Positive electrode active material, method of preparing positive electrode active material, and rechargeable lithium battery

By coating the surface of lithium-nickel composite oxide core particles with cobalt and phosphorus, and synthesizing single-particle positive electrode active materials by pre-doping zirconium raw materials at low temperature, the problems of agglomeration and cycle life degradation of high-nickel positive electrode active materials are solved, and the battery performance and stability are improved.

CN123162154APending Publication Date: 2026-11-24SAMSUNG SDI CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610680304.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2025-05-23
Filing Date
2026-05-18
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing high-nickel positive electrode active materials suffer from problems such as increased particle agglomeration and reduced productivity during preparation. Furthermore, the use of alkaline grain growth promoters leads to a decline in cycle life, and the cleaning process increases manufacturing costs and complexity. The problem of uneven element doping is also difficult to solve.

Method used

Cobalt and phosphorus are uniformly coated on the surface of lithium-nickel composite oxide core particles using coating technology. Single-particle positive electrode active material is synthesized at low temperature by pre-doping zirconium raw materials to avoid the residue of alkaline grain growth promoters. Oxide precursors are mixed with lithium raw materials to improve particle uniformity.

Benefits of technology

It achieves improved performance at high temperatures and high voltages, enhances capacity characteristics, initial charge/discharge efficiency and high-temperature cycle life characteristics, reduces gas generation, and improves productivity and battery stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123162154A_ABST
    Figure CN123162154A_ABST
Patent Text Reader

Abstract

A positive electrode active material, a method for preparing the positive electrode active material, and a rechargeable lithium battery are disclosed. The positive electrode active material comprises: core particles, each comprising a zirconium-containing lithium-nickel composite oxide, and each core particle having a nickel content greater than or equal to about 60 mol% based on 100 mol% of the total metals other than lithium in the zirconium-containing lithium-nickel composite oxide; and a coating disposed on the surface of each of the core particles and comprising cobalt and phosphorus. The positive electrode active material has a thickness of approximately 0.7 μm. 2 / g to approximately 0.9m 2 The BET specific surface area is / g, and it exists in single-particle form.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The positive electrode active material, the preparation method of the positive electrode active material, and the rechargeable lithium battery are disclosed. Background Technology

[0002] With the rapid proliferation of battery-powered electronic devices such as mobile phones, laptops, and electric vehicles, the demand for rechargeable batteries with high energy density and high capacity is increasing rapidly. Therefore, research and development efforts have been undertaken to improve the performance of rechargeable lithium-ion batteries.

[0003] A rechargeable lithium battery includes a positive electrode and a negative electrode, each containing active materials capable of inserting and deintercalating lithium ions, and an electrolyte solution. Electrical energy is generated through oxidation and reduction reactions as lithium ions are inserted / deintercalated at the positive and negative electrodes.

[0004] Various positive electrode active materials have been studied to provide rechargeable lithium-ion batteries for a variety of applications. Among these materials, lithium nickel oxides, lithium nickel manganese cobalt composite oxides, lithium nickel cobalt aluminum composite oxides, and lithium cobalt oxides are mainly used as positive electrode active materials. In recent years, high-nickel positive electrode active materials with a nickel content of about 80 mol% or more have been developed due to their ability to provide high energy density. However, such materials have various problems such as structural degradation with charge and discharge, surface side reactions with the electrolyte, and degradation due to particle breakage. Therefore, there is a need to develop positive electrode active materials that can achieve high energy density and long cycle life characteristics.

[0005] High-capacity nickel-based positive electrode active materials are primarily produced in the form of secondary particles, formed by agglomerating multiple primary particles. However, recently, single-particle materials have been considered to provide long cycle life while reducing gas generation. However, since single particles are prepared at elevated firing temperatures, there are problems with increased particle agglomeration and reduced productivity. To prevent particle agglomeration and lower firing temperatures, studies have been proposed on adding alkaline grain growth promoters during single-particle synthesis. However, this has the problem that the grain growth promoter may remain after firing and act as a resistor in the positive electrode, leading to reduced cycle life. Therefore, cleaning processes can be introduced to remove residual grain growth promoters or residual salts; however, these cleaning processes increase manufacturing costs and / or complicate the manufacturing process.

[0006] In other cases, methods have been used to dope the positive electrode active material precursor with an element that can replace the basic grain growth promoter (e.g., aluminum) when mixing the positive electrode active material precursor with the lithium feedstock. However, in such methods, it is difficult to uniformly dope the element into the positive electrode active material. Summary of the Invention

[0007] A positive electrode active material capable of uniform particle growth during the fabrication process and a method for preparing the positive electrode active material are disclosed. By introducing a coating, the performance of rechargeable lithium batteries at high temperatures and high voltages is improved, and capacity characteristics, initial charge / discharge efficiency, and high-temperature cycle life characteristics are enhanced.

[0008] In some example embodiments, the positive electrode active material includes: core particles, each comprising a zirconium-containing lithium-nickel composite oxide, and having a nickel content greater than or equal to about 60 mol% based on 100 mol% of the total metals other than lithium in the zirconium-containing lithium-nickel composite oxide; and a coating disposed on the surface of each core particle and comprising cobalt and phosphorus; wherein the positive electrode active material has a thickness of about 0.7 μm. 2 / g to approximately 0.9m 2 The BET specific surface area is / g, and the positive electrode active material is in the form of single particles.

[0009] In some example embodiments, the method for preparing the positive electrode active material includes the following steps: (i) mixing zirconium raw material and nickel raw material and performing a co-precipitation reaction to prepare a zirconium-containing nickel composite hydroxide; (ii) subjecting the zirconium-containing nickel composite hydroxide to a first heat treatment to prepare a zirconium-containing nickel composite oxide; (iii) mixing the zirconium-containing nickel composite oxide and lithium raw material and performing a second heat treatment to prepare a zirconium-containing lithium nickel composite oxide in the form of secondary particles as aggregates of primary particles; (iv) pulverizing the zirconium-containing lithium nickel composite oxide to obtain an initial positive electrode active material in the form of single particles; and (v) mixing the initial positive electrode active material, cobalt raw material and phosphorus raw material, performing a third heat treatment, and disintegrating the mixture after the heat treatment.

[0010] In some example embodiments, a rechargeable lithium battery includes: a current collector; a positive electrode disposed on the current collector and including a positive electrode active material layer comprising the positive electrode active material; a negative electrode; and an electrolyte.

[0011] According to the method for preparing the positive electrode active material according to the embodiments, uniform particle growth is possible, and a coating can be effectively introduced onto the surface of the positive electrode active material. The positive electrode active material and the rechargeable lithium battery including the positive electrode active material can exhibit high initial charge / discharge capacity and efficiency, and can have long cycle life characteristics. Attached Figure Description

[0012] Figure 1 This is a schematic perspective view of a cylindrical rechargeable lithium battery.

[0013] Figure 2 It is a cross-sectional view of a prismatic rechargeable lithium battery.

[0014] Figure 3 and Figure 4 This is a schematic exploded perspective view of a pouch-type rechargeable lithium battery. Detailed Implementation

[0015] Specific embodiments will be described in detail below, enabling those skilled in the art to implement them. However, this disclosure may be implemented in many different forms and is not to be construed as limited to the exemplary embodiments set forth herein.

[0016] The terminology used herein is for describing embodiments only and is not intended to limit this disclosure. Unless the context clearly indicates otherwise, singular expressions include plural expressions.

[0017] As used herein, “combination of them” means mixtures, laminates, complexes, copolymers, alloys, blends, reaction products, etc. of the components.

[0018] It should be understood that terms such as “comprising,” “including,” or “having” are intended to indicate the presence of the features, quantities, steps, elements, or combinations thereof embodied, but do not preclude the possibility of the presence or addition of one or more other features, quantities, steps, elements, or combinations thereof.

[0019] In the accompanying drawings, for clarity, the thickness of layers, films, panels, regions, etc., may be exaggerated, and the same reference numerals denote the same elements throughout the specification. It will be understood that when an element such as a layer, film, region, or substrate is referred to as being "on" another element, it may be directly on said other element, or an intervening element may be present. Conversely, when an element is referred to as being "directly on" another element, no intervening element is present.

[0020] Furthermore, the term "layer" here includes not only shapes that form across the entire surface when viewed from a plan view, but also shapes that form on a portion of the surface.

[0021] The average particle size can be measured using methods known to those skilled in the art, for example, by a particle size analyzer, or by transmission electron microscopy or scanning electron microscopy images. Alternatively, the average particle size value can be obtained by measuring using dynamic light scattering, performing data analysis, counting the number of particles for each particle size range, and calculating from there. Unless otherwise defined, the average particle size can be represented as the diameter (D) of particles having a cumulative volume of 50% of the particle size distribution. 50As used herein, unless otherwise defined, the average particle size represents the diameter (Di) of particles that constitute 50% of the total volume in a particle size distribution obtained by randomly measuring the size (diameter or major axis length) of approximately 20 particles in a scanning electron microscope image and calculating the volume of each particle using those measurements, assuming the particles are spherical. 50 ).

[0022] Here, "or" will not be interpreted as having an exclusive meaning; for example, "A or B" is interpreted as including A, B, A+B, etc.

[0023] "Metals" include common metals, transition metals, and metalloids (semi-metals).

[0024] Positive electrode active material nuclear particles Some example embodiments provide a positive electrode active material comprising core particles and a coating. The core particles comprise a zirconium-containing lithium-nickel composite oxide and have a nickel content greater than or equal to about 60 mol% based on 100 mol% of the total metals other than lithium in the positive electrode active layer. The coating is disposed on the surface of each core particle and comprises cobalt and phosphorus. The positive electrode active material may have a surface area of ​​about 0.7 μm. 2 / g to approximately 0.9m 2 / g BET (Brunauer, Emmett and Teller) specific surface area and in single particle form.

[0025] Zirconium can act as a grain growth promoter during the synthesis process. Therefore, by uniformly distributing zirconium within the precursor of the positive electrode active material, it is possible to prepare a single-particle form of the positive electrode active material with uniform grain growth. Thus, rechargeable lithium batteries incorporating the positive electrode active material can exhibit excellent charge / discharge efficiency and lifespan characteristics.

[0026] A single particle can exist independently without grain boundaries. Each single particle is composed of a single particle and can be a single particle, a monolithic structure, an integral structure, or a non-agglomerated particle that exists morphologically as an independent phase without agglomeration. A particle can be described as a single particle (monolithic particle, single grain), for example, as a single crystal. Single particles can exist independently or aggregate together. For example, two to ten single particles can aggregate and contact each other. For example, a single particle is a term used to distinguish it from secondary particles formed by aggregates of tens to hundreds of primary particles, and refers to a single particle composed of a single primary particle. A pseudo-single particle is a composite particle composed of 10 or fewer primary particles. A secondary particle is an aggregate (i.e., a secondary structure) in which tens to hundreds of primary particles are aggregated through physical or chemical bonds between primary particles, even without an intentional aggregation or assembly process of primary particles. Furthermore, primary particles refer to the smallest particle unit that can be distinguished as a single particle when the cross-section of the positive electrode active material is observed using a scanning electron microscope (SEM), and can be composed of a single crystallite (microcrystal) or multiple crystallites. Additionally, a crystallite (or microcrystal) refers to a region within a primary particle where atoms are arranged in a uniform orientation within the crystal lattice structure.

[0027] The span value can be an indicator of the width of the particle size distribution of the positive electrode active material; therefore, the span value can be used to evaluate the uniformity of the positive electrode active material particles. The span value can be represented by Equation 1.

[0028] [Equation 1] Span = (D 90 -D 10 ) / D 50 In equation 1, D 10 D is the particle size of particles that constitute 10% of the total volume in the particle size distribution. 50 It is the particle size of particles that constitute 50% of the cumulative volume in the particle size distribution, and D 90 It is the particle size of particles that account for 90% of the cumulative volume in the particle size distribution.

[0029] The span value can be measured using a particle size analyzer for positive electrode active materials. Specifically, devices such as laser diffraction particle size analyzers and dynamic light scattering analyzers can be used to measure the particle sizes corresponding to approximately 10%, approximately 50%, and approximately 90% of the cumulative volume in the particle size distribution, which are used to calculate the span value.

[0030] In some embodiments of this disclosure, the span value of the positive electrode active material can be from about 1.1 to about 1.3, for example, from about 1.12 to about 1.28, from about 1.14 to about 1.26, from about 1.16 to about 1.24, or from about 1.18 to about 1.22.

[0031] The BET specific surface area of ​​the positive electrode active material can be approximately 0.7 m². 2 / g to approximately 0.9m 2 / g, for example, about 0.8m 2 / g to approximately 0.9m 2 / g or approximately 0.85m 2 / g to approximately 0.9m 2 / g. The BET specific surface area can be measured using a BET specific surface area measuring device utilizing nitrogen adsorption, specifically using the method described in Evaluation Example 2 below. When the span values ​​of the positive electrode active material and the BET specific surface area are within these ranges, the particle size distribution is uniform, thus providing a positive electrode active material with excellent particle uniformity. Therefore, rechargeable lithium batteries comprising the positive electrode active material can exhibit excellent charge / discharge characteristics and cycle life characteristics.

[0032] In some examples, the positive electrode active material may have an average particle size (D) of about 1 μm to about 4 μm, for example about 1 μm to about 3 μm, about 2 μm to about 4 μm, or about 2 μm to about 3 μm. 50 The positive electrode active material can be in the form of single particles. In other examples, the positive electrode active material can be in the form of particles with a diameter of about 0.1 μm to about 3 μm, for example about 0.5 μm to about 2.5 μm, or about 1 μm to about 2 μm. 10 In a further example, the positive electrode active material may be in the form of single particles having a particle size of about 3 μm to about 6 μm, for example about 4 μm to about 6 μm, or about 4 μm to about 5.5 μm. 90 In single-particle form, the positive electrode active material may be in the form of particles having a particle size of about 0.5 μm to about 4 μm, for example about 1 μm to about 3 μm, or about 1.5 μm to about 2.5 μm. 25 The active material can be in the form of single particles. Furthermore, in a further example, the positive electrode active material can have a particle size (D) of about 2.5 μm to about 5 μm, for example about 3 μm to about 5 μm, or about 3 μm to about 4.5 μm. 75 The positive electrode active material is in single-particle form. Besides the span value, when the positive electrode active material is in single-particle form with particle sizes within these ranges, the particle size distribution is more uniform, thus providing a positive electrode active material with excellent particle uniformity. Furthermore, single particles are structurally stable, which can increase the energy density of the positive electrode and improve the long cycle life characteristics of rechargeable lithium batteries. Here, the average particle size (D...) 50 and particle size D 10 D 90 D 25 and D 75 The particle size can be measured using a particle size analyzer that utilizes, for example, laser diffraction.

[0033] Zirconium-containing lithium-nickel composite oxides can be high-nickel oxides. Based on 100 mol% of the total metals excluding lithium in the zirconium-containing lithium-nickel composite oxide, the high-nickel oxide has a nickel content greater than or equal to about 60 mol%. Based on 100 mol% of the total metals excluding lithium in the zirconium-containing lithium-nickel composite oxide, the nickel content can be, for example, greater than or equal to about 65 mol%, greater than or equal to about 70 mol%, greater than or equal to about 75 mol%, greater than or equal to about 80 mol%, greater than or equal to about 85 mol%, greater than or equal to about 90 mol%, greater than or equal to about 91 mol%, or greater than or equal to about 94 mol% and less than or equal to about 99 mol%, or less than or equal to about 98 mol%. When the nickel content in the zirconium-containing lithium-nickel composite oxide is within these ranges, high capacity and high energy density can be achieved.

[0034] In addition to nickel, lithium-nickel composite oxides may also include a specific amount of zirconium as a dopant. For example, based on 100 wt% zirconium-containing lithium-nickel composite oxides, the zirconium content can be from about 0.1 wt% to about 0.4 wt%, such as from about 0.1 wt% to about 0.3 wt%, from about 0.1 wt% to about 0.2 wt%, from about 0.15 wt% to about 0.2 wt%, or from about 0.16 wt% to about 0.18 wt%. If the zirconium content is less than about 0.1 wt% based on 100 wt% zirconium-containing lithium-nickel composite oxides, the positive electrode active material particles may be non-uniform. If the zirconium content exceeds about 0.4 wt%, the excessive addition of zirconium may lead to agglomeration within the positive electrode active material.

[0035] Zirconium-containing lithium-nickel composite oxides can be represented by chemical formula 1.

[0036] [Chemical Formula 1] Li a1 Ni x1 M 1 y1 Zr z1 O 2-b1 X b1 In chemical formula 1, 0.9 ≤ a1 ≤ 1.2, 0.6 ≤ x1 ≤ 0.991, 0 ≤ y1 ≤ 0.5, 0.001 ≤ z1 ≤ 0.003, 0.9 ≤ x1 + y1 + z1 ≤ 1.1, and 0 ≤ b1 ≤ 0.1, M 1X is one or more elements selected from Al, B, Ba, Ca, Ce, Co, Cr, Cu, Fe, Mg, Mn, Mo, Nb, Si, Sn, Sr, Ti, V, W, Y, and Zn, and X is one or more elements selected from F, P, and S. In other embodiments of Formula 1, 0.9 ≤ a1 ≤ 1.1, 0.9 ≤ a1 ≤ 1.05, or 0.9 ≤ a1 ≤ 1, 0.7 ≤ x1 ≤ 0.991 and 0 ≤ y1 ≤ 0.291, 0.8 ≤ x1 ≤ 0.991 and 0 ≤ y1 ≤ 0.191, or 0.9 ≤ x1 ≤ 0.991 and 0 ≤ y1 ≤ 0.091. z1, representing the Zr content, can, for example, be 0.001 ≤ z1 ≤ 0.002. The concentration of zirconium within a single particle can be uniform. For example, each single particle may not have a zirconium concentration gradient from the center to the surface, or the zirconium concentration in the portion closer to the surface may not be higher or lower than in the center of the single particle, and the zirconium may be uniformly distributed within the single particle. This structure can be obtained by synthesizing a positive electrode active material in the form of single particles using a precursor including zirconium, without additional doping of zirconium during the synthesis process of the single particles. For example, this structure can be obtained by using a zirconium-containing nickel oxide as a precursor, mixing the precursor with a lithium feedstock, and subjecting it to heat treatment to synthesize a lithium nickel zirconium composite oxide. Therefore, the zirconium content within the single particle is the same or similar, regardless of its position within the single particle. For example, when the zirconium content is measured at any location in the profile of a single particle, whether the location is near the center or near the surface of the single particle, the zirconium content can be expressed as the same, similar, or uniform.

[0037] In the case of zirconium doping in the synthesis process of single particles, such as in the preparation of zirconium-doped lithium-nickel composite oxides by mixing and sintering a nickel-containing precursor, zirconium feedstock, and lithium feedstock, zirconium may be unevenly distributed and instead condensed within the single particle. However, in the positive electrode active material according to the embodiments of the present disclosure, zirconium is uniformly distributed within the single particle, and no condensation occurs. Therefore, the initial charge / discharge capacity, initial charge / discharge efficiency, and cycle life characteristics of the positive electrode active material can be improved. The uniform distribution of zirconium within the single particle can be determined, for example, by analyzing the distribution of zirconium elemental in a cross-section of the single particle using scanning electron microscopy-energy dispersive spectroscopy (SEM-EDS). That is, the positive electrode active material according to the embodiments of the present disclosure can have zirconium uniformly distributed in the SEM-EDS analysis of the cross-section of the single particle.

[0038] coating According to some example embodiments, the positive electrode active material includes a coating disposed on the surface of the core particle and comprising cobalt and phosphorus.

[0039] In the positive electrode active material, based on the total metals of the positive electrode active material excluding lithium (100 mol%), the cobalt content in the coating can be from about 0.1 mol% to about 5.0 mol%, for example, from about 0.5 mol% to about 4.5 mol%, from about 1.0 mol% to about 4.0 mol%, from about 1.5 mol% to about 3.5 mol%, or from about 2.0 mol% to about 3.0 mol%. When the cobalt content is within these ranges, the positive electrode active material forms a good coating without reducing capacity or increasing resistance, effectively suppressing side reactions with the electrolyte, and effectively reducing gas generation under high voltage or high temperature conditions.

[0040] In the positive electrode active material, based on the total metals of the positive electrode active material excluding lithium (100 mol%), the phosphorus content in the coating can be from about 0.1 mol% to about 1.0 mol%, for example, from about 0.2 mol% to about 0.9 mol%, from about 0.3 mol% to about 0.8 mol%, from about 0.4 mol% to about 0.7 mol%, or from about 0.4 mol% to about 0.6 mol%. When the phosphorus content is within these ranges, the positive electrode active material has a good coating without reducing capacity or increasing resistance, effectively suppresses side reactions with the electrolyte, and effectively reduces gas generation under high voltage or high temperature conditions.

[0041] The coating can exist on the surface of the nucleus in the form of islands, or it can be in the form of a film continuously enveloping the surface of the nucleus, or it can be in the form of a shell enveloping the entire surface of the nucleus. The coating can be formed uniformly with a thin and uniform thickness. With such a structure, the positive electrode active material has improved structural stability without increasing resistance or reducing capacity, can effectively suppress side reactions with the electrolyte, can reduce gas generation under high voltage and high temperature conditions, and can have long cycle life characteristics.

[0042] The thickness of the coating on each particle can be from about 30 nm to about 2000 nm, for example, from about 30 nm to about 1000 nm, from about 30 nm to about 500 nm, from about 30 nm to about 450 nm, from about 30 nm to about 400 nm, from about 30 nm to about 350 nm, from about 30 nm to about 300 nm, from about 30 nm to about 250 nm, from about 30 nm to about 200 nm, from about 30 nm to about 150 nm, from about 50 nm to about 500 nm, from about 80 nm to about 500 nm, or from about 100 nm to about 500 nm. When the coating is within these thickness ranges, the structural stability of the positive electrode active material can be improved, and side reactions with the electrolyte can be effectively suppressed without increasing resistance or reducing capacity due to the coating. The thickness of the coating can be measured, for example, by TOF-SIMS (Time-of-Flight Second Ion Mass Spectrometry), XPS (X-ray Photoelectron Spectroscopy), or EDS (Energy Dispersive X-ray Spectroscopy), and the thickness range of the coating can be measured by TEM-EDS (Transmission Electron Microscopy with Energy Dispersive Spectroscopy) spectral profile.

[0043] Based on a total of 100 wt% zirconium-containing lithium-nickel composite oxide, the amount of residual lithium remaining on the surface of the core particles comprising the zirconium-containing lithium-nickel composite oxide can be less than or equal to about 1500 ppm, for example, from about 1000 ppm to about 1500 ppm. For example, based on a total of 100 wt% zirconium-containing lithium-nickel composite oxide, the amount of residual LiOH remaining on the surface of the core particles comprising the zirconium-containing lithium-nickel composite oxide can be less than or equal to about 0.29 wt%, for example, from about 0.2 wt% to about 0.29 wt%, and based on a total of 100 wt% zirconium-containing lithium-nickel composite oxide, the amount of residual Li₂CO₃ remaining on the surface of the core particles comprising the zirconium-containing lithium-nickel composite oxide can be less than or equal to about 0.4 wt%, for example, from about 0.1 wt% to about 0.4 wt% or from about 0.3 wt% to about 0.4 wt%. The amounts of residual lithium, LiOH, and Li₂CO₃ can be measured by HCl titration.

[0044] Methods for preparing positive electrode active materials The method for preparing the positive electrode active material includes: (i) mixing zirconium raw material and nickel raw material and performing a co-precipitation reaction to prepare a zirconium-containing nickel composite hydroxide; (ii) subjecting the zirconium-containing nickel composite hydroxide to a first heat treatment to prepare a zirconium-containing nickel composite oxide; (iii) mixing the zirconium-containing nickel composite oxide and lithium raw material and performing a second heat treatment to prepare a zirconium-containing lithium nickel composite oxide in the form of secondary particles formed by the aggregation of multiple primary particles; (iv) pulverizing the zirconium-containing lithium nickel composite oxide in the form of secondary particles to obtain an initial positive electrode active material in the form of single particles; and (v) mixing the initial positive electrode active material, cobalt raw material and phosphorus raw material, and performing a third heat treatment and disintegration.

[0045] To incorporate zirconium into positive electrode active materials including lithium-nickel composite oxides, a previous method involved mixing the nickel-based composite hydroxide or nickel-based composite oxide produced after a co-precipitation reaction with a lithium feedstock and subjecting it to heat treatment, followed by the addition of zirconium feedstock during the heat treatment process. This conventional method can be understood as a post-doping of zirconium, where the zirconium is unevenly distributed, leading to the problem of providing single-particle positive electrode active materials with uneven particle growth.

[0046] According to some example embodiments, the method involves adding zirconium feedstock to nickel feedstock for a co-precipitation reaction, which can be understood as a zirconium predoping method.

[0047] Here, zirconium feedstock can be used as a dopant and also as a particle growth promoter (flux). Adding zirconium feedstock promotes particle growth, enabling the efficient synthesis of single particles at lower temperatures compared to existing single-particle synthesis methods. As a result, particle aggregation is suppressed, and productivity is improved. The zirconium feedstock is used as a dopant for the positive electrode active material and does not remain on the surface of the positive electrode active material particles. Therefore, the cycle life characteristics of batteries including this positive electrode active material can be improved.

[0048] In some embodiments of preparing positive electrode active material monoparticles via pre-doping with zirconium, single crystals can be prepared with relatively uniform particle growth due to the uniform distribution of zirconium. Rechargeable lithium batteries comprising positive electrode active material monoparticles with uniform particle growth can exhibit increased charge / discharge capacity and efficiency, and possess excellent cycle life characteristics.

[0049] The preparation method can be understood as a method of mixing and calcining a zirconium-containing nickel composite oxide in oxide form (hereinafter referred to as "oxide precursor") with a lithium feedstock. Typically, a method is used where a lithium feedstock is mixed with a nickel composite hydroxide in hydroxide form (hereinafter referred to as "hydroxide precursor") and calcined. The oxide precursor has a smaller volume than the hydroxide precursor, and therefore can accommodate more material in the reactor (crucible, etc.) during the preparation of the positive electrode active material. This results in a higher reaction yield, which can be significantly advantageous in terms of production volume and economic efficiency. Furthermore, the oxide precursor has a reaction temperature range similar to that of the lithium feedstock, thus offering the advantage of achieving more uniform particle growth of the positive electrode active material compared to the hydroxide precursor.

[0050] The method for preparing the positive electrode active material is described below.

[0051] A method for preparing a positive electrode active material according to some example embodiments includes mixing zirconium raw materials and nickel raw materials and performing a co-precipitation reaction to prepare a zirconium-containing nickel-based composite hydroxide.

[0052] Zirconium feedstocks may include, for example, zirconium oxide, zirconium hydroxide, zirconium hydroxyoxide, zirconium sulfate, zirconium sulfide, zirconium acetate, zirconium nitrate, zirconium halide, or combinations thereof. Specific examples of zirconium feedstocks include ZrO2, ZrO(NO3)2·xH2O (2≤x≤6), Zr(SO4)2·4H2O, or combinations thereof. Nickel feedstocks may include nickel hydroxides, oxides, nitrates, sulfur oxides, carbonates, or combinations thereof.

[0053] In a coprecipitation reaction, metal (M) can be... 1 The raw materials are mixed together with zirconium and nickel raw materials. Here, M 1 It can be one or more of Al, B, Ba, Ca, Ce, Co, Cr, Cu, Fe, Mg, Mn, Mo, Nb, Si, Sn, Sr, Ti, V, W, Y, and Zn. In some embodiments, the metal (M 1 Raw materials may include those containing M 1 Hydroxides, oxides, nitrates, sulfates, carbonates, or combinations thereof of elements.

[0054] Complexing agents and pH control agents can be used in coprecipitation reactions. Complexing agents play a role in controlling the reaction rate of precipitate formation during coprecipitation. Complexing agents can include, for example, ammonium hydroxide (NH4OH), citric acid, or combinations thereof. The concentration of the complexing agent can be from about 0.1 to about 1.5 M, for example, from about 0.1 to about 1.4 M or from about 0.5 to about 1.4 M. pH control agents are used to control the pH of the reactants and can include, for example, sodium hydroxide (NaOH), sodium carbonate (Na2CO3), sodium oxalate (Na2C2O4), or combinations thereof.

[0055] The coprecipitation reaction may include a first step reacting in a pH range of about 11 to about 12 and a second step reacting at a pH lower than that of the first step. The pH of the first step may be, for example, about 11.5 to about 12, about 11.6 to about 11.9, or about 11.7 to about 11.8, and may be considered a pore-forming step. The pH of the second step is lower than that of the first step and may be a particle growth step. The pH of the second step may be, for example, about 10 to about 11.9, about 10.5 to about 11.7, about 11 to about 11.7, about 11.2 to about 11.6, or about 11.3 to about 11.6. The difference between the pH of the first step and the pH of the second step may be, for example, about 0.1 to about 1.5, such as about 0.1 to about 1.0, about 0.1 to about 0.8, about 0.1 to about 0.6, about 0.1 to about 0.5, about 0.1 to about 0.3, or about 0.1 to about 0.2. The first step may proceed for about 6 to about 12 hours or about 8 to about 10 hours. The second step can take approximately 10 to 30 hours, approximately 15 to 25 hours, or approximately 18 to 24 hours.

[0056] The preparation method according to some embodiments includes subjecting a zirconium-containing nickel-based composite hydroxide to a first heat treatment to prepare a zirconium-containing nickel-based composite oxide. The zirconium-containing nickel-based composite oxide can be a precursor of a positive electrode active material and can be referred to as a Zr-predoped oxide precursor. The zirconium-containing nickel-based composite oxide can be synthesized by subjecting a zirconium-containing nickel-based composite hydroxide prepared by a co-precipitation reaction to a first heat treatment.

[0057] The first heat treatment can be carried out at a temperature less than or equal to about 500°C, for example, about 250°C to about 500°C, about 300°C to about 500°C, about 350°C to about 500°C, or about 400°C to about 500°C, for example, about 400°C, about 450°C, or about 500°C. Furthermore, the first heat treatment can be carried out in an oxygen atmosphere or an air atmosphere for about 1 to about 10 hours, for example, about 2 to about 9 hours, or about 4 to about 8 hours.

[0058] The zirconium-containing nickel composite oxide prepared above can be represented by chemical formula 11.

[0059] [Chemical Formula 11] Ni x11 M 1 y11 Zr z11 O2 In Chemical Formula 11, 0.6≤x11≤1, 0≤y11<0.4, 0<z11≤0.3, and 0.9≤x11+y11+z11≤1.1, and M 1 is one or more of Al, B, Ba, Ca, Ce, Co, Cr, Cu, Fe, Mg, Mn, Mo, Nb, Si, Sn, Sr, Ti, V, W, Y, and Zn. In another embodiment of Chemical Formula 11, 0.7≤x11≤1, 0≤y11≤0.3, 0≤z11≤0.3, or 0.8≤x11≤1, 0≤y11≤0.2, 0.1≤z11≤0.3, or 0.9≤x11<1, 0<y11≤0.1, 0.2≤z11≤0.3.

[0060] Based on 100 wt% of the zirconium-containing nickel-based composite oxide, the content of zirconium may be about 0.1 wt% to about 0.5 wt%, for example, about 0.1 wt% to about 0.4 wt%, about 0.1 wt% to about 0.3 wt%, about 0.2 wt% to about 0.3 wt%, or about 0.2 wt% to about 0.25 wt%. If the content of zirconium is less than about 0.1 wt% based on 100 wt% of the zirconium-containing nickel-based composite oxide, it may be difficult to sufficiently promote the grain growth of the primary particles of the positive electrode active material. If the content of zirconium exceeds about 0.5 wt%, excessive addition of zirconium may cause agglomeration within the positive electrode active material.

[0061] The span value of the zirconium-containing nickel-based composite oxide may be about 0.2 to about 0.6, for example, about 0.3 to about 0.6. If the span value of the zirconium-containing nickel-based composite oxide as a precursor is within these ranges, the particle size distribution is uniform, and thus the uniformity of the positive electrode active material prepared using the nickel-based composite oxide is also improved.

[0062] The zirconium-containing nickel-based composite oxide may be in the form of secondary particles. The average particle diameter (D 50 ) of the zirconium-containing nickel-based composite oxide may be about 9 μm to about 16 μm, for example, about 10 μm to about 15 μm, about 11 μm to about 14 μm, or about 12 μm to about 14 μm.

[0063] The tap density (TD) of the zirconium-containing nickel-based composite oxide may be about 2 g / cm 3 to about 3 g / cm 3 , for example, about 2 g / cm 3 to about 2.5 g / cm 3 or about 2.05 g / cm 3Approximately 2.2 g / cm³ 3 When these ranges are met, the reaction yield is high, and uniform particle growth of the active material can be achieved.

[0064] The BET surface area of ​​zirconium-containing nickel composite oxides can be approximately 50 m². 2 / g to approximately 90m 2 / g, for example, about 60m 2 / g to approximately 80m 2 / g or approximately 70m 2 / g to approximately 80m 2 / g. When these ranges are met, the specific surface area of ​​the precursor is high, which can improve the reaction yield and enable uniform particle growth of the active material.

[0065] The preparation method according to some embodiments includes (iii) mixing a zirconium-containing nickel composite oxide and a lithium raw material and subjecting them to a second heat treatment to prepare a zirconium-containing lithium nickel composite oxide in the form of secondary particles as aggregates of primary particles.

[0066] Lithium feedstocks may include, for example, lithium hydroxide, lithium carbonate, lithium sulfate, lithium nitrate, or combinations thereof. Anhydrous lithium hydroxide may be an example of a lithium feedstock.

[0067] The method for preparing positive electrode active materials according to some embodiments promotes uniform grain growth of the positive electrode active material by using a doped zirconium-containing nickel composite oxide. Such a method has the advantage of being able to effectively synthesize single particles even when heat treatment is performed at a lower temperature than conventional single-particle synthesis methods.

[0068] The second heat treatment temperature may be less than or equal to about 900°C, less than or equal to about 890°C, less than or equal to about 850°C, or less than or equal to about 810°C, for example, about 600°C to about 900°C, about 600°C to about 850°C, or about 600°C to about 800°C. The second heat treatment may be carried out in an oxidizing gas atmosphere, for example, for about 4 hours to about 16 hours, about 5 hours to about 16 hours, or about 6 hours to about 16 hours.

[0069] In methods for preparing positive electrode active materials according to some embodiments, alkaline grain growth promoters or fluxes may not be added during the mixing of zirconium-containing nickel composite oxides and lithium feedstock, and during the second heat treatment. Therefore, an increase in resistance caused by residues after the second heat treatment can be prevented, which improves the cycle life characteristics of rechargeable lithium batteries including positive electrode active materials. Furthermore, because no additional residue removal process is required, productivity and processability can be improved. Alkaline grain growth promoters refer to additives that provide or contain alkali metal components during the heat treatment process, thereby promoting surface diffusion and mass transfer of particles, thus promoting grain growth, reducing sintering temperature, or controlling the state of particle aggregates. Examples of alkaline grain growth promoters include Na₂CO₃, NaOH, K₂CO₃, KOH, and Li₂CO₃.

[0070] Furthermore, as described above, in the method for preparing the positive electrode active material, zirconium raw material can be pre-added during the synthesis of the zirconium-containing nickel composite oxide before the second heat treatment of the zirconium-containing nickel composite oxide and the lithium raw material. Therefore, zirconium can be uniformly doped into the zirconium-containing nickel composite oxide, thereby promoting the growth of single particles of the positive electrode active material and providing uniformly grown positive electrode active material particles.

[0071] As a result of the second heat treatment, secondary particles comprising zirconium-containing lithium-nickel composite oxides can be obtained. For example, the zirconium-containing lithium-nickel composite oxides obtained after the second heat treatment may include secondary particles as aggregates of primary particles. Here, the primary particles forming the secondary particles can grow sufficiently and become single particles due to the addition of zirconium raw materials.

[0072] The average particle size (D) of the secondary particles obtained 50 The diameter of the secondary particles can be from about 10 μm to about 20 μm, for example, from about 10 μm to about 18 μm, from about 12 μm to about 16 μm, or from about 12 μm to about 14 μm. The average particle size (D) of the secondary particles... 50 It can be measured through SEM (scanning electron microscope) images.

[0073] The average particle size (D) of the primary particles that make up the secondary particles 50 The primary particle size can be from about 1 μm to about 4 μm, for example, from about 1 μm to about 3 μm, from about 2 μm to about 4 μm, or from about 2 μm to about 3 μm. The average particle size (D) of the primary particles... 50 It can be measured by SEM images of the surface of secondary particles.

[0074] According to some embodiments, a method for preparing a positive electrode active material includes pulverizing a lithium-nickel composite oxide in the form of secondary particles to obtain an initial positive electrode active material in the form of single particles.

[0075] The grinding of secondary particles refers to breaking down the prepared secondary particles so that the primary particles constituting the secondary particles separate from each other into individual particles. As a result of grinding, an average particle size (D) can be obtained. 50 The above-mentioned initial positive electrode active material is in the form of single particles of about 1 μm to about 4 μm.

[0076] Grinding can be carried out using jet milling equipment. When grinding with jet milling, the bed weight can be from about 250 kg to about 300 kg, the rotation speed of the screen wheel can be from about 1500 rpm to about 2000 rpm, the rotation speed of the blower can be from about 2500 rpm to about 3500 rpm, the pulse pressure can be from about 0.25 bar to about 0.75 bar, the gap pressure can be from about 0.3 bar to about 0.5 bar, and the G / A can be from about 6 bar to 8 bar.

[0077] The grinding time can vary depending on the rotational speed of the sieve wheel, the speed of the blower, the pressure, and the bed weight of the jet mill. In some examples, based on jet mill equipment, 4 kg to 6 kg of sample can be processed per minute.

[0078] As described above, the initial positive electrode active material in single-particle form may include a compound represented by chemical formula 1.

[0079] Based on 100 wt% of the initial positive electrode active material in single-particle form, the zirconium content can be from about 0.1 wt% to about 0.4 wt%, for example, from about 0.1 wt% to about 0.3 wt%, from about 0.1 wt% to about 0.2 wt%, from about 0.15 wt% to about 0.2 wt%, or from about 0.16 wt% to about 0.18 wt%. The zirconium content included in the initial positive electrode active material can be measured using SEM (scanning electron microscopy)-EDS (energy-dispersive X-ray spectroscopy) analysis techniques.

[0080] The method for preparing the positive electrode active material according to some embodiments further includes mixing the initial positive electrode active material, cobalt raw material, and phosphorus raw material, subjecting it to a third heat treatment, and then disintegrating the result. Through these steps, single particles coated with the desired material can be obtained. These steps can be referred to as a dry coating process.

[0081] Here, the cobalt raw material can be a cobalt hydroxide, oxide, sulfur oxide, nitrate, or carbonate. The phosphorus raw material can be a phosphorus hydroxide, oxide, sulfur oxide, phosphate, nitrate, or carbonate.

[0082] Based on the total metal content (excluding lithium) of 100 mol% in the positive electrode active material, the amount of cobalt in the cobalt raw material can be from about 0.1 mol% to about 5.0 mol%, for example, from about 0.5 mol% to about 4.5 mol%, from about 1.0 mol% to about 4.0 mol%, from about 1.5 mol% to about 3.5 mol%, or from about 2.0 mol% to about 3.0 mol%. When the cobalt content is within these ranges, the positive electrode active material forms a good coating without reducing capacity or increasing resistance, effectively suppresses side reactions with the electrolyte, and effectively reduces gas generation under high voltage or high temperature conditions.

[0083] Based on the total metal content (excluding lithium) of 100 mol% in the positive electrode active material, the amount of phosphorus in the phosphorus raw material can be from about 0.1 mol% to about 1.0 mol%, for example, from about 0.2 mol% to about 0.9 mol%, from about 0.3 mol% to about 0.8 mol%, from about 0.4 mol% to about 0.7 mol%, or from about 0.4 mol% to about 0.6 mol%. If the phosphorus content is within these ranges, the positive electrode active material forms a good coating without reducing capacity or increasing resistance, effectively suppresses side reactions with the electrolyte, and effectively reduces gas generation under high voltage or high temperature conditions.

[0084] The third heat treatment can be carried out in an oxidizing gas atmosphere. The third heat treatment can be carried out, for example, at about 500°C to about 900°C, or about 600°C to about 900°C, or about 600°C to about 800°C. The third heat treatment can be carried out for about 5 to about 20 hours, for example, about 7 to about 20 hours, or about 10 to about 20 hours.

[0085] Following the third heat treatment, a disintegration process can be performed. As a result of this disintegration process, particle agglomeration is further eliminated, enabling the manufacture of high-density, long-cycle-life rechargeable lithium-ion batteries, including the positive electrode active material. Here, "disintegration" refers to the dispersion and pulverization of relatively weakly cohesive materials, such as particle agglomerates or granules. Disintegration is typically carried out using equipment such as cutting mills, roller crushers, or coal mills to remove the weak cohesive forces between secondary particles. For example, the disintegration process can be performed using a rotary impact crusher, cutting mill, ball mill, or bead mill equipped with sorting devices such as screens.

[0086] The positive electrode active material obtained by this preparation method comprises particles with a core and a coating. The core contains a zirconium-containing lithium-nickel composite oxide, and the coating is disposed on the surface of the core and includes cobalt and phosphorus. The positive electrode active material can have an average particle size (D... 50 The particles are in the form of single particles from about 1 μm to about 4 μm, and may include, for example, a mixture of uncrushed secondary particles and crushed single particles.

[0087] positive electrode In some embodiments, a positive electrode comprising the aforementioned positive electrode active material is provided. The positive electrode comprises, for example, a current collector and a layer of positive electrode active material on the current collector. The positive electrode active material layer may include the aforementioned positive electrode active material and may also include a binder and / or a conductive material. The positive electrode may also include additives that can act as a sacrificial positive electrode.

[0088] The positive electrode active material may include core particles and a coating. The core particles comprise a zirconium-containing lithium-nickel composite oxide, and based on a total metal content of 100 mol% excluding lithium in the positive electrode active material, the amount of nickel is greater than or equal to about 60 mol%. The coating is disposed on the surface of each core particle and includes cobalt and phosphorus. The positive electrode active material may have a thickness of about 0.7 μm. 2 / g to approximately 0.9m 2 The BET specific surface area is / g, and it exists in single-particle form.

[0089] Based on a 100wt% positive electrode active material layer, the amount of positive electrode active material can be from about 90wt% to about 99.5wt%. Based on the 100wt% positive electrode active material layer, the amounts of binder and conductive material can be from about 0.5wt% to about 5wt%, respectively.

[0090] The binder is used to adhere the positive electrode active material particles to each other, and also to adhere the positive electrode active material to the current collector. Examples of binders include polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers containing ethylene oxide, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, (meth)acrylated styrene-butadiene rubber, epoxy resin, (meth)acrylate resin, polyester resin, nylon, etc. However, this disclosure is not limited to these examples.

[0091] Conductive materials are used to impart conductivity to electrodes and can be any material that conducts electrons without causing undesirable chemical changes in a battery. Examples of conductive materials include: carbon-based materials such as natural graphite, synthetic graphite, carbon black, acetylene black, Ketjen black, carbon fibers, carbon nanofibers, and carbon nanotubes; metallic materials, including copper, nickel, aluminum, silver, etc., in the form of metal powders or metal fibers; conductive polymers, such as polyphenylene derivatives; or mixtures thereof.

[0092] Aluminum film can be used as a current collector, but it is not limited to this.

[0093] Rechargeable lithium batteries Embodiments of this disclosure include a rechargeable lithium battery comprising the aforementioned positive electrode, negative electrode, and electrolyte. In an example, the rechargeable lithium battery may include a positive electrode, a negative electrode, a separator between the positive and negative electrodes, and an electrolyte solution.

[0094] Rechargeable lithium batteries can be cylindrical, prismatic, pouch-shaped, coin-shaped, etc., depending on their shape. Figures 1 to 4 This is a schematic diagram illustrating a rechargeable lithium battery according to some embodiments, wherein, Figure 1 It is a cylindrical battery. Figure 2 It is a prismatic battery, and Figure 3 and Figure 4 It's a pouch battery. (See reference) Figures 1 to 4 The rechargeable lithium battery 100 includes an electrode assembly 40 and a housing 50. The electrode assembly 40 has a separator 30 disposed between a positive electrode 10 and a negative electrode 20. The electrode assembly 40 is housed within the housing 50. The positive electrode 10, the negative electrode 20, and the separator 30 may be impregnated with an electrolyte solution (not shown). Figure 1 As shown, the rechargeable lithium battery 100 may include a sealing member 60 of the sealed housing 50. Furthermore, as... Figure 2 As shown, the rechargeable lithium battery 100 may include a positive electrode lead connector 11, a positive electrode terminal 12, a negative electrode lead connector 21, and a negative electrode terminal 22. Figure 3 and Figure 4 As shown, the rechargeable lithium battery 100 includes electrode terminals 70 (i.e., positive electrode terminal 71 and negative electrode terminal 72) that form an electrical path for guiding current formed in the electrode assembly 40 to the outside of the battery.

[0095] negative electrode The negative electrode may include a current collector and a layer of negative electrode active material on the current collector, and the layer of negative electrode active material may include a negative electrode active material. The negative electrode may also include a binder, a conductive material, or a combination thereof.

[0096] Negative electrode active material The negative electrode active material may include materials that can reversibly insert / deintercalate lithium ions, lithium metal, lithium metal alloys, materials that can be doped / dedoped with lithium, or transition metal oxides.

[0097] Materials that can reversibly insert / deintercalate lithium ions can include carbon-based negative electrode active materials, such as crystalline carbon, amorphous carbon, or combinations thereof. Crystalline carbon can be graphite, such as amorphous, flake-like, spherical, or fibrous natural or artificial graphite, while amorphous carbon can be soft carbon, hard carbon, mesophase pitch carbonization products, calcined coke, etc.

[0098] The lithium metal alloy may include an alloy of lithium and a metal of Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, and Sn.

[0099] The material capable of doping / de-doping lithium may be a Si-based negative active material or a Sn-based negative active material. The Si-based negative active material may include silicon, a silicon-carbon composite, SiO x (0<x≤2), a Si-Q alloy, or a combination thereof. In the formula Si-Q, Q is an element selected from among an alkali metal, an alkaline earth metal, a Group 13 element, a Group 14 element (excluding Si), a Group 15 element, a Group 16 element, a transition metal, a rare earth element, and a combination thereof, for example, Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Tl, Ge, P, As, Sb, Bi, S, Se, Te, Po, and a combination thereof. The Sn-based negative active material may be Sn, SnO2, a Sn alloy, or a combination thereof.

[0100] The silicon-carbon composite may be a composite of silicon and amorphous carbon. An average particle diameter (D 50 ) of the silicon-carbon composite particle may be, for example, about 0.5 μm to about 20 μm. According to some embodiments, the silicon-carbon composite material may be in the form of silicon particles and amorphous carbon coated on a surface of the silicon particles. For example, the silicon-carbon composite may include secondary particles (core) assembled from silicon primary particles and an amorphous carbon coating (shell) on the surface of the secondary particles. The amorphous carbon may also be present between the silicon primary particles, e.g., the silicon primary particles may be coated with amorphous carbon. The secondary particles may be dispersed in an amorphous carbon matrix.

[0101] The silicon-carbon composite may further include crystalline carbon. For example, the silicon-carbon composite may include a core including crystalline carbon and silicon particles and an amorphous carbon coating on the surface of the core. The crystalline carbon may be artificial graphite, natural graphite, or a combination thereof. The amorphous carbon may include soft carbon or hard carbon, a mesophase pitch carbonized product, and fired coke.

[0102] When the silicon-carbon composite comprises silicon and amorphous carbon, based on 100 wt% of the silicon-carbon composite, an amount of the silicon may be about 10 wt% to about 50 wt%, and an amount of the amorphous carbon may be about 50 wt% to about 90 wt%. Also, when the composite comprises silicon, amorphous carbon, and crystalline carbon, based on 100 wt% of the silicon-carbon composite, an amount of the silicon may be about 10 wt% to about 50 wt%, an amount of the crystalline carbon may be about 10 wt% to about 70 wt%, and an amount of the amorphous carbon may be about 20 wt% to about 40 wt%.

[0103] Also, a thickness of the amorphous carbon coating may be about 5 nm to about 100 nm. An average particle diameter (D 50 ) of the silicon particles (primary particles) may be about 10 nm to about 1 μm or about 10 nm to about 200 nm. The silicon particles may exist as silicon alone, may exist in the form of a silicon alloy, or may exist in an oxidized form. The oxidized form of silicon may be represented by SiO x (0<x≤2). A Si:O atomic content ratio representing an oxidation degree may be about 99:1 to about 33:67. As used herein, when a definition is not otherwise provided, an average particle diameter (D 50 ) refers to a diameter of particles having a cumulative volume of about 50 volume% in the particle distribution.

[0104] The Si-based negative electrode active material or the Sn-based negative electrode active material may be mixed with the carbon-based negative electrode active material. When the Si-based negative electrode active material or the Sn-based negative electrode active material is mixed with the carbon-based negative electrode active material, a mixing ratio may be about 1:99 to about 90:10 in a weight ratio.

[0105] adhesive A binder is used to adhere the negative electrode active material particles to each other and also to adhere the negative electrode active material to a current collector. The binder may include a non-aqueous binder, an aqueous binder, a dry binder, or a combination thereof.

[0106] The non-aqueous binder may include polyvinylchloride, carboxylated polyvinylchloride, polyfluoride, ethylene propylene copolymer, polystyrene, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyamideimide, polyimide, or a combination thereof.

[0107] The aqueous binder may be selected from styrene-butadiene rubber, (meth)acryliclated styrene-butadiene rubber, (meth)acrylonitrile-butadiene rubber, (meth)acrylic acid rubber, butyl rubber, fluorine rubber, polyethylene oxide, polyvinylpyrrolidone, polyepichlorohydrin, polyphosphazene, poly(meth)acrylonitrile, ethylene propylene diene copolymers, polyvinyl pyridine, chlorosulfonated polyethylene, latex, polyester resin, (meth)acrylic resin, phenolic resin, epoxy resin, polyvinyl alcohol, and a combination thereof.

[0108] When an aqueous binder is used as the negative electrode binder, it may also include a cellulose compound capable of imparting viscosity. The cellulose compound may include at least one of carboxymethyl cellulose, hydroxypropyl methyl cellulose, methyl cellulose, or an alkali metal salt thereof. The alkali metal may include Na, K, or Li.

[0109] The dry binder can be a polymeric material capable of forming fibers, and can be, for example, polytetrafluoroethylene, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polyethylene oxide, or a combination thereof.

[0110] conductive materials This includes conductive materials to provide electrode conductivity, and any electrically conductive material that does not cause undesirable chemical changes in the battery can be used as the conductive material. Examples of conductive materials include: carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fibers, carbon nanofibers, carbon nanotubes, etc.; metallic materials in the form of metal powders or metal fibers, including copper, nickel, aluminum, silver, etc.; conductive polymers, such as polyphenylene derivatives; or mixtures thereof.

[0111] Based on a 100wt% negative electrode active material layer, the amount of negative electrode active material can be from about 95wt% to about 99.5wt%, and the amount of binder can be from about 0.5wt% to about 5wt%. For example, the negative electrode active material layer may include about 90wt% to about 99wt% of negative electrode active material, about 0.5wt% to about 5wt% of binder, and about 0.5wt% to about 5wt% of conductive material.

[0112] current collector The negative electrode current collector may include, for example, indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or alloys thereof, and may be in the form of foil, sheet, or foam. The thickness of the negative electrode current collector may be, for example, about 1 μm to about 20 μm, about 5 μm to about 15 μm, or about 7 μm to about 10 μm.

[0113] electrolytes The electrolyte used in rechargeable lithium batteries can be an electrolyte solution, which may include non-aqueous organic solvents and lithium salts.

[0114] Non-aqueous organic solvents are used as media for transporting ions that participate in the electrochemical reactions of a battery. Non-aqueous organic solvents can be carbonate solvents, ester solvents, ether solvents, ketone solvents, alcohol solvents, aprotic solvents, or combinations thereof.

[0115] Carbonate solvents can include dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), methyl ethyl carbonate (MEC), ethylene carbonate (EC), propylene carbonate (PC), and butyl carbonate (BC), etc. Ester solvents can include methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, decanolactone, mevalonolactone, valproic acid lactone, caprolactone, etc. Ether solvents can include dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, dimethoxyethane, 2-methyltetrahydrofuran, 2,5-dimethyltetrahydrofuran, tetrahydrofuran, etc. Additionally, ketone solvents can include cyclohexanone, etc. Alcohol solvents may include ethanol, isopropanol, etc., and aprotic solvents may include: nitriles, such as R-CN (where R is a C2 to C20 straight-chain, branched or cyclic hydrocarbon group, and may include double bonds, aromatic rings or ether groups, etc.); amides, such as dimethylformamide; dioxolane, such as 1,3-dioxolane, 1,4-dioxolane, etc.; sulfolane, etc.

[0116] Non-aqueous organic solvents can be used alone or in mixtures of two or more types. As is known to those skilled in the art, when two or more types are used in a mixture, the mixing ratio can be appropriately adjusted according to the desired battery performance.

[0117] When using carbonate solvents, cyclic carbonates and chain carbonates can be mixed and used, and cyclic carbonates and chain carbonates can be mixed in a volume ratio of about 1:1 to about 1:9.

[0118] Non-aqueous organic solvents may also include aromatic organic solvents. For example, carbonate solvents and aromatic organic solvents can be mixed and used in a volume ratio of about 1:1 to about 30:1.

[0119] The electrolyte solution may also include vinyl ethyl carbonate, vinylene carbonate, or ethylene carbonate compounds to improve battery cycle life.

[0120] Examples of ethylene carbonate compounds include fluoroethylene carbonate, difluoroethylene carbonate, chloroethylene carbonate, dichloroethylene carbonate, bromoethylene carbonate, dibromoethylene carbonate, nitroethylene carbonate, and cyanoethylene carbonate.

[0121] Lithium salts dissolved in organic solvents supply lithium ions in batteries, enabling rechargeable lithium batteries to operate fundamentally and improving lithium ion transport between the positive and negative electrodes. Examples of lithium salts include LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiAlO2, LiAlCl4, LiPO2F2, LiCl, LiI, LiN(SO2C2F5)2, Li(FSO2)2N (lithium bis(fluorosulfonyl)imide; LiFSI), LiC4F9SO3, and LiN(C x F 2x+1 SO2)(C y F 2y+1 At least one of the following: (SO2) (where x and y are integers from 1 to 20), lithium trifluoromethanesulfonate, lithium tetrafluoroethanesulfonate, lithium difluorobis(oxalate)phosphate (LiDFBOP), and lithium bis(oxalate)borate (LiBOB).

[0122] The concentration of lithium salt can be from about 0.1 M to about 2.0 M. When the concentration of lithium salt is within this range, the electrolyte solution has suitable ionic conductivity and viscosity, thus achieving excellent performance and allowing lithium ions to move efficiently.

[0123] diaphragm Depending on the type of rechargeable lithium battery, a separator may be present between the positive and negative electrodes. The separator may include multilayer films of polyethylene, polypropylene, polyvinylidene fluoride, or two or more layers thereof, such as hybrid multilayer films such as polyethylene / polypropylene bilayer separators, polyethylene / polypropylene / polyethylene trilayer separators, polypropylene / polyethylene / polypropylene trilayer separators, etc.

[0124] The diaphragm may include a porous substrate and a coating on one or both surfaces of the porous substrate, comprising organic materials, inorganic materials, or combinations thereof.

[0125] The porous substrate can be a polymer film formed from any one or a copolymer or mixture of two or more of the following polymers: polyolefins (such as polyethylene and polypropylene), polyesters (such as polyethylene terephthalate and polybutylene terephthalate), polyacetal, polyamide, polyimide, polycarbonate, polyetherketone, polyaryletherketone, polyetherimide, polyamideimide, polybenzimidazole, polyethersulfone, polyphenylene ether, cyclic olefin copolymers, polyphenylene sulfide, polyethylene naphthalate, and polytetrafluoroethylene (such as TEFLON). ® The porous substrate may include glass fibers, or may include a composite film of polymer and glass fibers.

[0126] The porous substrate may have a thickness of about 1 μm to about 40 μm, for example about 1 μm to about 30 μm, about 1 μm to about 20 μm, about 5 μm to about 15 μm, or about 10 μm to about 15 μm.

[0127] Organic materials may include (meth)acrylic acid copolymers, which include a first structural unit and a second structural unit, wherein the first structural unit is derived from (meth)acrylamide, and the second structural unit includes at least one structural unit derived from (meth)acrylic acid or (meth)acrylate and a structural unit derived from (meth)acrylamide sulfonic acid or a salt thereof.

[0128] Inorganic materials may include inorganic particles selected from Al2O3, SiO2, TiO2, SnO2, CeO2, MgO, NiO, CaO, GaO, ZnO, ZrO2, Y2O3, SrTiO3, BaTiO3, Mg(OH)2, boehmite, and combinations thereof. However, this disclosure is not limited to these examples. The average particle size (D) of the inorganic particles... 50 The wavelength range can be from about 1 nm to about 2000 nm, for example, from about 100 nm to about 1000 nm or from about 100 nm to about 700 nm.

[0129] Organic and inorganic materials can be mixed in a coating, or coatings containing organic materials and coatings containing inorganic materials can be stacked.

[0130] The thickness of the coating can be from about 0.5 μm to about 20 μm, for example, from about 1 μm to about 10 μm or from about 1 μm to about 5 μm.

[0131] Examples and comparative examples of this disclosure are described below. However, this disclosure is not limited to the following examples.

[0132] Example 1 1. Preparation of positive electrode active material (1) Preparation of zirconium-containing nickel composite oxides First, zirconium-containing nickel composite oxides were prepared by the following co-precipitation method.

[0133] Nickel sulfate, cobalt sulfate, and manganese sulfate were dissolved in distilled water and then mixed with zirconium raw material Zr(SO4)2·4H2O to prepare a metal raw material mixture solution. The nickel sulfate, cobalt sulfate, manganese sulfate, and zirconium raw material were mixed in a molar ratio of Ni:Co:Mn:Zr = 94.8:4:1:0.2.

[0134] Prepare dilute solutions of ammonia (NH4OH) as a complexing agent and sodium hydroxide (NaOH) as a pH control agent. The concentration of ammonia is 10 wt%, and the concentration of sodium hydroxide is 20 wt%. Inject the prepared metal raw material mixture solution, the diluted ammonia solution, and the sodium hydroxide into the reactor.

[0135] A synthesis rate differential was created between the inside and outside of the particles by stirring the mixture for 10 hours with the pH set to 11.75 inside the reactor (step one), and then stirring for 22 hours by lowering the pH to 11.55 (step two). This resulted in the synthesis of zirconium-containing nickel-based composite hydroxides.

[0136] Subsequently, the zirconium-containing nickel-based composite hydroxide was heat-treated at 400°C for 6 hours in an oxygen atmosphere to form an average particle size (D). 50 The zirconium-containing nickel composite oxide with a diameter of 13.5 μm (hereinafter referred to as "Zr predoped oxide precursor").

[0137] (2) Preparation of the initial positive electrode active material The prepared zirconium-containing nickel composite oxide was mixed with anhydrous lithium hydroxide and then heat-treated at 770°C for 12 hours under an oxygen atmosphere. The zirconium-containing lithium-nickel composite oxide prepared by heat treatment exhibited LiNi 0.948 Co 0.04 Mn 0.01 Zr 0.002 The composition of O2 was determined, and it was confirmed to be in the form of secondary particles.

[0138] Subsequently, by setting the bed weight to 300 kg, the screen wheel speed to 1740 rpm, the blower speed to 3000 rpm, the pulse pressure to 0.5 bar, the gap pressure to 0.4 bar, and the G / A ratio to 6.3 bar, zirconium-containing lithium-nickel composite oxides were pulverized using jet milling (5 kg per minute). This yielded the initial positive electrode active material (LiNi) in single-particle form. 0.948 Co 0.04 Mn 0.01 Zr 0.002 O2).

[0139] The average particle size (D) of the initial positive electrode active material was confirmed. 50 The value is 2.5 μm, D 10 The particle size is 1.47 μm, D 90 The particle size is 4.87 μm.

[0140] The Zr content was 0.18 wt% based on the initial positive electrode active material of 100 wt% using ICP-OES (inductively coupled plasma emission spectroscopy).

[0141] (3) Preparation of positive electrode active material The prepared initial positive electrode active material in single-particle form, cobalt hydroxide (Co(OH)2), and monoammonium phosphate (NH4H2PO4, ammonium dihydrogen phosphate) were dry-mixed, heat-treated, and then disintegrated at 660°C for 8 hours in an oxygen atmosphere to prepare the positive electrode active material. Disintegration was performed using a needle mill at 12000 rpm. Based on the total metal content (excluding lithium) of 100 mol% in the positive electrode active material, the cobalt content in the cobalt hydroxide was designed to be 3.0 mol%, and the phosphorus content in the monoammonium phosphate was designed to be 0.5 mol%.

[0142] 2. Manufacturing of rechargeable lithium battery cells A slurry of positive electrode active material was prepared by mixing 98.5 wt% of positive electrode active material, 1.0 wt% of polyvinylidene fluoride binder, and 0.5 wt% of carbon nanotube conductive material. The slurry was coated onto an aluminum foil current collector, then dried and pressed to fabricate the positive electrode. The prepared positive electrode comprises positive electrode active material in the form of pulverized single particles.

[0143] A negative electrode active material slurry was prepared by mixing 97.5 wt% graphite negative electrode active material, 1.5 wt% carboxymethyl cellulose, and 1 wt% styrene-butadiene rubber in an aqueous solvent. The negative electrode active material slurry was coated onto a copper foil current collector, dried, and pressed to manufacture the negative electrode.

[0144] Rechargeable lithium-ion battery cells are manufactured using conventional methods, employing positive and negative electrodes, a polytetrafluoroethylene separator, and an electrolyte solution prepared by dissolving 1 M LiPF6 in a mixed solvent of ethylene carbonate and dimethyl carbonate in a volume ratio of 3:7.

[0145] Example 2 The positive electrode active material and rechargeable lithium battery cell are manufactured in the same manner as in Example 1, except that in the preparation of the positive electrode active material, the cobalt content in cobalt hydroxide is designed to be 2.0 mol based on the total metal content of 100 mol% excluding lithium in the positive electrode active material.

[0146] Comparison Example 1 The positive electrode active material and rechargeable lithium battery cell were prepared in the same manner as in Example 1, except that: in the preparation of the positive electrode active material, cobalt hydroxide was not mixed, and the amount of phosphorus in monoammonium phosphate was designed to be 0.1 mol based on 100 mol% of total metals other than lithium in the positive electrode active material.

[0147] Comparison Example 2 The positive electrode active material and the rechargeable lithium battery cell were manufactured in the same manner as in Comparative Example 1, except that in the preparation of the positive electrode active material, the amount of phosphorus in the monoammonium phosphate was designed to be 0.2 mol based on the total metal content of the positive electrode active material excluding lithium (100 mol%).

[0148] Comparison Example 3 The positive electrode active material and the rechargeable lithium battery cell were manufactured in the same manner as in Comparative Example 1, except that in the preparation of the positive electrode active material, the amount of phosphorus in the monoammonium phosphate was designed to be 0.5 mol based on the total metal content of the positive electrode active material excluding lithium (100 mol%).

[0149] Compare Example 4 The positive electrode active material and the rechargeable lithium battery cell were manufactured in the same manner as in Comparative Example 1, except that in the preparation of the positive electrode active material, the amount of phosphorus in the monoammonium phosphate was designed to be 1.0 mol based on the total metal content of the positive electrode active material excluding lithium of 100 mol%.

[0150] Compare Example 5 The positive electrode active material and rechargeable lithium battery cell are manufactured in the same manner as in Example 1, except that monoammonium phosphate is not mixed in the preparation of the positive electrode active material, and the cobalt content in cobalt hydroxide is designed to be 1.0 mol based on the total metal content of 100 mol% other than lithium in the positive electrode active material.

[0151] Comparison Example 6 The positive electrode active material and the rechargeable lithium battery cell were manufactured in the same manner as in Comparative Example 5, except that in the preparation of the positive electrode active material, the cobalt content in cobalt hydroxide was designed to be 2.0 mol based on the total metal content of 100 mol% excluding lithium in the positive electrode active material.

[0152] Compare Example 7 The positive electrode active material and rechargeable lithium battery cell were manufactured in the same manner as in Comparative Example 5, except that in the preparation of the positive electrode active material, the cobalt content in cobalt hydroxide was designed to be 3.0 mol based on the total metal content of 100 mol% excluding lithium in the positive electrode active material.

[0153] Compare Example 8 The positive electrode active material and rechargeable lithium battery cells are manufactured in the same manner as in Example 1, except that in the preparation of the zirconium-containing nickel composite oxide, steps one and two are replaced by stirring inside the reactor at pH 10.5 for 33 hours to prepare an average particle size (D). 50 ( ) is a zirconium-containing nickel composite oxide with a diameter of 3.0 μm.

[0154] Compare Example 9 A zirconium-containing nickel-based composite hydroxide was prepared according to the positive electrode active material preparation process of Example 1, and the zirconium-containing nickel-based composite hydroxide (hereinafter referred to as the "Zr pre-doped hydroxide precursor") was mixed with anhydrous lithium hydroxide. Subsequently, the mixture was heat-treated in the same manner as the second heat treatment in Example 1. Furthermore, the process after the second heat treatment was the same as the process in Example 1 to manufacture the positive electrode active material and the rechargeable lithium battery cell.

[0155] Compare Example 10 1. Preparation of positive electrode active material Nickel-based composite hydroxides were synthesized in the same manner as in Example 1, except that nickel sulfate, cobalt sulfate, and manganese sulfate were dissolved in distilled water as a solvent at a molar ratio of Ni:Co:Mn = 95:4:1 to prepare a mixed solution of metal raw materials (not mixed with zirconium raw material Zr(SO4)2·4H2O). Subsequently, the nickel-based composite hydroxides were heat-treated at 400°C for 6 hours under an oxygen atmosphere to prepare nickel-based composite oxides.

[0156] The prepared nickel-based composite oxide (hereinafter referred to as "Zr undoped oxide precursor") was mixed with anhydrous lithium hydroxide and ZrO2. The mixture was then heat-treated in the same manner as the second heat treatment in Example 1 to prepare the Zr post-doped oxide precursor.

[0157] In addition, the process following the second heat treatment is carried out in the same manner as in Example 1 to manufacture the positive electrode active material and the rechargeable lithium battery cell.

[0158] Evaluation Example 1: Evaluation of the properties of Zr predoped precursors The span and tap density (g / cm³) of the Zr pre-doped oxide precursor prepared in Example 1, the Zr pre-doped hydroxide precursor prepared in Comparative Example 9, and the Zr undoped oxide precursor prepared in Comparative Example 10 were measured. 3 ), BET (m 2 The results are shown in Table 1.

[0159] Specifically, the particle size D of each precursor was measured.10 D 50 and D 90 This corresponds to the 10%, 50%, and 90% cumulative values ​​in its particle size distribution. By calculating {(D... 90 -D 10 ) / D 50 The formula for} uses measured values ​​to derive the span value, and the results are shown in Table 1.

[0160] In addition, each precursor powder was tapped according to ASTM B527 standard, and the volume of the powder after tapping was measured. The tap density (g / cm³) was then measured by dividing the powder mass by the powder volume. 3 The results are shown in Table 1.

[0161] The BET specific surface area of ​​each precursor was also measured using a BET analyzer, and the results are shown in Table 1.

[0162] In addition, the Zr content of the Zr predoped oxide precursor prepared in Example 1, the Zr predoped hydroxide precursor prepared in Comparative Example 9, and the Zr undoped oxide precursor prepared in Comparative Example 10 were measured by ICP-OES (Inductively Coupled Plasma Emission Spectroscopy), and the results are shown in Table 1.

[0163] Table 1

[0164] Referring to Table 1, the Zr-predoped oxide precursor of Example 1 exhibits a lower span value than that of Comparative Examples 9 and 10. Therefore, it is confirmed that the Zr-predoped oxide precursor of Example 1 has a more uniform particle size distribution.

[0165] Compared to the materials of Comparative Examples 9 and 10, the Zr-predoped oxide precursor of Example 1 exhibits a higher tap density, resulting in a smaller volume after tapping for the same mass. Therefore, it is confirmed that the Zr-predoped oxide precursor of Example 1 exhibits a higher reaction yield than the comparative examples.

[0166] Compared to the materials of Comparative Examples 9 and 10, the Zr-predoped oxide precursor of Example 1 exhibits an extremely high BET specific surface area. Therefore, it can be seen that uniform precursor particles (or powder) contribute to the high specific surface area.

[0167] Evaluation Example 2: Evaluation of span value and BET specific surface area (confirmation of uniformity) The span values ​​of the positive electrode active materials were measured according to the example and comparative examples. Specifically, the D values ​​of each positive electrode active material corresponding to 10%, 50%, and 90% of its cumulative volume of particle size distribution were measured. 10 D 50 and D 90, to calculate {(D 90 -D 10 ) / D 50 The value is obtained as the span value. The results are shown in Table 2 below.

[0168] In addition, the BET specific surface area of ​​the positive electrode active materials prepared in the example and comparative examples was measured using a BET analyzer, and the results are shown in Table 2. The BET specific surface area was measured using a MOUNTECH HMmodel-1208 specific surface area measuring device via nitrogen adsorption. Specifically, approximately 0.3 g of the positive electrode active material was heated at 300°C for 1 hour in a pre-processor under a nitrogen atmosphere, then further pre-treated at 300°C for 15 minutes in the surface area measuring device, cooled to liquid nitrogen temperature, and saturated with a gas containing 30% nitrogen and 70% He. The amount of desorbed gas was then measured by heating to room temperature, and the specific surface area was calculated using the conventional BET method from the obtained results.

[0169] Evaluation Example 3: Surface Residual Lithium The residual lithium content on the surface of the positive electrode active materials prepared in the example and comparative examples was measured by HCl titration. The results are shown in Table 2 below. Specifically, 10 g of the positive electrode active material was placed in 100 ml of distilled water and stirred at 300 rpm for 30 minutes, and the pH change was measured while HCl was added. Because the unreacted residual lithium on the surface of the positive electrode active material exists in the form of Li₂CO₃, LiOH, etc., the residual lithium content on the surface of the positive electrode active material was measured by CO₃²⁻ titration. 2- OH - Ions react with the H+ in HCl to undergo titration. The amount of HCl solution injected is calculated to determine the unreacted residual lithium content. In Table 2, Li2CO3 and LiOH represent the amount based on 100 wt% of the positive electrode active material, and the total residual lithium (free Li) is expressed in ppm, which represents the content relative to 100 wt% of the positive electrode active material and indicates a 10... -4 wt%.

[0170] Table 2

[0171] When using large-particle precursors, a significant amount of residual lithium on the surface can be a problem. However, based on a total of 100 wt% lithium-nickel composite oxides, the amount of residual lithium on the surface in the example was confirmed to be less than or equal to 1500 ppm, the amount of LiOH less than or equal to 0.29 wt%, and the amount of Li₂CO₃ less than or equal to 0.4 wt%. Therefore, it can be seen that even when using large-particle precursors to prepare the positive electrode active material, the residual lithium on the surface is significantly reduced.

[0172] Furthermore, it was confirmed that the positive electrode active material of the example exhibited a range of values ​​and BET specific surface area within a specific range. Therefore, it can be seen that the particle size has grown uniformly.

[0173] Evaluation Example 4: Evaluation of Initial Charge / Discharge Efficiency and Cycle Life Characteristics The initial charge / discharge capacity and efficiency of the rechargeable lithium-ion battery cells manufactured in the evaluation and comparative examples are shown.

[0174] The rechargeable lithium-ion battery cells manufactured in the example and comparative examples were charged at 25°C with a constant current of 0.2C to an upper limit voltage of 4.3V and a constant voltage of 0.05C. The rechargeable lithium-ion battery cells manufactured in the example and comparative examples were then discharged at 0.2C to a termination voltage of 3.0V for initial charge-discharge. Table 3 shows the efficiency calculated using the initial charge capacity, initial discharge capacity, and the ratio of initial discharge capacity to initial charge capacity.

[0175] Subsequently, 50 cycles of charging and discharging at 1.0C were repeated at 45°C within a voltage range of 3.0V to 4.3V. The ratio of the discharge capacity after 50 charge-discharge cycles to the initial discharge capacity was calculated and presented as the cycle life in Table 3.

[0176] Table 3

[0177] Referring to Table 3, it can be seen that, compared with the rechargeable lithium battery cells manufactured in the comparative example, the rechargeable lithium battery cells manufactured in the example exhibit significantly superior initial discharge capacity, initial charge / discharge efficiency, and cycle life characteristics.

[0178] While this disclosure has been described in conjunction with exemplary embodiments now considered practical, it will be understood that the disclosure is not limited to the disclosed embodiments. Rather, the disclosure includes various modifications and equivalent arrangements.

Claims

1. A positive electrode active material, said positive electrode active material comprising: The core particles each comprise a zirconium-containing lithium-nickel composite oxide, and based on 100 mol% of total metals other than lithium in the zirconium-containing lithium-nickel composite oxide, each core particle has a nickel content of greater than or equal to 60 mol%. as well as A coating, applied to the surface of each of the core particles, comprises cobalt and phosphorus. The positive electrode active material has a density of 0.7m. 2 / g to 0.9m 2 The BET specific surface area is / g, and the positive electrode active material is in the form of single particles.

2. The positive electrode active material according to claim 1, wherein, The positive electrode active material has a range of values ​​from 1.1 to 1.3 according to the following equation: Span = (D 90 -D 10 ) / D 50 Among them, D 10 D is the particle size of particles that accumulate to 10% by volume in the particle size distribution of the positive electrode active material. 50 It is the particle size of particles that constitute 50% of the cumulative volume in the particle size distribution, and D 90 It is the particle size of particles that constitute 90% of the cumulative volume in the particle size distribution.

3. The positive electrode active material according to claim 1, wherein, The average particle size D of the positive electrode active material 50 The range is from 1μm to 4μm.

4. The positive electrode active material according to claim 1, wherein, Based on 100 wt% of the zirconium-containing lithium-nickel composite oxide, the zirconium content is from 0.1 wt% to 0.4 wt%.

5. The positive electrode active material according to claim 1, wherein, The zirconium-containing lithium-nickel composite oxide is represented by the following formula: He a1 We x1 M 1 y1 Zr z1 Oh 2-b1 X b1 Where, 0.9≤a1≤1.2, 0.6≤x1≤0.991, 0≤y1≤0.5, 0.001≤z1≤0.003, 0.9≤x1+y1+z1≤1.1, and 0≤b1≤0.1, M 1 X is one or more of Al, B, Ba, Ca, Ce, Co, Cr, Cu, Fe, Mg, Mn, Mo, Nb, Si, Sn, Sr, Ti, V, W, Y, and Zn, and X is one or more of F, P, and S.

6. The positive electrode active material according to claim 1, wherein, Based on 100 mol% of total metals other than lithium in the positive electrode active material, the amount of cobalt in the coating is from 0.1 mol% to 5.0 mol%.

7. The positive electrode active material according to claim 1, wherein, Based on 100 mol% of total metals other than lithium in the positive electrode active material, the amount of phosphorus in the coating is from 0.1 mol% to 1.0 mol%.

8. A method for preparing a positive electrode active material, the method comprising the following steps: (i) A zirconium and nickel raw materials are mixed and subjected to a co-precipitation reaction to prepare a zirconium-containing nickel composite hydroxide; (ii) subjecting the zirconium-containing nickel composite hydroxide to a first heat treatment to prepare a zirconium-containing nickel composite oxide; (iii) The zirconium-containing nickel composite oxide and lithium raw material are mixed and subjected to a second heat treatment to prepare a zirconium-containing lithium nickel composite oxide in the form of secondary particles, wherein the secondary particles are aggregates of primary particles. (iv) Crush the zirconium-containing lithium-nickel composite oxide to obtain an initial positive electrode active material in the form of single particles; as well as (v) The initial positive electrode active material, cobalt raw material and phosphorus raw material are mixed, subjected to a third heat treatment, and the mixture is disintegrated after the third heat treatment.

9. The method according to claim 8, wherein, The first heat treatment is performed at a temperature between 250°C and 500°C, and The first heat treatment is carried out for 1 to 10 hours in an oxygen atmosphere or an air atmosphere.

10. The method according to claim 8, wherein, The zirconium-containing nickel composite oxide is represented by the following formula: There is no x11 M 11 y11 Zr z11 O2 wherein 0.6≤x11≤1, 0≤y11<0.4, 0<z11≤0.3, and 0.9≤x11+y11+z11≤1.1, and M 11 is one or more elements selected from the group consisting of Al, B, Ba, Ca, Ce, Co, Cr, Cu, Fe, Mg, Mn, Mo, Nb, Si, Sn, Sr, Ti, V, W, Y, and Zn.

11. The method according to claim 8, wherein, The zirconium-containing nickel composite oxide is in particulate form and has an average particle size D of 9 μm to 16 μm. 50 .

12. The method according to claim 8, wherein, The second heat treatment is carried out at a temperature of 600°C to 900°C, and The second heat treatment is carried out for 4 to 16 hours.

13. The method according to claim 8, wherein, No alkaline grain growth promoter is added during the second heat treatment process of the zirconium-containing nickel composite oxide and the lithium raw material.

14. The method according to claim 8, wherein, The average particle size D of the secondary particles 50 The thickness is 10μm to 20μm, and Wherein, the average particle size D of the primary particles forming the secondary particles 50 The range is from 1μm to 4μm.

15. The method according to claim 8, wherein, The material is pulverized using jet milling equipment, and The sieve wheel of the jet mill rotates at a speed of 1500 rpm to 2000 rpm, the blower rotates at a speed of 2500 rpm to 3500 rpm, and the pulse pressure is 0.25 bar to 0.75 bar.

16. The method according to claim 8, wherein, The average particle size D of the initial positive electrode active material in single-particle form 50 The range is from 1μm to 4μm.

17. The method according to claim 8, wherein, Based on 100 wt% of the initial positive electrode active material in single-particle form, the zirconium content is from 0.1 wt% to 0.4 wt%.

18. The method according to claim 8, wherein, Based on the total metal content (excluding lithium) of 100 mol% in the positive electrode active material, the amount of cobalt in the cobalt raw material is from 0.1 mol% to 5.0 mol%. Wherein, based on the total metal content of 100 mol% excluding lithium in the positive electrode active material, the amount of phosphorus in the phosphorus raw material is 0.1 mol% to 1.0 mol%.

19. The method according to claim 8, wherein, The third heat treatment is carried out at a temperature of 500°C to 900°C, and The third heat treatment is carried out for 5 to 20 hours.

20. A rechargeable lithium battery, said rechargeable lithium battery comprising: A positive electrode includes a current collector and a positive electrode active material layer, the positive electrode active material layer being disposed on the current collector and including the positive electrode active material according to any one of claims 1 to 7; negative electrode; and Electrolytes.