A starting and stopping sodium iron pyrophosphate positive electrode material and a preparation method thereof

CN123162185APending Publication Date: 2026-11-24ANHUI XINNA MATERIAL SCIENCE & TECHNOLOGY CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202611331285.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-31
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

[0007]上述现有技术中的焦磷酸磷酸铁钠材料虽然解决了部分问题,但进行大规模工业化应用还有一定难度,并且目前工业化的焦磷酸磷酸铁钠材料尚存在多种技术路线选择,且工艺复杂多变,还不能实现针对于启动启停电池用的焦磷酸磷酸铁钠正极材料的大规模生产和广泛应用,因此亟需一种启动启停用焦磷酸磷酸铁钠正极材料及其制备方法解决上述问题

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123162185A_ABST
    Figure CN123162185A_ABST
Patent Text Reader

Abstract

The application discloses a kind of starting sodium pyrophosphate ferrous phosphate positive electrode material of start-stop and preparation method thereof, comprising S1: sodium source, iron source, phosphorus source, carbon source, vanadium source and binary acid are added in solvent water and dispersed uniformly to obtain slurry;S2: the slurry of mixing is carried out sand mill treatment, and grinding material is obtained;S3: the grinding material is carried out fine sand mill treatment, and fine grinding material is obtained;S4: fine grinding material is transferred into spray dryer, and spray granulation is carried out to obtain precursor;S5: the precursor is carried out crushing treatment to obtain precursor powder;S6: the precursor powder is sintered to obtain positive electrode material.The application is ground to smaller particle size by two-stage sand mill process, in cooperation with the corrosion effect of binary acid on iron phosphate, so as to obtain greater reactivity, which can reduce the production of non-active phase NaFePO4 in the preparation process, to obtain higher reversible capacity.Meanwhile, vanadium element can be more easily doped into the body phase of sodium pyrophosphate ferrous phosphate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of sodium-ion battery cathode material preparation technology, specifically to a sodium iron phosphate pyrophosphate cathode material for start-stop operation and its preparation method. Background Technology

[0002] Sodium iron phosphate pyrophosphate is one of the three main materials for sodium-ion cathodes, possessing advantages such as low production cost, high safety, and long cycle life, making it applicable to applications in small two- / three-wheeled vehicles, start-stop power supplies, and industrial and commercial energy storage. However, sodium iron phosphate pyrophosphate materials suffer from phase transition instability, low conductivity, slow ion migration, and instability during industrial production. To address these issues, existing technologies employ various methods such as carbon coating, ion doping, structural modulation, and multi-material composites to improve the overall performance of the material.

[0003] Patent application CN118811792A discloses a method for preparing sodium iron phosphate / C composite material by mechanical ball milling. The raw materials are mixed by ball milling and then calcined at high temperature to obtain carbon-coated sodium iron phosphate cathode material. The preparation method is simple and the product has a small specific surface area.

[0004] Patent application CN118630202A discloses a method for preparing niobium-doped sodium iron pyrophosphate by spray drying. The method improves the electrochemical performance of sodium iron pyrophosphate by having high-valence metallic niobium occupy some of the active iron sites in the sodium iron pyrophosphate.

[0005] Patent application CN118431464A discloses a method for preparing sodium iron pyrophosphate, which involves carbon-coating sodium iron pyrophosphate powder doped with metal elements. The doped metal elements are selected from one or more of Mg, Ca, Sr, Al, Ti, V, Cr, Zr, Nb, W, Cr, Cu, Zn, Mo, Sc, and Y. The method has the characteristics of high charge-discharge capacity and high compaction density.

[0006] Patent application CN117691075A discloses a composite material of sodium vanadium fluorophosphate coated with sodium iron pyrophosphate. The coating of sodium vanadium fluorophosphate shortens the sodium ion diffusion channel, improves the electrochemical activity, and can improve the overall electrochemical performance of the composite material.

[0007] While the sodium iron phosphate pyrophosphate material mentioned above has solved some problems, large-scale industrial application still faces certain difficulties. Furthermore, there are currently multiple technical routes to choose from for industrialized sodium iron phosphate pyrophosphate materials, and the processes are complex and varied. It is not yet possible to achieve large-scale production and widespread application of sodium iron phosphate pyrophosphate cathode materials for start-stop batteries. Therefore, there is an urgent need for a sodium iron phosphate pyrophosphate cathode material for start-stop batteries and its preparation method to solve the above problems. Summary of the Invention

[0008] The purpose of this invention is to provide a sodium iron phosphate pyrophosphate cathode material for start-up and shutdown and its preparation method, so as to overcome the above-mentioned shortcomings in the prior art.

[0009] To achieve the above objectives, the present invention provides the following technical solution:

[0010] A sodium iron phosphate pyrophosphate cathode material for start-stop operation, characterized in that the chemical formula of the cathode material is represented by Na. 4.08 Fe 2.9 V x T(PO4)2P2O7, where 0.006≤x≤0.024.

[0011] A method for preparing sodium iron phosphate pyrophosphate cathode material for start-stop operation, comprising the following steps:

[0012] S1: Add sodium source, iron source, phosphorus source, carbon source, vanadium source and dicarboxylic acid to water and disperse evenly to obtain a slurry;

[0013] S2: The mixed slurry is sand-milled to obtain grinding material;

[0014] S3: The abrasive material is finely ground to obtain fine abrasive material;

[0015] S4: Transfer the finely ground material into a spray dryer for spray granulation to obtain the precursor;

[0016] S5: The precursor is pulverized to obtain precursor powder;

[0017] S6: The precursor powder is sintered to obtain sodium iron phosphate pyrophosphate cathode material.

[0018] In S3, the fine sand milling process is configured to combine with the corrosive effect of dicarboxylic acid on ferric phosphate, grinding ferric phosphate to a particle size of D50=150±10nm, D90≤260nm.

[0019] Preferably, in S1, the iron source is iron-based ferric phosphate, and the iron-to-phosphorus ratio of the iron-based ferric phosphate is 0.965~0.971.

[0020] Preferably, in S1, the sodium source is one or more of sodium carbonate, sodium oxalate, sodium pyrophosphate, sodium dihydrogen pyrophosphate, sodium dihydrogen phosphate, and disodium hydrogen phosphate.

[0021] The phosphorus source is one or more of sodium pyrophosphate, sodium dihydrogen pyrophosphate, sodium dihydrogen phosphate, disodium hydrogen phosphate, ammonium dihydrogen phosphate, and diammonium hydrogen phosphate.

[0022] The carbon source is one or more of glucose, sucrose, citric acid, ascorbic acid, and polyethylene glycol;

[0023] The vanadium source is one or more of vanadium carbonate, vanadium pentoxide, and ammonium metavanadate.

[0024] The dicarboxylic acid is one or more of oxalic acid dihydrate, oxalic acid (ethanedioic acid), malonic acid, and succinic acid.

[0025] Preferably, in S1, the molar ratio of sodium, iron, and phosphorus is 4.08:2.9:4, the carbon source accounts for 12% to 16% of the total weight of the iron source, the molar doping amount of vanadium is 0.006 to 0.024, and the molar amount of the dicarboxylic acid is 120% to 160% of the sodium source.

[0026] Preferably, in step S2, the specific steps of the sand milling process are as follows: the mixed slurry is placed in a fine mill, and zirconia beads with a diameter of 0.3-0.4 mm and a 0.15 mm sieve are used to sand mill at a speed of 1200 rpm for several hours, controlling the particle size of the abrasive to be D50=220±10 nm and D90≤480 nm.

[0027] Preferably, in step S3, the specific steps of fine grinding are as follows: the grinding slurry of S2 is placed in a fine grinding machine, and zirconia beads with a diameter of 0.2-0.3 mm and a sieve with a diameter of 0.1 mm are used to grind the material at a speed of 1200 rpm for several hours.

[0028] Preferably, in step S4, the specific steps of spray granulation are as follows: the fine abrasive is transferred into a spray dryer and granulated under the conditions of an inlet air temperature of 220°C, an atomizing disc rotation speed of 400Hz, and an outlet air temperature of 96°C to obtain a spherical precursor with a particle size D50=35±5μm.

[0029] Preferably, in step S5, the particle size of the precursor is D50 = 6 ± 0.5 μm.

[0030] Preferably, in step S6, the sintering process is as follows: the temperature is increased from room temperature to 300°C at a heating rate of 2°C / min, held at this temperature for 3 hours in a N2 atmosphere, and then increased to 500°C~600°C at a heating rate of 2°C / min, held at this temperature for 10 hours in a N2 atmosphere.

[0031] A sodium-ion battery includes a positive electrode material, an electrolyte, a negative electrode material, and a separator, wherein the positive electrode material is the aforementioned sodium iron phosphate pyrophosphate positive electrode material for start-stop operation.

[0032] In the above technical solution, the beneficial effects of the present invention are:

[0033] 1. The doping scheme employed in this invention can enhance the electrochemical activity of sodium iron pyrophosphate: After introducing vanadium, since the atomic radius of vanadium is larger than that of iron, the introduced vanadium atoms preempt iron atom positions, increasing the size of the MO bond between the transition metal and oxygen atoms, thereby increasing the unit cell volume. This change lowers the Na ion diffusion barrier, improves ionic conductivity, and suppresses changes in cell volume during high-rate charge and discharge. Stable three-dimensional diffusion channels for sodium ions can be formed in the sodium iron pyrophosphate structure, achieving improved rate performance and cycle life.

[0034] 2. The two-stage sand milling process employed in this invention, combined with the corrosive effect of diacids on ferric phosphate, grinds ferric phosphate to a smaller particle size, thereby obtaining greater reactivity. This reduces the generation of the inactive NaFePO4 phase during preparation, resulting in higher reversible capacity. Simultaneously, it facilitates the incorporation of vanadium into the bulk phase of sodium ferric phosphate pyrophosphate.

[0035] 3. The iron-based ferric phosphate raw material selected in this invention has a layered microstructure. Compared with the spherical microstructure of ammonium-based and sodium-based ferric phosphate, it can avoid agglomeration during fine grinding. This makes the testing of grinding particle size more accurate, easier to calibrate and determine process parameters, and more suitable for a wide range of industrial applications.

[0036] 4. The chemical proportions of sodium, iron, phosphorus, and vanadium in the raw materials used in this invention are easy to control through ingredient proportioning, and the raw materials are simple and readily available; the process used in this invention is simple, reliable, fast, and easy to mass-produce and widely apply.

[0037] It should be understood that the foregoing general description and the following detailed description are exemplary and illustrative only, and are not intended to limit this disclosure.

[0038] This application provides an overview of various implementations or examples of the technology described in this disclosure, and is not a full disclosure of the entire scope or all features of the disclosed technology. Attached Figure Description

[0039] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in this invention. For those skilled in the art, other drawings can be obtained based on these drawings.

[0040] Figure 1 This is a scanning electron microscope image of the lamellar microstructure of the iron-based iron phosphate used in this invention.

[0041] Figure 2 This is a scanning electron microscope image of sodium iron pyrophosphate prepared in Example 2 of the present invention.

[0042] Figure 3 This is a rate charge-discharge curve of the sodium-ion battery prepared in Example 2 of the present invention. Detailed Implementation

[0043] To make the objectives, technical solutions, and advantages of the embodiments of this disclosure clearer, the technical solutions of the embodiments of this disclosure will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of this disclosure. All other embodiments obtained by those skilled in the art based on the described embodiments of this disclosure without creative effort are within the scope of protection of this disclosure.

[0044] Example 1

[0045] A method for preparing sodium iron phosphate pyrophosphate cathode material for start-up and shutdown, using iron-phosphorus ratio 0.971 as raw material, includes the following steps:

[0046] S1: Weigh 1.49 mol of sodium carbonate, 2.9 mol of ferric phosphate, 1.1 mol of sodium dihydrogen phosphate, 6% of glucose (total weight of ferric phosphate), 10% of polyethylene glycol (total weight of ferric phosphate), 0.006 mol of ammonium metavanadate, and 2.086 mol of oxalic acid dihydrate and add them sequentially to deionized water for dispersion.

[0047] S2: Place the mixed slurry in a sand mill and perform a two-stage sand milling process to control the particle size distribution of the grinding material at D50=150±10nm and D90=260±10nm.

[0048] S3: Transfer the abrasive material into a spray dryer and granulate it under the conditions of inlet air temperature of 220℃, atomizing disc speed of 400Hz and outlet air temperature of 96℃ to obtain the precursor.

[0049] S4: Place the precursor in an air jet mill and pulverize it to a particle size of D50=6±0.5μm to obtain precursor powder;

[0050] S5: The precursor powder is sintered by heating it from room temperature to 300°C at a sintering rate of 2°C / min and holding it for 3 hours, and then heating it to 570°C and holding it for 10 hours to obtain the finished cathode material.

[0051] Example 2

[0052] Compared with Example 1, the molar amount of ammonium metavanadate in S1 is 0.012 mol, and other operations and parameters are the same as in Example 1.

[0053] Example 3

[0054] Compared with Example 1, the molar amount of ammonium metavanadate in S1 is 0.018 mol, and other operations and parameters are the same as in Example 1.

[0055] Example 4

[0056] Compared with Example 1, the molar amount of ammonium metavanadate in S1 is 0.024 mol, and other operations and parameters are the same as in Example 1.

[0057] Example 5

[0058] Compared with Example 1, in S1, glucose was 6% of the total weight of ferric phosphate, polyethylene glycol was 6% of the total weight of ferric phosphate, and other operations and parameters were the same as in Example 1.

[0059] Example 6

[0060] Compared with Example 1, in S1, glucose is 10% of the total weight of ferric phosphate and polyethylene glycol is 6% of the total weight of ferric phosphate, and other operations and parameters are the same as in Example 1.

[0061] Example 7

[0062] Compared to Example 1, the molar amount of oxalic acid dihydrate in S1 was 1.788 mol, while the grinding particle size in S2 failed to meet the process requirements, with a particle size distribution of D50=160 nm and D90=290 nm. Other operations and parameters were the same as in Example 1.

[0063] Example 8

[0064] Compared with Example 1, the molar amount of oxalic acid dihydrate in S1 is 2.384 mol, and other operations and parameters are the same as in Example 1.

[0065] The present invention also proposes the following comparative examples:

[0066] Comparative Example 1

[0067] Compared with Example 1, S1 does not contain vanadium, but all other operations and parameters are the same as in Example 1.

[0068] Comparative Example 2

[0069] Compared to Example 1, no oxalic acid dihydrate was added in S1, while the grinding particle size in S2 failed to meet the process requirements, with a particle size distribution of D50=180nm and D90=330nm. Other operations and parameters were the same as in Example 1.

[0070] Comparative Example 3

[0071] Compared with Example 1, the raw material used was iron-phosphate produced by the iron-phosphorus method with an iron-phosphorus ratio of 0.968, and all other operations and parameters were the same as in Example 1.

[0072] Comparative Example 4

[0073] Compared with Example 1, the raw material used was iron-phosphate produced by the iron-phosphorus method with an iron-phosphorus ratio of 0.965, and all other operations and parameters were the same as in Example 1.

[0074] Comparative Example 5

[0075] Compared to Example 1, the raw material used was ammonium ferric phosphate with an iron-to-phosphorus ratio of 0.967, while the grinding particle size in S2 failed to meet the process requirements, with a particle size distribution of D50=190nm and D90=380nm. Other operations and parameters were the same as in Example 1.

[0076] Comparative Example 6

[0077] Compared to Example 1, the raw material used was sodium-processed ferric phosphate with an iron-to-phosphorus ratio of 0.968, while the grinding particle size in S2 failed to meet the process requirements, with a particle size distribution of D50=170nm and D90=310nm. Other operations and parameters were the same as in Example 1.

[0078] test:

[0079] Sodium iron pyrophosphate prepared in Examples 1-5 and Comparative Examples 1-3 was used as the positive electrode active material for sodium-ion batteries. It was mixed with conductive agent SP and binder PVDF (polyvinylidene fluoride) at a mass ratio of 90:5:5, with aluminum foil as the current collector, forming the positive electrode. A metallic sodium sheet was used as the negative electrode for sodium-ion batteries, glass fiber was used as the separator, and a 1 mol / L NaPF6 EC / DMC (ethylene carbonate / dimethyl carbonate) (volume ratio 1:1) + 5% FEC (fluoroethylene carbonate) solution was used as the electrolyte. The batteries were assembled in a glove box under an argon atmosphere with an oxygen partial pressure of less than 0.01 PPM, a moisture pressure of less than 0.01 PPM, and constant current / constant voltage charge-discharge mode. Charge-discharge tests were conducted using a voltage range of 2-4 V and a current density of 0.1 C-0.2 C-0.5 C-1 C.

[0080] The sodium iron phosphate pyrophosphate prepared in Examples 1-8 and Comparative Examples 1-6 were used as test samples for the compaction density meter. The test was conducted using a PCD2000 compaction-powder resistivity meter from Yuaneng Technology under a test pressure of 3T.

[0081] Table 1: Performance Test Data of Each Embodiment and Comparative Example

[0082] 0.1C charging (mAh / g) 0.1C discharge (mAh / g) 1C discharge (mAh / g) 5C discharge (mAh / g) 10C discharge (mAh / g) Powder resistivity (Ω·m) Example 1 118 105 102 95 87 10.3 Example 2 117 104 101 96 87 9.5 Example 3 114 100 98 95 84 8.6 Example 4 109 98 96 92 83 7.2 Example 5 117 104 101 94 80 10.4 Example 6 118 105 102 94 84 9.8 Example 7 118 104 102 94 82 9.6 Example 8 118 105 101 95 86 18.3 Comparative Example 1 120 107 104 93 79 30.9 Comparative Example 2 114 101 96 92 66 16.8 Comparative Example 3 117 104 101 94 84 9.9 Comparative Example 4 115 103 100 93 82 9.8 Comparative Example 5 114 101 96 93 83 13.9 Comparative Example 6 116 102 99 94 84 13.5

[0083] Examples 1-4 of the present invention and Comparative Example 1 were tested under the same conditions, and the results are shown in Table 1. With increasing vanadium doping content, the powder resistivity of the material decreased, indicating that the addition of vanadium effectively improved the conductivity and electrochemical activity of the material. Simultaneously, the high-rate performance of the material was significantly improved. Compared to the undoped material in Comparative Example 1, the 10C discharge specific capacity of the material doped with 0.006 mol of vanadium in Example 1 was significantly improved. However, with increasing vanadium doping content, the 0.1C first-cycle charge-discharge specific capacity of the material decreased. This is because after vanadium atoms occupy the positions of iron atoms, a larger amount of inactive NaFePO4 phase is generated, leading to a decrease in the specific capacity. Combining the discharge specific capacity, high-rate performance, and resistivity of the material, the material doped with 0.012 mol of vanadium can achieve a good balance between specific capacity and low resistivity.

[0084] Examples 5-6 of the present invention were tested under the same conditions as Example 2, and the results are shown in Table 1. After adjusting the proportion of the coated carbon source, it was found that more PEG (polyethylene glycol) coating is beneficial to the high-rate capacity of the material.

[0085] Examples 7-8, Example 2, and Comparative Example 2 of the present invention were tested under the same conditions, and the results are shown in Table 1. After adjusting the proportion of added oxalic acid dihydrate, it was found that an appropriate excess of oxalic acid dihydrate helps to grind to a finer particle size, and the molar ratio of oxalic acid dihydrate to sodium carbonate of 1.4:1 is more reasonable.

[0086] Comparative Examples 3-4 of the present invention were tested under the same conditions as Example 2, and the results are shown in Table 1: After selecting iron-based ferric phosphate with a low iron-to-phosphorus ratio, the discharge specific capacity of the material decreased by 1-2 mAh / g, indicating that iron-based ferric phosphate with a low iron-to-phosphorus ratio is not suitable for preparing high-capacity materials.

[0087] Comparative Examples 5-6 of the present invention were tested under the same conditions as Example 2, and the results are shown in Table 1: After selecting ammonium ferric phosphate and sodium ferric phosphate, the particle size in the fine grinding process could not meet the process requirements, and it was also not suitable for preparing high-capacity materials.

[0088] Figure 1 This is a scanning electron microscope image of the lamellar iron phosphate used in this invention. As can be seen from the image, the morphology of this iron phosphate is a typical lamellar structure, with layers stacked together to form irregularly shaped particles.

[0089] Figure 2This is a scanning electron microscope (SEM) image of sodium iron pyrophosphate prepared in Example 2 of this invention. As can be seen from the image, the particles are spherical, with a particle size of 3-15 μm. The particle surfaces are relatively smooth, and the carbon coating on the particle surfaces is well-done.

[0090] Figure 3 This is a rate charge-discharge curve of the sodium-ion battery prepared in Example 2 of the present invention. The sample can provide discharge specific capacities of 104.50 mAh / g, 103.01 mAh / g, 102.94 mAh / g, 101.54 mAh / g, 96.96 mAh / g, and 87.43 mAh / g at rates of 0.1C, 0.2C, 0.5C, 1C, 5C, and 10C, respectively.

[0091] The foregoing has only described certain exemplary embodiments of the present invention by way of illustration. Undoubtedly, those skilled in the art can modify the described embodiments in various ways without departing from the spirit and scope of the present invention. Therefore, the foregoing drawings and descriptions are illustrative in nature and should not be construed as limiting the scope of protection of the claims of the present invention.

Claims

1. A sodium iron phosphate pyrophosphate cathode material for start-stop operation, characterized in that, The chemical formula of the cathode material is Na. 4.08 Fe 2.9 V x T(PO4)2P2O7, where 0.006≤x≤0.

024.

2. A method for preparing a sodium iron phosphate pyrophosphate cathode material for start-stop operation, used to prepare the sodium iron phosphate pyrophosphate cathode material for start-stop operation as described in claim 1, characterized in that, The preparation method includes the following steps: S1: Add sodium source, iron source, phosphorus source, carbon source, vanadium source and dicarboxylic acid to water and disperse evenly to obtain a slurry; S2: The mixed slurry is sand-milled to obtain grinding material; S3: The abrasive material is finely ground to obtain fine abrasive material; S4: Transfer the finely ground material into a spray dryer for spray granulation to obtain the precursor; S5: The precursor is pulverized to obtain precursor powder; S6: The precursor powder is sintered to obtain sodium iron phosphate pyrophosphate cathode material. In S3, the fine sand milling process is configured to combine with the corrosive effect of dicarboxylic acid on ferric phosphate, grinding ferric phosphate to a particle size of D50=150±10nm, D90≤260nm.

3. The method for preparing sodium iron phosphate pyrophosphate cathode material for start-up and shutdown according to claim 2, characterized in that, In S1, the iron source is iron-based ferric phosphate, and the iron-to-phosphorus ratio of the iron-based ferric phosphate is 0.965~0.

971.

4. The method for preparing sodium iron phosphate pyrophosphate cathode material for start-up and shutdown according to claim 2, characterized in that, In S1, the sodium source is one or more of sodium carbonate, sodium oxalate, sodium pyrophosphate, sodium dihydrogen pyrophosphate, sodium dihydrogen phosphate, and disodium hydrogen phosphate. The phosphorus source is one or more of sodium pyrophosphate, sodium dihydrogen pyrophosphate, sodium dihydrogen phosphate, disodium hydrogen phosphate, ammonium dihydrogen phosphate, and diammonium hydrogen phosphate. The carbon source is one or more of glucose, sucrose, citric acid, ascorbic acid, and polyethylene glycol; The vanadium source is one or more of vanadium carbonate, vanadium pentoxide, and ammonium metavanadate. The dicarboxylic acid is one or more of oxalic acid dihydrate, oxalic acid (ethanedioic acid), malonic acid, and succinic acid.

5. The method for preparing sodium iron phosphate pyrophosphate cathode material for start-up and shutdown according to claim 2, characterized in that, In S1, the molar ratio of sodium, iron, and phosphorus is 4.08:2.9:4, the carbon source accounts for 12% to 16% of the total weight of the iron source, the molar doping amount of vanadium is 0.006 to 0.024, and the molar amount of the dicarboxylic acid is 120% to 160% of the sodium source.

6. The method for preparing sodium iron phosphate pyrophosphate cathode material for start-up and shutdown according to claim 2, characterized in that, In S2, the specific steps of the sand milling process are as follows: the mixed slurry is placed in a fine mill, and zirconia beads with a diameter of 0.3-0.4 mm and a 0.15 mm sieve are used. The milling is carried out at a speed of 1200 rpm for several hours, and the particle size of the grinding material is controlled to be D50=220±10nm and D90≤480nm.

7. The method for preparing sodium iron phosphate pyrophosphate cathode material for start-up and shutdown according to claim 2, characterized in that, In S3, the specific steps of fine grinding are as follows: the grinding slurry of S2 is placed in a fine grinding machine, and zirconia beads with a diameter of 0.2-0.3 mm and a 0.1 mm sieve are used to grind it at a speed of 1200 rpm for several hours.

8. The method for preparing sodium iron phosphate pyrophosphate cathode material for start-up and shutdown according to claim 2, characterized in that, In step S4, the specific steps of spray granulation are as follows: the fine grinding material is transferred into a spray dryer and granulated under the conditions of inlet air temperature of 220°C, atomizing disc rotation speed of 400Hz and outlet air temperature of 96°C to obtain a spherical precursor with a particle size D50=35±5μm.

9. The method for preparing sodium iron phosphate pyrophosphate cathode material for start-up and shutdown according to claim 2, characterized in that, In S5, the particle size of the precursor is D50 = 6 ± 0.5 μm.

10. The method for preparing sodium iron phosphate pyrophosphate cathode material for start-up and shutdown according to claim 2, characterized in that, In S6, the sintering process is as follows: the temperature is increased from room temperature to 300℃ at a heating rate of 2℃ / min, held at N2 atmosphere for 3 hours, and then increased to 500℃~600℃ at a heating rate of 2℃ / min, held at N2 atmosphere for 10 hours.

Citation Information

Patent Citations

  • Sodium vanadium fluorophosphate coated sodium ferric pyrophosphate composite material and preparation method thereof

    CN117691075A

  • Porous positive electrode material, preparation method thereof, positive electrode plate, secondary battery and electric equipment

    CN118431464A

  • Preparation method of metal niobium doped ferric sodium pyrophosphate positive electrode material and vehicle

    CN118630202A

  • NaaFeb (PO4) cP2O7 / C composite material, preparation method thereof and application of NaaFeb (PO4) cP2O7 / C composite material in sodium ion battery

    CN118811792A