A nickel-manganese-based p2-type sodium-ion battery layered oxide positive electrode material and a preparation method thereof
By introducing Li into the layered oxide cathode material of P2 type sodium-ion battery and using high-energy ball milling technology, the problems of uneven doping and high energy consumption caused by long-term high-temperature processing were solved, realizing high-performance doping modification and rapid synthesis of the material, and improving the stability and electrochemical performance of the material.
Patent Information
- Application Number
- CN202611505212.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-24
- Publication Date
- 2026-11-24
AI Technical Summary
Existing P2-type sodium-ion battery layered oxide cathode materials suffer from problems such as high energy consumption, uneven distribution of doped elements, and unstable electrochemical performance under high-temperature and long-term treatment, making it difficult to achieve the dual goals of high-performance doping modification and rapid synthesis.
By introducing Li and combining it with high-energy ball milling technology, the mechanical force generated by high-energy ball milling is used to uniformly disperse Li⁺, shorten the calcination time, and adopt a method of rapid heating and natural cooling to achieve uniform doping and rapid synthesis of materials.
It significantly improves the crystal structure stability and electrochemical performance of the material, enhances rate performance and cycle stability, shortens synthesis time, reduces energy consumption, and is suitable for industrial production.
Smart Images

Figure CN123162174A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a cathode material, specifically a nickel-manganese-based P2-type sodium-ion battery layered oxide cathode material. The invention also discloses a method for preparing this nickel-manganese-based P2-type sodium-ion battery layered oxide cathode material; it belongs to the field of battery technology. Background Technology
[0002] Sodium-ion batteries (SIBs) are considered one of the most promising electrochemical energy storage technologies for large-scale energy storage due to the abundance of sodium resources (approximately 2.83% in the Earth's crust, far exceeding lithium's 0.01%), their wide distribution, and low cost. The cathode material is the core component determining the performance and cost of sodium-ion batteries. Among numerous cathode material systems, layered transition metal oxides (Na₂O₃) are particularly important. x TMO2 (TM is a transition metal) has attracted widespread attention from the academic community due to its high theoretical specific capacity, good layered reversible structure, and relatively simple synthesis process.
[0003] Based on the differences in the coordination environment of sodium ions between transition metal layers, layered oxides can be divided into two main categories: P2-type and O3-type. Among them, P2-type materials, due to their larger interlayer spacing and open prismatic sodium ion diffusion channels, exhibit faster sodium ion diffusion kinetics and higher operating voltage, and are considered one of the most promising cathode material systems for sodium-ion batteries. Typical P2-type materials include Na... 0.67 Ni 0.33 Mn 0.67 O2 (P2-NNMO) has high specific capacity and operating voltage, and relatively good air stability.
[0004] However, P2-type layered oxide cathode materials still face a series of severe challenges in practical applications. Firstly, during charge and discharge processes, especially at high voltages, P2-type materials are prone to undergoing an irreversible P2-O2 phase transition, i.e., Na+. + During the extraction process, electrostatic repulsion between adjacent MO2 layers promotes oxygen layer slippage, leading to material volume expansion and structural degradation. Secondly, Mn... 3+ The Jahn-Teller effect of ions causes asymmetric distortion of the MnO6 octahedron, disrupting the integrity of the crystal structure and leading to rapid capacity decay. Furthermore, Na... + / Empty spaces arranged in an orderly manner, Na + The large ionic radius and other issues that cause kinetic barriers also severely restrict the rate performance and cycle stability of the material.
[0005] To overcome these problems, researchers have developed various modification strategies, mainly including elemental doping (bulk doping), surface coating, and composite phase structure design. Among these, elemental doping, by introducing heterogeneous ions to replace transition metal sites or sodium sites, can effectively regulate crystal structure, suppress phase transitions, alleviate the Jahn-Teller effect, and improve ion diffusion kinetics. For example, Ti doping can increase the Na interlayer spacing and reduce the Mn³⁺ content, thereby alleviating the Jahn-Teller effect; Al / K co-doping can establish a rigid structural framework and enhance electrostatic shielding; and K / Cu synergistic regulation can expand the interlayer spacing while reducing the proportion of Jahn-Teller active ions Mn³⁺.
[0006] Currently, the mainstream preparation method for P2-type layered oxide cathode materials is the high-temperature solid-state method and its derivative processes, which typically employ the following schemes:
[0007] (1) Traditional high-temperature solid-state method
[0008] The traditional high-temperature solid-state method is the most typical route for synthesizing P2-type layered oxides. The process involves weighing sodium (such as Na2CO3, NaOH, etc.), manganese (such as MnO2, MnCO3, etc.), and other transition metal sources (such as NiO, Co3O4, etc.) according to the stoichiometric ratio of the target chemical formula. The raw materials are then thoroughly mixed using methods such as ball milling or grinding. The mixed powder is then placed in a high-temperature furnace and calcined at high temperature in an air or oxygen atmosphere. Typical calcination conditions are 900℃ for 15 hours. The advantages of the high-temperature solid-state method are its simplicity, low cost, and suitability for large-scale production.
[0009] However, due to the extremely low diffusion coefficient between solid raw materials in solid-state reactions, the reactants need to be held at high temperatures for extended periods to achieve uniform diffusion of elements. Some literature reports even indicate that synthesis temperatures exceeding 900°C are required for the material to form a pure P2 phase. After calcination, the material typically needs to be cooled to room temperature with the furnace, making the entire process extremely time-consuming.
[0010] (2) Coprecipitation method combined with high temperature solid phase method
[0011] To overcome the problems of uneven elemental distribution and uncontrollable product morphology in traditional solid-state methods, some studies have adopted a co-precipitation method to first synthesize a precursor with highly uniform composition, and then combine it with high-temperature solid-state sintering to obtain the final product. This method first dissolves soluble salts (such as sulfates, nitrates, and acetates) of the transition metals (such as Ni, Mn, Co, Fe, and Cu) required for the target product in deionized water at precise stoichiometric ratios to prepare a mixed metal salt solution. Then, under continuous stirring, the mixed salt solution, along with a precipitant (such as NaOH or Na₂CO₃) and a complexing agent (such as ammonia), are simultaneously added to the reactor. By precisely controlling parameters such as the pH value, reaction temperature, and stirring speed, the metal ions co-precipitate to generate a homogeneous hydroxide or oxalate precursor precipitate. After precipitation, the slurry is aged, filtered, and washed to remove impurity ions, and finally dried to obtain the precursor powder. After mixing and grinding the obtained precursor with a sodium source (such as Na2CO3, NaOH, etc.) according to the target stoichiometric ratio, it is calcined at high temperature in an air or oxygen atmosphere to obtain P2-type or O3-type layered oxide cathode materials.
[0012] However, the above methods typically have the following problems: 1. Whether it is the traditional high-temperature solid-state method or the co-precipitation method combined with the high-temperature solid-state method, both require long-term heat treatment at 900℃ or higher (usually 12-16 hours or even longer). This prolonged high-temperature treatment not only consumes a large amount of energy and increases production costs, but also severely restricts production efficiency, hindering the large-scale industrial production and widespread application of sodium-ion battery cathode materials. 2. In existing solid-state doping processes, the dopant source (such as oxides or salts) is usually mixed with other raw materials through mechanical ball milling or grinding. Under conventional ball milling or grinding conditions, this physical mixing method is limited by input energy and solid-state diffusion kinetics, making it difficult to achieve uniform dispersion at the molecular / atomic level. Due to the limitations of solid-state diffusion, even after long-term high-temperature calcination, the distribution of dopant elements in the bulk phase of the material may still exhibit microscopic inhomogeneity, leading to inconsistent doping effects between the same batch of products, and even between different particles of the same product, thus affecting the stability and consistency of the material's electrochemical performance; existing modification strategies struggle to simultaneously meet the dual requirements of "structural stability" and "rapid synthesis."
[0013] While existing technologies have made some progress in elemental doping modification, the implementation of these doping strategies still relies on traditional high-temperature, long-time sintering processes. Sodium is prone to volatilization at high temperatures, causing the actual sodium content to deviate from the designed stoichiometry, which affects the consistency of the material's crystal structure and electrochemical performance.
[0014] Furthermore, prolonged high-temperature treatment may promote the formation of impurity phases and reduce the phase purity of the product. In other words, existing technologies either pursue material performance (using doping + prolonged high-temperature sintering) or synthesis efficiency (using simple solid-state methods with little or no doping), making it difficult to simultaneously achieve the dual goals of "high-performance doping modification" and "rapid and efficient synthesis". Summary of the Invention
[0015] In view of the defects and deficiencies in the prior art, the first objective of this invention is to provide a layered oxide cathode material for nickel-manganese-based P2 type sodium-ion batteries, which has uniform element distribution, good crystal structure stability, and excellent electrochemical performance.
[0016] The second objective of this invention is to provide a method for preparing a layered oxide cathode material for nickel-manganese-based P2-type sodium-ion batteries. This method can significantly shorten the synthesis time and reduce energy consumption, while achieving effective bulk phase doping modification through the introduction of Li elements. Combined with additional pretreatment by high-energy ball milling, the resulting cathode material has good crystal structure stability and excellent electrochemical performance.
[0017] The third objective of this invention is to apply the cathode material to sodium-ion batteries, so that the resulting sodium-ion batteries have both excellent rate performance and cycle stability.
[0018] Therefore, the first technical solution provided in this application is as follows:
[0019] A layered oxide cathode material for nickel-manganese-based P2-type sodium-ion batteries, wherein the molecular formula of the layered oxide cathode material for nickel-manganese-based P2-type sodium-ion batteries is Na. 0.75 Li 0.11 Mg 0.11 Ni 0.1 Mn 0.68 O2.
[0020] The second technical solution provided in this application is as follows: a method for preparing a layered oxide cathode material for nickel-manganese-based P2 type sodium-ion batteries, comprising the following steps in sequence:
[0021] 1) Weigh out sodium compound, lithium compound, nickel compound, magnesium compound, and manganese compound according to the molar ratio of Na:Li:Ni:Mg:Mn = 0.75:0.11:0.10:0.11:0.68, add anhydrous ethanol to obtain a mixture;
[0022] 2) Add the mixture prepared in step 1) into a ball mill jar, add zirconium dioxide grinding beads, and perform high-energy ball milling (including pauses).
[0023] 180min-480min; take out the material and centrifuge it. After drying, grind the resulting material evenly and compress it into tablets.
[0024] 3) After the material in step 2) is compressed into tablets, it is heated to 850-950℃ in air and then cooled directly to 50-200℃.
[0025] 4) Cooling and post-processing: Grind the product obtained in step 3) until the particles are uniform to obtain the nickel-manganese-based P2 type sodium-ion battery layered oxide cathode material.
[0026] Furthermore, in the above-mentioned method for preparing layered oxide cathode material for nickel-manganese-based P2 type sodium-ion batteries, the sodium compound mentioned in step 2) is sodium carbonate or sodium hydroxide;
[0027] The lithium compound is lithium hydroxide, lithium carbonate, or lithium oxide;
[0028] The nickel compound is nickel oxide;
[0029] The magnesium compound mentioned is magnesium oxide;
[0030] The manganese compound is manganese trioxide, manganese dioxide, or manganese carbonate.
[0031] Furthermore, in the above-mentioned method for preparing layered oxide cathode material for nickel-manganese-based P2 type sodium-ion batteries, the diameter of the zirconium dioxide ball milling beads in step 2) is 3 mm.
[0032] Furthermore, in the above-mentioned preparation method of layered oxide cathode material for nickel-manganese-based P2 type sodium-ion batteries, the high-energy ball milling is performed at a speed of 300 rpm for 5 minutes, then paused for 5 minutes, which constitutes one cycle, and a total of 18-48 cycles are performed.
[0033] Furthermore, in the above-mentioned preparation method of layered oxide cathode material for nickel-manganese-based P2 type sodium-ion batteries, the drying process involves placing the material in a vacuum drying oven at 100 °C for 12 h.
[0034] Furthermore, in the above-mentioned preparation method of layered oxide cathode material for nickel-manganese-based P2 type sodium-ion batteries, the pressing is performed by placing the material described in step 2) into a pressing mold and pressing it under a pressure of 10 MPa for 5 min.
[0035] Furthermore, in the above-mentioned preparation method of layered oxide cathode material for nickel-manganese-based P2 type sodium-ion batteries, the heating rate is 2 ℃ / min.
[0036] The layered oxide cathode material for nickel-manganese-based P2-type sodium-ion batteries provided in this application introduces Li into the raw materials. During high-temperature processing, Li partially replaces Ni sites in the transition metal layer. Due to Li's low oxidation state, small ionic radius, and strong Li-O bonding characteristics, its introduction can regulate the local electronic configuration and lattice framework stability of the layered oxide, suppress anion redox, and inhibit phase transitions and structural degradation, thereby significantly improving the crystal structure stability and electrochemical performance of the material.
[0037] The technical solution provided in this application introduces strong mechanical force through high-speed impact, shearing, and crushing in high-energy ball milling. This continuously breaks down the precursor particles and generates a large number of fresh reaction interfaces. Crystalline lithium compounds (such as lithium carbonate and lithium oxide) undergo interfacial ion diffusion under the mechanical force, leading to the formation of Li... + It is uniformly dispersed in the precursor mixture. Simultaneously, it significantly shortens the calcination time for Na. + The diffusion distance of transition metal ions is reduced, making the distribution of doped elements more uniform and further reducing calcination time.
[0038] Under the synergistic effect of the above two aspects, the technical solution provided in this application can be heated to 850-950 ℃ at a rate of 2 ℃ / min and then immediately cooled to 50-200 ℃, thereby obtaining a cathode material with a good P2 type layered structure, uniform element distribution and excellent electrochemical performance.
[0039] The present invention also provides a sodium-ion battery cathode, comprising the cathode material described in the first technical solution.
[0040] The present invention also provides a sodium-ion battery comprising the sodium-ion battery positive electrode described in the above technical solution.
[0041] Compared with the prior art, the technical solution provided in this application has the following technical advantages:
[0042] (1) The technical solution provided in this application achieves effective control of the crystal structure of the material by introducing Li element, suppressing the P2-O2 phase transition under high voltage and alleviating Mn 3+ The Jahn-Teller effect enhances the structural stability and cycling performance of the material; the structural reversibility of the material during charge and discharge is significantly improved, and the first-cycle discharge specific capacity at 1C rate reaches 167.2 mAh / g in the voltage range of 1.5-4.5 V; after 100 cycles at 1C, the capacity retention rate can reach more than 82.89%.
[0043] (2) The technical solution provided in this application introduces strong mechanical force through high-speed impact, shearing, and crushing in high-energy ball milling. The precursor particles are continuously broken and a large number of fresh reaction interfaces are generated. Crystalline Li2CO3 undergoes ion diffusion at the interface, and Li+ It is uniformly dispersed in the precursor mixture. Simultaneously, it significantly shortens the calcination time for Na. + The diffusion distance of transition metal ions makes the distribution of doped elements more uniform and further reduces the calcination time. Combined with the synergistic effect of high-energy ball milling, the heat preservation time of P2 type layered oxide cathode material is shortened by more than ten hours, energy consumption is significantly reduced, production efficiency is improved, and it is conducive to large-scale industrial production.
[0044] (3) The technical solution provided in this application achieves atomic-level uniform distribution of Li in the bulk phase of the material through the additional treatment of high-energy ball milling, which effectively overcomes the defect of uneven distribution of doped elements in the traditional solid phase method and ensures the consistency and stability of performance between the same batch of products and different batches of products.
[0045] In summary, the technical solution provided in this application achieves a balance between "high-performance doping modification" and "rapid and efficient synthesis" through the synergy of Li and high-energy ball milling. Attached Figure Description
[0046] Figure 1 These are the XRD patterns of Example 1, Comparative Example 1, Comparative Example 2, and Comparative Example 3;
[0047] Figure 2 These are the XRD patterns of Examples 2, 3, and 4;
[0048] Figure 3 This is a 1 C long cycle diagram of Example 1, Comparative Example 1, Comparative Example 2, and Comparative Example 3;
[0049] Figure 4 These are the rate performance charts of Example 1, Comparative Example 1, Comparative Example 2, and Comparative Example 3.
[0050] Figure 5 This is a SEM image of NM-LiMg-OH from Example 1;
[0051] Figure 6 This is a refined image of NM-LiMg-OH from Example 1;
[0052] Figure 7 These are charge-discharge curves for the first and third cycles of Example 1 and Comparative Example 3. Detailed Implementation
[0053] The technical solution of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0054] Example 1
[0055] This embodiment provides a layered oxide cathode material for nickel-manganese-based P2-type sodium-ion batteries, the molecular formula of which is Na. 0.75 Li 0.11 Mg 0.11 Ni 0.1 Mn 0.68 O 2, It is denoted as NM-LiMg-OH.
[0056] It is prepared sequentially through the following steps:
[0057] (1) Weigh 0.0375 mol sodium carbonate, 0.0055 mol lithium carbonate, 0.01 mol nickel oxide, 0.011 mol magnesium oxide, 0.068 mol manganese dioxide, an appropriate amount of 3 mm diameter zirconium dioxide grinding beads and anhydrous ethanol, just enough to cover the materials (sodium carbonate and lithium carbonate need to be added in excess by 5%).
[0058] (2) Add the material from step (1) into the ball mill jar, mill at 300 rpm for 5 min, then pause for 5 min, and repeat this cycle for a total of 36 cycles. After that, take out the material, centrifuge it, and place it in a vacuum drying oven at 100 ℃ for 12 h. After grinding the obtained material evenly, take an appropriate amount and put it into the tableting mold, and use a tableting machine to press it into tablets at a pressure of 10 MPa for 5 min.
[0059] (3) The material processed in step (2) is placed in a high-temperature muffle furnace and heated to 900 ℃ at 2 ℃ / min in an air atmosphere, and then cooled directly to 100 ℃ without heat preservation.
[0060] (4) Grind the product obtained in step (3) until the particles are uniform, and the layered oxide cathode material NM-LiMg-OH based on nickel-manganese P2 type sodium-ion battery is obtained.
[0061] Example 2
[0062] This embodiment provides a layered oxide cathode material for nickel-manganese-based P2-type sodium-ion batteries, the molecular formula of which is Na. 0.75 Li 0.11 Mg 0.11 Ni 0.1 Mn 0.68 O2, denoted as NM-LiMg-860.
[0063] It is prepared sequentially through the following steps:
[0064] (1) Weigh 0.0375 mol sodium carbonate, 0.0055 mol lithium carbonate, 0.01 mol nickel oxide, 0.011 mol magnesium oxide, 0.068 mol manganese dioxide, an appropriate amount of 3 mm diameter zirconium dioxide grinding beads and anhydrous ethanol, just enough to cover the materials (sodium carbonate and lithium carbonate need to be added in excess by 5%).
[0065] (2) Add the material from step (1) into the ball mill jar, mill at 300 rpm for 5 min, then pause for 5 min, and repeat this cycle for a total of 36 cycles. After that, take out the material, centrifuge it, and place it in a vacuum drying oven at 100 ℃ for 12 h. After grinding the obtained material evenly, take an appropriate amount and put it into the tableting mold, and use a tableting machine to press it into tablets at a pressure of 10 MPa for 5 min.
[0066] (3) The material processed in step (2) is placed in a high-temperature muffle furnace and heated to 860 ℃ at 2 ℃ / min in an air atmosphere, and then cooled directly to 100 ℃ without heat preservation.
[0067] (4) Grind the product obtained in step (3) until the particles are uniform, and the layered oxide cathode material NM-LiMg-860 based on nickel-manganese P2 type sodium-ion battery is obtained.
[0068] Example 3
[0069] This embodiment provides a layered oxide cathode material for nickel-manganese-based P2-type sodium-ion batteries, the molecular formula of which is Na. 0.75 Li 0.11 Mg 0.11 Ni 0.1 Mn 0.68 O2, denoted as NM-LiMg-880.
[0070] It is prepared sequentially through the following steps:
[0071] (1) Weigh 0.0375 mol sodium carbonate, 0.0055 mol lithium carbonate, 0.01 mol nickel oxide, 0.011 mol magnesium oxide, 0.068 mol manganese dioxide, an appropriate amount of 3 mm diameter zirconium dioxide grinding beads and anhydrous ethanol, just enough to cover the materials (sodium carbonate and lithium carbonate need to be added in excess by 5%).
[0072] (2) Add the material from step (1) into the ball mill jar, mill at 300 rpm for 5 min, then pause for 5 min, and repeat this cycle for a total of 36 cycles. After that, take out the material, centrifuge it, and place it in a vacuum drying oven at 100 ℃ for 12 h. After grinding the obtained material evenly, take an appropriate amount and put it into the tableting mold, and use a tableting machine to press it into tablets at a pressure of 10 MPa for 5 min.
[0073] (3) The material processed in step (2) is placed in a high-temperature muffle furnace and heated to 880 ℃ at 2 ℃ / min in an air atmosphere, and then cooled directly to 100 ℃ without heat preservation.
[0074] (4) Grind the product obtained in step (3) until the particles are uniform, and the layered oxide cathode material NM-LiMg-880 based on nickel-manganese-based P2 type sodium-ion battery is obtained.
[0075] Example 4
[0076] This embodiment provides a layered oxide cathode material for nickel-manganese-based P2-type sodium-ion batteries, the molecular formula of which is Na. 0.75 Li 0.11 Mg 0.11 Ni 0.1 Mn 0.68 O2, denoted as NM-LiMg-950.
[0077] It is prepared sequentially through the following steps:
[0078] (1) Weigh 0.0375 mol sodium carbonate, 0.0055 mol lithium carbonate, 0.01 mol nickel oxide, 0.011 mol magnesium oxide, 0.068 mol manganese dioxide, an appropriate amount of 3 mm diameter zirconium dioxide grinding beads and anhydrous ethanol, just enough to cover the materials (sodium carbonate and lithium carbonate need to be added in excess by 5%).
[0079] (2) Add the material from step (1) into the ball mill jar, mill at 300 rpm for 5 min, then pause for 5 min, and repeat this cycle for a total of 36 cycles. After that, take out the material, centrifuge it, and place it in a vacuum drying oven at 100 ℃ for 12 h. After grinding the obtained material evenly, take an appropriate amount and put it into the tableting mold, and use a tableting machine to press it into tablets at a pressure of 10 MPa for 5 min.
[0080] (3) The material processed in step (2) is placed in a high-temperature muffle furnace and heated to 950 ℃ at 2 ℃ / min in an air atmosphere, and then cooled directly to 100 ℃ without heat preservation.
[0081] (4) Grind the product obtained in step (3) until the particles are uniform, and the NM-LiMg-950 layered oxide cathode material based on nickel-manganese-based P2 type sodium-ion battery is obtained.
[0082] Comparative Example 1
[0083] This comparative example provides a layered oxide cathode material for nickel-manganese-based P2-type sodium-ion batteries, the molecular formula of which is Na. 0.75 Li 0.11 Mg 0.11 Ni 0.1 Mn 0.68 O 2, It is denoted as NM-LiMg-15H.
[0084] It is prepared sequentially through the following steps:
[0085] (1) Weigh 0.0375 mol sodium carbonate, 0.0055 mol lithium carbonate, 0.01 mol nickel oxide, 0.011 mol magnesium oxide, and 0.068 mol manganese dioxide (sodium carbonate and lithium carbonate need to be added in excess by 5%).
[0086] (2) Add the materials from step (1) into the mortar and grind manually for 20 min;
[0087] (3) The material after step (2) is placed in a high-temperature muffle furnace and heated to 900 ℃ at 2 ℃ / min in an air atmosphere. After holding at the temperature for 15 h, it is naturally cooled to 100 ℃.
[0088] (4) Grind the product obtained in step (3) until the particles are uniform, and the nickel-manganese-based P2 type sodium-ion battery layered oxide cathode material is obtained, denoted as NM-LiMg-15H.
[0089] Comparative Example 2
[0090] This comparative example provides a layered oxide cathode material for nickel-manganese-based P2-type sodium-ion batteries, with the molecular formula Na. 0.64 Mg 0.11 Ni 0.21 Mn 0.68 O 2, It is denoted as NM-Mg-OH.
[0091] It is prepared sequentially through the following steps:
[0092] (1) Weigh out 0.032 mol sodium carbonate, 0.021 mol nickel oxide, 0.011 mol magnesium oxide and 0.068 mol manganese dioxide (sodium carbonate needs to be added in excess by 5%).
[0093] (2) Add the materials from step (1) into the mortar and grind manually for 20 min;
[0094] (3) The material processed in step (2) is placed in a high-temperature muffle furnace and heated to 900 ℃ at 2 ℃ / min in an air atmosphere, and then cooled directly to 100 ℃ without heat preservation.
[0095] (4) Grind the product obtained in step (3) until the particles are uniform to obtain the layered oxide cathode material based on nickel-manganese P2 type sodium-ion battery, denoted as NM-Mg-OH.
[0096] Comparative Example 3
[0097] This comparative example provides a layered oxide cathode material for nickel-manganese-based P2-type sodium-ion batteries, with the molecular formula Na. 0.64 Mg 0.11 Ni 0.21 Mn 0.68 O2, denoted as NM-Mg-15H.
[0098] It is prepared sequentially through the following steps:
[0099] (1) Weigh out 0.032 mol sodium carbonate, 0.021 mol nickel oxide, 0.011 mol magnesium oxide and 0.068 mol manganese dioxide (sodium carbonate needs to be added in excess by 5%).
[0100] (2) Add the materials from step (1) into the mortar and grind manually for 20 min;
[0101] (3) The material after step (2) is placed in a high-temperature muffle furnace and heated to 900 ℃ at 2 ℃ / min in an air atmosphere. After holding at the temperature for 15 h, it is naturally cooled to 100 ℃.
[0102] (4) Grind the product obtained in step (3) until the particles are uniform, and the nickel-manganese-based P2 type sodium-ion battery layered oxide cathode material is obtained, denoted as NM-Mg-15H.
[0103] NM-LiMg-OH prepared in Example 1; NM-LiMg-15H prepared in Comparative Example 1; NM-Mg-OH prepared in Comparative Example 2; NM-Mg-15H prepared in Comparative Example 3.
[0104] To verify the performance of the positive electrode provided in this application, button half-cells were assembled in Example 1, Comparative Example 1, Comparative Example 2, and Comparative Example 3 using the same steps, as follows:
[0105] (1) Weigh 80 mg of the prepared P2 type nickel-manganese base layer oxide positive electrode material, 10 mg of conductive agent (Super P) and 10 mg of binder (polyvinylidene fluoride) (mass ratio 8:1:1), and add an appropriate amount of dispersant N-methylpyrrolidone (NMP). After the above materials are mixed evenly, they are coated on carbon-coated aluminum foil, dried in a vacuum oven at 80°C for 12 hours, and then stamped into a positive electrode sheet with a diameter of 12 mm.
[0106] (2) Assemble the above positive electrode sheets into a CR20232 button cell in an argon glove box; wherein the negative electrode is a sodium metal sheet, the electrolyte is 1 M sodium perchlorate (NaClO4) dissolved in a 1:1 volume ratio of propylene carbonate (PC) and ethylene carbonate (EC) mixed solvent, and 5 wt% (mass fraction) of fluoroethylene carbonate (FEC) is added, and glass fiber GF / D (Whatman) is used as the separator;
[0107] (3) Charge-discharge tests were performed on the above button batteries at room temperature using the Blue Battery Testing System:
[0108] Using constant current charge / discharge mode, the charging / discharging current density is set to n (n=0.1,0.25,0.5,1,5) C (1C=200 mA g). -1 The voltage range is 1.5-4.5 V (vs. Na). + / Na), the test temperature was 30℃.
[0109] pass Figure 1 As can be seen from the comparison with the standard PDF card of P2-type layered oxides, NM-LiMg-OH doped with Li and without heat preservation, NM-LiMg-15H doped with Li and heat preservation for 15 h, and NM-Mg-15H without Li doping but heat preservation for 15 h have all become pure P2 phases; NM-Mg-OH without Li doping and without heat preservation still contains a lot of intermediate phases; indicating that the material synthesized in this application is confirmed to be a P2 phase material, and the synthesis method provided in this application can significantly shorten the heat preservation time, reduce energy consumption, and improve production efficiency.
[0110] pass Figure 2 As can be seen, compared with the standard PDF card of P2-type layered oxides, NM-LiMg-950, NM-LiMg-880, and NM-LiMg-860 prepared in this application have all formed pure P2 phase.
[0111] pass Figure 3It can be seen that among the four materials, NM-LiMg-0H consistently maintains the highest and most stable specific capacity: the specific capacity reaches 167 mAh / g in the initial cycling stage and can still maintain about 139 mAh / g after 100 cycles. The capacity decay is extremely gradual throughout the cycling process, without any sudden drop or stepwise decrease in capacity. In contrast, the specific capacity of undoped NM-Mg-0H drops to 82 mAh / g after 100 cycles, with a significantly faster capacity decay rate. The specific capacity of NM-LiMg-15H with extended sintering time is about 100 mAh / g after 100 cycles, with both capacity and stability lower than NM-LiMg-0H. NM-Mg-15H exhibits the worst specific capacity and stability. It can be seen that compared with the undoped sample and the control sample with extended sintering time, NM-LiMg-0H improves structural stability without sacrificing discharge specific capacity, achieving an excellent balance between high capacity and long cycle life.
[0112] pass Figure 4 It can be seen that the capacity of NM-LiMg-OH decreases in a stepwise manner as the current increases from 0.1C to 5C, but the decrease is relatively gradual. The initial capacity at 0.1C is 180~185 mAh / g, and the capacity at 1C is about 160 mAh / g (due to 15 cycles at low current density, the capacity is slightly lower than the initial capacity after long cycling). At the high rate of 5C, the capacity is maintained at around 120 mAh / g. After stabilizing at the initial 0.1C, the capacity of NM-LiMg-15H remains at 160 mAh / g, and the capacity at 1C is 130-140 mAh / g. At the high rate of 5C, the capacity decays to 80-90 mAh / g.
[0113] The two undoped Li samples showed similar capacity changes with varying current density. Initially, they exhibited high capacity at 0.1C, ranging from 190 to 210 mAh / g. Subsequently, the capacity decreased rapidly, reaching approximately 130 to 140 mAh / g at 1C, and then rapidly decaying to 80 to 90 mAh / g at a high rate of 5C.
[0114] Therefore, NM-LiMg-OH exhibits stable stepped capacity output across a wide current density range from 0.1C to 5C. Particularly at 5C, this material maintains a high discharge specific capacity (82.89% capacity retention at 5C). Compared to NM-LiMg-15H with a longer sintering time and the undoped NM-Mg-OH / 15H system, the NM-LiMg-OH described in this invention exhibits superior capacity retention in the high-rate region from 1C to 5C.
[0115] pass Figure 5It can be seen that the cathode material powder particles obtained in Example 1 exhibit a uniform blocky morphological feature.
[0116] Figure 6 This is a refined image of NM-LiMg-OH from Example 1, obtained using GSAS-II software. The fitting variance is 8.97%, which meets the requirement of less than 15%, indicating a relatively accurate fit. The fitting shows that Example 1 has a close-packed hexagonal crystal system with lattice constants a, b, and c of 2.886 Å and a cell volume of 79.83 Å. 3 .
[0117] Figure 7 These are the charge-discharge curves of Example 1 and Comparative Example 3 at a current density of 1C for the first and third cycles. It can be observed that the charge-discharge curve of NM-Mg-15H has a clear plateau, while the charge-discharge curve of NM-LiMg-0H is smoother. This indicates that NM-Mg-15H undergoes multiple phase transitions during electrochemical cycling, affecting the stability of the cycle. The solid solution effect of NM-LiMg-0H is more obvious, resulting in stronger cycle stability.
[0118] In summary, the NM-LiMg-OH crystal structure prepared in Example 1 exhibits higher cycling stability and can effectively buffer the volume expansion and contraction caused by sodium ion extraction / intercalation during long-term charge and discharge processes, thus effectively suppressing structural collapse and phase transformation degradation.
Claims
1. A layered oxide cathode material for nickel-manganese-based P2-type sodium-ion batteries, characterized in that, The molecular formula of the layered oxide cathode material for nickel-manganese-based P2 type sodium-ion batteries is Na. 0.75 Li 0.11 Mg 0.11 Ni 0.1 Mn 0.68 O2.
2. The preparation method of the layered oxide cathode material for nickel-manganese-based P2-type sodium-ion batteries according to claim 1, characterized in that, The steps are as follows: 1) Weigh out sodium compound, lithium compound, nickel compound, magnesium compound, and manganese compound according to the molar ratio of Na:Li:Ni:Mg:Mn = 0.75:0.11:0.10:0.11:0.68, add anhydrous ethanol to obtain a mixture; 2) Add the mixture prepared in step 1) into a ball mill jar, add zirconium dioxide ball milling beads, and ball mill for 180 min-480 min at high energy; take out the material, centrifuge, dry it, grind the obtained material evenly, and then compress it into tablets; 3) After the material in step 2) is compressed, it is heated to 850-950℃ in air, and then cooled directly to 50-200℃. 4) Cooling and post-processing: Grind the product obtained in step 3) until the particles are uniform to obtain the nickel-manganese-based P2 type sodium-ion battery layered oxide cathode material.
3. The method for preparing the layered oxide cathode material for nickel-manganese-based P2-type sodium-ion batteries according to claim 2, characterized in that, The sodium compound mentioned in step 1) is sodium carbonate or sodium hydroxide; The lithium compound is lithium hydroxide, lithium carbonate, or lithium oxide; The nickel compound is nickel oxide; The magnesium compound mentioned is magnesium oxide; The manganese compound is manganese trioxide, manganese dioxide, or manganese carbonate.
4. The method for preparing the layered oxide cathode material for nickel-manganese-based P2-type sodium-ion batteries according to claim 2, characterized in that, The zirconia grinding beads mentioned in step 2) have a diameter of 3 mm.
5. The method for preparing the layered oxide cathode material for nickel-manganese-based P2-type sodium-ion batteries according to claim 2, characterized in that, The high-energy ball milling is performed using a planetary ball mill at a speed of 300 rpm for 5 minutes, followed by a 5-minute pause, which constitutes one cycle, and a total of 18-48 cycles are performed.
6. The method for preparing the layered oxide cathode material for nickel-manganese-based P2-type sodium-ion batteries according to claim 2, characterized in that, The drying process involved placing the product in a vacuum drying oven at 100 °C for 12 hours.
7. The method for preparing the layered oxide cathode material for nickel-manganese-based P2-type sodium-ion batteries according to claim 2, characterized in that, The tableting process involves placing the material described in step 2) into a tableting mold and using a tableting machine to compress the tablet at a pressure of 10 MPa for 5 minutes. The heating rate in step 3) is 2 °C / min.
8. A sodium-ion battery positive electrode, characterized in that, Including the nickel-manganese-based P2-type sodium-ion battery layered oxide cathode material as described in claim 1.
9. The method for preparing the sodium-ion battery positive electrode sheet according to claim 8, characterized in that, Includes the following steps: The layered oxide cathode material of nickel-manganese-based P2 type sodium-ion battery as described in claim 1, the conductive agent Super-P and the binder polyvinylidene fluoride are mixed in a mass ratio of 8:1:1, N-methylpyrrolidone is added as a dispersant, and the mixture is stirred and ground to form a uniform slurry. The slurry is coated on carbon-coated aluminum foil and dried in a vacuum oven to obtain the sodium-ion battery cathode sheet.
10. A sodium-ion battery, characterized in that, It includes the sodium-ion battery positive electrode sheet as described in claim 8.