A transition metal sulfide positive electrode material, a preparation method and application thereof
By integrating layered conductive sulfides with conversion sulfides to form a locally symbiotic structure, the transition metal sulfide cathode material solves the problems of insufficient electronic conductivity and structural stability in all-solid-state lithium batteries, achieving efficient electron/ion transport and long-term cycle performance.
Patent Information
- Application Number
- CN202611245065.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2025-09-30
- Filing Date
- 2026-08-17
- Publication Date
- 2026-11-24
AI Technical Summary
Traditional transition metal sulfide cathode materials in all-solid-state lithium batteries suffer from poor electronic conductivity, slow electrochemical reaction kinetics, and insufficient structural stability, resulting in low charge-discharge efficiency and short cycle life, which cannot meet the requirements for high energy density.
By employing a symbiotic modification strategy, layered conductive sulfides are integrated with conversion-type sulfides to form a transition metal sulfide cathode material with a locally symbiotic structure. This provides a continuous electron transport channel and lithium storage function, realizing a lithium intercalation-conversion coupled lithium storage mechanism and enhancing structural stability.
It improves the electron/ion transport efficiency of all-solid-state lithium batteries, enhances cycle performance and rate performance, and significantly improves the charge/discharge efficiency and cycle stability of the batteries.
Smart Images

Figure CN123162183A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of battery technology, and in particular to a transition metal sulfide cathode material, its preparation method, and its application. Background Technology
[0002] With the rapid development of new energy storage technologies, electric vehicles, and portable electronic devices, the market has placed higher demands on the safety performance, energy density, and cycle life of lithium batteries. Traditional liquid lithium batteries, due to their use of organic liquid electrolytes, pose safety hazards such as flammability, leakage, and explosion, and their energy density improvement has reached a bottleneck, making them difficult to meet the development needs of high-end energy storage and power equipment. Against this backdrop, all-solid-state lithium batteries, with their excellent intrinsic safety, ultra-high energy density, and long-term cycle stability, have become the core research direction and key candidate technology for the next generation of energy storage batteries.
[0003] Cathode materials are the core components that determine the energy density and electrochemical performance of all-solid-state lithium batteries. The performance limitations of cathode materials have become a major bottleneck restricting the large-scale practical application of all-solid-state lithium batteries. Currently, commercially available and research-mature oxide-based cathode materials have the advantages of structural stability and high cycle reliability. However, due to their relatively low theoretical capacity, they cannot meet the core requirement of ultra-high energy density for advanced all-solid-state lithium batteries. The industry urgently needs to develop new alternative cathode materials with high capacity and high adaptability.
[0004] Transition metal sulfides, with their extremely high theoretical specific capacity, flexibly tunable redox chemistry, and good compatibility with solid-state electrolytes, have become popular candidate materials for high-capacity cathodes in all-solid-state lithium batteries, effectively compensating for the insufficient energy density of traditional oxide cathodes and possessing excellent application potential. However, at present, traditional transition metal sulfide cathode materials still face many insurmountable technical shortcomings in the practical application of all-solid-state battery systems.
[0005] Specifically, traditional transition metal sulfide cathodes generally suffer from poor intrinsic electronic conductivity and slow electrochemical reaction kinetics, significantly reducing battery charge / discharge efficiency and capacity utilization. Simultaneously, these materials are prone to severe structural collapse, volume deformation, and interface degradation during long-term charge / discharge cycles, leading to a substantial decrease in battery cycle life. More critically, current conventional modification strategies for transition metal sulfide cathode materials are limited by the inherent characteristics of the material conversion reactions and cannot fundamentally solve the problem of poor electrode durability. The difficulty in ensuring the long-term stability of the material structure and electrochemical performance severely hinders the full release of the high capacity and high energy density advantages of transition metal sulfide cathodes in all-solid-state systems, greatly limiting their industrialization and large-scale application. Therefore, a scalable and long-lasting electrode engineering method is urgently needed to unleash the actual potential of transition metal sulfide-based cathode materials. Summary of the Invention
[0006] This invention aims to at least solve one of the aforementioned technical problems existing in the prior art. Therefore, the first objective of this invention is to provide a transition metal sulfide cathode material. The second objective of this invention is to provide a method for preparing such a transition metal sulfide cathode material. The third objective of this invention is to provide applications of such a transition metal sulfide cathode material.
[0007] The inventive concept of this invention is as follows: This invention employs a symbiotic modification strategy to integrate layered conductive sulfides with conversion-type sulfides, forming a transition metal sulfide cathode material with a locally symbiotic structure. This transition metal sulfide cathode material can serve as the cathode material for all-solid-state lithium batteries. The layered conductive sulfides provide continuous electron and ion transport channels; the conversion-type sulfides have high capacity and, as the main lithium-storing active phase, undertake the lithium storage function. The combination of the two achieves a synergistic effect of a lithium intercalation-conversion coupled lithium storage mechanism. The locally symbiotic structure of the layered conductive sulfides and conversion-type sulfides ensures close contact at the heterogeneous interface and a continuous transport path, forming an efficient electron / ion transport network, accelerating the lithium... + / e - The migration enables synergistic optimization of electron transport and lithium storage.
[0008] To achieve the above objectives, the technical solution adopted by the present invention is as follows: In a first aspect, the present invention provides a transition metal sulfide cathode material, comprising a layered conductive sulfide M x S y and conversion sulfide M' a S b The layered conductive sulfide M x S y With conversion sulfide M' a Sb It has a local symbiotic structure.
[0009] The transition metal sulfide cathode material of this invention can be used as a cathode material in all-solid-state lithium batteries. The layered conductive sulfide provides a continuous electron transport channel, while the conversion-type sulfide acts as the lithium storage active phase, achieving a synergistic lithium intercalation-conversion coupled lithium storage mechanism. The local symbiotic structure (a dual-scale heterogeneous structure at the local symbiotic interface) of the layered conductive sulfide and the conversion-type sulfide ensures close contact and continuous transport paths at the heterogeneous interface, forming a highly efficient electron / ion transport network and accelerating the lithium... + / e - The migration of electrons enables synergistic optimization of electron transport and lithium storage. Furthermore, the localized symbiotic structure of the transition metal sulfide cathode material buffers structural strain, stabilizes the solid-solid interface in the all-solid-state lithium battery, and improves the cycle performance of the all-solid-state lithium battery.
[0010] Preferably, the layered conductive sulfide M x S y In the equation, 1≤x≤8, 1≤y≤8.
[0011] More preferably, x is taken from any value of 1, 2, 3, 4, 5, 6, 7, 8 or a range of values between any two.
[0012] More preferably, y is taken from any value of 1, 2, 3, 4, 5, 6, 7, 8 or a range of values between any two.
[0013] Preferably, M is selected from at least one of niobium (Nb), titanium (Ti), vanadium (V), molybdenum (Mo), tantalum (Ta), and tungsten (W).
[0014] Preferably, the layered conductive sulfide M x S y The mixture includes at least one of niobium disulfide (NbS2), titanium disulfide (TiS2), vanadium disulfide (VS2), molybdenum disulfide (MoS2), tantalum disulfide (TaS2), and tungsten disulfide (WS2); more preferably, the layered conductive sulfide is NbS2. Compared with other layered conductive sulfides, NbS2 possesses intrinsic metallicity, a stable layered structure, and excellent interface matching characteristics, enabling it to construct continuous electron transport channels in the composite system and form a stable symbiotic interface with the converted sulfide. Furthermore, NbS2 not only significantly reduces polarization but also promotes reaction kinetics, thus exhibiting superior overall performance in improving battery rate performance and cycle stability.
[0015] Preferably, the converted sulfide M' a S bIn the given condition, 1≤a≤6, 1≤b≤6.
[0016] More preferably, 'a' is taken from any value of 1, 2, 3, 4, 5, 6 or a range of values between any two.
[0017] More preferably, b is taken from any value of 1, 2, 3, 4, 5, 6 or a range of values between any two.
[0018] Preferably, M' is selected from at least one of iron (Fe), cobalt (Co), nickel (Ni), and manganese (Mn).
[0019] Preferably, the converted sulfide M' a S b It includes at least one of iron disulfide (FeS2), cobalt disulfide (CoS2), nickel disulfide (NiS2), and manganese disulfide (MnS2); more preferably, the converted sulfide is FeS2.
[0020] Preferably, the layered conductive sulfide M x S y M and the converted sulfide M' a S b The molar ratio of M' in the medium is 1:(0.4~9); more preferably, the layered conductive sulfide M x S y M and the converted sulfide M' a S b The molar ratio of M' in the middle is 1:(1~8); more preferably, the layered conductive sulfide M x S y M and the converted sulfide M' a S b The molar ratio of M' in the middle is 1:(2~6); more preferably, the layered conductive sulfide M x S y M and the converted sulfide M' a S b The molar ratio of M' in the middle is 1:(3~5).
[0021] In the transition metal sulfide cathode material of this invention, layered conductive sulfides provide electron transport channels, and increasing their content can improve the electronic conductivity of the cathode material. However, a relatively low content of converted sulfides will reduce the capacity performance of the cathode material. Within the scope defined by this invention, layered conductive sulfides and converted sulfides can form a stable local symbiotic structure, and the transition metal sulfide cathode material exhibits both excellent rate performance and capacity performance, possessing the best overall electrochemical performance.
[0022] Secondly, this invention provides a method for preparing the transition metal sulfide cathode material described in the first aspect, comprising the following steps: mixing an M source, an M' source, and a sulfur source, followed by a solid-state reaction to obtain the transition metal sulfide cathode material. This invention integrates layered conductive sulfides with conversion-type sulfides through a one-step solid-state reaction, forming a dual-scale heterostructure with a locally symbiotic interface. This structure enhances the structural integrity of the cathode material, promotes rapid ion transport, and improves the cycle performance in solid-state lithium battery systems.
[0023] Preferably, the M source includes one or more of the following: elemental M, halide containing element M, nitrate containing element M, alkoxide containing element M, carbonate containing element M, sulfate containing element M, acetate containing element M, oxide containing element M, and hydroxide containing element M; more preferably, the M source is elemental M; and even more preferably, the M source is elemental niobium.
[0024] Preferably, the M' source includes one or more of the following: elemental M', halide containing M', nitrate containing M', alkoxide containing M', carbonate containing M', sulfate containing M', acetate containing M', oxide containing M', and hydroxide containing M'; more preferably, the M' source is elemental M'; and even more preferably, the M' source is elemental iron.
[0025] Preferably, the sulfur source comprises elemental sulfur or a sulfur-containing compound; the sulfur-containing compound comprises at least one of Li2S, Na2S, K2S, Rb2S, Cs2S, Li2S2, Na2S2, Sb2S3, Bi2S3, and TiS3; more preferably, the sulfur source is elemental sulfur.
[0026] In this invention, when the M source, M' source, and sulfur source are all in elemental form, it has the advantages of clear reaction pathway and controllable product structure.
[0027] Preferably, the temperature of the solid-phase reaction is 600~800℃; more preferably, the temperature of the solid-phase reaction is 620~770℃; even more preferably, the temperature of the solid-phase reaction is 680~730℃.
[0028] Preferably, the solid-phase reaction time is 12-72 hours; more preferably, the solid-phase reaction time is 14-60 hours; even more preferably, the solid-phase reaction time is 16-40 hours; and even more preferably, the solid-phase reaction time is 20-30 hours.
[0029] Preferably, the heating rate of the solid-phase reaction is 5~15℃ / min; more preferably, the heating rate of the solid-phase reaction is 6~14℃ / min; and even more preferably, the heating rate of the solid-phase reaction is 8~12℃ / min.
[0030] The temperature of the solid-state reaction affects the formation and degree of crystallization of the crystal phase, the reaction time determines the sufficiency of the reaction, and the heating rate affects the uniformity of the microstructure of the cathode material and the formation of local symbiotic structures. Within the temperature, time, and heating rate range of the solid-state reaction defined in this invention, the M source, M' source, and sulfur source can fully undergo a solid-state reaction and form M... x S y With M' a S b Local symbiotic structures.
[0031] Thirdly, the present invention provides a solid-state battery cathode material, comprising the transition metal sulfide cathode material described in the first aspect, a solid electrolyte, and conductive additives.
[0032] Preferably, the solid-state battery cathode material includes a solid-state lithium battery cathode material, that is, the solid-state electrolyte includes a lithium electrolyte; the lithium electrolyte further includes a sulfide lithium electrolyte.
[0033] Preferably, the solid electrolyte comprises Li 5.4 PS 4.4 Cl 1.6 Li3Ps4, Li4P2S7, Li7P3S 11 , Li6PS5Cl, Li6PS5Br, Li6PS5I, Li3SbS4, Li3AsS 4、 Li 10 GeP2S 12 At least one of the following; more preferably, the solid electrolyte is Li. 5.4 PS 4.4 Cl 1.6 .
[0034] Preferably, the conductive additive includes at least one of graphene, acetylene black, Ketjen black, SuperP, carbon nanotubes, and carbon fibers; more preferably, the conductive additive is vapor-grown carbon fiber (VGCF).
[0035] Preferably, the mass percentage of transition metal sulfide cathode material in the solid-state battery cathode material is 20% to 75%; more preferably, the mass percentage of transition metal sulfide cathode material in the solid-state battery cathode material is 22% to 70%; and even more preferably, the mass percentage of transition metal sulfide cathode material in the solid-state battery cathode material is 25% to 65%.
[0036] Preferably, in the solid-state battery cathode material, the mass ratio of solid electrolyte to transition metal sulfide cathode material is 1:(0.5~2.5); more preferably, in the solid-state battery cathode material, the mass ratio of solid electrolyte to transition metal sulfide cathode material is 1:(0.7~2.3).
[0037] Preferably, in the solid-state battery cathode material, the mass ratio of conductive additive to transition metal sulfide cathode material is 1:(2~15); more preferably, in the solid-state battery cathode material, the mass ratio of conductive additive to transition metal sulfide cathode material is 1:(2.3~14).
[0038] Preferably, the solid-state battery cathode material further includes an interface modifier.
[0039] Preferably, the interface modifier includes at least one of lithium iodide, lithium bromide, and lithium chloride.
[0040] Preferably, the mass ratio of the interface modifier to the transition metal sulfide cathode material is 1:(5~15); more preferably, the mass ratio of the interface modifier to the transition metal sulfide cathode material is 1:(7~14).
[0041] Fourthly, the present invention provides a method for preparing the solid-state battery cathode material described in the third aspect, comprising the following steps: mixing the transition metal sulfide cathode material, solid electrolyte and conductive additive and then ball milling to obtain the cathode material.
[0042] In some embodiments of the present invention, the solid-state battery cathode material includes an interface modifier, and the preparation method is as follows: the transition metal sulfide cathode material, solid electrolyte, conductive additive and interface modifier are mixed and then ball-milled.
[0043] Preferably, the ball milling method is dry ball milling.
[0044] Preferably, the ball milling time is 1 to 5 hours; more preferably, the ball milling time is 1 to 4 hours; and even more preferably, the ball milling time is 1 to 3 hours.
[0045] Preferably, the ball mill rotates at a speed of 400 rpm to 600 rpm; more preferably, the ball mill rotates at a speed of 450 rpm to 550 rpm.
[0046] Fifthly, the present invention provides a positive electrode sheet comprising the solid-state battery positive electrode material described in the third aspect.
[0047] Preferably, the loading of transition metal sulfide cathode material in the cathode sheet is 1.5~5 mg cm⁻¹.-2 More preferably, the loading of transition metal sulfide cathode material in the cathode sheet is 1.5 mg cm⁻¹. -2 1.8 mg cm -2 2mg cm -2 2.11mg cm -2 2.6 mg cm -2 2.9 mg cm -2 3.2 mg cm -2 3.8 mg cm -2 4 mg cm -2 4.3mg cm -2 4.6 mg cm -2 5 mg cm -2 The range of values formed by any one of the values in the range or by any two of them.
[0048] In a sixth aspect, the present invention provides an all-solid-state battery, the all-solid-state battery comprising a solid electrolyte sheet, a negative electrode sheet and a positive electrode sheet as described in the fifth aspect; the solid electrolyte sheet is located between the negative electrode sheet and the positive electrode sheet.
[0049] Preferably, the all-solid-state battery is an all-solid-state lithium battery.
[0050] In a seventh aspect, the present invention provides a method for preparing an all-solid-state battery, comprising the following steps: S1: Cold-press solid electrolyte powder into solid electrolyte sheets; S2: The solid-state battery cathode material described in the third aspect is laid on one side of the solid electrolyte sheet and cold-pressed into a cathode sheet; S3: After placing the negative electrode sheet on the other side of the solid electrolyte sheet, the whole assembly is compacted to obtain an all-solid-state battery.
[0051] Preferably, the solid electrolyte powder mentioned in step S1 includes a silver-germanium sulfide electrolyte (Li). 5.4 PS 4.4 Cl 1.6 ).
[0052] Preferably, the cold pressing pressure in step S1 is 200~300 MPa; more preferably, the cold pressing pressure in step S1 is 220~280 MPa; and even more preferably, the cold pressing pressure in step S1 is 240~260 MPa.
[0053] Preferably, the cold pressing pressure in step S2 is 320~420 MPa; more preferably, the cold pressing pressure in step S2 is 340~400 MPa; and even more preferably, the cold pressing pressure in step S2 is 360~390 MPa.
[0054] Preferably, the negative electrode in step S3 includes one of lithium metal foil, lithium alloy negative electrode, graphite-based negative electrode, and silicon-based negative electrode; more preferably, the negative electrode in step S3 is a Li-In composite negative electrode.
[0055] The beneficial effects of this invention are: (1) This invention employs a symbiotic modification strategy to integrate layered conductive sulfides with conversion-type sulfides, forming a transition metal sulfide cathode material with a locally symbiotic structure (a dual-scale heterogeneous structure with a locally symbiotic interface). This transition metal sulfide cathode material can be used as a cathode material for all-solid-state lithium batteries. The layered conductive sulfides provide continuous electron transport channels, while the conversion-type sulfides act as the lithium storage active phase, fulfilling the lithium storage function. The two achieve a synergistic effect of a lithium intercalation-conversion coupled lithium storage mechanism. The locally symbiotic structure of the layered conductive sulfides and conversion-type sulfides ensures close contact at the heterogeneous interface and a continuous transport path, forming an efficient electron / ion transport network and accelerating the lithium... + / e - The migration of electrons enables synergistic optimization of electron transport and lithium storage. Furthermore, the localized symbiotic structure of the transition metal sulfide cathode material buffers structural strain, stabilizes the solid-solid interface in the all-solid-state lithium battery, and improves the cycle performance of the all-solid-state lithium battery.
[0056] (2) The all-solid-state lithium battery prepared using transition metal sulfide cathode material of this invention exhibits excellent rate performance. Compared with all-solid-state lithium batteries prepared using pure FeS2, the all-solid-state lithium battery prepared using the transition metal sulfide cathode material of this invention achieves a rate performance >200 mA g. -1 At the same time, it can maintain a higher reversible capacity. The all-solid-state lithium battery of the present invention can maintain a higher reversible capacity over a wide current density range (50~3000 mA g). -1 Its highest achieved values were 649.6, 651.1, 618.7, 552.2, 472.6, 359.3 and 269.3 mAh g. -1 High discharge capacity.
[0057] (3) The all-solid-state lithium battery prepared using transition metal sulfide cathode material in this invention exhibits excellent cycle stability. At 600 mA g -1 At the specified current density, the all-solid-state lithium battery prepared using the transition metal sulfide cathode material of this invention can retain up to 92.3% of its capacity after 300 cycles and up to 80.7% after 500 cycles. In contrast, the all-solid-state lithium battery prepared using pure FeS2 experienced rapid degradation, retaining only 45.4% of its initial capacity after 500 cycles. Attached Figure Description
[0058] Figure 1 This is a schematic diagram of the all-solid-state lithium battery in Example 7; Figure 2 The image shows the XRD patterns of the NbS2-FeS2 locally symbiotic cathode material and FeS2 in Example 1. Figure 3 Here is a SEM image of the NbS2-FeS2 locally symbiotic cathode material from Example 1; Figure 4 Here is an HRTEM image of the NbS2-FeS2 locally symbiotic cathode material of Example 1; Figure 5 The graphs show the electrochemical performance of the all-solid-state lithium batteries in Example 7 and Comparative Example 1. Figure 6 The electrochemical performance graphs for the all-solid-state lithium batteries of Example 8 and Comparative Example 1 are shown. Figure 7 The graph shows the electrochemical performance of the all-solid-state lithium batteries in Example 9 and Comparative Example 1. Detailed Implementation
[0059] To enable those skilled in the art to better understand this application, the present invention will be further described in detail below with reference to embodiments. However, it should be understood that the following embodiments are merely preferred embodiments of the present invention, and the scope of protection of the present invention should be determined by the scope defined in the claims.
[0060] In the description of this invention, it should be noted that unless specific conditions are specified in the examples, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all commercially available products.
[0061] Furthermore, to better illustrate the present invention, numerous specific details are provided in the following detailed embodiments. Those skilled in the art should understand that the present invention can be practiced without certain specific details. In some embodiments, materials, methods, and means well-known to those skilled in the art are not described in detail in order to highlight the spirit of the invention.
[0062] Unless otherwise expressly stated, throughout the specification and claims, the term "comprising" or its variations such as "including" or "comprising" shall be understood to include the stated elements or components without excluding other elements or other components.
[0063] In both the embodiments and comparative examples of this invention, the assembly process of the all-solid-state batteries was carried out in an argon-filled glove box, with environmental conditions controlled as follows: oxygen content below 0.1 ppm and moisture content below 0.1 ppm. Electrochemical tests in both the embodiments and comparative examples of this invention were conducted under an applied pressure of 50 MPa.
[0064] Example 1 This embodiment provides a NbS2-FeS2 locally symbiotic cathode material, which is prepared by the following method: 0.186g of niobium (Nb) powder, 0.447g of Fe powder, and 0.641g of S powder are mixed evenly to obtain a mixture powder; the mixture powder is sealed in a quartz tube by vacuum sealing, and then placed in a muffle furnace, heated to 700℃ at a heating rate of 10℃ / min and held for 24h to obtain the NbS2-FeS2 locally symbiotic cathode material, wherein the molar ratio of NbS2 to FeS2 is 1:4.
[0065] Example 2 This embodiment provides a VS2-FeS2 locally symbiotic cathode material, which differs from Example 1 in that 0.102g of vanadium (V) elemental powder is used to replace 0.186g of niobium (Nb) elemental powder in Example 1. All other aspects are the same as in Example 1 to obtain the VS2-FeS2 locally symbiotic cathode material, wherein the molar ratio of VS2 to FeS2 is 1:4.
[0066] Example 3 This embodiment provides a TiS2-FeS2 locally symbiotic cathode material, which differs from Example 1 in that 0.096 g of titanium (Ti) elemental powder is used to replace 0.186 g of niobium (Nb) elemental powder in Example 1. All other aspects are the same as in Example 1, resulting in a TiS2-FeS2 locally symbiotic cathode material, wherein the molar ratio of TiS2 to FeS2 is 1:4.
[0067] Example 4 This embodiment provides a solid-state battery cathode material, prepared using the following method: The NbS2-FeS2 locally symbiotic structure cathode material from Example 1, and a sulfide solid electrolyte (Li...) are combined... 5.4 PS 4.4 Cl 1.6 The solid-state battery cathode material was obtained by mixing vapor-grown carbon fiber (VGCF) and lithium iodide (LiI) in a mass ratio of 35:50:15:5 and then ball-milling at 500 rpm for 2 hours.
[0068] Example 5 This embodiment provides a solid-state battery cathode material, which differs from Embodiment 4 in that the VS2-FeS2 locally symbiotic structure cathode material of Embodiment 2 is used instead of the NbS2-FeS2 locally symbiotic structure cathode material of Embodiment 1, while the rest is the same as Embodiment 4.
[0069] Example 6 This embodiment provides a solid-state battery cathode material, which differs from Embodiment 4 in that the TiS2-FeS2 locally symbiotic cathode material of Embodiment 3 is used instead of the NbS2-FeS2 locally symbiotic cathode material of Embodiment 1, while the rest is the same as Embodiment 4.
[0070] Example 7 This embodiment provides an all-solid-state lithium battery, which is prepared using the following method: S1: Add 80mg of solid electrolyte powder (Li) 5.4 PS 4.4 Cl 1.6 Solid electrolyte sheets were prepared by cold pressing at 250 MPa. S2: Take 5 mg of the solid-state battery cathode material from Example 4 and lay it on one side of the solid electrolyte sheet from step S1. Cold press it under 375 MPa pressure to ensure tight interfacial contact, thus preparing the cathode sheet. The loading of the NbS2-FeS2 locally symbiotic cathode material on the cathode sheet is 2.11 mg cm⁻¹. -2 ; S3: Indium foil and lithium foil are pressed together under 125 MPa pressure to form a Li-In negative electrode sheet. The Li-In negative electrode sheet is then placed on the other side of the solid electrolyte sheet and compacted to obtain an all-solid-state lithium battery. The assembled all-solid-state lithium battery is then sandwiched between stainless steel current collectors. A schematic diagram of its structure is shown below. Figure 1 .
[0071] Example 8 This embodiment provides an all-solid-state lithium battery, which differs from Embodiment 7 in that the solid-state battery cathode material of Embodiment 5 is used instead of the solid-state battery cathode material of Embodiment 4 in step S2, while the rest is the same as Embodiment 7.
[0072] Example 9 This embodiment provides an all-solid-state lithium battery, which differs from Embodiment 7 in that the solid-state battery cathode material of Embodiment 6 is used instead of the solid-state battery cathode material of Embodiment 4 in step S2, while the rest is the same as Embodiment 7.
[0073] Comparative Example 1 This comparative example provides an all-solid-state lithium battery, which differs from Example 7 in that the cathode material of the solid-state battery in step S2 is pure FeS2 and Li. 5.4 PS 4.4 Cl 1.6 VGCF and lithium iodide were mixed evenly at a mass ratio of 35:50:15:5, and then dry ball milled at 500 rpm for 2 hours to obtain the solid-state battery cathode material. All other steps were the same as in Example 7.
[0074] Structural characterization 1. Figure 2 The image shows the XRD patterns of the NbS2-FeS2 locally symbiotic cathode material and FeS2 in Example 1. Figure 2 It can be seen that the NbS2-FeS2 locally symbiotic cathode material in Example 1 contains two crystal phases, including layered NbS2 and converted pyrite FeS2.
[0075] 2. Figure 3 This is a SEM image of the NbS2-FeS2 locally symbiotic cathode material from Example 1. Figure 3 It can be seen that the NbS2-FeS2 locally symbiotic cathode material has a hierarchical locally symbiotic structure. Among them, hexagonal layered NbS2 and bulk FeS2 coexist in an interwoven manner. Figure 3 This indicates that the NbS2-FeS2 locally symbiotic cathode material is not a uniform solid solution, but a composite material in which NbS2 and FeS2 are locally symbiotic.
[0076] 3. Figure 4 This is a high-resolution transmission electron microscope (HRTEM) image of the NbS2-FeS2 locally symbiotic cathode material of Example 1. Figure 4 In the image, a is the HRTEM image of the NbS2-FeS2 locally symbiotic cathode material at the symbiotic interface. Figure 4 In the middle, b is a magnified HRTEM image of the FeS2 region in the NbS2-FeS2 locally symbiotic cathode material. Figure 4 Image c is a magnified HRTEM image of the NbS2 region in the NbS2-FeS2 locally symbiotic cathode material. Figure 4 It can be seen that two different lattice fringes were observed in the NbS2-FeS2 locally symbiotic cathode material, with spacings of 0.221 nm and 0.207 nm, respectively, corresponding to the (211) crystal plane of FeS2 and the (104) crystal plane of NbS2, and the two are in close contact. Figure 4 This indicates that the NbS2-FeS2 locally symbiotic cathode material has a dual-scale heterostructure with a locally symbiotic interface.
[0077] Performance testing The electrochemical performance (rate performance and constant current long-cycle stability) of the all-solid-state lithium batteries in Examples 7-9 and Comparative Example 1 were tested using a LAND battery testing system. The voltage range was set to 0.4-2.4 V (relative to the Li-In negative electrode). During the rate performance test, the voltage was measured at 50, 100, 200, 500, 1000, 2000, and 3000 mA g. -1 The test was conducted at a current density of 600 mA. The constant current long-cycle stability test used a g... -1The current was tested, and the test results are as follows: Figures 5-7 As shown.
[0078] Figure 5 The graphs show the electrochemical performance of the all-solid-state lithium batteries in Example 7 and Comparative Example 1. Figure 5 (A) shows the all-solid-state lithium battery of Example 7 and the all-solid-state lithium battery of Comparative Example 1 at 50 to 3000 mA g. -1 Rate performance graph for current density range and voltage range of 0.4-2.4V. Figure 5 (B) shows the all-solid-state lithium battery of Example 7 and the all-solid-state lithium battery of Comparative Example 1 at 600 mA g. -1 Cyclic stability plot after 500 cycles at current density and voltage range of 0.4-2.4 V.
[0079] Depend on Figure 5 As shown in (A), compared with Comparative Example 1, the all-solid-state lithium battery of Example 7 has a current density >200 mAg. -1 It consistently provides the highest reversible capacity, demonstrating its efficient ion and electron transport. This is achieved over a wide current density range (50 to 3000 mA g). -1 The all-solid-state lithium battery in Example 7 achieved mAh g⁻¹ of 649.6, 651.1, 618.7, 552.2, 472.6, 359.3, and 269.3 mAh g⁻¹. -1 Its high discharge capacity indicates that it has excellent rate performance and active material utilization (maintaining high capacity even at high rates).
[0080] Depend on Figure 5 From (B), we know that 600 mA g -1 At the specified current density, the all-solid-state lithium battery of Example 7 provided the highest initial capacity of 517.1 mAh g⁻¹. -1 It retained 92.3% of its capacity after 300 cycles and 80.7% after 500 cycles. In contrast, the all-solid-state lithium battery in Comparative Example 1 experienced rapid degradation, retaining only its initial capacity (391.2 mAh g⁻¹) after 500 cycles. -1 45.4% of ).
[0081] In summary, compared to FeS2, the NbS2-FeS2 locally symbiotic cathode material ensures tight interfacial contact, continuous transport channels, and effective strain buffering, and achieves a coupled intercalation-conversion mechanism. Therefore, all-solid-state lithium batteries fabricated using NbS2-FeS2 locally symbiotic cathode materials exhibit superior rate performance and cycle stability.
[0082] Figure 6The graphs show the electrochemical performance of the all-solid-state lithium batteries in Example 8 and Comparative Example 1. Figure 6 (A) shows the all-solid-state lithium battery of Example 8 and the all-solid-state lithium battery of Comparative Example 1 at 50 to 3000 mA g. -1 Rate performance graph for current density range and voltage range of 0.4-2.4V. Figure 6 (B) shows the all-solid-state lithium battery of Example 8 and the all-solid-state lithium battery of Comparative Example 1 at 600 mA g. -1 Cyclic stability plot after 100 cycles at current density and voltage range of 0.4-2.4 V. Figure 6 It can be seen that the all-solid-state lithium battery of Example 8 has better rate performance and cycle stability.
[0083] Figure 7 The graphs show the electrochemical performance of the all-solid-state lithium batteries in Example 9 and Comparative Example 1. Figure 7 (A) shows the all-solid-state lithium battery of Example 9 and the all-solid-state lithium battery of Comparative Example 1 at 50 to 3000 mA g. -1 Rate performance graph for current density range and voltage range of 0.4-2.4V. Figure 7 (B) shows the all-solid-state lithium battery of Example 9 and the all-solid-state lithium battery of Comparative Example 1 at 600 mA g. -1 Cyclic stability plot after 100 cycles at current density and voltage range of 0.4-2.4 V. Figure 7 It can be seen that the all-solid-state lithium battery of Example 9 has superior rate performance and cycle stability.
[0084] In summary, compared to FeS2, the transition metal sulfide cathode material of this invention (with a locally symbiotic structure of layered conductive sulfides and conversion-type sulfides) possesses a highly efficient electron / ion transport network, accelerating the Li... + / e - The migration of electrons and the synergistic optimization of lithium storage can significantly improve the rate performance and cycle stability of all-solid-state lithium batteries.
[0085] comprehensive Figures 5-7The results show that the transition metal sulfide cathode materials constructed from different layered conductive sulfides have varying effects on improving the performance of all-solid-state lithium batteries. Compared with the NbS2-FeS2 local symbiotic structure cathode material, the all-solid-state lithium battery (Example 8) prepared using the VS2-FeS2 local symbiotic structure cathode material gradually decreases in capacity during cycling, indicating that the structural stability of the VS2-FeS2 local symbiotic structure cathode material is insufficient. While the all-solid-state lithium battery (Example 9) prepared using the TiS2-FeS2 local symbiotic structure cathode material shows an improvement in rate capacity, the voltage plateau polarization increases, indicating that the electron transport and interface synergy capabilities of the TiS2-FeS2 local symbiotic structure cathode material are limited. This is because NbS2 has intrinsic metallicity, a stable layered structure, and excellent interface matching characteristics, enabling it to construct continuous electron transport channels in the composite system and form a more stable local symbiotic structure interface with FeS2. This localized symbiotic structure not only significantly reduces polarization but also promotes reaction kinetics, resulting in superior overall performance in terms of rate capability and cycle stability.
[0086] In summary, this invention employs a symbiotic modification strategy to integrate layered conductive sulfides with conversion-type sulfides, forming a transition metal sulfide cathode material with a locally symbiotic structure (a dual-scale heterostructure with a locally symbiotic interface). In this transition metal sulfide cathode material, the layered conductive sulfides provide continuous electron transport channels, while the conversion-type sulfides, as the lithium storage active phase, undertake the lithium storage function, achieving a synergistic effect of the lithium intercalation-conversion coupled lithium storage mechanism. The locally symbiotic structure of the layered conductive sulfides and conversion-type sulfides ensures close contact at the heterogeneous interface and a continuous transport path, forming an efficient electron / ion transport network, accelerating the lithium... + / e - The migration of electrons enables synergistic optimization of electron transport and lithium storage. Furthermore, the localized symbiotic structure of the transition metal sulfide cathode material buffers structural strain, stabilizes the solid-solid interface in the all-solid-state lithium battery, and improves the cycle performance of the all-solid-state lithium battery.
[0087] The above embodiments are preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the above embodiments. Any changes, modifications, substitutions, combinations, or simplifications made without departing from the spirit and principle of the present invention shall be considered equivalent substitutions and shall be included within the protection scope of the present invention.
Claims
1. A transition metal sulfide cathode material, characterized in that, Transition metal sulfide cathode materials include layered conductive sulfides M x S y and conversion sulfide M' a S b The layered conductive sulfide M x S y With the converted sulfide M' a S b It has a locally symbiotic structure.
2. The transition metal sulfide cathode material according to claim 1, characterized in that, The layered conductive sulfide M x S y In the given condition, 1 ≤ x ≤ 8, 1 ≤ y ≤ 8; And / or, the layered conductive sulfide M x S y M is selected from at least one of Nb, Ti, V, Mo, Ta, and W; And / or, the converted sulfide M' a S b In the given condition, 1 ≤ a ≤ 6, 1 ≤ b ≤ 6; And / or, the converted sulfide M' a S b M' is selected from at least one of Fe, Co, Ni, and Mn.
3. The transition metal sulfide cathode material according to claim 1, characterized in that, The layered conductive sulfide M x S y Including at least one of niobium disulfide, titanium disulfide, vanadium disulfide, molybdenum disulfide, tantalum disulfide, and tungsten disulfide; And / or, the converted sulfide M' a S b Including at least one of iron disulfide, cobalt disulfide, nickel disulfide, and manganese disulfide; And / or, the layered conductive sulfide M x S y M and the converted sulfide M' a S b The molar ratio of M' in the middle is 1:(0.4~9).
4. The method for preparing the transition metal sulfide cathode material according to any one of claims 1 to 3, characterized in that, Includes the following steps: The M source, M' source and sulfur source are mixed and subjected to a solid-state reaction to obtain the transition metal sulfide cathode material.
5. The method for preparing the transition metal sulfide cathode material according to claim 4, characterized in that, The M source and the M' source each independently include one or more of the following: elements containing M or M': halides, nitrates, alkoxides, carbonates, sulfates, acetates, oxides, and hydroxides. And / or, the sulfur source includes elemental sulfur or sulfur-containing compounds.
6. The method for preparing the transition metal sulfide cathode material according to claim 4, characterized in that, The temperature of the solid-phase reaction is 600~800℃; And / or, the solid-phase reaction takes 12 to 72 hours; And / or, the heating rate of the solid-phase reaction is 5~15℃ / min.
7. A solid-state battery cathode material, characterized in that, It includes the transition metal sulfide cathode material, solid electrolyte, and conductive additive as described in any one of claims 1 to 3.
8. A positive electrode plate, characterized in that, Includes the solid-state battery cathode material as described in claim 7.
9. An all-solid-state battery, characterized in that, The all-solid-state battery includes a solid electrolyte sheet, a negative electrode sheet, and a positive electrode sheet as described in claim 8; the solid electrolyte sheet is located between the negative electrode sheet and the positive electrode sheet.
10. The method for preparing the all-solid-state battery according to claim 9, characterized in that, Includes the following steps: S1: Cold-press solid electrolyte powder into solid electrolyte sheets; S2: The solid-state battery positive electrode material is laid on one side of the solid electrolyte sheet and cold-pressed into a positive electrode sheet; S3: After placing the negative electrode sheet on the other side of the solid electrolyte sheet, the whole assembly is compacted to obtain the all-solid-state battery.