet, said positive electrode sheet comprising a positive electrode active material, characterized in that, The positive electrode active material includes a core material and a polymer coating layer covering at least a portion of the surface of the core material, wherein the polymer coating layer contains a benzoxazine ring; The core material includes one of lithium-containing transition metal oxides.
2. The secondary battery as described in claim 1, characterized in that, The polymer coating layer comprises at least one of the compounds shown in formula (I) and formula (II): Equation (I), Equation (II), Wherein, R1 includes at least one of hydrogen atom, alkyl, aromatic group, and halogen atom, R2 includes at least one of hydrogen atom, alkyl, olefinic group, aromatic group, siloxane group, and phosphate group, and R includes one of alkylene groups.
3. The secondary battery as described in claim 1 or 2, characterized in that, The polymer coating layer comprises benzoxazine oligomers, wherein the degree of polymerization n of the benzoxazine oligomers is 2-15.
4. The secondary battery according to any one of claims 1 to 3, characterized in that, The polymer coating layer also contains the chain segment shown in formula (III): Formula (III) Wherein, X includes at least one of nitrogen- and / or phosphorus-containing flame-retardant groups.
5. The secondary battery as described in claim 4, characterized in that, The X includes at least one of the following: melamine group, dicyandiamine group, guanidine salt group, phosphaphenanthrene group, phosphazene group, and nitrogen-containing phosphate group.
6. The secondary battery according to any one of claims 1 to 5, characterized in that, The thickness of the polymer coating layer is 1nm-5nm.
7. The secondary battery according to any one of claims 1 to 5, characterized in that, The volume average particle size of the positive electrode active material is 5μm-20μm.
8. A method for preparing a secondary battery, characterized in that, include: A positive electrode is provided, the positive electrode comprising a positive active material, the positive active material comprising a core material and a polymer coating layer covering at least a portion of the surface of the core material, the polymer coating layer containing a benzoxazine ring, the core material comprising one of lithium-containing transition metal oxides; We provide negative electrode plates, separators, and electrolytes; The positive electrode, separator, and negative electrode are assembled into an electrode assembly, which is then placed in an outer packaging for sealing. After injecting the electrolyte, a secondary battery is obtained.
9. The method for preparing a secondary battery as described in claim 8, characterized in that, The preparation steps of the positive electrode active material include: A polymer coating material is provided, the polymer coating material containing a benzoxazine ring; The polymer coating material is dissolved in an organic solvent to prepare a polymer solution; The core material is added to the polymer solution and stirred until homogeneous. It is then ultrasonically dispersed to form a suspension. The organic solvent is then removed by vacuum evaporation. After the organic solvent is removed, the positive electrode active material is obtained; or... A polymer monomer material is provided, the polymer monomer material containing a benzoxazine ring; The polymer monomer material is dissolved in an organic solvent to obtain a monomer solution; The core material is added to the monomer solution and stirred until homogeneous. Then, the mixture is heated to 120℃-150℃ and reacted for 6-10 hours. After the reaction is completed, the positive electrode active material is obtained.
10. The method for preparing a secondary battery as described in claim 9, characterized in that, The polymer coating material comprises 1%-10% by mass in the polymer solution; and / or, The polymer coating material includes at least one of benzoxazine oligomers, wherein the degree of polymerization n of the benzoxazine oligomer is 2-15.
11. The method for preparing a secondary battery as described in claim 9 or 10, characterized in that, The temperature of the vacuum evaporation step is 40℃-60℃, and the vacuum degree is -0.08MPa--0.1MPa.
12. The method for preparing a secondary battery as described in claim 9 or 10, characterized in that, The stirring speed in the stirring step is 500 rpm-1500 rpm, and the stirring time is 1 h-3 h; and / or, The ultrasonic dispersion step uses an ultrasonic frequency of 20kHz-100kHz and an ultrasonic duration of 0.5h-1h.
13. The method for preparing a secondary battery according to any one of claims 9 to 12, characterized in that, The step of providing the polymer coating material includes: Provides polymer monomer materials and flame retardant compounds; The polymer monomer material and the flame retardant compound are added to a solvent and stirred to dissolve, thereby obtaining a mixture. The mixture is heated to 120℃-150℃ and reacted for 6h-10h. After the reaction is completed, a polymer coating material is obtained.
14. The method for preparing a secondary battery as described in claim 13, characterized in that, The molar ratio of the polymer monomer material to the flame retardant compound is 1:(0.1-0.5); and / or, The polymer monomer material includes at least one of the following: aromatic amine-type benzoxazine, aliphatic amine-type benzoxazine, bisphenol A-type benzoxazine, bisphenol F-type benzoxazine, halogen-modified benzoxazine, and olefin-modified benzoxazine: and / or, The flame retardant compound includes at least one of melamine, dicyandiamine, guanidine salt, phosphaphenanthrene, phosphazene, and nitrogen-containing phosphate.
15. An electrical appliance, characterized in that, This includes the secondary battery as described in any one of claims 1 to 7 or the secondary battery prepared by any one of claims 8 to 14.