Fluorinated metal composite silicon-carbon material, and preparation method and application thereof

By introducing nitrogen doping and fluorinated metal layers into porous carbon materials, the structural collapse and SEI film rupture problems caused by volume changes in silicon-carbon anode materials in lithium batteries were solved, improving the cycle life and first coulombic efficiency of the battery and achieving higher battery performance stability.

CN123162157APending Publication Date: 2026-11-24JIANGXI JIANGTONG SIYING NEW ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611025403.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-10
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

In existing lithium batteries, silicon-carbon anode materials suffer from structural collapse and SEI film rupture due to volume changes during charge and discharge, leading to a decline in battery performance. Furthermore, pre-lithiation and surface coating present interfacial bonding issues, affecting the battery's cycle life and initial coulombic efficiency.

Method used

By introducing oxyacid metal salts into porous carbon materials and performing high-temperature nitriding to form a nitrogen-doped composite carbon framework, and forming a fluorinated metal layer on the surface of the silicon-carbon precursor, combined with the uniform distribution of nano-silicon and lithium particles, a stable lithium fluoride film is formed, which improves the interfacial bonding force and electrolyte stability.

Benefits of technology

It effectively inhibits electrolyte decomposition, improves the uniformity and interface stability of active silicon, enhances the first coulombic efficiency and long cycle life of the battery, and strengthens the structural stability and safety of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123162157A_ABST
    Figure CN123162157A_ABST
Patent Text Reader

Abstract

This invention provides a fluorinated metal composite silicon-carbon material, its preparation method, and its application, relating to the field of silicon-carbon material technology. The preparation method includes mixing porous carbon in an oxyacid metal salt solution and evaporating it to obtain a composite precursor; subjecting the composite precursor to high-temperature nitriding to obtain a composite carbon material; vacuum drying the composite carbon material in a composite solution containing dissolved lithium salt and organosilicon to obtain a composite intermediate; subjecting the composite intermediate to high-temperature reduction in a reducing atmosphere to obtain a silicon-carbon precursor; mixing the silicon-carbon precursor in a metal salt solution and desolvating it to obtain a silicon-carbon intermediate; and mixing the silicon-carbon intermediate with a fluorinating agent followed by high-temperature treatment to obtain the fluorinated metal composite silicon-carbon material. This invention can effectively suppress electrolyte decomposition during cycling, improve the uniformity and interfacial stability of active silicon, and significantly improve the initial coulombic efficiency and cycle life of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of silicon-carbon materials technology, and in particular to a fluorinated metal composite silicon-carbon material, its preparation method, and its application. Background Technology

[0002] Lithium-ion batteries, as one of the most promising clean energy storage devices, are widely used in portable electronic devices such as smartphones and laptops, and have broad prospects in emerging fields such as new energy vehicles and grid energy storage. As the application scenarios of lithium-ion batteries continue to expand, higher requirements are being placed on their energy density, cycle life, and fast-charging performance. Currently, graphite is commonly used as the negative electrode material in lithium-ion batteries, but the relatively low theoretical specific capacity of graphite greatly restricts the development of high-energy-density batteries. Therefore, silicon, with its higher theoretical specific capacity and lower lithium insertion / extraction potential, is considered to have the potential to become a high-density negative electrode material. However, elemental silicon undergoes drastic volume changes during charging and discharging. The enormous mechanical stress generated by these volume changes leads to silicon pulverization, electrode structure collapse, and the continuous rupture and formation of the surface SEI film, ultimately resulting in a sharp decline in lithium-ion battery performance.

[0003] Currently, to address the issues of expansion and poor conductivity in silicon anodes, research focuses primarily on the microstructure design and surface interface control of silicon-carbon materials. On one hand, porous carbon supports with high specific surface area and abundant pores are developed. Highly dispersed elemental silicon is introduced into these supports using methods such as chemical vapor deposition or liquid-phase wetting reduction. The pores of the support accommodate the volume expansion of silicon, achieving spatial confinement. On the other hand, coating the outer surface of silicon-carbon materials prevents direct contact between the electrolyte and the internal active silicon. For example, an amorphous carbon layer can be coated onto the outer surface of the silicon-carbon material. Furthermore, pre-lithiation of silicon-carbon materials can be performed to embed an appropriate amount of active lithium into the silicon-carbon anode in advance. This compensates for the irreversible lithium loss during the first charge-discharge cycle due to the formation of the SEI film, thus improving the electrochemical performance of the silicon-carbon material.

[0004] While porous carbon with its high surface area provides excellent space for the volume expansion of silicon, it also leads to extensive contact between the electrolyte and the silicon-carbon material. This can result in large-area electrolyte decomposition, reducing the initial coulombic efficiency. Furthermore, pre-lithiation of the silicon-carbon material can easily cause localized overreactions, reducing the uniformity of lithium distribution. Coating the outer surface of the silicon-carbon material can also lead to interfacial bonding problems, potentially causing interface separation between the silicon-carbon material and the outer coating layer during long-term cycling. This can result in coating layer breakage, exposing the active components within the silicon-carbon material, triggering continuous rupture and growth of the SEI film, and causing a sharp decline in battery performance after long-term cycling. Therefore, there is an urgent need to provide a solution to address these issues. Summary of the Invention

[0005] The purpose of this invention is to provide a fluorinated metal composite silicon-carbon material, its preparation method and application, which can effectively suppress electrolyte decomposition during cycling, improve the uniformity and interface stability of active silicon, and significantly improve the first coulombic efficiency and long cycle life of the battery.

[0006] In a first aspect, the present invention provides a method for preparing a fluorinated metal composite silicon-carbon material, comprising: mixing porous carbon in an oxyacid metal salt solution and evaporating it to obtain a composite precursor; subjecting the composite precursor to high-temperature nitriding to obtain a composite carbon material; vacuum drying the composite carbon material in a composite solution containing dissolved lithium salt and organosilicon to obtain a composite intermediate; subjecting the composite intermediate to high-temperature reduction in a reducing atmosphere to obtain a silicon-carbon precursor; mixing the silicon-carbon precursor in a metal salt solution and desolvating it to obtain a silicon-carbon intermediate; and mixing the silicon-carbon intermediate with a fluorinating agent and then treating it at high temperature to obtain a fluorinated metal composite silicon-carbon material.

[0007] Optionally, the specific surface area of ​​the porous carbon is 1500 m². 2 / g-2500m 2 / g.

[0008] Optionally, the porous carbon has a particle size of 1 μm-50 μm.

[0009] Optionally, the oxyacid metal salt dissolved in the oxyacid metal salt solution includes one of metal sulfate and metal nitrate.

[0010] Optionally, the metal ions in the oxyacid metal salt solution include one of aluminum ions, titanium ions, and magnesium ions.

[0011] Optionally, the mass ratio of porous carbon to metal ions in the oxyacid metal salt solution is 1:(0.01-0.1).

[0012] Optionally, the oxyacid metal salt solution also contains a dispersant.

[0013] Optionally, the dispersant includes polyvinylpyrrolidone.

[0014] Optionally, the mass ratio of the porous carbon to the dispersant is 1:(0.05-0.2).

[0015] Alternatively, porous carbon can be mechanically mixed with an oxyacid metal salt solution.

[0016] Optionally, the mechanical mixing includes ultrasound, stirring, and oscillation.

[0017] Optionally, the mixture is evaporated at 50℃-80℃ to obtain the composite precursor.

[0018] Optionally, the composite precursor is nitrided at high temperature of 700℃-1100℃.

[0019] Optionally, the composite precursor is nitrided at high temperature in a nitrogen-containing atmosphere.

[0020] Optionally, the nitrogen-containing atmosphere includes either a nitrogen atmosphere or an ammonia atmosphere.

[0021] Optionally, high-temperature nitriding is performed in a nitrogen-containing atmosphere of 0.5 kPa to 2 kPa.

[0022] Optionally, the composite precursor is nitrided at high temperature for 60-180 minutes.

[0023] Optionally, high-temperature nitriding followed by cooling yields a composite carbon material.

[0024] Optionally, the lithium salt includes one of lithium carbonate, lithium hydroxide, lithium tetrafluoroborate, and organolithium.

[0025] Optionally, the organic lithium includes one of lithium acetate and lithium tert-butoxide.

[0026] Optionally, the organosilicon includes one of tetraethyl orthosilicate and alkyl orthosilicate.

[0027] Optionally, the mass ratio of the composite carbon material to the lithium element in the lithium salt is 1:(0.01-0.05).

[0028] Optionally, the mass ratio of the composite carbon material to the silicon in the organosilicon is 1:(0.5-1).

[0029] Optionally, the composite carbon material is impregnated in a composite solution under reduced pressure and then dried.

[0030] Optionally, it can be immersed at 60kPa-80kPa.

[0031] Optionally, soak for 60-120 minutes.

[0032] Optionally, it can be impregnated in a composite solution at 40℃-60℃.

[0033] Optionally, vacuum drying can be performed at 80℃-100℃.

[0034] Optionally, drying can be performed at 1 kPa-50 kPa.

[0035] Optionally, the reducing atmosphere includes a reducing gas and an inert carrier gas.

[0036] Optionally, the reducing gas includes hydrogen.

[0037] Optionally, the concentration of the reducing gas is 5 vol%-15 vol%.

[0038] Optionally, the inert carrier gas includes one of argon, helium, and nitrogen.

[0039] Optionally, reduction can be performed in a reducing atmosphere of 0.5 kPa to 2 kPa.

[0040] Optionally, the material can be reduced at high temperature in a reducing atmosphere for 2-5 hours.

[0041] Optionally, reduction can be carried out in a reducing atmosphere at 800℃-1300℃.

[0042] Optionally, the silicon-carbon precursor is obtained by high-temperature reduction followed by cooling.

[0043] Optionally, the metal salt dissolved in the metal salt solution includes one of metal chloride, metal sulfate, and metal nitrate.

[0044] Optionally, the metal ions in the metal salt solution include one of cobalt ions, magnesium ions, and silver ions.

[0045] Optionally, the mass ratio of the silicon carbide precursor to the metal ions in the metal salt solution is 1:(0.05-0.2).

[0046] Optionally, the mixture is spray-dried to obtain a silicon-carbon intermediate.

[0047] Optionally, the metal salt solution may also contain a silane activator.

[0048] Optionally, the silane activator includes one of KH550 and KH560.

[0049] Optionally, the mass ratio of the silicon carbide precursor to the silane activator is 1:(0.05-0.08).

[0050] Optionally, the surface of the silicon-carbon precursor is pretreated with a short-term oxygen plasma.

[0051] Optionally, the surface of the silicon-carbon precursor is subjected to short-term oxygen plasma treatment in an activating gas.

[0052] Optionally, the activating gas includes one of air, oxygen, and water vapor.

[0053] Optionally, the absolute pressure of the activating gas is 10 Pa to 200 Pa.

[0054] Optionally, the plasma source for oxygen plasma treatment includes one of microwave plasma, radio frequency plasma, and DC plasma.

[0055] Optionally, the power for oxygen plasma treatment is 100W-200W.

[0056] Optionally, the surface of the silicon-carbon precursor is subjected to oxygen plasma treatment for 30s-90s.

[0057] Optionally, the silicon-carbon precursor is mixed in a metal salt solution containing a dissolved transition carbon source and then desolvated to obtain a silicon-carbon intermediate.

[0058] Optionally, the transition carbon source includes one of citric acid and glucose.

[0059] Optionally, the mass ratio of the silicon-carbon precursor to the transition carbon source is 1:(0.05-0.15).

[0060] Optionally, the fluorinating agent includes one of ammonium fluoride and ammonium bifluoride.

[0061] Optionally, the mass ratio of the silicon-carbon intermediate to the fluorinating agent is 1:(0.01-0.2).

[0062] Optionally, the silicon-carbon intermediate is mixed with the fluorinating agent in a solvent environment and then desolventized.

[0063] Optionally, fluorinated metal composite silicon-carbon materials are obtained by high-temperature treatment at 200℃-400℃.

[0064] Optionally, fluorinated metal composite silicon-carbon materials can be obtained by high-temperature treatment for 60-120 minutes.

[0065] Optionally, fluorinated metal composite silicon-carbon materials are obtained by high-temperature treatment in a protective atmosphere.

[0066] Optionally, the high-temperature treatment is carried out in a protective atmosphere of 0.1 MPa-1 MPa.

[0067] Optionally, the fluorinated metal composite silicon-carbon material is obtained by cooling after high-temperature treatment.

[0068] Secondly, the present invention also provides a fluorinated metal composite silicon-carbon material prepared by any of the above-mentioned optional preparation methods, comprising a silicon-carbon skeleton and a fluorinated metal layer formed on the surface of the silicon-carbon skeleton, wherein the silicon-carbon skeleton comprises a porous carbon skeleton and composite silicon within its pores, the porous carbon skeleton is doped with nitrogen, and the composite silicon comprises a silicon skeleton bonded to the inner wall of the porous carbon pores and a metal composite and lithium nanoparticles doped within the silicon skeleton, wherein the metal composite is formed by in-situ decomposition of an oxyacid metal salt at high temperature and subsequent nitriding.

[0069] Thirdly, the present invention also provides an application of the fluorinated metal composite silicon-carbon material prepared by any of the above-mentioned optional preparation methods.

[0070] Optionally, the application includes a secondary battery.

[0071] The fluorinated metal composite silicon-carbon material provided by this invention has at least one of the following beneficial technical effects compared with the prior art: 1. By uniformly infiltrating oxyacid metal salts into the pores of porous carbon and then performing high-temperature nitriding, not only can nitrogen doping be applied to the porous carbon framework to improve the intrinsic electronic conductivity and lithium-ion transport efficiency of the porous carbon matrix, but the oxyacid metal salts can also be decomposed in situ into metal complexes, which helps to improve the structural stability of the porous carbon matrix and enhance its buffering capacity against volume expansion. Then, organosilicon and lithium salts are impregnated into the pores of the composite carbon material and reduced in situ at high temperature to generate nano-silicon and lithium nanoparticles, which helps to improve the dispersion uniformity of nano-silicon and lithium nanoparticles in the silicon-carbon framework. 2. By mixing and desolventizing the silicon-carbon precursor in a metal salt solution, the metal salt can be coated onto the surface of the silicon-carbon precursor. After mixing with a fluorinating agent, the metal salt on the surface of the silicon-carbon precursor is converted into metal fluoride under high temperature. This helps to form a dense fluorinated metal-based SEI film on the surface of the silicon-carbon material, which can effectively inhibit the continuous decomposition of the electrolyte and irreversible lithium loss during long-term cycling. At the same time, in-situ fluorination helps to improve the interfacial bonding force between the surface fluorinated metal layer and the silicon-carbon precursor skeleton, which can prevent the silicon-carbon material from peeling and breaking during long-term cycling, effectively improving the cycle life and safety of the silicon-carbon material. Attached Figure Description

[0072] Figure 1 The present invention provides a flowchart of a method for preparing a fluorinated metal composite silicon-carbon material. Detailed Implementation

[0073] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. Unless otherwise defined, the technical or scientific terms used herein should have the ordinary meaning understood by those skilled in the art to which this invention pertains.

[0074] See Figure 1 This invention provides a method for preparing a fluorinated metal composite silicon-carbon material, comprising the following steps: S1. Porous carbon is mixed in an oxyacid metal salt solution and evaporated to dryness to obtain a composite precursor; S2. High-temperature nitriding of the composite precursor yields a composite carbon material. S3. The composite carbon material is vacuum dried in a composite solution containing dissolved lithium salt and organosilicon to obtain a composite intermediate. S4. The composite intermediate is subjected to high-temperature reduction in a reducing atmosphere to obtain a silicon-carbon precursor. S5. Mix the silicon-carbon precursor with a metal salt solution and remove the solvent to obtain the silicon-carbon intermediate; S6. After mixing the silicon-carbon intermediate with the fluorinating agent, the mixture is subjected to high temperature treatment to obtain a fluorinated metal composite silicon-carbon material.

[0075] In fact, by infiltrating the oxoacid metal salt into the pores of porous carbon in step S1 and performing high-temperature nitriding in step S2, this invention not only enables nitrogen doping in porous carbon to improve the intrinsic electronic conductivity of the carbon framework, but also transforms the oxoacid metal salt into a metal composite, forming a high-strength metal support framework in the pores of porous carbon. This helps improve the overall support stability of the porous carbon framework, disperses stress during charge-discharge cycles, and effectively suppresses the collapse of the silicon-carbon structure and material pulverization caused by volume expansion during lithium insertion / extraction of active silicon. This helps improve the rate performance and long-cycle structural stability of silicon-carbon materials.

[0076] Furthermore, in step S3, the composite carbon material is vacuum dried in a composite solution. The negative pressure environment helps the lithium salt and organosilicon fully penetrate into the pores of the composite carbon material. In step S4, the organosilicon and lithium salt are pyrolyzed in situ during high-temperature treatment in a reducing atmosphere. Under the confinement effect of the pores of the composite carbon material, nanoscale active silicon and lithium particles are directionally grown in the pores, which effectively improves the stability of active silicon in the carbon skeleton. As a result, the stress generated by the volume expansion of active silicon during charging and discharging can be fully absorbed by the carbon skeleton, avoiding the deterioration of the cycle performance of silicon-carbon material caused by the peeling of active silicon. At the same time, during the first charge and discharge, the lithium particles can effectively replenish the irreversible lithium loss caused by the formation of the SEI film, which can improve the first coulombic efficiency of silicon-carbon material.

[0077] Furthermore, by mixing and desolventizing the silicon-carbon precursor in a metal salt solution in step S5, this invention enables the metal salt to uniformly coat the surface of the silicon-carbon precursor. Then, in step S6, mixing and high-temperature treatment with a fluorinating agent allows the metal salt on the surface of the silicon-carbon precursor to form a fluorinated metal layer through an in-situ fluorination reaction, effectively improving the interfacial bonding stability between the external fluorinated metal layer and the internal silicon-carbon precursor. Moreover, during battery cycling, the fluorinated metal layer can construct a stable, lithium-fluoride-rich SEI film in situ at the electrode interface. The high mechanical strength and good ion conductivity of lithium fluoride rigidly bind the amorphous silicon, suppressing the volume expansion of silicon during lithium insertion / extraction, thus preventing silicon particles from pulverizing and falling off. Furthermore, the lithium-fluoride-rich SEI film has strong interfacial stability, blocking contact between the electrolyte and the active material, thereby reducing interfacial side reactions and irreversible lithium consumption, effectively improving the long-cycle stability of the electrode material.

[0078] In some embodiments, the porous carbon used in step S1 has a specific surface area of ​​1500 m². 2 / g-2500m 2 / g. In fact, using porous carbon with a high specific surface area can provide more adsorption sites and a uniform liquid-phase wetting interface, which can effectively alleviate the mechanical stress caused by volume expansion during lithium insertion / extraction of active silicon. It can also improve the adsorption uniformity and loading of oxyacid metal salts, lithium salts and organosilicon. At the same time, the carbon framework in porous carbon forms an ion transport network, which helps to shorten the lithium-ion diffusion path and reduce charge transfer resistance. In addition, uniform pre-lithiation in the pores of porous carbon helps to improve the problem of reduced initial coulombic efficiency caused by the excessive specific surface area of ​​porous carbon during electrolyte wetting, effectively improving the initial coulombic efficiency and cycle stability of silicon-carbon materials.

[0079] In some embodiments, the porous carbon used in step S1 has a particle size of 1 μm-50 μm. In fact, using micron-sized porous carbon can effectively shorten the long-range diffusion paths of lithium ions and electrons within silicon-carbon materials, helping to reduce the charge transfer impedance and solid-phase diffusion impedance of silicon-carbon materials, thereby improving their rate performance. Furthermore, when silicon-carbon materials are mixed with binders and conductive agents to form an active slurry, micron-sized porous carbon (silicon-carbon material) can suppress its agglomeration and sedimentation in the active slurry, while simultaneously increasing the compaction density of the electrode and thus improving the volumetric energy density of the lithium-ion battery.

[0080] In some embodiments, the porous carbon used in step S1 can be spherical porous carbon, which helps to uniformly coat the surface of the spherical porous carbon with a fluorinated metal layer. Specifically, the porous carbon used can be a commercially available conventional product, such as a porous carbon framework purchased from Jinbo Carbon Co., Ltd., with grades KBC / PC-1, KBC / PC-2, and KBC / PC-3. Alternatively, it can be prepared using porous carbon preparation methods commonly used in the art, such as spray drying a phenolic resin solution followed by high-temperature carbonization, and then activation and pore formation in an active atmosphere to obtain spherical porous carbon.

[0081] In some embodiments, the oxyacid metal salt dissolved in the oxygen-containing metal salt solution used in step S1 includes one of metal sulfate and metal nitrate. In fact, when the oxyacid metal salt is dispersed in the pores of porous carbon, it undergoes thermal decomposition during high-temperature nitriding to produce metal oxides and gaseous byproducts, such as sulfur oxides and nitrogen oxides. This improves the bonding stability between the metal oxides and the porous carbon framework. Simultaneously, the generated gaseous byproducts can also act as an endogenous heteroelement doping source in a high-temperature environment, synergistically working with the external nitrogen-containing atmosphere to dope the porous carbon framework with heteroelements.

[0082] In some embodiments, the metal ions in the oxygen-containing metal salt solution used in step S1 include one of aluminum ions, titanium ions, and magnesium ions. In practice, after the oxygen-containing metal salt decomposes at high temperature to form metal oxides, it is then transformed into a metal composite in a high-temperature nitrogen-containing atmosphere, thereby improving the bonding stability with the porous carbon framework. This strengthens the mechanical strength of the composite carbon material framework, which is beneficial for improving the structural stability of the carbon framework during cycling and avoiding structural collapse and pulverization due to silicon volume expansion. Furthermore, aluminum-based metal composites, titanium-based metal composites, and magnesium-based metal composites exhibit high electrochemical stability.

[0083] In some embodiments, the mass ratio of porous carbon to metal ions in the oxyacid metal salt solution used in step S1 is 1:(0.01-0.1). In practice, adjusting the mass ratio of porous carbon to metal ions helps to adjust the loading of the metal composite in the porous carbon. This allows the metal composite to improve the structural stability of the porous carbon framework while avoiding excessive metal composite blocking the pores of the porous carbon and affecting the loading of active silicon. Specifically, the solvent used in the oxyacid metal salt solution includes deionized water and solvents commonly used in the art, necessary to fully dissolve the oxyacid metal salt without causing side reactions.

[0084] Furthermore, the mass ratio of porous carbon to metal ions in the oxyacid metal salt solution can also be any sub-interval within the range of 1:(0.01-0.1), such as 1:(0.01-0.03), 1:(0.02-0.04), 1:(0.03-0.05), 1:(0.04-0.06), 1:(0.05-0.07), 1:(0.06-0.08), 1:(0.07-0.09), 1:(0.08-0.1), etc. It can also be any specific ratio within the range of 1:(0.01-0.1), such as 1:0.01, 1:0.03, 1:0.05, 1:0.07, 1:0.09, 1:0.1, etc., and is not limited to the values ​​listed above. Values ​​and ranges not listed within the range of 1:(0.01-0.1) can all achieve the purpose of this invention.

[0085] In some embodiments, a dispersant is also dissolved in the oxyacid metal salt solution used in step S1. In fact, after adding porous carbon to the oxyacid metal salt solution, the dispersant can improve the dispersion uniformity of the porous carbon in the oxyacid metal salt solution, and at the same time help the oxyacid metal solution to fully wet the interior of the porous carbon pores. Furthermore, during the desolventizing process, the dispersant can inhibit the migration of the oxyacid metal salt during crystallization, effectively improving the bonding stability and uniformity of the oxyacid metal salt with the inner wall of the porous carbon pores during desolventizing.

[0086] In some embodiments, the dispersant used in step S1 includes polyvinylpyrrolidone (PVP). In fact, in the oxyacid metal salt solution, PPVP binds to metal ions through complexation and electrostatic adsorption, leading to the continuous precipitation of the oxyacid metal salt during desolvation. PPVP, through steric hindrance, prevents the oxyacid metal salt crystals from migrating onto the inner walls of the porous carbon pores, thus improving the uniformity of dispersion of the oxyacid metal salt in the porous carbon pores. Furthermore, during high-temperature nitriding, PPVP can pyrolyze to form amorphous carbon that bonds with the porous carbon framework, further enhancing the interfacial bonding strength between the metal composite and the porous carbon framework.

[0087] Furthermore, in step S1, the mass ratio of porous carbon to dispersant can be 1:(0.05-0.2). In practice, when the dispersant is dissolved in the oxyacid metal salt solution and during desolventizing, the dispersant remains in the oxyacid metal salt crystal layer within the pores of the porous carbon. Therefore, by adjusting the mass ratio of porous carbon to dispersant, the loading amount of the amorphous carbon framework formed by the thermal decomposition of the dispersant in the porous carbon framework can be adjusted. This avoids excessive amorphous carbon causing over-crowding of the porous carbon pores, making it difficult to subsequently load organosilicon and lithium salts. Simultaneously, it avoids insufficient amorphous carbon, which would prevent the dispersion uniformity of the metal composite from being improved.

[0088] Furthermore, the mass ratio of porous carbon to dispersant can be any sub-interval within the range of 1:(0.05-0.2), such as 1:(0.05-0.08), 1:(0.07-0.1), 1:(0.9-0.12), 1:(0.11-0.14), 1:(0.13-0.16), 1:(0.15-0.18), 1:(0.17-0.2), etc. It can also be any specific ratio within the range of 1:(0.05-0.2), such as 1:0.05, 1:0.08, 1:0.11, 1:0.14, 1:0.17, 1:0.2, etc., and is not limited to the values ​​listed above. Values ​​and ranges not listed within the range of 1:(0.05-0.2) can all achieve the purpose of this invention.

[0089] In some embodiments, in step S1, porous carbon can be mechanically mixed with an oxyacid metal salt solution and then evaporated to dryness at 50°C-80°C to obtain the composite precursor. Mechanical action helps improve the dispersion uniformity of porous carbon in the oxyacid metal salt solution, preventing agglomeration and sedimentation. Furthermore, solvent removal can also be performed under mechanical mixing, thereby improving the uniformity of the oxyacid metal salt precipitation process. In practice, the mechanical mixing employed includes one of ultrasound, stirring, or oscillation. For example, ultrasonic mixing can utilize the ultrasonic cavitation effect to remove air bubbles adhering to the pores of the porous carbon, thereby effectively improving the wetting uniformity.

[0090] In some embodiments, in step S2, the composite precursor can be subjected to high-temperature nitriding in a nitrogen-containing atmosphere at 0.5 kPa-2 kPa and 700°C-1100°C for 60 min-180 min, followed by cooling to obtain a composite carbon material. The nitrogen-containing atmosphere used includes either a nitrogen atmosphere or an ammonia atmosphere. In fact, heat treatment in a low-pressure, high-temperature environment can decompose the oxyacid metal salts on the surface and within the pores of the composite precursor into metal composites in situ, and nitrogen doping of the porous carbon framework can improve intrinsic electronic conductivity and lithium-ion transport efficiency.

[0091] In some embodiments, the lithium salt used in step S3 includes one of lithium carbonate, lithium hydroxide, lithium tetrafluoroborate, and organolithium, and the organosilicon used includes one of tetraethyl orthosilicate and alkyl orthosilicate; specifically, the organolithium used includes one of lithium acetate and lithium tert-butoxide. In practice, when the lithium salt and organolithium are impregnated and dispersed within the pores of the composite carbon material, the organosilicon decomposes in situ after heat treatment and is carbothermally reduced to nano-silicon, while the lithium salt is carbothermally reduced to lithium nanoparticles.

[0092] In some embodiments, the mass ratio of the composite carbon material to lithium in the composite solution and silicon in the organosilicon in step S3 is 1:(0.01-0.05):(0.5-1). Furthermore, the composite carbon material can be dispersed in a composite solution at 40℃-60℃, and then impregnated under reduced pressure at 60kPa-80kPa for 60min-120min, followed by drying and solvent removal at 80℃-100℃ and 1kPa-50kPa. In fact, impregnation under reduced pressure helps the composite solution to fully penetrate the interior of the composite carbon material, thereby promoting uniform dispersion of lithium salt and organosilicon in the pores and surface of the composite carbon material.

[0093] In some embodiments, the reducing atmosphere used in step S4 includes a reducing gas and an inert carrier gas. Specifically, the reducing gas used includes hydrogen, and the concentration of the reducing gas in the reducing atmosphere is 5 vol%-15 vol%. The inert carrier gas used includes one of argon, helium, and nitrogen. Further, the composite intermediate can be reduced in a reducing atmosphere of 800℃-1300℃ and 0.5 kPa-2 kPa for 2 h-5 h and then cooled to obtain a silicon-carbon precursor.

[0094] In some embodiments, the metal salt dissolved in the metal salt solution in step S5 includes one of metal chloride, metal sulfate, and metal nitrate. Specifically, the metal ions in the metal salt solution include one of cobalt ions, magnesium ions, and silver ions, and the mass ratio of the silicon carbide precursor to the metal ions in the metal salt solution is 1:(0.05-0.2).

[0095] In some embodiments, after mixing the silicon-carbon precursor with the metal salt solution in step S5, the silicon-carbon intermediate can be obtained by spray drying to remove the solvent. In fact, spray drying helps the metal salt to be uniformly distributed on the surface of the silicon-carbon precursor. Furthermore, a silane activator is also dissolved in the metal salt solution, which can improve the dispersion uniformity of the silicon-carbon precursor in the metal salt solution. Specifically, the silane activator used includes one of KH550 and KH560, and the mass ratio of the silicon-carbon precursor to the silane activator can be 1:(0.05-0.08).

[0096] In some embodiments, the surface of the silicon-carbon precursor may be subjected to short-time oxygen plasma treatment in step S5. Short-time oxygen plasma treatment can improve the surface hydrophilicity of the silicon-carbon precursor, which helps to uniformly adsorb metal ions in the metal salt solution, thereby improving the density and uniformity of the fluorinated metal layer on the surface of the composite material after fluorination treatment.

[0097] Furthermore, in step S5, the silicon-carbon precursor can be subjected to surface oxygen plasma treatment in an activation gas with an absolute pressure of 10 Pa-200 Pa, wherein the activation gas used includes one of air, oxygen, and water vapor. In addition, the plasma source used for oxygen plasma treatment includes one of microwave plasma, radio frequency plasma, and DC plasma, and the power of the plasma source can be 100 W-200 W. In practice, the surface of the silicon-carbon precursor can be subjected to oxygen plasma treatment for 30 s-90 s. This short-duration oxygen plasma treatment avoids deep oxidation of the silicon-carbon precursor that could damage the conductive network.

[0098] In other embodiments, in step S5, the silicon-carbon precursor can be mixed and desolvated in a metal salt solution containing a dissolved transition carbon source to obtain a silicon-carbon intermediate. Specifically, the transition carbon source used includes one of citric acid and glucose, and the mass ratio of the silicon-carbon precursor to the transition carbon source can be 1:(0.05-0.15). In fact, such mixing can form a composite layer of uniformly mixed transition carbon source and metal salt on the surface of the silicon-carbon intermediate. Then, during the high-temperature fluorination process, the transition carbon source decomposes in situ to form a carbon skeleton, which is pinned to the silicon-carbon matrix. At the same time, the fluorinated metal layer and the carbon skeleton are intertwined and interlocked, which helps to improve the interfacial bonding strength.

[0099] In some embodiments, in step S6, the silicon-carbon intermediate and the fluorinating agent can be ultrasonically blended in a solvent environment at a mass ratio of 1:(0.01-0.2), followed by desolventizing and drying. This helps improve the mixing uniformity of the silicon-carbon intermediate and the fluorinating agent. The mixture is then transferred to a protective atmosphere at 200℃-400℃ and 0.1MPa-1MPa for high-temperature heat treatment for 60min-120min, followed by cooling to obtain the fluorinated metal composite silicon-carbon material. Specifically, the fluorinating agent used includes one of ammonium fluoride and ammonium hydrogen fluoride, and the solvent environment used must be such that it does not react with the silicon-carbon intermediate or the fluorinating agent.

[0100] The present invention also provides a fluorinated metal composite silicon-carbon material prepared by any of the above preparation methods, comprising a silicon-carbon skeleton and a fluorinated metal layer formed on the surface of the silicon-carbon skeleton, wherein the silicon-carbon skeleton comprises a porous carbon skeleton at least doped with nitrogen and composite silicon within its pores, the composite silicon comprises a silicon skeleton bonded to the inner wall of the porous carbon pores and a metal composite and lithium nanoparticles doped within the silicon skeleton, and the metal composite is formed by in-situ decomposition of an oxyacid metal salt at high temperature and subsequent nitriding.

[0101] Example 1: A method for preparing a fluorinated metal composite silicon-carbon material, comprising the following steps: S1. Magnesium nitrate and polyvinylpyrrolidone (PVP, purchased from Boai Xinkaiyuan Pharmaceutical Co., Ltd., K30) were mixed and dissolved in anhydrous ethanol to prepare a magnesium nitrate composite solution. Porous carbon (purchased from Jinbo Carbon Co., Ltd., brand name KBC / PC-1) was added to the magnesium nitrate composite solution, and the mass ratio of porous carbon to magnesium ions and polyvinylpyrrolidone was adjusted to 1:0.05:0.05. After mixing under ultrasonic power of 300W for 15 minutes, the mixture was evaporated to dryness in a water bath at 60℃ and dried continuously at 60℃ until constant weight to obtain the composite precursor. S2. The composite precursor is transferred to an atmosphere furnace. After evacuation, ammonia gas is introduced and the pressure of ammonia gas in the atmosphere furnace is adjusted to 1 kPa. The atmosphere furnace is heated to 800°C at a rate of 5°C / min and then held at the temperature for nitriding treatment for 120 min. After cooling to room temperature with the furnace, the composite carbon material is obtained. S3. After dissolving lithium acetate and tetraethyl orthosilicate in ethanol to prepare a composite solution, the composite carbon material is added to the composite solution and ultrasonically dispersed. The mass ratio of the composite carbon material to lithium in the composite solution and silicon in tetraethyl orthosilicate is controlled to be 1:0.03:0.8. The mixture is then transferred to 50℃ and 80kPa for 90min and then dried at 100℃ and 30kPa to constant weight to obtain the composite intermediate. S4. The composite intermediate was transferred to an atmosphere furnace, and after evacuation, a reducing atmosphere (containing 10 vol% hydrogen and 90 vol% argon) was introduced. The atmosphere furnace pressure was adjusted to 1 kPa. The atmosphere furnace was heated to 1100℃ at a rate of 5℃ / min and held for 3 hours. After cooling to room temperature with the furnace, the silicon-carbon precursor was obtained. S5. Silver nitrate solution is prepared by stirring and dissolving silver nitrate in deionized water. Silicon carbon precursor is added to silver nitrate solution and ultrasonically dispersed. After adjusting the mass ratio of silicon carbon precursor to silver ions to 1:0.15, it is spray dried in a spray drying equipment to obtain silicon carbon intermediate. S6. The silicon-carbon intermediate and ammonium bifluoride were mixed at a mass ratio of 1:0.1 and then ultrasonically dispersed in acetone. After centrifugation at 3000 rpm and discarding the upper acetone layer, the lower solid layer was dried in a vacuum environment at 50°C and then transferred to an atmosphere furnace. The atmosphere furnace was heated to 300°C in an argon atmosphere of 0.5 MPa and held for 90 min. After cooling to room temperature in the furnace, the fluorinated metal composite silicon-carbon material was obtained.

[0102] Example 2: A method for preparing a fluorinated metal composite silicon-carbon material, which differs from Example 1 in that, in step S5, cobalt nitrate is dissolved in deionized water to obtain a cobalt nitrate solution, and a silicon-carbon precursor is added to the cobalt nitrate solution and ultrasonically dispersed, adjusting the mass ratio of silicon-carbon precursor to cobalt ions to 1:0.15.

[0103] Example 3: A method for preparing a fluorinated metal composite silicon-carbon material, which differs from Example 1 in that, in step S5, silver nitrate and KH550 are mixed and dissolved in deionized water to obtain a silver nitrate mixed solution, and the silicon-carbon precursor is added to the mixed solution and ultrasonically dispersed. The mass ratio of silicon-carbon precursor to silver ions and KH550 is adjusted to 1:0.15:0.06, and spray drying is carried out in a spray drying device to obtain a silicon-carbon intermediate.

[0104] Example 4: A method for preparing a fluorinated metal composite silicon-carbon material, which differs from Example 3 in that, in step S5, the silicon-carbon precursor is transferred to the chamber of a plasma device beforehand, oxygen is introduced and the oxygen pressure in the chamber is adjusted to 100 Pa, and then the silicon-carbon precursor is treated with a microwave plasma source at a power of 150 W for 60 s.

[0105] Example 5: A method for preparing a fluorinated metal composite silicon-carbon material, which differs from Example 3 in that, in step S5, silver nitrate, KH550 and glucose are mixed and dissolved in deionized water to obtain a silver nitrate mixed solution. The silicon-carbon precursor is added to the mixed solution and ultrasonically dispersed. The mass ratio of silicon-carbon precursor, silver ions, KH550 and glucose is adjusted to 1:0.15:0.06:0.10. After spray drying in a spray drying device, the material is transferred to an atmosphere furnace. After evacuation, ammonia gas is introduced and the pressure of ammonia gas in the atmosphere furnace is adjusted to 1 kPa. The atmosphere furnace is heated to 800°C at a rate of 5°C / min and then held at that temperature for nitriding treatment for 120 min. After cooling to room temperature with the furnace, a silicon-carbon intermediate is obtained.

[0106] Example 6: A method for preparing a fluorinated metal composite silicon-carbon material, which differs from Example 5 in that, in step S5, the silicon-carbon precursor is transferred to the chamber of a plasma device beforehand, oxygen is introduced and the oxygen pressure in the chamber is adjusted to 100 Pa, and then the silicon-carbon precursor is treated with a microwave plasma source at a power of 150 W for 60 s.

[0107] Comparative Example 1: A method for preparing a fluorinated metal composite silicon-carbon material, which differs from Example 1 in that steps S1 and S2 are not performed. In step S3, porous carbon (purchased from Jinbo Carbon Co., Ltd., brand name KBC / PC-1) is directly added to the composite solution for ultrasonic dispersion, and the mass ratio of porous carbon to lithium element in the composite solution and silicon element in tetraethyl orthosilicate is controlled to be 1:0.03:0.8.

[0108] Comparative Example 2: A method for preparing a fluorinated metal composite silicon-carbon material, which differs from Example 1 in that, after evacuation in step S2, argon gas is introduced and the pressure of the argon gas in the atmosphere furnace is adjusted to 1 kPa.

[0109] Comparative Example 3: A method for preparing a fluorinated metal composite silicon-carbon material, which differs from Example 1 in that lithium acetate is not added in step S3, tetraethyl orthosilicate is dissolved in ethanol to obtain a tetraethyl orthosilicate solution, the composite carbon material is added to the tetraethyl orthosilicate solution for ultrasonic dispersion, and the mass ratio of the composite carbon material to silicon in tetraethyl orthosilicate is controlled to be 1:0.8.

[0110] Comparative Example 4: A method for preparing a fluorinated metal composite silicon-carbon material, which differs from Example 3 in that, in step S5, a microwave plasma source is used to treat the silicon-carbon precursor at a power of 150W for 5 minutes.

[0111] Comparative Example 5: A method for preparing a composite silicon-carbon material, which differs from Example 1 in that steps S5 and S6 are not performed, and the silicon-carbon precursor obtained in step S4 is the composite silicon-carbon material.

[0112] Performance testing: The silicon-carbon materials prepared in Examples 1 to 6 and Comparative Examples 1 to 5 were mixed with binder (LA136D) and conductive agent (Super P) in a ratio of 8:1:1 to prepare active slurries. The active slurries were coated on copper current collectors, vacuum dried, and rolled into composite sheets. Lithium metal was used as the counter electrode, lithium hexafluorophosphate as the electrolyte, and polypropylene microporous membrane as the separator. The cells were assembled into coin cells in a glove box. After activation at a current density of 0.05C for three cycles, the cells were cycled at a current density of 0.5C at room temperature for 200 cycles. The initial reversible specific capacity, initial coulombic efficiency, and capacity retention rate after 200 cycles were calculated. The process was repeated three times and the average value was calculated. The results are shown in Table 1 below.

[0113] Table 1 Electrochemical performance test data of coin cells

[0114] Combining Example 1 and Comparative Example 1, Table 1 shows that in-situ decomposition of oxyacid metal salts in silicon-carbon materials and the formation of metal composites in a nitrogen-containing atmosphere, along with the dispersion of these metal composites within the nano-silicon framework to support the framework and disperse expansion stress, prevents structural collapse and pulverization of the nano-silicon framework during battery cycling when the nano-silicon undergoes volume changes, significantly improving the battery's long cycle life. Furthermore, Comparative Example 2 shows that high-temperature nitriding of the composite precursor in ammonia can synergize with the nitrogen source generated from the decomposition of magnesium nitrate and nitrogen doping of porous carbon, improving the intrinsic electronic conductivity and lithium-ion transport efficiency of the silicon-carbon material, thereby enhancing electrochemical performance. Comparative Example 3 shows that pre-lithiation treatment in silicon-carbon materials can improve the battery's initial coulombic efficiency; however, due to the continuous rupture and regeneration of the SEI film during cycling, the battery's cycle performance also significantly decreases.

[0115] As can be seen from Example 1 and Comparative Example 5, the fluorinated metal layer formed on the outside of the silicon-carbon material can form a LiF-rich fluorinated metal SEI film during the first charge of the battery, effectively isolating the inside of the silicon-carbon material from the electrolyte and preventing the electrolyte from penetrating into the silicon-carbon material and causing side reactions with the nano-silicon. This effectively improves the first coulombic efficiency and long cycle life of the battery. In addition, as can be seen from Example 1 and Example 2, the silver fluoride layer and cobalt fluoride layer on the surface of the silicon-carbon material can improve the electrochemical performance of the battery. However, the silver nanoparticles generated in situ at the silver fluoride interface during battery cycling can further improve the electrochemical performance.

[0116] As can be seen from Examples 1 and 3, adding KH550 as a silane activator to the silver nitrate solution helps to improve the dispersion uniformity of the silicon-carbon precursor in the silver nitrate mixed solution. During the spray drying process, it helps the silver nitrate to be evenly distributed on the surface of the silicon-carbon precursor, avoids the aggregation of silver nitrate on the surface of the silicon-carbon precursor, improves the uniformity and density of the fluorinated metal layer on the surface of the fluorinated silicon-carbon material, optimizes the interface stability of the battery, and improves the long cycle performance of the battery.

[0117] As can be seen from Examples 3 and 4, pre-treatment of the surface of the silicon-carbon precursor with short-time oxygen plasma improves the hydrophilicity of the silicon-carbon precursor and works synergistically with KH550 in the silver nitrate mixed solution to further improve the density and uniformity of the fluorinated metal layer on the surface of the silicon-carbon precursor. This results in the formation of a LiF-rich fluorinated metal SEI film with better structural stability on the surface of the silicon-carbon material, further improving the electrochemical performance. In addition, as can be seen from Comparative Example 4, short-time oxygen plasma treatment can avoid deep oxidation of the silicon-carbon precursor, which would otherwise lead to irreversible degradation of the electrochemical performance of the battery.

[0118] As can be seen from Examples 3 and 5, by adding glucose as a transition carbon source to the silver nitrate mixed solution and performing nitriding treatment in high-temperature ammonia, glucose is pyrolyzed in situ to form a transition carbon framework and forms a pinned bond with the silicon-carbon precursor. At the same time, during the spray drying process, glucose and silver nitrate form a uniform composite. After pyrolysis and carbonization, silver nitrate decomposes and is uniformly doped into the transition carbon framework, which helps to avoid the aggregation of silver fluoride during fluorination, thereby improving the uniformity and density of the silver fluoride layer. In addition, it can further improve the strength of the silver fluoride-based SEI film during battery cycling and alleviate stress expansion during cycling, significantly improving the long-cycle performance of the battery.

[0119] While embodiments of the present invention have been described in detail above, it will be apparent to those skilled in the art that various modifications and variations can be made to these embodiments. However, it should be understood that such modifications and variations fall within the scope and spirit of the invention as set forth in the claims. Furthermore, the invention described herein may have other embodiments and can be implemented or carried out in various ways.

Claims

1. A method for preparing a fluorinated metal composite silicon-carbon material, characterized in that, include: Porous carbon was mixed in an oxyacid metal salt solution and evaporated to dryness to obtain a composite precursor; High-temperature nitriding of the composite precursor yields a composite carbon material; The composite carbon material was vacuum dried in a composite solution containing dissolved lithium salt and organosilicon to obtain a composite intermediate. The composite intermediate is subjected to high-temperature reduction in a reducing atmosphere to obtain a silicon-carbon precursor; the silicon-carbon precursor is mixed in a metal salt solution and desolventized to obtain a silicon-carbon intermediate; the silicon-carbon intermediate is mixed with a fluorinating agent and then subjected to high-temperature treatment to obtain a fluorinated metal composite silicon-carbon material.

2. The preparation method according to claim 1, characterized in that: The porous carbon has a specific surface area of ​​1500 m². 2 / g-2500m 2 / g; and / or, the porous carbon has a particle size of 1μm-50μm; and / or, the oxyacid metal salt dissolved in the oxyacid metal salt solution includes one of metal sulfate and metal nitrate; and / or, the metal ions in the oxyacid metal salt solution include one of aluminum ions, titanium ions, and magnesium ions; and / or, the mass ratio of the porous carbon to the metal ions in the oxyacid metal salt solution is 1:(0.01-0.1); and / or, the oxyacid metal salt solution also contains a dispersant, preferably polyvinylpyrrolidone, and preferably the mass ratio of the porous carbon to the dispersant is 1:(0.05-0.2).

3. The preparation method according to claim 1, characterized in that: Porous carbon is mechanically mixed with an oxyacid metal salt solution, preferably the mechanical mixing includes ultrasonication, stirring, and oscillation; and / or, the mixture is evaporated to dryness at 50℃-80℃ to obtain a composite precursor; and / or, the composite precursor is nitrided at high temperature at 700℃-1100℃; and / or, the composite precursor is nitrided at high temperature in a nitrogen-containing atmosphere, preferably the nitrogen-containing atmosphere includes a nitrogen atmosphere or an ammonia atmosphere, preferably nitrided at high temperature in a nitrogen-containing atmosphere of 0.5kPa-2kPa; and / or, the composite precursor is nitrided at high temperature for 60min-180min; and / or, the composite carbon material is obtained by cooling after high-temperature nitriding.

4. The preparation method according to claim 1, characterized in that: The lithium salt includes one of lithium carbonate, lithium hydroxide, lithium tetrafluoroborate, and organolithium, preferably one of lithium acetate and lithium tert-butoxide; and / or, the organosilicon includes one of tetraethyl orthosilicate and alkyl orthosilicate; and / or, the mass ratio of the composite carbon material to the lithium element in the lithium salt is 1:(0.01-0.05); and / or, the mass ratio of the composite carbon material to the silicon in the organosilicon is 1:(0.5-1); and / or, the composite carbon material is impregnated in a composite solution under reduced pressure and then dried, preferably impregnated at 60kPa-80kPa for 60min-120min, preferably impregnated in a composite solution at 40℃-60℃; and / or, dried under vacuum at 80℃-100℃; and / or, dried at 1kPa-50kPa.

5. The preparation method according to claim 1, characterized in that: The reducing atmosphere includes a reducing gas and an inert carrier gas. Preferably, the reducing gas includes hydrogen. Preferably, the concentration of the reducing gas is 5 vol%-15 vol%. Preferably, the inert carrier gas includes one of argon, helium, and nitrogen. Reduction is performed in a reducing atmosphere of 0.5 kPa-2 kPa. Reduction is performed at high temperature in the reducing atmosphere for 2-5 hours. Reduction is performed in a reducing atmosphere of 800℃-1300℃. Reduction is performed at high temperature followed by cooling to obtain a silicon-carbon precursor.

6. The preparation method according to claim 1, characterized in that: The metal salt dissolved in the metal salt solution includes one of metal chloride, metal sulfate, and metal nitrate; and / or, the metal ion in the metal salt solution includes one of cobalt ion, magnesium ion, and silver ion; and / or, the mass ratio of the silicon-carbon precursor to the metal ion in the metal salt solution is 1:(0.05-0.2); and / or, after mixing, the silicon-carbon intermediate is obtained by spray drying; and / or, the metal salt solution also contains a silane activator, preferably one of KH550 and KH560, and preferably the mass ratio of the silicon-carbon precursor to the silane activator is 1:(0.05-0.08).

7. The preparation method according to claim 1, characterized in that: The surface of the silicon-carbon precursor is pretreated with short-time oxygen plasma; preferably, the surface of the silicon-carbon precursor is treated with short-time oxygen plasma in an activation gas, more preferably, the activation gas includes one of air, oxygen, and water vapor, and more preferably, the absolute pressure of the activation gas is 10 Pa-200 Pa; preferably, the plasma source for oxygen plasma treatment includes one of microwave plasma, radio frequency plasma, and DC plasma; preferably, the power for oxygen plasma treatment is 100 W-200 W; preferably, the surface of the silicon-carbon precursor is treated with oxygen plasma for 30 s-90 s; and / or, the silicon-carbon precursor is mixed with a metal salt solution containing a transition carbon source and desolvated, and then carbonized at 700 °C-1100 °C to obtain a silicon-carbon intermediate; preferably, the transition carbon source includes one of citric acid and glucose; preferably, the mass ratio of the silicon-carbon precursor to the transition carbon source is 1:(0.05-0.15).

8. The preparation method according to claim 1, characterized in that: The fluorinating agent includes one of ammonium fluoride and ammonium hydrogen fluoride; and / or, the mass ratio of the silicon-carbon intermediate to the fluorinating agent is 1:(0.01-0.2); and / or, the silicon-carbon intermediate and the fluorinating agent are mixed in a solvent environment and then desolventized; and / or, a fluorinated metal composite silicon-carbon material is obtained by high-temperature treatment at 200℃-400℃; and / or, a fluorinated metal composite silicon-carbon material is obtained by high-temperature treatment for 60min-120min; and / or, a fluorinated metal composite silicon-carbon material is obtained by high-temperature treatment in a protective atmosphere, preferably in a protective atmosphere of 0.1MPa-1MPa; and / or, a fluorinated metal composite silicon-carbon material is obtained by cooling after high-temperature treatment.

9. A fluorinated metal composite silicon-carbon material prepared by the preparation method according to any one of claims 1 to 8, characterized in that, The invention includes a silicon-carbon framework and a fluorinated metal layer formed on the surface of the silicon-carbon framework. The silicon-carbon framework includes a porous carbon framework and composite silicon within its pores. The porous carbon framework is doped with nitrogen. The composite silicon includes a silicon framework bonded to the inner wall of the porous carbon pores and a metal composite and lithium nanoparticles doped within the silicon framework. The metal composite is formed by in-situ decomposition of an oxyacid metal salt at high temperature followed by nitriding.

10. An application of a fluorinated metal composite silicon-carbon material prepared by the preparation method according to any one of claims 1 to 8, characterized in that, The application includes secondary batteries.