Lithium iron phosphate material, preparation method and application thereof

By coating the surface of lithium iron phosphate material with a fluorosilicon-carbon layer, the problem of low compaction density of lithium iron phosphate material is solved, thereby improving the specific capacity and energy efficiency of the battery.

CN123162181APending Publication Date: 2026-11-24WANHUA CHEM GRP BATTERY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510660050.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-21
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing lithium iron phosphate materials have low compaction density, resulting in low specific capacity and energy efficiency of the batteries.

Method used

A fluorosilicon-carbon coating is applied to the surface of lithium iron phosphate material to enhance the bonding force between particles, form a stable conductive network, and reduce the interfacial impedance between the electrode and the electrolyte.

Benefits of technology

The increased compaction density of lithium iron phosphate materials enhances electron transport efficiency, reduces polarization effects, and improves the specific capacity and energy efficiency of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123162181A_ABST
    Figure CN123162181A_ABST
Patent Text Reader

Abstract

This invention provides a lithium iron phosphate material, its preparation method, and its applications. The lithium iron phosphate material includes a lithium iron phosphate matrix and a fluorosilicon-carbon coating layer on the surface of the lithium iron phosphate matrix. The lithium iron phosphate material provided by this invention has a fluorosilicon-carbon coating layer on the surface of the lithium iron phosphate matrix. This fluorosilicon-carbon coating layer can enhance the bonding force between lithium iron phosphate particles, which is beneficial for reducing voids between particles during compaction, thereby increasing the compaction density of the material. Furthermore, the fluorosilicon-carbon coating layer can form a stable interface layer, reducing the interfacial impedance between the electrode and the electrolyte, which is beneficial for reducing polarization effects in electrochemical reactions, thereby improving the specific capacity and energy efficiency of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of battery technology, and particularly relates to a lithium iron phosphate material, its preparation method, and its application. Background Technology

[0002] Lithium-ion batteries have become the preferred power source for modern portable electronic devices, electric vehicles, and energy storage systems due to their superior performance characteristics. Their high voltage, high energy density, and long cycle life make them dominant in various applications. However, with the increasing demand for renewable energy and electric vehicles, the performance requirements for lithium-ion batteries are also constantly increasing.

[0003] Lithium iron phosphate (LFP), as the cathode material for lithium-ion batteries, has attracted widespread attention due to its low cost, environmental friendliness, and high safety. Its unique olivine structure provides excellent thermal and chemical stability, enabling it to perform well under high temperature and overcharge conditions. Furthermore, LFP has a stable operating voltage platform, ensuring stable output during battery discharge. However, its relatively low compaction density leads to lower specific capacity and energy efficiency, which remains a key technical challenge to be addressed. Summary of the Invention

[0004] The main objective of this invention is to provide a lithium iron phosphate material with a high compaction density, which, when applied to batteries, can improve the specific capacity and energy efficiency of the batteries.

[0005] The present invention also provides a method for preparing lithium iron phosphate material, which can prepare the above-mentioned lithium iron phosphate material, and the process is simple and low in cost.

[0006] The present invention also provides a positive electrode sheet comprising the above-mentioned lithium iron phosphate material or lithium iron phosphate material prepared according to the above-mentioned method for preparing lithium iron phosphate material. Therefore, when this positive electrode sheet is applied to a battery, it can improve the specific capacity and energy efficiency of the battery.

[0007] The present invention also provides a battery comprising the above-mentioned positive electrode, thereby the battery having a high specific capacity and energy efficiency.

[0008] In a first aspect, the present invention provides a lithium iron phosphate material, comprising a lithium iron phosphate matrix and a fluorosilicon carbon coating layer present on the surface of the lithium iron phosphate matrix.

[0009] The lithium iron phosphate material described above has a carbon content of 1.05%-1.35% by mass.

[0010] And / or, the fluorosilicon-carbon coating layer accounts for 1.11%-1.64% of the mass percentage of the lithium iron phosphate material.

[0011] The lithium iron phosphate material described above further includes titanium, and the content of titanium increases along the direction from the lithium iron phosphate matrix to the fluorosilicon carbon coating layer.

[0012] The lithium iron phosphate material described above has a titanium content of 1000ppm-6000ppm by mass.

[0013] The lithium iron phosphate material described above has a Dv50 of 300nm-1300nm, preferably 500nm-1000nm;

[0014] And / or, the specific surface area of ​​the lithium iron phosphate material is 9m². 2 / g-15m 2 / g, preferably 11m 2 / g-14m 2 / g;

[0015] And / or, the particle size distribution (SPAN) of the lithium iron phosphate material is 2.5-4.

[0016] Secondly, the present invention provides a method for preparing the lithium iron phosphate material as described above, comprising the following steps:

[0017] 1) Under an inert atmosphere, the first system, including an iron source, a phosphorus source, a lithium source, and a first carbon source, is subjected to a first sintering process to obtain a first sintered material;

[0018] 2) Under an inert atmosphere, the second system, including the primary sintering material, fluorinated siloxane, and the second carbon source, is subjected to a secondary sintering treatment to obtain the lithium iron phosphate material.

[0019] In the preparation method of lithium iron phosphate material as described above, the fluorinated siloxane accounts for 0.1%-5% of the mass percentage of the second system, preferably 0.5%-3%.

[0020] And / or, the fluorinated siloxane comprises at least one of (3,3,3-trifluoropropyl)cyclopolysiloxane methyl ester, poly(methyl-3,3,3-trifluoropropyl)siloxane, tetramethyltri-3-trifluoropropylcyclotetrasiloxane, perfluorooctylethyltrisiloxane, hexacarbon perfluoropolyether trimethoxysilane, trifluoropropyltris(dimethylsiloxane)silane, and bis(nonafluorohexyl)tetramethyldisiloxane.

[0021] In the preparation method of lithium iron phosphate material as described above, the molar ratio of lithium element in the lithium source to iron element in the iron source is (1.02-1.10):1;

[0022] And / or, the molar ratio of iron in the iron source to phosphorus in the phosphorus source is (0.96-0.985):1;

[0023] And / or, the first carbon source accounts for 0.5%-5% of the mass percentage of the first system;

[0024] And / or, the second carbon source accounts for 0.5%-5% of the mass of the second system;

[0025] And / or, the temperature of the first sintering treatment is 500℃-800℃, and the time is 3h-10h;

[0026] And / or, the temperature of the secondary sintering treatment is 650℃-790℃, and the time is 5h-12h.

[0027] The method for preparing lithium iron phosphate material as described above further includes additives in the first system;

[0028] The additive includes at least one of compounds containing Ti, V, Nb, Mg, W, and Y, preferably including compounds containing Ti;

[0029] And / or, the additive accounts for 0.1%-2% of the mass percentage of the first system;

[0030] And / or, the second system further includes a titanium source;

[0031] The titanium source includes at least one of bis(acetylacetonyl)diisopropoxytitanate, tetrabutyl titanate, and tetra(trimethylsiloxy)titanium.

[0032] And / or, the titanium source accounts for 0.2%-2% of the mass percentage of the second system.

[0033] The lithium iron phosphate material preparation method described above, wherein the lithium source includes at least one of lithium carbonate, lithium hydroxide, lithium phosphate, lithium dihydrogen phosphate, and lithium acetate;

[0034] And / or, the iron source includes at least one of ferric oxide, ferric oxide, ferric hydroxyl oxide, and ferric nitrate;

[0035] And / or, the phosphorus source includes at least one of phosphoric acid, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, lithium phosphate, and lithium dihydrogen phosphate;

[0036] And / or, the first carbon source includes at least one of glucose, sucrose, fructose, starch, polyethylene glycol, polyvinylpyrrolidone, and polyvinyl alcohol;

[0037] And / or, the second carbon source includes at least one of glucose, sucrose, fructose, starch, polyethylene glycol, polyvinylpyrrolidone, and polyvinyl alcohol.

[0038] Thirdly, the present invention provides a positive electrode sheet comprising the lithium iron phosphate material as described above or the lithium iron phosphate material prepared according to the preparation method of the lithium iron phosphate material as described above.

[0039] Fourthly, the present invention provides a battery comprising the positive electrode sheet as described above.

[0040] The lithium iron phosphate material provided by this invention has a fluorosilicon-carbon coating layer on the surface of the lithium iron phosphate matrix. This fluorosilicon-carbon coating layer enhances the bonding force between lithium iron phosphate particles, which helps reduce voids between particles during compaction, thereby increasing the compaction density of the material. Furthermore, the fluorosilicon-carbon coating layer forms a stable interface layer, reducing the interfacial impedance between the electrode and the electrolyte, which helps reduce polarization effects in electrochemical reactions, thus improving the specific capacity and energy efficiency of the battery. Attached Figure Description

[0041] To more clearly illustrate the technical solutions in the embodiments of the present invention or related technologies, the accompanying drawings used in the description of the embodiments of the present invention or related technologies are briefly introduced below. Obviously, the drawings described below are merely some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0042] Figure 1 Here is a SEM image of the lithium iron phosphate material of Example 1 of the present invention;

[0043] Figure 2 The image shows the XRD pattern of the lithium iron phosphate material in Example 1 of this invention.

[0044] Figure 3 This is a particle size distribution diagram of the lithium iron phosphate material in Example 1 of the present invention;

[0045] Figure 4 This is an EDS scan pattern of the lithium iron phosphate material in Example 1 of the present invention;

[0046] Figure 5 This is an EDS test image of the lithium iron phosphate material in Example 1 of the present invention;

[0047] Figure 6 This is an XPS test image of the lithium iron phosphate material in Example 1 of the present invention. Detailed Implementation

[0048] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions in the embodiments of this invention will be clearly and completely described below in conjunction with the embodiments of this invention. Obviously, the described embodiments are only some embodiments of this invention, not all embodiments. Based on the embodiments of this invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this invention.

[0049] With increasing global emphasis on sustainable development and environmental protection, the development and utilization of green energy has become particularly important. The non-renewable nature of fossil fuels and their environmental pollution have spurred the search for alternative energy sources. Green energy, such as solar, wind, and hydropower, has attracted significant attention due to its clean and renewable characteristics. However, these energy sources are intermittent and unstable, thus requiring efficient energy storage systems to balance supply and demand and ensure a stable energy supply.

[0050] Lithium-ion batteries are an ideal choice for energy storage systems due to their high voltage, excellent energy density, long cycle life, and wide operating temperature range. Among them, lithium iron phosphate (LiFePO4), as a cathode material, has attracted widespread research and attention due to its low cost, environmental friendliness, and high safety. LiFePO4 possesses a stable operating voltage platform and excellent thermal stability, resulting in outstanding performance in safety and cycle life. However, the low compaction density of existing lithium iron phosphate materials limits the specific capacity and energy efficiency of the batteries.

[0051] The inventors of this application have discovered that by coating the surface of lithium iron phosphate particles with a fluorosilicon-carbon coating layer, the compaction density of lithium iron phosphate materials can be significantly improved, thereby increasing the specific capacity and energy efficiency of the battery.

[0052] Based on this, in a first aspect, the present invention provides a lithium iron phosphate material, comprising a lithium iron phosphate matrix and a fluorosilicon carbon coating layer present on the surface of the lithium iron phosphate matrix.

[0053] It is understood that the fluorosilicon-carbon coating layer in this invention refers to a coating layer including fluorine, silicon and carbon elements.

[0054] The lithium iron phosphate material provided by this invention features a fluorosilicon-carbon coating layer on the surface of the lithium iron phosphate matrix, which increases the compaction density of the lithium iron phosphate material, thereby improving the specific capacity and energy efficiency of the battery. The reason for this is that the fluorosilicon-carbon coating layer enhances the bonding force between lithium iron phosphate particles, reducing voids between particles during compaction and thus increasing the material's compaction density. Furthermore, the fluorosilicon-carbon coating layer provides a conductive network, reducing the material's internal resistance. This conductive network not only improves electron transport efficiency but also allows for denser particle packing, further increasing the material's compaction density. In addition, the fluorosilicon-carbon coating layer forms a stable interface layer, reducing the interfacial impedance between the electrode and electrolyte, which helps reduce polarization effects in electrochemical reactions. The introduction of fluorine and silicon can suppress side reactions between the electrode material and the electrolyte, reducing polarization caused by side reactions and improving the battery's specific capacity and energy efficiency. Simultaneously, the coating layer improves the structural stability of the lithium iron phosphate material, reducing structural degradation caused by volume changes during charge and discharge, helping to maintain a low polarization state and improving the battery's cycle performance.

[0055] Therefore, the lithium iron phosphate material provided by the present invention can improve the compaction density of the lithium iron phosphate material by setting a fluorosilicon carbon coating layer on the surface of the lithium iron phosphate matrix, thereby improving the specific capacity and energy efficiency of the battery.

[0056] In some embodiments of the present invention, the mass percentage of carbon in the lithium iron phosphate material is 1.05%-1.35%, for example, it can be a range of 1.05%, 1.10%, 1.15%, 1.20%, 1.25%, 1.30%, 1.35% or any combination thereof.

[0057] The lithium iron phosphate material of the present invention has a carbon content within the above-mentioned range, which can improve the electronic conductivity of the lithium iron phosphate material, thus improving the rate performance and energy efficiency of the battery. It can also reduce the internal resistance of the electrode, reduce polarization effects, and improve the specific capacity and cycle life of the battery. Furthermore, carbon can improve the interfacial compatibility between lithium iron phosphate and the electrolyte, reduce the occurrence of side reactions, and improve the coulombic efficiency and stability of the battery.

[0058] In some embodiments of the present invention, the fluorosilicon carbon coating layer accounts for 1.11%-1.64% of the mass percentage of the lithium iron phosphate material, for example, it can be a range of 1.11%, 1.15%, 1.2%, 1.25%, 1.3%, 1.35%, 1.4%, 1.5%, 1.6%, 1.64%, or any combination thereof.

[0059] An appropriate amount of fluorosilicon-carbon coating can form a stable and uniform interface on the material surface, reducing interfacial reactions and impedance between the electrode and the electrolyte, which is beneficial to improving the cycle life and energy efficiency of the battery. Furthermore, this coating can buffer the volume changes of the material during charging and discharging, reducing structural degradation caused by volume expansion or contraction, thereby improving the mechanical stability and cycle performance of the material.

[0060] In some embodiments of the present invention, the lithium iron phosphate material further includes titanium, and the content of titanium increases along the direction from the lithium iron phosphate matrix to the fluorosilicon carbon coating layer.

[0061] In this invention, the enrichment of titanium on the surface of lithium iron phosphate material can improve surface conductivity, especially when combined with a fluorosilicon-carbon coating layer, forming a more efficient electron transport path, which helps reduce the battery's internal resistance and improve rate performance. Furthermore, the presence of titanium can enhance the interfacial compatibility between lithium iron phosphate and the coating layer, reducing interfacial stress and side reactions, and improving the battery's cycle stability and lifespan. In addition, titanium can promote ion insertion and extraction processes, improving the electrochemical reaction kinetics of the material, thereby increasing the battery's specific capacity and energy efficiency.

[0062] In some embodiments of the present invention, the mass percentage of titanium in the lithium iron phosphate material is 1000ppm-6000ppm, for example, it can be a range of 1000ppm, 2000ppm, 3000ppm, 4000ppm, 5000ppm, 6000ppm or any two of these.

[0063] In this invention, the mass percentage of titanium in the lithium iron phosphate material is within the above-mentioned range, which can further improve the specific capacity and energy efficiency of the battery.

[0064] In some embodiments of the present invention, the Dv50 of the lithium iron phosphate material is 300nm-1300nm, for example, it can be a range of 300nm, 400nm, 500nm, 600nm, 700nm, 800nm, 900nm, 1000nm, 1100nm, 1200nm, 1300nm or any two of these, preferably 500nm-1000nm.

[0065] It is understandable that Dv50 is the particle size corresponding to a cumulative volume distribution percentage of 50% for lithium iron phosphate materials.

[0066] The lithium iron phosphate material of this invention has a Dv50 within the aforementioned range, which can improve the electron and ion transport rate, reduce the battery's internal resistance and polarization, and achieve a higher compaction density, thereby increasing the battery's specific capacity. Simultaneously, it helps maintain the material's structural stability during charge and discharge, reducing material pulverization or electrode structure degradation caused by volume changes.

[0067] The Dv50 of the lithium iron phosphate material in this invention can be tested using a Malvern 3000 laser particle size analyzer.

[0068] In some embodiments, the specific surface area of ​​the lithium iron phosphate material is 9m². 2 / g-15m 2 / g, for example, can be 9m 2 / g, 10m 2 / g、11m 2 / g、12m 2 / g、13m 2 / g、14m 2 / g, 15m 2 The range of / g or any two thereof, preferably 11m 2 / g-14m 2 / g.

[0069] As we understand it, specific surface area is the total surface area of ​​particles per unit volume or unit mass. The specific surface area of ​​lithium iron phosphate materials directly affects the capacity utilization of their active materials, and thus affects the rate and cycle performance of the battery.

[0070] In this invention, the specific surface area of ​​the lithium iron phosphate material is within the above-mentioned range, the number of active sites on the material surface increases, the interfacial impedance of the material decreases, which is conducive to the insertion of active ions (such as lithium ions), reduces the electrochemical polarization of the material, and allows for high capacity utilization, thereby improving the rate performance and cycle performance of the battery.

[0071] In some embodiments, the particle size distribution SPAN of the lithium iron phosphate material is 2.5-4, for example, it can be a range of 2.5, 2.7, 2.9, 3, 3.5, 4 or any two of them.

[0072] In this invention, the particle size distribution SPAN of lithium iron phosphate material can be calculated according to the formula (Dv90-Dv10) / Dv50, where Dv10 is the particle size corresponding to a cumulative volume distribution percentage of 10% for lithium iron phosphate material; Dv50 is the particle size corresponding to a cumulative volume distribution percentage of 50% for lithium iron phosphate material; and Dv90 is the particle size corresponding to a cumulative volume distribution percentage of 90% for lithium iron phosphate material.

[0073] The lithium iron phosphate material in this invention has a suitable particle size distribution, which can improve the compaction density of the material and also help ensure that the stress on the particles is more uniform, avoid particle cracking, and further improve the specific capacity and energy efficiency of the battery.

[0074] In this invention, the Dv10 and Dv90 of the lithium iron phosphate material can also be tested using a Malvern 3000 laser particle size analyzer.

[0075] Secondly, the present invention provides a method for preparing the lithium iron phosphate material as described above, comprising the following steps:

[0076] 1) Under an inert atmosphere, the first system, including an iron source, a phosphorus source, a lithium source, and a first carbon source, is subjected to a first sintering process to obtain a first sintered material;

[0077] 2) Under an inert atmosphere, a second system consisting of primary sintering material, fluorinated siloxane, and a second carbon source is subjected to a secondary sintering treatment to obtain lithium iron phosphate material.

[0078] Specifically, in step 1), the inert atmosphere can be a nitrogen atmosphere, which is beneficial for removing impurities, promoting the crystallization of lithium iron phosphate, forming a stable olivine structure, and ensuring the uniform distribution of iron, phosphorus, lithium, and carbon elements in the material.

[0079] In specific implementation, iron source, phosphorus source, lithium source, first carbon source and deionized water can be uniformly mixed, and then the mixed slurry can be sand-milled and sprayed, and sintered in one step to obtain a one-time sintered material. Among them, sand milling includes coarse grinding and fine grinding. Coarse grinding can be carried out using a basket mill, and the coarse grinding time can be 30min-100min, preferably 40min-70min; fine grinding can be carried out using a pin mill, and the fine grinding time can be 60min-180min, preferably 60min-100min, and the fine grinding particle size can be 300nm-500nm, preferably 350nm-450nm.

[0080] In the first system, the first carbon source plays a reducing role, preventing ferrous iron from being oxidized to ferric iron.

[0081] In step 2), the inert atmosphere can be nitrogen. Fluorosiloxane and the second carbon source decompose and deposit on the surface of lithium iron phosphate particles during secondary sintering, forming a fluorosilicon-carbon coating layer, which improves the material's conductivity and interfacial stability. Carbon provides an effective electron transport channel, reducing the material's internal resistance and improving the battery's rate performance. The introduction of fluorine and silicon enhances the material's chemical resistance and thermal stability, reduces side reactions with the electrolyte, and improves battery safety and lifespan. Furthermore, the coating layer improves the interfacial compatibility between the electrode and the electrolyte, reduces interfacial impedance, and increases the battery's specific capacity and energy efficiency.

[0082] In a specific embodiment, the primary sintering material, fluorinated siloxane, and the second carbon source are dispersed in an organic solvent, followed by sand milling and spraying, secondary sintering, and air jet milling to obtain fluorosilicon-carbon coated lithium iron phosphate material. The organic solvent includes at least one of methanol, ethanol, and dimethyl carbonate. Air jet milling can be performed using an air jet mill, with the classifier wheel frequency of the air jet mill being 75Hz-140Hz, preferably 85Hz-130Hz.

[0083] The method for preparing lithium iron phosphate material provided by the present invention can prepare the lithium iron phosphate material provided in the first aspect above, and the material has a large compaction density, which can improve the specific capacity and energy efficiency of the battery.

[0084] In some embodiments of the present invention, the fluorinated siloxane accounts for 0.1%-5% of the mass percentage of the second system, for example, it can be a range of 0.1%, 0.5%, 1%, 2%, 3%, 4%, 5% or any two of these, preferably 0.5%-3%.

[0085] In some embodiments, fluorinated siloxanes include at least one of (3,3,3-trifluoropropyl)cyclopolysiloxane methyl ester, poly(methyl-3,3,3-trifluoropropyl)siloxane, tetramethyltri-3-trifluoropropylcyclotetrasiloxane, perfluorooctylethyltrisiloxane, hexacarbon perfluoropolyether trimethoxysilane, trifluoropropyltris(dimethylsiloxane)silane, and bis(nonafluorohexyl)tetramethyldisiloxane.

[0086] In this invention, the content and type of fluorinated siloxanes within the aforementioned range can optimize the interfacial compatibility between lithium iron phosphate and the electrolyte, reduce interfacial impedance, and improve the specific capacity and energy efficiency of the battery. It can also improve the thermal stability of the material, reduce decomposition and performance degradation under high-temperature conditions, and thus enhance battery safety.

[0087] In some embodiments of the present invention, the molar ratio of lithium in the lithium source to iron in the iron source is (1.02-1.10):1, for example, it can be a range of 1.02:1, 1.03:1, 1.04:1, 1.05:1, 1.06:1, 1.07:1, 1.08:1, 1.09:1, 1.10:1 or any two of them, preferably (1.04-1.08):1.

[0088] An excess of lithium relative to iron can compensate for potential lithium loss during high-temperature sintering, ensuring sufficient lithium in the final product and improving the material's electrochemical performance and capacity. It also helps optimize the material's crystal structure, promoting lithium-ion transport and enhancing the battery's rate performance.

[0089] In some embodiments, the molar ratio of iron in the iron source to phosphorus in the phosphorus source is (0.96-0.985):1, for example, it can be a range of 0.96:1, 0.965:1, 0.97:1, 0.975:1, 0.98:1, 0.985:1 or any two of them, preferably (0.965-0.98):1.

[0090] A slight excess of phosphorus ensures the formation of a complete lithium iron phosphate structure, reduces phosphorus defects, and improves the structural integrity and cycle stability of the material. By controlling the molar ratio of iron to phosphorus, the formation of impurity phases can be reduced, thereby improving the purity and electrochemical performance of the material.

[0091] In some embodiments, the first carbon source accounts for 0.5%-5% of the mass percentage of the first system, for example, it can be a range of 0.5%, 1%, 2%, 3%, 4%, 5% or any two of these, preferably 1%-3.5%.

[0092] In this invention, the appropriate content of the first carbon source effectively prevents ferrous iron from being oxidized to ferric iron, thereby maintaining the stoichiometry and structural integrity of lithium iron phosphate. Furthermore, the first carbon source can be partially converted into a conductive carbon network during sintering, enhancing the overall conductivity of the material and improving the battery's rate performance and charge / discharge efficiency.

[0093] In some embodiments, the second carbon source accounts for 0.5%-5% of the mass percentage of the second system, for example, it can be a range of 0.5%, 1%, 2%, 3%, 4%, 5% or any two of these, preferably 1%-3.5%.

[0094] An appropriate amount of secondary carbon source can improve the electronic conductivity of lithium iron phosphate materials, which is beneficial for reducing the battery's internal resistance and improving rate performance and energy efficiency. It can also improve the electrochemical reaction kinetics of the electrodes, reduce polarization effects, and thus improve the battery's specific capacity and cycle life.

[0095] In some embodiments, the temperature of the first sintering process is 500℃-800℃, for example, it can be a range of 500℃, 550℃, 600℃, 650℃, 700℃, 750℃, 800℃ or any two of them, preferably 600℃-800℃; the time is 3h-10h, for example, it can be a range of 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h or any two of them, preferably 4h-9h.

[0096] When the temperature and time of the primary sintering process are within the above-mentioned range, the primary sintered material can fully crystallize and form a stable olivine structure. Appropriate primary sintering temperature and time are beneficial for controlling particle size and morphology, providing a suitable matrix for subsequent coating processes.

[0097] In some embodiments, the temperature of the secondary sintering treatment is 650℃-790℃, for example, it can be a range of 650℃, 670℃, 690℃, 700℃, 720℃, 750℃, 790℃ or any two of them, preferably 680℃-780℃; the time is 5h-12h, for example, it can be a range of 5h, 6h, 7h, 8h, 9h, 10h, 11h, 12h or any two of them, preferably 6h-10h.

[0098] When the temperature and time of the secondary sintering process are within the aforementioned range, the fluorinated siloxane and the second carbon source can be effectively decomposed and form a uniform coating layer on the material surface, which can significantly improve the conductivity and interfacial stability of the material. It also helps to improve the mechanical strength, chemical stability, and thermal stability of the material, thereby enhancing the safety and lifespan of the battery.

[0099] In some embodiments of the present invention, the first system further includes additives; the additives include at least one compound containing Ti, V, Nb, Mg, W, and Y. These elements can enter the crystal lattice of lithium iron phosphate, acting as dopant and enhancing the crystal structure stability of the material. They can also improve the electrochemical reaction kinetics of the material, increasing the specific capacity and cycle life of the battery.

[0100] In some embodiments, the additive accounts for 0.1%-2% of the mass percentage of the first system, for example, it can be a range of 0.1%, 0.3%, 0.5%, 0.7%, 1%, 1.2%, 1.5%, 2%, or any two thereof, preferably 0.5%-1%. An appropriate amount of additive can reduce the formation of undesirable impurities and improve the purity and consistency of the material.

[0101] In some embodiments, the second system further includes a titanium source; the titanium source accounts for 0.2%-2% of the mass percentage of the second system, for example, it can be a range of 0.2%, 0.3%, 0.5%, 0.7%, 1%, 1.2%, 1.5%, 2% or any two of these, preferably 0.4%-2%.

[0102] Specifically, the titanium source can be selected from at least one of organotitanium such as bis(acetylacetonyl)diisopropoxytitanate, tetrabutyl titanate, and tetra(trimethylsiloxy)titanium.

[0103] Titanium sources can accumulate on the material surface during secondary sintering, enhancing surface chemical stability. They can also improve the interfacial compatibility between lithium iron phosphate and the coating layer, reducing interfacial impedance and increasing battery energy efficiency. The introduction of an appropriate amount of titanium source can synergistically enhance the conductive network of the material with the coating layer, further improving the overall battery performance.

[0104] In some embodiments of the present invention, the additives include Ti-containing compounds.

[0105] When additives include Ti-containing compounds, the titanium content can increase along the direction from the lithium iron phosphate matrix to the fluorosilicon-carbon coating layer, resulting in a gradient distribution of titanium. This improves the material's conductivity and enhances the battery's rate performance. Furthermore, it strengthens the crystal structure stability of lithium iron phosphate, reducing volume changes and structural degradation during charge and discharge, thus extending the battery's cycle life.

[0106] In some embodiments of the present invention, the lithium source includes at least one of lithium carbonate, lithium hydroxide, lithium phosphate, lithium dihydrogen phosphate, and lithium acetate.

[0107] In some embodiments, the iron source includes at least one of ferric oxide, iron tetroxide, ferric hydroxide, and ferric nitrate.

[0108] In some embodiments, the phosphorus source includes at least one of phosphoric acid, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, lithium phosphate, and lithium dihydrogen phosphate.

[0109] In some embodiments, the first carbon source includes at least one of glucose, sucrose, fructose, starch, polyethylene glycol, polyvinylpyrrolidone, and polyvinyl alcohol.

[0110] In some embodiments, the second carbon source includes at least one of glucose, sucrose, fructose, starch, polyethylene glycol, polyvinylpyrrolidone, and polyvinyl alcohol.

[0111] The aforementioned lithium source, iron source, phosphorus source, first carbon source, and second carbon source can enable the effective preparation of lithium iron phosphate materials.

[0112] Thirdly, the present invention provides a positive electrode sheet comprising the lithium iron phosphate material as described above or the lithium iron phosphate material prepared according to the preparation method of the lithium iron phosphate material as described above.

[0113] The positive electrode sheet of the present invention can be prepared using conventional techniques in the art. Specifically, the above-mentioned lithium iron phosphate material, conductive agent, and binder can be uniformly dispersed in a solvent to obtain a positive electrode active layer slurry. Then, the positive electrode active layer slurry is coated on at least one functional surface of the positive electrode current collector, and after drying, the positive electrode sheet of the present invention can be obtained.

[0114] This invention does not specifically limit the types of conductive agents and adhesives. The conductive agents, adhesives and other components can all be conventional substances in the field. For example, the conductive agent can be selected from one or more of conductive carbon black, carbon nanotubes, conductive graphite and graphene, and the adhesive can be selected from one or more of polyvinylidene fluoride (PVDF), acrylic modified PVDF, polyacrylate polymers, polyimide, styrene-butadiene rubber and styrene-acrylic rubber.

[0115] The present invention does not specifically limit the coating method, and any coating method such as gravure coating, extrusion coating, spraying, screen printing, etc. can be used to achieve the coating of the positive electrode active layer slurry.

[0116] The positive electrode provided by the present invention includes the above-mentioned lithium iron phosphate material. Therefore, when the positive electrode is applied to a battery, the specific capacity and energy efficiency of the battery can be improved.

[0117] Fourthly, the present invention provides a battery comprising the positive electrode sheet as described above, which has advantages corresponding to the positive electrode sheet described above, and will not be elaborated further.

[0118] In addition to the positive electrode, the battery of the present invention also includes a separator, a negative electrode, and an electrolyte. The composition of the negative electrode can refer to conventional negative electrode sheets in the art, and the separator can also be a separator commonly used in the art, such as a PP film or a PE film.

[0119] The battery of the present invention can be prepared using conventional methods in the art. Specifically, the positive electrode, separator and negative electrode can be stacked in sequence, and the cell can be obtained by stacking or winding. Then, the battery can be obtained by baking, liquid injection, formation and packaging.

[0120] The battery of the present invention may be in the form of a battery cell, a battery module, or a battery pack. In some embodiments, battery cells may be assembled into a battery module, and the number of battery cells contained in a battery module may be one or more, the specific number of which can be selected by those skilled in the art according to the application and capacity of the battery module. In some embodiments, battery modules may also be assembled into a battery pack, and the number of battery modules contained in a battery pack may be one or more, the specific number of which can be selected by those skilled in the art according to the application and capacity of the battery pack.

[0121] The specific type of battery of this invention is not particularly limited. For example, from the perspective of shape, the battery includes, but is not limited to, prismatic batteries, pouch batteries, and cylindrical batteries, etc., and this invention does not impose any particular limitations on any of them. From the perspective of the core structure, the core of this battery can be a wound core (i.e., a core formed by stacking positive electrode sheets, negative electrode sheets, and separators and then winding them) or a stacked core (i.e., multiple positive electrode sheets, negative electrode sheets, and separators are stacked to form a core). The outer shell can be a hard shell (such as a steel shell, a hard plastic shell, etc.) or a soft shell (such as an aluminum-plastic film, a pouch-type soft shell, etc.). This application does not impose any particular limitations on any of these.

[0122] The technical solution of the present invention will be further described below with reference to specific embodiments.

[0123] Example 1

[0124] The preparation method of lithium iron phosphate material in this embodiment includes the following steps:

[0125] 1) Weigh out ferric oxide, ammonium dihydrogen phosphate, lithium carbonate, glucose, PEG2000, and titanium dioxide sequentially, and add them to deionized water to form the first system. The molar ratio of Fe to P is 0.97:1, the molar ratio of Li to Fe is 1.05:1, the additive (titanium dioxide) accounts for 1.8% of the mass of the first system, and the first carbon source (glucose and PEG2000) accounts for 1.27% of the mass of the first system. Mill the first system in a basket mill for 50 minutes. Then, pump the slurry into a pin mill and mill for 70 minutes to obtain a slurry with a particle size Dv50 of 400 nm and a solid content of 40.79%.

[0126] 2) Spray dry the slurry obtained in step 1), and sinter the obtained spray material in a nitrogen atmosphere furnace. The temperature of the first sintering treatment is 750℃, and the reaction is kept at a constant temperature for 6 hours. After the temperature drops to room temperature, the sintered material is crushed and sieved to obtain the first sintered material.

[0127] 3) Weigh out the primary sintering material, glucose, PEG2000, tetramethyltri-3-trifluoropropylcyclotetrasiloxane, and tetrabutyl titanate sequentially, and disperse them in methanol to form a second system. The fluorinated siloxane (tetramethyltri-3-trifluoropropylcyclotetrasiloxane) accounts for 0.64% of the mass of the second system, the second carbon source (glucose and PEG2000) accounts for 2.58% of the mass of the second system, and the titanium source (tetrabutyl titanate) accounts for 1.03% of the mass of the second system. Mill the second system in a sand mill for 60 minutes until Dv50 = 650 nm.

[0128] 4) The slurry obtained in step 3) is spray-dried, and then subjected to secondary sintering in a nitrogen atmosphere furnace at 720℃ for 8 hours. After the temperature drops to room temperature, the secondary sintered material is subjected to air jet milling with the classifier wheel frequency adjusted to 95Hz to obtain lithium iron phosphate material. The lithium iron phosphate material includes a lithium iron phosphate matrix and a fluorosilicon-carbon coating layer on the surface of the lithium iron phosphate matrix. The lithium iron phosphate material also includes titanium, with the titanium content increasing from the lithium iron phosphate matrix to the fluorosilicon-carbon coating layer.

[0129] Example 2

[0130] The preparation method of lithium iron phosphate material in this embodiment includes the following steps:

[0131] 1) Weigh out iron(III) oxide, phosphoric acid, lithium carbonate, glucose, PEG2000, and titanium dioxide sequentially, and add them to deionized water to form the first system. The molar ratio of Fe to P is 0.96:1, the molar ratio of Li to Fe is 1.07:1, the additive (titanium dioxide) accounts for 1.5% of the mass of the first system, and the first carbon source (glucose and PEG2000) accounts for 1.21% of the mass of the first system. Mill the first system in a basket mill for 45 minutes. Then, transfer the slurry to a pin mill and mill for 75 minutes to obtain a slurry with a particle size Dv50 of 350 nm and a solid content of 41.02%.

[0132] 2) Spray dry the slurry obtained in step 1), and sinter the obtained spray material in a nitrogen atmosphere furnace. The temperature of the first sintering treatment is 760℃, and the reaction is kept at a constant temperature for 6 hours. After the temperature drops to room temperature, the sintered material is crushed and sieved to obtain the first sintered material.

[0133] 3) Weigh out the primary sintering material, glucose, PEG2000, (3,3,3-trifluoropropyl)cyclopolysiloxane methyl ester, and bis(acetylacetonyl)diisopropoxytitanate in sequence, and disperse them in methanol to form a second system. The fluorinated siloxane ((3,3,3-trifluoropropyl)cyclopolysiloxane methyl ester) accounts for 0.71% of the mass of the second system, the second carbon source (glucose and PEG2000) accounts for 2.55% of the mass of the second system, and the titanium source (bis(acetylacetonyl)diisopropoxytitanate) accounts for 1.27% of the mass of the second system. Mill the second system in a sand mill for 55 minutes until Dv50 = 650 nm.

[0134] 4) The slurry obtained in step 3) is spray-dried, and then subjected to secondary sintering in a nitrogen atmosphere furnace at 740℃ for 9 hours. After the temperature drops to room temperature, the sintered material is subjected to air jet milling with the classifier wheel frequency adjusted to 115Hz to obtain lithium iron phosphate material. The lithium iron phosphate material includes a lithium iron phosphate matrix and a fluorosilicon-carbon coating layer on the surface of the lithium iron phosphate matrix. The lithium iron phosphate material also includes titanium, with the titanium content increasing from the lithium iron phosphate matrix to the fluorosilicon-carbon coating layer.

[0135] Example 3

[0136] The preparation method of lithium iron phosphate material in this embodiment includes the following steps:

[0137] 1) Weigh out iron hydroxide, diammonium hydrogen phosphate, lithium carbonate, starch, polyvinyl alcohol, and titanium dioxide sequentially, and add them to deionized water to form the first system. The molar ratio of Fe to P is 0.985:1, the molar ratio of Li to Fe is 1.10:1, the additive (titanium dioxide) accounts for 1.75% of the mass of the first system, and the first carbon source (starch and polyvinyl alcohol) accounts for 1.19% of the mass of the first system. Mill the first system in a basket mill for 80 minutes. Then, pump the slurry into a pin mill and mill for 150 minutes to obtain a slurry with a particle size Dv50 of 450 nm and a solid content of 40.48%.

[0138] 2) Spray dry the slurry obtained in step 1), and sinter the obtained spray material in a nitrogen atmosphere furnace. The temperature of the first sintering treatment is 780℃, and the reaction is kept at a constant temperature for 6 hours. After the temperature drops to room temperature, the sintered material is crushed and sieved to obtain the first sintered material.

[0139] 3) Weigh out the primary sintering material, glucose, PEG2000, polyvinyl alcohol, trifluoropropyltris(dimethylsiloxane)silane, and tetra(trimethylsiloxy)titanium in sequence, and disperse them in methanol to form a second system. The fluorinated siloxane (trifluoropropyltris(dimethylsiloxane)silane) accounts for 0.76% of the mass of the second system, the second carbon source (glucose, PEG2000, and polyvinyl alcohol) accounts for 2.69% of the mass of the second system, and the titanium source (tetra(trimethylsiloxy)titanium) accounts for 1.27% of the mass of the second system. Mill the second system in a sand mill for 55 minutes until Dv50 = 650 nm.

[0140] 4) The slurry obtained in step 3) is spray-dried, and then subjected to secondary sintering in a nitrogen atmosphere furnace at 790℃ for 6 hours. After the temperature drops to room temperature, the sintered material is subjected to air jet milling with the classifier wheel frequency adjusted to 120Hz to obtain lithium iron phosphate material. The lithium iron phosphate material includes a lithium iron phosphate matrix and a fluorosilicon-carbon coating layer on the surface of the lithium iron phosphate matrix. The lithium iron phosphate material also includes titanium, with the titanium content increasing from the lithium iron phosphate matrix to the fluorosilicon-carbon coating layer.

[0141] Example 4

[0142] The preparation method of lithium iron phosphate material in this embodiment includes the following steps:

[0143] 1) Weigh out ferric nitrate nonahydrate, lithium dihydrogen phosphate, fructose, polyvinylpyrrolidone, and titanium dioxide sequentially, and add them to deionized water to form the first system. The molar ratio of Fe to P is 0.98:1, the molar ratio of Li to Fe is 1.02:1, the additive (titanium dioxide) accounts for 2.0% of the mass of the first system, and the first carbon source (fructose and polyvinylpyrrolidone) accounts for 1.9% of the mass of the first system. Mill the first system in a basket mill for 30 minutes. Then, pump the slurry into a pin mill and mill for 160 minutes to obtain a slurry with a particle size Dv50 of 300 nm and a solid content of 39.8%.

[0144] 2) Spray dry the slurry obtained in step 1), and sinter the obtained spray material in a nitrogen atmosphere furnace. The temperature of the first sintering treatment is 770℃, and the reaction is kept at a constant temperature for 6 hours. After the temperature drops to room temperature, the sintered material is crushed and sieved to obtain the first sintered material.

[0145] 3) Weigh out the primary sintering material, glucose, PEG2000, polyvinylpyrrolidone, bis(nonafluorohexyl)tetramethyldisiloxane, and bis(acetylacetonyl)diisopropoxytitanate sequentially, and disperse them in methanol to form a second system. The fluorinated siloxane (bis(nonafluorohexyl)tetramethyldisiloxane) accounts for 0.64% of the mass of the second system, the second carbon source (glucose, PEG2000, and polyvinylpyrrolidone) accounts for 2.05% of the mass of the second system, and the titanium source (bis(acetylacetonyl)diisopropoxytitanate) accounts for 1.03% of the mass of the second system. Mill the second system in a sand mill for 60 minutes until Dv50 = 650 nm.

[0146] 4) The slurry obtained in step 3) is spray-dried, and then subjected to secondary sintering in a nitrogen atmosphere furnace at a temperature of 787℃ for 8 hours. After the temperature drops to room temperature, the sintered material is subjected to air jet milling with the classifier wheel frequency adjusted to 125Hz to obtain lithium iron phosphate material. The lithium iron phosphate material includes a lithium iron phosphate matrix and a fluorosilicon-carbon coating layer on the surface of the lithium iron phosphate matrix. The lithium iron phosphate material also includes titanium, with the titanium content increasing from the lithium iron phosphate matrix to the fluorosilicon-carbon coating layer.

[0147] Example 5

[0148] The preparation method of lithium iron phosphate material in this embodiment is basically the same as that in Example 1, except that the mass percentage of fluorinated siloxane (tetramethyltri-3-trifluoropropylcyclotetrasiloxane) in the second system is 0.1%, and the mass percentage of the second carbon source (glucose and PEG2000) in the second system is 5%.

[0149] Example 6

[0150] The preparation method of lithium iron phosphate material in this embodiment is basically the same as that in Example 1, except that the mass percentage of fluorinated siloxane (tetramethyltri-3-trifluoropropylcyclotetrasiloxane) in the second system is 5%, and the mass percentage of the second carbon source (glucose and PEG2000) in the second system is 0.5%.

[0151] Example 7

[0152] The preparation method of lithium iron phosphate material in this embodiment is basically the same as that in Example 1, except that the titanium source (tetrabutyl titanate) accounts for 0.2% of the mass of the second system.

[0153] Example 8

[0154] The preparation method of lithium iron phosphate material in this embodiment is basically the same as that in Example 1, except that the titanium source (tetrabutyl titanate) accounts for 2% of the mass percentage of the second system.

[0155] Example 9

[0156] The preparation method of lithium iron phosphate material in Example 9 is basically the same as that in Example 1, except that the additive in step 1) is replaced with vanadium pentoxide.

[0157] Example 10

[0158] The preparation method of lithium iron phosphate material in Example 10 is basically the same as that in Example 1, except that the additive in step 1) is replaced with tungsten trioxide.

[0159] Example 11

[0160] The preparation method of lithium iron phosphate material in Example 11 is basically the same as that in Example 1, except that the amount of additive added in step 1) is changed to 0.1% of the mass percentage of the first system.

[0161] Comparative Example 1

[0162] The preparation method of the lithium iron phosphate material in this comparative example includes the following steps:

[0163] 1) Weigh out ferric oxide, ammonium dihydrogen phosphate, lithium carbonate, glucose, PEG2000, and titanium dioxide sequentially, and add them to deionized water to form the first system. The molar ratio of Fe to P is 0.97:1, the molar ratio of Li to Fe is 1.05:1, and the additive (titanium dioxide) accounts for 1.7% of the mass of the first system. Mill the first system in a basket mill for 50 minutes. Then, transfer the slurry to a pin mill and mill for 70 minutes to obtain a slurry with a particle size Dv50 of 400 nm and a solid content of 40.79%.

[0164] 2) Spray dry the slurry obtained in step 1), and sinter the obtained spray material in a nitrogen atmosphere furnace. The temperature of the first sintering treatment is 750℃, and the reaction is kept at a constant temperature for 6 hours. After the temperature drops to room temperature, the sintered material is crushed and sieved to obtain the first sintered material.

[0165] 3) Weigh out the primary sintering material, glucose, and PEG2000 sequentially, and disperse them in methanol to form a second system. The carbon source accounts for 2.60% of the mass of the second system. Mill the second system in a sand mill for 60 minutes until Dv50 = 650 nm.

[0166] 4) The slurry obtained in step 3) is spray-dried, and then subjected to secondary sintering in a nitrogen atmosphere furnace at 720℃ for 8 hours. After the temperature drops to room temperature, the secondary sintered material is subjected to air jet milling with the classifier wheel frequency adjusted to 95Hz to obtain lithium iron phosphate material. The lithium iron phosphate material includes a lithium iron phosphate matrix and a carbon coating layer on the surface of the lithium iron phosphate matrix.

[0167] Comparative Example 2

[0168] The preparation method of lithium iron phosphate material in Comparative Example 2 is basically the same as that in Example 1, except that in step 3): the primary sintering material, glucose, PEG2000, and tetrabutyl titanate are weighed sequentially and dispersed in methanol to form a second system. The second carbon source (glucose and PEG2000) accounts for 2.57% of the mass of the second system, and the titanium source (tetrabutyl titanate) accounts for 1.03% of the mass of the second system. The second system is then milled in a sand mill for 60 minutes until Dv50 = 650 nm.

[0169] Experimental example:

[0170] Using the lithium iron phosphate material prepared in the examples and comparative examples as the positive electrode active material, it was mixed with the binder polyvinylidene fluoride and the conductive agent Super P at a mass ratio of 96.5:1.5:2. N-methylpyrrolidone was added and stirred until a uniform and fluid positive electrode active slurry was formed. The positive electrode active slurry was uniformly coated on both sides of an aluminum foil with a thickness of 12 μm, and after baking, a positive electrode sheet was obtained. Using lithium metal as the negative electrode, a 2032 coin cell was assembled.

[0171] 1. Dv10, Dv50, Dv90, SPAN: The Dv10, Dv50, and Dv90 of the lithium iron phosphate material were tested using a Malvern 3000 laser particle size analyzer, and the particle size distribution of the lithium iron phosphate material was calculated using the formula SPAN = (Dv90 - Dv10) / Dv50.

[0172] 2. Carbon content: The sample is heated and burned in an oxygen stream in a high-frequency induction furnace. The generated carbon dioxide is carried by the oxygen to the measuring chamber of the infrared analyzer. Since carbon dioxide absorbs infrared energy of a specific wavelength, its absorption energy is proportional to its concentration. The carbon content of the sample can be determined by measuring the change in energy received by the detector. For specific operation, please refer to the standard: GB / T20123-2006.

[0173] 3. Titanium content: Tested using ICP-OES. For specific procedures, please refer to the standard GB / T30825-2014.

[0174] 4. Specific surface area: The specific surface area of ​​solid substances is determined by the gas adsorption BET method. For specific operation, please refer to the standard GB / T19587-2017.

[0175] 5. Compacted Density: A certain amount of lithium iron phosphate powder is placed on a compaction mold of known diameter (e.g., a Sansi Zongheng UTM7305 mold). The mold has a metal sheet at the top and bottom, with the powder placed in the middle. A pressure of 3T is applied, and the corresponding powder thickness is measured simultaneously. The compacted density is calculated using the formula ρ = m / v. Specific procedures can be performed according to standard GB / T24533-2009. Test results are shown in Table 2.

[0176] 6. Charge / Discharge Specific Capacity and Initial Coulombic Efficiency: At 25℃, charge to 3.75V at a constant power of 0.1P. The charge capacity at this point is recorded as the 0.1P charge specific capacity. After resting for 10 minutes, discharge to 2.5V at a constant power of 0.1P. The discharge capacity at this point is recorded as the 0.1P discharge specific capacity. The initial coulombic efficiency is calculated by dividing the 0.1P discharge specific capacity by the 0.1P charge specific capacity.

[0177] At 25℃, the battery is charged to 3.75V at a constant power of 0.5P. The charging capacity at this point is recorded as 1P charging specific capacity. After resting for 10 minutes, the battery is discharged to 2.5V at a constant power of 1P. The discharge capacity at this point is recorded as 1P discharge specific capacity.

[0178] 7. Energy Efficiency: The energy efficiency can be obtained by deriving the discharge specific capacity of 1P and dividing the discharge specific capacity of 1P by the discharge specific capacity at a discharge voltage of 3.2V.

[0179] Figure 1 This is a SEM image of the lithium iron phosphate material of Example 1 of the present invention.

[0180] from Figure 1 It can be seen that the lithium iron phosphate particles have a relatively smooth surface and a relatively uniform coating, and are composed of particles of different sizes.

[0181] Figure 2 The image shows the XRD pattern of the lithium iron phosphate material in Example 1 of this invention.

[0182] from Figure 2 It can be seen that the XRD pattern of the lithium iron phosphate material in Example 1 is consistent with the standard lithium iron phosphate pattern (PDF#40-1499), with no impurity peaks, indicating that the lithium iron phosphate material prepared by this method is a pure phase.

[0183] Figure 3 This is a particle size distribution diagram of the lithium iron phosphate material in Example 1 of the present invention.

[0184] from Figure 3 It can be seen that the particle size of the lithium iron phosphate material in Example 1 is between 300nm and 1300nm, and the particle size distribution shows a single-peak distribution with a maximum value of around 1000nm.

[0185] Figure 4 This is an EDS scan pattern of the lithium iron phosphate material in Example 1 of the present invention.

[0186] Figure 5 This is an EDS test image of the lithium iron phosphate material in Example 1 of the present invention.

[0187] Using an EDS spectrometer along Figure 4 Line scan tests were performed along the oblique direction to measure the elemental distribution of Li and Ti. Figure 5 As can be seen, since no lithium was added during the secondary mixing process, the Li element concentration did not change significantly on the surface or inside. However, after adding a titanium source to the secondary mixing process, Ti element doping entered the surface lithium iron phosphate during the secondary sintering process, making the surface titanium element higher than the inner titanium element. This can improve the discharge capacity.

[0188] Figure 6This is an XPS test image of the lithium iron phosphate material in Example 1 of the present invention.

[0189] from Figure 6 As can be seen from the XPS test of the lithium iron phosphate material coating layer, C-Si bonds, CC bonds, and CF bonds are found in the coating layer, indicating that fluorine, silicon, and carbon elements are present in the coating layer, achieving the effect of fluorine-silicon-carbon co-coating.

[0190] Table 1

[0191]

[0192] Table 2

[0193]

[0194] As shown in Table 1, compared with the comparative example, the lithium iron phosphate material provided by this invention has a fluorosilicon-carbon coating layer on the surface of the lithium iron phosphate matrix. This fluorosilicon-carbon coating layer enhances the bonding force between lithium iron phosphate particles, which helps reduce voids between particles during compaction, thereby increasing the compaction density of the material. Furthermore, the fluorosilicon-carbon coating layer can form a stable interface layer, reducing the interfacial impedance between the electrode and the electrolyte, which helps reduce polarization effects in electrochemical reactions, thus improving the specific capacity and energy efficiency of the battery.

[0195] Finally, it should be noted that other embodiments of the invention will readily occur to those skilled in the art upon consideration of the specification and practice of the invention disclosed herein. This invention is intended to cover any variations, uses, or adaptations of the invention that follow the general principles of the invention and include common knowledge or customary techniques in the art not disclosed herein, and is not limited to the precise structures described above and shown in the accompanying drawings, and various modifications and changes can be made without departing from its scope. The scope of the invention is limited only by the appended claims.

Claims

1. A lithium iron phosphate material, characterized in that, It includes a lithium iron phosphate matrix and a fluorosilicon carbon coating layer present on the surface of the lithium iron phosphate matrix.

2. The lithium iron phosphate material of claim 1, wherein, The mass percentage of carbon in the lithium iron phosphate material is 1.05%-1.35%; And / or, the fluorosilicon-carbon coating layer accounts for 1.11%-1.64% of the mass percentage of the lithium iron phosphate material.

3. The lithium iron phosphate material according to claim 1 or 2, characterized in that, The lithium iron phosphate material also includes titanium, and the content of titanium increases along the direction from the lithium iron phosphate matrix to the fluorosilicon carbon coating layer.

4. The lithium iron phosphate material according to claim 3, characterized in that, The mass percentage of titanium in the lithium iron phosphate material is 1000ppm-6000ppm.

5. The lithium iron phosphate material according to any one of claims 1-4, characterized in that, The Dv50 of the lithium iron phosphate material is 300nm-1300nm, preferably 500nm-1000nm; and / or the specific surface area of the lithium iron phosphate material is 9 m 2 / g to 15 m 2 / g, preferably 11 m 2 / g to 14 m 2 / g; And / or, the particle size distribution (SPAN) of the lithium iron phosphate material is 2.5-4.

6. A method for preparing lithium iron phosphate material as described in any one of claims 1-5, characterized in that, Includes the following steps: 1) Under an inert atmosphere, the first system, including an iron source, a phosphorus source, a lithium source, and a first carbon source, is subjected to a first sintering process to obtain a first sintered material; 2) Under an inert atmosphere, the second system, including the primary sintering material, fluorinated siloxane, and the second carbon source, is subjected to a secondary sintering treatment to obtain the lithium iron phosphate material.

7. The method for preparing lithium iron phosphate material according to claim 6, characterized in that, The fluorinated siloxane accounts for 0.1%-5% of the mass of the second system, preferably 0.5%-3%; And / or, the fluorinated siloxane comprises at least one of (3,3,3-trifluoropropyl)cyclopolysiloxane methyl ester, poly(methyl-3,3,3-trifluoropropyl)siloxane, tetramethyltri-3-trifluoropropylcyclotetrasiloxane, perfluorooctylethyltrisiloxane, hexacarbon perfluoropolyether trimethoxysilane, trifluoropropyltris(dimethylsiloxane)silane, and bis(nonafluorohexyl)tetramethyldisiloxane.

8. The method for preparing lithium iron phosphate material according to claim 6 or 7, characterized in that, The molar ratio of lithium in the lithium source to iron in the iron source is (1.02-1.10):1; And / or, the molar ratio of iron in the iron source to phosphorus in the phosphorus source is (0.96-0.985):1; And / or, the first carbon source accounts for 0.5%-5% of the mass percentage of the first system; And / or, the second carbon source accounts for 0.5%-5% of the mass of the second system; And / or, the temperature of the first sintering treatment is 500℃-800℃, and the time is 3h-10h; And / or, the temperature of the secondary sintering treatment is 650℃-790℃, and the time is 5h-12h.

9. The method for preparing lithium iron phosphate material according to any one of claims 6-8, characterized in that, The first system also includes additives; The additive includes at least one of compounds containing Ti, V, Nb, Mg, W, and Y, preferably including compounds containing Ti; And / or, the additive accounts for 0.1%-2% of the mass percentage of the first system; And / or, the second system further includes a titanium source; The titanium source includes at least one of bis(acetylacetonyl)diisopropoxytitanate, tetrabutyl titanate, and tetra(trimethylsiloxy)titanium. And / or, the titanium source accounts for 0.2%-2% of the mass percentage of the second system.

10. The method for preparing lithium iron phosphate material according to any one of claims 6-9, characterized in that, The lithium source includes at least one of lithium carbonate, lithium hydroxide, lithium phosphate, lithium dihydrogen phosphate, and lithium acetate. And / or, the iron source includes at least one of ferric oxide, ferric oxide, ferric hydroxyl oxide, and ferric nitrate; And / or, the phosphorus source includes at least one of phosphoric acid, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, lithium phosphate, and lithium dihydrogen phosphate; And / or, the first carbon source includes at least one of glucose, sucrose, fructose, starch, polyethylene glycol, polyvinylpyrrolidone, and polyvinyl alcohol; And / or, the second carbon source includes at least one of glucose, sucrose, fructose, starch, polyethylene glycol, polyvinylpyrrolidone, and polyvinyl alcohol.

11. A positive electrode plate, characterized in that, The lithium iron phosphate material includes the lithium iron phosphate material according to any one of claims 1-5 or the lithium iron phosphate material prepared according to the preparation method of the lithium iron phosphate material according to any one of claims 6-10.

12. A battery, characterized in that, Includes the positive electrode sheet as described in claim 11.