A sodium-rich composite sodium iron phosphate positive electrode material, a preparation method and application thereof

By employing a sol-gel combined two-stage calcination process and a CO reducing atmosphere generated by the decomposition of anhydrous oxalic acid, the limitations of sodium content and Fe²⁺ oxidation in composite sodium iron phosphate materials were solved, enabling the preparation of sodium-rich composite sodium iron phosphate cathode materials with high energy density and low energy consumption, thereby improving the electrochemical performance and stability of the materials.

CN123162168APending Publication Date: 2026-11-24GANNAN NORMAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611675737.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-28
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing composite sodium iron phosphate materials suffer from limitations in sodium content, easy oxidation of Fe²⁺, complex processes, and high energy consumption, making it difficult to meet the requirements for high energy density.

Method used

A two-stage calcination process combining sol-gel is adopted. The intense decomposition of anhydrous oxalic acid during the pre-calcination stage generates a CO reducing atmosphere to protect Fe²⁺, forming transient micropores. This induces excess sodium ions to embed into the interstitial spaces of the crystal lattice or occupy vacant sodium sites. The surface is then coated with an amorphous carbon film, which reduces the Na⁺ migration barrier.

Benefits of technology

The formation of a sodium-rich structure was achieved, which improved the specific capacity and electrochemical performance of the material, reduced energy consumption and production costs, avoided Fe²⁺ oxidation, and improved the stability and conductivity of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123162168A_ABST
    Figure CN123162168A_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of sodium iron phosphate cathode materials, in particular to a sodium-rich composite sodium iron phosphate cathode material, preparation method and application thereof, wherein the general chemical formula of the composite sodium iron phosphate cathode material is Na 4+m Fe3(PO4)2P2O7 / C, wherein 0<m≤0.2, and the surface of the composite sodium iron phosphate cathode material is coated with a 3-8 nm continuous amorphous carbon film. The preparation method provided by the invention adopts a sol-gel combined two-stage calcination process, and does not require a strong reducing atmosphere (such as hydrogen) in the whole process. The violent decomposition of anhydrous oxalic acid in the pre-calcination stage is used to generate a CO reducing atmosphere to protect Fe 2+ , while releasing gas to form instantaneous micropores, which effectively reduces the Na + migration barrier, induces excess sodium ions to intercalate into lattice gaps or occupy originally vacant specific sodium sites, and forms a unique sodium-rich structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of sodium iron phosphate cathode material technology, and in particular to a sodium-rich composite sodium iron phosphate cathode material, its preparation method, and its application. Background Technology

[0002] Sodium-ion batteries (SIBs) have attracted much attention in large-scale energy storage and low-speed electric vehicles due to the high abundance and wide distribution of sodium resources in the Earth's crust and their low cost. Composite sodium iron phosphate (Na4Fe3(PO4)2P2O7, NFPP), as a typical polyanionic cathode material, possesses a three-dimensional open framework structure, which facilitates the rapid transport of sodium ions. It also boasts advantages such as excellent thermal stability, low raw material cost, and environmental friendliness, making it considered one of the most promising cathode materials.

[0003] However, existing technologies for preparing composite sodium iron phosphate materials still have significant drawbacks: First, the limited sodium content leads to a capacity bottleneck. In Na4Fe3(PO4)2P2O7 synthesized by the traditional solid-state method, the sodium ion content strictly conforms to the stoichiometry. Limited by the number of specific sodium sites in the crystal structure, the actual specific capacity is usually only maintained at around 91 mAh / g, which is insufficient to meet the requirements for high energy density. Second, Fe... 2+ Easily oxidized, the iron in the composite sodium iron phosphate has a +2 valence. During the traditional high-temperature solid-state method (>700℃) preparation process, Fe... 2+ It is easily oxidized into electrochemically inert Fe. 3+ This leads to the formation of impurity phases in the material, severely degrading its electrochemical performance. Finally, the process is complex and energy-intensive; to avoid Fe... 2+ Oxidation, in existing technologies, often requires long-term calcination in a strong reducing atmosphere (such as a hydrogen-argon mixture), which increases process complexity, production costs, and safety hazards.

[0004] Therefore, it is necessary to develop a process that is simple, energy-efficient, and can overcome traditional sodium content limitations through structural regulation, effectively protecting Fe. 2+ The preparation method and materials are crucial. Summary of the Invention

[0005] The purpose of this invention is to provide a sodium-rich composite sodium iron phosphate cathode material, its preparation method, and its application. It employs a sol-gel combined two-stage calcination process, requiring no strong reducing atmosphere (such as hydrogen) throughout the process. The process utilizes the CO reducing atmosphere generated by the vigorous decomposition of anhydrous oxalic acid during the pre-calcination stage to protect the Fe... 2+ Simultaneously, the released gas forms instantaneous micropores, effectively reducing Na... + The migration barrier induces excess sodium ions to embed into interstitial spaces or occupy previously vacant sodium sites, forming a unique sodium-rich structure.

[0006] To achieve the above objective, the present invention provides a sodium-rich composite sodium iron phosphate cathode material, the general chemical formula of which is Na 4+m Fe3(PO4)2P2O7 / C, wherein 0<m≤0.2, and the surface of the composite sodium iron phosphate cathode material is coated with a 3-8 nm continuous amorphous carbon film.

[0007] Preferably, the main phase of the composite sodium iron phosphate cathode material is orthorhombic. Transient pores formed by decomposition gas of anhydrous oxalic acid induce excess sodium ions to intercalate into lattice gaps or occupy originally vacant sodium sites.

[0008] A preparation method of the sodium-rich composite sodium iron phosphate cathode material, for preparing the above composite sodium iron phosphate cathode material, comprises the following steps: S1: Weigh a sodium source, an iron source, a phosphorus source, a complexing agent and anhydrous oxalic acid according to a molar ratio, add them into deionized water and stir until dissolved, and heat in a water bath at 80-100°C after ball milling to obtain a gel precursor; S2: Perform high-temperature vacuum drying on the gel precursor obtained in S1, and fully grind it to obtain a precursor powder; S3: Pre-calcine the precursor powder obtained in S2 at 250-350°C for 2-4 hours in an inert gas atmosphere, where anhydrous oxalic acid decomposes to generate a reducing atmosphere and form pores. Continue heating at the same heating rate to 550-650°C for calcination for 8-12 hours, and cool down with the furnace to obtain the composite sodium iron phosphate cathode material.

[0009] Preferably, in S1, the molar ratio of the sodium source, the iron source, the phosphorus source and the complexing agent is 1.3-1.5:1:1-1.2:0.5-1.5.

[0010] Preferably, in S1, the phosphorus source includes at least one of ammonium dihydrogen phosphate, diammonium hydrogen phosphate and sodium dihydrogen phosphate; the molar ratio of the phosphorus source to anhydrous oxalic acid is 2-4:1.

[0011] Preferably, in S1, the sodium source includes at least one of anhydrous sodium carbonate, sodium dihydrogen phosphate, sodium acetate and sodium oxalate; the iron source includes at least one of iron phosphate, ferrous oxalate, ferric nitrate, ferric acetate, ferrous sulfate and ferric chloride; the complexing agent includes at least one of citric acid or oxalic acid.

[0012] Preferably, in S1, the ball milling speed is 200-400 r / min, the ball milling time is 150-200 min, and the ball milling medium is zirconia balls.

[0013] Preferably, in S2, the temperature of high-temperature vacuum drying is 110-120°C, and the time of high-temperature vacuum drying is 12-15 h.

[0014] Preferably, in S3, the heating rate is 1-3℃ / min, and the inert gas is nitrogen or argon.

[0015] An application of a sodium-rich composite sodium iron phosphate cathode material in the preparation of sodium-ion batteries.

[0016] Therefore, the present invention employs the above-mentioned sodium-rich composite sodium iron phosphate cathode material, its preparation method, and its application, and its beneficial effects are as follows: 1. In the sodium-rich composite sodium iron phosphate cathode material provided by the present invention, sodium ions not only occupy the conventional sites in the crystal lattice, but also induce excessive sodium ions to embed into the interstitial spaces of the crystal lattice or occupy the originally vacant specific sodium sites through the transient pores formed by the decomposition of oxalic acid, thus forming a sodium-rich structure. 2. The preparation method provided by this invention employs a sol-gel combined two-stage calcination process, which requires no strong reducing atmosphere (such as hydrogen) throughout the process and can be completed using inert gas protection. Compared with the traditional solid-state method, the calcination temperature is reduced by more than 100°C, the holding time is significantly shortened, which significantly reduces energy consumption and production costs, and avoids Fe... 2+ High-temperature oxidation; 3. The preparation method provided by this invention utilizes the vigorous decomposition of anhydrous oxalic acid during the pre-calcination stage to generate a CO reducing atmosphere to protect Fe. 2+ Simultaneously, the released gas forms instantaneous micropores, effectively reducing Na... + The migration barrier induces excess sodium ions to embed into the interstitial spaces of the crystal lattice or occupy specific sodium sites that were originally vacant, forming a unique sodium-rich structure that breaks through the sodium content limitations of traditional materials.

[0017] The technical solution of the present invention will be further described in detail below with reference to the accompanying drawings and embodiments. Attached Figure Description

[0018] Figure 1 This is the XRD pattern of Embodiment 1 of the present invention; Figure 2 This is the first charge-discharge curve of Embodiment 1 of the present invention; Figure 3 This is a rate performance diagram of Embodiment 1 of the present invention; Figure 4 This is a long-cycle performance diagram of Embodiment 1 of the present invention under 0.5C conditions; Figure 5 This is a SEM image of Embodiment 1 of the present invention. Detailed Implementation

[0019] The present invention will be further described below with reference to the accompanying drawings and examples. Unless otherwise defined, technical or scientific terms used in the present invention shall have the ordinary meaning as understood by those of ordinary skill in the art to which the present invention belongs. The features mentioned in the present invention or in the specific examples can be combined arbitrarily, and these specific examples are only used to illustrate the present invention and not to limit the scope of the present invention.

[0020] The present invention provides a method for preparing a sodium-rich composite sodium iron phosphate cathode material, wherein the general chemical formula of the composite sodium iron phosphate cathode material is Na 4+m Fe3(PO4)2P2O7 / C, where 0<m≤0.2, and the surface of the composite sodium iron phosphate cathode material is coated with a 3-8 nm continuous amorphous carbon film. In-situ pyrolytic carbon exists on the surface, and the generated amorphous carbon is not particle accumulation, but a continuous film seamlessly attached to the surface of crystal grains, which improves electronic conductivity, isolates the electrolyte from directly eroding active materials, enhances cycle stability, and simultaneously inhibits excessive growth of crystal grains.

[0021] In some embodiments of the present invention, the main phase of the composite sodium iron phosphate cathode material is orthorhombic (space group Pn21a), indicating that the final product has a pure crystal phase without generating inert Fe 3+ impurity phases. Transient pores formed by decomposition gas of anhydrous oxalic acid induce excess sodium ions to intercalate into lattice gaps or occupy originally vacant sodium sites. The present invention utilizes the transient pores generated by gas from anhydrous oxalic acid decomposition to impact the solid-phase precursor powder, reducing the Na + migration barrier. During high-temperature crystallization, excess Na in the raw materials + is filled into originally vacant Na sites or lattice gaps, increasing active sodium reserves.

[0022] A method for preparing a sodium-rich composite sodium iron phosphate cathode material, which prepares the above composite sodium iron phosphate cathode material, comprises the following steps: S1. Weigh a sodium source, an iron source, a phosphorus source, a complexing agent and anhydrous oxalic acid according to a molar ratio, add them to deionized water and stir until dissolved, and perform water bath heating at 80-100°C after ball milling to obtain a gel precursor; ball milling breaks particle agglomeration, increases reaction contact area, ensures uniform composition during subsequent water bath gelation, and avoids local segregation. Water bath heating promotes complexation and crosslinking of citric acid with Fe 3+ to form a wet gel with a three-dimensional network structure. As water evaporates, the solution viscosity increases sharply, eventually forming a dark green gel-like gel precursor. Na + , Fe 3+ , PO4 3- are immobilized in the gel skeleton, and phase separation is unlikely to occur after drying.

[0023] S2. The gel precursor in S1 is dried under high temperature and vacuum, and then ground thoroughly to obtain precursor powder. Vacuum lowers the boiling point of water, accelerates the removal of free water and some bound water, and obtains fluffy, porous amorphous precursor powder.

[0024] S3. The precursor powder from S2 is pre-calcined at 250-350℃ for 2-4 hours in an inert gas atmosphere. Anhydrous oxalic acid decomposes to generate a CO reducing atmosphere, which forms pores through CO and CO2. The heating rate is maintained, and the temperature is further increased to 550-650℃ for calcination for 8-12 hours. The material is then cooled in the furnace to obtain the composite sodium iron phosphate cathode material. The reducing atmosphere generated by the decomposition of anhydrous oxalic acid suppresses Fe... 2+ Oxidation occurs, and transient pores and sodium ion transport channels are formed in the phosphorus-oxygen tetrahedral network by releasing gaseous products.

[0025] At 250-350℃, the CO obtained from the decomposition of anhydrous oxalic acid reduces the +3 valence Fe in FePO4 to the +2 valence active state, avoiding the formation of Fe at high temperatures. 3+ Impurity phase. This stage mainly involves the decomposition of anhydrous oxalic acid and the initial condensation of the precursor. The gas from the decomposition of anhydrous oxalic acid escapes rapidly, releasing Na... + Diffusion microchannels.

[0026] At 550-650℃, the existing crystal nuclei are fully crystallized, transforming the amorphous precursor into a long-range ordered orthorhombic crystal system, and citric acid is completely decomposed into amorphous carbon. Slow cooling reduces lattice thermal stress and avoids microcracks. A final pure-phase sodium-rich structure is prepared, with the amorphous carbon film seamlessly bonded to the grains.

[0027] In some embodiments of the present invention, in S1, the molar ratio of sodium source, iron source, phosphorus source and complexing agent is 1.3-1.5:1:1-1.2:0.5-1.5.

[0028] In some embodiments of the present invention, in S1, the phosphorus source includes at least one of ammonium dihydrogen phosphate, diammonium hydrogen phosphate, and sodium dihydrogen phosphate; The molar ratio of phosphorus source to anhydrous oxalic acid is 2-4:1.

[0029] In some embodiments of the present invention, in S1, the sodium source includes at least one of anhydrous sodium carbonate, sodium dihydrogen phosphate, sodium acetate, and sodium oxalate; The iron source includes at least one of ferric phosphate, ferrous oxalate, ferric nitrate, ferric acetate, ferrous sulfate, and ferric chloride; The complexing agent includes at least one of citric acid or oxalic acid.

[0030] In some embodiments of the present invention, in S1, the ball milling speed is 200-400 r / min, the ball milling time is 150-200 min, and the ball milling medium is zirconia balls.

[0031] In some embodiments of the present invention, in step S2, the high-temperature vacuum drying temperature is 110-120°C, and the high-temperature vacuum drying time is 12-15 hours. This temperature setting avoids premature decomposition of citric acid and also prevents Fe from being oxidized by air.

[0032] In some embodiments of the present invention, in step S3, the heating rate is 1-3°C / min, and the inert gas is nitrogen or argon.

[0033] An application of a sodium-rich composite sodium iron phosphate cathode material in the preparation of sodium-ion batteries.

[0034] Example 1 S1. Weigh 7.43g of anhydrous sodium carbonate (sodium source), 15.18g of ferric phosphate (iron source), 13.79g of ammonium dihydrogen phosphate (phosphorus source), 25.21g of citric acid (complexing agent), and 5.7g of anhydrous oxalic acid in a molar ratio of 1.4:1:1.15:1.2. Add these to 70mL of deionized water and stir until dissolved. Ball mill the mixture using zirconia balls at 300r / min for 180min, then heat in a water bath at 90℃ to obtain a dark green gel precursor.

[0035] S2. The gel precursor in S1 is dried under high temperature and vacuum at 120°C for 12 hours to obtain precursor powder.

[0036] S3. The precursor powder from S2 is heated to 300°C in an inert nitrogen (99.99%) atmosphere at a heating rate of 2°C / min, and pre-calcined for 3 hours. Anhydrous oxalic acid decomposes to produce CO, and a reducing atmosphere is used to protect Fe. 2+ Pore ​​formation was achieved through instantaneous CO and CO2 reactions. The temperature was maintained at a rate of 2℃ / min and continued to rise to 600℃ for calcination for 10 hours. After furnace cooling, the composite sodium iron phosphate cathode material Na was obtained. 4.15 Fe3(PO4)2P2O7 / C (NFPP), such as Figure 5 As shown.

[0037] Example 2 S1. Weigh anhydrous sodium carbonate (sodium source), ferric phosphate (iron source), ammonium dihydrogen phosphate (phosphorus source), citric acid (complexing agent), and anhydrous oxalic acid in a molar ratio of 1.5:1:1.2:1.5:1.5. Add these to 70 mL of deionized water and stir until dissolved. Ball mill the mixture using zirconia balls at 350 rpm for 180 min, then heat in a water bath at 90 °C to obtain a dark green gel precursor.

[0038] S2. The gel precursor in S1 is dried under high temperature and vacuum at 120℃ for 10h and then thoroughly ground to obtain precursor powder.

[0039] S3. The precursor powder from S2 is heated to 320°C in an inert nitrogen (99.99%) atmosphere at a heating rate of 3°C / min, and pre-calcined for 2.5 hours. Anhydrous oxalic acid decomposes to produce CO, and a reducing atmosphere is used to protect Fe. 2+ Pore ​​formation was achieved through instantaneous CO and CO2 reactions. The temperature was maintained at a rate of 3℃ / min and continued to rise to 620℃ for calcination for 9 hours. After furnace cooling, the composite sodium iron phosphate cathode material Na was obtained. 4.2 Fe3(PO4)2P2O7 / C.

[0040] Example 3 S1. Weigh anhydrous sodium carbonate (sodium source), ferric phosphate (iron source), ammonium dihydrogen phosphate (phosphorus source), citric acid (complexing agent), and anhydrous oxalic acid in a molar ratio of 1.3:1:1.1:0.8:1.5, and add them to 80 mL of deionized water. Stir until dissolved. Ball mill the mixture using zirconia balls at 250 r / min for 200 min, and then heat in a water bath at 85 °C to obtain a dark green gel precursor.

[0041] S2. The gel precursor in S1 is dried under high temperature and vacuum at 100℃ for 14h to obtain precursor powder.

[0042] S3. The precursor powder from S2 is heated to 280°C in a nitrogen (99.99%) inert gas atmosphere at a heating rate of 1.5°C / min, and pre-calcined for 4 hours to produce CO by decomposition of anhydrous oxalic acid. Fe is protected under the original atmosphere. 2+ Pore ​​formation was achieved through instantaneous CO and CO2 reactions. The temperature was maintained at a rising rate and continued to rise to 560℃ for calcination for 11 hours, followed by furnace cooling to obtain the composite sodium iron phosphate cathode material Na. 4.08 Fe3(PO4)2P2O7 / C.

[0043] Comparative Example 1 Traditional solid-phase synthesis of Na4Fe3(PO4)2P2O7 / C typically involves weighing sodium source (Na2HPO4), iron source (FeC2O4·2H2O), phosphorus source (NH4H2PO4), and carbon source (citric acid, 6wt%) according to a Na:Fe:P molar ratio of 4:3:4.2 (with an additional 2-5% sodium added as needed to compensate for high-temperature volatilization). The raw materials are then dry-mixed or mixed with anhydrous ethanol / water and ball-milled for 6 hours to obtain a macroscopically homogeneous slurry. The precursor was then dried at 100℃ for 12 hours to remove the solvent. Next, the temperature was increased at 3℃ / min in a tube furnace under an inert Ar / N2 atmosphere (sometimes with a small amount of H2 added). It was first pre-calcined at 300℃ for 3 hours to decompose oxalate and organic matter and remove volatiles. Then, it was heated to 600℃ for 10 hours to allow PO4 and P2O7 units to crystallize on the FeO6 framework. After cooling in the furnace, it was ground and sieved to obtain the blackish-gray Na4Fe3(PO4)2P2O7 / C composite material.

[0044] Performance testing a. The composite sodium iron phosphate cathode material Na prepared in Example 1 4.15 XRD analysis was performed on Fe3(PO4)2P2O7 / C, and the results are as follows: Figure 1 As shown, the main phase is an orthorhombic Na4Fe3(PO4)2P2O7, and no obvious Fe was detected. 3+ Impurity peaks demonstrate that the low-temperature process effectively protects Fe. 2+ A distinct diffuse peak exists around 22°, corresponding to the presence of an amorphous sodium-rich phase; and the intensity ratio of the diffraction peaks of the (020) and (200) crystal planes, I(020) / I(200), is as high as 1.62, significantly higher than that of the traditional solid-state method product in Comparative Example 1 (theoretically usually <1.2), proving that the present invention successfully induced the intercalation of excess sodium ions and lattice distortion. Figure 1 (The red curve represents the NFPP sample) The main diffraction peaks are concentrated in the 30-35° range; the gradual rise of the baseline in the 15-20° region and the diffuse "bulge" near 22° directly reflect the existence of the amorphous sodium-rich phase; the diffraction peak group in the 30° to 60° range, combined with the intensity ratio analysis of the (020) / (200) plane, further supports the structural features of lattice distortion and excessive sodium embedding.

[0045] b. Using the composite sodium iron phosphate cathode material Na prepared in Example 1 4.15 A sodium-ion button cell was assembled using Fe3(PO4)2P2O7 / C (with metallic sodium as the negative electrode and a 1 mol / L NaPF6 EC / DMC = 1:1 solution as the electrolyte), and its electrochemical performance was tested. The results are as follows: Figure 2 As shown, at a 0.1C rate, the initial discharge specific capacity reaches 126.8 mAh / g. Rate performance is as follows... Figure 3 As shown, even at a high current density of 5C (500 mA / g), the discharge capacity still reaches 110.3 mAh / g, demonstrating excellent rate performance. Cycling performance is as follows... Figure 4 As shown, after 100 cycles at a 0.5C rate, the capacity retention rate reached 97.8%, demonstrating excellent structural stability.

[0046] c. Using the composite sodium iron phosphate cathode material Na prepared in Example 2 4.2 A sodium-ion button cell was assembled using Fe3(PO4)2P2O7 / C (with metallic sodium as the negative electrode and a 1 mol / L NaPF6 EC / DMC = 1:1 solution as the electrolyte). Electrochemical tests were conducted, and the initial discharge specific capacity at 0.1C rate was 126.2 mAh / g, the discharge capacity at 5C rate was 110.6 mAh / g, and the capacity retention rate after 100 cycles at 0.5C was 96.5%.

[0047] d. Using the composite sodium iron phosphate cathode material Na prepared in Example 3 4.08 A sodium-ion button cell was assembled using Fe3(PO4)2P2O7 / C (with metallic sodium as the negative electrode and a 1 mol / L NaPF6 EC / DMC = 1:1 solution as the electrolyte). Electrochemical tests were conducted, and the initial discharge specific capacity at 0.1C was 125.4 mAh / g, the discharge capacity at 5C was 111.9 mAh / g, and the capacity retention rate after 100 cycles at 0.5C was 96.2%.

[0048] Therefore, this invention employs the aforementioned sodium-rich composite sodium iron phosphate cathode material, its preparation method, and its application. It utilizes a sol-gel combined two-stage calcination process, eliminating the need for a strong reducing atmosphere (such as hydrogen) throughout the process. The intense decomposition of anhydrous oxalic acid during the pre-calcination stage generates a CO reducing atmosphere to protect the Fe... 2+ Simultaneously, the released gas forms instantaneous micropores, effectively reducing Na... + The migration barrier induces excess sodium ions to embed into interstitial spaces or occupy previously vacant sodium sites, forming a unique sodium-rich structure.

[0049] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and not to limit them. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can still be made to the technical solutions of the present invention, and these modifications or equivalent substitutions cannot cause the modified technical solutions to deviate from the spirit and scope of the technical solutions of the present invention.

Claims

1. A sodium-rich composite sodium iron phosphate cathode material, characterized in that: The general chemical formula of the composite sodium iron phosphate positive electrode material included is Na 4+m Fe3(PO4)2P2O7 / C, where 0<m≤0.2, and the surface of the composite sodium iron phosphate positive electrode material is coated with a 3-8 nm continuous amorphous carbon film.

2. The sodium-rich composite sodium iron phosphate cathode material according to claim 1, characterized in that: The main phase of the composite sodium iron phosphate cathode material is an orthorhombic crystal system. Through the transient pores formed by the decomposition of anhydrous oxalic acid gas, excess sodium ions are induced to embed into the interstitial lattice or occupy the originally vacant sodium sites.

3. A method for preparing a sodium-rich composite sodium iron phosphate cathode material, characterized in that: The preparation of the composite sodium iron phosphate cathode material according to any one of claims 1-2 includes the following steps: S1. Weigh out sodium source, iron source, phosphorus source, complexing agent and anhydrous oxalic acid by molar ratio, add to deionized water and stir until dissolved, ball mill and heat in a water bath at 80-100℃ to obtain gel precursor; S2. The gel precursor in S1 is dried under high temperature and vacuum, and then thoroughly ground to obtain precursor powder. S3. The precursor powder in S2 is heated and pre-calcined at 250-350℃ for 2-4 hours in an inert gas atmosphere. Anhydrous oxalic acid decomposes to generate a reducing atmosphere and create pores. The heating rate is maintained and the temperature is continued to rise to 550-650℃ for calcination for 8-12 hours. The composite sodium iron phosphate cathode material is obtained by furnace cooling.

4. The method for preparing a sodium-rich composite sodium iron phosphate cathode material according to claim 3, characterized in that: In S1, the molar ratio of sodium source, iron source, phosphorus source and complexing agent is 1.3-1.5:1:1-1.2:0.5-1.

5.

5. The method for preparing a sodium-rich composite sodium iron phosphate cathode material according to claim 3, characterized in that: In S1, the phosphorus source includes at least one of ammonium dihydrogen phosphate, diammonium hydrogen phosphate, and sodium dihydrogen phosphate. The molar ratio of phosphorus source to anhydrous oxalic acid is 2-4:

1.

6. The method for preparing a sodium-rich composite sodium iron phosphate cathode material according to claim 3, characterized in that: In S1, the sodium source includes at least one of anhydrous sodium carbonate, sodium dihydrogen phosphate, sodium acetate, and sodium oxalate; The iron source includes at least one of ferric phosphate, ferrous oxalate, ferric nitrate, ferric acetate, ferrous sulfate, and ferric chloride; The complexing agent includes at least one of citric acid or oxalic acid.

7. The method for preparing a sodium-rich composite sodium iron phosphate cathode material according to claim 3, characterized in that: In S1, the ball milling speed is 200-400 r / min, the ball milling time is 150-200 min, and the ball milling medium is zirconia balls.

8. The method for preparing a sodium-rich composite sodium iron phosphate cathode material according to claim 3, characterized in that: In S2, the temperature for high-temperature vacuum drying is 110-120℃, and the drying time is 12-15h.

9. The method for preparing a sodium-rich composite sodium iron phosphate cathode material according to claim 3, characterized in that: In S3, the heating rate is 1-3℃ / min, and the inert gas is nitrogen or argon.

10. An application of a sodium-rich composite sodium iron phosphate cathode material, characterized in that: The composite sodium iron phosphate cathode material according to any one of claims 1-2 is used in the preparation of sodium-ion batteries.