Positive electrode laminate, solid-state battery, and method for manufacturing solid-state battery
By controlling the S/Ni ratio on the surface of the positive electrode active material layer and partially covering the sulfide solid electrolyte, the problem of insufficient adhesion between the positive electrode stack and the solid electrolyte layer in solid-state batteries was solved, achieving a positive electrode stack with high adhesion and low resistance, thus improving the charge and discharge performance of solid-state batteries.
Patent Information
- Application Number
- CN202610654071.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2025-05-22
- Filing Date
- 2026-05-13
- Publication Date
- 2026-11-24
AI Technical Summary
In the manufacturing process of solid-state batteries, insufficient adhesion between the positive electrode stack and the solid electrolyte layer leads to increased resistance and affects charge and discharge performance.
By controlling the mass ratio of sulfur atoms to nickel atoms (S/Ni) to be above 0.50 and below 0.90 on the side of the positive electrode active material layer that is not in contact with the positive electrode current collector layer, the tightness of the positive electrode stack and the solid electrolyte layer is ensured. Sulfide solid electrolyte is also covered on part of the surface, and its content and particle size are adjusted to optimize the contact effect.
This improves the adhesion between the positive electrode stack and the solid electrolyte layer, while reducing resistance and enhancing the charge and discharge performance of the solid-state battery.
Smart Images

Figure CN123162175A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a positive electrode stack, a solid-state battery, and a method for manufacturing a solid-state battery. Background Technology
[0002] Solid-state batteries are secondary batteries that use a solid electrolyte as the electrolyte. Compared with liquid batteries that use only a liquid electrolyte, they have higher performance in terms of charging performance and other aspects, and therefore have attracted attention. Solid-state batteries are usually composed of a positive electrode stack, a solid electrolyte layer, and a negative electrode stack stacked sequentially. Various stacking methods for improving quality have been disclosed.
[0003] Patent Document 1 discloses a method for manufacturing a battery, comprising: a step of pressing a layer of positive and negative electrode layers with a smaller area of the surface orthogonal to the stacking direction under a first pressing pressure; a step of pressing another layer of positive and negative electrode layers with a larger area of the surface orthogonal to the stacking direction under a second pressing pressure; a step of disposing an electrolyte layer on the surface of the other layer and disposing the electrolyte layer between the first and second layers in an electrolyte arrangement step; and a final pressing step of pressing the positive electrode layer, the electrolyte layer, and the negative electrode layer under a third pressing pressure lower than the second pressing pressure. According to the disclosure of Patent Document 1, a method for manufacturing a battery in which crack formation is suppressed can be provided.
[0004] Existing technical documents
[0005] Patent documents
[0006] Patent Document 1: Japanese Patent Application Publication No. 2014-207104 Summary of the Invention
[0007] The problem that the invention aims to solve
[0008] In the manufacturing process of solid-state batteries, when a solid electrolyte layer is stacked on the positive electrode stack, an adhesive layer is placed between the positive electrode stack and the solid electrolyte to improve adhesion and suppress lamination defects. However, since the adhesive layer does not participate in the charge-discharge reaction of the solid-state battery and thus becomes a resistor, it can adversely affect the charge-discharge performance of the solid-state battery.
[0009] Therefore, the object of the present invention is to provide a positive electrode stack with high adhesion to the solid electrolyte layer and low resistance.
[0010] Methods for solving problems
[0011] The present invention achieves the above objectives through the following means.
[0012] <Method 1>
[0013] A positive electrode stack comprising a positive electrode current collector layer on which a positive electrode active material layer is stacked, wherein the positive electrode active material layer comprises a nickel-containing positive electrode active material and a sulfide solid electrolyte, and when elemental analysis is performed on the surface of the side of the positive electrode active material layer not in contact with the positive electrode current collector layer using energy-dispersive X-ray spectroscopy with a scanning electron microscope, the mass ratio of sulfur atoms to nickel atoms (S / Ni) is 0.50 or more and 0.90 or less.
[0014] <Method 2>
[0015] According to the positive electrode stack of method 1, the mass ratio is 0.60 or more and 0.80 or less.
[0016] <Method 3>
[0017] According to method 1 or 2, the positive electrode stack is wherein the sulfide solid electrolyte is coated on a portion of the surface of the positive electrode active material.
[0018] Method 4
[0019] According to any one of methods 1 to 3, the positive electrode laminate contains nickel and cobalt.
[0020] Method 5
[0021] According to any one of the embodiments 1 to 4, the positive electrode laminate further comprises a binder, and the content of the binder relative to the positive electrode active material layer is 0.5% by mass or more and 1.0% by mass or less.
[0022] <Method 6>
[0023] A solid-state battery, comprising, in sequence, any one of embodiments 1 to 5, a positive electrode stack, a solid electrolyte layer, and a negative electrode stack.
[0024] <Method 7>
[0025] According to the solid-state battery of method 6, the solid electrolyte layer has a sulfide solid electrolyte.
[0026] Method 8
[0027] The method for manufacturing a solid-state battery according to method 6 or 7 includes: stacking the solid electrolyte layer on the positive electrode active material layer of the positive electrode laminate.
[0028] Invention Effects
[0029] According to the present invention, a positive electrode laminate with high adhesion to the solid electrolyte layer and low resistance can be provided. Attached Figure Description
[0030] Figure 1 This is a schematic diagram illustrating the positive electrode laminate of the present invention.
[0031] Figure 2 This is a schematic diagram illustrating the solid-state battery of the present invention. Detailed Implementation
[0032] The embodiments of the present invention will now be described in detail. It should be noted that the present invention is not limited to the following embodiments, and various modifications can be made within the scope of the present invention.
[0033] Positive electrode stack
[0034] A positive electrode stack comprising a positive electrode current collector layer on which a positive electrode active material layer is stacked, wherein the positive electrode active material layer comprises a nickel-containing positive electrode active material and a sulfide solid electrolyte, and when elemental analysis is performed on the surface of the positive electrode active material layer on the side not in contact with the positive electrode current collector layer using energy-dispersive X-ray spectroscopy with a scanning electron microscope, the mass ratio of sulfur atoms to nickel atoms (S / Ni) is 0.50 or more and 0.90 or less.
[0035] According to the present invention, a positive electrode laminate with high adhesion to the solid electrolyte layer and low resistance can be provided.
[0036] The inventors have studied ways to improve the adhesion between the positive electrode stack and the solid electrolyte layer. Furthermore, they discovered that by exposing more of the electrode active material on the surface of the positive electrode stack where the solid electrolyte layer will be deposited (the surface of the positive electrode active material layer that is not in contact with the positive electrode current collector layer), the adhesion between the positive electrode stack and the solid electrolyte layer is improved. While not limited by theory, this is believed to be because the electrode active material is hard and has an anchoring shape, thus facilitating its adhesion to the solid electrolyte layer. Additionally, this is believed to be because the electrode active material, especially nickel in the electrode active material, has a high affinity for the solid electrolyte, thus facilitating its adhesion to the solid electrolyte layer.
[0037] On the other hand, when a significant portion of the electrode active material is exposed on the aforementioned surface, it becomes impossible to adequately ensure the ion conduction path between the positive electrode active material layer and the solid electrolyte layer, leading to an increase in the resistance of the solid-state battery. In response, the inventors discovered that when the exposure of the electrode active material is within a specified range—specifically, when elemental analysis of the aforementioned surface using energy-dispersive X-ray spectroscopy with a scanning electron microscope reveals that the mass ratio of sulfur atoms to nickel atoms (S / Ni) is within a specified range—the adhesion between the positive electrode stack and the solid electrolyte layer can be improved, and the increase in the resistance of the solid-state battery can be suppressed.
[0038] Specifically, for example, such as Figure 1 As shown, the positive electrode stack 100 is formed by stacking a positive electrode active material layer 120 on a positive electrode current collector layer 110. Furthermore, the positive electrode active material layer 120 includes a nickel-containing positive electrode active material 121 and a sulfide solid electrolyte 122. Moreover, when elemental analysis was performed on the surface A of the positive electrode active material layer 120, which is not in contact with the positive electrode current collector layer, using energy-dispersive X-ray spectroscopy with a scanning electron microscope, the mass ratio of sulfur atoms to nickel atoms (S / Ni) was 0.50 or more and 0.90 or less.
[0039] The constituent elements of the present invention will be described below.
[0040] The positive electrode stack of the present invention is constructed by stacking a positive electrode active material layer on a positive electrode current collector layer.
[0041] Regarding the positive electrode stack of the present invention, when performing elemental analysis on the surface of the side of the positive electrode active material layer not in contact with the positive electrode current collector layer using energy-dispersive X-ray spectroscopy (EDS) with a scanning electron microscope (SEM), the mass ratio of sulfur atoms to nickel atoms (S / Ni) is 0.50 or more and 0.90 or less. The aforementioned mass ratio can be 0.55 or more, 0.60 or more, 0.65 or more, or 0.70 or more, or it can be 0.85 or less, 0.80 or less, 0.75 or less, or 0.70 or less.
[0042] Here, the SEM observation magnification was 500x. Additionally, EDS was used to perform cross-sectional machining of the analyte using ion milling, and measurements were taken at an accelerating voltage of 0.5 kV and in mapping mode. It should be noted that a relatively high probe current was set to improve detection sensitivity.
[0043] The mass ratio of sulfur atoms to nickel atoms (S / Ni) can be adjusted by the content of positive electrode active material and solid electrolyte relative to the positive electrode active material layer, the particle size of positive electrode active material and solid electrolyte, and the coating of sulfide solid electrolyte on at least a portion of the surface of positive electrode active material.
[0044] <Positive Electrode Active Material Layer>
[0045] The positive electrode active material layer contains a nickel-containing positive electrode active material and a sulfide solid electrolyte. The positive electrode active material layer may also optionally contain a binder and conductive additives. The positive electrode active material layer may contain various other additives.
[0046] There is no particular limitation on the content of the positive electrode active material. For example, the content relative to the positive electrode active material layer can be more than 40% by mass, more than 50% by mass, more than 60% by mass, or less than 100% by mass or less than 90% by mass.
[0047] There is no particular limitation on the content of sulfide solid electrolyte. For example, the content relative to the positive electrode active material layer can be more than 1% by mass, more than 5% by mass, more than 10% by mass, more than 15% by mass, or more than 20% by mass, or it can be less than 90% by mass, less than 80% by mass, less than 70% by mass, less than 60% by mass, or less than 50% by mass.
[0048] There is no particular limitation on the content of the binder. For example, its content relative to the positive electrode active material layer can be 0.5% by mass or more, 0.6% by mass or more, or 0.7% by mass or less, or less than 1.0% by mass, 0.9% by mass or less, or less than 0.8% by mass. When the binder content is high, the adhesion between the positive electrode stack and the positive electrode current collector layer is improved, but the resistance of the solid-state battery increases.
[0049] There is no particular limitation on the content of conductive additives. For example, the content relative to the positive electrode active material layer can be more than 0.5% by mass, more than 1.0% by mass, more than 3.0% by mass, or more than 5.0% by mass, or less than 20.0% by mass, less than 15.0% by mass, or less than 10.0% by mass.
[0050] The shape of the positive electrode active material layer is not particularly limited; for example, it can be a sheet with a generally planar shape. The thickness of the positive electrode active material layer is not particularly limited; for example, it can be 0.1 μm or more, 1 μm or more, or 10 μm or more, or it can be less than 2 mm, less than 1 mm, or less than 500 μm.
[0051] (Positive electrode active material)
[0052] The positive electrode active material contains nickel. It may also optionally contain cobalt, manganese, or aluminum. The positive electrode active material absorbs and releases lithium ions. Examples of positive electrode active materials include lithium nickel oxide (LiNiO2) and lithium nickel cobalt manganese oxide (NCM:LiCo). 1 / 3 Ni 1 / 3 Mn 1 / 3 O2), lithium nickel cobalt aluminum oxide (LiNi) 0.8 (CoAl) 0.2O2), etc., but not limited to these.
[0053] A portion of the surface of the positive electrode active material can be coated with a sulfide solid electrolyte. Specifically, for example, such as... Figure 1 As shown, a sulfide solid electrolyte coating 121-1 is coated on a portion of the surface of the positive electrode active material 121. The mass ratio (S / Ni) of sulfur atoms to nickel atoms on the side of the positive electrode active material layer that is not in contact with the positive electrode current collector layer can be easily adjusted depending on the amount of sulfide solid electrolyte coating. For information on sulfide electrolytes, please refer to the relevant description of sulfide electrolytes described later.
[0054] There are no particular limitations on the coating method for sulfide solid electrolytes. For example, it can be a method of mixing and processing the positive electrode active material with the sulfide solid electrolyte using a balance granulator. The rotation speed of the balance granulator is not particularly limited; for example, it can be 2000 minutes per second. -1 Above, 2500 minutes -1 Above, 3000 minutes -1 The above can also be 5000 minutes. -1 Below or 4000 minutes -1 The processing time is not specifically limited and can be more than 5 minutes, more than 6 minutes, more than 7 minutes, more than 8 minutes, more than 9 minutes, or more than 10 minutes, or less than 30 minutes, less than 25 minutes, less than 20 minutes, or less than 15 minutes.
[0055] The positive electrode active material can be coated with a material other than a sulfide solid electrolyte. This material can be one that possesses lithium-ion conductivity, low reactivity with the positive electrode active material or solid electrolyte, and maintains its coating morphology without flowing even when in contact with the active material or solid electrolyte. Specific examples of such materials include LiNbO3 and Li4Ti5O4. 12 Examples include Li3PO4, but it is not limited to these.
[0056] The shape of the positive electrode active material is not particularly limited as long as it is a typical shape used for positive electrode active materials in batteries. For example, the positive electrode active material can be in particle form. It can be primary particles or secondary particles formed by the aggregation of multiple primary particles. The particle size of the positive electrode active material can be, for example, greater than 1 nm, greater than 5 nm, or greater than 10 nm, and can be less than 500 μm, less than 100 μm, less than 50 μm, or less than 30 μm. It should be noted that the particle size of the positive electrode active material is the particle size (median diameter) at the 50% cumulative value of the particle size distribution on a volume basis determined by laser diffraction scattering method.
[0057] (Sulfide solid electrolyte)
[0058] The particle size of the sulfide solid electrolyte is not particularly limited; for example, it can be greater than 1 nm, greater than 5 nm, or greater than 10 nm, and it can be less than 500 μm, less than 100 μm, less than 50 μm, or less than 30 μm. Here, the particle size of the sulfide solid electrolyte is the particle size (median diameter) that accounts for 50% of the cumulative value of the particle size distribution on a volume basis determined by laser diffraction scattering method.
[0059] Examples of sulfide solid electrolytes include amorphous sulfide solid electrolytes, crystalline sulfide solid electrolytes, and sulfide-silver-germanium ore type solid electrolytes, but are not limited to these. Specific examples of sulfide solid electrolytes include the Li₂S-P₂S₅ system (Li₇P₃S₅). 11 , Li3PS4, Li8P2S9, etc.), Li2S-SiS2, LiI-Li2S-SiS2, LiI-Li2S-P2S5, LiI-LiBr-Li2S-P2S5, Li2S-P2S5-GeS2 (Li 13 GeP3S 16 Li 10 GeP2S 12 etc.), LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, Li 7-x PS 6-x Cl x etc., or combinations thereof, but not limited to these.
[0060] Sulfide solid electrolytes can be glass or crystallized glass (glass ceramic).
[0061] (Adhesive)
[0062] There are no particular limitations on the material of the adhesive. Adhesives can be, for example, polyvinylidene fluoride (PVdF), butadiene rubber (BR), polytetrafluoroethylene (PTFE), styrene-butadiene rubber (SBR), etc., but are not limited to these. There are no particular limitations on the adhesive; a single type can be used, or two or more types can be used in combination.
[0063] (Conductive additive)
[0064] There are no particular limitations on the conductive additives. Examples of conductive additives include vapor-grown carbon fiber (VGCF), acetylene black (AB), Ketjen black (KB), carbon nanotubes (CNT), and carbon nanofibers (CNF), but these are not limited to these. Conductive additives can be in particulate or fibrous form, and their size is not particularly limited. There are no particular limitations on the use of conductive additives; a single additive may be used, or two or more additives may be used in combination.
[0065] Positive current collector layer
[0066] The material used for the positive electrode current collector layer is not particularly limited, and materials commonly used as positive electrode current collectors in solid-state batteries can be appropriately used. Examples of materials for the positive electrode current collector layer include Cu, Ni, Cr, Au, Pt, Ag, Al, Fe, Ti, Zn, Co, and stainless steel, but are not limited to these. Furthermore, the positive electrode current collector layer may have a coating on its surface for purposes such as adjusting resistance. Additionally, the positive electrode current collector layer can be formed by depositing or vapor-depositing the aforementioned metals onto a metal foil or substrate.
[0067] The shape of the positive current collector layer is not particularly limited; for example, it can be foil-shaped, plate-shaped, or mesh-shaped. Foil-shaped is preferred. The thickness of the positive current collector layer is not particularly limited; it can be 0.1 μm or more, 1 μm or more, less than 1 mm, or less than 100 μm.
[0068] The positive electrode laminate can be manufactured using known methods. For example, it can be manufactured by forming a composite material containing a layer of positive electrode active material onto the positive electrode current collector layer in a dry or wet manner.
[0069] Solid-state batteries
[0070] The solid-state battery of the present invention comprises, in sequence, the positive electrode stack, the solid electrolyte layer, and the negative electrode stack.
[0071] According to the present invention, a solid-state battery with high adhesion between the positive electrode stack and the solid electrolyte layer and low resistance can be provided.
[0072] Specifically, for example, such as Figure 2 As shown, in the solid-state battery 200, a positive electrode stack 100, a solid electrolyte layer 210, and a negative electrode stack 220 are sequentially stacked. Furthermore, the negative electrode stack 220 is constructed by stacking a negative electrode active material layer 222 on a negative electrode current collector layer 221.
[0073] The solid-state battery of the present invention comprises, in sequence, the positive electrode stack, the solid electrolyte layer, and the negative electrode stack. The solid-state battery may optionally also include a liquid electrolyte. Regarding the positive electrode stack, please refer to the relevant description of the positive electrode stack described above.
[0074] In this invention, a "solid-state battery" refers to a battery that uses at least a solid electrolyte as the electrolyte. Therefore, a solid-state battery can also use a combination of solid and liquid electrolytes as electrolytes. Furthermore, in this invention, a "solid-state battery" can also be an all-solid-state battery, that is, a battery that uses only a solid electrolyte as the electrolyte.
[0075] <Solid Electrolyte Layer>
[0076] The solid electrolyte layer contains at least a solid electrolyte and may optionally contain a binder. The solid electrolyte layer may also contain various other additives. For information on binders, please refer to the relevant description of the positive electrode laminate described above.
[0077] There are no particular limitations on the solid electrolyte; it can be a sulfide solid electrolyte. Alternatively, the solid electrolyte can be, for example, an oxide solid electrolyte or polymer electrolyte particles.
[0078] Examples of oxide solid electrolytes include Li7La3Zr2O. 12 Li 7-x La3Zr 1-x Nb x O 12 Li 7- 3x La3Zr2Al x O 12 Li 3x La 2 / 3-x TiO3, Li 1+x Al x Ti 2-x (PO4)3, Li 1+x Al x Ge 2-x (PO4)3, Li3PO4 or Li 3+x PO 4-x N x (LiPON) and other combinations thereof, but not limited to these.
[0079] Oxide solid electrolytes can be glass or crystallized glass (glass ceramic).
[0080] Examples of polymer electrolyte particles include polyethylene oxide (PEO), polypropylene oxide (PPO), and their copolymers, but are not limited to these.
[0081] Solid electrolyte layers can be manufactured using known methods. For example, they can be manufactured by forming a composite material containing a solid electrolyte layer onto a substrate using a dry or wet method.
[0082] <Negative electrode stack>
[0083] The negative electrode stack can have a negative electrode active material layer and a negative electrode current collector layer.
[0084] (Negative electrode active material layer)
[0085] The negative electrode active material layer comprises at least a negative electrode active material and a solid electrolyte, and may optionally include a binder and conductive additives. The negative electrode active material layer may also contain various other additives. For information on the solid electrolyte, please refer to the relevant description of the solid electrolyte layer described above; for information on binders and conductive additives, please refer to the relevant description of the positive electrode laminate described above.
[0086] The content of each of the negative electrode active material, solid electrolyte, and conductive additive in the negative electrode active material layer can be appropriately determined according to the target battery performance. For example, when the total solid content of the negative electrode active material layer is set to 100% by mass, the content of the negative electrode active material can be above 40%, above 50%, or above 60% by mass, or below 100% by mass or below 90% by mass.
[0087] The shape of the negative electrode active material layer is not particularly limited; for example, it can be a sheet with a generally planar shape. The thickness of the negative electrode active material layer is not particularly limited; for example, it can be 0.1 μm or more, 1 μm or more, or 10 μm or more, or it can be less than 2 mm, less than 1 mm, or less than 500 μm.
[0088] As the negative electrode active material, various materials whose charge / discharge potential for absorbing and releasing lithium ions is lower than that of the positive electrode active material of the present invention can be used. The material of the negative electrode active material is not particularly limited; it can be metallic lithium or a material capable of absorbing and releasing metal ions such as lithium ions. Examples of materials capable of absorbing and releasing metal ions such as lithium ions include alloy-based negative electrode active materials, carbon materials, or lithium titanate (Li4Ti5O). 12 (etc.), but not limited to these.
[0089] As an alloy-based anode active material, there are no particular limitations; for example, Si alloy-based anode active materials or Sn alloy-based anode active materials can be listed. Si alloy-based anode active materials include silicon, silicon oxides, silicon carbides, silicon nitrides, or their solid solutions. Furthermore, Si alloy-based anode active materials can contain metallic elements other than silicon, such as Fe, Co, Sb, Bi, Pb, Ni, Cu, Zn, Ge, In, Sn, and Ti. Sn alloy-based anode active materials include tin, tin oxides, tin nitrides, or their solid solutions. Furthermore, Sn alloy-based anode active materials can contain metallic elements other than tin, such as Fe, Co, Sb, Bi, Pb, Ni, Cu, Zn, Ge, In, Ti, and Si.
[0090] As a carbon material, there are no particular limitations; examples include hard carbon, soft carbon, and graphite.
[0091] There are no particular limitations on the shape of the negative electrode active material; any shape commonly used as a negative electrode active material in batteries is acceptable. For example, the negative electrode active material can be in particle or sheet form.
[0092] (Negative electrode current collector layer)
[0093] There are no particular limitations on the materials used for the negative electrode current collector layer; materials commonly used as negative electrode current collectors in solid-state batteries can be appropriately used. Examples of materials for the negative electrode current collector layer include Cu, Ni, Cr, Au, Pt, Ag, Al, Fe, Ti, Zn, Co, stainless steel, or carbon sheets, but these are not limited to. The negative electrode current collector layer may have a coating on its surface for purposes such as adjusting resistance.
[0094] The shape of the negative electrode current collector layer is not particularly limited; for example, it can be foil-shaped, plate-shaped, or mesh-shaped. Foil-shaped is preferred. The thickness of the negative electrode current collector layer is not particularly limited; it can be 0.1 μm or more, 1 μm or more, or less than 1 mm or less than 100 μm.
[0095] The negative electrode laminate can be manufactured using known methods. For example, it can be manufactured by forming a composite material containing a negative electrode active material layer onto the negative electrode current collector layer in a dry or wet manner.
[0096] <Liquid Electrolytes>
[0097] There are no particular limitations on the liquid electrolyte, but it is preferred to contain a supporting salt and a solvent.
[0098] Lithium salts, which serve as supporting salts for electrolytes with lithium-ion conductivity, are not particularly limited and can include inorganic and organic lithium salts. Examples of inorganic lithium salts include LiPF6, LiBF4, LiClO4, and LiAsF6, but are not limited to these. Examples of organic lithium salts include LiCF3SO3, LiN(CF3SO2)2, LiN(C2F5SO2)2, LiN(FSO2)2, and LiC(CF3SO2)3, but are not limited to these.
[0099] There are no particular limitations on the solvent used as the electrolyte, and examples include cyclic carbonates and chain carbonates. Examples of cyclic carbonates include ethylene carbonate (EC), propylene carbonate (PC), and butyl carbonate (BC), but these are not limited to these. Examples of chain carbonates include dimethyl carbonate (DMC), diethyl carbonate (DEC), and methyl ethyl carbonate (EMC), but these are not limited to these. There are no particular limitations on the electrolyte; a single type can be used, or two or more types can be used in combination.
[0100] Manufacturing Methods of Solid-State Batteries
[0101] The method for manufacturing a solid-state battery according to the present invention includes: stacking a solid electrolyte layer on a positive electrode active material layer of a positive electrode laminate.
[0102] According to the present invention, a method for manufacturing a solid-state battery with high adhesion between the positive electrode stack and the solid electrolyte layer and low resistance can be provided.
[0103] The method for manufacturing a solid-state battery according to the present invention includes: stacking a solid electrolyte layer on a positive electrode active material layer of a positive electrode laminate. For information regarding solid-state batteries and solid electrolyte layers, please refer to the relevant descriptions of solid-state batteries described above; for information regarding positive electrode laminates and positive electrode active material layers, please refer to the relevant descriptions of positive electrode laminates described above.
[0104] There is no particular limitation on the method of laminating the solid electrolyte layer. For example, it can be transfer printing, pressing, or slurry coating. From the point of view of improving the adhesion between the positive electrode laminate and the solid electrolyte layer, transfer printing is particularly preferred.
[0105] Transfer printing can be performed using a roller press. There are no particular limitations on the pressing pressure; for example, it can be above 0.5 t / cm, above 1.0 t / cm, above 1.5 t / cm, or above 2.0 t / cm, or below 5.0 t / cm, below 4.0 t / cm, or below 3.0 t / cm. Similarly, there are no particular limitations on the pressing temperature; for example, it can be above 50℃, above 60℃, above 70℃, or above 80℃, or below 150℃, below 120℃, or below 100℃.
[0106] The method for manufacturing a solid-state battery according to the present invention may include: stacking a negative electrode stack on the surface of the side of the solid electrolyte layer that is not stacked as a positive electrode stack.
[0107] The method of stacking the negative electrode stack is not particularly limited. For example, it can be a method of stacking the negative electrode stack on the surface of the unstacked positive electrode stack of the solid electrolyte layer and then pressing it. The pressing pressure is not particularly limited; for example, it can be 1 t / cm. 2 Above, 2t / cm 2 Above, 3t / cm 2 Above or 5t / cm 2 The above can also be 20t / cm 2 Below, 15t / cm 2 Below or 10t / cm 2 the following.
[0108] Other processes used in the manufacture of solid-state batteries can be carried out by applying well-known methods.
[0109] Example
[0110] The invention has been specifically described through examples and comparative examples, but the invention is not limited thereto.
[0111] Solid-state battery manufacturing
[0112] <Positive electrode stack>
[0113] LiNi, a precursor for the positive electrode active material, is fed into a balanced granulator (manufactured by Freund Corporation). x Co y Al z 500g of O2 (NCA) and 45g of Li2S-P2S5 glass-ceramic containing LiI (D50=0.8μm) as a sulfide solid electrolyte were treated for 3000 minutes as shown in Table 1. -1 The mixture was mixed and a sulfide solid electrolyte was coated on a portion of the surface of the positive electrode active material precursor, which served as the positive electrode active material for Examples 1-4 and Comparative Examples 1-4.
[0114] Next, the positive electrode active materials of Examples 1-4 and Comparative Examples 1-4, and the Li2S-P2S5 glass-ceramic (D50 = 0.8 μm) containing LiI as the solid electrolyte were weighed, so that the volume ratio of positive electrode active material to solid electrolyte was 75:25. Then, these materials, along with carbon nanotubes (CNTs) as a conductive additive, styrene-butadiene rubber as a binder, and tetrahydronaphthalene as a solvent, were added to a FILMIX apparatus (30-L, Primix) and mixed at 25 m / s for 20 minutes to prepare a positive electrode composite slurry. The positive electrode composite slurry was then coated onto an aluminum foil serving as the positive electrode current collector layer and dried at 100°C for 30 minutes. Afterward, it was cut into 1 cm pieces. 2 The positive electrode laminates of Examples 1-4 and Comparative Examples 1-4 were prepared by pressing them at 175°C with a pressing pressure of 5 t / cm. It should be noted that the binder content (mass ratio relative to the electrode active material layer) of the positive electrode active material layer is shown in Table 1.
[0115] Here, for the positive electrode stacks of Examples 1-4 and Comparative Examples 1-4, elemental analysis was performed on the surface of the positive electrode active material layer on the side not in contact with the positive electrode current collector layer using scanning electron microscopy and energy-dispersive X-ray spectroscopy to determine the mass ratio of sulfur atoms to nickel atoms (S / Ni). The results are shown in Table 1. Here, S / Ni was determined by quantifying the mass of S and Ni and calculating their mass ratio using a scanning electron microscope (SU8030, manufactured by Hitachi Advanced Technology), an energy-dispersive X-ray spectroscopy apparatus, and its software at a magnification of 500x.
[0116] <Solid Electrolyte Layer>
[0117] A Li2S-P2S5-based glass-ceramic containing LiI (D50 = 0.8 μm) as a solid electrolyte, butadiene rubber as a binder, and tetrahydronaphthalene as a solvent were added to a FILMIX apparatus (30-L, made by Primix) and mixed at a peripheral speed of 20 m / s for 10 minutes to prepare a solid electrolyte slurry. The solid electrolyte slurry was then coated onto aluminum foil and dried at 100°C for 30 minutes to form a solid electrolyte layer.
[0118] <Negative electrode stack>
[0119] Li₂S-P₂S₅ glass-ceramic containing LiI (D₅₀ = 0.8 μm) as a solid electrolyte, vapor-grown carbon fiber (VGCF) as a conductive additive, butadiene rubber as a binder, and heptane as a solvent were added to the mixing vessel of the FILMIX apparatus (30-L, made by Primix). The mixture was stirred at 20,000 rpm for 30 minutes. Next, Li₄Ti₅O₅ was added as the negative electrode active material. 12 Particles (D50 = 1 μm) were added to a mixing container at a volume ratio of 70:30 to the solid electrolyte, and stirred at 15,000 rpm for 60 minutes to prepare the negative electrode slurry. The prepared negative electrode slurry was coated onto copper foil, which served as the negative electrode current collector layer, and dried at 100°C for 30 minutes. Afterward, it was cut into 1 cm pieces. 2 The size of the negative electrode stack is thus obtained.
[0120] <Layering of positive electrode stack, solid electrolyte layer and negative electrode stack>
[0121] The surface of the electrode active material layer of the positive electrode laminate of Examples 1-4 and Comparative Examples 1-4 was bonded to the surface of the solid electrolyte layer. After passing through a roller press at 90°C and a pressing pressure of 2t / cm, the aluminum foil on the solid electrolyte layer side was peeled off, thereby transferring the solid electrolyte layer onto the surface of the electrode active material layer.
[0122] Then, on the surface of the un-laminated positive electrode stack of the solid electrolyte layer, the surface of the negative electrode active material layer of the negative electrode stack is laminated, and at room temperature at 6 tons / cm² 2 Press for 1 minute. Finally, place a stainless steel rod into the positive electrode stack and the negative electrode stack, and constrain with 1 ton to obtain solid-state batteries of Examples 1-4 and Comparative Examples 1-4.
[0123] "evaluate"
[0124] <Evaluation of Fit>
[0125] For the positive electrode stacks of Examples 1-4 and Comparative Examples 1-4, photographs of the transfer surface were taken during the stage of transferring the solid electrolyte layer to the surface of the electrode active material layer. The area of the transferred solid electrolyte layer and the area of the transfer surface were measured using image analysis software (ImageJ, manufactured by the National Institutes of Health). Then, the transfer rate was calculated by the formula: transfer rate = [area of transferred solid electrolyte] / [area of transfer surface]. The results are shown in Table 1.
[0126] <Evaluation of Resistance>
[0127] For the solid-state batteries of Examples 1-4 and Comparative Examples 1-4, two cycles of constant current-constant voltage charging and discharging were performed at a set voltage of 2.8V or 1.5V and a 1 / 3C rate, and then the SOC was adjusted to 40% at a 1 / 3C rate. The batteries were discharged in a constant temperature bath at 25°C with a DC current equivalent to a 2.5C rate, and the resistance value was calculated from the voltage drop after 5 seconds relative to 0 seconds and the applied current.
[0128] [Table 1]
[0129] According to Examples 1-4 and Comparative Examples 1-4, when the mass ratio of sulfur atoms to nickel atoms (S / Ni) on the surface of the positive electrode active material layer that is not in contact with the positive electrode current collector layer is lower than a specified value, the transfer rate between the positive electrode stack and the solid electrolyte layer is high, and the adhesion between the positive electrode stack and the solid electrolyte layer is high.
[0130] Furthermore, based on Examples 1, 2, and 4, and Comparative Examples 1, 3, and 4, it can be understood that when the S / Ni ratio is higher than the specified value, the resistance of the solid-state battery is low. Therefore, it can be understood that when the S / Ni ratio is within the specified range, the adhesion between the positive electrode stack and the solid electrolyte layer is high and the resistance is low.
[0131] Symbol Explanation
[0132] 100 Positive Electrode Stack
[0133] 110 Positive current collector layer
[0134] 120 Positive Electrode Active Material Layer
[0135] 121 Positive Electrode Active Material
[0136] 121-1 Sulfide solid electrolyte coating
[0137] 122 Sulfide solid electrolyte
[0138] 200 solid-state battery
[0139] 210 Solid electrolyte layer
[0140] 220 Negative Electrode Laminate
[0141] 221 Negative current collector layer
[0142] 222 Negative Electrode Active Material Layer
Claims
1. A positive electrode laminate, wherein a positive electrode active material layer is laminated on a positive electrode current collector layer, wherein, The positive electrode active material layer contains a nickel-containing positive electrode active material and a sulfide solid electrolyte, and When elemental analysis of the surface of the positive electrode active material layer that is not in contact with the positive electrode current collector layer is performed using energy-dispersive X-ray spectroscopy with a scanning electron microscope, the mass ratio of sulfur atoms to nickel atoms (S / Ni) is greater than 0.50 and less than 0.
90.
2. The positive electrode laminate according to claim 1, wherein The mass ratio is 0.60 or higher and 0.80 or lower.
3. The positive electrode laminate according to claim 1 or 2, wherein The sulfide solid electrolyte is coated on a portion of the surface of the positive electrode active material.
4. The positive electrode laminate according to claim 1 or 2, wherein The positive electrode active material contains nickel and cobalt.
5. The positive electrode laminate according to claim 1 or 2, wherein, The positive electrode active material layer also has a binder, and The binder content is 0.5% by mass or more and 1.0% by mass or less relative to the positive electrode active material layer.
6. A solid-state battery, comprising, in sequence, the positive electrode stack, the solid electrolyte layer, and the negative electrode stack as described in claim 1 or 2.
7. The solid-state battery of claim 6, wherein, The solid electrolyte layer has a sulfide solid electrolyte.
8. The method of manufacturing a solid state battery of claim 7, comprising: The solid electrolyte layer is stacked on the positive electrode active material layer of the positive electrode laminate.
Citation Information
Patent Citations
Method of manufacturing battery
JP2014207104A