Silicon-carbon composite negative electrode material, and preparation method and application thereof

By using silicon waste from retired photovoltaic modules and waste plastics to prepare silicon-carbon composite anode materials, the problems of volume expansion and poor conductivity of silicon-based anode materials have been solved, enabling high-performance and low-cost lithium battery applications and possessing industrialization potential.

CN123162160APending Publication Date: 2026-11-24TONGJI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611321020.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-28
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing technologies cannot simultaneously solve the problems of volume expansion, poor conductivity, and weak interfacial bonding of silicon-based anode materials, and traditional composite structures are prone to failure during long-term cycling, leading to a decline in battery performance.

Method used

Using silicon waste from retired photovoltaic modules and waste plastics as raw materials, carbon nanotubes are grown in situ under metal salt catalysis, combined with a segmented carbon deposition process to form Si-C chemical bonds and a three-dimensional conductive network, thus constructing a stable silicon-carbon composite anode material.

Benefits of technology

A silicon-carbon composite anode material with high initial coulombic efficiency, high reversible specific capacity and long cycle life has been developed, which reduces raw material costs, realizes the high-value utilization of solid waste, and conforms to the concept of green and low-carbon development.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123162160A_ABST
    Figure CN123162160A_ABST
Patent Text Reader

Abstract

This invention relates to the fields of new energy materials and solid waste resource utilization, and discloses a silicon-carbon composite anode material, its preparation method, and its application. The silicon-carbon composite anode material comprises silicon particles, a surface oxide layer of SiOx, metal particles, and in-situ grown carbon nanotubes, with a carbon outer shell. The silicon particles are derived from silicon waste from decommissioned photovoltaic modules, and the carbon nanotubes are formed by the pyrolysis growth of waste plastics catalyzed by the metal particles. This invention constructs a composite anode material possessing both strong Si-C chemical bonding and a three-dimensional conductive network, solving the problems of large volume expansion and poor conductivity in silicon-based anodes. It achieves high-value utilization of dual-source solid waste and provides a practical technical path for the green industrialization of high-performance, low-cost silicon-carbon anodes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the fields of new energy materials and solid waste resource utilization technology, specifically to a silicon-carbon composite anode material and its preparation method and application. Background Technology

[0002] The global energy structure is rapidly transitioning to renewable energy, with global cumulative installed photovoltaic (PV) capacity increasing dramatically from 1.4 TW in 2023 to over 2.2 TW by the end of 2024, and new PV systems exceeding 800 GW in operation. PV solar modules have a lifespan of approximately 20 to 30 years, generating a large amount of decommissioned silicon waste. Due to the potentially complex and energy-intensive manufacturing processes, solar-grade silicon wafers remain the most valuable component in PV modules. Directly discharging PV silicon waste into the environment not only causes pollution but also results in significant secondary resource waste. Therefore, the recycling and high-value utilization of silicon waste from decommissioned PV modules is urgently needed. Considering the low cost of the waste and the relatively relaxed purity requirements for lithium-ion battery silicon anodes (compared to 6N solar silicon requirements), the direct one-step preparation of silicon nanomaterials from decommissioned PV module silicon waste and their application in lithium-ion battery anodes has attracted considerable market attention. However, a series of problems caused by the volume expansion and poor conductivity of silicon anode materials have become the main challenges facing current research and application. Carbon's good electrical conductivity can effectively improve the electronic conductivity of silicon, prevent excessive formation of the SEI layer, and provide mechanical support to accommodate silicon volume changes during cycling. Therefore, carbon coating design for silicon-based anode materials is a widely adopted strategy to enhance battery performance.

[0003] Plastics are among the most important chemicals that have changed daily life. Due to their high carbon content, well-defined composition, and controllable carbonization process, waste plastics hold immense potential for conversion into carbon resources. Pyrolysis is an effective method for thermally degrading polymers into smaller molecules, and catalytic pyrolysis can lower the energy barrier and cost of waste plastic decomposition, bringing more possibilities for the resource recovery of valuable carbon nanomaterials. Existing carbon composite technologies for lithium-ion batteries all have significant limitations. For example, while simple physical mixing is convenient, the bonding force between carbon materials (such as carbon nanotubes and graphene) and silicon particles is weak, failing to form effective binding during cycling, leading to easy failure of the buffer layer, and the carbon materials are prone to agglomeration and poor dispersibility. While chemical vapor deposition for external carbon coating can alleviate expansion to some extent, the interfacial bonding force between the coating layer and silicon is limited, making it prone to cracking under long-term drastic volume changes, leading to side reactions caused by silicon contacting the electrolyte.

[0004] In summary, there is a clear technological gap in the current silicon-carbon anode field: there is an urgent need for an innovative solution that can achieve strong interfacial bonding, a stable three-dimensional conductive network, efficient expansion management, and low cost and environmental friendliness. Summary of the Invention

[0005] The purpose of this invention is to overcome the problems of volume expansion, poor conductivity and weak interfacial bonding of silicon-based materials in the prior art, and to achieve low-cost green manufacturing.

[0006] To achieve the above objectives, the first aspect of the present invention provides a silicon-carbon composite anode material comprising silicon particles, a surface oxide layer SiOx, metal particles, and in-situ grown carbon nanotubes, with a carbon layer as the outer shell. The silicon particles are derived from silicon waste from decommissioned photovoltaic modules, and the carbon nanotubes are formed by the pyrolysis growth of waste plastics under the catalysis of the metal particles. Si-C chemical bonds are formed between the silicon particles and the carbon layer, as well as between the silicon particles and the carbon nanotubes. The silicon-carbon composite anode material is prepared by the following method: purified nano-silicon powder, metal salt and waste plastic are reacted in a solvent, and after removing the solvent, a mixture I is obtained. The mixture I is subjected to segmented carbon deposition under a protective atmosphere; wherein, the carbon nanotubes are grown in situ inside the mixture I.

[0007] A second aspect of the present invention provides a method for preparing the silicon-carbon composite anode material described in the first aspect, the method comprising the following steps: (1) In the presence of a solvent, purified nano-silicon powder, metal salt and waste plastic were reacted in contact, and after removing the solvent, mixture I was obtained; The purified nano-silicon powder is obtained by sequentially purifying decommissioned photovoltaic module silicon waste through ball milling and acid washing. (2) The mixture I is subjected to segmented carbon deposition under a protective atmosphere, wherein the segmented carbon deposition includes: S1: Raise the temperature to 200-400℃ at a rate of 5-20℃ / min and perform a first heat preservation treatment for 0.5-5h to preliminarily carbonize the waste plastic and form catalytic active sites with the metal particles reduced by the metal salt, thus obtaining mixture II; S2: Continue heating to 700-1000℃ at a rate of 5-20℃ / min, and perform a second heat preservation treatment for 0.5-5h to grow carbon nanotubes in the mixture II through in-situ catalytic reaction. After cooling, silicon-carbon composite anode material is obtained.

[0008] The third aspect of this invention provides the application of the silicon-carbon composite anode material described in the first aspect in the preparation of lithium-ion batteries.

[0009] Compared with existing technologies, the method provided by this invention has at least the following beneficial effects: (1) Thanks to the unique design of “SiOx oxide coating” and “in-situ carbon nanotube (CNT) growth”, this invention successfully constructed a robust three-dimensional conductive network. This network not only greatly enhances the electronic conductivity of the material and ensures excellent high-rate performance, but also, the synergistic effect of the elastic carbon nanotubes and the dense carbon shell provides an effective buffer space for the large volume expansion of silicon particles during charging and discharging, significantly inhibiting the pulverization and shedding of active materials. Furthermore, in the segmented carbon deposition process of this invention, the first heat preservation treatment is carried out at a lower temperature. While achieving pyrolysis, more importantly, a microporous structure is formed inside the solid mixture, providing a gas diffusion channel for the CNT growth in the second heat preservation treatment at a higher temperature. This prevents the dense plastic from completely sealing the silicon surface after carbonization, thereby avoiding the deactivation of silicon active materials. Metal salts play multiple key roles in this process: the metal particles generated by their reduction serve as catalytic active sites to drive the in-situ growth of CNTs and also act as the skeleton nodes for constructing the three-dimensional conductive network. Through this unique structural design and composition control, the preparation of high-performance silicon-carbon composite anodes is achieved in one step. This structural advantage directly translates into a significant improvement in battery performance: the material exhibits high initial coulombic efficiency, high reversible specific capacity, and maintains extremely high capacity retention even after long cycles.

[0010] (2) This invention first constructs a tight contact interface between silicon, catalyst, and carbon source through a liquid-phase mixing and drying process, ensuring the in-situ directional growth of CNTs on the surface of silicon particles, rather than the disordered deposition in the traditional vapor deposition process. Then, a segmented carbon deposition process is used to promote a strong interfacial bond between silicon and carbon, while simultaneously growing carbon nanotubes in situ. This is far superior to simple physical mixing or external coating, and can effectively resist interfacial stress during cycling, prevent carbon layer cracking, thereby reducing the direct contact between silicon and electrolyte, stabilizing the SEI film, and fundamentally improving the structural integrity and cycle life of the electrode.

[0011] (3) The core innovation of this invention lies in transforming silicon waste and waste plastics from retired photovoltaic modules into high-value-added battery materials. This not only significantly reduces raw material costs and eliminates dependence on high-purity chemical raw materials, but also realizes the high-value resource utilization of solid waste, perfectly aligning with the concept of green, low-carbon, and sustainable development, and has significant environmental and social benefits.

[0012] (4) The preparation method provided by the present invention has a clear process and controllable parameters. From raw material pretreatment to final segmented carbon deposition, the entire process is easy to achieve kilogram-level stable production and has great potential to move from laboratory to industrial application. It provides a practical and feasible technical path for the commercialization of high-performance, low-cost silicon-carbon anodes. Attached Figure Description

[0013] Figure 1 This is a SEM image of the silicon-carbon composite anode material P1 prepared in Example 1 of this invention; Figure 2 This is a TEM image of the silicon-carbon composite anode material P1 prepared in Example 1 of this invention; Figure 3 This is a TEM-Mapping image of the silicon-carbon composite anode material P1 prepared in Example 1 of this invention; Figure 4 This is the constant current charge-discharge curve of P1 prepared in Example 1 of the present invention; Figure 5 This is a SEM image of the silicon-carbon composite anode material P2 prepared in Example 2 of this invention; Figure 6 This is a half-cell cycle performance diagram of the silicon-carbon composite anode material P3 prepared in Example 3 of the present invention; Figure 7 This is a rate performance diagram of the silicon-carbon composite anode material P3 prepared in Example 3 of the present invention; Figure 8 These are the dq / dv curves of silicon-carbon composite anode materials P1 and DP1 prepared in Example 1 of this invention; Figure 9 This is a half-cell cycle performance diagram of silicon-carbon composite anode materials P2 and DP2 prepared in Example 2 of this invention; Figure 10 This is a half-cell cycle performance diagram of the silicon-carbon composite anode materials P3 and DP3 prepared in Example 3 of this invention. Detailed Implementation

[0014] The endpoints and any values ​​of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of the various ranges, the endpoint values ​​of the various ranges and individual point values, and individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.

[0015] As mentioned above, the first aspect of the present invention provides a silicon-carbon composite anode material comprising silicon particles, a surface oxide layer SiOx, metal particles and in-situ grown carbon nanotubes, with a carbon layer as the outer shell. The silicon particles are derived from silicon waste from decommissioned photovoltaic modules, and the carbon nanotubes are formed by the pyrolysis growth of waste plastics under the catalysis of the metal particles. Si-C chemical bonds are formed between the silicon particles and the carbon layer, as well as between the silicon particles and the carbon nanotubes. The silicon-carbon composite anode material is prepared by the following method: purified nano-silicon powder, metal salt and waste plastic are reacted in a solvent, and after removing the solvent, a mixture I is obtained. The mixture I is subjected to segmented carbon deposition under a protective atmosphere; wherein, the carbon nanotubes are grown in situ inside the mixture I.

[0016] Preferably, the average length of the carbon nanotubes is 1-5 μm.

[0017] In a preferred embodiment, the metal particles are selected from at least one of copper, iron, nickel, cobalt, and silver.

[0018] In a preferred embodiment, the waste plastic is selected from at least one of low-density polyethylene, high-density polyethylene, polypropylene, polyvinyl chloride, polystyrene, and polyethylene terephthalate.

[0019] As described above, a second aspect of the present invention provides a method for preparing the silicon-carbon composite anode material described in the first aspect, the method comprising the following steps: (1) In the presence of a solvent, purified nano-silicon powder, metal salt and waste plastic were reacted in contact, and after removing the solvent, mixture I was obtained; The purified nano-silicon powder is obtained by sequentially purifying decommissioned photovoltaic module silicon waste through ball milling and acid washing. (2) The mixture I is subjected to segmented carbon deposition under a protective atmosphere, wherein the segmented carbon deposition includes: S1: Raise the temperature to 200-400℃ at a rate of 5-20℃ / min and perform a first heat preservation treatment for 0.5-5h to preliminarily carbonize the waste plastic and form catalytic active sites with the metal particles reduced by the metal salt, thus obtaining mixture II; S2: Continue heating to 700-1000℃ at a rate of 5-20℃ / min, and perform a second heat preservation treatment for 0.5-5h to grow carbon nanotubes in the mixture II through in-situ catalytic reaction. After cooling, silicon-carbon composite anode material is obtained.

[0020] Preferably, in step (1), the solvent is at least one of ethanol, methanol, propanol, butanol, ethylene glycol, propylene glycol, allyl alcohol, and vinyl alcohol.

[0021] Preferably, in step (1), the solvent removal is carried out by heating in a water bath at a temperature of 60-80°C for 1-5 hours.

[0022] Preferably, in step (1), the contact reaction is carried out under water bath conditions, and at least the following conditions are met: temperature is 60-80℃, and time is 1-5h. Under this preferred condition, the SiOx layer on the surface of the nano-silicon powder can achieve molecular-scale contact with metal salt ions and waste plastic organic chains in the solvent, which is more conducive to the metal catalyst particles being locked on the surface or in the pores of the silicon particles.

[0023] In a preferred embodiment, in step (1), the purified nano-silicon powder is obtained by a method comprising the following steps: first, crushing and ball milling the silicon waste from retired photovoltaic modules to obtain coarse silicon powder with an average volume diameter of 1-3 μm; then, wet milling using a sand mill for 0.5-2 h to obtain fine silicon powder with an average volume diameter of 150-200 nm. Under stirring conditions, the fine silicon powder is sequentially treated with an ethanol solution of hydrofluoric acid for 30-80 min, then treated with a hydrochloric acid solution for 30-80 min. After solid-liquid separation, it is washed with deionized water until neutral, and finally dried under vacuum at 80°C for 5 h to obtain the purified nano-silicon powder.

[0024] More preferably, the stirring speed is 500-800 rpm.

[0025] Preferably, the solid-liquid ratio of the wet milling is 1g:100mL.

[0026] Preferably, in the ethanol solution of hydrofluoric acid, the concentration of hydrofluoric acid is 1-5 mol / L.

[0027] Preferably, the concentration of the hydrochloric acid solution is 1-5 mol / L.

[0028] In a preferred embodiment, in step (1), the metal salt is selected from at least one of chloride, nitrate, sulfate and acetate.

[0029] More preferably, in step (1), the metal salt is selected from at least one of chloride, nitrate, sulfate and acetate salts that can provide at least one of copper, iron, nickel, cobalt and silver.

[0030] More preferably, the metal salt is selected from at least one of chloride, nitrate, sulfate and acetate salts that can provide copper and / or nickel.

[0031] Preferably, the method of the present invention further includes, in step (1), the waste plastic is first pretreated to obtain purified waste plastic carbon powder, which is then applied to the contact reaction.

[0032] More preferably, the pretreatment includes: cutting, crushing, and ball milling waste plastics to obtain coarse carbon powder, washing them sequentially with deionized water and ethanol to obtain purified waste plastic carbon powder with an average volume diameter of 400-800 nm.

[0033] According to a preferred embodiment, in step (1), the mass ratio of the purified nano-silicon powder, the metal salt and the waste plastic is 8:1:1-3.

[0034] Preferably, in step (1), the total mass ratio of the purified nano-silicon powder, the metal salt, and the waste plastic to the volume ratio of the solvent is 1:50.

[0035] It should be noted that, in this invention, the total mass of the purified nano-silicon powder, the metal salt, and the waste plastic is expressed in g, and the volume of the solvent is expressed in mL.

[0036] Preferably, in step (2), the segmented carbon deposition is carried out in a tubular furnace.

[0037] Preferably, in step (2), the protective atmosphere is a mixture of argon and hydrogen, wherein the hydrogen content is 5-20 vol.

[0038] In a preferred embodiment, in step S2, the cooling rate is 5-20℃ / min.

[0039] As previously stated, the third aspect of this invention provides the application of the silicon-carbon composite anode material described in the first aspect in the preparation of lithium-ion batteries.

[0040] The present invention will be described in detail below through examples. Unless otherwise specified, the raw materials used are all commercially available products.

[0041] Waste plastics: Low-density polyethylene with an average volume diameter of 2-3 μm, derived from recycled waste plastic packaging materials; Purified waste plastic toner: The waste plastic is pretreated by cutting, crushing and ball milling to obtain coarse toner, which is then washed with deionized water and ethanol in sequence to obtain purified waste plastic toner with an average volume diameter of 600 nm.

[0042] Purified nano-silicon powder: Silicon waste from decommissioned photovoltaic modules (derived from crystalline silicon cell waste separated after dismantling decommissioned crystalline silicon photovoltaic modules) was first crushed and ball-milled to obtain coarse silicon powder with an average volume diameter of 1 μm. Then, it was wet-milled for 2.0 h using ethanol at a solid-liquid ratio of 1 g:100 mL in a sand mill to obtain fine silicon powder with an average volume diameter of 200 nm. Under stirring at 700 rpm, the fine silicon powder was sequentially treated with a 1 mol / L hydrofluoric acid ethanol solution for 80 min, followed by a 1.5 mol / L hydrochloric acid solution for 80 min. After solid-liquid separation, it was washed with deionized water until neutral, and finally vacuum-dried at 80℃ for 5 h to obtain purified nano-silicon powder.

[0043] Example 1: This embodiment illustrates that the silicon-carbon composite anode material provided by the present invention is prepared by a method including the following steps: (1) In the presence of a solvent, purified nano-silicon powder, metal salt (NiCl2·6H2O) and purified waste plastic carbon powder are subjected to a contact reaction, specifically including: 250 mL of solvent (ethanol), 4 g of purified nano-silicon powder, 1 g of purified waste plastic carbon powder, and 0.5 g of metal salt (NiCl2·6H2O) were placed in a water bath and heated at 80 °C for 3 h for contact reaction. The water bath was then heated at 80 °C for another 2 h until the solvent was completely removed, resulting in mixture I.

[0044] (2) Mixture I was placed in a tube furnace and subjected to segmented carbon deposition under an Ar-H2 atmosphere (H2 content of 10 vol%, gas flow rate of 200 mL / min), specifically including: S1: Raise the temperature to 200℃ at a rate of 5℃ / min and perform a first heat preservation treatment for 2 hours to preliminarily carbonize the waste plastic and form catalytic active sites with the metal particles reduced by the metal salt to obtain mixture II. S2: Continue heating to 800℃ at a rate of 5℃ / min, perform a second heat treatment for 3 hours, and then cool down (at a rate of 5℃ / min) to grow carbon nanotubes in the mixture II through in-situ catalytic reaction, thereby obtaining a silicon-carbon composite anode material, named P1.

[0045] P1 was analyzed by scanning electron microscopy and transmission electron microscopy. Figure 1 The scanning electron microscope (SEM) image of P1 is shown. Figure 2 The transmission electron microscopy (TEM) image of P1 is shown. It can be seen that the in-situ grown carbon nanotubes can be uniformly distributed inside or on the surface of silicon materials to form a good conductive network. The segmented carbon deposition in the tube furnace achieves a more uniform distribution of carbon nanotubes in the composite material, which is more conducive to improving the electrochemical performance of silicon-based materials.

[0046] Figure 3 The TEM-Mapping image of P1 is shown, revealing that the entire material is encapsulated in a carbon shell, confirming the uniform distribution of Si and Ni. Stable cycling of the silicon-based anode depends on the carbon coating, and high discharge capacity depends on Ni and Ag doping.

[0047] Figure 4 The constant current charge-discharge curve of P1 is shown. It can be seen from the figure that the Si / SiOx / Ni / CNTs composite material exhibits excellent initial properties, with an initial coulombic efficiency (ICE) of 91.14%.

[0048] Example 2: This embodiment uses a method similar to that of Embodiment 1, except that in step (1), the metal salt used is CuSO4; Ultimately, a silicon-carbon composite anode material was obtained and named P2.

[0049] Figure 5 The SEM image of P2 is shown. It can be seen from the image that the carbon nanotubes grown in situ in P2 can be uniformly distributed inside or on the surface of silicon material to form a good conductive network. The segmented carbon deposition in the tube furnace achieves a more uniform distribution of carbon nanotubes in the composite material, which is more conducive to improving the electrochemical performance of silicon-based materials.

[0050] Example 3: This embodiment uses a method similar to that of Embodiment 1, except that in step (1), the metal salt used is Co(NO3)2; Ultimately, a silicon-carbon composite anode material was obtained and named P3.

[0051] Figure 6 The figure shows P3 at 1.0 A·g -1 The graph shows the half-cell cycle performance at the given current density. It can be seen from the graph that after 100 cycles, P3 still maintains 637.37 mAh·g. -1 The discharge capacity has a capacity retention rate of 40%.

[0052] Figure 7 The figure shows P3 at 0.1 A·g -1 Up to 5 A·g -1 The rate performance graph shows that even at 2.0 A·g -1 Even at this time, P3 can maintain a discharge specific capacity greater than 300 mAh·g -1 Additionally, when the current density increases from 5.0 A·g -1 Reduced to 0.1 A·g -1 With a capacity retention rate of up to 90%, it highlights its outstanding rate capability.

[0053] Comparative Example 1 This comparative example was carried out using a method similar to that of Example 1. The difference was that, in step (1), an equal mass of commercially available high-purity micron-sized silicon powder (purity of 99.99%, average volume diameter of 1-2 μm, purchased from Macklin) was used instead of purified nano-sized silicon powder. Ultimately, a silicon-carbon composite anode material was obtained and named DP1.

[0054] Figure 8The dq / dv curves of P1 and DP1 are shown. The figures reveal that both P1 and DP1 materials exhibit characteristic alloying and dealloying reaction peaks of silicon in the low potential region, indicating that the lithium storage reaction mechanism of silicon is preserved after composite treatment. Compared to DP1, the redox peak intensity of the P1 composite anode material is reduced and the peak shape is broadened, indicating that its lithium insertion and delithiation reactions are distributed over a wider potential range. This phenomenon suggests that the SiOx interface layer, carbon coating layer, and carbon nanotube conductive network have a regulatory effect on the electrochemical reaction process of silicon, which is beneficial for dispersing the local reaction stress of silicon particles during charge and discharge.

[0055] Comparative Example 2 This comparative example was carried out using a method similar to that of Example 2, except that in step (2), a one-step heating process was used instead of segmented carbon deposition, specifically including: (2) Mixture I was placed in a tube furnace and heated directly to 800℃ in an Ar-H2 atmosphere (H2 content was 10 vol%, gas flow rate was 200 mL / min). The temperature was increased at a rate of 5℃ / min for a second heat preservation treatment for 3 hours. After cooling (cooling rate was 5℃ / min), silicon-carbon composite anode material was obtained and named DP2.

[0056] Figure 9 The half-cell long-cycle performance graphs of P2 and DP2 are shown. The graphs reveal that the P2 electrode exhibits significantly better cycle stability than the DP2 electrode. Although its capacity initially drops rapidly from a high value to approximately 450-500 mAh / g, it subsequently shows gradual activation, maintaining around 650-700 mAh / g after approximately 300-600 cycles, and still retaining approximately 450-500 mAh / g after 1000 cycles. In contrast, the capacity of DP2 rapidly decays to nearly 100 mAh / g within the first 100 cycles, indicating poor structural stability and conductive contact. The coulombic efficiency of the P2 electrode remains relatively stable at 99%-100% after the initial cycling, demonstrating that the CNT conductive network not only improves electron transport and mitigates volume changes in silicon-based materials during cycling, but also promotes the gradual and full participation of active materials in the reaction, thereby significantly improving the electrode's reversible capacity and cycle performance.

[0057] Comparative Example 3 This comparative example was carried out using a method similar to that of Example 3, except that in step (1), coarse silicon powder with an average volume diameter of 2 μm of equal mass was used instead of purified nano silicon powder. Ultimately, a silicon-carbon composite anode material was obtained and named DP3.

[0058] Figure 10The half-cell cycling performance graphs for P3 and DP3 are shown. The graphs reveal that in the first 100 cycles, the P3 electrode exhibits higher capacity and more pronounced activation characteristics. Its capacity initially decreases from approximately 550-600 mAh / g to approximately 420 mAh / g, then gradually recovers, reaching approximately 750-800 mAh / g around cycle 100. In contrast, the capacity of DP3 remains relatively stable at approximately 400-450 mAh / g, showing a smaller increase. These results demonstrate that P3 exhibits better reaction reversibility and long-term cycling reliability, highlighting the significant role of nanoscale silicon particles in electrochemical performance.

[0059] The results above demonstrate that this invention, through the synergistic effect of the highly active surface of decommissioned photovoltaic silicon waste, specific impurities, carbon sources from waste plastic pyrolysis, and metal catalysts, combined with a segmented carbon deposition process, successfully constructs a composite material possessing a robust Si-C bond interface, a three-dimensional conductive network, and a buffer structure. This fundamentally solves the problems of volume expansion and poor conductivity in silicon anodes. This solution not only achieves high capacity, high initial efficiency, and long cycle life in silicon-carbon anode materials but also enables low-cost, green, and sustainable manufacturing through high-value reuse of solid waste, demonstrating significant prospects for industrial application.

[0060] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.

Claims

1. A silicon-carbon composite anode material, characterized in that, The silicon-carbon composite anode material comprises silicon particles, a surface oxide layer of SiOx, metal particles, and in-situ grown carbon nanotubes, with a carbon outer shell. The silicon particles are derived from silicon waste from decommissioned photovoltaic modules, and the carbon nanotubes are formed by the pyrolysis growth of waste plastics under the catalysis of the metal particles. Si-C chemical bonds are formed between the silicon particles and the carbon layer, as well as between the silicon particles and the carbon nanotubes. The silicon-carbon composite anode material is prepared by the following method: purified nano-silicon powder, metal salt and waste plastic are reacted in a solvent, and after removing the solvent, a mixture I is obtained. The mixture I is subjected to segmented carbon deposition under a protective atmosphere; wherein, the carbon nanotubes are grown in situ inside the mixture I.

2. The silicon-carbon composite anode material according to claim 1, characterized in that, The metal particles are selected from at least one of copper, iron, nickel, cobalt and silver.

3. The silicon-carbon composite anode material according to claim 1 or 2, characterized in that... The waste plastics are selected from at least one of low-density polyethylene, high-density polyethylene, polypropylene, polyvinyl chloride, polystyrene, and polyethylene terephthalate.

4. A method for preparing the silicon-carbon composite anode material as described in any one of claims 1-3, characterized in that, Includes the following steps: (1) In the presence of a solvent, purified nano-silicon powder, metal salt and waste plastic were reacted in contact, and after removing the solvent, mixture I was obtained; The purified nano-silicon powder is obtained by sequentially purifying decommissioned photovoltaic module silicon waste through ball milling and acid washing. (2) The mixture I is subjected to segmented carbon deposition under a protective atmosphere, wherein the segmented carbon deposition includes: S1: Raise the temperature to 200-400℃ at a rate of 5-20℃ / min and perform a first heat preservation treatment for 0.5-5h to preliminarily carbonize the waste plastic and form catalytic active sites with the metal particles reduced by the metal salt, thus obtaining mixture II; S2: Continue heating to 700-1000℃ at a rate of 5-20℃ / min, and perform a second heat preservation treatment for 0.5-5h to grow carbon nanotubes in the mixture II through in-situ catalytic reaction. After cooling, silicon-carbon composite anode material is obtained.

5. The method according to claim 4, characterized in that, The purified nano-silicon powder is obtained by a method comprising the following steps: First, silicon waste from decommissioned photovoltaic modules is crushed and ball-milled to obtain coarse silicon powder with an average volume diameter of 1-3 μm. Then, it is wet-milled using a sand mill for 0.5-2 hours to obtain fine silicon powder with an average volume diameter of 150-200 nm. Under stirring conditions, the fine silicon powder is sequentially treated with an ethanol solution of hydrofluoric acid for 30-80 minutes, followed by treatment with a hydrochloric acid solution for 30-80 minutes. After solid-liquid separation, it is washed with deionized water until neutral, and finally dried under vacuum at 80°C for 5 hours to obtain the purified nano-silicon powder.

6. The method according to claim 4 or 5, characterized in that, In step (1), the metal salt is selected from at least one of chloride, nitrate, sulfate and acetate.

7. The method according to claim 4 or 5, characterized in that, In step (1), the mass ratio of the purified nano-silicon powder, the metal salt and the waste plastic is 8:1:1-3.

8. The method according to claim 4 or 5, characterized in that, In step S2, the cooling rate is 5-20℃ / min.

9. The application of the silicon-carbon composite anode material according to any one of claims 1-3 in the preparation of lithium-ion batteries.