A non-active element doped high-entropy p2-type sodium-ion battery cathode material and a preparation method thereof
High-entropy P2-type sodium-ion battery cathode materials were prepared by sol-gel synthesis, overcoming the limitations of P2-type materials in terms of overall performance. This resulted in sodium-ion battery cathode materials with high energy density, long cycle life, and air stability, making them suitable for large-scale industrial production.
Patent Information
- Application Number
- CN202611328943.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-31
- Publication Date
- 2026-11-24
AI Technical Summary
Existing technologies struggle to achieve a comprehensive performance of high phase transition reversibility, voltage stability, air storage stability, and long cycle life in P2-type sodium-ion battery cathode materials. Furthermore, traditional synthesis methods are prone to elemental segregation and phase separation, making it difficult to form high-entropy single-phase solid solutions.
The sol-gel synthesis route is adopted, and a transparent gel is formed in the liquid phase environment by using a complexing agent to ensure the uniform dispersion of various inactive elements. High-entropy P2 type sodium-ion battery cathode material is formed by high-temperature sintering. The chelating effect of the complexing agent is used to suppress metal ion segregation at the microscale, forming a long-range disordered high-entropy single-phase solid solution.
A P2-type sodium-ion battery cathode material with high energy density, high power density, and long cycle life has been developed. It suppresses harmful phase transitions, improves the material's air stability and electrochemical performance, reduces costs, and broadens application scenarios.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] This invention relates to the field of sodium-ion batteries, specifically to a high-entropy P2 type sodium-ion battery cathode material doped with inactive elements and its preparation method. Background Technology
[0002] With the advancement of "dual carbon" goals and the large-scale development of renewable energy, the importance of electrochemical energy storage technology is becoming increasingly prominent. Lithium-ion batteries face severe limitations in large-scale energy storage applications due to limited and unevenly distributed lithium resources and continuously rising costs. Sodium-ion batteries, with their abundant sodium resources, low cost, and similar working principle to lithium-ion batteries, are considered an ideal choice for large-scale energy storage.
[0003] In sodium-ion battery cathode materials, layered transition metal oxides have attracted widespread attention due to their high theoretical specific capacity and relatively simple synthesis process. Based on the different oxygen layer stacking methods and sodium ion coordination modes, layered oxides are mainly classified into O3 type and P2 type. Among them, P2 type materials have larger interlayer spacing and open sodium ion diffusion channels, which are conducive to the rapid migration of sodium ions, exhibiting better rate performance and cycle performance.
[0004] However, when P2-type layered oxides are charged to high voltages, the transition metal layer is prone to slippage, inducing harmful phase transitions such as P2→O2 or P2→OP4. This is accompanied by drastic changes in lattice volume, leading to particle pulverization and rapid capacity decay. Furthermore, P2-type materials are highly sensitive to air and moisture, easily forming residual alkali on the surface and undergoing structural degradation, increasing the difficulty of storage and electrode fabrication. These problems severely restrict the practical application of P2-type sodium-ion battery cathode materials.
[0005] Elemental doping is a common strategy for suppressing harmful phase transitions and improving cycle stability in P2-type layered oxides. By introducing electrochemically inert or active heteroions into the transition metal or sodium layer, the electronic structure and ion occupancy of the crystal structure can be modulated to some extent. However, the improvement effect of single-element doping is often limited to one aspect, making it difficult to achieve a comprehensive balance between the full voltage window, high energy density, long cycle life, and air stability. For example, Mg ions are electrochemically inert and can act as lattice pillars to alleviate lattice distortion, but they cannot effectively suppress harmful phase transitions at high voltages; Ca ions can enhance TM-O covalent bonds and strengthen the metal framework, but may hinder ion transport and exacerbate lattice oxidation at high voltages. While dual-element synergistic doping can suppress Na vacancy ordering and smooth the charge-discharge plateau to some extent, it often comes at the cost of reduced structural reversibility. Although co-doping with one or two elements can produce some synergistic gains, it is still difficult to fundamentally and fully suppress transition metal migration, vacancy ordering, and multiphase transitions.
[0006] High-entropy materials typically refer to single-phase solid solutions formed by five or more main elements occupying the same crystallographic lattice sites. According to thermodynamic principles, higher configurational entropy can reduce the Gibbs free energy of the system, suppress phase separation and short-range order, and is beneficial for maintaining a stable single-phase structure with long-range disorder. Previous studies have attempted to introduce the high-entropy design concept into layered cathode materials for sodium-ion batteries, aiming to broaden the solid solution reaction range, suppress harmful phase transitions, and improve overall electrochemical performance through the synergistic effect of multiple components. However, for P2-type layered oxides, the ionic radii and valence states of different dopants vary significantly. When synthesized using traditional solid-state methods or conventional co-precipitation methods, elemental segregation, phase separation, and impurity phase formation are easily observed, making it difficult to obtain a uniformly composed and thermodynamically stable high-entropy single-phase solid solution. Therefore, how to achieve uniform solid solution of multiple inactive elements in the P2-type layered oxide lattice while balancing high-entropy structural stability and electrochemical performance remains a technical problem to be solved in this field.
[0007] In summary, current technologies have not yet fully overcome the comprehensive performance limitations of P2-type sodium-ion battery cathode materials in terms of phase transition reversibility, voltage stability, air storage stability, and high-voltage cycle life. Therefore, developing a P2-type layered cathode material with high phase transition reversibility, good air stability, and excellent long-cycle performance is a practical necessity for promoting the practical application of sodium-ion batteries. Summary of the Invention
[0008] The purpose of this invention is to overcome the shortcomings of the prior art and provide a high-entropy P2-type sodium-ion battery cathode material doped with inactive elements and its preparation method. The high-entropy cathode material prepared by this method enables sodium-ion batteries to exhibit high energy density, high power density, and long cycle life.
[0009] To achieve the above objectives, the present invention adopts the following technical solution:
[0010] This solution provides a method for preparing a non-active element-doped high-entropy P2 type sodium-ion battery cathode material and its preparation method, and its application in sodium-ion batteries. The general chemical formula is Na. 0.7 Mn 0.6 Ni 0.35-x A x O2, where 0 < x ≤ 0.3, and A is composed of three or more elements such as Li, Mg, Zn, Al, and Ca. The specific steps are as follows:
[0011] (1) Weigh the required stoichiometric ratio of metal salts and dissolve them in a solvent to form a mixed solution of metal salts;
[0012] (2) Add an appropriate amount of complexing agent to the solution obtained in step (1) to form a transparent gel through the chelation effect of the complexing agent with metal ions. Place the transparent gel in a water bath or oil bath and stir to evaporate. Place the wet gel obtained after evaporation in an oven to dry, and grind the dried gel to obtain precursor powder;
[0013] (3) The precursor powder obtained in step (2) is sintered at high temperature in air atmosphere to obtain P2 phase high entropy oxide.
[0014] In step (1), the metal salt is selected from one or more metal salts such as nitrates, sulfates, and chlorides.
[0015] In step (1), the solvent is selected from one or more mixed solvents such as water, alcohol solvents, ester solvents, and amine solvents.
[0016] In step (2), the complexing agent is selected from one or more of citric acid, acrylic acid, urea, glucose, etc.
[0017] The evaporation temperature in step (2) is 60-100℃ and the evaporation time is 4-8 h.
[0018] The oven drying temperature in step (2) is 100-200℃, and the drying time is 8-15 h.
[0019] In step (3), the heating rate is 3–6 °C / min. -1 The insulation temperature is 850-950℃, and the insulation time is 9-15 hours.
[0020] The present invention also discloses a high-entropy doped P2-type sodium-ion battery cathode material prepared by the above method.
[0021] This invention also discloses the application of the high-entropy doped P2 type sodium-ion battery cathode prepared by the above method in the preparation of sodium-ion batteries.
[0022] The beneficial effects of this invention are:
[0023] In traditional solid-state methods, the asynchrony between the reactivity and diffusion rate of metal oxides or carbonate precursors after simple mechanical mixing leads to local enrichment, causing severe phase separation and impurity phase formation, making it impossible to form a single-phase solid solution. To address this significant challenge, this invention employs a sol-gel synthesis route, fully utilizing the chelating effect between specific functional groups such as carboxyl and hydroxyl groups in the complexing agent molecule and metal ions. This allows for the simultaneous stabilization of multiple different metal ions in the same homogeneous precursor solution within a liquid environment. As a multidentate ligand, the complexing agent molecule can form stable soluble chelates with various metal ions, effectively suppressing segregation and independent nucleation of metal ions at the microscale due to hydrolysis or concentration changes, ensuring uniform dispersion of each element in the gel or precipitate precursor. This highly mixed state at the molecular level significantly shortens the solid-phase diffusion distance during subsequent high-temperature calcination, reducing the temperature and time required for phase formation. This allows dopant ions to smoothly and orderly enter the target lattice sites in the transition metal layer under the synergistic effect of thermodynamics and configurational entropy, forming a high-entropy single-phase solid solution occupied by long-range disorder. The entire synthesis process has clear operation steps, excellent repeatability, low cost and wide availability of raw materials, mild and controllable reaction conditions, and does not rely on any precise or expensive special equipment. It is conducive to the direct scale-up from laboratory scale to industrial production, and provides a practical and cost-effective technical path for the large-scale preparation of high-entropy layered oxide cathode materials.
[0024] The high-entropy P2 oxide material of this invention exhibits advantages that are difficult for traditional P2-type materials to match. The long-range disordered occupation of various metal ions at the transition metal sites generates high configurational entropy. This significant increase in configurational entropy effectively reduces the Gibbs free energy of the system at high temperatures, thereby fundamentally suppressing the transition metal layer slip that is prone to occur when charging to high voltages and the resulting harmful P2→O2 or P2→OP4 phase transitions. Throughout the entire process of deep sodium insertion / extraction within a wide voltage window, the lattice volume change of the material is minimal. After hundreds of deep charge-discharge cycles, the layered structure remains intact, and no microcracks are observed inside or on the surface of the particles. The material enters an extremely stable capacity plateau after several dozen activation cycles, and its capacity retention rate during hundreds or even thousands of deep cycles is significantly better than that of traditional P2-type materials and various known doped and modified materials. In terms of charge / discharge behavior and energy efficiency, the introduction of multiple ions effectively disrupts the original charge order and Na⁺ / vacancy order arrangement within the transition metal layer, transforming the multi-step voltage ladder plateau caused by sodium ion insertion / extraction in traditional P2-type materials into a smooth charge / discharge curve. This transformation not only significantly improves energy efficiency during charge / discharge and reduces energy loss caused by voltage steps, but also ensures highly stable battery output voltage, greatly facilitating battery management system monitoring, balancing, and state-of-charge estimation, laying the foundation for reliable integration of battery packs in practical energy storage systems. The incorporation of multiple ions expands the interlayer spacing of sodium layers, providing a more spacious prismatic diffusion channel for the rapid migration of Na⁺ between layers. Simultaneously, the inherent lattice distortion effect and multi-component coupling environment of the high-entropy structure effectively reduce the activation energy barrier for ion transitions. The material maintains high usable capacity and excellent cycle reversibility even under extremely high-rate conditions, meeting the stringent requirements of power storage devices for rapid charge / discharge capabilities. Regarding air stability, the high-entropy configuration effectively reduces the surface free energy of the material, while the strong covalent bonding between inactive metal ions and lattice oxygen stabilizes the electronic state of surface oxygen at the electronic structure level. This dual mechanism synergistically suppresses side reactions between the material surface and moisture and carbon dioxide in the air, resulting in a reduction of surface residual alkali formation by several orders of magnitude compared to traditional materials. After prolonged exposure to humid air, the material's structural integrity and electrochemical activity degradation are reduced, fundamentally solving the long-standing practical bottlenecks of P2-type layered oxides, such as storage and transportation difficulties and the hygroscopic gelation of electrode pastes, greatly expanding its commercial application scenarios. Furthermore, the material system of this invention reduces dependence on expensive and high-supply-risk strategic metals such as cobalt and nickel. The constituent elements are inexpensive and environmentally friendly, demonstrating outstanding cost-effectiveness and sustainable development potential in the field of large-scale energy storage, which is subject to requirements for cycle cost and environmental impact. This is expected to accelerate the process of sodium-ion batteries moving from laboratory research to large-scale commercial applications. Attached Figure Description
[0025] Figure 1 This is the XRD pattern of a high-entropy doped inactive element P2-type sodium-ion battery cathode material prepared in Example 1 of this invention;
[0026] Figure 2 This is a Raman diagram of a high-entropy doped inactive element P2-type sodium-ion battery cathode material prepared in Example 1 of this invention;
[0027] Figure 3 This is a scanning electron microscope image of a high-entropy doped inactive element P2-type sodium-ion battery cathode material prepared in Example 1 of the present invention;
[0028] Figure 4 These are transmission electron microscope (TEM) images and elemental distribution diagrams of a high-entropy doped inactive element P2 type sodium-ion battery cathode material prepared in Example 1 of this invention, wherein (a) is a TEM image, (b) is the elemental distribution diagram of Na, (c) is the elemental distribution diagram of Ni, (d) is the elemental distribution diagram of Mn, (e) is the elemental distribution diagram of Mg, (f) is the elemental distribution diagram of Zn, (g) is the elemental distribution diagram of Ca, (h) is the elemental distribution diagram of Al, and (i) is the elemental distribution diagram of O.
[0029] Figure 5 This invention relates to a high-entropy doped inactive element P2-type sodium-ion battery cathode material prepared in Example 1 of the present invention, in (a) 0.5 A g -1 and (b) 1 A g -1 The charge / discharge cycle diagram. Detailed Implementation
[0030] The present invention will be further described below with reference to the accompanying drawings and embodiments.
[0031] Example 1:
[0032] Weigh 0.7 mol sodium citrate, 0.6 mol manganese acetate tetrahydrate, 0.35 mol nickel acetate, 0.01 mol calcium acetate monohydrate, 0.01 mol aluminum nitrate nonahydrate, 0.01 mol zinc nitrate hexahydrate, 0.01 mol magnesium acetate tetrahydrate, 0.01 mol lithium acetate dihydrate, and 1 mol citric acid into a beaker containing a certain amount of deionized water. Stir for one hour to ensure complete dissolution. Transfer the beaker containing the clear solution to an oil bath and set the temperature to 80℃ for stirring and evaporation for 4 hours until a gel is formed. Place the gel in a 200℃ oven to dry for 12 hours. Grind the dried gel in a mortar to form a fine, uniform powder. Then, place the powder into a crucible. Place the crucible in a muffle furnace and set the heating rate to 5℃ / min. -1The temperature was raised from room temperature to 900℃ and held at 900℃ for 12 hours. After the process ended and the furnace temperature cooled to room temperature, the product was collected to obtain Na. 0.7 Mn 0.6 Ni 0.35 Ca 0.01 Al 0.01 Zn 0.01 Mg 0.01 Li 0.01 O2.
[0033] like Figure 1 The X-ray diffraction (XRD) pattern shown indicates that all characteristic diffraction peaks of the sample are consistent with the standard P2, and no significant impurity peaks were detected, indicating high product purity. The observation that the (002) main diffraction peak shifted slightly to a lower angle confirms successful atomic incorporation into the crystal structure, expanding the interlayer spacing. Figure 2 Raman spectroscopy results showed obvious characteristic signals of the P2 phase cathode material. Figure 3 Scanning electron microscopy (SEM) images show that the synthesized material exhibits a uniformly sized, sheet-like morphology. Combined with... Figure 4 Transmission electron microscopy (TEM) and elemental mapping further confirmed the formation of the sheet-like structure, and that Li, Mg, Zn, Ca, and Al were successfully doped and uniformly distributed. The combined effect of these characterization methods fully demonstrates that this embodiment successfully prepared the target product, a high-entropy doped P2-type sodium-ion battery cathode material.
[0034] Coin cells were assembled and their charge-discharge specific capacity and cycle stability were tested at room temperature to verify the electrochemical performance of the obtained high-entropy doped P2-type sodium-ion battery cathode material. Active material, conductive carbon black, and polyvinylidene fluoride (PVDF) were weighed at a mass ratio of 8:1:1 and placed in a mortar, and ground for 10 min. Then, an appropriate amount of N-methylpyrrolidone (NMP) solvent was added to prepare a uniform slurry, and grinding was continued for another 10 min. The slurry was then uniformly coated onto the surface of a clean copper foil current collector. The coated electrode was dried in a 60℃ vacuum oven for 12 hours, and after roll forming, it was punched into circular electrode sheets with a diameter of 12 mm for later use. In a glove box filled with high-purity argon, CR2032 type coin cells were assembled using a sodium metal sheet as the counter electrode, glass fiber as the separator, and 1 M NaClO4 / EC:DMC and 5% FEC as the electrolyte. The specific capacity and cycle stability were tested using conventional methods at 0.5 A g... -1 and 1 A g -1 Constant current charge-discharge performance was tested using a battery testing system at current density.
[0035] Test results: such as Figure 5 As shown, the high-entropy doped P2 type sodium-ion battery cathode material at 0.5 A g -1At the given current density, the first discharge specific capacity reached 101.2 mAh g. -1 At 0.5 Ag -1 After 500 cycles at the current density, its specific capacity remained stable at 78.8 mAh g⁻¹. -1 This demonstrates that the material possesses excellent structural integrity. Furthermore, at 1 Ag... -1 Under a current density of 1000 cycles, its initial discharge capacity was 82 mAh g⁻¹. -1 .
[0036] Example 2:
[0037] Weigh 0.7 mol sodium citrate, 0.6 mol manganese acetate tetrahydrate, 0.325 mol nickel acetate, 0.015 mol calcium acetate monohydrate, 0.015 mol aluminum nitrate nonahydrate, 0.015 mol zinc nitrate hexahydrate, 0.015 mol magnesium acetate tetrahydrate, 0.015 mol lithium acetate dihydrate, and 1.2 mol citric acid into a beaker containing a certain amount of deionized water. Stir for one hour to ensure complete dissolution. Transfer the beaker containing the clear solution to an oil bath and set the temperature to 60℃ for stirring and evaporation for 8 hours until a gel is formed. Place the gel in a 100℃ oven to dry for 15 hours. Grind the dried gel in a mortar to form a fine, uniform powder. Then, place the powder into a crucible. Place the crucible in a muffle furnace and set the heating rate to 4℃ / min. -1 The temperature was raised from room temperature to 920℃ and held at 920℃ for 11 hours. After the process ended and the furnace temperature cooled to room temperature, the product was collected to obtain Na. 0.7 Mn 0.6 Ni 0.325 Ca 0.015 Al 0.015 Zn 0.015 Mg 0.015 Li 0.015 O2.
[0038] Coin cells were assembled and their charge-discharge specific capacity and cycle stability were tested at room temperature to verify the electrochemical performance of the obtained high-entropy doped P2-type sodium-ion battery cathode material. Active material, conductive carbon black, and polyvinylidene fluoride (PVDF) were weighed at a mass ratio of 8:1:1 and placed in a mortar, and ground for 10 min. Then, an appropriate amount of N-methylpyrrolidone (NMP) solvent was added to prepare a uniform slurry, and grinding was continued for another 10 min. The slurry was then uniformly coated onto the surface of a clean copper foil current collector. The coated electrode was dried in a 60℃ vacuum oven for 12 hours, and after roll forming, it was punched into circular electrode sheets with a diameter of 12 mm for later use. In a glove box filled with high-purity argon, CR2032 type coin cells were assembled using a sodium metal sheet as the counter electrode, glass fiber as the separator, and 1 M NaClO4 / EC:DMC and 5% FEC as the electrolyte. The specific capacity and cycle stability were tested using conventional methods at 0.5 A g... -1 and 1 A g -1 Constant current charge-discharge performance was tested using a battery testing system at current density.
[0039] At 0.5 A g -1 The first-cycle discharge specific capacity at the specified current density was 98.3 mAh g. -1 At 0.5 Ag -1 After 500 cycles at the current density, the specific capacity remained stable at 75.3 mAh g⁻¹. -1 This demonstrates that the material possesses excellent structural integrity. Furthermore, at 1 Ag... -1 Under a current density of 1000 cycles, its initial discharge capacity was 80 mAhg. -1 .
[0040] Example 3:
[0041] Weigh 0.7 mol sodium citrate, 0.6 mol manganese acetate tetrahydrate, 0.3 mol nickel acetate, 0.02 mol calcium acetate monohydrate, 0.02 mol aluminum nitrate nonahydrate, 0.02 mol zinc nitrate hexahydrate, 0.02 mol magnesium acetate tetrahydrate, 0.02 mol lithium acetate dihydrate, and 1.4 mol citric acid into a beaker containing a certain amount of deionized water. Stir for one hour to ensure complete dissolution. Transfer the beaker containing the clear solution to an oil bath and set the temperature to 80℃ for stirring and evaporation for 4 hours until a gel is formed. Place the gel in a 150℃ oven and dry for 14 hours. Grind the dried gel in a mortar to form a fine, uniform powder. Then, place the powder into a crucible. Place the crucible in a muffle furnace and set the heating rate to 6℃ / min. -1The temperature was raised from room temperature to 930℃ and held at 930℃ for 9 hours. After the process ended and the furnace temperature cooled to room temperature, the product was collected to obtain Na. 0.7 Mn 0.6 Ni 0.3 Ca 0.02 Al 0.02 Zn 0.02 Mg 0.02 Li 0.02 O2.
[0042] Coin cells were assembled and their charge-discharge specific capacity and cycle stability were tested at room temperature to verify the electrochemical performance of the obtained high-entropy doped P2-type sodium-ion battery cathode material. Active material, conductive carbon black, and polyvinylidene fluoride (PVDF) were weighed at a mass ratio of 8:1:1 and placed in a mortar, and ground for 10 min. Then, an appropriate amount of N-methylpyrrolidone (NMP) solvent was added to prepare a uniform slurry, and grinding was continued for another 10 min. The slurry was then uniformly coated onto the surface of a clean copper foil current collector. The coated electrode was dried in a 60℃ vacuum oven for 12 hours, and after roll forming, it was punched into circular electrode sheets with a diameter of 12 mm for later use. In a glove box filled with high-purity argon, CR2032 type coin cells were assembled using a sodium metal sheet as the counter electrode, glass fiber as the separator, and 1 M NaClO4 / EC:DMC and 5% FEC as the electrolyte. The specific capacity and cycle stability were tested using conventional methods at 0.5 A g... -1 and 1 A g -1 Constant current charge-discharge performance was tested using a battery testing system at current density.
[0043] At 0.5 A g -1 The first-cycle discharge specific capacity at the specified current density is 99.5 mAh g. -1 At 0.5 Ag -1 After 500 cycles at the current density, the specific capacity remained stable at 76.2 mAh g⁻¹. -1 In 1 A g -1 Under a current density of 1000 cycles, its initial discharge capacity was 81.4 mAh g⁻¹. -1 .
[0044] Example 4:
[0045] Weigh 0.7 mol sodium citrate, 0.6 mol manganese acetate tetrahydrate, 0.275 mol nickel acetate, 0.025 mol calcium acetate monohydrate, 0.025 mol aluminum nitrate nonahydrate, 0.025 mol zinc nitrate hexahydrate, 0.025 mol magnesium acetate tetrahydrate, 0.025 mol lithium acetate dihydrate, and 1.8 mol citric acid into a beaker containing a certain amount of deionized water. Stir for one hour to ensure complete dissolution. Transfer the beaker containing the clear solution to an oil bath and set the temperature to 70℃ for stirring and evaporation for 6 hours until a gel is formed. Place the gel in a 190℃ oven and dry for 8 hours. Grind the dried gel in a mortar to form a fine, uniform powder. Then, place the powder into a crucible. Place the crucible in a muffle furnace and set the heating rate to 4℃ / min. -1 The temperature was raised from room temperature to 850℃ and held at 850℃ for 15 hours. After the process ended and the furnace temperature cooled to room temperature, the product was collected to obtain Na. 0.7 Mn 0.6 Ni 0.275 Ca 0.025 Al 0.02 5Zn 0.025 Mg 0.025 Li 0.025 O2.
[0046] Coin cells were assembled and their charge-discharge specific capacity and cycle stability were tested at room temperature to verify the electrochemical performance of the obtained high-entropy doped P2-type sodium-ion battery cathode material. Active material, conductive carbon black, and polyvinylidene fluoride (PVDF) were weighed at a mass ratio of 8:1:1 and placed in a mortar, and ground for 10 min. Then, an appropriate amount of N-methylpyrrolidone (NMP) solvent was added to prepare a uniform slurry, and grinding was continued for another 10 min. The slurry was then uniformly coated onto the surface of a clean copper foil current collector. The coated electrode was dried in a 60℃ vacuum oven for 12 hours, and after roll forming, it was punched into circular electrode sheets with a diameter of 12 mm for later use. In a glove box filled with high-purity argon, CR2032 type coin cells were assembled using a sodium metal sheet as the counter electrode, glass fiber as the separator, and 1 M NaClO4 / EC:DMC and 5% FEC as the electrolyte. The specific capacity and cycle stability were tested using conventional methods at 0.5 A g... -1 and 1 A g -1 Constant current charge-discharge performance was tested using a battery testing system at current density.
[0047] At 0.5 A g -1 The first-cycle discharge specific capacity at the specified current density was 97.6 mAh g. -1 At 0.5 Ag -1After 500 cycles at the current density, the specific capacity remained stable at 75.7 mAh g⁻¹. -1 In 1 A g -1 Under a current density of 1000 cycles, its initial discharge capacity was 81.4 mAh g⁻¹. -1 .
[0048] Example 5:
[0049] Weigh 0.7 mol sodium citrate, 0.6 mol manganese acetate tetrahydrate, 0.25 mol nickel acetate, 0.03 mol calcium acetate monohydrate, 0.03 mol aluminum nitrate nonahydrate, 0.03 mol zinc nitrate hexahydrate, 0.03 mol magnesium acetate tetrahydrate, 0.03 mol lithium acetate dihydrate, and 2 mol citric acid into a beaker containing a certain amount of deionized water. Stir for one hour to ensure complete dissolution. Transfer the beaker containing the clear solution to an oil bath and set the temperature to 100℃ for stirring and evaporation for 5 hours until a gel is formed. Dry the gel in a 120℃ oven for 13 hours. Grind the dried gel in a mortar to form a fine, uniform powder. Place the powder into a crucible and place the crucible in a muffle furnace, setting the heating rate to 5℃ / min. -1 The temperature was raised from room temperature to 950℃ and held at 950℃ for 12 hours. After the program ended and the furnace temperature cooled to room temperature, the product was collected to obtain Na. 0.7 Mn 0.6 Ni 0.25 Ca 0.03 Al 0.03 Zn 0.03 Mg 0.03 Li 0.03 O2.
[0050] Coin cells were assembled and their charge-discharge specific capacity and cycle stability were tested at room temperature to verify the electrochemical performance of the obtained high-entropy doped P2-type sodium-ion battery cathode material. Active material, conductive carbon black, and polyvinylidene fluoride (PVDF) were weighed at a mass ratio of 8:1:1 and placed in a mortar, and ground for 10 min. Then, an appropriate amount of N-methylpyrrolidone (NMP) solvent was added to prepare a uniform slurry, and grinding was continued for another 10 min. The slurry was then uniformly coated onto the surface of a clean copper foil current collector. The coated electrode was dried in a 60℃ vacuum oven for 12 hours, and after roll forming, it was punched into circular electrode sheets with a diameter of 12 mm for later use. In a glove box filled with high-purity argon, CR2032 type coin cells were assembled using a sodium metal sheet as the counter electrode, glass fiber as the separator, and 1 M NaClO4 / EC:DMC and 5% FEC as the electrolyte. The specific capacity and cycle stability were tested using conventional methods at 0.5 A g... -1and 1 A g -1 Constant current charge-discharge performance was tested using a battery testing system at current density.
[0051] At 0.5 A g -1 The first-cycle discharge specific capacity at the specified current density is 99.7 mAh g. -1 At 0.5 Ag -1 After 500 cycles at the current density, the specific capacity remained stable at 74.8 mAh g⁻¹. -1 In 1 A g -1 Under a current density of 1000 cycles, its initial discharge capacity was 81.8 mAh g⁻¹. -1 .
[0052] This invention provides a method for preparing a high-entropy doped P2-type sodium-ion battery cathode material. The synthesis process is simple and low-cost, making it suitable for large-scale industrial production. Compared with traditional sodium-ion batteries, the high-entropy doped P2-type sodium-ion battery cathode material suppresses harmful phase transitions, broadens sodium-ion transport channels, and disrupts sodium layer vacancies, resulting in higher specific capacity and capacity retention.
[0053] The above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit it. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A non-active element doped high-entropy P2-type sodium-ion battery cathode material and a preparation method thereof, characterized in that A P2-type sodium-ion battery cathode material is prepared by doping a plurality of non-active elements to form a high-entropy structure. The chemical general formula is Na 0.7 Mn 0.6 Ni 0.35-x A x O2, wherein 0 < x ≤ 0.3, A is composed of three or more elements of Li, Mg, Zn, Al, Ca, etc.
2. The method for preparing the high-entropy P2 type sodium-ion battery cathode material doped with inactive elements as described in claim 1, characterized in that, The resulting crystal structure is a single-phase solid solution of pure P2 phase.
3. The method for preparing a high-entropy P2 type sodium-ion battery cathode material doped with an inactive element as described in claim 1, characterized in that, The cathode material has a P2 phase sheet-like morphology.
4. The method for preparing a high-entropy P2 type sodium-ion battery cathode material doped with inactive elements as described in claims 1 to 3 is characterized in that... Includes the following steps: 1) Dissolve various metal salts in a solvent and stir to obtain a mixed solution of metal salts. 2) Add a complexing agent to the solution obtained in step 1. A transparent gel is formed through the chelation effect of the complexing agent and the metal ions. The gel is stirred and evaporated to obtain a wet gel. The wet gel is then dried and ground to obtain the precursor powder. 3) The precursor powder obtained in step 2 is sintered at high temperature in air atmosphere, and after cooling, P2 type high entropy oxide is obtained.
5. The method for preparing a high-entropy doped inactive element P2-type sodium-ion battery cathode material as described in claim 4, characterized in that, The sodium source, manganese source, nickel source, and the metal salts corresponding to each element in A mentioned in step 1 are selected from one or more metal salts such as nitrates, sulfates, and chlorides. The solvent mentioned in step 1 is selected from one or more mixed solvents such as water, alcohol solvents, ester solvents, and amine solvents.
6. The method for preparing a high-entropy P2 type sodium-ion battery cathode material doped with an inactive element as described in claim 4, characterized in that, The complexing agent mentioned in step 2 is selected from one or more of citric acid, acrylic acid, urea, and glucose, and the molar ratio of the complexing agent to the transition layer precursor is (1-2):
1.
7. The method for preparing a high-entropy P2 type sodium-ion battery cathode material doped with an inactive element as described in claim 4, characterized in that, The evaporation temperature in step 2 is 60–100°C, and the evaporation time is 4–8 h; the drying temperature of the wet gel is 100–200°C, and the drying time of the wet gel is 8–15 h.
8. The method for preparing a high-entropy doped inactive element P2-type sodium-ion battery cathode material as described in claim 4, characterized in that, The sintering stage described in step 3 has a temperature increase rate of 3-6 ℃ min -1 , a holding temperature of 850-950 ℃, and a holding time of 9-15 h.
9. The application of the preparation method of the high-entropy P2 type sodium-ion battery cathode material doped with inactive elements as described in claims 1 to 4 in sodium-ion battery electrode materials.