A sodium-ion battery hard carbon negative electrode material based on zinc-containing viscose fiber and a preparation method, battery and application thereof
By utilizing the enrichment characteristics of zinc ions in the skin layer during viscose fiber spinning, a gradient pore structure with a porous skin layer and a dense core layer is formed, which solves the problems of lengthy process and skeleton pulverization in the preparation of hard carbon anode materials, improves electrochemical performance and resource utilization, and is suitable for industrial production.
Patent Information
- Application Number
- CN202611302108.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-26
- Publication Date
- 2026-11-24
AI Technical Summary
Existing hard carbon anode materials suffer from lengthy preparation processes, severe skeleton pulverization, uneven pore structure distribution, low initial coulombic efficiency, and the viscose fiber industry has failed to effectively utilize the zinc ion resources enriched during spinning.
By utilizing the enrichment characteristics of zinc ions in the fiber skin during viscose fiber spinning, zinc ions are converted into metallic zinc vapor during carbonization, selectively creating pores in the skin to form a gradient pore structure with a porous skin and a dense core, simplifying the process and improving electrochemical performance.
This technology achieves high specific surface area and high structural strength in hard carbon materials, improving the reversible capacity and first coulombic efficiency of sodium-ion batteries, reducing production costs and environmental pressure, and making it suitable for large-scale industrial production.
Smart Images

Figure CN123162159A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of battery electrode technology, specifically a sodium-ion battery hard carbon anode material based on zinc-containing viscose fiber, its preparation method, battery, and application. Background Technology
[0002] Hard carbon materials, due to their large interlayer spacing and abundant defect sites, are currently the most promising anode materials for large-scale application in sodium-ion batteries.
[0003] The electrochemical performance of hard carbon anode materials is closely related to the choice of their precursors. Existing hard carbon precursors are mainly divided into three categories: resin-based precursors such as phenolic resins, which have excellent performance but high raw material costs; biomass precursors such as coconut shells and straw, which are abundant but have low carbon yields and their performance is greatly affected by fluctuations in raw material sources; and coal-based precursors such as anthracite and bitumen, which are inexpensive but require pre-oxidation treatment to prevent graphitization, and the resulting hard carbon materials generally have low sodium storage capacity. In the preparation of hard carbon using these precursors, to improve the sodium storage capacity and initial coulombic efficiency, it is generally necessary to introduce pore-forming agents such as zinc chloride, potassium hydroxide, and phosphoric acid before carbonization treatment, constructing a porous structure in the fiber skeleton through chemical activation.
[0004] However, existing pore-forming processes still have several inherent limitations. On the one hand, the additional impregnation and drying processes significantly increase the process length, extend the production cycle, and correspondingly raise energy consumption and labor costs. On the other hand, when the pore-forming agent is introduced through exogenous liquid-phase impregnation, the metal salt is uniformly distributed throughout the precursor. During carbonization, the pore-forming reaction occurs synchronously throughout the entire process, inevitably causing excessive etching and severe pulverization of the framework, resulting in a significant decrease in the particle mechanical strength of the obtained carbon material. Moreover, the pore structure formed by uniform etching usually exhibits a wide pore size distribution and a mixture of micropores and mesopores, leading to a tortuous transport path and low transport efficiency for sodium ions within the electrode material, which is not conducive to achieving excellent rate performance. For example, CN119735195B discloses a hard carbon anode material and its preparation method, which mixes organic matter with a pore-forming agent before carbonization. This pore-forming agent is a strong acid-weak base salt. Because the pore-forming agent is fully mixed with the organic matter before carbonization, the pore-forming reaction is uniformly initiated inside the material during the carbonization process. This method cannot selectively control the pore-forming area, and the resulting carbon material still suffers from structural pulverization caused by the formation of pores throughout the material. Furthermore, the pore size distribution is difficult to control precisely.
[0005] In addition, the initial coulombic efficiency of hard carbon materials prepared by conventional pore-forming processes is generally low, and the use of large amounts of pore-forming agents also increases the procedures and costs of subsequent wastewater treatment.
[0006] Regenerated cellulose viscose fiber, as an optional raw material for hard carbon precursors, directly influences the formation of the pore structure of carbon materials due to its structural characteristics. Industrially, viscose fiber is prepared via wet spinning. Its coagulation bath standard system consists of a compound of sulfuric acid, sodium sulfate, and zinc sulfate, with zinc sulfate used to adjust the osmotic pressure of the acid bath to ensure fiber smoothness. During spinning coagulation, zinc ions diffuse from the coagulation bath to the fiber cortex, reacting with sodium cellulose xanthate in the cortex to form insoluble zinc cellulose xanthate, thus naturally enriching zinc ions in the fiber cortex region. This structural feature originating from the spinning process means that viscose fiber itself carries zinc ions enriched in the cortex when used as a hard carbon precursor. However, due to environmental compliance requirements in the viscose fiber industry, manufacturers typically employ enhanced washing processes to remove zinc ions from the fibers to extremely low levels to ensure that the zinc residue in the fiber products meets relevant standards. Correspondingly, current research on viscose-based carbon materials is highly focused on the purification of raw materials, primarily concentrating on how to remove zinc ions as much as possible through processes such as water washing. No research has yet addressed or utilized the zinc ions naturally enriched in the fiber sheath. This results in the zinc ions introduced into the sheath during viscose fiber coagulation being removed as waste in subsequent water washing stages, failing to be effectively utilized. Summary of the Invention
[0007] The purpose of this invention is to provide a sodium-ion battery hard carbon anode material based on zinc-containing viscose fiber, its preparation method, battery, and application, in order to solve the prominent problems of existing hard carbon anode material preparation technology that relies on pore-forming agents, such as lengthy process routes, severe skeleton pulverization, uniform pore structure, low initial coulombic efficiency, and high wastewater treatment pressure. In particular, this invention also overcomes the inherent technical biases in the viscose fiber industry and realizes the utilization of residual zinc ion waste in viscose fiber.
[0008] This invention directly utilizes zinc ions, which are in-situ entrained in the spinning acid bath and enriched in the cortex, as an internal pore-building template and activator. During the carbonization process, zinc ions undergo an in-situ evolution from zinc ions and zinc oxide to metallic zinc vapor, selectively creating pores only in the fiber cortex. This forms a gradient pore structure with a porous cortex and a dense core, without the need for any additional pore-building agents. This simplifies the process and reduces the environmental pressure on existing viscose spinning production lines. The resulting hard carbon has both abundant sodium storage active sites and a continuous conductive framework, improving reversible capacity and first coulombic efficiency.
[0009] To achieve the above objectives, the technical solution of the present invention is as follows:
[0010] In a first aspect, a sodium-ion battery hard carbon anode material based on zinc-containing viscose fiber is provided. The sodium-ion battery hard carbon anode material has a skin-core structure, wherein the skin layer is a porous layer with pores, the core layer is a dense layer with pores, and the porosity gradually decreases from the skin layer to the core layer, forming a pore gradient distribution structure.
[0011] The thickness of the skin layer accounts for 5% to 25% of the cross-sectional radius of the sodium-ion battery hard carbon anode material;
[0012] The pores in the core-sheath structure are formed when zinc ions in zinc-containing viscose fibers are converted into metallic zinc vapor through zinc oxide intermediate state and escape.
[0013] The zinc content in the dry basis of the zinc-containing viscose fiber is 0.2wt% to 5wt%.
[0014] Let the radial cross-sectional radius of the hard carbon anode material for sodium-ion batteries be R, the thickness of the skin layer be d, and the radius of the core layer be r, i.e., r = Rd. Based on the kinetic process of zinc ions diffusing from the coagulation bath to the fiber interior during wet spinning, and the dry-basis zinc content specified in this invention being 0.2wt%~5wt%, the thickness d of the skin layer accounts for 5%~25% of the radius R, i.e.: d : r = 1 : 19 ~ 1 : 3. Further, in terms of radial cross-sectional area, the cross-sectional area of the skin layer accounts for 10%~45% of the total cross-sectional area of the fiber, and the cross-sectional area of the core layer accounts for 55%~90% of the total cross-sectional area of the fiber.
[0015] Preferably, the pore size of the skin layer is 0.5–3 nm.
[0016] The zinc-containing viscose fiber is obtained by wet spinning from viscose solution;
[0017] The coagulation bath of the wet spinning process contains water-soluble zinc salts, and zinc ions diffuse into the viscose fibers during the coagulation and molding of the viscose solution.
[0018] Preferably, zinc ions diffuse into the skin region of the viscose fiber during the solidification of the viscose solution.
[0019] When the viscose solution enters the coagulation bath and solidifies, zinc ions react with sodium cellulose xanthate on the fiber surface to form zinc cellulose xanthate. Zinc ions preferentially accumulate in the fiber cortex region, which inhibits the further inward diffusion of zinc ions, thus resulting in a relatively low zinc ion content in the core layer.
[0020] As a limitation of the present invention, the raw material of the viscose base is at least one selected from wood pulp, cotton pulp, bamboo pulp, and hemp pulp; the pulp cellulose content of the raw material is ≥90%, and the degree of polymerization is 650-1200; and / or
[0021] The water-soluble zinc salt is at least one of zinc sulfate, zinc chloride, zinc nitrate, and zinc acetate.
[0022] Among them, viscose fibers obtained from cellulose pulp commonly used in various wet spinning processes can achieve zinc ion enrichment in the coagulation bath of this invention, without affecting the gradient pore structure and electrochemical performance of the raw materials. Dissolving-grade wood pulp or cotton pulp is preferred, as the raw materials are widely available and inexpensive, making them suitable for large-scale industrial production of viscose fibers.
[0023] As another limitation of the present invention, the coagulation bath comprises: zinc sulfate 5-12 g / L, sulfuric acid 90-120 g / L, and sodium sulfate 150-250 g / L.
[0024] Secondly, the present invention also provides a method for preparing a hard carbon anode material for sodium-ion batteries based on zinc-containing viscose fibers, comprising the following steps performed sequentially:
[0025] The zinc-containing viscose fiber was placed in an inert atmosphere with a gas flow rate of 50-500 mL / min (per gram of fiber) to carry away impurities released during carbonization from the reaction system. The carbonization process was completed by heating to 1000-1600℃ and holding for 1-5 hours, followed by natural cooling to obtain the carbonized product.
[0026] The obtained carbonized products were purified by acid washing, dried and pulverized to obtain hard carbon anode material for sodium-ion batteries.
[0027] The mechanism of in-situ evolution of zinc ions during the carbonization process in an inert atmosphere is as follows:
[0028] At around 600℃, zinc ions in the cortex combine with oxygen-containing groups in the zinc-containing viscose fiber to form nano-zinc oxide; when the temperature rises to above 1000℃, the nano-zinc oxide is carbothermally reduced to generate metallic zinc vapor (ZnO+C=Zn↑+CO). The zinc vapor escapes outward along the short path of the cortex, and only the zinc-containing viscose fiber cortex is etched to generate a large number of micropores and small mesopores.
[0029] It should be noted that due to the presence of sulfuric acid in the coagulation bath and residues from the xanthation process, a small amount of sulfur is inevitably introduced into viscose fibers during spinning. Under the carbonization conditions of this invention, the sulfur is released from the fibers primarily as gaseous sulfides such as SO2 and H2S before the carbonization temperature reaches 600°C. Since zinc ions only begin to transform into nano-zinc oxide at around 600°C, the release temperature window of sulfur oxides is earlier than the formation temperature of ZnO, and the two are staggered in time. Therefore, sulfur will not substantially interfere with the subsequent conversion of ZnO into metallic zinc vapor. Furthermore, the continuous carrier gas flow in the inert atmosphere can also promptly carry the released sulfur-containing gases out of the reaction system, further avoiding the risk of ZnS formation.
[0030] The core layer of zinc-containing viscose fiber has an extremely low zinc ion content and no obvious vaporization etching, thus preserving a dense, disordered carbon skeleton.
[0031] Through the above process, a gradient pore structure is finally formed with a porous skin layer and a relatively dense core layer. The pores in the skin layer provide active sites for sodium ion insertion and fast transport channels, while the dense carbon structure in the core layer serves as a high-speed conductive framework for electrons. Therefore, the sodium-ion battery hard carbon anode material based on zinc-containing viscose fiber of the present invention has both high specific surface area and high structural strength.
[0032] As a limitation of the present invention, when preparing the zinc-containing viscose fiber, the coagulation bath temperature is 40-60°C and the fiber draw ratio is 1-1.5.
[0033] Unlike conventional high-temperature, long-duration deep water washing zinc removal processes, this invention shortens the washing time, reduces the washing temperature and flow rate, and precisely controls the dry zinc content of the resulting zinc-containing viscose fiber to be 0.2–5 wt%. The zinc content range can be stably controlled using existing continuous washing equipment. A high zinc content of 5 wt% is suitable for laboratory pilot tests, while the preferred range for mass production is 1–3.5 wt% to ensure stable production. During carbonization, an industrial continuous carbonization furnace is used, with a preferred carbonization temperature of 1200–1400℃. This temperature range allows for long-term stable operation, balancing pore-forming effect and equipment lifespan.
[0034] As another limitation of the present invention, the heating rate of the carbonization treatment is 1–10 °C / min; and / or
[0035] Acid washing purification involves washing with 0.5–2 mol / L dilute hydrochloric acid or dilute sulfuric acid at room temperature with stirring for 2–6 hours, followed by washing with water until the washing solution is neutral; and / or
[0036] Drying is carried out at 80-120℃.
[0037] As a further limitation of the present invention, when the thickness of the zinc-containing viscose fiber is ≥3mm, the zinc-containing viscose fiber is subjected to pre-oxidation treatment and then carbonization treatment.
[0038] The pre-oxidation treatment involves placing the zinc-containing viscose fiber in an air atmosphere and heating it to 200-300°C at a rate of 0.5-2°C / min, and holding it at that temperature for 1-3 hours.
[0039] When using industrial thick tows of zinc-containing viscose fiber with a thickness ≥3mm and dense stacking, direct carbonization without pre-oxidation treatment will cause the surface cellulose to melt and agglomerate rapidly, blocking the flow of inert atmosphere and causing the zinc in the cortex to be lost prematurely with the low-temperature flue gas, affecting the subsequent formation of gradient pore structure. On the other hand, thin fiber tows are fully permeable, that is, zinc-containing viscose fiber is a single layer or a loose thin layer, especially when the thickness is <2mm, the risk of melting and agglomeration is low, and the pre-oxidation treatment process can be omitted.
[0040] Thirdly, the present invention also provides a sodium-ion battery comprising a separator, a positive electrode, and a negative electrode, wherein the negative electrode is prepared by uniformly mixing the above-mentioned sodium-ion battery hard carbon negative electrode material based on zinc-containing viscose fiber, conductive carbon black, and binder, and coating it onto a current collector.
[0041] The positive electrode is a sodium metal sheet;
[0042] Preferably, the sodium-ion battery hard carbon anode material based on zinc-containing viscose fiber, conductive carbon black, and binder are mixed uniformly in a mass ratio of 80:10:10;
[0043] The preferred adhesive is a PVDF adhesive;
[0044] The diaphragm is preferably a glass fiber diaphragm;
[0045] The preferred current collector is a copper foil current collector;
[0046] Sodium hexafluorophosphate solution is used as the electrolyte, preferably with a concentration of 1 mol / L, and the solvent is prepared by mixing ethylene carbonate and dimethyl carbonate in equal volume ratio.
[0047] Fourthly, the present invention also provides the application of the preparation method of the sodium-ion battery hard carbon anode material based on zinc-containing viscose fiber described in any one of the above-mentioned methods in the preparation of sodium-ion batteries.
[0048] By adopting the above technical solution, the technical progress achieved by this invention compared with the prior art is as follows:
[0049] This invention addresses the industry's technical bottlenecks in existing viscose-based hard carbon materials, such as lengthy processes, skeleton pulverization, and low initial efficiency due to reliance on exogenous pore-forming agents, as well as the long-standing technical bias in the viscose fiber industry of removing native zinc ions from the sheath as impurities through washing. By reverse-regulating the washing intensity, this invention actively retains zinc ions enriched in the sheath during the spinning and coagulation stage, transforming the textile byproduct impurity zinc into a functional pore-forming component in situ. Utilizing the selective enrichment of zinc ions in the sheath region, directional pores are created in the fiber sheath after carbonization, while a dense conductive skeleton is retained in the core layer, forming a gradient pore structure with a porous sheath and a dense core layer. This simultaneously meets the dual requirements of sodium ion embedding and storage and rapid electron conduction. Details are as follows:
[0050] (1) In terms of simplifying the process and reducing production costs, this invention directly utilizes the zinc sulfate naturally present in the viscose fiber coagulation bath as the zinc source, eliminating the need for additional exogenous pore-forming agents such as zinc chloride and potassium hydroxide, and eliminating independent processes such as impregnation and drying, thus significantly shortening the process flow. Unlike the conventional high-temperature, long-duration deep water washing process for zinc removal in the industry, this invention can control the zinc content in the fiber by shortening the washing time, reducing the washing temperature and flow rate, thereby reducing the energy consumption and water consumption of the washing process. The overall preparation cost of the resulting hard carbon anode material is lower than that of the existing exogenous pore-forming activation process, and it can be directly connected to existing industrial viscose staple fiber or filament production lines without the need for large-scale equipment modification.
[0051] (2) Regarding improving pore structure distribution and maintaining skeleton strength, after liquid-phase impregnation, the metal salt of the exogenous pore-forming agent is uniformly distributed throughout the fiber, resulting in excessive etching and severe pulverization of the skeleton after carbonization, and a wide pore size distribution. In this invention, zinc ions diffuse from the outside to the inside during the spinning and solidification stage, reacting with sodium cellulose xanthate on the fiber surface to form insoluble zinc cellulose xanthate, which preferentially accumulates in the fiber skin. During carbonization, zinc vapor only escapes outward along a short path in the skin, resulting in the etching of a large number of micropores and small mesopores only in the skin, with no obvious vaporization etching in the core layer. The resulting hard carbon material has skin pores concentrated in a narrow range of 0.5–3 nm, and the fiber skeleton does not undergo overall pulverization. The particle mechanical strength and structural integrity are superior to the material obtained by overall activation with exogenous pore-forming agents.
[0052] (3) Regarding the improvement of electrochemical performance, the initial coulombic efficiency of hard carbon materials prepared by existing chemical activation methods is generally low, making it difficult to break through 80%. In this invention, the 0.5-3 nm pores in the skin layer provide abundant active sites and rapid transport channels for sodium ion insertion, while the dense carbon skeleton in the core layer serves as a high-speed electron conduction pathway, effectively reducing sodium ion transport resistance and electronic conduction impedance. When coin cells are assembled using the hard carbon anode material of this invention, the reversible specific capacity can reach over 300 mAh / g, and the capacity retention rate after 100 cycles is 95.68%. Both the rate performance and cycle stability meet the requirements of commercial sodium-ion batteries.
[0053] (4) Regarding improving zinc resource utilization and reducing environmental pressure, the existing viscose fiber industry, for environmental compliance reasons, removes zinc ions from the fibers to below 0.05 wt% through intensified washing, which wastes zinc resources and increases the treatment load of zinc-containing wastewater. This invention reverses the washing intensity to actively retain zinc ions in the outer layer, transforming the zinc component that was originally removed as an impurity into a functional pore-forming component, thereby reducing the discharge of zinc-containing wastewater and water treatment costs.
[0054] (5) In terms of raw material universality and mass production adaptability, this invention is applicable to two mainstream industrial fibers: viscose staple fiber and viscose filament. Zinc ion enrichment can be achieved in viscose dope solutions made from dissolving wood pulp or cotton pulp, and the raw material sources are wide. The zinc content in the obtained zinc-containing viscose fiber can be stably controlled within the range of 0.2wt% to 5wt% using existing continuous washing equipment. The carbonization temperature range is compatible with the long-term operating conditions of industrial continuous carbonization furnaces, and the process window is wide, making it suitable for large-scale industrial production of anode materials. Attached Figure Description
[0055] Figure 1 This is a scanning electron microscope image of HC-1 prepared in Example 1 of the present invention.
[0056] Figure 2 This is a constant current charge-discharge curve of the first charge-discharge process of HC-1 prepared in Example 1 of the present invention.
[0057] Figure 3 The graph shows the 100-cycle performance of HC-1 prepared in Example 1 of this invention.
[0058] Figure 4 This is a constant current charge-discharge curve of the first charge-discharge process based on HC-2 prepared in Example 2 of the present invention.
[0059] Figure 5 This is a constant current charge-discharge curve of the first charge-discharge process based on HC-3 prepared in Example 3 of the present invention.
[0060] Figure 6 This is a graph showing the 100-cycle performance of the hard carbon material prepared in Comparative Example 1 of this invention.
[0061] Figure 7 This is a graph showing the 100-cycle performance of the hard carbon material prepared in Comparative Example 2 of this invention.
[0062] Figure 8 This is a graph showing the 100-cycle performance of the hard carbon material prepared in Comparative Example 3 of this invention.
[0063] Figure 9 The graph shows the 100-cycle performance of the hard carbon material prepared in Comparative Example 4 of this invention.
[0064] Figure 10 This is a graph showing the 100-cycle performance of the hard carbon material prepared in Comparative Example 5 of this invention. Detailed Implementation
[0065] The present invention will be further described in detail below through specific embodiments. It should be understood that the described embodiments are only for explaining the present invention and do not limit the present invention.
[0066] Unless otherwise specified, the experimental methods used in the following examples are conventional methods in the art. Unless otherwise specified, the materials and reagents used in the following examples are commercially available.
[0067] In this invention, "native" refers to the source and introduction method of zinc ions. Specifically, the zinc ions originate from the zinc sulfate naturally present in the coagulation bath of viscose fiber spinning. During fiber coagulation, they diffuse from the coagulation bath into the fiber interior and accumulate in the cortex, rather than being introduced through subsequent impregnation or other external methods. "In-situ" refers to the reaction and pore-forming method of zinc ions during the carbonization process. The zinc ions enriched in the cortex do not require additional migration or external treatment; they directly undergo a valence state transformation from zinc ions and zinc oxide to metallic zinc vapor at their original location within the fiber cortex. The zinc vapor escapes outward along a short path within the cortex, selectively creating pores only in the cortex region where the zinc ions were originally located.
[0068] Example 1
[0069] This embodiment discloses a hard carbon anode material for sodium-ion batteries based on zinc-containing viscose fibers and its preparation method. The hard carbon anode material has a core-skin structure, with the skin layer being a porous layer and the core layer being a dense layer with pores. The porosity gradually decreases from the skin layer to the core layer, forming a pore gradient distribution structure. The pores in the core-skin structure are formed when zinc ions in the zinc-containing viscose fibers are converted from zinc oxide intermediates to metallic zinc vapor and escape. The zinc-containing viscose fibers are obtained from viscose dossile through wet spinning. The coagulation bath of the wet spinning process contains water-soluble zinc salts, and zinc ions diffuse into the viscose fibers during the coagulation of the viscose dossile.
[0070] Tests showed that the pore size of the cortex of zinc-containing viscose fiber is approximately 0.5–3 nm.
[0071] In this embodiment, the radial cross-sectional radius of the sodium-ion battery hard carbon anode material is set to R, the thickness of the skin layer to d, and the radius of the core layer to r, i.e., r = Rd. Based on the kinetic process of zinc ions diffusing from the coagulation bath to the fiber interior during wet spinning, and the dry basis zinc content, the thickness d of the resulting skin layer accounts for 25% of the radius R, i.e., d : r = 1 : 3.
[0072] The preparation method of the sodium-ion battery hard carbon anode material based on zinc-containing viscose fiber in this embodiment is as follows:
[0073] S1. Preparation of zinc-containing viscose fibers:
[0074] The viscose base solution is prepared by using wood pulp as raw material, with a pulp cellulose content of 92% and a degree of polymerization of 800, and through impregnation, xanthation and other processes.
[0075] A coagulation bath was prepared, comprising: 8 g / L zinc sulfate, 120 g / L sulfuric acid, and 200 g / L sodium sulfate. The coagulation bath temperature was set to 50℃, and the fiber draw ratio to be 1.2. The viscose solution was introduced into the coagulation bath via wet spinning. Zinc ions reacted with sodium cellulose xanthate on the fiber surface to form insoluble zinc cellulose xanthate, with zinc ions preferentially concentrated in the fiber cortex region.
[0076] The nascent fibers obtained by wet spinning are treated with a water washing process. Unlike the conventional high-temperature, long-term deep water washing process for zinc removal, this embodiment shortens the water washing time, reduces the water washing temperature and flow rate, and controls the zinc content in the dry basis of zinc-containing viscose fibers to 2.5 wt%.
[0077] In particular, this invention has discovered that the setting of parameters in the washing process affects the zinc content in the dry basis of zinc-containing viscose fibers. Specifically:
[0078] The washing process adopts the following process parameters: the washing temperature is 40℃~65℃, the washing residence time is 0.5min~5min, and the water bath ratio (water:fiber mass ratio) is 3:1~15:1.
[0079] To further precisely control the zinc content on a dry basis in the fiber, an optimal process range can be selected based on the target content range:
[0080] When the target zinc content is 0.2wt% to 1.0wt%, the preferred washing temperature is 60℃ to 65℃, the residence time is 3min to 5min, and the bath ratio is 10:1 to 15:1.
[0081] When the target zinc content is 1.0wt% to 3.5wt%, the preferred washing temperature is 50℃ to 60℃, the residence time is 1min to 3min, and the bath ratio is 5:1 to 10:1.
[0082] When the target zinc content is 3.5wt% to 5.0wt%, the preferred washing temperature is 40℃ to 50℃, the residence time is 0.5min to 1min, and the bath ratio is 3:1 to 5:1.
[0083] This invention limits the washing temperature to 40℃~65℃, based on the following: Conventional deep washing for zinc removal typically uses 70℃~80℃, which accelerates the decomposition of zinc xanthate in cellulose, leading to a large amount of zinc ions being released. However, within the temperature range selected in this invention, the solubility of zinc xanthate in the cortex cellulose is low, significantly slowing the outward diffusion rate of zinc ions. This allows for stable control of the residual zinc content in the fiber within the target range of 0.2wt%~5.0wt%. If the temperature is below 40℃, residual sulfuric acid and byproducts in the fiber after spinning are difficult to remove, affecting the purity of subsequent carbonization products. If the temperature is above 65℃, the zinc removal rate is too fast, making precise control within the desired range difficult.
[0084] Furthermore, the washing residence time and the liquor ratio have a synergistic effect. The residence time needs to be designed in conjunction with the actual linear speed of the industrial viscose fiber washing line to determine the length of the washing section; the liquor ratio directly affects the washing driving force. The smaller the liquor ratio, the lower the driving force, and the easier it is for zinc ions to be "locked" in the fiber skin. The larger the liquor ratio, the more thorough the removal. Thus, the amount of zinc residue can be flexibly controlled by adjusting the liquor ratio.
[0085] S2. Pre-oxidation treatment:
[0086] The zinc-containing viscose fiber obtained from S1 has a thickness ≥3mm. To reduce the risk of melt adhesion, the zinc-containing viscose fiber undergoes pre-oxidation treatment before carbonization treatment. Specifically, the zinc-containing viscose fiber is placed in an air atmosphere tube furnace and heated to 250℃ at a heating rate of 1℃ / min, and held at that temperature for 2 hours to complete the pre-oxidation treatment.
[0087] S3. Carbonization treatment:
[0088] The pre-oxidized zinc-containing viscose fiber obtained from S2 was placed in an inert atmosphere tube furnace and heated to 1300℃ at a heating rate of 5℃ / min. The temperature was held for 3 hours to complete the carbonization treatment. The inert atmosphere gas flow rate was 200 mL / min (per gram of fiber). The furnace was then allowed to cool naturally to obtain the carbonized product.
[0089] S4. Acid washing, purification, drying, and pulverization:
[0090] The carbonized product obtained from S3 was placed in 1 mol / L dilute hydrochloric acid and washed at room temperature (25°C) for 3 hours for acid purification. It was then washed with water until the washing solution was neutral to remove residual zinc species and impurities from the surface and open pores. The washing solution was filtered off, and the filter residue was dried at 80°C, ball-milled, and the powder was pulverized through a 100-mesh sieve to obtain a hard carbon anode material for sodium-ion batteries, named HC-1. Its scanning electron microscopy results are shown below. Figure 1 .
[0091] Example 2
[0092] This embodiment describes a sodium-ion battery hard carbon anode material HC-2 based on zinc-containing viscose fiber and its preparation method. The structure of this sodium-ion battery hard carbon anode material is basically the same as that in Example 1.
[0093] The preparation method of the sodium-ion battery hard carbon anode material based on zinc-containing viscose fiber in this embodiment is as follows:
[0094] S1. Preparation of zinc-containing viscose fibers:
[0095] The same wood pulp raw materials and viscose solution preparation process as in Example 1 were used. A coagulation bath was prepared, comprising: 5 g / L zinc sulfate, 100 g / L sulfuric acid, and 150 g / L sodium sulfate. The coagulation bath temperature was set at 45°C, the fiber draw ratio at 1.5, and the zinc content in the dry basis of the zinc-containing viscose fiber was controlled at 1.2 wt%.
[0096] The thin fiber bundles obtained in this embodiment are highly breathable, meaning that the zinc-containing viscose fibers are single-layer or loose thin layers with a thickness of <2mm, resulting in a low risk of melt adhesion. Therefore, the pre-oxidation treatment process is omitted.
[0097] S2. Carbonization treatment:
[0098] The zinc-containing viscose fiber obtained from S1 was placed in an argon atmosphere tube furnace and heated to 1400℃ at a heating rate of 2℃ / min. The temperature was held for 2 hours to complete the carbonization treatment. The inert atmosphere gas flow rate was 150 mL / min (per gram of fiber). The furnace was then allowed to cool naturally to obtain the carbonized product.
[0099] S3. The carbonized product obtained in S2 was subjected to the same acid washing purification, drying and pulverization treatment as in Example 1 to obtain a hard carbon anode material for sodium-ion batteries, named HC-2.
[0100] Example 3
[0101] S1. Preparation of zinc-containing viscose fibers:
[0102] The same wood pulp raw materials and viscose preparation process as in Example 1 were used. A coagulation bath was prepared, comprising: 12 g / L zinc sulfate, 120 g / L sulfuric acid, and 200 g / L sodium sulfate.
[0103] The coagulation bath temperature was set at 55℃, the fiber draw ratio was 1.0, and the zinc content in the dry basis of the zinc-containing viscose fiber was controlled at 4.0 wt%.
[0104] S2. Pre-oxidation treatment:
[0105] In this embodiment, the zinc-containing viscose fiber obtained in S1 has a thickness of ≥3mm. The zinc-containing viscose fiber is placed in an air atmosphere tube furnace and heated to 250℃ at a heating rate of 1℃ / min. The temperature is maintained for 2h to complete the pre-oxidation treatment.
[0106] S3. Carbonization treatment:
[0107] The pre-oxidized zinc-containing viscose fiber obtained from S2 was placed in a nitrogen atmosphere tube furnace and heated to 1200℃ at a heating rate of 3℃ / min. The temperature was held for 4 hours to complete the carbonization treatment. The inert atmosphere gas flow rate was 300 mL / min (per gram of fiber). The furnace was then allowed to cool naturally to obtain the carbonized product.
[0108] S4. The acid washing, purification, drying, and pulverization processes are the same as in Example 1, yielding a sodium-ion battery hard carbon anode material, named HC-3.
[0109] In other embodiments, the radial cross-sectional radius of the sodium-ion battery hard carbon anode material is R, the thickness of the skin layer is d, and the radius of the core layer is r, i.e., r = Rd. Based on the kinetic process of zinc ions diffusing from the coagulation bath to the fiber interior during wet spinning, and the corresponding dry-basis zinc content, the thickness d of the resulting skin layer is any value within the range of 5% to 25% of the radius R, such as 5%, 11%, 15%, or 25%, i.e., corresponding to d : r = 1 : 19 ~ 1 : 3.
[0110] Comparative Example 1
[0111] This comparative example describes a method for preparing hard carbon materials by carbonizing conventional zinc-containing viscose fibers after deep washing to remove zinc ions from the outer layer. The only difference from Example 1 is that the zinc ions in the fibers are removed by enhanced water washing until the dry basis zinc content is less than 0.05 wt%. The rest of the preparation method is exactly the same as that of Example 1, including the atmosphere and gas flow conditions during carbonization.
[0112] Comparative Example 2
[0113] This comparative example describes a method for preparing hard carbon materials by dezincifying viscose fibers, introducing zinc salts through impregnation with an exogenous ZnCl2 solution, and then carbonizing them. The only difference from Example 1 is that after the fibers are dezincified by enhanced water washing until the dry basis zinc content is less than 0.05wt%, they are then impregnated with a 5wt% zinc chloride aqueous solution for 24 hours to control the dry basis zinc content of the fibers to 2.5wt%. The rest of the preparation method is exactly the same as that of Example 1, including the atmosphere and gas flow conditions during the carbonization treatment.
[0114] Comparative Example 3
[0115] This comparative example is a method for preparing high-zinc-content viscose fiber and carbonizing it to prepare hard carbon material using a high-concentration zinc sulfate coagulation bath. The only difference from Example 1 is that the zinc sulfate concentration in the coagulation bath is 30 g / L, and the dry zinc content of the fiber is controlled to be 8.5 wt% after washing. The rest of the preparation method is exactly the same as that of Example 1, including the atmosphere and gas flow conditions during carbonization.
[0116] Comparative Example 4
[0117] This comparative example is a method for preparing hard carbon materials by direct carbonization using commercially available conventional viscose staple fiber as a precursor. The only difference from Example 1 is that the raw material is commercially available conventional viscose staple fiber with a dry basis zinc content of less than 0.01 wt%, and the pre-oxidation treatment step is omitted. The rest of the preparation method is exactly the same as that of Example 1, including the atmosphere and gas flow conditions during carbonization.
[0118] Comparative Example 5
[0119] This comparative example is a method for preparing zinc-free viscose fiber and carbonizing it to prepare hard carbon material without adding zinc sulfate in a coagulation bath. The only difference from Example 1 is that zinc sulfate is not added in the coagulation bath and the dry zinc content of the fiber is less than 0.001 wt%. The rest of the preparation method is exactly the same as that of Example 1, including the atmosphere and gas flow conditions during carbonization.
[0120] Comparative Example 6
[0121] This comparative example is a method for preparing cobalt-containing viscose fibers by replacing zinc sulfate with cobalt sulfate and then carbonizing them to prepare hard carbon materials. The only difference from Example 1 is that equimolar amounts of cobalt sulfate are used to replace zinc sulfate in the coagulation bath, and the total dry metal content of the fibers is 2.5 wt%. The rest of the preparation method is exactly the same as that of Example 1, including the atmosphere and gas flow conditions during the carbonization process.
[0122] Comparative Example 7
[0123] This comparative example is a method for preparing nickel-containing viscose fibers by replacing zinc sulfate with nickel sulfate and then carbonizing them to prepare hard carbon materials. The only difference from Example 1 is that equimolar amounts of nickel sulfate are used to replace zinc sulfate in the coagulation bath, and the total dry metal content of the fibers is 2.5 wt%. The rest of the preparation method is exactly the same as that of Example 1, including the atmosphere and gas flow conditions during the carbonization process.
[0124] Comparative Example 8
[0125] This comparative example is a method for preparing hard carbon materials by introducing zinc salts through exogenous impregnation of commercially available zinc-free viscose fiber with zinc sulfate solution and then carbonizing it. The only difference from Example 1 is that the raw material is commercially available zinc-free viscose fiber. After impregnation with zinc sulfate aqueous solution at room temperature for 24 hours, the dry basis zinc content of the fiber is 2.5 wt%. The rest of the preparation method is exactly the same as that of Example 1, including the atmosphere and gas flow conditions during carbonization.
[0126] Comparative Example 9
[0127] This comparative example describes a method for preparing hard carbon materials by carbonizing viscose fibers after activating them with KOH solution. The only difference from Example 1 is the use of exogenous KOH as a pore-forming agent. Specifically, after the fibers are washed with water to remove zinc until the dry basis zinc content is less than 0.05 wt%, they are impregnated with a 20% KOH solution for 12 hours. The molar amount of potassium loaded in the fibers matches the molar amount of zinc in Example 1. The rest of the preparation method is exactly the same as that in Example 1, including the atmosphere and gas flow conditions during the carbonization process.
[0128] Comparative Example 10
[0129] This comparative example describes a method for preparing hard carbon materials by carbonizing viscose fibers after activation by phosphoric acid impregnation. The only difference from Example 1 is the use of exogenous phosphoric acid as a pore-forming agent. Specifically, after the fibers are washed with water to remove zinc until the dry basis zinc content is less than 0.05 wt%, they are impregnated with an 85% concentrated phosphoric acid aqueous solution for 12 hours. The mass ratio of fiber to pure phosphoric acid is 1:0.35. After impregnation, the fibers are dried at 110°C for 10 hours. The rest of the preparation method is exactly the same as in Example 1, including the atmosphere and gas flow conditions during carbonization.
[0130] Comparative Example 11
[0131] This comparative example is a method for preparing hard carbon materials by direct carbonization of industrial thick tow zinc-containing viscose fibers. The only difference from Example 1 is that industrial thick tow raw materials with a tow thickness of ≥5mm are selected and the pre-oxidation treatment step is omitted. The rest of the preparation method is exactly the same as that of Example 1, including the atmosphere and gas flow conditions during carbonization.
[0132] Example 4
[0133] This embodiment is a sodium-ion battery comprising a separator, a positive electrode, and a negative electrode. The specific preparation method is as follows:
[0134] The sodium-ion battery hard carbon negative electrode material HC-1 obtained in Example 1, conductive carbon black, and PVDF binder were mixed evenly in a mass ratio of 80:10:10. An appropriate amount of N-methylpyrrolidone was added and ground into a uniform slurry. The slurry was then coated onto the surface of a copper foil current collector, dried, and cut to form a negative electrode sheet.
[0135] A sodium metal sheet was used as the positive electrode, a glass fiber separator was used as the separator, and a 1 mol / L sodium hexafluorophosphate solution of ethylene carbonate / dimethyl carbonate was used as the electrolyte, wherein the volume ratio of ethylene carbonate to dimethyl carbonate was 1:1. In an argon-filled glove box, the negative electrode, separator, and positive electrode were stacked sequentially, and the electrolyte was added dropwise to fully wet the separator, thus encapsulating a CR2032 coin cell.
[0136] The assembled CR2032 button half-cell was left to stand at a constant temperature of 25℃ for 12 hours. A constant current charge-discharge test was then conducted at a current density of 20mA / g within a voltage window of 0.001V to 2V. The first discharge specific capacity and the first charge specific capacity were recorded, and the first coulombic efficiency was calculated.
[0137] The constant current charge-discharge curves of the first charge-discharge process are shown in the figure below. Figure 2 Calculations showed that the initial reversible specific capacity was over 300 mAh / g. Capacity retention after 100 cycles was tested, and the results are as follows: Figure 3 As shown, the calculated capacity retention rate after 100 cycles is 95.68%.
[0138] Effect Experiment Example
[0139] The interlayer spacing, specific surface area, and closed-cell volume of the hard carbon anode materials prepared in Examples 1-3 and Comparative Examples 1-11 were measured. Anode sheets were prepared from the hard carbon anode materials obtained in each example and comparative example according to the method in Example 4, and CR2032 coin cells were assembled. The reversible specific capacity, initial coulombic efficiency, and 100-cycle retention rate of the resulting cells were tested. The results are shown in Table 1. The performance graphs of the hard carbon materials prepared in Examples 2-3 and Comparative Examples 1-5 are shown in Table 1. Figures 4 to 10 As shown.
[0140] Table 1. Structural parameters and electrochemical performance of the hard carbon anode materials in each embodiment and comparative example.
[0141]
[0142] As shown in Table 1, in Examples 1 to 3, the appropriate primary zinc content was 1.2 wt% to 4.0 wt%. After carbonization, only the skin layer produced a large number of 0.5 to 3 nm micropores and small mesopores, which gave it a suitable specific surface area and the highest closed-pore volume. At the same time, the interlayer spacing increased, providing sufficient insertion sites and fast diffusion channels for sodium ions. The dense framework of the core layer ensured high-speed electron conduction. Therefore, the reversible specific capacity was higher, with an initial coulombic efficiency of 86.7% to 88.5% and a 100-cycle retention rate of 94.5% to 96.5%.
[0143] And combining Table 1, Figures 2 to 10 Among the comparative examples: in Comparative Examples 1, 4, and 5, water washing and zinc removal resulted in excessively low specific surface area and closed-cell volume, small interlayer spacing, and a lack of sodium storage sites, leading to significantly lower capacity and initial coulombic efficiency; in Comparative Examples 2 and 8, exogenous zinc salt impregnation was used, and in Comparative Example 3, the zinc content was as high as 8.5 wt%, causing overall etching or excessive etching of the skin layer, resulting in an artificially high specific surface area, but a decrease in closed-cell volume and pore fragmentation, disordered pore size, increased resistance to sodium ion transport, exacerbated side reactions, and a sharp drop in initial coulombic efficiency; in Comparative Examples 6 and 7, cobalt ions or nickel ions were used to replace zinc ions, and the cobalt ions or Nickel ions cannot selectively coordinate and accumulate in the fiber sheath, thus failing to form a core-shell structure and prevent gradient pore formation. This results in disordered pore sizes after carbonization, leading to electrochemical performance significantly inferior to zinc-based systems. In Comparative Example 9, KOH activation and in Comparative Example 10, phosphoric acid activation both failed to form effective closed-pore structures, and the pore size distribution was wide. In Comparative Example 11, industrial thick fiber bundles were used, and pre-oxidation treatment was omitted. In the early stage of carbonization, a large amount of zinc in the sheath was lost through volatilization, resulting in only a small number of open pores on the fiber surface. There were no sodium-storing closed pores inside, and the reversible capacity dropped significantly to 190 mAh / g. At the same time, there was no continuous and dense conductive core layer, and the cycle stability was significantly reduced.
[0144] In summary, the selective enrichment of native zinc ions in the fiber skin and the in-situ evolution mechanism from zinc ions to zinc oxide to zinc vapor directly determine the porous skin and dense core layer gradient pore structure, thereby achieving synergistic optimization of sodium storage activity and conductive framework. Exogenous zinc salt impregnation results in uniform zinc distribution throughout the fiber, and after high-temperature vaporization, all areas are simultaneously etched, forming numerous interconnected open macropores. In contrast, the native zinc from spinning is only enriched in the fiber skin region, with zinc vapor escaping unidirectionally outwards, etching to form independent closed nanopores. The core layer is unetched, preserving a complete and dense carbon framework. Therefore, the closed-pore volume of the hard carbon in this invention is significantly higher than all exogenously activated samples. The 0.5–3 nm closed pores in the skin provide a low-voltage plateau for sodium storage capacity, while the expanded carbon layer spacing provides interlayer embedding capacity in the ramp section. The dense core layer forms a continuous conductive path, reducing the overall electrode impedance and achieving a synergistic effect of high reversible capacity with excellent rate performance and cycling performance.
[0145] In other embodiments, the zinc content in the dry basis of the zinc-containing viscose fiber is not limited to the specific values given in the examples, and can be adjusted within the range of 0.2wt% to 5wt%. For example, the zinc content can also be 0.2wt%, 1.0wt%, 1.5wt%, 2.0wt%, 2.5wt%, 3.0wt%, 3.5wt%, 4.0wt%, or 5wt%. When the zinc content is low, the degree of pore formation in the skin is relatively mild, the specific surface area of the resulting hard carbon material is small, and the initial coulombic efficiency is higher; when the zinc content is high, the porosity of the skin increases, the number of sodium storage active sites increases, and the reversible specific capacity is further improved. Any value within the above-mentioned zinc content range can be achieved by adjusting the duration, temperature, and flow rate of the washing process, and all fall within the protection scope of the claims of this invention.
[0146] In other embodiments, the raw materials for the viscose stock solution are not limited to the specific types given in the examples, and can be selected from at least one of wood pulp, cotton pulp, bamboo pulp, and hemp pulp. The pulp cellulose content of the above raw materials is not less than 90%, and the degree of polymerization is 650~1200. Viscose fibers obtained from various types of cellulose pulp can achieve zinc ion cortex enrichment in the coagulation bath system of the present invention. The type of raw material does not affect the gradient pore structure and electrochemical performance, and can be flexibly selected according to the source and cost of the raw materials.
[0147] In other embodiments, the water-soluble zinc salt in the coagulation bath is not limited to zinc sulfate, but may also be at least one of zinc chloride, zinc nitrate, and zinc acetate. All of the above zinc salts can dissociate zinc ions in the coagulation bath and diffuse into the fiber cortex region for enrichment during spinning. Among these, zinc sulfate is the most commonly used coagulation bath component in industrial applications, being widely available and inexpensive, and is therefore a preferred option.
[0148] In other embodiments, the concentrations of the components in the coagulation bath can be adjusted within the following ranges: zinc sulfate 5-12 g / L, sulfuric acid 90-120 g / L, and sodium sulfate 150-250 g / L. For example, the zinc sulfate concentration can be 5 g / L, 7 g / L, 8 g / L, 9 g / L, 10 g / L, or 12 g / L; the sulfuric acid concentration can be 90 g / L, 100 g / L, 105 g / L, 110 g / L, or 120 g / L; and the sodium sulfate concentration can be 150 g / L, 170 g / L, 180 g / L, 190 g / L, 200 g / L, 210 g / L, 220 g / L, 230 g / L, or 250 g / L. The concentrations of the above components within the stated range work synergistically to ensure stable spinning and achieve zinc ion enrichment in the cortex.
[0149] In other embodiments, the coagulation bath temperature can be adjusted within the range of 40~60℃, and the fiber draw ratio can be adjusted within the range of 1.0~1.5. For example, the coagulation bath temperature can be 40℃, 45℃, 48℃, 50℃, 52℃, 55℃, or 60℃; the draw ratio can be 1.0, 1.1, 1.2, 1.3, 1.4, or 1.5. At lower temperatures, the fiber coagulation speed is moderate, and the zinc ion cortex is more fully enriched; at higher temperatures, the spinning stability is improved. Increasing the draw ratio helps the fiber molecular chain orientation and improves the fiber mechanical properties, but an excessively high draw ratio may lead to an increase in fiber breakage rate.
[0150] In other embodiments, the carbonization temperature can be adjusted within the range of 1000~1600℃, and the holding time can be adjusted within the range of 1~5h. For example, the carbonization temperature can be 1000℃, 1100℃, 1150℃, 1200℃, 1250℃, 1300℃, 1350℃, 1400℃, 1450℃, 1500℃, or 1600℃; the holding time can be 1h, 2h, 2.5h, 3h, 3.5h, 4h, or 5h. When the carbonization temperature is lower, the interlayer spacing of the resulting hard carbon material is larger, but the degree of graphitization is lower, and the conductivity decreases; when the carbonization temperature is higher, the carbon layer arrangement tends to be more ordered, and the conductivity is improved, but the interlayer spacing may decrease. The carbonization heating rate can be adjusted within the range of 1~10℃ / min, for example, 1℃ / min, 3℃ / min, 4℃ / min, 5℃ / min, 6℃ / min, 7℃ / min, 8℃ / min, or 10℃ / min. When the heating rate is slower, the heat distribution inside the fiber is more uniform and the pore structure is more fully developed; when the heating rate is faster, the production efficiency is improved.
[0151] In other embodiments, the acid concentration used for acid washing and purification can be adjusted within the range of 0.5~2 mol / L, and the washing time can be adjusted within the range of 2~6 h. For example, the acid concentration can be 0.5 mol / L, 1 mol / L, 1.2 mol / L, 1.5 mol / L, or 2 mol / L; the washing time can be 2 h, 3 h, 3.5 h, 4 h, 4.5 h, 6 h, or 5.5 h. The higher the acid concentration and the longer the washing time, the more thoroughly residual zinc species and impurities are removed, but excessively long washing times may cause some degree of erosion to the carbon framework. After acid washing, the material is washed with water until the washing solution is neutral, and the drying temperature can be adjusted within the range of 80~120℃, for example, 80℃, 90℃, 95℃, 100℃, 105℃, 110℃, or 120℃. The above adjustments to the acid washing, water washing, and drying conditions do not change the gradient pore structure characteristics of the hard carbon material of the present invention.
[0152] In other embodiments, when the thickness of the zinc-containing viscose fiber is large, a pre-oxidation treatment can be performed before carbonization. The heating rate of the pre-oxidation treatment can be adjusted within the range of 0.5~2℃ / min, the pre-oxidation temperature can be adjusted within the range of 200~300℃, and the holding time can be adjusted within the range of 1~3h. For example, the heating rate can be 0.5℃ / min, 1.0℃ / min, 1.2℃ / min, 1.5℃ / min, or 2℃ / min; the pre-oxidation temperature can be 200℃, 220℃, 230℃, 240℃, 250℃, 260℃, 270℃, 280℃, or 300℃; and the holding time can be 1h, 1.5h, 1.8h, 2h, 2.2h, 2.5h, or 3h. The pre-oxidation treatment is carried out in an air atmosphere, causing thermal oxidative cross-linking of the cellulose molecular chains, improving the thermal stability of the fiber, and preventing the surface layer from melting and sticking together during the carbonization heating process. For thin-layer fiber bundles, sufficient air permeability and low risk of melt adhesion mean that the pre-oxidation process can be omitted. The aforementioned pre-oxidation conditions are matched with the thickness and stacking density of the fiber bundles and can be selected and adjusted according to actual production conditions, all of which fall within the protection scope of the claims of this invention.
[0153] Based on the disclosure of this invention, those skilled in the art can make equivalent modifications or adaptive adjustments to similar solutions within the scope of the claims. If the modified or adjusted solution includes all the technical features described in the claims, it falls within the protection scope of this invention. It should be specifically noted that the materials involved in the embodiments are all commercially available products or prepared using methods known in the art; the content of these embodiments is not intended to limit the scope of protection of the claims.
Claims
1. A sodium-ion battery hard carbon anode material based on a viscose fiber containing zinc, characterized by The sodium-ion battery hard carbon anode material has a skin-core structure, with the skin layer being a porous layer and the core layer being a dense layer with pores. The porosity gradually decreases from the skin layer to the core layer, forming a pore gradient distribution structure. The pores in the core-sheath structure are formed when zinc ions in zinc-containing viscose fibers are converted into metallic zinc vapor through zinc oxide intermediate state and escape. The zinc content in the dry basis of the zinc-containing viscose fiber is 0.2wt% to 5wt%; The thickness of the skin layer accounts for 5% to 25% of the cross-sectional radius of the sodium-ion battery hard carbon anode material.
2. The sodium-ion battery hard carbon anode material based on viscose fiber containing zinc according to claim 1, characterized in that, The zinc-containing viscose fiber is obtained by wet spinning from viscose solution; The coagulation bath of the wet spinning process contains water-soluble zinc salts, and zinc ions diffuse into the viscose fibers during the coagulation and molding of the viscose solution.
3. A hard carbon anode material for sodium-ion batteries based on zinc-containing viscose fiber according to claim 1 or 2, characterized in that, The raw material for the viscose solution is at least one of wood pulp, cotton pulp, bamboo pulp, and hemp pulp; the pulp cellulose content of the raw material is ≥90%, and the degree of polymerization is 650–1200; and / or The water-soluble zinc salt is at least one of zinc sulfate, zinc chloride, zinc nitrate, and zinc acetate.
4. The sodium-ion battery hard carbon anode material based on zinc-containing viscose fiber according to claim 3, characterized in that, The coagulation bath comprises: zinc sulfate 5-12 g / L, sulfuric acid 90-120 g / L, and sodium sulfate 150-250 g / L.
5. A method for preparing a sodium-ion battery hard carbon anode material based on zinc-containing viscose fiber as described in any one of claims 1 to 4, characterized in that, This includes the following steps performed sequentially: The zinc-containing viscose fiber was placed in an inert atmosphere and heated to 1000-1600℃ for 1-5 hours to complete the carbonization treatment. After natural cooling, the carbonized product was obtained. The obtained carbonized products were purified by acid washing, dried and pulverized to obtain hard carbon anode material for sodium-ion batteries.
6. The method for preparing the hard carbon anode material for sodium-ion batteries based on zinc-containing viscose fiber according to claim 5, characterized in that, When preparing the zinc-containing viscose fiber, the coagulation bath temperature is 40-60℃ and the fiber draw ratio is 1-1.
5.
7. The method for preparing the hard carbon anode material for sodium-ion batteries based on zinc-containing viscose fiber according to claim 5 or 6, characterized in that, The heating rate for carbonization is 1–10 °C / min; and / or Acid washing purification involves washing with 0.5–2 mol / L dilute hydrochloric acid or dilute sulfuric acid at room temperature with stirring for 2–6 hours, followed by washing with water until the washing solution is neutral; and / or Drying is carried out at 80-120℃.
8. The method for preparing the sodium-ion battery hard carbon anode material based on zinc-containing viscose fiber according to claim 7, characterized in that, When the thickness of the zinc-containing viscose fiber is ≥3mm, the zinc-containing viscose fiber is subjected to pre-oxidation treatment and then carbonization treatment. The pre-oxidation treatment involves placing the zinc-containing viscose fiber in an air atmosphere and heating it to 200-300°C at a rate of 0.5-2°C / min, and holding it at that temperature for 1-3 hours.
9. A sodium-ion battery, characterized in that, It includes a separator, a positive electrode, and a negative electrode. The negative electrode is prepared by uniformly mixing the sodium-ion battery hard carbon negative electrode material based on zinc-containing viscose fiber as described in any one of claims 1 to 4, conductive carbon black, and a binder, and coating it onto a current collector.
10. The application of the method for preparing the sodium-ion battery hard carbon anode material based on zinc-containing viscose fiber as described in any one of claims 5 to 8 in the preparation of sodium-ion batteries.
Citation Information
Patent Citations
Hard carbon negative electrode material, preparation method thereof, negative electrode and battery
CN119735195B