Magnesium-air battery anode material and preparation method thereof
By using a Mg-xLi-1Ca alloy structure and hot extrusion process, the problems of self-corrosion and hydrogen evolution side reaction in magnesium-air battery anode materials have been solved, resulting in anode materials with high discharge activity and stability, suitable for industrial production.
Patent Information
- Application Number
- CN202611471510.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-21
- Publication Date
- 2026-11-24
AI Technical Summary
Existing magnesium-air battery anode materials are severely limited by self-corrosion and hydrogen evolution side reactions, resulting in low anode efficiency. Current technologies cannot achieve a synergistic design of high discharge activity, self-corrosion inhibition, and discharge product film stability through simple and easily industrialized methods.
By employing a Mg-xLi-1Ca alloy structure and through the electrochemical synergistic effect of Li and Mg and the Ca-induced anodic Mg₂Ca phase regulation, combined with hot extrusion process, an appropriate amount of Li and finely dispersed Mg₂Ca phase were prepared to optimize the anodic reaction driving force and interfacial diffusion, thereby suppressing self-corrosion and hydrogen evolution reaction.
This process improves the discharge activity and utilization rate of magnesium anodes, suppresses self-corrosion and hydrogen evolution side reactions, achieves high-efficiency electrochemical performance and stable discharge product film, and is simple and easy to industrialize.
Smart Images

Figure CN123162170A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of battery materials technology, specifically relating to a magnesium-air battery anode material and its preparation method. Background Technology
[0002] With the continued depletion of traditional fossil fuels and the increasingly severe problem of greenhouse gas emissions, the development of efficient, clean, safe, and sustainable electrochemical energy conversion and storage systems has become an important development direction in the field of energy materials. Especially in special application scenarios such as seabed exploration, maritime rescue, field emergency response, mining, battlefield support, and natural disaster relief, power systems often need to simultaneously possess high energy density, long storage life, rapid start-up and shutdown capabilities, safety and reliability, and environmental adaptability. Therefore, developing new portable emergency power supplies capable of stably outputting electrical energy in complex environments has significant strategic importance and practical application value.
[0003] Metal-air batteries, such as zinc-air, aluminum-air, and magnesium-air batteries, are considered highly promising electrochemical energy storage and conversion systems because they utilize ambient oxygen as the cathode reactant, thus significantly increasing theoretical energy density. However, different systems still have significant limitations. Zinc-air batteries are prone to problems such as zinc dendrite growth, uneven deposition / dissolution, and limited oxygen transport during charge and discharge. Furthermore, their high overpotential during charging limits cycle performance. Aluminum-air batteries typically use strongly alkaline electrolytes (such as NaOH), which, while able to dissolve the discharge product Al(OH)3, result in a highly corrosive environment that leads to severe self-corrosion of the aluminum anode, battery structural failure, and electrolyte leakage risks, accompanied by severe hydrogen evolution side reactions.
[0004] In comparison, magnesium-air batteries exhibit superior overall performance compared to zinc- and aluminum-air systems due to magnesium's lower standard electrode potential (–2.37 V vs. SHE), higher theoretical specific capacity (2200 mA·h·g⁻¹), and higher energy density (6.8 kW·h·kg⁻¹). Their theoretical voltage can reach approximately 3.1 V. Furthermore, magnesium's abundant resources, low cost, and environmental friendliness make it a promising candidate for applications in emergency power supplies and off-grid energy systems.
[0005] However, the practical application of magnesium-air batteries is still severely limited by the self-corrosion behavior of magnesium anodes. In neutral or chlorine-containing electrolytes, magnesium anodes are prone to self-corrosion during open circuit and discharge processes, accompanied by significant hydrogen evolution reaction (HER). Simultaneously, magnesium anodes also exhibit a negative difference effect (NDE), meaning that the HER is not effectively suppressed when anodic polarization is enhanced, and may even be further exacerbated. These side reactions continuously consume active magnesium, reduce anode utilization, damage the stability of the discharge product film, and lead to a decrease in discharge voltage and energy conversion efficiency. Currently, the anode efficiency of most magnesium-based anode materials is less than 60%, which has become a key bottleneck restricting the actual energy density and engineering applications of magnesium-air batteries.
[0006] To improve the corrosion behavior of magnesium anodes, existing research mainly focuses on alloying strategies to control their microstructure and electrochemical properties, such as introducing Al, Zn, Sn, In, Ca, Li, and rare earth elements (REEs). However, these methods typically introduce a large number of cathodic second phases into the alloy. These second phases form microcouples with the magnesium matrix in the electrolyte, exacerbating localized corrosion and inducing non-uniform dissolution, thus making it difficult to fundamentally suppress the self-corrosion process. For example, patent CN111455248A uses the Zn / Ca ratio to form Ca2Mg6Zn3 and Mg2Ca phases to alleviate hydrogen evolution in NaCl solution and optimize the discharge process; patent CN115874100A uses a Mg–Zn–Er alloy to control the accumulation of discharge products and hydrogen evolution through a quasi-crystalline I phase; and patent CN111916766A uses a Mg–Bi–Ca–In extruded alloy to improve discharge performance through micro / nano second phases and fine-grained structure. However, the above-mentioned technical routes still mainly rely on strategies such as multi-element alloying, specific second phase construction, or redeposition of interface elements, which have problems such as complex alloy systems, increased material density, increased costs, or difficulty in accurately controlling the continuity of the second phase.
[0007] For Mg-Li alloys, patent CN119265454A uses spark plasma sintering (SPS) technology to prepare Mg-Li-Al-Zn-Y-Gd multi-element alloys. Although this can refine the grains and avoid the volatilization and oxidation of Li, the SPS process is expensive, has low production efficiency, and is difficult to scale up for continuous production of large-size plates, thus limiting its industrial application prospects. Patent CN119265455A adds Ga to the Mg-Ca base, utilizing Ga oxide films to improve corrosion resistance; however, Ga is a rare and dispersed metal, with high cost and limited resources.
[0008] Therefore, how to achieve high discharge activity, self-corrosion inhibition, reduced hydrogen evolution side reactions, and stable discharge product films in magnesium anodes through reasonable element selection and process design without excessively increasing the complexity and cost of the alloy system is a core problem that urgently needs to be solved in the design of magnesium-air battery anode materials. Current technology still lacks a magnesium-based anode material system that is relatively simple in composition, lightweight, and has an easily industrialized preparation process, and that can be synergistically designed from the perspectives of "microstructure regulation—interfacial electrochemical process optimization—side reaction inhibition." In particular, there is a lack of magnesium-air battery anode materials that can, through reasonable control of Li and Ca content, enable the second phase to both promote anode activation and avoid the formation of severe continuous corrosion channels. Summary of the Invention
[0009] The technical problem to be solved by the present invention is to provide a magnesium-air battery anode material and its preparation method. While maintaining the advantages of high theoretical capacity and low density of the Mg matrix, the anode activity is improved and non-uniform self-corrosion and blocky shedding are inhibited by the electrochemical synergy between Li and Mg and the Ca-induced anodic Mg2Ca phase regulation.
[0010] The technical solution adopted in this invention is as follows: A magnesium-air battery anode material with a structure of Mg- x Li-1Ca, by mass percentage, comprises: Li 0.50~10.50 wt.%; Ca 0.50~1.50 wt.%; The balance is Mg; Where x is the nominal mass percentage of Li, satisfying a Li mass percentage of 0.50–10.50%; the specific alloy is based on Mg- x The sequential representation of Li-1Ca.
[0011] An appropriate amount of Li solid dissolved in α The Mg matrix enters the electrolyte as Li⁺ during discharge, enhancing the driving force of the anodic reaction and interfacial diffusion kinetics; finely dispersed Mg₂Ca preferentially and uniformly dissolves, reducing local polarization. Continuous polarization occurs when the Li content is too high. β -Li networks will form through corrosion channels, so the present invention achieves a balance between activation and stability through the joint control of composition and hot extrusion structure.
[0012] Preferably, the Li content is 0.88 to 7.73 wt.% and the Ca content is 1.12 to 1.15 wt.%.
[0013] A method for preparing a magnesium-air battery anode material includes the following steps: S1. Melting and casting Mg- under argon protection xLi-1Ca alloy billet; S11. First, evacuate the melting chamber, then fill the melting chamber with protective gas for gas washing; S12. Add metallic magnesium, metallic calcium, and metallic lithium to a graphite crucible in sequence; heat in stages to completely melt the raw materials to obtain an alloy melt; wherein metallic lithium is pressed into the melt after magnesium and calcium have melted to reduce volatilization and oxidation; S13. Hold the alloy melt at a high-purity argon atmosphere for 10–20 min and stir to ensure uniform distribution of Li and Ca; S14. Remove oxides or slag from the surface of the alloy melt, and cast the melt into a preheated steel mold at 700–720°C to obtain Mg– x Li–1Ca alloy billet; S2. Cold treatment yields alloy ingots; S3. For the prepared Mg- x Li-1Ca alloy billets were hot-extruded to obtain Mg- x Li-1Ca alloy anode material.
[0014] Preferably, in step S11, the vacuum level of the melting chamber is evacuated to 20 Pa, and the protective gas is argon; the gas washing is repeated 2 to 3 times.
[0015] Preferably, in step S12, the purity of Mg metal is ≥99.97%, the purity of Li metal is ≥99.95%, and the purity of Ca metal is ≥99.75%.
[0016] Preferably, in step S12, the melting process adopts three-stage temperature control: first, the temperature is raised to 350-400℃ and held for 10-15 minutes, then the temperature is raised to 500-550℃ and held for 10-15 minutes, and finally the temperature is raised to 800-850℃, and after complete melting, it is held for 15-20 minutes.
[0017] Preferably, the final melting temperature is 830-850℃. After complete melting, the mixture is kept at this temperature for 20 minutes under the protection of high-purity argon and stirred evenly. Then, it is cast at 700-720℃.
[0018] Preferably, in step S13, argon gas with a purity of not less than 99.99% is continuously introduced as a protective gas to avoid using oxidizing gases that will react with highly reactive Li melt; after complete melting, the mixture is kept at a temperature for 10 to 20 minutes.
[0019] Preferably, room temperature water cooling is used in step S2.
[0020] Preferably, in step S3, the Mg- xThe preheating temperature of the Li-1Ca alloy billet is 300–370℃, the hot extrusion temperature is 280–330℃, the die temperature is 320–380℃, the extrusion ratio is (10–50):1, and the extrusion speed is 0.5–5 m / min. -1 .
[0021] Preferably, Mg- x The Li-1Ca alloy billet was preheated at 350℃, the hot extrusion temperature was 300℃, the die temperature was 350℃, the extrusion ratio was 30:1, and the extrusion speed was 1 m / min. -1 .
[0022] Preferably, in step S1, the raw materials must be baked in an oven at 90-110°C for 1-2 hours before melting to remove the moisture they contain. In step S3, Mg- is removed before hot extrusion. x The Li-1Ca alloy billet is preheated at 300-370℃ for 1-3 hours, preferably at 350℃; The Mg- prepared in this invention x Li-1Ca alloys can be used as anode materials in the preparation of magnesium-air batteries.
[0023] Technical principle: The Mg matrix provides high theoretical specific capacity and forms a continuous structure. α -Mg-supported phase; the standard electrode potential of Li (−3.04V vs. SHE) is more negative than that of Mg (−2.37V vs. SHE). Appropriate Li solid solution can increase the thermodynamic dissolution driving force of the Mg-based anode and reduce discharge polarization. During discharge, Li does not form insoluble deposits, but rather... + It enters the electrolyte, promoting interfacial mass transfer. The formation potential of Ca and Mg is lower than that of... α The Mg2Ca anodic second phase of Mg, with its fine and dispersed particles, preferentially dissolves as uniform activation sites, reducing the strong micro-galvanic corrosion caused by the cathodic second phase. The synergy of Mg, Li, and Ca is not a simple superposition, but is achieved through the combined effects of matrix capacity, soluble ion diffusion, anodic second phase distribution, and the dynamic evolution of the product film.
[0024] The role of Ca is mainly manifested in the regulation of microstructure and interface: Ca promotes the formation of fine and dispersed Mg2Ca phase and refines the microstructure; Mg(OH)2, MgO and CaCO3 were detected on the surface after discharge. This dynamic product layer is relatively intact on the surface of Mg–4Li–1Ca alloy, which can inhibit hydrogen evolution and self-corrosion, while not completely blocking anodic dissolution.
[0025] When the Li mass percentage is 3.71%, the Ca mass percentage is 1.15%, and the balance is Mg and unavoidable impurities, the resulting Mg-4Li-1Ca alloy maintains...α It possesses a Mg-based structure with optimized Mg2Ca volume fraction and dispersion state. Insufficient Li content results in limited activation and interfacial diffusion promotion; continuous Li content at 7.73% leads to... β -Li phase, preferential dissolution of Mg2Ca can induce β The -Li network continues to dissolve and form through-corrosion channels, leading to blocky detachment. Therefore, the Mg-4Li-1Ca alloy achieves optimal synergy between discharge activity, corrosion inhibition, and product film stability.
[0026] Compared with the prior art, the beneficial effects of the present invention are as follows: (1) This invention discloses and utilizes the synergistic effect of Mg and Li: the Mg matrix provides the main capacity and continuous structure, an appropriate amount of Li increases the driving force of the anodic reaction, and Li + It promotes interfacial diffusion; combined with the uniform activation effect of anodic Mg2Ca, the Mg–4Li–1Ca alloy has both high discharge voltage and anodic utilization rate.
[0027] (2) This invention avoids continuous defects in high-Li alloys by limiting the Li content and hot extrusion structure. β -Li network-induced through-corrosion and blocky detachment, transforming Mg2Ca from a potential corrosion source into a controllable anodic activation site.
[0028] (3) The present invention controls the final melting temperature at 700-720℃ and adopts a three-stage gradual heating and high-purity argon protection: the low and medium temperature sections ensure uniform heating of the charge, the high temperature section reduces local overheating, Li volatilization and melt oxidation; after complete melting, short-term heat preservation and stirring promote uniform composition. Combined with 350℃ billet preheating, 300℃ hot extrusion and 350℃ die temperature, the microstructure can be refined and the Mg2Ca distribution can be improved.
[0029] (4) Simple process and easy to industrialize: The present invention is prepared by conventional melting, casting, heating, extrusion and deformation process. Compared with the existing spark plasma sintering (SPS) technology, it has low equipment cost, high production efficiency, simple process and easy to industrialize. It is suitable for continuous production of large-size plates and has significant industrialization advantages. Attached Figure Description
[0030] Figure 1 The Mg- obtained in Examples 1-3 x SEM microstructure images and corresponding EDS elemental distribution diagrams of Li-1Ca anode materials, where a represents Mg-1Li-1Ca, b represents Mg-4Li-1Ca, and c represents Mg-8Li-1Ca.
[0031] Figure 2 The Mg- obtained in Examples 1-3 xPolarization curves of Li-1Ca anode material in 3.5 wt.% NaCl solution.
[0032] Figure 3 The Mg- obtained in Examples 1-3 x Nyquist plot (a) and Bode phase angle plot (b) of Li-1Ca anode material in 3.5 wt.% NaCl solution.
[0033] Figure 4 The Mg- obtained in Examples 1-3 x Equivalent circuit diagram of Li-1Ca anode material in 3.5 wt.% NaCl solution.
[0034] Figure 5 The Mg- obtained in Examples 1-3 x Hydrogen evolution curve of Li-1Ca anode material after immersion in 3.5 wt.% NaCl solution for 160 h.
[0035] Figure 6 The Mg- obtained in Examples 1-3 x Li-1Ca anode material was used to assemble a full cell in 3.5 wt.% NaCl solution at 2.5 mA cm⁻¹ –2 Voltage-time plot.
[0036] Figure 7 The Mg- obtained in Examples 1-3 x Li-1Ca anode material was used to assemble a full cell in 3.5 wt.% NaCl solution at 5 mA / cm². –2 Voltage-time plot.
[0037] Figure 8 The Mg- obtained in Examples 1-3 x Li-1Ca anode material was used to assemble a full cell in 3.5 wt.% NaCl solution at 10 mA cm⁻¹ –2 Voltage-time plot.
[0038] Figure 9 The Mg- obtained in Examples 1-3 x Li-1Ca anode material was used to assemble a full cell in 3.5 wt.% NaCl solution at 20 mA cm⁻¹ –2 Voltage-time plot. Detailed Implementation
[0039] The accompanying drawings are for illustrative purposes only; the invention will be further described in detail below with reference to specific embodiments. Unless otherwise specified, the equipment and reagents used in the embodiments and test examples are commercially available.
[0040] Example 1 The Mg-1Li-1Ca anode material of this embodiment is prepared from the following raw materials in weight percentages: Ca: 1.12%, Li: 0.88%, Mg: 98%. The purity of Mg is 99.99%, the purity of Li is 99.95%, and the purity of Ca is 99.75%.
[0041] A method for preparing a magnesium-air battery anode material includes the following steps: (1) Weigh the raw materials and pre-treat them to remove surface dirt and oxide scale. All raw materials must be baked in an oven at about 100°C for 1.5 hours before melting to remove the moisture they contain.
[0042] (2) Smelting: First, evacuate the melting chamber to a vacuum level of 20 Pa, then use a protective gas (argon) to purge the gas. Then, fill the melting chamber with a protective gas (gas partial pressure of -0.04 MPa) in a low vacuum state, and repeat this process three times.
[0043] First, place metallic magnesium and metallic calcium in a graphite crucible and heat it in stages under the protection of high-purity argon gas. After they melt, metallic lithium is pressed into the melt. Finally, the melt is completely melted at about 835℃ and held for 20 minutes. After stirring evenly, an alloy melt is obtained.
[0044] The smelting and heat preservation process is continuously protected with argon gas of no less than 99.99% purity; after removing surface slag, it is cast into a preheated steel mold at 720℃.
[0045] (3) Cooling: After casting, controlled water cooling or in-mold cooling is used to obtain an alloy ingot with dimensions of Φ40mm×60mm.
[0046] (4) Extrusion: The ingot is preheated to 350℃ and then hot extruded; the extrusion temperature is 300℃, the die temperature is 350℃, and the extrusion speed is 1m / min. -1 The extrusion ratio was 30:1. This parameter is consistent with the material preparation conditions in the English paper.
[0047] The middle area of the extruded sheet was selected as the test sample, denoted as Mg–1Li–1Ca, or LX11 for short.
[0048] Example 2 This embodiment provides a Mg-4Li-1Ca anode material, abbreviated as LX41, whose preparation method is basically the same as that in Example 1, the only difference being the weight percentage composition of each element in the alloy: The Mg-4Li-1Ca anode material of this embodiment is prepared from the following raw materials by weight percentage: Ca: 1.15%, Li: 3.71%, Mg: 95.14%. Among them, Ca, Li and Mg are all pure metals with a purity of 99.99%.
[0049] Example 3 This embodiment provides a Mg-8Li-1Ca anode material, abbreviated as LX81, whose preparation method is basically the same as that of Example 1, the only difference being the weight percentage composition of each element in the alloy.
[0050] The Mg-8Li-1Ca anode material of this embodiment is prepared from the following raw materials by weight percentage: Ca: 1.13%, Li: 7.73%, Mg: 91.14%. Among them, Ca, Li and Mg are all pure metals with a purity of 99.99%.
[0051] The magnesium-air battery anode materials prepared in Examples 1-3 of this invention were tested.
[0052] (1) Microstructure analysis like Figure 1 As shown, both Mg-1Li-1Ca and Mg-4Li-1Ca alloys are based on... α -Mg is the matrix and contains dotted Mg2Ca; continuous network structures also appear in Mg-8Li-1Ca alloys. β -Li phase. Mg2Ca phase relative to α The Volta potential difference of -Mg is approximately 105 mV. β -Li phase relative to α The potential difference between -Mg and Mg is approximately 55 mV, and both exhibit anodic second-phase behavior. In Mg-4Li-1Ca, the fine dispersion of Mg2Ca promotes uniform activation; the continuous dispersion in Mg-8Li-1Ca... β -Li tends to form continuous dissolution pathways.
[0053] (2) Polarization curve analysis like Figure 2 As shown, in a 3.5 wt.% NaCl solution, the corrosion potentials of Mg-1Li-1Ca, Mg-4Li-1Ca, and Mg-8Li-1Ca are −1.59, −1.49, and −1.54 V vs. SCE, respectively, and the self-corrosion current densities are 11.11, 7.10, and 15.56 μA / cm, respectively. -2 Mg-4Li-1Ca exhibits the lowest instantaneous self-corrosion current density and the largest impedance response, indicating that it has the best short-term interfacial stability.
[0054] (3) Electrochemical impedance spectroscopy like Figure 3 , 4 As shown, the alloys obtained in Examples 1-3 were placed in a 3.5 wt.% NaCl solution and electrochemical impedance spectroscopy was performed using a three-electrode system, wherein the reference electrode was a saturated calomel electrode and the counter electrode was a platinum electrode. Figure 3 In (a) the Nyquist curves, the Mg-4Li-1Ca alloy (LX41) has the largest capacitive arc diameter, and its real impedance extends to approximately 1700 Ω·cm. 2 It is significantly higher than that of Mg-8Li-1Ca alloy (LX81, approximately 1000 Ω·cm). 2 ) and Mg-1Li-1Ca alloy (LX11, approximately 400 Ω·cm) 2 This indicates that LX41 exhibits greater interfacial charge transfer resistance and a more stable surface film. The 15.84 Hz, 7.94 Hz, and 10 Hz values marked in the figure correspond to representative mid-to-high frequency response positions on each impedance arc; 199.52 mHz, 158.49 mHz, and 125.89 mHz correspond to low-frequency response positions, reflecting the corrosion reaction and surface film mass transfer process. LX41 maintains a high impedance in the low-frequency region, indicating that its corrosion product film has a stronger blocking effect on electrolyte penetration and charge transfer. Figure 3 In (b), LX41 exhibits the highest impedance modulus in the low-frequency region, along with the largest absolute value of the peak phase angle and a wider effective frequency range, indicating a more pronounced capacitive interface and a more continuous and dense surface film. LX11 has the lowest impedance modulus, and while LX81 shows increased activity due to the increased Li content, its continuous... β -Li phase and local dissolution channels can weaken the integrity of the film. Figure 4 The equivalent circuit further shows that LX11 and LX41 require solution resistance. R s Film response Q 1 and charge transfer response Q The results are described by two factors, and the response of LX81 can be simplified to a charge transfer process, reflecting a weakened surface film protective effect. These results are consistent with the polarization test results, where LX41 exhibits the highest corrosion potential (−1.49 V vs. SCE) and the lowest self-corrosion current density (7.10 μA cm⁻¹). -2 The results are consistent, indicating that an appropriate amount of Li and dispersed Mg2Ca synergistically form an organization state that combines activation ability and interfacial stability.
[0055] like Figure 4 As shown, the electrochemical impedance was measured using a Princeton V4 electrochemical workstation. The sample was immersed in the solution for 60 minutes and the measurement was performed when the sample was stable. The frequency range was 100 kHz-10 mHz, with 10 points per octave. The largest impedance modulus was observed at x=4, indicating that it has the best corrosion resistance in 3.5 wt.% NaCl solution.
[0056] (4) Hydrogen evolution test like Figure 5As shown, the hydrogen evolution rate of the three alloys was relatively high in the initial stage of immersion, then gradually decreased and tended to stabilize; the cumulative hydrogen evolution volume after 160 h was in the order of Mg-1Li-1Ca > Mg-4Li-1Ca > Mg-8Li-1Ca. The long-term hydrogen evolution and instantaneous polarization tests reflect different time scales, and the lower cumulative hydrogen evolution of Mg-8Li-1Ca does not negate its higher instantaneous self-corrosion current density.
[0057] (6) Full battery discharge test like Figures 6-9 As shown, at 1, 2.5, 5, 10, and 20 mA cm -2 Under these conditions, the average discharge voltage first increases and then decreases with increasing Li content, with the overall ranking being Mg-4Li-1Ca > Mg-8Li-1Ca > Mg-1Li-1Ca. Mg-4Li-1Ca has a more stable discharge plateau; Mg-1Li-1Ca is prone to blocky shedding, while Mg-8Li-1Ca, due to its continuous discharge... β -Li and Mg2Ca preferentially dissolve in sequence to form corrosion channels.
[0058] As can be seen from the above, the present invention uses Mg- x Using Li-1Ca alloy as the research object, by adjusting the Li content, the composition and quantity of the second phase were changed, which enhanced the discharge voltage of the magnesium anode during the discharge process and improved the discharge activity of the magnesium anode in the electrolyte. Mg-4Li-1Ca showed the best discharge voltage performance.
[0059] Comparative example (anode of AZ31 magnesium-air battery from literature) Literature reports that AZ31 alloy, in 3.5 wt.% NaCl and 20 mA cm⁻¹, -2 The average discharge voltage under the given conditions was approximately 1.10 V, and the anodic efficiency was 46.22%. After adding 3 vol.% glycerol to the electrolyte, the voltage and efficiency increased to 1.25 V and 65.12%, respectively (Inorg. Chem. Front., 2024, DOI:10.1039 / D4QI00803K).
[0060] The prior art uses its disclosed preparation and battery testing conditions; however, due to differences in electrode size, current, and discharge regime, its data are not directly incorporated into the embodiment table of this invention.
[0061] The above values are data from publicly available papers, not the applicant's actual measurements, and are only used for performance reference of the same magnitude; their alloy composition, air cathode, and electrolyte additive conditions are different from those of this invention.
[0062] Compared to AZ31, this invention does not rely on the Al-Zn cathode-type second phase or electrolyte organic additives, but achieves stable discharge through the anodic second phase and Li⁺ diffusion regulation within the Mg-Li-Ca ternary system.
[0063] Comparative Example 2 (Anode of Mg–5La magnesium-air battery from the literature) Literature reports that Mg-5La alloys at 20 mA cm -2 Under the given conditions, the anodic efficiency was 57.67%, and the specific discharge capacity was 1259.45 mA·hg. -2 (J. Alloys Compd. 2023, DOI:10.1016 / j.jallcom.2022.167170).
[0064] The above values are from published papers. The testing system is used to evaluate similar magnesium-air battery anodes. The data serve as a reference for the performance of existing materials and are not presented as comparative experiments conducted by the applicant.
[0065] The published results show that Mg-5La at 20 mA cm⁻¹ -2 The anodic efficiency and specific capacity of the alloy were both lower than the highest performance levels achieved by the Mg–4Li–1Ca alloy in the English paper.
[0066] This comparison demonstrates that while using a rare earth anode second phase can improve discharge, the present invention achieves better capacity utilization and stability without introducing a high content of rare earth elements through the synergy of low-density Li and Mg matrix and the regulation of dispersed Mg2Ca.
[0067] Electrochemical and 10 mA cm in Examples 1-3 -2 The discharge data are summarized in Table 1; the comparative examples in the literature are listed separately in their respective comparative examples due to differences in testing systems and battery configurations, and are not statistically compared with the applicant's sample data under the same conditions.
[0068] Table 1. Mg1- obtained in Examples 1-3 x Electrochemical performance of Li-1Ca alloy anode material As shown in Table 1, the Mg-4Li-1Ca alloy has the lowest self-corrosion current density, which is within 10 mA cm⁻¹. -2 It exhibits the highest and most stable average discharge voltage and high anodic efficiency. Combined with microstructure and surface analysis, its advantages stem from… α The synergistic effect of Mg capacity matrix, Li activation and Li⁺ interfacial diffusion, uniform activation of dispersed Mg₂Ca and inhibition of self-corrosion by dynamic product film.
[0069] Example 4 A method for preparing a magnesium-air battery anode material, wherein the alloy anode material in this embodiment has a structure of Mg-2Li-1Ca, includes the following steps: (1) Weigh the raw materials and pre-treat them to remove surface dirt and oxide scale. All raw materials must be baked in an oven at about 100°C for 1.5 hours before melting to remove the moisture they contain.
[0070] (2) Melting: First, the vacuum degree of the melting chamber is evacuated to 20 Pa, and then the protective gas (argon) is used for purging. The protective gas (gas partial pressure of -0.04 MPa) is then introduced into the melting chamber under low vacuum, and this process is repeated three times. First, metallic magnesium and metallic calcium are placed in a graphite crucible and heated in stages under the protection of high-purity argon. After they melt, metallic lithium is pressed into the melt, and finally, it is completely melted at about 835℃ and held for 20 minutes. After stirring evenly, an alloy melt is obtained. Argon with a purity of not less than 99.99% is continuously used for protection during the melting and holding process. After removing the surface slag, it is cast into a preheated steel mold at 720℃.
[0071] (3) Cooling: After casting, controlled water cooling or in-mold cooling is used to obtain an alloy ingot with dimensions of Φ40mm×60mm.
[0072] (4) Extrusion: The ingot is preheated to 350℃ and then hot extruded; the extrusion temperature is 300℃, the die temperature is 350℃, and the extrusion speed is 1m / min. -1 The extrusion ratio is 30:1.
[0073] The middle area of the extruded sheet was selected as the test sample, denoted as Mg-2Li-1Ca, or LX21 for short.
[0074] Example 5 The difference from Example 4 is that the alloy anode material structure in this example is Mg-6Li-1Ca. The middle region of the extruded sheet is selected as the test sample, denoted as Mg-6Li-1Ca, or simply LX61.
[0075] Example 6 The difference from Example 4 is that the alloy anode material structure in this example is Mg-9Li-1Ca. The middle region of the extruded sheet is selected as the test sample, denoted as Mg-9Li-1Ca, or simply LX91.
[0076] Electrochemical testing showed that LX41 exhibited the highest corrosion potential (Ecorr = −1.49 V vs. SCE) and the lowest self-corrosion current density (7.10 μA / cm²). -2 The LX21, LX61, and LX91 are all inferior to the LX41. This further confirms... x =4 is the optimal amount of Li to add.
[0077] Example 7 The Mg-4Li-1Ca anode material of this embodiment is prepared from the following raw materials in weight percentages: Ca: 1.12%, Li: 3.71%, Mg: 95.17%. The purity of Mg is 99.99%, the purity of Li is 99.95%, and the purity of Ca is 99.75%.
[0078] A method for preparing a magnesium-air battery anode material includes the following steps: (1) Weigh the raw materials for pretreatment: Weigh the magnesium source, lithium source and calcium source according to the ratio, and remove surface dirt and oxide scale. All raw materials must be baked in an oven at 100°C for 1.5 hours before smelting to remove the moisture they contain.
[0079] (2) Melting: First, the vacuum degree of the melting chamber is evacuated to 20Pa, then high-purity argon is used for gas washing, and protective gas (gas partial pressure of -0.04MPa) is introduced into the melting chamber under low vacuum state. This is repeated three times.
[0080] First, place metallic magnesium and metallic calcium in a graphite crucible and heat them in a three-stage gradient under the protection of high-purity argon: first, heat to 350℃ and hold for 15 minutes, then heat to 500℃ and hold for 15 minutes; finally, heat to 830℃, melt completely, and hold for 15 minutes to obtain a homogeneous alloy melt.
[0081] The smelting and heat preservation process is continuously protected with argon gas of no less than 99.99% purity; after removing surface slag, it is cast into a preheated steel mold at 720℃.
[0082] (3) Cooling: After casting, controlled water cooling or in-mold cooling is used to obtain an alloy ingot with dimensions of Φ40mm×60mm.
[0083] (4) Extrusion: The ingot is preheated to 350℃ and then hot extruded; the extrusion temperature is 300℃, the die temperature is 350℃, and the extrusion speed is 1m / min. -1 The extrusion ratio is 30:1.
[0084] The middle area of the extruded sheet was selected as the test sample and denoted as LX4A.
[0085] Example 8 The only difference between this embodiment and Embodiment 7 is the three-stage gradient heating regime in the melting process: first, the temperature is raised to 380°C and held for 10 minutes; then, it is raised to 520°C and held for 10 minutes; finally, it is raised to 840°C, completely melted at 840°C, and held for 15 minutes; the casting temperature is 715°C. The remaining raw material proportions, pretreatment, cooling, and extrusion steps are the same as in Embodiment 7.
[0086] The middle area of the extruded sheet was selected as the test sample and denoted as LX4B.
[0087] Example 9 The only difference between this embodiment and Embodiment 7 is the three-stage gradient heating regime in the melting process: first, the temperature is raised to 400°C and held for 10 minutes; then, it is raised to 550°C and held for 10 minutes; finally, the temperature is raised to 850°C, and after complete melting at 850°C, it is held for 15 minutes; the casting temperature is 710°C. The remaining raw material proportions, pretreatment, cooling, and extrusion steps are the same as in Embodiment 7.
[0088] The middle area of the extruded sheet was selected as the test sample and denoted as LX4C.
[0089] Example 10 The only difference between this embodiment and Embodiment 7 is the three-stage gradient heating regime in the melting process: first, the temperature is raised to 350°C and held for 15 minutes; then, it is raised to 500°C and held for 15 minutes; finally, the temperature is raised to 830°C, and after complete melting at 830°C, it is held for another 20 minutes; the casting temperature is 720°C. The remaining raw material proportions, pretreatment, cooling, and extrusion steps are the same as in Embodiment 7.
[0090] The middle area of the extruded sheet was selected as the test sample and denoted as LX4D.
[0091] The final melting temperature in Example 9 was too high (850°C). Although this was beneficial for the complete melting of the alloy, the high temperature would exacerbate the volatilization of Li (Li has a melting point of 180.5°C and a boiling point of 1342°C), causing the actual Li composition to deviate from the design value and accelerating crucible erosion. Examples 7 and 8 had relatively short final holding times (15 min). While this saved melting time, sufficient diffusion time is required for the complete alloying of magnesium and calcium. Insufficient holding time could lead to uneven composition, affecting the uniformity of the second phase distribution and thus preventing optimal electrochemical performance. Example 10, by extending the intermediate holding time to 15 min under a mild temperature gradient, balanced the requirements of "composition homogenization" and "controlling Li volatilization," representing the optimal gradient heating process.
[0092] Comparative Example 3: The temperature was directly increased to the maximum temperature without gradient heat preservation.
[0093] The preparation method of the Mg-4Li-1Ca anode material in this comparative example differs from that in Example 7 in that: First, place metallic magnesium and metallic calcium in a graphite crucible and directly heat them under the protection of high-purity argon: directly heat from room temperature to 830℃ until completely melted, then hold at that temperature for 20 minutes and stir evenly to obtain the alloy melt.
[0094] The middle area of the extruded sheet was selected as the test sample and denoted as DX4-1.
[0095] Comparative Example 4: Heating is performed in two stages, not in a three-stage gradient.
[0096] The preparation method of the Mg-4Li-1Ca anode material in this comparative example differs from that in Example 7 in that: First, place metallic magnesium and metallic calcium in a graphite crucible and heat them in two stages under the protection of high-purity argon: first, heat to 400℃ and hold for 15 minutes, then directly heat to 830℃ until completely melted, hold for 20 minutes and stir evenly to obtain the alloy melt.
[0097] The middle area of the extruded sheet was selected as the test sample, denoted as DX4-2.
[0098] The test results of Example 10 were compared with those of Comparative Examples 3 and 4, and the results are shown in Table 2.
[0099] Table 2 Comparison of test results between Example 10 and Comparative Examples 3-4 As shown in Table 2, the overall performance of the alloy materials prepared in Comparative Examples 3 and 4 is lower than that in Example 10. In Example 10, after a three-stage gradient heating process, the self-corrosion current density was approximately 7.10 μA / cm². -2 At 10mA cm -2 The average discharge voltage under direct heating was approximately 1.34 V, and the anode efficiency was approximately 72%; the comparative example 3, with direct heating, had an average discharge voltage of approximately 18.5 μA / cm. -2 The comparative example 4, with two temperature increases of 1.25V and 52%, had an amplification value of approximately 13.8 μA cm⁻¹. -2 1.29V and 59%. This indicates that staged heating and heat preservation are beneficial for uniform heating of the charge, reducing local overheating and Li volatilization, and promoting the homogenization of Mg, Li and Ca composition, thereby obtaining finer grains and a more uniformly dispersed second phase; direct heating or reducing the intermediate heat preservation stage can easily cause compositional segregation and local aggregation of the second phase, leading to increased self-corrosion, decreased discharge voltage and anodic efficiency.
[0100] Of course, the above description is not intended to limit the present invention, and the present invention is not limited to the examples given above. Any changes, modifications, additions or substitutions made by those skilled in the art within the scope of the present invention should also fall within the protection scope of the present invention.
Claims
1. A magnesium-air battery anode material, characterized in that, The structure is Mg- x Li-1Ca, by mass percentage, comprises: Li 0.50~10.50 wt.%; Ca 0.50~1.50 wt.%; The balance is Mg; Where x is the nominal mass percentage of Li, which satisfies the mass percentage of Li being 0.50 to 10.50%.
2. The magnesium-air battery anode material according to claim 1, characterized in that, The content of Li is 0.88 to 7.73 wt.%, and the content of Ca is 1.12 to 1.15 wt.%.
3. A method for preparing a magnesium-air battery anode material as described in claim 1 or 2, characterized in that, Includes the following steps: S1. Melting and casting Mg- under argon protection x Li-1Ca alloy billet; S11. First, evacuate the melting chamber, then fill the melting chamber with protective gas for gas washing; S12. Add metallic magnesium, metallic calcium, and metallic lithium sequentially to a steel crucible; heat in stages to completely melt the raw materials and obtain an alloy melt; S13. The alloy melt is kept at a constant temperature under the protection of high-purity argon gas to ensure uniform distribution of Li and Ca; S14. Remove oxides or slag from the surface of the alloy melt, and cast the melt into a preheated steel mold at 700–720°C to obtain Mg- x Li-1Ca alloy billet; S2. Cold treatment yields alloy ingots; S3. For the prepared Mg- x Li-1Ca alloy billets were hot-extruded to obtain Mg- x Li-1Ca alloy anode material.
4. The method for preparing a magnesium-air battery anode material according to claim 3, characterized in that, In step S11, the melting chamber is evacuated to 20 Pa and then filled with argon gas with a purity of not less than 99.99%. The evacuation and argon filling process is repeated 2 to 3 times.
5. The method for preparing a magnesium-air battery anode material according to claim 3, characterized in that, In step S12, the purity of Mg metal is ≥99.99%, the purity of Li metal is ≥99.95%, and the purity of Ca metal is ≥99.75%.
6. The method for preparing a magnesium-air battery anode material according to claim 3, characterized in that, In step S12, the melting process adopts a three-stage heating process: first, the temperature is raised to 350-400℃ and held for 10-15 minutes; then the temperature is raised to 500-550℃ and held for 10-15 minutes; finally, the temperature is raised to 800-850℃, and after complete melting, it is held for 15-20 minutes. The melting and holding process is protected by argon gas with a purity of not less than 99.99%.
7. The method for preparing a magnesium-air battery anode material according to claim 3, characterized in that, In step S2, room temperature water cooling is used.
8. The method for preparing a magnesium-air battery anode material according to claim 3, characterized in that, In step S3, Mg- x The preheating temperature of the Li-1Ca alloy billet is 300–370℃, the hot extrusion temperature is 280–330℃, the die temperature is 320–380℃, the extrusion ratio is 10–50:1, and the extrusion speed is 0.5–5 m / min. -1 .
9. The method for preparing a magnesium-air battery anode material according to claim 8, characterized in that, The alloy billet is preheated at 350°C, hot extrusion at 300°C, die at 350°C, extrusion ratio at 30:1, and extrusion speed at 1 m / min. -1 .
10. The method for preparing a magnesium-air battery anode material according to claim 3, characterized in that, In step S1, the raw materials must be baked in an oven at 90-110°C for 1-2 hours before melting to remove the moisture they contain. In step S3, Mg- is removed before hot extrusion treatment. x The Li-1Ca alloy billet is preheated at 300-370℃ for 1-3 hours.
Citation Information
Patent Citations
Aluminum alloy bar and application thereof in field of rail transit
CN119265454A
High-toughness high-thermal-conductivity high-temperature-resistant aluminum alloy and preparation method thereof
CN119265455A