Positive electrode active material, positive electrode plate, and nonaqueous electrolyte secondary battery
Patent Information
- Application Number
- CN202610688854.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2025-05-23
- Filing Date
- 2026-05-19
- Publication Date
- 2026-11-24
Smart Images

Figure CN123162178A_ABST
Abstract
Description
Technical Field
[0001] This disclosure relates to positive electrode active materials, and further to positive electrode plates and non-aqueous electrolyte secondary batteries containing positive electrode active materials. Background Technology
[0002] Japanese Patent Application Publication No. 2024-160551 discloses a positive electrode active material that comprises secondary particles formed by the aggregation of primary particles, wherein the total content of nickel relative to the total content of metal elements other than lithium is 75 mol% or more and the aspect ratio is 1.9 or more. Summary of the Invention
[0003] Non-aqueous electrolyte secondary batteries using positive electrode plates containing a high percentage (e.g., 60 mol% or more) of nickel relative to the total content of metals other than lithium, tend to exhibit increased volume expansion and contraction of the positive electrode active material during charge and discharge. Therefore, repeated charge-discharge cycles can sometimes lead to cracks forming within the positive electrode active material particles, resulting in rapid degradation.
[0004] The purpose of this disclosure is to provide a positive electrode active material with a nickel content of 60 mol% or more and improved charge-discharge cycle characteristics, a positive electrode plate containing the positive electrode active material, and a non-aqueous electrolyte secondary battery.
[0005] [1] A positive electrode active material, comprising a first active material
[0006] The aforementioned first active substance comprises secondary particles formed by the aggregation of multiple primary particles.
[0007] The first active material is the lithium transition metal composite oxide represented by formula (1).
[0008] Li a Ni x Co y Mn z M (1-x-y-z) O2 (1)
[0009] [In equation (1), x, y, z, and a satisfy 0.6≤x≤1.0, 0≤y≤0.3, 0≤z≤0.3, and 0.90≤a / (x+y+z)≤1.25,]
[0010] M is one or more elements selected from Mg, Ca, Al, Ti, V, Cr, Zr, Nb, Mo, Hf, Ta, and W.
[0011] The ratio of the number of boundaries in the aforementioned secondary particles where the crystal orientation difference between adjacent primary particles is 60° or more to the number of the aforementioned primary particles in the aforementioned secondary particles is 0.5 or less.
[0012] The aforementioned secondary particles have a coating layer containing a boron compound on the surface of the aforementioned primary particles and at the interface between adjacent primary particles.
[0013] [2] According to the positive electrode active material described in [1], the porosity of the above-mentioned secondary particles is 2 to 8%.
[0014] [3] The positive electrode active material according to [1] or [2], wherein the coating layer comprises LiBO2.
[0015] [4] The positive electrode active material according to any one of [1] to [3], wherein the coating layer further comprises Al2O3.
[0016] [5] The positive electrode active material according to any one of [1] to [4], wherein in the above formula (1), x satisfies 0.7≤x≤1.0.
[0017] [6] The positive electrode active material according to any one of [1] to [4], wherein in the above formula (1), x satisfies 0.9≤x≤1.0.
[0018] [7] The positive electrode active material according to any one of [1] to [6], wherein in the above formula (1), x, y, z and a satisfy 1.06≤a / (x+y+z)≤1.25.
[0019] [8] The positive electrode active material according to any one of [1] to [6], wherein in the above formula (1), x, y, z and a satisfy 1.06≤a / (x+y+z)≤1.15.
[0020] [9] The positive electrode active material according to any one of [1] to [8], wherein the number of the primary particles in the secondary particles is 10 or more.
[0021]
[10] The positive electrode active material according to any one of [1] to [9], wherein the first active material comprises a particle group consisting of a plurality of the above-mentioned secondary particles.
[0022]
[11] The positive electrode active material according to any one of [1] to
[10] , wherein the aspect ratio of the primary particles is 1.9 or more.
[0023]
[12] The positive electrode active material according to any one of [1] to
[11] , wherein the average particle size of the primary particles is 0.1 to 2.5 μm.
[0024]
[13] The positive electrode active material according to any one of [1] to
[12] , wherein the average particle size D50 of the first active material is 2 to 50 μm.
[0025]
[14] A positive electrode plate having a positive electrode active material layer comprising any one of [1] to
[13] .
[0026]
[15] A non-aqueous electrolyte secondary battery comprising the positive electrode plate described in
[14] .
[0027] The foregoing and other objects, features, aspects and advantages of the present invention will become clear from the following detailed description relating to the invention, which is understood in conjunction with the accompanying drawings. Attached Figure Description
[0028] Figure 1 This is a schematic diagram of the appearance of a secondary particle.
[0029] Figure 2 It is a schematic cross-sectional view of a secondary particle.
[0030] Figure 3 It is a graph showing the volume change of a non-aqueous electrolyte secondary battery before and after charging.
[0031] Figure 4 It is a schematic cross-sectional view of multiple primary particles used to illustrate the boundary between adjacent primary particles.
[0032] Figure 5 This is an IPF diagram showing the crystal orientation of primary particles in a cross-section of secondary particles.
[0033] Figure 6 This is a diagram representing the IPF (Integrated Photon Fold) plot used to illustrate the analysis of crystal orientation difference lines.
[0034] Figure 7 It is a graph that shows the crystal orientation difference obtained by plotting the part overlapping the IPF diagram.
[0035] Figure 8 This is a simplified flowchart of the manufacturing process of the positive electrode active material.
[0036] Figure 9 This is a schematic cross-sectional view of the positive electrode plate.
[0037] Figure 10 This is a schematic cross-sectional view representing an example of a non-aqueous electrolyte secondary battery.
[0038] Figure 11 This is a schematic diagram showing an example of an electrode. Detailed Implementation
[0039] <Positive Electrode Active Material>
[0040] The positive electrode active material disclosed herein is a positive electrode active material for use in the positive electrode plate of a non-aqueous electrolyte secondary battery. The non-aqueous electrolyte secondary battery can be, for example, a lithium-ion secondary battery.
[0041] The positive electrode active material includes a first active material. The first active material is a substance capable of reversibly adsorbing and releasing charge carriers. The first active material is a lithium transition metal composite oxide.
[0042] The lithium transition metal complex oxide has a layered structure and contains lithium (Li) and nickel (Ni). For lithium transition metal complex oxides, the ratio of the total moles of Ni to the total moles of metal elements other than Li (hereinafter also referred to as Ni content) is 60 mol% or more.
[0043] In lithium transition metal composite oxides, from the viewpoint of high volumetric energy density in non-aqueous electrolyte secondary batteries, the Ni content is preferably 70 mol% or more, more preferably 80 mol% or more, and even more preferably 90 mol% or more. On the other hand, from the viewpoint of high stability, the Ni content is preferably 95 mol% or less.
[0044] Examples of lithium transition metal composite oxides include lithium-nickel-manganese composite oxides, lithium-nickel-cobalt-manganese composite oxides, lithium-nickel-cobalt-aluminum composite oxides, and lithium-iron-nickel-manganese composite oxides. They can be used individually or in combination of two or more. The layered structure (i.e., layered crystal structure) of the particles in lithium transition metal composite oxides can be confirmed by methods such as X-ray diffraction.
[0045] The lithium transition metal composite oxide has the composition represented by formula (1).
[0046] Li a Ni x Co y Mn z M (1-x-y-z) O2 (1)
[0047] [In equation (1), x, y, z, and a satisfy 0.6≤x≤1.0, 0≤y≤0.3, 0≤z≤0.3, and 0.90≤a / (x+y+z)≤1.25,]
[0048] M is one or more elements selected from Mg, Ca, Al, Ti, V, Cr, Zr, Nb, Mo, Hf, Ta, and W.
[0049] In equation (1), from the viewpoint of energy density and charge-discharge cycle characteristics, x preferably satisfies 0.7≤x≤1.0, more preferably 0.8≤x≤1.0, and even more preferably 0.9≤x≤1.0. From the viewpoint of charge-discharge cycle characteristics, y preferably satisfies 0.05≤y≤0.25, more preferably 0.1≤y≤0.25, and even more preferably 0.1≤y≤0.2. From the viewpoint of charge-discharge cycle characteristics, z preferably satisfies 0.05≤z≤0.25, and even more preferably 0.1≤z≤0.2. x, y, and z preferably satisfy x+y+z=1. “x+y+z=1” includes not only x+y+z being 1, but also the case where it is substantially considered as 1 as long as the technical effect disclosed herein can be achieved. Typically, it can be x+y+z=0.95~1.1, and preferably x+y+z=0.99~1.05.
[0050] In equation (1), "a / (x+y+z)" corresponds to the ratio of the total molar number of lithium to the total molar number of Ni, Co, and Mn (hereinafter also referred to as the Li / Me ratio). When the Ni content in the lithium transition metal composite oxide is 70 mol% or more, there is a tendency for the thermal stability of the positive electrode active material to deteriorate easily. With a Li / Me ratio of 1.06 to 1.25, even when the Ni content is 70 mol% or more, there is a tendency for the crystal structure stability at high SOC and high temperature to be improved. As a result, it is easy to obtain a positive electrode active material with high thermal stability that suppresses oxygen desorption from the positive electrode active material. Therefore, x, y, z, and a preferably satisfy 1.06 ≤ a / (x+y+z) ≤ 1.25, and more preferably satisfy 1.06 ≤ a / (x+y+z) ≤ 1.15. It should be noted that when the positive electrode active material includes the coating layer described later and the coating layer contains a Li-containing compound, and when a Li-containing compound (e.g., LiOH, Li2CO3) is present on the surface of the positive electrode active material, the "a" representing the molar ratio of Li in formula (1) includes the molar ratio of Li in the coating layer and the Li-containing compound present on the surface of the positive electrode active material. Furthermore, when the positive electrode active material layer includes the coating layer described later and the coating layer contains a tungsten compound, the "1-x-y-z" representing the molar ratio of M in formula (1) includes the molar ratio of tungsten in the tungsten compound.
[0051] In some preferred embodiments, the lithium transition metal composite oxide preferably contains W in addition to the coating layer described later. In other words, the lithium transition metal composite oxide is preferably doped with W as an additive element. This stabilizes the layered structure of the lithium transition metal composite oxide, thus not only improving the initial resistance but also suppressing the dissolution of Mn into the non-aqueous electrolyte, resulting in better suppression of resistance increase during storage. When W is doped (solid-dissolved) as an additive element in the lithium transition metal composite oxide, the doping concentration is preferably 0.1 to 0.5 mol%, more preferably 0.1 to 0.3 mol%, relative to the total amount of transition metal elements in the lithium transition metal composite oxide excluding W.
[0052] The first active substance comprises secondary particles formed by the aggregation of multiple primary particles. Preferably, the first active substance comprises a particle group consisting of multiple secondary particles. When the first active substance comprises a particle group consisting of multiple secondary particles, the number of secondary particles in the particle group can be, for example, 2 or more, preferably 10 or more, more preferably 30 or more, and even more preferably 50 or more. There is no particular upper limit to the number of secondary particles in the particle group. Figure 1 and 2 As shown, a secondary particle can be a secondary particle 10 formed by the condensation of multiple primary particles 10p through physical or chemical binding forces. Figure 1 For convenience, all primary particles 10p are shown as spheres (circles), but the shape of primary particles 10p is not particularly limited. For example, it can be rod-shaped, plate-shaped, circular plate-shaped, ellipsoidal, cuboid-shaped, cubic, polyhedral, and combinations thereof. The cross-sectional shape of primary particles 10p can be, for example, a strip shape, or a circle, square, ellipse, polygon, line, and combinations thereof.
[0053] The number of primary particles 10p constituting the secondary particles 10 is 10 or more, preferably 30 or more, and more preferably 50 or more. The number of primary particles 10p is not particularly limited; for example, it can be less than 100,000, less than 60,000, less than 40,000, or less than 20,000. It should be noted that, in this specification, "primary particle" refers to the smallest unit of particles constituting the positive electrode active material, and is the smallest unit determined based on the geometric morphology observed under, for example, a scanning electron microscope (SEM).
[0054] In the first active material, the ratio of the number of boundaries in the secondary particles where the crystal orientation difference between adjacent primary particles is 60° or more to the number of primary particles in the secondary particles (hereinafter also referred to as the first ratio) is 0.50 or less. Figure 3This is a graph showing the volume change (c-axis length change) of non-aqueous electrolyte secondary batteries with a nickel content of 60 mol% or more and non-aqueous electrolyte secondary batteries with a nickel content of less than 60 mol% before and after charging. Figure 3 As shown, if the nickel content is 60 mol% or higher, the volume after charging tends to decrease compared to the state before charging, and sometimes the load caused by the expansion and contraction of the positive electrode active material particles during charging and discharging increases. However, contrary to the expectation that a higher orientation of the crystal orientation of the primary particles would result in higher stress within the particles, it was unexpectedly found that even when the nickel content of the first active material is 60 mol% or higher, the direction of the expansion and contraction of the positive electrode active material during charging and discharging is easily controlled. As a result, the stress applied to the secondary particles is easily reduced in the evaluation of charge-discharge cycle characteristics, and particle breakage is easily suppressed. This is consistent with the result that, in the simulation of stress generated in secondary particles due to the expansion and contraction of the primary particles, secondary particles with controlled crystal orientation of the primary particles have a smaller stress load due to volume expansion and contraction compared to secondary particles without controlled crystal orientation of the primary particles. It should be noted that when the first active material contains multiple secondary particles, the first proportion is the average of the first proportions of the multiple secondary particles.
[0055] The crystal orientation difference between adjacent primary particles in a secondary particle refers to, for example, Figure 4 The diagram shows the angle α between the crystal orientations R1 and R2 of adjacent primary particles P1 and P2 in a secondary particle. Furthermore, the boundary where the crystal orientation difference between adjacent primary particles in a secondary particle is 60° or more refers to... Figure 4 The boundary B1 between the crystal orientation R1 of primary particle P1 and the crystal orientation R2 of primary particle P2, where the crystal orientation difference (angle α) is greater than 60°. On the other hand, in Figure 4 In the case of adjacent primary particles P1 and P3, the angle β between the crystal orientation R1 of primary particle P1 and the crystal orientation R3 of primary particle P3 is less than 60°. Therefore, the boundary B2 between primary particles P1 and P3 is not included in the boundary where the crystal orientation difference between adjacent primary particles in the secondary particle is 60° or more. Furthermore, in the case where primary particles in two or more secondary particles are adjacent to each other, even if the crystal orientation difference between these primary particles is 60° or more, it is not included in the boundary where the crystal orientation difference between adjacent primary particles in the secondary particle is 60° or more.
[0056] Specifically, the first proportion can be obtained through the following steps (1) to (4).
[0057] (1) In the cross section of the secondary particle, the inverse pole diagram (IPF) of the crystal orientation of the primary particle is determined by electron beam backscatter diffraction (EBSD).
[0058] (2) In the IPF diagram, select the cross-section of the secondary particles whose cross-sectional diameter is the same as or approximately the average particle size D50 of the first active material. Divide the cross-section of the secondary particles into 10 equal parts by crystal orientation difference line analysis to analyze the crystal orientation and number of primary particles on each line. The cross-sectional diameter of the secondary particles judged to be the same as or approximately the average particle size D50 of the first active material is preferably the average particle size D50 ± 1 μm of the first active material.
[0059] (3) Calculate the total number of boundaries between primary particles with a crystal orientation difference of 60° or more among adjacent primary particles on the 10 lines obtained by crystal orientation difference line analysis, Xs, and the total number of primary particles on the 10 lines, Ys.
[0060] (4) As the first proportion, the ratio Zs of Xs to Ys is obtained by dividing Xs by Ys. It should be noted that when the first active substance contains a group of particles consisting of multiple secondary particles, the ratio Zs of the multiple secondary particles can be obtained by following the steps (1) to (3) above, and the average value of the obtained ratio Zs is taken as the first proportion.
[0061] In step (1), the cross-section of the secondary particles can be fabricated from the powder of the first active material by cross-section polishing (CP). EBSD analysis can be performed using a scanning electron microscope-energy dispersive X-ray spectroscopy (SEM-EDS). IPF images, for example, can be fabricated from a 5000x magnified image of the cross-section of the secondary particles obtained from SEM-EDS. Figure 5This is an IPF (Integrated Photogrammetry) plot showing the crystal orientation of primary particles within a cross-section of secondary particles. In the IPF plot, crystal orientation is represented by color, and the boundaries where crystal orientations differ are displayed. EBSD analysis involves observing a cross-section near the center of secondary particles representing the first active material. From the viewpoint of improving the accuracy of the first proportion measurement, a cross-section in the IPF plot with a diameter of secondary particles that is the same as or approximately the average particle size D50 of the first active material is selected. The average particle size D50 of the first active material can be determined using a particle size distribution measuring device such as a laser diffraction-scattering type based on the powder state of the first active material before it is used to fabricate the positive electrode active material layer. Alternatively, the average particle size D50 of the first active material can also be determined by immersing the positive electrode plate in an NMP solution and then ultrasonically treating it, followed by measuring the particle size distribution of the collected first active material. When the positive electrode active material contains two or more active materials with different average particle sizes D50, particle size distribution measurement can be performed after grading the positive electrode active material. Alternatively, the surface of the positive electrode plate can be observed using SEM, and the particle size of the observed secondary particles can be calculated through image analysis. When the positive electrode active material contains two or more active materials with different average particle sizes (D50), it can be separated into particles with different average particle sizes (D50) for analysis by particle size filtering in image analysis.
[0062] In step (2), crystal orientation difference line analysis is performed on the IPF plot of the crystal orientation of the primary particles in the cross-section of the secondary particles obtained by EBSD analysis. For example... Figure 6 As shown, in the IPF diagram of the primary particles in the cross-section of the secondary particles obtained through EBSD analysis, the secondary particles are divided equally by 10 lines. The crystal orientation difference analysis is performed on each line to analyze the crystal orientation and number of primary particles. The 10 lines are parallel to each other, and the direction of the lines is not particularly limited and can be arbitrary. Considering the average particle size of the primary particles and the average particle size D50 of the secondary particles in the first positive electrode active material, from the viewpoint of the accuracy of the first ratio measurement, dividing the secondary particles into 11 equal parts by 10 lines and performing orientation difference line analysis is considered advantageous.
[0063] In step (3), based on the orientation difference line analysis results, in the IPF diagram of the crystal orientation of the primary particles in the cross section of the secondary particles obtained by EBSD analysis, the total number of boundaries between primary particles with a crystal orientation difference of 60° or more in adjacent primary particles on the 10 lines that divide the secondary particles into 11 equal parts is calculated, along with the total number of primary particles on the 10 lines, Ys. By setting the crystal orientation difference to 60° or more, differences are easily observed in the evaluation of charge-discharge cycle characteristics. Figure 7It is a graph obtained by plotting the crystal orientation difference on a line on the IPF diagram and overlaying it onto a portion of the corresponding IPF diagram.
[0064] In step (4), the ratio Zs of Xs to Ys is obtained by dividing Xs by Ys, and is taken as the first ratio. In steps (1) to (3) above, EBSD analysis is performed on the cross-section of the secondary particles whose cross-sectional diameter is equal to the average particle size D50 of the first active material. The cross-section of the secondary particles is divided into 11 equal parts by 10 lines. The number of primary particles on the 10 lines and the number of boundaries on the 10 lines where the crystal orientation difference between adjacent primary particles is 60° or more are obtained. Therefore, the ratio Zs is a value equivalent to the first ratio. The first ratio is the ratio of the number of boundaries where the crystal orientation difference between adjacent primary particles is 60° or more in the entire secondary particles to the number of primary particles in the entire secondary particles. The ratio Zs can be regarded as the first ratio. In addition, when the first active material contains a particle group composed of multiple secondary particles, the ratio Zs of multiple secondary particles can be obtained by following steps (1) to (3) above, and the average value of the ratio Zs of multiple secondary particles is taken as the first ratio. The first ratio is preferably the average value of the ratio Zs of 10 or more, and more preferably the average value of the ratio Zs of 30 or more secondary particles. When the first ratio is the average value of the ratio Zs of multiple secondary particles, the average value of the ratio Zs can be regarded as the first ratio when the first active substance contains multiple secondary particles.
[0065] The upper limit of the average value of the first proportion can be, for example, below 0.49 or below 0.48. The lower limit of the average value of the first proportion can be, for example, above 0, above 0.20, above 0.30, or above 0.40.
[0066] The first ratio can be controlled by adjusting the manufacturing conditions of the first active material. Specifically, this includes adjusting the NH3 concentration, pH, supply rate of alkaline compound and metal element, reaction time, reaction temperature, stirring speed, and atmosphere in the crystallization process of the reaction solution preparation and crystallization steps in the positive electrode active material precursor manufacturing process. Additionally, this includes adjusting the firing conditions in the positive electrode active material manufacturing process, such as the firing temperature and firing time in two-stage firing (e.g., the firing temperature and firing time in the second-stage firing). The manufacturing method of the first active material will be described later.
[0067] like Figure 2As shown, the primary particle 10p can be elongated. The aspect ratio (length / short diameter ratio) of the primary particle 10p can be, for example, 1.9 or higher. This tends to easily improve the initial resistance. For the primary particle 10p, the long diameter extends substantially parallel to the direction (a-axis) orthogonal to the stacking direction (c-axis) of the layered lithium transition metal composite oxide. The short diameter of the primary particle 10p is formed substantially parallel to the stacking direction (c-axis). There is no particular upper limit to the aspect ratio of the primary particle 10p, but it is preferably 2.5 or less, more preferably 2.2 or less.
[0068] It should be noted that in this specification, the aspect ratio of primary particles 10p represents the aspect ratio of the primary particles 10p constituting the lithium transition metal composite oxide. The aspect ratio of primary particles 10p is obtained from a cross-sectional SEM image of the lithium transition metal composite oxide and refers to the average aspect ratio of any selected plurality of primary particles 10p. For example, there can be more than 20 primary particles 10p. Specifically, the aspect ratio of primary particles 10p can be obtained, for example, by preparing a cross-sectional observation sample of the lithium transition metal composite oxide using CP processing. Next, an SEM image of the cross-sectional observation sample of the lithium transition metal composite oxide is obtained using SEM. Then, using image analysis particle size distribution measurement software (e.g., "Mac-View"), the aspect ratio (the ratio of the aspect ratio to the aspect ratio) is calculated based on the aspect ratios of any selected plurality of primary particles 10p from the SEM image, and the arithmetic mean is obtained.
[0069] like Figure 2 As shown, the primary particle 10p in the secondary particle 10 can be configured to extend radially from the center of the secondary particle 10 toward its outer diameter (surface). One end of the long side of the primary particle 10p can be positioned on the outer diameter side of the secondary particle 10, and the other end can be positioned on the center side of the secondary particle 10. The a-axis of the primary particle 10p can be configured to extend radially from the center of the secondary particle 10 toward its outer diameter.
[0070] The average particle size of the primary particles (10p) can be, for example, 0.05 to 2.5 μm, and from the viewpoint of charge-discharge cycle characteristics, preferably 0.1 to 2.3 μm, more preferably 0.2 to 2.1 μm. It should be noted that the average particle size of the primary particles (10p) refers to the average particle size obtained by observing the surface of the secondary particles by SEM and measuring the particle size of 10 primary particles (10p).
[0071] The average particle size D50 of the first active material or the particle group composed of multiple secondary particles can be, for example, 2 μm to 50 μm, and from the viewpoint of charge-discharge cycle characteristics, preferably 5 μm to 30 μm, more preferably 10 μm to 20 μm.
[0072] It should be noted that in this specification, the average particle size D50 refers to the median particle size (D50), which is the particle size that accumulates to 50% of the volume frequency from the smallest particle side in a volume-based particle size distribution based on laser diffraction and scattering. Therefore, the average particle size D50 of the first active material or a particle group composed of multiple secondary particles can be determined using a particle size distribution measuring device of the laser diffraction and scattering type.
[0073] Secondary particles can be formed by the simple condensation of primary particles, resulting in what is known as a solid structure. However, this is not the only possibility; for example... Figure 2 As shown, the secondary particle 10 may have a void 11 inside it, formed by gaps between the condensed primary particles 10p. It should be noted that the void 11 may or may not be open. When the void 11 is open, it may have two or more openings. In the cross-sectional view, the void 11 is located inside the secondary particle 10 and may be a space surrounded by multiple primary particles 10p.
[0074] From the viewpoint of charge-discharge cycle characteristics, when secondary particles have voids, the porosity is preferably 2 to 8%. The porosity of the secondary particles is, for example, 2% or more, and can be 3% or more, or 5% or more. By ensuring the porosity of the secondary particles is above a specified value, the initial resistance of the non-aqueous electrolyte secondary battery can be reduced. Furthermore, appropriate voids can be ensured within the secondary particles. Additionally, when the secondary particles have a coating layer (described later), the coating layer can be properly positioned at the interface between adjacent primary particles and at the center of the secondary particles. On the other hand, if the porosity of the secondary particles is too high (typically, exceeding 8%), the resistance during storage increases. Therefore, the porosity of the secondary particles is, for example, 8% or less, and can be 7% or less, or 6% or less. It should be noted that in this specification, the porosity of the secondary particles can be calculated by averaging the porosities of arbitrarily selected secondary particles in an SEM image of the cross-section of the secondary particles. In measuring the porosity of the secondary particles, the number of secondary particles can be, for example, 20 or more. First, a sample for observing the cross-section of the secondary particles is prepared by CP processing or the like. Next, SEM images of the specimens for cross-sectional observation were obtained using SEM. From the obtained SEM images, the area of the entire secondary particle and the total area of all voids within the secondary particle were calculated using image analysis software (e.g., ImageJ). Then, the porosity was calculated using equation (i) shown below, and the average value was calculated.
[0075] Porosity (%) = (Total area of all voids / Total area of secondary particles) × 100 (i)
[0076] The porosity of the secondary particles can be adjusted, for example, by changing the synthesis conditions when synthesizing hydroxides as precursors for positive electrode active materials using a crystallization method. Specifically, in the crystallization method, an aqueous solution containing a metal element other than lithium and a pH adjusting solution are added to the reaction solution to synthesize the hydroxide. By changing the pH value and stirring speed of the reaction solution at this time, the porosity of the hydroxide can be adjusted. By mixing this hydroxide with a compound that serves as a lithium source (such as lithium hydroxide) and calcining it, a lithium transition metal composite oxide with secondary particles and adjusted porosity can be obtained. In addition, during the calcination process in the positive electrode active material manufacturing step, it can also be controlled by adjusting the calcination temperature, for example, by adjusting the calcination temperature of the second stage.
[0077] like Figure 2 As shown, the first active material may have a coating layer 12 at the interface between the surface of the secondary particle 10 and the adjacent primary particle 10p. The coating layer 12 is disposed on the secondary particle 10 by physical and / or chemical bonding. The coating layer can be formed by mixing the secondary particles and the material constituting the coating layer and firing them. It should be noted that... Figure 1 The middle covering layer is not shown in the diagram.
[0078] The coating layer 12 contains a boron compound. By depositing the boron compound as the coating layer 12 on the surface of the secondary particles 10, the degradation of the primary particles 10p is easily suppressed, and the cycle durability characteristics are easily improved. Furthermore, the leaching of Mn from the secondary particles 10 into the non-aqueous electrolyte can be suppressed, thus inhibiting the increase in resistance during storage. Additionally, in the first active material, the binding force between the primary particles 10p is increased by having the coating layer 12. This mitigates the stress during expansion and contraction, suppressing the breakage of the secondary particles 10. From this perspective, the increase in resistance during storage can also be effectively suppressed. As the aforementioned boron compound, boron oxides or oxides containing boron and lithium are preferred, and lithium borate salts are particularly preferred. Examples of boron compounds include B2O2, B2O3, B4O3, B4O5, LiBO2, and Li3B7O. 12 Li6B4O9, Li3B 11 O 18 Examples of active materials include Li₂B₄O₇, Li₃BO₃, and LiB(OH)₄. From the viewpoint of charge-discharge cycle characteristics, LiBO₂ is preferred. From the viewpoint of charge-discharge cycle characteristics, the secondary particle 10 preferably has a coating layer 12 containing LiBO₂. The ratio of the total moles of boron (B) to the total moles of metal elements other than Li in the first active material (hereinafter also referred to as the B content) can be, for example, 0.5 to 2.0 mol%, and from the viewpoint of charge-discharge cycle characteristics, it is preferably 0.7 to 1.5 mol%.
[0079] In addition to the boron compound, the coating layer 12 may further contain aluminum oxide (Al₂O₃). Aluminum oxide has the function of capturing hydrogen fluoride gas (hydrofluoric acid) generated by the decomposition of the non-aqueous electrolyte. This suppresses the dissolution of Mn into the non-aqueous electrolyte caused by the reaction of the first active material (lithium transition metal complex oxide) with hydrogen fluoride gas. By configuring the coating layer 12, which further contains aluminum oxide in addition to the boron compound, on the surface of the secondary particles 10, charge-discharge cycle characteristics can be further improved. The ratio of the total moles of aluminum (Al) to the total moles of metal elements other than Li in the first active material (hereinafter also referred to as the Al content) can be, for example, 0.1 to 0.5 mol%, and from the viewpoint of charge-discharge cycle characteristics, preferably 0.3 to 0.5 mol%.
[0080] The coating layer 12 may further contain a tungsten compound. When the coating layer 12 contains a tungsten compound, the electronic resistance of the secondary particle surface tends to increase, the short-circuit current in the evaluation of thermal stability is easily suppressed, the thermal stability is easily improved, and the bonding force between the primary particles 10p tends to increase. As a result, there is a tendency to: mitigate stress during expansion and contraction, easily suppress particle breakage of secondary particles, and easily improve charge-discharge cycle characteristics.
[0081] From the viewpoint of thermal stability and charge-discharge cycle characteristics, the tungsten compound preferably contains at least one selected from CoWO4, MnWO4 and LiWO4.
[0082] The thickness of the coating layer 12 can be, for example, 50–200 nm, and from the viewpoint of thermal stability and cycle durability, preferably 60–190 nm, more preferably 70–180 nm. The thickness of the coating layer 12 can be determined, for example, by XPS (X-ray Photoelectron Spectroscopy) depth analysis or cross-sectional observation by transmission electron microscopy (TEM).
[0083] From the viewpoint of charge-discharge cycle characteristics, the coating layer 12 preferably exists inside the secondary particles 10, either on the surface of the secondary particles 10 or replacing the surface of the secondary particles 10. Specifically, it is preferable that the coating layer 12 exists on the surface of the primary particles 10p inside the secondary particles 10. When the secondary particles 10 have voids 11, it is easy to form the coating layer 12 inside the secondary particles 10. In addition, the coating layer 12 can exist at the interface between adjacent primary particles 10p. When the coating layer 12 exists on the surface of the primary particles 10p constituting the voids 11 of the secondary particles 10, it is presumed that the coating layer 12 exists between adjacent primary particles 10p. The amount of coating layer 12 existing inside the secondary particles 10 can be more or less than the amount of coating layer 12 existing on the surface of the secondary particles.
[0084] The coverage of the secondary particles 10 by the coating layer 12 can be, for example, more than 60%, less than 100%, or less than 95%. It should be noted that the proportion (coverage rate) of the coating layer 12 disposed on the surface of the secondary particles 10 and the portion covered by the coating layer 12 can be confirmed, for example, by XPS analysis of the secondary particles 10, using the boron coverage rate (%). The boron coverage rate (%) can be quantified by XPS analysis from the peaks of boron (B):B1s, nickel (Ni):Ni2p3, cobalt (Co):Co2p3, and manganese (Mn):Mn2p1, and calculated using the following formula.
[0085] Boron coating percentage (%) = B / (B + Ni + Co + Mn)
[0086] Furthermore, the coating rate of active material containing porous secondary particles can be compared with the coating rate of active material containing 0% porosity secondary particles. If the value decreases, it can be determined that a coating layer has formed inside the secondary particles, i.e., at the interface between adjacent primary particles, and the protection of the primary particles is underway. The surface of the secondary particles can be observed, for example, by SEM-EDS analysis, and the coating state of the interface between adjacent primary particles inside the secondary particles can be observed, for example, by STEM-EDS analysis or LA-ICP-MS (Laser Ablation Inductively Coupled Plasma Mass Spectrometry).
[0087] The method for manufacturing the first active substance is, for example, as follows: Figure 8 The process may include a positive electrode active material precursor manufacturing step (S1) to manufacture a positive electrode active material precursor; followed by a positive electrode active material manufacturing step (S2) to manufacture a positive electrode active material by mixing the positive electrode active material precursor and a lithium compound and calcining them. The positive electrode active material manufacturing step may further include at least one of a step of mixing the positive electrode active material and a compound forming a coating layer, and a step of mixing two or more different active materials.
[0088] In the manufacturing process of the cathode active material precursor, a hydroxide is prepared as the cathode active material precursor. The hydroxide typically contains a metal element other than lithium from the metal elements contained in lithium transition metal complex oxides. The metal elements can be combined in a molar ratio of the metal elements other than lithium that constitute the first active material. When generating the cathode active material precursor, a compound containing ammonium ions, such as ammonia (NH3), is used as the alkaline compound. At this time, by adjusting the NH3 concentration, pH, the supply rate of the alkaline compound and the metal element, and the reaction time, the crystal orientation, aspect ratio (major and minor axes of the primary particles at 10p), and arrangement of the primary particles can be controlled. By adjusting the NH3 concentration, NH3 molecules can be coordinated on the crystal surface of the NCM seed crystals generated in the early stage of co-precipitation, easily inhibiting crystal growth. Furthermore, the ease of coordination of NH3 molecules varies depending on the crystal face; therefore, by controlling the NH3 concentration, the growth of specific crystal faces can be easily promoted. Adjustment of pH and the supply rate of the alkaline compound and the metal element can also be factors controlling the crystal growth rate. If the pH is too high, crystal growth will proceed rapidly regardless of the NH3 concentration, easily resulting in non-oriented crystals. If the pH is too low, crystal growth tends to be difficult. By appropriately adjusting the pH and reducing the supply rate of alkaline compounds and metal elements, crystal growth can be carried out slowly, tending to produce particles with consistent crystal orientation.
[0089] The process for manufacturing the positive electrode active material precursor may include, for example, a reaction solution preparation process and a crystallization process. In the reaction solution preparation process, the pH of distilled water can be adjusted to 11–12, and the NH3 concentration (hereinafter also referred to as the initial ammonia concentration) can be adjusted to 0.3–1.0% by mass. The pH is the pH at a liquid temperature of 25°C. pH adjustment can be achieved by adding 9–11 mol / L of sodium hydroxide (NaOH) aqueous solution. The NH3 concentration can be adjusted by adding an NH3 aqueous solution (e.g., NH4OH). The ammonia (ammonium ion) concentration in the NH3 aqueous solution can, for example, be below 15.0 mol / L, or 13.0–13.5 mol / L. A nitrogen atmosphere can be created by bubbling nitrogen into the reaction solution. In the reaction solution preparation process, an aqueous solution containing a metal element (hereinafter also referred to as a raw material metal aqueous solution) can be prepared for supply in the subsequent crystallization process. The metal element concentration in the raw material metal aqueous solution can, for example, be 0.5–2.5 mol / L, or 1.0–2.0 mol / L.
[0090] Next, in the crystallization step, an aqueous solution of the raw metal and an aqueous solution of NH3, adjusted for pH and NH3 concentration in the reaction solution preparation step, are supplied to distilled water for crystallization, thereby producing hydroxides. Crystallization can be carried out while bubbling nitrogen. The supply rate of the raw metal aqueous solution can be, for example, 50–70 mL / hr or 55–65 mL / hr. The supply rate of the NH3 aqueous solution can be, for example, 15–35 mL / hr or 20–30 mL / hr. The raw metal aqueous solution and the NH3 aqueous solution can be supplied in a molar ratio of ammonia to metal element of, for example, 2.0–3.5 or 2.5–3.0. During crystallization, an aqueous solution of sodium hydroxide is supplied to maintain a constant pH. The pH can be 11.0–12.0. The reaction time can be, for example, 25–60 hours. The reaction temperature can be, for example, 40–60°C or 50°C. The reaction solution can be stirred during the crystallization step. The stirring speed can be, for example, 600-1000 rpm or 800 rpm.
[0091] Next, in the positive electrode active material manufacturing process, the obtained positive electrode active material precursor is mixed with a lithium compound (e.g., lithium hydroxide) and calcined. At this time, by adjusting the calcination temperature and calcination time, the morphology of the secondary particles of the lithium transition metal composite oxide can be well controlled. Calcination can be a two-stage process. In the two-stage calcination, the calcination temperature of the first stage can be, for example, 300°C to 600°C. Furthermore, the calcination time of the first stage can be, for example, 1 hour to 20 hours. The heating rate up to the first stage calcination temperature can be, for example, 10°C / min. The calcination temperature of the second stage can be, for example, 650°C to 800°C. Furthermore, the calcination time of the second stage can be, for example, 5 hours to 30 hours. The heating rate up to the second stage calcination temperature can be, for example, 10°C / min.
[0092] Next, the first active material can be prepared by mixing the obtained secondary particles, the positive electrode active material, and the boron compound that forms the coating layer.
[0093] The positive electrode active material may consist of only the first active material, or it may contain positive electrode active materials other than the first active material within a range that does not impede the effects of this disclosure (e.g., less than 10% by mass relative to the total mass of the positive electrode active material, preferably less than 5% by mass).
[0094] <Positive Plate>
[0095] The positive electrode plate has a positive electrode active material layer containing the above-mentioned positive electrode active material. Figure 9 This is a schematic cross-sectional view taken from a direction perpendicular to the thickness direction (stack direction) of the positive electrode plate. For example... Figure 9As shown, in the positive electrode plate 20, the positive electrode active material layer 22 can be formed directly or indirectly on one or both sides of the positive electrode substrate 21. The positive electrode substrate 21 can be, for example, a conductive sheet made of Al alloy foil, pure Al foil, etc. The positive electrode active material layer 22 contains positive electrode active material 60. The positive electrode active material 60 contains the aforementioned positive electrode active material. The positive electrode active material 60 can be manufactured by the aforementioned method for manufacturing positive electrode active materials. The positive electrode active material layer 22 may further contain conductive materials and adhesives, etc.
[0096] The positive electrode active material layer 22 can, for example, have a thickness of 10 μm to 200 μm. The positive electrode active material layer 22 can have a high density. For example, the density of the positive electrode active material layer 22 can be 3.5 g / cm³. 3 The above can also be 3.6 g / cm³. 3 Above or 3.7g / cm 3 The above. For example, the positive electrode active material layer 22 can have a content of 4.0 g / cm³. 3 The following densities.
[0097] The content of positive electrode active material 60 in the positive electrode active material layer 22 (i.e., the ratio of the mass of positive electrode active material 60 to the total mass of the positive electrode active material layer 22) is not particularly limited. For example, it is 80% by mass or more, preferably 87% by mass or more, more preferably 90% by mass or more, further preferably 95% by mass or more, and most preferably 97% by mass or more, relative to the total mass of the positive electrode active material layer 22.
[0098] The manufacturing method of the positive electrode plate 20 includes the preparation (A) of the positive electrode slurry, coating (B) and rolling (C). In the preparation (A) of the positive electrode slurry, a positive electrode slurry containing the positive electrode active material manufactured by the above-described method for manufacturing positive electrode active material is prepared. The positive electrode slurry is prepared by dispersing the positive electrode active material in a dispersion medium. The dispersion medium can be an organic solvent, such as N-methyl-2-pyrrolidone (NMP), tetrahydrofuran (THF), dimethylformamide (DMF), methyl ethyl ketone (MEK), and dimethyl sulfoxide (DMSO). The positive electrode slurry may contain a conductive material and a binder. Examples of conductive materials include carbon nanotubes (CNTs), carbon black such as acetylene black (AB), and other carbon materials (such as graphite). Examples of adhesives include polyvinylidene fluoride (PVdF), polytetrafluoroethylene (PTFE), polyimide (PI), polyamide (PA), polyamide-imide (PAI), butadiene rubber (BR), styrene-butadiene rubber (SBR), acrylonitrile-butadiene rubber (NBR), styrene-ethylene-butene-styrene block copolymer (SEBS), carboxymethyl cellulose (CMC), or combinations thereof. The slurry may have a solids content of, for example, from 40% to 80%. Mixing can be performed using any stirring, mixing, or dispersing apparatus.
[0099] In coating (B), a positive electrode active material layer 22 is formed by coating the positive electrode slurry onto the surface of the positive electrode substrate 21. In rolling (C), a positive electrode plate 20 is manufactured by rolling the positive electrode active material layer 22 and the positive electrode substrate 21. The primary plate of the positive electrode plate 20 is manufactured by rolling. The primary plate can be cut into specified planar dimensions according to the specifications of the battery 100.
[0100] <Non-aqueous electrolyte secondary battery>
[0101] Figure 10 This is a schematic diagram illustrating an example of a non-aqueous electrolyte secondary battery in this embodiment. Figure 10 The battery 100 shown may be, for example, a lithium-ion battery that is the main power source or auxiliary power source for an electric vehicle.
[0102] The battery 100 includes an outer casing 90. The outer casing 90 houses the electrode body 50 and the electrolyte (not shown). The electrode body 50 is connected to the positive terminal 91 via a positive current collector 81. The electrode body 50 is connected to the negative terminal 92 via a negative current collector 82. Figure 11This is a schematic diagram illustrating an example of an electrode body in this embodiment. The electrode body 50 is a wound type. The electrode body may be a stacked type. The electrode body 50 includes a positive electrode plate 20, a separator 40, and a negative electrode plate 30. That is, the battery 100 includes a positive electrode plate 20. The positive electrode plate 20 includes a positive electrode active material layer 22 and a positive electrode substrate 21. The negative electrode plate 30 includes a negative electrode active material layer 32 and a negative electrode substrate 31.
[0103] The negative electrode plate 30 typically has a negative electrode substrate 31 and a negative electrode active material layer 32 formed on one or both sides of the negative electrode substrate 31. The negative electrode substrate 31 is, for example, a metal foil made of copper materials such as copper and copper alloys. The negative electrode active material layer 32 contains the negative electrode active material and may further contain conductive materials and adhesives.
[0104] Examples of known materials that can be used as negative electrode active materials include carbon-based active material particles such as graphite, and metal-based active material particles containing elements selected from Si, Sn, Sb, Bi, Ti, and Ge. Negative electrode active materials may include, for example, carbon-based active material particles and silicon-containing materials. Silicon-containing materials may be, for example, Si-C composites. Conductive materials include the aforementioned conductive materials. Adhesives include cellulose resins such as CMC, methylcellulose (MC), and hydroxypropyl cellulose; polyacrylic acid; and styrene-butadiene rubber (SBR). CMC can also be used as a thickener.
[0105] The separator 40 has a single-layer or multi-layer substrate, and may have a functional layer on at least one side of the substrate. The substrate may be a porous sheet such as a membrane made of polyolefins such as polyethylene and polypropylene, polyester, cellulose, polyamide, etc., or a non-woven fabric. Examples of functional layers include adhesive layers and / or heat-resistant layers. Adhesive layers may be formed, for example, by adhesives. Heat-resistant layers may include, for example, fillers and adhesives.
[0106] The electrolyte can be, for example, a non-aqueous electrolyte. Preferably, the non-aqueous electrolyte contains the electrolyte in a non-aqueous solvent such as an organic solvent. Examples of electrolytes include one or more of LiPF6, LiBF4, LiClO4, LiFSO3, and LiBOB. Examples of non-aqueous solvents include one or more of ethylene carbonate (EC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), propylene carbonate (PC), butyl carbonate (BC), and diethyl carbonate (DEC). The non-aqueous electrolyte may further contain additives such as vinylene carbonate (VC), vinyl ethylene carbonate (VEC), and fluoroethylene carbonate.
[0107] The present invention will be further described in detail below through examples.
[0108] Example
[0109] [Making the positive electrode plate]
[0110] 100 parts by weight of the first active material of the examples and comparative examples, 1 part by weight of graphite as a conductive material, and 0.9 parts by weight of polyvinylidene fluoride powder as a binder were mixed, and an appropriate amount of N-methyl-2-pyrrolidone (NMP) was further added to prepare a positive electrode composite slurry. The positive electrode composite slurry was coated on both sides of a positive electrode current collector made of aluminum foil and dried. Then, the coating was rolled using rolling rolls to produce a positive electrode plate with positive electrode active material layers formed on both sides of the positive electrode current collector.
[0111] [Fabrication of Non-Aqueous Electrolyte Secondary Batteries]
[0112] (Making the negative electrode plate)
[0113] Graphite, as a carbon material, is used as the negative electrode active material. It is mixed with styrene-butadiene rubber (SBR) as a binder and carboxymethyl cellulose (CMC) as a thickener at a solid content mass ratio of negative electrode active material:SBR:CMC = 100:1:1 to prepare a slurry for forming the negative electrode active material layer. The obtained slurry is coated onto a 10 μm thick copper foil negative electrode current collector and dried to form the negative electrode active material layer. The resulting negative electrode active material layer is then rolled using rolling mills and cut to specified dimensions to fabricate the negative electrode plate.
[0114] (Preparation of isolation components)
[0115] As a separator, a porous polyolefin sheet with a thickness of 20 μm and a three-layer structure of PP / PE / PP is prepared.
[0116] (Preparation of non-aqueous electrolytes)
[0117] As a non-aqueous electrolyte, a non-aqueous electrolyte was prepared by dissolving LiPF6, which served as the supporting salt, in a mixed solvent containing ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) at a volume ratio of EC:EMC:DMC = 30:40:30 at a concentration of 1 mol / L.
[0118] (Fabrication of a non-aqueous electrolyte secondary battery)
[0119] The positive and negative electrode plates are overlapped with a separator sandwiched between them to obtain a laminate. Next, the laminate is wound to obtain a wound body, which is then pressed into a flat shape to obtain a flat electrode body. Current collector terminals are installed on the electrode body, inserted into the battery casing and soldered, and then a non-aqueous electrolyte is injected. Finally, the non-aqueous electrolyte secondary battery is manufactured by sealing the battery casing.
[0120] [Determination of the average particle size D50 of the positive electrode active material (secondary particles)]
[0121] The particle size distribution was measured using a laser diffraction-scattering particle size distribution measuring device.
[0122] [Determination of the average particle size of primary particles]
[0123] The width of the primary particles is measured in the SEM image of the secondary particle surface and is taken as the particle size of the primary particles. The average particle size of the primary particles is calculated by measuring the particle size of 100 primary particles in total, which are obtained by further randomly selecting 10 primary particles from each of the 10 randomly selected secondary particles.
[0124] [Determination of the first proportion]
[0125] Ten secondary particles were collected from the positive electrode active material prepared in the examples and comparative examples, and cross-sectional samples for EBSD analysis were prepared by CP processing. Using SEM-EDS (SEM: JSM-IT800, NEC Corporation; EDS: AZtecLive, AZtecHKL, AZtecCrystal, SymmetryS3), IPF maps were prepared on a 5000x magnification image to show the crystal orientation of primary particles in the cross-section of the positive electrode active material, selecting particles with a cross-sectional diameter that is the same as or approximately the same as the average particle size D50 of the positive electrode active material (a particle group composed of multiple secondary particles).
[0126] In the IPF diagram, the total number of boundaries between primary particles with a crystal orientation difference of 60° or more among adjacent primary particles on the 10 lines dividing the particle into 11 equal parts, and the total number of primary particles on the 10 lines, are calculated. The total number of boundaries is divided by the total number of primary particles to obtain the first ratio. The average value of the first ratio obtained from the 10 secondary particles is then calculated. Table 1 shows the calculated average value as the first ratio.
[0127] [Evaluation of charge-discharge cycle characteristics]
[0128] At an ambient temperature of 60°C, the fabricated non-aqueous electrolyte secondary battery was charged to 4.2V at a constant current of 0.5C, and then discharged to 2.5V at a constant current of 0.5C. This charge-discharge cycle was defined as one cycle, and 200 cycles were performed. The capacity retention rate (%) during the charge-discharge cycle was calculated using the following formula.
[0129] Capacity retention (%) = (Discharge capacity at 200th cycle / Discharge capacity at 1st cycle) × 100
[0130] A higher capacity retention rate (%) indicates better charge-discharge cycle characteristics.
[0131] [Evaluation of boron coverage]
[0132] XPS analysis was performed on the prepared positive electrode active material powder to quantify the surface coating state. Next, the presence of boron was qualitatively analyzed based on peak positions. In the quantitative analysis, the peaks of boron (B):B1s, nickel (Ni):Ni2p3, cobalt (Co):Co2p3, and manganese (Mn):Mn2p1 were used for quantification, and the values were calculated using the following formula.
[0133] Boron coating percentage (%) = B / (B + Ni + Co + Mn)
[0134] [Evaluation of porosity]
[0135] The prepared positive electrode plate was cross-sectionally processed using CP (Polymerization Processing), and a 5000x magnified reflected electron image was obtained using SEM (Search Engine Electron Microscopy). Otsu's method was used to binarize the image, separating the secondary particles into particle and void portions. The ratio of the void portion to the total area of the secondary particles (particle portion + void portion) was calculated as the porosity (%).
[0136] <Comparative Example 1>
[0137] [Preparation of positive electrode active material precursor]
[0138] (Reaction solution preparation process)
[0139] NiSO4, CoSO4, and MnSO4 were mixed in distilled water at a nickel:cobalt:manganese molar ratio of 80:10:10 to prepare a raw material metal aqueous solution with a concentration of 2.0 mol / L. Next, a 10 mol / L sodium hydroxide (NaOH) aqueous solution was added to a reaction tank containing distilled water at a pH of 11.5 based on a liquid temperature of 25°C, and a 13.3 mol / L ammonia aqueous solution was added with an ammonia (NH3) concentration (hereinafter referred to as the initial ammonia concentration) of 1.0% by mass.
[0140] (Crystallization process)
[0141] Nitrogen gas was then introduced into the reaction vessel and bubbled. A 10 mol / L sodium hydroxide aqueous solution was supplied at a rate of 60 mL / hr to maintain the pH at a base of 25°C (hereinafter also referred to as the pH during crystallization) at 11.5. Simultaneously, an aqueous solution of the raw metal was supplied at a rate of 60 mL / hr with a molar ratio of ammonia to the raw metal (hereinafter also referred to as the supply rate ratio) of 2.7, and an aqueous solution of 13.3 mol / L ammonia (NH3) was supplied at a rate of 25 mL / hr. Crystallization was carried out for 48 hours at a reaction temperature of 50°C and a stirring speed of 800 rpm. The pH in the reaction vessel was controlled by adjusting the flow rate of the sodium hydroxide aqueous solution using a pH controller. Next, the solution supply was stopped to end the crystallization. The product was then sequentially filtered, washed with water, and dried to produce the positive electrode active material precursor C1.
[0142] [Manufacturing of positive electrode active material]
[0143] The cathode active material precursor Cl and lithium hydroxide (LiOH) were mixed with a Li / Me ratio of 1.01 (the ratio of the total moles of lithium to the total moles of other metal elements, excluding lithium). The mixture was then calcined under the following conditions to obtain the cathode active material: the temperature was increased to 500°C at a rate of 10°C / min in an oxidizing atmosphere, held at 500°C for 3 hours, then increased to 760°C at a rate of 2°C / min, and held at 760°C for 10 hours. The resulting cathode active material consisted of secondary particles composed of more than 100 primary particles. The aspect ratio of the primary particles was 1.9, the average particle size was 0.4 μm, and the average particle size D50 of the secondary particles was 13.7 μm. The first ratio, porosity, and charge-discharge cycle characteristics were evaluated. The results are shown in Table 1.
[0144] <Example 1>
[0145] The positive electrode active material prepared in the same manner as in Comparative Example 1 was mixed with H3BO3 at 1 mol% relative to the positive electrode active material and heat-treated at 300°C for 3 hours to prepare a positive electrode active material having a coating layer composed of LiBO2. The obtained positive electrode active material consisted of secondary particles formed by the aggregation of more than 100 primary particles. The aspect ratio of the primary particles was 1.9, the average particle size of the primary particles was 0.4 μm, and the average particle size D50 of the secondary particles was 13.7 μm. The first ratio, boron coating efficiency, porosity, and charge-discharge cycle characteristics were evaluated. The results are shown in Table 1.
[0146] <Example 2>
[0147] In Example 1, the stirring speed was 900 rpm during the crystallization process, and the firing temperature of the second stage in the manufacture of the positive electrode active material was changed to 750°C. Otherwise, the positive electrode active material was prepared in the same manner as in Example 1. The obtained positive electrode active material consisted of secondary particles formed by the aggregation of more than 100 primary particles. The aspect ratio of the primary particles was 1.9, the average particle size of the primary particles was 0.3 μm, and the average particle size D50 of the secondary particles was 13.0 μm. The first ratio, boron coating, porosity, and charge-discharge cycle characteristics were evaluated. The results are shown in Table 1.
[0148] <Example 3>
[0149] In Example 1, the stirring speed was 750 rpm during the crystallization process, and the positive electrode active material was prepared in the same manner as in Example 1. The obtained positive electrode active material consisted of secondary particles formed by the aggregation of more than 100 primary particles. The aspect ratio of the primary particles was 1.9, the average particle size of the primary particles was 0.4 μm, and the average particle size D50 of the secondary particles was 13.5 μm. The first ratio, boron coating, porosity, and charge-discharge cycle characteristics were evaluated. The results are shown in Table 1.
[0150] <Example 4>
[0151] In Example 1, the stirring speed was 700 rpm during the crystallization process, and the positive electrode active material was prepared in the same manner as in Example 1. The obtained positive electrode active material consisted of secondary particles formed by the aggregation of more than 100 primary particles. The aspect ratio of the primary particles was 1.8, the average particle size of the primary particles was 0.4 μm, and the average particle size D50 of the secondary particles was 13.5 μm. The first ratio, boron coating, porosity, and charge-discharge cycle characteristics were evaluated. The results are shown in Table 1.
[0152] <Example 5>
[0153] A positive electrode active material prepared in the same manner as Comparative Example 1 was mixed with 1 mol% H3BO3 and 1 wt% Al2O3 relative to the positive electrode active material, and heat-treated at 300°C for 3 hours to prepare a positive electrode active material having a coating layer composed of LiBO2 and Al2O3. The obtained positive electrode active material consisted of secondary particles formed by the aggregation of more than 100 primary particles. The aspect ratio of the primary particles was 1.9, the average particle size of the primary particles was 0.4 μm, and the average particle size D50 of the secondary particles was 13.4 μm. The first ratio, boron coating efficiency, porosity, and charge-discharge cycle characteristics were evaluated. The results are shown in Table 1.
[0154] <Comparative Example 2>
[0155] A positive electrode active material prepared in the same manner as in Comparative Example 1 was mixed with 1 wt% Al₂O₃ relative to the positive electrode active material to prepare a positive electrode active material having a coating layer composed of Al₂O₃. The obtained positive electrode active material consisted of secondary particles formed by the aggregation of more than 100 primary particles. The aspect ratio of the primary particles was 1.9, the average particle size of the primary particles was 0.4 μm, and the average particle size D50 of the secondary particles was 13.4 μm. The first ratio, porosity, and charge-discharge cycle characteristics were evaluated. The results are shown in Table 1.
[0156] <Comparative Example 3>
[0157] [Preparation of positive electrode active material precursor]
[0158] (Reaction tank preparation process)
[0159] NiSO4, CoSO4, and MnSO4 were mixed in distilled water at a nickel:cobalt:manganese molar ratio of 80:10:10 to prepare a raw material metal aqueous solution with a raw material metal concentration of 2.0 mol / L. Next, a 10 mol / L sodium hydroxide (NaOH) aqueous solution was added to a reaction tank containing distilled water at a pH of 11.5 based on a liquid temperature of 25°C, and a 13.3 mol / L ammonia aqueous solution was added at an ammonia (NH3) concentration (hereinafter also referred to as the initial ammonia concentration) of 1.0% by mass.
[0160] (Crystallization process)
[0161] Nitrogen gas was then introduced into the reaction vessel and bubbled. A 10 mol / L sodium hydroxide aqueous solution was supplied at a rate of 60 mL / hr to maintain the pH at 11.5 at a base temperature of 25°C. Simultaneously, an aqueous solution of the raw metal was supplied at a rate of 60 mL / hr with a molar ratio of ammonia to the raw metal of 2.7, and an aqueous solution of 13.3 mol / L ammonia was supplied at a rate of 25 mL / hr. Crystallization was carried out for 48 hours at a reaction temperature of 50°C and a stirring speed of 800 rpm. The pH in the reaction vessel was controlled by adjusting the flow rate of the sodium hydroxide aqueous solution using a pH controller. Next, the solution supply was stopped to end the crystallization. The product was then filtered, washed with water, and dried sequentially to produce the positive electrode active material precursor C3.
[0162] [Manufacturing of positive electrode active material]
[0163] The cathode active material precursor C3 and lithium hydroxide (LiOH) were mixed such that the ratio of the total moles of lithium to the total moles of other metal elements (hereinafter also referred to as the Li / Me ratio) was 1.01, and then calcined under the following conditions: held at 760°C for 13 hours in an oxidizing atmosphere; thus obtaining the cathode active material. The obtained cathode active material consists of secondary particles formed by the aggregation of more than 100 primary particles. The aspect ratio of the primary particles is 1.9, the average particle size of the primary particles is 0.4 μm, and the average particle size D50 of the secondary particles is 14.1 μm. First-phase and charge-discharge cycle characteristics were evaluated. The results are shown in Table 1.
[0164] <Comparative Example 4>
[0165] The positive electrode active material prepared in the same manner as in Comparative Example 3 was mixed with H3BO3 at 1 mol% relative to the positive electrode active material and heat-treated at 300°C for 3 hours to prepare a positive electrode active material having a coating layer composed of LiBO2. The obtained positive electrode active material consisted of secondary particles formed by the aggregation of more than 100 primary particles. The aspect ratio of the primary particles was 1.9, the average particle size of the primary particles was 0.4 μm, and the average particle size D50 of the secondary particles was 14.1 μm. The first ratio, boron coating efficiency, porosity, and charge-discharge cycle characteristics were evaluated. The results are shown in Table 1.
[0166] <Comparative Example 5>
[0167] [Preparation of positive electrode active material precursor]
[0168] In the crystallization process of manufacturing the positive electrode active material precursor in Comparative Example 1, the initial ammonia concentration was set to 0.3% by mass. Otherwise, the positive electrode active material was prepared in the same manner as in Comparative Example 1. The obtained positive electrode active material consisted of secondary particles formed by the aggregation of more than 100 primary particles. The aspect ratio of the primary particles was 2.0, the average particle size of the primary particles was 0.4 μm, and the average particle size D50 of the secondary particles was 14.0 μm. The first ratio, boron coating, porosity, and charge-discharge cycle characteristics were evaluated. The results are shown in Table 1.
[0169] <Example 6>
[0170] The positive electrode active material prepared in the same manner as in Comparative Example 5 was mixed with H3BO3 at 1 mol% relative to the positive electrode active material and heat-treated at 300°C for 3 hours to prepare a positive electrode active material having a coating layer composed of LiBO2. The obtained positive electrode active material consisted of secondary particles formed by the aggregation of more than 100 primary particles. The aspect ratio of the primary particles was 2.0, the average particle size of the primary particles was 0.4 μm, and the average particle size D50 of the secondary particles was 14.0 μm. The first ratio, boron coating efficiency, porosity, and charge-discharge cycle characteristics were evaluated. The results are shown in Table 1.
[0171] <Comparative Example 6>
[0172] In the reaction tank preparation step of the positive electrode active material precursor manufacturing process in Comparative Example 5, NiSO4, CoSO4, and MnSO4 were mixed in distilled water at a nickel:cobalt:manganese molar ratio of 60:20:20 to prepare a raw material metal aqueous solution with a raw material metal concentration of 2.0 mol / L. In the manufacturing of the positive electrode active material, the second-stage firing temperature was changed to 780°C. Otherwise, the positive electrode active material was prepared in the same manner as in Comparative Example 1. The obtained positive electrode active material consisted of secondary particles formed by the aggregation of more than 100 primary particles. The aspect ratio of the primary particles was 1.9, the average particle size of the primary particles was 0.4 μm, and the average particle size D50 of the secondary particles was 13.7 μm. The first ratio, porosity, and charge-discharge cycle characteristics were evaluated. The results are shown in Table 1.
[0173] <Example 7>
[0174] The positive electrode active material prepared in the same manner as in Comparative Example 6 was mixed with H3BO3 at 1 mol% relative to the positive electrode active material and heat-treated at 300°C for 3 hours to prepare a positive electrode active material having a coating layer composed of LiBO2. The obtained positive electrode active material consisted of secondary particles formed by the aggregation of more than 100 primary particles. The aspect ratio of the primary particles was 1.9, the average particle size of the primary particles was 0.4 μm, and the average particle size D50 of the secondary particles was 13.7 μm. The first ratio, boron coating efficiency, porosity, and charge-discharge cycle characteristics were evaluated. The results are shown in Table 1.
[0175] <Comparative Example 7>
[0176] In the reaction tank preparation step of the positive electrode active material precursor manufacturing process in Comparative Example 5, NiSO4, CoSO4, and MnSO4 were mixed in distilled water at a nickel:cobalt:manganese molar ratio of 70:10:20 to prepare a raw material metal aqueous solution with a raw material metal concentration of 2.0 mol / L. In the manufacturing of the positive electrode active material, the second-stage firing temperature was changed to 770°C. Otherwise, the positive electrode active material was prepared in the same manner as in Comparative Example 1. The obtained positive electrode active material consisted of secondary particles formed by the aggregation of more than 100 primary particles. The aspect ratio of the primary particles was 1.9, the average particle size of the primary particles was 0.3 μm, and the average particle size D50 of the secondary particles was 13.9 μm. The first ratio, porosity, and charge-discharge cycle characteristics were evaluated. The results are shown in Table 1.
[0177] <Example 8>
[0178] The positive electrode active material prepared in the same manner as in Comparative Example 7 was mixed with H3BO3 at 1 mol% relative to the positive electrode active material and heat-treated at 300°C for 3 hours to prepare a positive electrode active material having a coating layer composed of LiBO2. The obtained positive electrode active material consisted of secondary particles formed by the aggregation of more than 100 primary particles. The aspect ratio of the primary particles was 1.9, the average particle size of the primary particles was 0.3 μm, and the average particle size D50 of the secondary particles was 13.9 μm. The first ratio, boron coating efficiency, porosity, and charge-discharge cycle characteristics were evaluated. The results are shown in Table 1.
[0179] <Comparative Example 8>
[0180] In the reaction tank preparation step of the positive electrode active material precursor manufacturing process in Comparative Example 5, NiSO4, CoSO4, and MnSO4 were mixed in distilled water at a nickel:cobalt:manganese molar ratio of 90:5:5 to prepare a raw material metal aqueous solution with a raw material metal concentration of 2.0 mol / L. In the manufacturing of the positive electrode active material, the second-stage firing temperature was changed to 750°C. Otherwise, the positive electrode active material was prepared in the same manner as in Comparative Example 1. The obtained positive electrode active material consisted of secondary particles formed by the aggregation of more than 100 primary particles. The aspect ratio of the primary particles was 1.9, the average particle size of the primary particles was 0.4 μm, and the average particle size D50 of the secondary particles was 14.1 μm. The first ratio, porosity, and charge-discharge cycle characteristics were evaluated. The results are shown in Table 1.
[0181] <Example 9>
[0182] The positive electrode active material prepared in the same manner as in Comparative Example 8 was mixed with H3BO3 at 1 mol% relative to the positive electrode active material and heat-treated at 300°C for 3 hours to prepare a positive electrode active material having a coating layer composed of LiBO2. The obtained positive electrode active material consisted of secondary particles formed by the aggregation of more than 100 primary particles. The aspect ratio of the primary particles was 1.9, the average particle size of the primary particles was 0.4 μm, and the average particle size D50 of the secondary particles was 14.1 μm. The first ratio, boron coating efficiency, porosity, and charge-discharge cycle characteristics were evaluated. The results are shown in Table 1.
[0183]
[0184] As shown in Table 1, Examples 1 to 9, which have a Ni content of 60 mol% or more, a first ratio of 0.50 or less, and a coating layer containing a boron compound, exhibited high capacity retention rates. Furthermore, in Example 5, where the coating layer further contained Al₂O₃, a higher capacity retention rate than Example 1 was obtained. Compared to Example 4, which had a porosity of 0%, the coating percentages in Examples 1 to 3 decreased, indicating that a coating layer was formed within the secondary particles and at the interfaces between adjacent primary particles, thus protecting the primary particles. Therefore, according to this disclosure, a positive electrode active material, a positive electrode plate, and a non-aqueous electrolyte secondary battery with a nickel content of 60 mol% or more and improved charge-discharge cycle characteristics are provided.
[0185] Embodiments of the present invention have been described, but should be considered as illustrative in all respects and not restrictive. The scope of the invention is defined by the scope of the patent claims and is intended to include all variations within the meaning and scope equivalent to the scope of the patent claims.
Claims
1. A positive electrode active material, comprising a first active material, The first active substance comprises secondary particles formed by the aggregation of multiple primary particles. The first active material is the lithium transition metal composite oxide represented by formula (1). Li a Ni x Co y Mr z M (1-x-y-z) O2 (1) In equation (1), x, y, z, and a satisfy 0.6≤x≤1.0, 0≤y≤0.3, 0≤z≤0.3, and 0.90≤a / (x+y+z)≤1.
25. M is one or more elements selected from Mg, Ca, Al, Ti, V, Cr, Zr, Nb, Mo, Hf, Ta, and W. The number of boundaries in the secondary particle where the crystal orientation difference between adjacent primary particles is 60° or more is less than 0.5 relative to the number of primary particles in the secondary particle. The secondary particle has a coating containing a boron compound on the surface of the primary particle and at the interface between adjacent primary particles.
2. The positive electrode active material according to claim 1, wherein, The porosity of the secondary particles is 2-8%.
3. The positive electrode active material according to claim 1 or 2, wherein, The coating layer contains LiBO2.
4. The positive electrode active material according to claim 3, wherein, The coating layer further comprises Al2O3.
5. The positive electrode active material according to claim 1, wherein, In the above equation (1), x satisfies 0.7≤x≤1.
0.
6. The positive electrode active material according to claim 1, wherein, In the above equation (1), x satisfies 0.9≤x≤1.
0.
7. The positive electrode active material according to claim 5 or 6, wherein, In the formula (1), x, y, z and a satisfy 1.06≤a / (x+y+z)≤1.
25.
8. The positive electrode active material according to claim 5 or 6, wherein, In the formula (1), x, y, z and a satisfy 1.06≤a / (x+y+z)≤1.
15.
9. The positive electrode active material according to claim 1 or 2, wherein, The number of primary particles in the secondary particles is 10 or more.
10. The positive electrode active material according to claim 1 or 2, wherein, The first active substance comprises a particle group consisting of a plurality of said secondary particles.
11. The positive electrode active material according to claim 1 or 2, wherein, The aspect ratio of the primary particle is 1.9 or higher.
12. The positive electrode active material according to claim 1 or 2, wherein, The average particle size of the primary particles is 0.1–2.5 μm.
13. The positive electrode active material according to claim 1 or 2, wherein, The average particle size D50 of the first active substance is 2–50 μm.
14. A positive electrode plate comprising a positive electrode active material layer including the positive electrode active material according to claim 1 or 2.
15. A non-aqueous electrolyte secondary battery comprising the positive electrode plate as described in claim 14.
Citation Information
Patent Citations
Lithium ion secondary battery
JP2024160551A