A lithium-rich manganese oxide positive electrode material with high magnification long cycle stability, a preparation method and application
By controlling the lithium content and heat treatment conditions, lithium-rich manganese oxide cathode materials were prepared, solving the problems of lithium-ion kinetics and structural stability, achieving high-rate long-cycle stability and cost reduction, and making them suitable for ultra-fast charging lithium-ion batteries.
Patent Information
- Application Number
- CN202611385950.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-08
- Publication Date
- 2026-11-24
AI Technical Summary
Existing lithium-rich manganese oxide cathode materials suffer from problems such as limited lithium-ion kinetics, poor electronic conductivity, and structural instability at high rates, resulting in insufficient fast charging performance and cycle stability. Furthermore, the high lithium content leads to higher costs.
By controlling the lithium content and heat treatment conditions, Li1.26(1-x)Ni0.119Co0.119Mn0.503O2 material was prepared by spray drying combined with air atmosphere heat treatment. The lithium content was reduced by 10-20 at%, and the material was kept at 750-1000℃ for a long time to form a high-density stacked fault structure, thereby improving the structural flexibility and lithium ion diffusion capacity of the material.
It significantly improves the rate performance and long-cycle stability of the material, reduces costs, and simplifies the preparation process, thus facilitating large-scale industrial production.
Smart Images

Figure CN123162173A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of battery technology, specifically to a lithium-rich manganese oxide cathode material with high rate and long cycle stability, its preparation method, and its application. Background Technology
[0002] Governments worldwide have implemented regulations and incentive policies to reduce carbon emissions and promote battery electric vehicles. Significant improvements in lithium-ion battery performance and cost reductions have driven this trend. However, the charging experience remains a key factor influencing consumer acceptance. Improving the charging process to approach the convenience of traditional refueling is crucial. Developing ultra-fast charging (XFC) technology that can complete a charge in 5 to 15 minutes (charging rate exceeding 4C) is significant in alleviating these concerns. Furthermore, the rapid development of the low-altitude economy—especially driven by electric vertical takeoff and landing (eVTOL) aircraft—demands battery solutions with both high energy density and superior power output capabilities.
[0003] With the development of power batteries towards XFC and high energy density, the development of high-capacity positive and negative electrode materials has become an indispensable requirement. Lithium-rich oxides are advantageous due to their low cost, abundant resources, and high specific capacity (>250 mAh g⁻¹). -1 ) and high voltage (~3.60V vs. Li + Silicon-carbon (Si / C) composites have become highly promising cathode material candidates. In contrast, silicon-carbon (Si / C) composite anodes are nearing their performance limits, offering over 1500 mAh / g. - ¹ It possesses high specific capacity and lithium-ion diffusion kinetics necessary for fast charging. Therefore, it is urgent to solve the kinetic bottlenecks and structural stability problems of lithium-rich oxide cathode materials, as these issues limit their ultra-fast charging performance and restrict their application in high-energy-density battery systems.
[0004] The fast charge / discharge performance of lithium-ion battery lithium-rich oxide cathode materials is affected by several key factors, involving kinetic and dynamic effects. (i) Ion transport bottleneck. The lithium-ion diffusion coefficient in LRO particles is extremely low, approximately 10. -18 ~10 - 15 cm 2 / s, limiting lithium-ion diffusion within the material at high charging rates. (ii) Poor electronic conductivity. Due to the large band gap (approximately 0.50 eV), lithium-rich oxide cathode materials exhibit low electronic conductivity, only 10. -9 ~10 -7 S·cm -1Therefore, the kinetics of lithium-rich oxide cathode materials are relatively slow. At high current densities, significant polarization enhancement and a decrease in discharge capacity occur. (iii) Electrochemical-mechanical degradation. During rapid delithiation, greater stress leads to lattice displacement and strain accumulation, resulting in a significant capacity decrease. Ultimately, high-rate cycling stability decreases significantly. In-depth research on lithium-rich oxide cathode materials with high rate and long-cycle stability is urgently needed. Related research mainly focuses on surface engineering, elemental doping, and composite material preparation. Elemental doping achieves better improvement through substitution, but due to lattice mismatch, the compatibility between heteroatoms and the crystal structure is weak. Similarly, surface engineering may enhance structural integrity and prevent O2 escape, but its impact on the overall electronic and crystal structure is negligible. Furthermore, most methods involve cumbersome synthesis processes and easily introduce impurity phases during modification, resulting in less than ideal improvements in high-rate, long-cycle performance.
[0005] Existing lithium-rich manganese oxide cathode materials include lithium, nickel, cobalt, and manganese elements, with a basic ratio typically of Li... 1.2 Mn 0.54 Ni 0.13 Co 0.13 The O2 solution contains 1.2 mol of lithium per structural unit. The existing solution has the following problems: 1. The stoichiometric lithium source easily leaves residues on the particle surface, forming LiOH and Li2CO3; after water absorption, the slurry viscosity becomes uncontrollable, making electrode coating difficult; residual lithium also exacerbates cell gas expansion and self-discharge. 2. High lithium content leads to higher costs. 3. During the first charge >4.5V, when activating the Li2MnO3 phase, lattice oxygen irreversibly escapes, generating irreversible Li2O, reducing the effective lithium source and capacity. 4. The addition of large amounts of lithium restricts lithium-ion kinetics, resulting in insufficient rate performance and difficulty in fast charging adaptation; finally, poor cycle stability under high current, and the layered-to-spinel / rock salt phase transition during cycling leads to poor cycle performance.
[0006] Therefore, there is an urgent need to develop an effective strategy to synergistically regulate its bulk and surface structures in order to enhance interfacial stability, strengthen the stability of the bulk structure, and optimize the electron and ion transport involved in the electrochemical reaction kinetics, thereby improving the overall performance. Summary of the Invention
[0007] The present invention provides a lithium-rich manganese oxide cathode material with high rate and long cycle stability, a preparation method and application, to solve the problems of existing technologies, such as easy lithium source residue, high cost, reduced capacity, poor rate performance and poor stability, due to high lithium content.
[0008] To achieve the above objectives, the present invention provides the following technical solution: a lithium-rich manganese oxide cathode material with high rate-capacity and long-cycle stability, the chemical formula of which is Li.1.26(1-x) Ni 0.119 Co 0.119 Mn 0.503 O2, where x = 0.10-0.20.
[0009] Furthermore, x = 0.15 above.
[0010] Furthermore, the preparation method of the above-mentioned lithium-rich manganese oxide cathode material with high rate and long cycle stability includes the following steps: first, preparing a precursor solution, then using a spray drying method, and finally performing heat treatment to prepare Li. 1.26(1-x) Ni 0.119 Co 0.119 Mn 0.503 In the O2 precursor solution, the total concentration of acetate is 0.1-0.2 mol / L, the concentration of citric acid monohydrate is 0.2-0.5 mol / L, and lithium with a total mass of 3.0% is added.
[0011] Furthermore, the above heat treatment conditions are: 750-1000℃, holding for 20-300 minutes.
[0012] Furthermore, the preferred heat treatment conditions are 850℃ for 300 minutes.
[0013] Furthermore, the above-mentioned lithium-rich manganese oxide cathode material with high rate and long cycle stability is applied in the preparation of lithium-ion batteries.
[0014] Compared with the prior art, the beneficial effects of the present invention are as follows: (1) This invention achieves material modification through component control, which only involves adjusting the basic ratio and sintering process, making it simple and easy to implement. Specifically, the lithium element adopts a non-stoichiometric lithium-deficient design, reducing the lithium content by 10~20 at% (x=0.10-0.20), which not only reduces residual lithium (LiOH, Li2CO3) on the particle surface and alleviates slurry processing problems, but also reduces the lithium content to approximately 1.134-1.008 mol per structural unit, which is significantly lower than the Li content of traditional lithium-rich manganese materials (1.2 mol per structural unit) by 5.5-16%, resulting in a significant reduction in cost.
[0015] Simultaneously, specific heat treatment temperatures and holding times are matched: compared to conventional lithium-rich manganese sintering, a process condition of moderately reduced sintering temperature and long holding time (850℃, 300min) is adopted to induce the formation of high-density stacking fault defects inside the crystal. Stacking faults endow the crystal with higher structural flexibility, which can not only promote the transport and diffusion of lithium ions, but also adapt to the lattice strain during the high-rate lithium ion insertion / extraction process, dissipate the internal stress generated by charging and discharging, and significantly improve the crystal structure stability during cycling.
[0016] (2) The preparation process of this invention only uses spray drying combined with air atmosphere heat treatment, without the need for additional coating, doping and post-treatment steps. The process is simple and controllable, providing convenient conditions for large-scale industrial production and application.
[0017] (3) The optimal component sample Li obtained by the present invention 1.071 Ni 0.119 Co 0.119 Mn 0.503 O2-850 (x=0.15) exhibits an initial discharge specific capacity of up to 303 mAh / g at a current density of 20 mA / g; after 500 cycles at a current density of 1.0 A / g (5C), the capacity retention rate is 90.45%; and after 1000 cycles at a current density of 4.0 A / g (20C), the capacity retention rate is as high as 90.22%.
[0018] (4) This invention obtains a lithium-rich manganese oxide cathode rich in stacking faults through synergistic regulation of components and heat treatment, which has high specific capacity, excellent rate capability and ultra-long cycle stability, and greatly improves the overall performance of lithium-ion batteries. It can be widely used in ultra-fast charging batteries and eVTOL low-altitude aircraft batteries. Attached Figure Description
[0019] Figure 1 The images show the XRD patterns of the lithium-rich manganese oxide cathode materials prepared in Example 7 and Comparative Example 3 of Experimental Example 1. in, Figure 1 (a) XRD patterns of Comparative Example 7 and Example 3; Figure 1 (b) is a comparison diagram of the (003) diffraction peaks; Figure 1 (c) is a comparison diagram of superstructure diffraction peaks; Figure 2 The XRD patterns of the lithium-rich manganese oxide cathode materials prepared in Examples 2, 5, 7 and 8 of Experimental Example 2 are shown; Figure 2 (a) XRD patterns of Examples 2, 5, 7, and 8; Figure 2 (b) is a comparison diagram of the (003) diffraction peaks; Figure 2 (c) is a comparison diagram of superstructure diffraction peaks; Figure 3 This is a TEM image of the lithium-rich manganese oxide cathode material prepared in Comparative Example 3 in Experimental Example 3; Figure 4 This is a TEM image of the lithium-rich manganese oxide cathode material prepared in Example 7 of Experimental Example 3; Figure 5 The figures show the initial charge-discharge curves at 0.1C for the lithium-rich manganese oxide cathode materials prepared in Examples 1-7 and Comparative Examples 1-3 of Experimental Example 4; among them, Figure 5 (a) is a graph showing the first charge-discharge curves of Comparative Example 1 and Examples 1-3. Figure 5 (b) is a graph showing the first charge-discharge curves for Comparative Example 2 and Examples 4-6. Figure 5 (c) is the first charge-discharge curve of Comparative Example 3 and Example 7; Figure 6 The graphs show the specific capacity cycling stability of the lithium-rich manganese oxide cathode materials prepared in Examples 4-7 and Comparative Examples 2-3 at 1C and 5C current densities, as shown in Experimental Example 4. Figure 6 (a) is a graph showing the specific capacity cycling stability of Comparative Example 2 and Examples 4-6 at a current density of 1C. Figure 6 (b) is a graph showing the specific capacity cycling stability of Comparative Example 2 and Examples 4-6 at a current density of 5C. Figure 6 (c) is a graph showing the specific capacity cycling stability of Comparative Example 3 and Example 7 at a current density of 1C. Figure 6 (d) is a graph showing the specific capacity cycling stability of Comparative Example 3 and Example 7 at a current density of 5C; Figure 7 The graphs show the specific capacity cycling stability of the lithium-rich manganese oxide cathode materials prepared in Examples 2, 5, 7, and 8 of Experiment 4 at current densities of 1C and 5C; among them, Figure 7 (a) is a graph showing the specific capacity cycling stability of Examples 2 and 5-8 at a current density of 1C. Figure 7 (b) is a graph showing the specific capacity cycling stability of Examples 2 and 5-8 at a current density of 5C; Figure 8 The figures show the lithium-ion diffusion coefficient test and rate performance of the lithium-rich manganese oxide cathode materials prepared in Example 7 and Comparative Example 3 of Experimental Example 4; among them, Figure 8 (a) is a graph showing the lithium-ion diffusion coefficient measured by GITT during the charging and discharging process in Example 7. Figure 8 (b) is a rate performance diagram of Example 7; Figure 9 The graph shows the specific capacity cycling stability of the lithium-rich manganese oxide cathode materials prepared in Example 7 and Comparative Example 3 of Experimental Example 4 at a current density of 20C; where, Figure 9 (a) is the specific capacity cycling stability diagram of Comparative Example 3 at a current density of 20C. Figure 9 (b) is a graph showing the specific capacity cycling stability of Example 7 at a current density of 20C; Figure 10 The images show the Raman spectra of the lithium-rich manganese oxide cathode materials prepared in Example 7 and Comparative Example 3 under different charge-discharge voltages during the first charge-discharge cycle in Experimental Example 5; among them, Figure 10 (a) Raman spectra of the lithium-rich manganese oxide cathode material prepared in Comparative Example 3 under different charge-discharge voltages during the first charge-discharge cycle. Figure 10 (b) Raman spectra of the lithium-rich manganese oxide cathode material prepared in Example 7 under different charge-discharge voltages during the first charge-discharge cycle; Figure 11 This is a TEM image of the lithium-rich manganese oxide cathode material prepared in Example 7 of Experiment 6 after 1000 cycles at 20C; wherein, Figure 11 (a) is a TEM image of the lithium-rich manganese oxide cathode material prepared in Example 7 after 1000 cycles at 20C. Figure 11 (b) is Figure 11 (a) is a magnified view of a portion of the image. Figure 11 (c) is the FFT plot. Detailed Implementation
[0020] The principles and features of the present invention are described below with reference to the accompanying drawings. The examples given are for illustrative purposes only and are not intended to limit the scope of the invention. Unless otherwise specified in the examples, conventional conditions or conditions recommended by the manufacturer should be followed. Reagents or instruments whose manufacturers are not specified are all commercially available products.
[0021] Example 1: A method for preparing a lithium-rich manganese oxide cathode material with high rate and long cycle stability, comprising the following steps: Step 1: Prepare the precursor solution; Weigh out 17.874 g of lithium acetate dihydrate, 4.442 g of nickel acetate tetrahydrate, 4.446 g of cobalt acetate tetrahydrate and 18.492 g of manganese acetate tetrahydrate, dissolve them in 1 L of deionized water, add 63.042 g of citric acid monohydrate, and add an additional 3% by mass of lithium acetate dihydrate to compensate for lithium loss during heat treatment; mechanically stir at 500 rpm for 1 h at room temperature to obtain the precursor solution.
[0022] Step 2: Preparation of precursor materials The precursor solution obtained in step one is fed to a spray dryer using a peristaltic pump. The inlet temperature of the spray dryer is set to 230℃, the outlet temperature is set to 100℃, and the feed rate is set to 1L / h. The precursor material is obtained by spray drying under high temperature and high pressure.
[0023] Step 3: Preparation of cathode material The precursor material obtained in step two was placed in an alumina crucible, which was then placed in a box furnace. Under an air atmosphere, the temperature was increased at a rate of 3°C / min, and the material was heat-treated at 750°C for 300 min to obtain Li. 1.134 Ni 0.119 Co 0.119 Mn 0.503 O2-750 cathode material, where x=0.10.
[0024] Example 2: A method for preparing a lithium-rich manganese oxide cathode material with high rate and long cycle stability, comprising the following steps: The preparation method is the same as in Example 1, except that when preparing the precursor solution, 16.881 g of lithium acetate dihydrate, 4.442 g of nickel acetate tetrahydrate, 4.446 g of cobalt acetate tetrahydrate, and 18.492 g of manganese acetate tetrahydrate were weighed, dissolved in 1 L of deionized water, and 63.042 g of citric acid monohydrate was added. An additional 3% (w / w) of lithium acetate dihydrate was added to compensate for lithium loss during heat treatment. The solution was mechanically stirred at 500 rpm for 1 h at room temperature to obtain the precursor solution. The remaining steps were the same as in Example 1. The cathode material Li was thus prepared. 1.071 Ni 0.119 Co 0.119 Mn 0.503 O2-750, where x=0.15.
[0025] Example 3: A method for preparing a lithium-rich manganese oxide cathode material with high rate and long cycle stability, comprising the following steps: The preparation method is the same as in Example 1, except that when preparing the precursor solution, 15.888 g of lithium acetate dihydrate, 4.442 g of nickel acetate tetrahydrate, 4.446 g of cobalt acetate tetrahydrate, and 18.492 g of manganese acetate tetrahydrate were weighed, dissolved in 1 L of deionized water, and 63.042 g of citric acid monohydrate was added. An additional 3% (w / w) of lithium acetate dihydrate was added to compensate for lithium loss during heat treatment. The solution was mechanically stirred at 500 rpm for 1 h at room temperature to obtain the precursor solution. The remaining steps were the same as in Example 1. The cathode material Li was thus prepared. 1.071 Ni 0.119 Co 0.119 Mn 0.503 O2-750, where x=0.20.
[0026] Example 4: A method for preparing a lithium-rich manganese oxide cathode material with high rate and long cycle stability, comprising the following steps: The preparation method is the same as in Example 1, except that in the preparation of the cathode material, the precursor material obtained in step (2) is placed in an alumina crucible, the alumina crucible is placed in a box furnace, and the temperature is increased at a rate of 3℃ / min under air atmosphere, and heat-treated at 800℃ for 300min. The remaining steps are the same as in Example 1. The cathode material Li was thus obtained. 1.134 Ni 0.119 Co 0.119 Mn 0.503 O2-800 cathode material, where x=0.10.
[0027] Example 5: A method for preparing a lithium-rich manganese oxide cathode material with high rate and long cycle stability, comprising the following steps: The preparation method is the same as in Example 2, except that, in the preparation of the cathode material, the precursor material obtained in step (2) is placed in an alumina crucible, the alumina crucible is placed in a box furnace, and the temperature is increased at a rate of 3℃ / min under air atmosphere, and heat-treated at 800℃ for 300min. The remaining steps are the same as in Example 2. The cathode material Li was thus obtained. 1.071 Ni 0.119 Co 0.119 Mn 0.503 O2-800, where x=0.15.
[0028] Example 6: A method for preparing a lithium-rich manganese oxide cathode material with high rate and long cycle stability, comprising the following steps: The preparation method is the same as in Example 3, except that, in the preparation of the positive electrode material, the precursor material obtained in step (2) is placed in an alumina crucible, the alumina crucible is placed in a box furnace, and the temperature is increased at a rate of 3℃ / min under an air atmosphere, and heat-treated at 800℃ for 300min. The remaining steps are the same as in Example 3. The positive electrode material Li is obtained. 1.071 Ni 0.119 Co 0.119 Mn 0.503 O2-800, where x=0.20.
[0029] Example 7: A method for preparing a lithium-rich manganese oxide cathode material with high rate and long cycle stability, comprising the following steps: The preparation method is the same as in Example 2, except that, in the preparation of the cathode material, the precursor material obtained in step (2) is placed in an alumina crucible, the alumina crucible is placed in a box furnace, and the temperature is increased at a rate of 3℃ / min under an air atmosphere, and heat-treated at 850℃ for 300min. The remaining steps are the same as in Example 2. The cathode material Li is thus obtained. 1.071 Ni 0.119 Co 0.119 Mn 0.503 O2-850, where x=0.15.
[0030] Example 8: A method for preparing a lithium-rich manganese oxide cathode material with high rate and long cycle stability, comprising the following steps: The preparation method is the same as in Example 2, except that, in the preparation of the cathode material, the precursor material obtained in step (2) is placed in an alumina crucible, the alumina crucible is placed in a box furnace, and the temperature is increased at a rate of 3℃ / min under an air atmosphere, and heat-treated at 1000℃ for 20min. The remaining steps are the same as in Example 2. The cathode material Li is thus obtained. 1.071 Ni 0.119 Co 0.119 Mn0.503 O2-1000(x=0.15), where x=0.15.
[0031] Comparative Example 1: A method for preparing a lithium-rich manganese oxide cathode material with adjustable Li content and controlled heat treatment conditions includes the following steps: (1) Preparation of precursor solution Weigh 19.86 g of lithium acetate dihydrate, 4.442 g of nickel acetate tetrahydrate, 4.446 g of cobalt acetate tetrahydrate and 18.492 g of manganese acetate tetrahydrate, dissolve them in 1 L of deionized water, add 63.042 g of citric acid monohydrate, and add an additional 3% by mass of lithium acetate dihydrate to compensate for lithium loss during heat treatment; mechanically stir at 500 rpm for 1 h at room temperature to obtain the precursor solution.
[0032] (2) Preparation of precursor materials The precursor solution obtained in step (1) was fed to a spray dryer using a peristaltic pump. The inlet temperature of the spray dryer was set to 230℃, the outlet temperature to 100℃, and the feed rate to 1L / h. Spray drying was performed under high temperature and high pressure to obtain the precursor material Li. 1.26(1-x) Ni 0.119 Co 0.119 Mn 0.119 O2, where x=0.
[0033] (3) Preparation of cathode materials The precursor material obtained in step (2) was placed in an alumina crucible, which was then placed in a box furnace. Under an air atmosphere, the temperature was increased at a rate of 3°C / min, and the material was heat-treated at 750°C for 300 min to obtain Li. 1.26 Ni 0.119 Co 0.119 Mn 0.119 O2-750 (x=0) cathode material.
[0034] Comparative Example 2: A method for preparing a lithium-rich manganese oxide cathode material with adjustable Li content and controlled heat treatment conditions includes the following steps: The preparation method is the same as that of Comparative Example 1, except that in the preparation of the positive electrode material, the precursor material obtained in step (2) is placed in an alumina crucible, the alumina crucible is placed in a box furnace, and the temperature is increased at a rate of 3℃ / min under an air atmosphere, and heat-treated at 800℃ for 300min to obtain Li. 1.26 Ni 0.119 Co 0.119 Mn 0.119 O2-800 (x=0) cathode material.
[0035] Comparative Example 3: A method for preparing a lithium-rich manganese oxide cathode material with adjustable Li content and controlled heat treatment conditions includes the following steps: The preparation method is the same as that of Comparative Example 1, except that in the preparation of the positive electrode material, the precursor material obtained in step (2) is placed in an alumina crucible, the alumina crucible is placed in a box furnace, and the temperature is increased at a rate of 3℃ / min under air atmosphere, and heat-treated at 850℃ for 300min to obtain Li. 1.26 Ni 0.119 Co 0.119 Mn 0.119 O2-850 (x=0) cathode material.
[0036] Experimental Example 1: XRD Test The lithium-rich manganese-based cathode materials prepared in Example 7 and Comparative Example 3 were subjected to XRD tests to observe the phase structure of the lithium-rich manganese-based cathode materials.
[0037] Experimental results are as follows Figure 1 As shown, all samples can be attributed to typical R... The "honeycomb" ordered arrangement of the m-symmetry (α-NaFeO2) and the additional peak at 20-25° in Li2MnO3 with the C2 / m space group. However, with a decrease in lithium content, the (003) peak in Example 7 shifts to the left (Fig. b), indicating an increase in the lithium interlayer spacing. The intensity of the superstructure peak at 20-25° increases (Fig. c), indicating improved crystallinity of the Li2MnO3 phase in the material.
[0038] Experimental Example 2: XRD Test The lithium-rich manganese-based cathode materials prepared in Examples 2, 5, 7, and 8 were subjected to XRD tests to determine the average structure of the lithium-rich manganese-based cathode materials at different heat treatment temperatures.
[0039] Experimental results are as follows Figure 2 As shown in the figure. It can be seen that all samples in Examples 2 and 5-8 can be attributed to typical R. The "honeycomb" ordered arrangement in Li2MnO3 with C2 / m space group exhibits m-symmetry (α-NaFeO2) and additional peaks at 20-25°. Figure 2 a, c). As the heat treatment temperature increases, Figure 2 In b, the (003) peak shifts to the right, indicating a decrease in the lithium interlayer spacing. The I(003) / I(104) ratio fluctuates around 1.50. Figure 2 As can be seen from c, the intensity of the superstructure peak located at 20-25° also increases with the increase of heat treatment temperature, indicating that the crystallinity of the Li2MnO3 phase in the material is improved.
[0040] Experimental Example 3: TEM Test The lithium-rich manganese-based cathode materials prepared in Example 7 and Comparative Example 3 were subjected to TEM testing to test the local structure of the lithium-rich manganese-based cathode materials.
[0041] Experimental results are as follows Figure 3 and 4 As shown in the figure, the lithium-rich manganese-based cathode material prepared in this embodiment of the invention exhibits a high-density stacking fault in its bulk crystal structure when the Li content decreases. After performing FFT on the corresponding HRTEM image, continuous connecting lines / elongated fringes appear between the Bragg diffraction spots, which are typical diffraction characteristics of planar defects, further proving the formation of high-density, through-type stacking faults. Figure 4 This crystal structure, rich in stacking defects, can improve the performance of Li. + The insertion / extraction dynamics during charge / discharge. Simultaneously, during lithium-ion desorption cycles, lattice flexibility adapts to or dissipates strain. In contrast, comparative lithium-rich manganese materials exhibit a typical layered structure, such as... Figure 3 As shown.
[0042] Experimental Example 4: Electrochemical Performance Testing (1) Preparation of positive electrode sheet The lithium-rich manganese-based cathode materials, SuperP, and CMC prepared in Examples 1-8 and Comparative Examples 1-3 were weighed in a mass ratio of 86.7:10.8:2.5 and placed in a ball mill jar. 1250 mg of deionized water was added, and the mixture was placed on a ball mill and milled at 400 rpm for 4 hours. The mixture was then coated onto aluminum foil using a 0.15 μm scraper and dried in a vacuum drying oven at 110 °C for 20 hours. The coated material was then cut into electrode sheets with a diameter of 10 mm and then transferred to a vacuum oven at 115 °C for drying for 10 hours before use.
[0043] (2) Assemble CR2025 stainless steel button batteries Using lithium metal sheets as the negative electrode, 200 μL of LBC-3045I(G) commercial electrolyte was added. The CR2025 stainless steel button cell was assembled in a glove box filled with argon gas and with a moisture content of less than 0.01 ppm. Its charge and discharge performance was tested after standing at 45°C for 40 h.
[0044] Electrochemical performance testing of CR2025 stainless steel button cells: The battery cycle performance of Examples 1-8 and Comparative Examples 1-3 was tested using constant current charge-discharge method. The test temperature was 25℃, the voltage window was 2.0-4.8V, and the test current densities were 0.1C, 0.2C, 0.5C, 1C, 2C, 5C, 10C and 20C, respectively, where 1C = 200mA / g.
[0045] like Figure 5As shown, when the Li content is reduced by 10-20 at%, and the heat treatment temperature is controlled at 750-1000℃, the discharge specific capacity is significantly improved. The lithium-rich manganese oxide cathode material Li in this invention... 1.071 Ni 0.119 Co 0.119 Mn 0.119 The lithium-ion battery prepared by O2-850 (x=0.15) has a maximum initial discharge specific capacity of 303 mAh / g at a current density of 20 mA / g.
[0046] like Figure 6 As shown, by reducing the Li content by 10-20 at% (x=0.10-0.20) and controlling the heat treatment temperature to 800℃ in this invention, the lithium-ion battery obtained from the lithium-rich manganese oxide cathode material exhibits a capacity retention of up to 80.02% after 400 cycles at a current density of 200 mA / g (1C). This demonstrates a significant improvement in stability. After 500 cycles at a current density of 1 A / g (5C), the capacity retention reaches 90.54%. This shows a significant improvement in long-cycle stability at high rates. Under the same test conditions, the lithium-rich manganese oxide cathode material with a Li content reduced by 15 at% (x=0.15) and a heat treatment temperature controlled to 850℃... 1.071 Ni 0.119 Co 0.119 Mn 0.503 The lithium-ion batteries prepared with O2 maintained a capacity of 79.70% and 90.45% at current densities of 200 mA / g (1C) and 1 A / g (5C), respectively.
[0047] like Figure 7 As shown, the Li content was reduced by 15 at%, and the heat treatment temperature was controlled at 800, 850, and 1000 °C, resulting in a lithium-rich manganese oxide cathode material with Li content of 15 at%. 1.071 Ni 0.119 Co 0.119 Mn 0.503 The lithium-ion battery prepared by O2 exhibits good cycle stability at current densities of 200 mA / g (1C) and 1 A / g (5C).
[0048] like Figure 8 As shown, the Li content was reduced by 15 at%, and the heat treatment temperature was controlled at 850℃, resulting in a higher Li content in the lithium-rich manganese oxide cathode material of this invention. 1.071 Ni 0.119 Co 0.119 Mn 0.503 The lithium-ion battery prepared with O2 has a significantly higher lithium-ion diffusion coefficient than that of Comparative Example 3, exhibiting better kinetic characteristics and thus significantly improved rate performance. Figure 8 b).
[0049] like Figure 9 As shown, the Li content was reduced by 15 at%, and the heat treatment temperature was controlled at 850℃, resulting in a higher Li content in the lithium-rich manganese oxide cathode material of this invention. 1.071 Ni 0.119 Co 0.119 Mn 0.503 The lithium-ion battery prepared by O2 has good cycle stability at 4A / g (20C), with a discharge capacity of 133mAh / g and a capacity retention of 90.22% after 1000 cycles.
[0050] Experimental Example 5: Raman Test During the First Charge and Discharge Process Raman tests were performed on the lithium-rich manganese-based cathode materials prepared in Example 7 and Comparative Example 3 at different voltages during the first charge and discharge process to test the structural changes of the lithium-rich manganese-based cathode materials.
[0051] Experimental results are as follows Figure 10 As shown, the lithium-rich manganese-based cathode material provided in this embodiment exhibits higher structural reversibility and stability during the first charge-discharge cycle when the lithium content is reduced.
[0052] Experimental Example 6: TEM Test The lithium-rich manganese-based cathode materials prepared in Example 7 and Comparative Example 3 were subjected to TEM testing after being cycled 1000 times at 20C to test the microstructure changes of the lithium-rich manganese-based cathode materials after long-term cycling.
[0053] Experimental results are as follows Figure 11 As shown in the figure, the lithium-rich manganese-based cathode material with reduced Li content provided in this embodiment retains its original stacking fault structure after 1000 cycles at a high rate of 20C. This indicates that the structure can adapt to the strain of high-rate lithium insertion / extraction cycles, thereby maintaining good structural stability.
[0054] Of the above embodiments, Embodiment 7 is the best embodiment.
[0055] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A lithium-rich manganese oxide cathode material with high rate and long cycle stability, characterized in that: Its chemical formula is Li 1.26(1-x) Ni 0.119 Co 0.119 Mn 0.503 O2, where x = 0.10-0.
20.
2. The lithium-rich manganese oxide cathode material with high rate and long cycle stability according to claim 1, characterized in that: The value of x is 0.
15.
3. The method for preparing a lithium-rich manganese oxide cathode material with high rate and long cycle stability according to claim 1, characterized in that: First, a precursor solution was prepared, then spray-dried, and finally heat-treated to prepare Li. 1.26(1-x) Ni 0.119 Co 0.119 Mn 0.503 In the O2 precursor solution, the total concentration of acetate is 0.1-0.2 mol / L, the concentration of citric acid monohydrate is 0.2-0.5 mol / L, and lithium with a total mass of 3.0% is added.
4. The method for preparing a lithium-rich manganese oxide cathode material with high rate and long cycle stability according to claim 3, characterized in that: The heat treatment conditions are: 750-1000℃, holding for 20-300 minutes.
5. The method for preparing a lithium-rich manganese oxide cathode material with high rate and long cycle stability according to claim 4, characterized in that: The preferred heat treatment conditions are 850℃ for 300 min.
6. The application of the lithium-rich manganese oxide cathode material with high rate and long cycle stability as described in claim 1 in the preparation of lithium-ion batteries.