A method for low-temperature rapid synthesis of MOF structure modified lithium iron phosphate cathode material by microwave hydrothermal method
The rapid synthesis of MOF-structured modified lithium iron phosphate cathode material via microwave hydrothermal method solves the problem of insufficient energy density of lithium iron phosphate material under high voltage and high discharge rate, achieving high real density and low resistivity, simplifying the preparation process, and improving the electrochemical performance and safety of the battery.
Patent Information
- Application Number
- CN202611387604.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-08
- Publication Date
- 2026-11-24
AI Technical Summary
Existing lithium iron phosphate cathode materials have low electronic conductivity and lithium-ion diffusion rate, resulting in a sharp decrease in energy density under high voltage and high discharge rate, insufficient compaction density, complex preparation process and high energy consumption, which makes it difficult to meet the needs of electric vehicles.
MOF-structured modified lithium iron phosphate cathode material was rapidly synthesized at low temperature using a microwave hydrothermal method. Lithium carbonate, ferrous sulfate, and phosphoric acid were mixed in a high-pressure reactor in a one-pot process. After adjusting the pH with ascorbic acid, the mixture was microwave-heated. Subsequently, chromium sulfate and 2-aminoterephthalic acid were added and microwave-heated again. The mixture was then filtered, washed, and dried to form a Cr-N co-doped MOF structure.
It improves the compaction density and electronic conductivity of the material, shortens the preparation time, reduces the resistivity, and enhances the electrochemical performance and safety of the material, making it suitable for use under high compaction density.
Smart Images

Figure CN123162162A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of battery cathode material technology. Specifically, this invention relates to a method for preparing MOF-structured modified lithium iron phosphate cathode material by microwave hydrothermal method at low temperature and rapid synthesis. Background Technology
[0002] The biggest drawback of lithium iron phosphate (LFP) cathode materials is their relatively low electronic conductivity (~10). -9 The low compressibility (S / cm) and lithium-ion diffusion rate of lithium iron phosphate (LFP) put it at a disadvantage in competition with ternary lithium batteries, especially at high voltage and high discharge rates (10C), where its energy density drops sharply (≤100mAh / g), and its actual capacity can only reach about 58% of the theoretical capacity. While some literature reports the existence of lithium iron phosphate cathode materials for high-rate applications, their compaction density is generally around 2.20 g / cm³. 3 This is uneconomical and undesirable in power electric vehicle batteries. Currently, the mainstream power batteries on the market are mainly third- and fourth-generation batteries, which have higher standards for compaction density and electrochemical performance. Especially when the compaction density is ≥2.60 g / cm³... 3 The challenge lies in achieving ultra-long battery life with even faster charging speeds, comparable to gasoline refueling—specifically, ≥135mAh / g at 10C charging—which would completely replace gasoline vehicles. Simultaneously, extremely low resistivity is required at the high charging voltage (3.85V) to prevent the battery pack from overheating and catching fire due to rapid charging. Furthermore, the manufacturing process of lithium iron phosphate is complex and cumbersome, typically requiring 2-3 days, significantly reducing production capacity and increasing energy consumption, which is detrimental to current market competitiveness. Summary of the Invention
[0003] One object of the present invention is to solve at least the above-mentioned problems and / or defects, and to provide at least the advantages described below.
[0004] To achieve these objectives and other advantages of the present invention, a method for rapidly synthesizing MOF-structured modified lithium iron phosphate cathode materials at low temperatures using a microwave hydrothermal method is provided, comprising the following steps: Step 1: Add lithium carbonate, ferrous sulfate and phosphoric acid to a high-pressure reactor containing solvent and mix. Then add ascorbic acid, adjust the pH with ammonia, stir and mix under an inert atmosphere, and then microwave heat to obtain the reaction solution. Step 2: After cooling the reaction solution to room temperature, add chromium sulfate, 2-aminoterephthalic acid and glacial acetic acid, stir thoroughly and microwave heat, then remove, filter, wash and dry to obtain MOF structure modified lithium iron phosphate cathode material.
[0005] Preferably, in step one, the molar ratio of lithium carbonate, ferrous sulfate, and phosphoric acid is 1-2:1:1 (Li:Fe:P); the solvent is deionized water; the amount of solvent added is 60-80% of the polytetrafluoroethylene liner filling degree; and the Fe content is controlled. 2+ The molar concentration of the substance in the mixed system is 0.5~1.5 mol / L.
[0006] Preferably, in step one, the amount of ascorbic acid added is 8-12% of the mass of ferrous sulfate, and the pH is adjusted to 7-8.
[0007] Preferably, in step one, the inert atmosphere is one or both of nitrogen and argon, and the stirring and mixing time is 0.5 to 2 hours.
[0008] Preferably, in step one, the microwave heating temperature is 200~220℃, the microwave heating power is 2~4kW, and the microwave heating time is 0.5~2h.
[0009] Preferably, in step two, chromium sulfate, 2-aminoterephthalic acid, and glacial acetic acid are prepared according to Cr... 3+ The molar ratio of H2BDC-NH2:CH3COOH is 1:1:1, and the amount of chromium sulfate added is 6-10% of the mass of ferrous sulfate.
[0010] Preferably, in step two, the stirring time is 20-40 minutes; the microwave heating temperature is 200-220°C; the microwave heating power is 2-4 kW; and the microwave heating time is 1-3 hours.
[0011] Preferably, in step two, a polytetrafluoroethylene (PTFE) filter membrane with a pore size of 0.1~0.2μm is used for filtration; the washing method is as follows: first wash with N,N-dimethylformamide (DMF) at 100℃, then wash with anhydrous ethanol at 80℃, and then wash with deionized water.
[0012] Preferably, in step two, a vacuum oven is used for drying, the drying temperature is 50~70℃, and the drying time is 6~8h.
[0013] Application of MOF-structured modified lithium iron phosphate cathode material prepared by the method described above in batteries.
[0014] Preferably, Cr is used in this invention. 3+ Using 2-aminoterephthalic acid as the MOF template framework, 2-aminoterephthalic acid contains nitrogen-containing groups, which form a Cr-N co-doped structure with chromium ions.
[0015] Preferably, all of the present inventions are prepared by hydrothermal synthesis, and the heating method is not traditional electric heating, but microwave-assisted heating to 200~220°C, which greatly shortens the reaction time.
[0016] Preferably, the one-pot process of the present invention is completed in a high-pressure reactor. The specific steps are to first synthesize lithium iron phosphate and then synthesize MIL-101 with MOF structure.
[0017] Preferably, the present invention involves stirring and mixing under an inert atmosphere of N2 or Ar to avoid Fe 2+ It is oxidized.
[0018] Preferably, the single-pot high-pressure reactor used in this invention is equipped with a jacketed microwave heating system and a real-time pressure gauge. The lining is made of polytetrafluoroethylene, and the lid has a feeding port, an air inlet, and an air outlet. An embedded metal measuring rod extends to the bottom of the reactor and connects to pH and temperature sensors. A discharge port is located in the center of the bottom of the reactor, and both ports are equipped with high-pressure shut-off valves.
[0019] The present invention has at least the following beneficial effects: 1. Good gradation effect between particles: The lithium iron phosphate coated by in-situ MIL-101 has a prismatic octahedral structure, and the resulting lithium iron phosphate particles are tightly bonded, with low porosity and high compaction density.
[0020] 2. Excellent ion conductivity and transport performance: Cr-N co-doping forms a rich electron cloud, which is beneficial for electron transport and rapid diffusion of lithium ions.
[0021] 3. More stable inorganic carbon skeleton and high pressure resistance: By in-situ coating with MIL-101, the surface of LFP contains abundant organic carbon polymers, which are assembled into a stable carbon skeleton to avoid the increase of free carbon, enabling LFP to withstand high pressure environment and with extremely low resistivity.
[0022] 4. The synthesis process of LFP products is simple: MOF-type modified lithium iron phosphate is synthesized in a one-pot low temperature (≤220℃) process, which makes the overall process cost and energy consumption lower, the synthesis time faster, and the material performance better, making it cost-effective.
[0023] Other advantages, objectives and features of the present invention will become apparent in part from the following description, and in part from those skilled in the art through study and practice of the invention. Attached Figure Description
[0024] Figure 1 This is a schematic diagram of the preparation method of the present invention. Detailed Implementation
[0025] The present invention will now be described in further detail so that those skilled in the art can implement it based on the description.
[0026] It should be understood that terms such as “having,” “comprising,” and “including” as used herein do not exclude the presence or addition of one or more other elements or combinations thereof.
[0027] Example 1 A method for rapidly synthesizing MOF-structured modified lithium iron phosphate cathode materials at low temperature using a microwave hydrothermal method includes the following steps: Step 1: Add lithium carbonate, ferrous sulfate, and phosphoric acid (Li:Fe:P molar ratio of 1.2:1:1) to a high-pressure reactor containing deionized water and mix. The amount of deionized water added should be 70% of the polytetrafluoroethylene liner filling density, and the Fe content should be controlled. 2+ The molar concentration of the mixture was 1 mol / L. Then, 10% ferrous sulfate was added ascorbic acid, the pH was adjusted to 8 with ammonia, and the mixture was stirred and mixed for 1 h under a nitrogen atmosphere. Subsequently, the mixture was microwaved at 200 °C and 3 kW for 1 h to obtain the reaction solution. Step 2: After cooling the reaction solution to room temperature, add 6% ferrous sulfate, chromium sulfate (by mass), 2-aminoterephthalic acid, and glacial acetic acid (Cr). 3+ The molar ratio of H2BDC-NH2:CH3COOH was 1:1:1. After stirring thoroughly for 30 min, the mixture was microwave-heated at 200℃ and 3kW for 2 h. Then, it was removed, filtered through a 0.1 μm pore size PTFE membrane, washed first with 100℃ DMF, then with 80℃ anhydrous ethanol, then with deionized water, and finally dried in a 60℃ vacuum oven for 6 h to obtain the MOF-structured modified lithium iron phosphate cathode material, denoted as LFP@MIL1.
[0028] Example 2 A method for rapidly synthesizing MOF-structured modified lithium iron phosphate cathode materials at low temperature using a microwave hydrothermal method includes the following steps: Step 1: Add lithium carbonate, ferrous sulfate, and phosphoric acid (Li:Fe:P molar ratio of 1.2:1:1) to a high-pressure reactor containing deionized water and mix. The amount of deionized water added should be 70% of the polytetrafluoroethylene liner filling density, and the Fe content should be controlled. 2+ The molar concentration of the mixture was 1 mol / L. Then, 10% ferrous sulfate was added ascorbic acid, the pH was adjusted to 8 with ammonia, and the mixture was stirred and mixed for 1 h under a nitrogen atmosphere. Subsequently, the mixture was microwaved at 200 °C and 3 kW for 1 h to obtain the reaction solution. Step 2: After cooling the reaction solution to room temperature, add 8% ferrous sulfate, chromium sulfate by mass, 2-aminoterephthalic acid, and glacial acetic acid (Cr). 3+The molar ratio of H2BDC-NH2:CH3COOH was 1:1:1. After stirring thoroughly for 30 min, the mixture was microwave-heated at 200℃ and 3kW for 2 h. After holding at this temperature, the mixture was removed and filtered through a 0.1 μm pore size PTFE membrane. It was first washed with 100℃ DMF, then with 80℃ anhydrous ethanol, then with deionized water, and finally dried in a 60℃ vacuum oven for 6 h to obtain the MOF-structured modified lithium iron phosphate cathode material, denoted as LFP@MIL2.
[0029] Example 3 A method for rapidly synthesizing MOF-structured modified lithium iron phosphate cathode materials at low temperature using a microwave hydrothermal method includes the following steps: Step 1: Add lithium carbonate, ferrous sulfate, and phosphoric acid (Li:Fe:P molar ratio of 1.2:1:1) to a high-pressure reactor containing deionized water and mix. The amount of deionized water added should be 70% of the polytetrafluoroethylene liner filling density, and the Fe content should be controlled. 2+ The molar concentration of the mixture was 1 mol / L. Then, 10% ferrous sulfate was added ascorbic acid, the pH was adjusted to 8 with ammonia, and the mixture was stirred and mixed for 1 h under a nitrogen atmosphere. Subsequently, the mixture was microwaved at 200 °C and 3 kW for 1 h to obtain the reaction solution. Step 2: After cooling the reaction solution to room temperature, add 10% ferrous sulfate, chromium sulfate (by mass), 2-aminoterephthalic acid, and glacial acetic acid (Cr). 3+ The molar ratio of H2BDC-NH2:CH3COOH was 1:1:1. After stirring thoroughly for 30 min, the mixture was microwave-heated at 200℃ and 3kW for 2 h. After holding at this temperature, the mixture was removed and filtered through a 0.1 μm pore size PTFE membrane. It was first washed with 100℃ DMF, then with 80℃ anhydrous ethanol, then with deionized water, and finally dried in a 60℃ vacuum oven for 6 h to obtain the MOF-structured modified lithium iron phosphate cathode material, denoted as LFP@MIL3.
[0030] Example 4 A method for rapidly synthesizing MOF-structured modified lithium iron phosphate cathode materials at low temperature using a microwave hydrothermal method includes the following steps: Step 1: Add lithium carbonate, ferrous sulfate, and phosphoric acid (Li:Fe:P molar ratio of 1.2:1:1) to a high-pressure reactor containing deionized water and mix. The amount of deionized water added should be 70% of the polytetrafluoroethylene liner filling density, and the Fe content should be controlled. 2+ The molar concentration of the mixture was 1 mol / L. Then, 10% ferrous sulfate was added ascorbic acid, the pH was adjusted to 8 with ammonia, and the mixture was stirred and mixed for 1 h under a nitrogen atmosphere. Subsequently, the mixture was microwaved at 200 °C and 3 kW for 1 h to obtain the reaction solution. Step 2: After cooling the reaction solution to room temperature, add 6% ferrous sulfate, chromium sulfate (by mass), 2-aminoterephthalic acid, and glacial acetic acid (Cr). 3+ The molar ratio of H2BDC-NH2:CH3COOH was 1:1:1. After stirring thoroughly for 30 min, the mixture was microwave-heated at 220℃ and 3kW for 2 h. After holding at this temperature, the mixture was removed and filtered through a 0.1 μm pore size PTFE membrane. It was first washed with 100℃ DMF, then with 80℃ anhydrous ethanol, then with deionized water, and finally dried in a 60℃ vacuum oven for 6 h to obtain the MOF-structured modified lithium iron phosphate cathode material, denoted as LFP@MIL4.
[0031] Comparative Example 1 A method for preparing a lithium iron phosphate cathode material includes the following steps: Step 1: Add lithium carbonate, ferrous sulfate, and phosphoric acid (Li:Fe:P molar ratio of 1.2:1:1) to a high-pressure reactor containing deionized water and mix. The amount of deionized water added should be 70% of the polytetrafluoroethylene liner filling density, and the Fe content should be controlled. 2+ The molar concentration of the mixture was 1 mol / L. Then, 10% ferrous sulfate was added ascorbic acid, the pH was adjusted to 8 with ammonia, and the mixture was stirred and mixed for 1 h under a nitrogen atmosphere. Subsequently, the mixture was microwaved at 200 °C and 3 kW for 1 h to obtain the reaction solution. Step 2: After cooling the reaction solution to room temperature, filter it through a 0.1 μm pore size PTFE membrane, wash it with deionized water, and dry it in a vacuum oven at 60℃ for 6 hours to obtain lithium iron phosphate cathode material, denoted as LFP-1.
[0032] Comparative Example 2 A method for preparing a lithium iron phosphate cathode material includes the following steps: Step 1: Add lithium carbonate, ferrous sulfate, and phosphoric acid (Li:Fe:P molar ratio of 1.2:1:1) to a high-pressure reactor containing deionized water and mix. The amount of deionized water added should be 70% of the polytetrafluoroethylene liner filling density, and the Fe content should be controlled. 2+ The molar concentration of the mixture was 1 mol / L. Then, 10% ferrous sulfate was added ascorbic acid, the pH was adjusted to 8 with ammonia, and the mixture was stirred and mixed for 1 h under a nitrogen atmosphere. Subsequently, the mixture was microwaved at 140 °C and 3 kW for 1 h to obtain the reaction solution. Step 2: After cooling the reaction solution to room temperature, filter it through a 0.1 μm pore size PTFE membrane, wash it with deionized water, and dry it in a vacuum oven at 60℃ for 6 hours to obtain lithium iron phosphate cathode material, denoted as LFP-2.
[0033] Comparative Example 3 A method for preparing a lithium iron phosphate cathode material includes the following steps: Step 1: Add lithium carbonate, ferrous sulfate, and phosphoric acid (Li:Fe:P molar ratio of 1.2:1:1) to a high-pressure reactor containing deionized water and mix. The amount of deionized water added should be 70% of the polytetrafluoroethylene liner filling density, and the Fe content should be controlled. 2+ The molar concentration of the mixture was 1 mol / L. Then, 10% ferrous sulfate was added ascorbic acid, the pH was adjusted to 8 with ammonia, and the mixture was stirred and mixed for 1 h under a nitrogen atmosphere. Then, it was heated at 200 °C for 1 h to obtain the reaction solution. Step 2: After cooling the reaction solution to room temperature, add 6% ferrous sulfate, chromium sulfate (by mass), 2-aminoterephthalic acid, and glacial acetic acid (Cr). 3+ The molar ratio of H2BDC-NH2:CH3COOH is 1:1:1. After stirring thoroughly for 30 min, the mixture is heated at 200℃ for 2 h. Then, it is removed, filtered through a 0.1 μm pore size PTFE membrane, washed first with 100℃ DMF, then with 80℃ anhydrous ethanol, then with deionized water, and finally dried in a 60℃ vacuum oven for 6 h to obtain lithium iron phosphate cathode material, denoted as LFP@MIL5.
[0034] Comparative Example 4 A method for preparing a lithium iron phosphate cathode material includes the following steps: Step 1: Add lithium carbonate, ferrous sulfate, and phosphoric acid (Li:Fe:P molar ratio of 1.2:1:1) to a high-pressure reactor containing deionized water and mix. The amount of deionized water added should be 70% of the polytetrafluoroethylene liner filling density, and the Fe content should be controlled. 2+ The molar concentration of the mixture was 1 mol / L. Then, 10% ferrous sulfate was added ascorbic acid, the pH was adjusted to 8 with ammonia, and the mixture was stirred and mixed for 1 h under a nitrogen atmosphere. Subsequently, the mixture was microwaved at 200 °C and 3 kW for 1 h to obtain the reaction solution. Step 2: After cooling the reaction solution to room temperature, add 6% ferrous sulfate, chromium sulfate (by mass), 2-aminoterephthalic acid, and glacial acetic acid (Cr). 3+ The molar ratio of H2BDC-NH2:CH3COOH was 1:1:1. After stirring thoroughly for 30 min, the mixture was heated at 200℃ for 2 h. Then, it was removed, filtered through a 0.1 μm pore size PTFE membrane, washed first with 100℃ DMF, then with 80℃ anhydrous ethanol, then with deionized water, and finally dried in a 60℃ vacuum oven for 6 h to obtain lithium iron phosphate cathode material, denoted as LFP@MIL6.
[0035] The lithium iron phosphate cathode materials prepared in Examples 1-4 and Comparative Examples 1-4 were tested. The lithium iron phosphate cathode materials were fabricated into coin cells. The specific preparation method was as follows: lithium iron phosphate cathode material, Super-P conductive agent, and PVDF-NMP binder were mixed in a 90:5:5 ratio in a high-speed shaker. The slurry was uniformly coated onto aluminum foil to a thickness of 150 μm, then dried at 80°C for 6 hours. The electrode sheet was then compacted to a thickness of 80 μm using a roller press. The electrode sheet was then cut using a Φ12 mm punch, and further vacuum dried at 120°C for 6 hours before being transferred to a glove box. The cells were then assembled into 2032 coin cells sequentially as follows: negative electrode shell, lithium sheet, electrolyte, separator, electrolyte, positive electrode sheet, and positive electrode shell. After 0.1C formation and capacity testing, the cells were charged at a 10C constant current rate to 3.85V and discharged at a 10C constant current rate to 2.5V. The results are shown in Tables 1 and 2.
[0036] Table 1 Table 2 As can be seen from Tables 1 and 2, Examples 1-4 exhibit better electrochemical performance and lower resistivity compared to Comparative Examples 1-4. The main difference in Examples 1-3 lies in the addition of 6%, 8%, and 10% chromium sulfate by mass of ferrous sulfate. With the increase of chromium sulfate, the compaction density is greater than 2.6 g / cm³. 3 However, the electrochemical performance differed. The LFP@MIL2 sample (Example 2) exhibited the best 10C / 3.85V charging capacity of 136.8 mAh / g and the lowest resistivity of 4.1 Ω·cm, indicating that there is an optimal range for the amount of chromium sulfate added. As can be seen from Examples 4 and 1, controlling the Cr... 3+ The molar ratio of H2BDC-NH2:CH3COOH was 1:1:1. Microwave heating at 220℃ and 200℃ resulted in varying degrees of decrease in the compaction density and 10C charge / discharge capacity of Example 4, indicating an optimal temperature range for microwave heating. Comparing Example 1 and Comparative Example 1, after modification with the MOF structure, the compaction density and electrochemical performance of lithium iron phosphate (LFP) were improved to varying degrees. In particular, the 10C charging capacity increased from 91.3 mAh / g to 135.1 mAh / g, and the capacity retention rate after 1000 cycles increased from 46.8% to 90.5%. This indicates that the MOF structure can improve the stability and lifespan of LFP materials, and the resistivity is less than 10 Ω·cm, enhancing the battery's safety. Comparative Examples 1 and 2 show that the compaction density only reaches 2.6 g / cm³ when the microwave heating temperature reaches 200℃. 3 As can be seen from Comparative Examples 3-4 compared to Example 1, the materials prepared by microwave heating have better electrochemical performance, and the microwave heating method can greatly shorten the reaction time.
[0037] This invention involves microwave heating of lithium carbonate, ferrous sulfate, and phosphoric acid in a high-pressure reactor, followed by the addition of Cr... 3+ 2-Aminoterephthalic acid (H2BDC-NH2) was introduced as a MOF template agent and carbon source to prepare an in-situ MIL-101-coated MOF-modified lithium iron phosphate cathode material via hydrothermal synthesis. Due to the prismatic octahedral structure of the MOF in this lithium iron phosphate cathode material, the generated particles are tightly bonded, with low porosity and high compaction density. Cr-N co-doping forms an abundant electron cloud, which is beneficial for electron transport and rapid lithium-ion diffusion. The in-situ coating with MIL-101 results in an abundance of organic carbon polymers on the LFP surface, assembling into a stable inorganic carbon framework that avoids the increase of free carbon, enabling the LFP to withstand high-voltage environments and exhibiting extremely low resistivity.
[0038] Meanwhile, the MOF-structured modified lithium iron phosphate cathode material prepared using the method of this invention not only possesses excellent electrical properties and extremely low resistivity under high solid density, but also exhibits an extremely short reaction synthesis time throughout the entire preparation process. The one-pot hydrothermal synthesis mechanism reduces the traditional lithium iron phosphate preparation time to one day. Ultimately, MOF-structured modified lithium iron phosphate cathode material was synthesized in a very short time, resulting in a 10C charging performance of no less than 134.7 mAh / g and a resistivity reduced to 10 Ω·cm or less. This provides valuable reference for improving electrochemical performance under high solid density.
[0039] Although embodiments of the present invention have been disclosed above, they are not limited to the applications listed in the specification and embodiments. They can be applied to various fields suitable for the present invention. For those skilled in the art, other modifications can be easily made. Therefore, without departing from the general concept defined by the claims and their equivalents, the present invention is not limited to the specific details and embodiments shown and described herein.
Claims
1. A method for rapidly synthesizing MOF-structured modified lithium iron phosphate cathode materials at low temperature using a microwave hydrothermal method, characterized in that, Includes the following steps: Step 1: Add lithium carbonate, ferrous sulfate and phosphoric acid to a high-pressure reactor containing solvent and mix. Then add ascorbic acid, adjust the pH with ammonia, stir and mix under an inert atmosphere, and then microwave heat to obtain the reaction solution. Step 2: After cooling the reaction solution to room temperature, add chromium sulfate, 2-aminoterephthalic acid and glacial acetic acid, stir thoroughly and microwave heat, then remove, filter, wash and dry to obtain MOF structure modified lithium iron phosphate cathode material.
2. The method for preparing MOF-structured modified lithium iron phosphate cathode material by microwave hydrothermal method at low temperature and rapid synthesis as described in claim 1, characterized in that, In step one, lithium carbonate, ferrous sulfate, and phosphoric acid are added in a Li:Fe:P molar ratio of 1~2:1:1; the solvent is deionized water, and the amount of solvent added is 60~80% of the polytetrafluoroethylene lining filling degree, and the Fe content is controlled. 2+ The molar concentration of the substance in the mixed system is 0.5~1.5 mol / L.
3. The method for preparing MOF-structured modified lithium iron phosphate cathode material by microwave hydrothermal method at low temperature and rapid synthesis as described in claim 1, characterized in that, In step one, the amount of ascorbic acid added is 8-12% of the mass of ferrous sulfate, and the pH is adjusted to 7-8.
4. The method for preparing MOF-structured modified lithium iron phosphate cathode material by microwave hydrothermal method at low temperature and rapid synthesis as described in claim 1, characterized in that, In step one, the inert atmosphere is one or both of nitrogen and argon, and the stirring and mixing time is 0.5 to 2 hours.
5. The method for preparing MOF-structured modified lithium iron phosphate cathode material by microwave hydrothermal method at low temperature and rapid synthesis as described in claim 1, characterized in that, In step one, the microwave heating temperature is 200~220℃, the microwave heating power is 2~4kW, and the microwave heating time is 0.5~2h.
6. The method for preparing MOF-structured modified lithium iron phosphate cathode material by microwave hydrothermal method at low temperature and rapid synthesis as described in claim 1, characterized in that, In step two, chromium sulfate, 2-aminoterephthalic acid, and glacial acetic acid are disposed according to Cr... 3+ The molar ratio of H2BDC-NH2:CH3COOH is 1:1:1, and the amount of chromium sulfate added is 6-10% of the mass of ferrous sulfate.
7. The method for preparing MOF-structured modified lithium iron phosphate cathode material by microwave hydrothermal method at low temperature and rapid synthesis as described in claim 1, characterized in that, In step two, the stirring time is 20-40 minutes; the microwave heating temperature is 200-220°C; the microwave heating power is 2-4 kW; and the microwave heating time is 1-3 hours.
8. The method for preparing MOF-structured modified lithium iron phosphate cathode material by microwave hydrothermal method at low temperature and rapid synthesis as described in claim 1, characterized in that, In step two, a polytetrafluoroethylene filter membrane with a pore size of 0.1~0.2μm is used for filtration; the washing method is as follows: first wash with N,N-dimethylformamide at 100℃, then wash with anhydrous ethanol at 80℃, and then wash with deionized water.
9. The method for preparing MOF-structured modified lithium iron phosphate cathode material by microwave hydrothermal method at low temperature and rapid synthesis as described in claim 1, characterized in that, In step two, a vacuum oven is used for drying, with a drying temperature of 50~70℃ and a drying time of 6~8 hours.
10. The application of a MOF-structured modified lithium iron phosphate cathode material prepared by any one of claims 1-9 in a battery.