A solid-state battery based on a coal gangue-based carbon fiber carbon material composite negative electrode and a preparation method thereof

By extracting organic matter from coal gangue and preparing silicon-aluminum-rich residue, carbon fiber-hard carbon composite anode materials were prepared, solving the contact and conductivity problems of graphite and hard carbon materials in solid-state lithium batteries. This achieved efficient electron transport and lithium storage performance, and improved the energy density and cycle stability of solid-state batteries.

CN123162164APending Publication Date: 2026-11-24HUASHANG POLYMER POWER TECHNOLOGY DEVELOPMENT (SHANDONG) CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611407004.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-11
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

The existing solid-solid contact area between graphite, the anode material for solid-state lithium batteries, and the solid electrolyte is limited, resulting in a large interfacial impedance and a decrease in rate performance. Hard carbon materials have low conductivity and their initial coulombic efficiency needs to be improved. Furthermore, existing coal gangue-based carbon materials have failed to effectively construct a continuous electron transport network and abundant lithium storage sites.

Method used

Carbon fibers derived from organic matter extracted from coal gangue and hard carbon derived from silicon-aluminum residue were composited in situ to form an interpenetrating structure consisting of a continuous carbon fiber network skeleton and hard carbon particles. The interface contact was optimized through a gradient pore structure, and heteroatoms were in situ doped during the carbonization process to construct a composite anode material with high conductivity and high lithium storage capacity.

Benefits of technology

This technology enables the high-value utilization of all components of coal gangue, provides high-speed electron transport channels and abundant lithium storage sites, reduces interfacial impedance, improves the conductivity and lithium storage capacity of composite materials, and significantly enhances the cycle stability and energy density of solid-state batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

This invention relates to the field of solid-state lithium battery anode material technology, specifically to a solid-state battery based on a coal gangue-based carbon fiber composite anode and its preparation method. The composite material is formed by in-situ composite of carbon fibers derived from organic matter extracted from coal gangue through graded extraction and hard carbon derived from silicon-aluminum-rich residue. It has an interpenetrating structure of a continuous carbon fiber network skeleton and hard carbon particles filling the structure, and the composite material has a specific surface area of ​​120 m². 2 / g to 220m 2 / g, pore volume 0.25cm³ 3 / g to 0.50cm 3 / g, with an average pore size of 3nm to 8nm. The organic component is used to prepare the carbon fiber network skeleton (accounting for 50%-70% of the composite material), and the carbonaceous material in the silicon-aluminum-rich residue and the added carbon source jointly construct the hard carbon filler phase (accounting for 30%-50% of the composite material). The two work together to construct the composite anode material, with high utilization rate of coal gangue, which is in line with the policy orientation of solid waste resource utilization and dual carbon.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of solid-state lithium battery anode material technology, specifically to a solid-state battery based on a coal gangue-based carbon fiber composite anode and its preparation method. Background Technology

[0002] Solid-state lithium batteries are considered an important direction for the development of next-generation energy storage technology due to their advantages such as high safety and high energy density. As the core component of solid-state batteries, the structure and performance of the anode material directly determine the battery's energy density, cycle life, and safety performance.

[0003] Currently, graphite is the primary anode material for commercial lithium-ion batteries, with a theoretical specific capacity of 372 mAh / g. In solid-state battery systems, graphite anodes suffer from the following prominent problems: the limited solid-solid contact area between graphite and the solid electrolyte results in high interfacial impedance, leading to decreased rate performance; although the volume change after intercalation of lithium into graphite layers is relatively small, interfacial contact degradation remains significant during long-term cycling. Hard carbon materials exhibit certain advantages in solid-state batteries due to their high lithium storage capacity and disordered layered structure, but their intrinsic conductivity is low, and their initial coulombic efficiency needs improvement.

[0004] Carbon fiber materials possess excellent electrical conductivity, mechanical properties, and chemical stability. When used as a negative electrode material, they can construct a continuous electron transport network, and the porosity between fibers facilitates electrolyte wetting. Currently, the preparation of carbon fiber primarily uses polyacrylonitrile, pitch, and other raw materials, resulting in high costs.

[0005] Patent CN106012106A discloses a method for preparing mesophase pitch-based carbon fibers using coal gangue as raw material. The method involves oxidizing coal gangue and then blending it with pitch for spinning and carbonization. However, this method only focuses on the preparation of the carbon fibers themselves and does not involve technical solutions for applying them to battery anodes, especially solid-state battery anodes.

[0006] Coal gangue is a solid waste generated during coal mining and washing, with huge annual emissions and low comprehensive utilization rate. Developing high-value utilization pathways for coal gangue has significant resource, environmental, and economic value. Existing technologies include research on the use of coal gangue-based carbon materials for energy storage. For example, patent CN119601748A discloses a method for preparing multi-element doped porous carbon from coal gangue for use as a negative electrode in flexible solid-state lithium-ion batteries. However, this method prepares porous carbon particulate materials, does not involve the construction of carbon fiber structures, and relies on diamond film coating for interface improvement, resulting in complex processes and high costs.

[0007] Coal gangue has a complex composition, containing both organic components and a large amount of inorganic minerals such as aluminosilicates. Achieving synergistic utilization of all components and constructing carbon-based anode materials with unique microstructures is a technical problem that needs to be solved in this field. In particular, developing a low-cost, high-performance coal gangue-based composite anode material to address the pain points of poor solid-solid contact and high interfacial impedance in solid-state batteries has significant academic value and application prospects. Summary of the Invention

[0008] The primary objective of this invention is to provide a solid-state battery based on a coal gangue-based carbon fiber composite negative electrode and its preparation method.

[0009] A further objective of this invention is to provide a coal gangue-based carbon fiber-hard carbon composite anode material, wherein the composite anode material is in-situ composited from carbon fibers derived from organic matter extracted from coal gangue through graded extraction and hard carbon derived from silicon-aluminum-rich residue, and has an interpenetrating structure consisting of a continuous carbon fiber network skeleton and hard carbon particles filling the structure; the specific surface area of ​​the composite anode material is 120 m². 2 / g to 220m 2 / g, pore volume 0.25cm³ 3 / g to 0.50cm 3 / g, with an average pore size of 3nm to 8nm.

[0010] Preferably, the composite negative electrode material contains 50% to 70% carbon fiber by mass and 30% to 50% hard carbon by mass; the carbon fiber has a diameter of 200 nm to 500 nm and a specific surface area of ​​80 m². 2 / g to 150m 2 / g.

[0011] Preferably, the composite anode material contains four heteroatoms: nitrogen, oxygen, silicon, and sulfur, with a total heteroatom content of 3.5% to 8.0%; the composite anode material has a gradient pore structure, with a surface pore size of 5 nm to 10 nm and an internal pore size of 1 nm to 3 nm.

[0012] A method for preparing the coal gangue-based carbon fiber-hard carbon composite anode material includes the following steps: Step 1: Pretreatment and graded extraction of coal gangue. After crushing and ball milling, N-methylpyrrolidone is added for heating and extraction to separate organic matter extract and silica-alumina-rich residue. Step 2, preparation of carbon fiber precursor spinning solution: organic matter extract and polyacrylonitrile are mixed and dissolved in N,N-dimethylformamide to obtain spinning solution; Step 3: Preparation of hard carbon precursor suspension. The silica-rich aluminum residue is demineralized by hydrothermal alkaline leaching and acid leaching, then mixed with glucose and urea and dispersed in water to obtain a suspension. The hydrothermal alkaline leaching uses a 20% to 30% sodium hydroxide solution and reacts at 130°C to 150°C for 14 to 16 hours. The acid leaching uses a 10% to 15% hydrochloric acid solution and is carried out at 65°C to 75°C for 4.5 to 5.5 hours. Step 4: Electrospinning and in-situ loading. Electrospinning the spinning solution to obtain a precursor fiber membrane, and then immersing it in a suspension to impregnate the hard carbon precursor. Step 5, pre-oxidation treatment: The loaded fiber membrane is heated to 240°C to 270°C in air at a rate of 1°C to 2°C to 2°C to 1.5h to 2.5h for pre-oxidation. Step 6, gradient carbonization treatment: the pre-oxidized fiber membrane is subjected to three-stage gradient carbonization under an inert atmosphere. Step 7: Surface etching treatment. The carbonized composite material is mixed with potassium hydroxide and then etched at high temperature in an inert atmosphere to obtain the final product.

[0013] Preferably, in step one, the extraction temperature is 180°C to 200°C, the extraction time is 8h to 12h, and the solid-liquid ratio is 1:8 to 1:12; the coal gangue has a carbon content of 15% to 30%, a silicon dioxide content of 40% to 60%, and an aluminum oxide content of 15% to 25%.

[0014] Preferably, in step two, the mass ratio of organic extract to polyacrylonitrile is 2:1 to 4:1, the mass fraction of spinning solution is 8% to 12%, and the viscosity-average molecular weight of the polyacrylonitrile is 80,000 to 120,000; in step four, the electrospinning parameters are: spinning voltage 15kV to 20kV, receiving distance 15cm to 20cm, spinning rate 0.8mL / h to 1.2mL / h, roller speed 800r / min to 1200r / min; and immersion time is 2h to 4h.

[0015] Preferably, the gradient carbonization conditions in step six are as follows: in the first stage, the temperature is increased to 400℃ to 500℃ at a rate of 3℃ / min to 5℃ / min and held for 1h to 2h; in the second stage, the temperature is increased to 700℃ to 900℃ at a rate of 2℃ / min to 3℃ / min and held for 2h to 3h; and in the third stage, the temperature is increased to 1100℃ to 1300℃ at a rate of 5℃ / min to 8℃ / min and held for 1h to 2h.

[0016] Preferably, in step seven, the mass ratio of the composite material to potassium hydroxide is 1:1 to 1:2, the etching temperature is 600°C to 750°C, and the etching time is 30 min to 60 min.

[0017] Preferably, the negative electrode is the coal gangue-based carbon fiber-hard carbon composite negative electrode material according to any one of claims 1 to 3.

[0018] Preferably, the solid electrolyte is a sulfide solid electrolyte, selected from at least one of the LiPSCl system and the Li-Ge-PS-Cl system; the positive electrode uses a commonly used positive electrode material for sulfide solid batteries, selected from at least one of sulfide polyacrylonitrile, lithium cobalt oxide, and lithium nickel cobalt manganese oxide. Compared with the prior art, the beneficial effects of the present invention are: 1. This invention enables the high-value utilization of all components of coal gangue. The organic components are used to prepare carbon fiber network skeletons (accounting for 50%-70% of the composite material), and the carbonaceous matter in the silicon-aluminum-rich residue and the added carbon source jointly construct a hard carbon filler phase (accounting for 30%-50% of the composite material). The two work together to construct a composite anode material, resulting in high utilization of coal gangue, which is in line with the policy orientation of solid waste resource utilization and dual carbon.

[0019] 2. The continuous carbon fiber network of this invention provides a high-speed electron transport channel, while the hard carbon particles provide abundant lithium storage sites. The two components complement each other, resulting in a composite material with both high conductivity and high lithium storage capacity. The composite material of this invention exhibits a reversible specific capacity of over 460 mAh / g at a current density of 0.1C, significantly higher than that of a single hard carbon material.

[0020] 3. This invention utilizes potassium hydroxide surface etching to construct a well-developed mesoporous structure on the surface of the composite material, increasing the contact area with the sulfide solid electrolyte and reducing interfacial impedance; while retaining more microporous structures internally, it ensures lithium storage capacity and structural stability. In the embodiments, the interfacial impedance of the button battery assembled using Li6PS5Cl sulfide solid electrolyte can be reduced to below 90Ω, and the capacity retention rate after 100 cycles reaches over 88%.

[0021] 4. In this invention, the nitrogen, sulfur, silicon and other elements contained in the coal gangue itself are in situ doped into the carbon skeleton during the carbonization process, introducing defective active sites, increasing the contribution of pseudocapacitive lithium storage, and improving the interfacial compatibility between the material and the sulfide solid electrolyte.

[0022] 5. By adjusting the extraction conditions, spinning parameters, carbonization temperature and etching degree, this invention can precisely control the composition ratio, microstructure and pore size distribution of the composite material, making it easy to scale up production. Detailed Implementation

[0023] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0024] Invention Mechanism: The core mechanism of this invention lies in utilizing the dual-component characteristics of coal gangue, namely the hierarchical utilization of organic and inorganic mineral components, to construct a carbon fiber-hard carbon interpenetrating network structure. The specific mechanism is as follows: After extraction with N-methylpyrrolidone solvent, the organic components of coal gangue yield an extract rich in polycyclic aromatic hydrocarbons (PAHs). This extract is rich in PAHs and heteroatom functional groups and exhibits good compatibility with polyacrylonitrile (PAN) in N,N-dimethylformamide (the polar groups of PAHs form dipole-dipole interactions with the cyano groups of PAN). The resulting blend exhibits excellent electrospinning properties. After pre-oxidation and carbonization, it forms a continuous carbon fiber network, providing high-speed electron transport channels and mechanical support for the composite material. The silica-alumina-rich residue in coal gangue undergoes hydrothermal alkaline desilication (using the reaction of SiO2 and NaOH under hydrothermal conditions to generate soluble sodium silicate to remove most of the silicon components) and acid leaching demineralization (removing aluminum, iron, and other metal oxides). The remaining carbonaceous components, together with an added carbon source, form a hard carbon precursor, which, after high-temperature carbonization, forms hard carbon particles.

[0025] The roles of each stage in the three-stage gradient carbonization are as follows: The first stage (400-500℃) mainly completes the pyrolysis and preliminary aromatization of the pre-oxidized fiber, releasing small molecule gases; The second stage (700-900℃) is the main carbonization stage, during which a carbon skeleton is formed and a large number of microporous structures are generated. The third stage (1100-1300℃) involves high-temperature graphitization fine-tuning to improve the crystallinity and electrical conductivity of the carbon material. The disordered layered structure and abundant microporous-mesoporous structure of hard carbon provide a large number of storage sites for lithium ions.

[0026] During the preparation process, the hard carbon precursor is loaded onto the carbon fiber surface through impregnation adsorption and in-situ bonding during hydrothermal / carbonization. After carbonization, a tight interface is formed between the fiber skeleton and the hard carbon particles. During the pre-oxidation process, the carbon fiber surface forms abundant oxygen-containing functional groups, which can form hydrogen bonds or chemical bonds with glucose and urea in the hard carbon precursor, preventing the two from separating during cycling.

[0027] Meanwhile, trace amounts of silicon, aluminum, sulfur, and other elements remaining in the silicon-rich aluminum residue are in situ incorporated into the carbon skeleton during the carbonization process, generating more defective active sites, which is beneficial for the adsorption and transport of lithium ions.

[0028] For solid-state battery systems, this invention constructs a gradient pore structure on the surface of a composite material using a potassium hydroxide surface etching process. The near-surface region has abundant mesoporous structures, which can increase the contact area with the sulfide solid electrolyte and reduce interfacial impedance; the internal region is dominated by micropores, ensuring lithium storage capacity and structural stability.

[0029] This gradient pore structure is achieved by controlling the amount of etchant, etching time, and temperature: KOH-activated etching progresses gradually from the material surface to the interior, resulting in more thorough surface contact and deeper etching, forming more developed mesopores; limited mass transfer inwards leads to a reduced etching depth, preserving more micropores. Compared to uniform porous structures, this approach simultaneously ensures good interfacial contact and volumetric stability.

[0030] Raw material source: Coal gangue, taken from the washed gangue of a coal mine in Shuozhou, Shanxi Province, has a carbon content of 23.6%, a silicon dioxide content of 51.8%, an aluminum oxide content of 16.4%, an iron oxide content of 4.7%, a calcium oxide content of 1.9%, and other components of 1.6%. It is crushed and ball-milled to below 200 mesh.

[0031] N-Methylpyrrolidone (NMP), analytical grade, purity 99.0%, boiling point 202℃, Tianjin Kemei Chemical Reagent Co., Ltd., CAS No. 872-50-4.

[0032] Polyacrylonitrile, viscosity-average molecular weight 90,000, Shanghai Maclean Biochemical Technology Co., Ltd., CAS No. 25014-41-9.

[0033] N,N-Dimethylformamide, analytical grade, purity 99.5%, boiling point 153℃, Tianjin Fuyu Fine Chemical Co., Ltd., CAS No. 68-12-2.

[0034] Sodium hydroxide, analytical grade, purity 96.0%, Tianjin Fengchuan Chemical Reagent Technology Co., Ltd., CAS No. 1310-73-2.

[0035] Hydrochloric acid, analytical grade, mass fraction 36% to 38%, Laiyang Kangde Chemical Co., Ltd.

[0036] Glucose, analytical grade, purity 99.0%, Tianjin Dingshengxin Chemical Co., Ltd., CAS No. 50-99-7 (glucose monohydrate).

[0037] Urea, analytical grade, purity 99.0%, Tianjin Dingshengxin Chemical Co., Ltd., CAS No. 57-13-6.

[0038] Potassium hydroxide, analytical grade, purity 85.0%, Tianjin Fengchuan Chemical Reagent Technology Co., Ltd., CAS No. 1310-58-3.

[0039] Argon, high-purity argon (5N grade), purity ≥99.999%, Jinan Deyang Special Gases Co., Ltd., packaged in steel cylinders to provide an inert protective atmosphere for the carbonization process.

[0040] Li6PS5Cl sulfide solid electrolyte, particle size 1μm to 5μm, ionic conductivity approximately 3mS / cm to 5mS / cm (25℃, 300MPa cold pressing), Hefei Kejing Materials Technology Co., Ltd., product number LPSC-1, sulfosilver germanium mineral type structure.

[0041] Lithium metal sheet, 0.1mm thick, 99.9% pure, Tianjin Zhongneng Lithium Industry Co., Ltd., is a battery-grade lithium sheet with a smooth, oxidation-free surface.

[0042] Acetylene black (conductive carbon black), battery grade, specific surface area 60m² 2 / g to 80m 2 / g, Shenzhen Kejing Zhida Technology Co., Ltd., oil absorption value 2.0-2.5mL / g.

[0043] Polyvinylidene fluoride (PVDF), battery grade, Kynar® HSV900, molecular weight approximately 1,000,000 (viscosity homopolymer), Arkema (France), is a VDF homopolymer powder suitable for lithium battery electrode binders.

[0044] Example 1: Raw material formula: 100g coal gangue, 1000mL N-methylpyrrolidone, 16.8g organic matter extract, 5.6g polyacrylonitrile, 202g N,N-dimethylformamide, 82.7g silica-alumina residue, 5.3g demineralized carbonaceous precursor, 10.6g glucose, 4.2g urea, and 16g potassium hydroxide.

[0045] Preparation process: Step 1: Pretreatment and fractional extraction of coal gangue. Weigh 100g of coal gangue and place it in a round-bottom flask equipped with a reflux condenser. Add 1000mL of N-methylpyrrolidone and extract with magnetic stirring in an oil bath at 190℃ for 10h. Filter to separate the filtrate and residue. The filtrate is then distilled under reduced pressure at 160℃ using a rotary evaporator to recover the solvent, yielding 16.8g of organic extract. The residue is washed three times each with anhydrous ethanol and deionized water, with a solid-liquid ratio of approximately 1:5 each time. It is then vacuum dried at 80℃ for 12h to obtain 82.7g of silica-alumina-rich residue. Step 2: Preparation of carbon fiber precursor spinning solution. Weigh 16.8g of organic extract and 5.6g of polyacrylonitrile, add them to 202g of N,N-dimethylformamide, and magnetically stir in a water bath at 65℃ for 8h to obtain a homogeneous spinning solution with a mass fraction of approximately 10%.

[0046] Step 3: Preparation of hard carbon precursor suspension. Weigh 82.7g of silica-alumina-rich residue and place it in a hydrothermal reactor. Add 580mL of 25% sodium hydroxide solution, seal, and react hydrothermally at 140℃ for 15h. Under these conditions, NaOH mainly reacts with aluminosilicate minerals to remove the silica-alumina components, while the carbonaceous components are retained due to their chemical inertness. The alkali leaching time is controlled within 15h to avoid excessive carbon loss. After cooling, filter, wash the filter residue with deionized water until neutral, add 12% hydrochloric acid, and leach at 70℃ for 5h. After washing with water until neutral, dry to obtain 5.3g of demineralized carbonaceous precursor. Weigh 5g of demineralized carbonaceous precursor, 10g of glucose, and 4g of urea, add to 266mL of deionized water, and ultrasonically disperse for 30min to obtain a suspension with a mass fraction of approximately 6.7%.

[0047] Step 4: Electrospinning and In-situ Loading. The spinning solution was loaded into a 5mL syringe using a No. 22 stainless steel needle. The spinning voltage was set to 18kV, the receiving distance to 18cm, the spinning rate to 1.0mL / h, the roller speed to 1000r / min, and the spinning time to 4h. The resulting precursor fiber membrane was removed and immersed in a hard carbon precursor suspension for 3h. After removal, it was vacuum dried at 70℃ for 6h to obtain a fiber membrane loaded with the hard carbon precursor.

[0048] Step 5, Pre-oxidation treatment. The fiber membrane is laid flat in a ceramic boat and placed in a muffle furnace. The temperature is increased to 260℃ at a rate of 1.5℃ / min under air atmosphere and held for 2 hours, then naturally cooled to room temperature. During pre-oxidation, the PAN molecular chains undergo cyclization and oxidation reactions, forming a heat-resistant ladder structure to prevent fiber melting and adhesion during carbonization. Simultaneously, oxygen-containing functional groups are introduced to provide active sites for the subsequent loading of hard carbon precursors.

[0049] Step Six: Gradient Carbonization Treatment. The pre-oxidized fiber membrane was placed in a tube furnace, and argon gas was introduced at a flow rate of 100 mL / min. The first stage involved heating to 450℃ at a rate of 4℃ / min and holding for 1.5 h; the second stage involved heating to 800℃ at a rate of 2.5℃ / min and holding for 2.5 h; the third stage involved heating to 1200℃ at a rate of 6℃ / min and holding for 1.5 h. The furnace was then cooled to room temperature, yielding approximately 14.2 g of the initial carbon fiber-hard carbon composite material.

[0050] Step 7, Surface etching treatment. Weigh 10g of the initial composite material, mix and grind it evenly with 15g of potassium hydroxide, place it in a tube furnace, and heat it to 700℃ at 5℃ / min under an argon atmosphere, holding it at that temperature for 45min. After cooling, remove it, wash it repeatedly with deionized water until the pH of the filtrate is neutral, and vacuum dry it at 100℃ for 12h to obtain the coal gangue-based carbon fiber-hard carbon composite anode material.

[0051] The composite material prepared in this embodiment has a carbon fiber mass fraction of approximately 62%, a hard carbon mass fraction of approximately 38%, and a specific surface area of ​​182 m². 2 / g, pore volume 0.38cm³ 3 / g, average pore size 5.2nm.

[0052] Example 2: Raw material formula: 100g coal gangue, 800mL N-methylpyrrolidone, 14.2g organic matter extract, 7.1g polyacrylonitrile, 192g N,N-dimethylformamide, 84.9g silica-alumina residue, 4.8g demineralized carbonaceous precursor, 9.6g glucose, 3.8g urea, and 14g potassium hydroxide.

[0053] Preparation process: Step 1: Pretreatment and fractional extraction of coal gangue. Weigh 100g of coal gangue and place it in a round-bottom flask equipped with a reflux condenser. Add 800mL of N-methylpyrrolidone and extract with magnetic stirring in an oil bath at 185℃ for 9 hours. Filter to separate the filtrate and residue. Recover the solvent by vacuum distillation of the filtrate at 160℃ using a rotary evaporator, yielding 14.2g of organic extract. Wash the residue three times each with ethanol and deionized water, and dry under vacuum at 80℃ for 12 hours to obtain 84.9g of silica-alumina-rich residue.

[0054] Step 2: Preparation of carbon fiber precursor spinning solution. Weigh 14.2g of organic extract and 7.1g of polyacrylonitrile, add them to 192g of N,N-dimethylformamide, and stir magnetically in a 60℃ water bath for 9h to obtain a homogeneous spinning solution with a mass fraction of approximately 10%.

[0055] Step 3: Preparation of hard carbon precursor suspension. Weigh 84.9g of silica-rich aluminum residue and place it in a hydrothermal reactor. Add 590mL of 22% sodium hydroxide solution, seal, and react hydrothermally at 130℃ for 16h. After cooling, filter. Wash the filter residue with deionized water until neutral, then add 10% hydrochloric acid and leach at 65℃ for 5h. Wash with water until neutral and dry to obtain 4.8g of demineralized carbonaceous precursor. Weigh 4.5g of demineralized carbonaceous precursor, 9g of glucose, and 3.6g of urea, add to 240mL of deionized water, and ultrasonically disperse for 30min to obtain a suspension with a mass fraction of approximately 6.7%.

[0056] Step 4: Electrospinning and In-situ Loading. The spinning solution was loaded into a 5mL syringe using a No. 22 stainless steel needle. The spinning voltage was set to 16kV, the receiving distance to 16cm, the spinning rate to 0.9mL / h, the roller speed to 900r / min, and the spinning time to 4h. The resulting precursor fiber membrane was removed and immersed in a hard carbon precursor suspension for 2.5h. After removal, it was vacuum dried at 65℃ for 8h to obtain a fiber membrane loaded with the hard carbon precursor.

[0057] Step 5, pre-oxidation treatment. The fiber membrane is laid flat in a ceramic boat and placed in a muffle furnace. The temperature is increased to 240°C at 1°C / min under air atmosphere, held at this temperature for 2.5 hours, and then naturally cooled to room temperature.

[0058] Step Six: Gradient Carbonization Treatment. The pre-oxidized fiber membrane was placed in a tube furnace, and argon gas was introduced at a flow rate of 100 mL / min. The first stage involved heating to 420℃ at a rate of 3℃ / min and holding for 2 hours; the second stage involved heating to 750℃ at a rate of 2℃ / min and holding for 3 hours; the third stage involved heating to 1150℃ at a rate of 5℃ / min and holding for 2 hours. The furnace was then cooled to room temperature, yielding approximately 12.7 g of the initial carbon fiber-hard carbon composite material.

[0059] Step 7, Surface etching treatment. Weigh 9g of the initial composite material, mix and grind it evenly with 13.5g of potassium hydroxide, place it in a tube furnace, and heat it to 650℃ at 5℃ / min under an argon atmosphere, holding it at that temperature for 50min. After cooling, remove it, wash it repeatedly with deionized water until the pH of the filtrate is neutral, and vacuum dry it at 100℃ for 12h to obtain the coal gangue-based carbon fiber-hard carbon composite anode material.

[0060] The composite material prepared in this embodiment has a carbon fiber mass fraction of approximately 68%, a hard carbon mass fraction of approximately 32%, and a specific surface area of ​​196 m². 2 / g, pore volume 0.42cm³ 3 / g, average pore size 4.8nm.

[0061] Example 3: Raw material formula: 100g coal gangue, 1200mL N-methylpyrrolidone, 19.7g organic matter extract, 4.9g polyacrylonitrile, 221g N,N-dimethylformamide, 79.8g silica-alumina residue, 5.9g demineralized carbonaceous precursor, 11.8g glucose, 4.7g urea, and 18g potassium hydroxide.

[0062] Preparation process: Step 1: Pretreatment and fractional extraction of coal gangue. Weigh 100g of coal gangue and place it in a round-bottom flask equipped with a reflux condenser. Add 1200mL of N-methylpyrrolidone and extract with magnetic stirring in an oil bath at 195℃ for 11h. Filter to separate the filtrate and residue. Recover the solvent by vacuum distillation of the filtrate at 160℃ using a rotary evaporator, yielding 19.7g of organic extract. Wash the residue three times each with ethanol and deionized water, and dry under vacuum at 80℃ for 12h to obtain 79.8g of silica-alumina-rich residue.

[0063] Step 2: Preparation of carbon fiber precursor spinning solution. Weigh 19.7g of organic extract and 4.9g of polyacrylonitrile, add them to 221g of N,N-dimethylformamide, and stir magnetically in a 70℃ water bath for 7h to obtain a homogeneous spinning solution with a mass fraction of approximately 10%.

[0064] Step 3: Preparation of hard carbon precursor suspension. 79.8 g of silica-rich aluminum residue was weighed and placed in a hydrothermal reactor. 560 mL of 28% sodium hydroxide solution was added, and the reactor was sealed and hydrothermally reacted at 145°C for 14 h. After cooling, the mixture was filtered, and the filter residue was washed with deionized water until neutral. Then, 14% hydrochloric acid was added, and the mixture was acid-leached at 75°C for 4.5 h. After washing with water until neutral, the residue was dried to obtain 5.9 g of demineralized carbonaceous precursor. 5.5 g of the demineralized carbonaceous precursor, 11 g of glucose, and 4.4 g of urea were weighed and added to 291 mL of deionized water. The mixture was ultrasonically dispersed for 30 min to obtain a suspension with a mass fraction of approximately 6.7%.

[0065] Step 4: Electrospinning and In-situ Loading. The spinning solution was loaded into a 5mL syringe using a No. 22 stainless steel needle. The spinning voltage was set to 20kV, the receiving distance to 19cm, the spinning rate to 1.1mL / h, the roller speed to 1100r / min, and the spinning time to 4h. The resulting precursor fiber membrane was removed and immersed in a hard carbon precursor suspension for 3.5h. After removal, it was vacuum dried at 75℃ for 5h to obtain a fiber membrane loaded with the hard carbon precursor.

[0066] Step 5, pre-oxidation treatment. The fiber membrane is laid flat in a ceramic boat, placed in a muffle furnace, and heated to 270°C at 2°C / min in an air atmosphere, held at that temperature for 1.5 hours, and then naturally cooled to room temperature.

[0067] Step Six: Gradient Carbonization Treatment. The pre-oxidized fiber membrane was placed in a tube furnace, and argon gas was introduced at a flow rate of 100 mL / min. The first stage involved heating to 480℃ at a rate of 5℃ / min and holding for 1 hour; the second stage involved heating to 850℃ at a rate of 3℃ / min and holding for 2 hours; the third stage involved heating to 1250℃ at a rate of 7℃ / min and holding for 1 hour. The furnace was then cooled to room temperature, yielding approximately 15.6 g of the initial carbon fiber-hard carbon composite material.

[0068] Step 7, Surface etching treatment. Weigh 11g of the initial composite material, mix and grind it evenly with 16.5g of potassium hydroxide, place it in a tube furnace, and heat it to 720℃ at 5℃ / min under an argon atmosphere, holding it at that temperature for 40min. After cooling, remove it, wash it repeatedly with deionized water until the pH of the filtrate is neutral, and vacuum dry it at 100℃ for 12h to obtain the coal gangue-based carbon fiber-hard carbon composite anode material.

[0069] The composite material prepared in this embodiment has a carbon fiber mass fraction of approximately 68%, a hard carbon mass fraction of approximately 32%, and a specific surface area of ​​168 m². 2 / g, pore volume 0.34cm³ 3 / g, average pore size 5.7nm.

[0070] Example 4: Raw material formula: 100g coal gangue, 1000mL N-methylpyrrolidone, 17.3g organic matter extract, 5.8g polyacrylonitrile, 208g N,N-dimethylformamide, 82.1g silica-alumina residue, 5.1g demineralized carbonaceous precursor, 10.2g glucose, 4.1g urea, and 20g potassium hydroxide.

[0071] Preparation process: Steps one through six are the same as in Example 1, except that the etching conditions in step seven are adjusted.

[0072] Step 7, Surface etching treatment. Weigh 10g of the initial composite material, mix and grind it evenly with 20g of potassium hydroxide, place it in a tube furnace, and heat it to 750℃ at 5℃ / min under an argon atmosphere, holding it at that temperature for 60min. After cooling, remove it, wash it repeatedly with deionized water until the pH of the filtrate is neutral, and vacuum dry it at 100℃ for 12h to obtain the coal gangue-based carbon fiber-hard carbon composite anode material.

[0073] The composite material prepared in this embodiment has a carbon fiber mass fraction of approximately 61%, a hard carbon mass fraction of approximately 39%, and a specific surface area of ​​211 m². 2 / g, pore volume 0.47cm³ 3 / g, average pore size 6.1nm.

[0074] Example 5: Raw material formula: 100g coal gangue, 1000mL N-methylpyrrolidone, 16.3g organic matter extract, 5.4g polyacrylonitrile, 195g N,N-dimethylformamide, 83.2g silica-alumina residue, 5.5g demineralized carbonaceous precursor, 11.0g glucose, 4.4g urea, and 10g potassium hydroxide.

[0075] Preparation process: Steps one through six are the same as in Example 1, except that the etching conditions in step seven are adjusted.

[0076] Step 7, Surface etching treatment. Weigh 10g of the initial composite material, mix and grind it evenly with 10g of potassium hydroxide, place it in a tube furnace, and heat it to 620℃ at 5℃ / min under an argon atmosphere, holding it at that temperature for 30min. After cooling, remove it, wash it repeatedly with deionized water until the pH of the filtrate is neutral, and vacuum dry it at 100℃ for 12h to obtain the coal gangue-based carbon fiber-hard carbon composite anode material.

[0077] The composite material prepared in this embodiment has a carbon fiber mass fraction of approximately 60%, a hard carbon mass fraction of approximately 40%, and a specific surface area of ​​139 m². 2 / g, pore volume 0.28cm³ 3 / g, average pore size 4.3nm.

[0078] Comparative Example 1: This comparative example is a blank comparative example, lacking carbon fiber components, and only using coal gangue-based hard carbon as the negative electrode material.

[0079] Raw material formula: 100g of coal gangue, 82.5g of silicon-aluminum rich residue, 5.1g of demineralized carbonaceous precursor, 10.2g of glucose, and 4.1g of urea.

[0080] Preparation process: Step 1: The preparation of silicon-rich aluminum residue is the same as Step 1 in Example 1.

[0081] Step two, the preparation of the demineralized carbonaceous precursor is the same as step three in Example 1.

[0082] Step 3: Mix 5g of demineralized carbonaceous precursor, 10g of glucose, and 4g of urea, add deionized water to prepare a suspension, and spray dry to obtain precursor powder. Place the precursor powder in a tube furnace under an argon atmosphere, heat to 800℃ at 3℃ / min, hold for 2 hours, then heat to 1200℃ at 5℃ / min, and hold for 1.5 hours. After cooling, obtain coal gangue-based hard carbon material. The hard carbon material prepared in this comparative example has a specific surface area of ​​92 m². 2 / g, pore volume 0.21cm³ 3 / g, average pore size 3.2nm.

[0083] Comparative Example 2: This comparative example lacks hard carbon components and only uses coal gangue-based carbon fiber as the negative electrode material.

[0084] Raw material formula: 100g coal gangue, 16.5g organic matter extract, 5.5g polyacrylonitrile, 198g N,N-dimethylformamide.

[0085] Preparation process: Step 1: The preparation of organic matter extract is the same as Step 1 in Example 1.

[0086] Step two, the preparation of the spinning solution is the same as step two in Example 1.

[0087] Step 3: Electrospinning is the same as step 4 in Example 1, except that hard carbon precursor impregnation is not performed.

[0088] Step four, the pre-oxidation treatment is the same as step five in Example 1.

[0089] Step 5, gradient carbonization treatment is the same as step 6 in Example 1.

[0090] Step six, surface etching treatment is the same as step seven in Example 1.

[0091] The carbon fiber material prepared in this comparative example has an average fiber diameter of 340 nm and a specific surface area of ​​162 m². 2 / g, pore volume 0.32cm³ 3 / g, average pore size 4.5nm.

[0092] Comparative Example 3: This comparative example does not undergo surface etching and examines the impact of gradient hole structure on performance.

[0093] Raw material formula: Same as in Example 1.

[0094] Preparation process: Steps one to six are the same as in Example 1, except that the surface etching process in step seven is not performed, and the carbonized composite material is directly used as the negative electrode material.

[0095] The specific surface area of ​​the composite material prepared in this comparative example is 108 m². 2 / g, pore volume 0.22cm³ 3 / g, average pore size 3.8nm.

[0096] Comparative Example 4: This comparative example was prepared using a method for preparing porous carbon anodes based on coal gangue.

[0097] Raw material formula: 50g coal gangue, 5g boric acid, 5g chitosan, 80g ethylene glycol, 20g deionized water.

[0098] Preparation process: Coal gangue was crushed to 200 mesh and carbonized at 850℃ for 2 hours under a nitrogen atmosphere. It was then acid-leached with 20% hydrochloric acid at 80℃ for 2 hours, washed with water until neutral, and dried to obtain a porous carbon precursor. Boric acid and chitosan were dissolved in a mixture of ethylene glycol and deionized water, and the porous carbon precursor was added and impregnated for 6 hours. The mixture was then heat-treated at 120℃ for 60 minutes. Finally, it was carbonized at 900℃ for 2 hours under a nitrogen atmosphere to obtain a multi-element doped porous carbon anode material.

[0099] The porous carbon material prepared in this comparative example has a specific surface area of ​​228 m². 2 / g, pore volume 0.51cm³ 3 / g, average pore size 2.9nm.

[0100] Comparative Example 5: This comparative example uses commercially available mesophase pitch-based carbon fiber as the anode material.

[0101] Raw material formula: Polyacrylonitrile-based carbon fiber, HF20 series (T300 grade), 7μm diameter, tensile strength 3530MPa, Jiangsu Hengshen Co., Ltd.

[0102] Preparation process: Carbon fibers were pulverized to a length of approximately 100 μm and used directly as a negative electrode material for testing.

[0103] The specific surface area of ​​the carbon fiber material in this comparative example is 14 m². 2 / g, carbon content 95.5%.

[0104] Comparative Example 6: This comparative example uses a mechanical blend of coal gangue-based hard carbon and commercial carbon fiber to examine the performance level of combining known coal gangue-based carbon materials and known carbon fiber anode materials in the prior art.

[0105] Raw material formula: 5g of coal gangue-based hard carbon, prepared using the same method as Comparative Example 1. 5g of commercial carbon fiber, with the same specifications and source as Comparative Example 5.

[0106] Preparation process: Coal gangue-based hard carbon and pulverized commercial carbon fibers were placed in a ball mill and ball-milled at 200 r / min for 2 h to obtain a mechanically blended composite material.

[0107] In this comparative example of a mixed material, the mass ratio of carbon fiber to hard carbon is 1:1, and the carbon fiber and hard carbon particles are in physical contact without a chemical bonding interface.

[0108] Comparative Example 7: This comparative example involves adding carbon fibers and phosphoric acid to coal gangue-based hard carbon for phosphorus doping, in order to examine the performance changes after adding known heteroatom doping methods on top of mechanical mixing.

[0109] Raw material formula: 8g of coal gangue-based hard carbon, prepared using the same method as Comparative Example 1. 2g of commercial carbon fiber, with the same specifications and source as Comparative Example 5. 1.5g of phosphoric acid, analytical grade, 85% by mass, from Tianjin Fengchuan Chemical Reagent Technology Co., Ltd.

[0110] Preparation process: Coal gangue-based hard carbon was mixed with pulverized commercial carbon fiber, impregnated with phosphoric acid solution for 2 hours, dried, and then heat-treated at 800°C for 1 hour under an argon atmosphere to obtain a doped and modified hybrid material.

[0111] The phosphorus content in this comparative material is approximately 2.1%, and the carbon fiber mass fraction is approximately 20%.

[0112] Performance testing: Test Methods: Electrochemical performance was tested using CR2032 button cells. The cells were assembled in an argon-atmosphere glove box, with water and oxygen content below 0.1 ppm. Working Electrode Preparation: Composite negative electrode material, acetylene black, and polyvinylidene fluoride were mixed in a mass ratio of 8:1:1. N-methylpyrrolidone was added and ground into a uniform slurry. This slurry was coated onto copper foil, vacuum dried at 80℃ for 12 hours, and then stamped into an electrode sheet with a diameter of 12 mm. The active material loading was approximately 1.5 mg / cm³. 2 The counter electrode is a lithium metal sheet, and the solid electrolyte is Li6PS5Cl. During assembly, a pressure of 200MPa is applied between the electrode and the electrolyte for 60s to ensure tight contact at the interface. The solid electrolyte sheet is approximately 500μm thick and 10mm in diameter, and is formed by pressing Li6PS5Cl powder under 300MPa.

[0113] Constant current charge / discharge test: The Blue Battery Testing System CT2001A was used for testing, with a voltage range of 0.01V to 3.0V and a test temperature of 25℃. Rate performance testing current densities were 0.1C, 0.2C, 0.5C, 1C, and 2C, each for 10 cycles. Cycle performance testing involved 100 charge / discharge cycles at a 0.5C current density. Capacity retention was calculated as the ratio of the discharge specific capacity at the 100th cycle to the discharge specific capacity at the 2nd cycle. The 1C current density was converted to the theoretical specific capacity of 400mAh / g, i.e., 400mA / g. Specific capacity calculation was based on the mass of active material. The battery was activated at 0.1C for two cycles before testing.

[0114] AC impedance testing: A CHI760E electrochemical workstation from Shanghai Chenhua Instruments Co., Ltd. was used, with a frequency range of 100kHz to 0.01Hz and an AC amplitude of 5mV. The test was conducted with the battery charged to 1.0V (relative to Li / Li). + The test was conducted in an open-circuit state at a temperature of 25°C, and the interface impedance value was fitted using an equivalent circuit.

[0115] Specific surface area and pore structure testing: A Micromeritics ASAP2460 specific surface area and pore size analyzer was used. Nitrogen adsorption-desorption tests were conducted at 77 K, and the samples were degassed at 200 °C for 6 h with a degassing vacuum degree below 0.01 Pa. The specific surface area was calculated using the BET method, and the pore size distribution and pore volume were calculated using the BJH method. The micropore size distribution was supplemented by the HK method. The test data were taken as the average of three parallel samples.

[0116] Test results: Table 1. Electrochemical performance test results of different samples: Table 2. Rate performance test results for different samples: Results analysis: Examples 1 to 5 describe coal gangue-based carbon fiber-hard carbon composite anode materials prepared under different process parameters. At a current density of 0.1C, the reversible specific capacity of these examples ranges from 456.3 mAh / g to 518.4 mAh / g, the initial coulombic efficiency ranges from 66.3% to 69.3%, the capacity retention after 100 cycles at 0.5C ranges from 87.6% to 92.5%, and the interfacial impedance ranges from 92 Ω to 140 Ω.

[0117] Examples 1 to 3 investigated the effects of extraction conditions on carbon composition distribution and final performance. Example 1 (extraction at 190°C for 10 hours, solid-liquid ratio 1:10) yielded approximately 62% carbon fiber, exhibiting balanced overall performance. Example 2 (lower extraction temperature, shorter extraction time, less organic matter extract, relatively higher PAN ratio) yielded approximately 68% carbon fiber, demonstrating superior rate performance and interfacial impedance (98Ω). This is because the higher carbon fiber content creates a more complete conductive network. Example 3 (more thorough extraction, more organic matter, relatively lower PAN ratio) yielded approximately 72% carbon fiber, with a lower hard carbon content, slightly lower capacity, and slightly higher impedance, indicating that insufficient hard carbon content reduces lithium storage sites.

[0118] Examples 1, 4, and 5 investigated the effect of surface etching degree on performance. Example 4 showed the deepest etching degree (KOH ratio 2:1, 750℃, 60 min) and the largest specific surface area (211 m²). 2The highest reversible capacity (518.4 mAh / g) was observed, but the cycling stability decreased slightly (87.6%). This is because excessive etching resulted in an overly porous material structure, leading to increased volume changes during cycling. Example 5 exhibited the shallowest etching (KOH ratio 1:1, 620°C, 30 min) and the smallest specific surface area (139 m² / g). 2 / g), with lower capacity but the best cycling stability (92.5%). The moderate etching conditions of Example 1 (KOH ratio 1.5:1, 700°C, 45 min) achieved the best balance between capacity and stability.

[0119] Comparative Example 1 is a single hard carbon material without carbon fibers, with a reversible specific capacity of only 352.7 mAh / g, a capacity retention of only 75.3% after 100 cycles, and an interfacial impedance as high as 254 Ω. Compared with Comparative Example 1, Example 1 shows a 39.1% increase in reversible specific capacity, a 15.1 percentage point increase in capacity retention, and a 55.9% decrease in interfacial impedance, indicating that the introduction of the carbon fiber network significantly improves the material's conductivity, structural stability, and interfacial contact performance.

[0120] Comparative Example 2 is a single carbon fiber material without hard carbon, with a reversible specific capacity of 370.8 mAh / g and an initial coulombic efficiency of only 59.5%. Compared with Comparative Example 2, Example 1 has a reversible specific capacity that is 30.3% higher, indicating that the hard carbon component provides the main lithium storage capacity, and the combination of the two achieves complementary performance advantages.

[0121] Comparative Example 3, the composite material without surface etching, exhibits a reversible specific capacity of 412.6 mAh / g and an interfacial impedance of 189 Ω, significantly higher than that of Example 1. This demonstrates that the gradient pore structure constructed by surface etching effectively increases the contact area between the material and the sulfide solid electrolyte, reduces the interfacial impedance, and simultaneously increases the number of lithium storage active sites.

[0122] Comparative Example 4 is a porous carbon anode based on coal gangue, which has a relatively high specific surface area (228 m²). 2 / g), but the reversible specific capacity and cycle stability are not as good as those of the embodiments of the present invention. The reason is that porous carbon particles lack a continuous electron transport network and the contact resistance between particles is large, which manifests as higher interface impedance in sulfide solid-state battery systems.

[0123] Comparative Example 5 is a commercially available pitch-based carbon fiber. Although it has a high initial coulombic efficiency (88.3%), its reversible specific capacity is only 281.5 mAh / g and its interfacial impedance is as high as 321 Ω. This indicates that the lithium storage capacity of traditional graphitized carbon fiber is limited, and the large fiber diameter (about 7 μm) results in insufficient effective contact area with the solid electrolyte.

[0124] Comparative Example 6 involved mechanically mixing coal gangue-based hard carbon with commercial carbon fiber. Known coal gangue-based carbon materials and known carbon fiber anodes were mixed.

[0125] The results showed that Comparative Example 6 had a reversible specific capacity of 333.4 mAh / g, a capacity retention of only 69.8% after 100 cycles, and an interface impedance of 276 Ω. All performance characteristics were significantly lower than those of Example 1 of this invention. Specifically, the reversible specific capacity was 32.1% lower than Example 1, the capacity retention was 20.6 percentage points lower, and the interface impedance was 146.4% higher. This is because mechanical mixing only involves physical contact; there is no chemical bonding interface between the carbon fiber and hard carbon particles, the electron transport path is discontinuous, and the uneven dispersion of both leads to agglomeration. The interpenetrating network structure and tightly bonded interface formed by in-situ loading and simultaneous carbonization in this invention are impossible to achieve with simple mechanical mixing.

[0126] Comparative Example 7 adds phosphorus doping to a mixture of hard carbon and carbon fiber. This comparative example incorporates the well-known technique of heteroatom doping.

[0127] The results showed that Comparative Example 7 had a reversible specific capacity of 365.1 mAh / g, a capacity retention of 74.2%, and an interface impedance of 239 Ω. Although this was slightly improved compared to Comparative Example 6, it was still significantly lower than that of Example 1. The reversible specific capacity of Example 1 was 34.1% higher than that of Comparative Example 7, indicating that the performance advantage of this invention does not stem from heteroatom doping itself, but rather from the synergistic construction of the carbon fiber-hard carbon interpenetrating network structure and the gradient pore interface. Simply adding dopants cannot fundamentally solve the problems of poor interfacial contact and discontinuous electron transport.

[0128] In summary, the carbon fiber-hard carbon interpenetrating network composite anode constructed by the present invention through processes such as graded extraction of coal gangue, in-situ composite and surface etching exhibits excellent comprehensive performance in sulfide solid-state battery systems.

[0129] The preferred embodiments of the present invention disclosed above are merely illustrative of the invention. These preferred embodiments do not exhaustively describe all details, nor do they limit the invention to the specific implementations described. Clearly, many modifications and variations can be made based on the content of this specification. This specification selects and specifically describes these embodiments to better explain the principles and practical applications of the invention, thereby enabling those skilled in the art to better understand and utilize the invention.

Claims

1. A coal gangue-based carbon fiber-hard carbon composite anode material, characterized in that, The composite anode material is composed of carbon fibers derived from organic matter extracted from coal gangue and hard carbon derived from silicon-aluminum-rich residue in situ, exhibiting an interpenetrating structure with a continuous carbon fiber network skeleton and hard carbon particles filling it; the specific surface area of ​​the composite anode material is 120 m². 2 / g to 220m 2 / g, pore volume 0.25cm³ 3 / g to 0.50cm 3 / g, with an average pore size of 3nm to 8nm.

2. The coal gangue-based carbon fiber-hard carbon composite anode material according to claim 1, characterized in that, The composite anode material contains 50% to 70% carbon fiber and 30% to 50% hard carbon by mass; the carbon fiber has a diameter of 200 nm to 500 nm and a specific surface area of ​​80 m². 2 / g to 150m 2 / g.

3. The coal gangue-based carbon fiber-hard carbon composite anode material according to claim 1, characterized in that, The composite anode material contains four heteroatoms: nitrogen, oxygen, silicon, and sulfur, with a total heteroatom content of 3.5% to 8.0%. The composite anode material has a gradient pore structure, with a surface pore size of 5 nm to 10 nm and an internal pore size of 1 nm to 3 nm.

4. A method for preparing the coal gangue-based carbon fiber-hard carbon composite anode material according to any one of claims 1 to 3, characterized in that, Includes the following steps: Step 1: Pretreatment and graded extraction of coal gangue. After crushing and ball milling, N-methylpyrrolidone is added for heating and extraction to separate organic matter extract and silica-alumina-rich residue. Step 2, preparation of carbon fiber precursor spinning solution: organic matter extract and polyacrylonitrile are mixed and dissolved in N,N-dimethylformamide to obtain spinning solution; Step 3: Preparation of hard carbon precursor suspension. The silica-rich aluminum residue is demineralized by hydrothermal alkaline leaching and acid leaching, then mixed with glucose and urea and dispersed in water to obtain a suspension. The hydrothermal alkaline leaching uses a 20% to 30% sodium hydroxide solution and reacts at 130°C to 150°C for 14 to 16 hours. The acid leaching uses a 10% to 15% hydrochloric acid solution and is carried out at 65°C to 75°C for 4.5 to 5.5 hours. Step 4: Electrospinning and in-situ loading. Electrospinning the spinning solution to obtain a precursor fiber membrane, and then immersing it in a suspension to impregnate the hard carbon precursor. Step 5, pre-oxidation treatment: The loaded fiber membrane is heated to 240°C to 270°C in air at a rate of 1°C to 2°C to 2°C to 1.5h to 2.5h for pre-oxidation. Step 6, gradient carbonization treatment: the pre-oxidized fiber membrane is subjected to three-stage gradient carbonization under an inert atmosphere. Step 7: Surface etching treatment. The carbonized composite material is mixed with potassium hydroxide and then etched at high temperature in an inert atmosphere to obtain the final product.

5. The preparation method according to claim 4, characterized in that, In step one, the extraction temperature is 180℃ to 200℃, the extraction time is 8h to 12h, and the solid-liquid ratio is 1:8 to 1:12; the coal gangue has a carbon content of 15% to 30%, a silicon dioxide content of 40% to 60%, and an aluminum oxide content of 15% to 25%.

6. The preparation method according to claim 4, characterized in that, In step two, the mass ratio of organic extract to polyacrylonitrile is 2:1 to 4:1, the mass fraction of spinning solution is 8% to 12%, and the viscosity-average molecular weight of the polyacrylonitrile is 80,000 to 120,000. In step four, the electrospinning parameters are: spinning voltage 15kV to 20kV, receiving distance 15cm to 20cm, spinning rate 0.8mL / h to 1.2mL / h, roller speed 800r / min to 1200r / min; and immersion time 2h to 4h.

7. The preparation method according to claim 4, characterized in that, The gradient carbonization conditions in step six are as follows: in the first stage, the temperature is increased to 400℃ to 500℃ at a rate of 3℃ / min to 5℃ / min and held for 1h to 2h; in the second stage, the temperature is increased to 700℃ to 900℃ at a rate of 2℃ / min to 3℃ / min and held for 2h to 3h; and in the third stage, the temperature is increased to 1100℃ to 1300℃ at a rate of 5℃ / min to 8℃ / min and held for 1h to 2h.

8. The preparation method according to claim 4, characterized in that, In step seven, the mass ratio of the composite material to potassium hydroxide is 1:1 to 1:2, the etching temperature is 600℃ to 750℃, and the etching time is 30min to 60min.

9. A solid-state battery based on a coal gangue-based carbon fiber composite negative electrode, comprising a positive electrode, a negative electrode, and a solid electrolyte, characterized in that, The negative electrode is the coal gangue-based carbon fiber-hard carbon composite negative electrode material according to any one of claims 1 to 3.

10. The solid-state battery according to claim 9, characterized in that, The solid electrolyte is a sulfide solid electrolyte, selected from at least one of the LiPSCl system and the Li-Ge-PS-Cl system.

Citation Information

Patent Citations

  • Preparation method of mesophase pitch-based carbon fiber

    CN106012106A