A hard carbon material, a preparation method and application thereof
By subjecting hard carbon materials to controlled oxidation and high-temperature reconstruction, an interconnected pore network is formed, solving the problem of isolated closed pores after high-temperature treatment and improving the electrochemical performance and large-scale application potential of sodium-ion batteries.
Patent Information
- Application Number
- CN202611094262.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-22
- Publication Date
- 2026-11-24
AI Technical Summary
Existing hard carbon materials form a large number of isolated closed pores after high-temperature treatment, which leads to slow sodium ion diffusion kinetics and reduced rate performance. Moreover, existing methods are complex, costly and difficult to scale up.
By subjecting hard carbon materials to controlled oxidation, blocked pores are opened and an interconnected pore network structure is formed. Combined with high-temperature reconstruction, an interconnected network of internal pores is formed, thus solving the problem of isolated closed pores.
It improves the low-voltage plateau capacity and reversible specific capacity of sodium-ion batteries, enhances the first coulombic efficiency and ion transport kinetics, simplifies the process flow, and is suitable for performance upgrades of commercial hard carbon materials.
Smart Images

Figure CN123162186A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of hard carbon materials technology, and in particular to a hard carbon material, its preparation method, and its application. Background Technology
[0002] With the development of large-scale energy storage, low-speed electric vehicles, and renewable energy grid connection technologies, low-cost, high-safety, and long-life rechargeable battery systems have attracted widespread attention. Sodium-ion batteries, due to the abundance and wide distribution of sodium resources, low cost, and environmental friendliness, are considered an important supplement or even replacement for lithium-ion batteries in the field of large-scale energy storage.
[0003] Anode materials are a key component determining the energy density, rate performance, and cycle life of sodium-ion batteries. Hard carbon materials, with their complex structures including amorphous carbon layers, disordered graphite microcrystals, defect sites, and internal nanopores, are considered one of the most promising anode materials for sodium-ion batteries due to their high sodium storage capacity, low operating potential, good cycle stability, and good compatibility with sodium-ion battery electrolyte systems.
[0004] The sodium storage curves of hard carbon materials typically include a high-voltage ramp region and a low-voltage plateau region. The ramp region is mainly related to adsorption from surface defects, adsorption at edge sites, and a small amount of interlayer intercalation processes; the low-voltage plateau region is generally associated with the accumulation and filling of sodium ions in the closed pores within the hard carbon, and the formation of quasi-metallic sodium clusters. Since the sodium storage potential in the low-voltage plateau region is close to the metallic sodium potential, a higher plateau capacity is more beneficial for improving the output voltage and energy density of the full cell. Therefore, improving the low-voltage plateau capacity of hard carbon materials is an important direction for developing high-energy-density sodium-ion battery anode materials.
[0005] Existing technologies for enhancing the capacity of hard carbon platforms mainly include precursor regulation, pore-forming with template agents, chemical activation, metal salt-assisted pyrolysis, and increasing carbonization temperature. For example, by introducing zinc oxide, zinc acetate, magnesium oxide, potassium hydroxide, or other inorganic templates / activators into the carbon precursor, more porous structures can be constructed during pyrolysis, thereby increasing sodium storage capacity. However, these methods typically rely on specific precursors or template agents, and suffer from complex steps, cumbersome washing processes, high risk of impurity residues, high production costs, and difficulties in scaling up. For commercially available or already prepared hard carbon materials, the aforementioned precursor engineering strategies are difficult to apply directly.
[0006] Another simpler strategy is to perform high-temperature annealing on hard carbon materials. High-temperature annealing can promote carbon layer ordering, reduce surface defect content, decrease irreversible reaction sites, and improve initial coulombic efficiency to some extent. Simultaneously, high-temperature treatment also facilitates the closure of some pore structures, thereby forming the pores required for sodium storage. However, direct high-temperature annealing presents a significant structural contradiction: on the one hand, high-temperature treatment promotes pore formation; on the other hand, it can also induce excessive densification and localized graphitization shrinkage of the carbon layer, blocking or interrupting the diffusion channels between the external environment and internal pores. This results in a large number of internal pores transforming into isolated closed pores or "dead pores" that are difficult for sodium ions to enter. Although these isolated closed pores may be detected as internal pores in structural characterization, they are difficult to utilize effectively in electrochemical processes, ultimately leading to insufficient plateau capacity, sluggish ion diffusion kinetics, and decreased rate performance.
[0007] Therefore, how to increase the number and volume of pores while maintaining an accessible internal transport network for ions, transforming pores from isolated closed pores or "dead pores" into "accessible interconnected pores," is a key technical problem that urgently needs to be solved in the design of high-capacity hard carbon anode materials. Furthermore, developing a simple, scalable post-treatment upgrade method for commercial or existing hard carbon materials, without the need for complex template agents and highly corrosive washing steps, is also a significant technical challenge for promoting the industrial application of high-performance hard carbon materials. Summary of the Invention
[0008] The purpose of this application is to provide a new hard carbon material, its preparation method, and its application.
[0009] To achieve the above objectives, this application adopts the following technical solution:
[0010] This application discloses a hard carbon material having an internal network structure with interconnected pores.
[0011] It should be noted that, compared with existing high-temperature treated hard carbon materials, the biggest difference of the hard carbon material in this application lies in the fact that its internal pores are interconnected to form a network structure. While increasing or maintaining the number and volume of pores, this allows ions to enter the internal transport network, solving the problem of forming a large number of isolated closed pores or "dead pores" at high temperatures. The internal pores of this application possess both closure and accessibility. The closure mainly refers to the ability of the pore space to effectively block the co-intercalation or direct contact of electrolyte solvent molecules; the accessibility refers to the ability of the pore space to allow ions to enter, diffuse, and aggregate. This accessibility is achieved through the interconnected network structure of the pores.
[0012] It should also be noted that, compared with existing high-temperature treated hard carbon materials, the hard carbon material of this application possesses an interconnected network structure that combines closure and accessibility, avoiding problems such as insufficient plateau capacity, sluggish ion diffusion kinetics, and decreased rate performance. When used, for example, as an anode material in sodium-ion batteries, the hard carbon material of this application can accommodate and store more sodium ions, thereby improving the low-voltage plateau capacity of the battery anode, enhancing the reversible specific capacity and initial coulombic efficiency, and laying the foundation for the preparation of high-capacity hard carbon anode materials.
[0013] In some implementations, hard carbon materials contain micropores or ultramicropores with a pore size of 0.3 to 2.0 nm.
[0014] Preferably, the hard carbon material contains ultramicropores with a pore size of 0.3~0.8 nm.
[0015] In some implementations, in a network structure where pores are interconnected, the interconnected channels between pores allow ions to enter and diffuse, and can prevent the co-intercalation of electrolyte solvent molecules or prevent direct contact between the electrolyte and the pores.
[0016] In some implementations, the raw materials for hard carbon materials are at least one of commercial hard carbon, coal-based hard carbon, resin-based hard carbon, pitch-based hard carbon, biomass-based hard carbon, organic polymer-based hard carbon, and recycled hard carbon from waste batteries.
[0017] It should be noted that the hard carbon material in this application can be any existing hard carbon material, including but not limited to commercial hard carbon, coal-based hard carbon, resin-based hard carbon, pitch-based hard carbon, biomass-based hard carbon, organic polymer-based hard carbon, and recycled hard carbon from waste batteries.
[0018] In some implementations, the pore network interconnection factor of the hard carbon material is 0.50~0.65, and the specific surface area is no higher than 20 m². 2 / g.
[0019] Preferably, the interconnection factor of the pore network is 0.54~0.60, and the specific surface area is not higher than 10 m². 2 / g.
[0020] In this application, the pore network interconnection factor (fa) is obtained by small-angle X-ray scattering (SAXS) testing of the hard carbon material and fitting it using a semi-empirical Teubner-Strey model, while the specific surface area (BET) is measured by nitrogen adsorption at 77 K. The hard carbon material in this application simultaneously satisfies the following requirements: a pore network interconnection factor (fa) of 0.50–0.65 and a nitrogen BET specific surface area at 77 K not exceeding 20 m². 2 / g; preferably, fa is 0.54~0.60, and the BET specific surface area of nitrogen is not higher than 10 m². 2 / g. The hard carbon material of this application has a high fa, indicating that it has a more interconnected internal pore network structure; at the same time, it has a low BET specific surface area of N2, indicating that its pore network is closed externally; this application can more accurately represent the interconnected network structure of the internal pores of the hard carbon material by combining the two parameters. In some implementations of this application, the hard carbon material (ICP-HC) has d=6.599nm and ξ=0.559nm, and the calculated fa=0.559; while the hard carbon material (ISO-HC) that is directly treated at 1600 °C without controlled oxidation treatment has a fa of only 0.186; the original commercial hard carbon material (HC) has a fa of 0.276; obviously, the fa of ICP-HC is about 3.0 times that of ISO-HC and 2.0 times that of the original HC, proving that the degree of interconnection of the internal pore network of ICP-HC is significantly improved.
[0021] It should be noted that in this application, the nitrogen BET specific surface area is calculated using the 77 K nitrogen adsorption isotherm and the BET model. The nitrogen BET specific surface area primarily reflects the open surface area directly connected to the outer surface of the particles and detectable by nitrogen. A lower nitrogen BET specific surface area does not alone equate to a higher internal porosity, but it indicates that the pore openings are closed or significantly narrowed after high-temperature reconstruction, thus reducing the external exposure of the pore network. Nitrogen adsorption and SAXS characterization are complementary: nitrogen BET specific surface area is used to evaluate the degree of openness of the pore structure, while SAXS and fa are used to evaluate the overall pore network topology, including internal pores that are difficult for gases to enter. Combining the two avoids judging the interconnected pore structure based on only a single result. Therefore, this application uses a higher fa and a lower nitrogen BET specific surface area as a combined quantitative characteristic of the interconnected pore network structure: a higher fa corresponds to internal pore network interconnection, and a lower nitrogen BET specific surface area corresponds to the external closure of the pore network. This combination can be distinguished from both oxidized hard carbon intermediates with high fa but a large number of open pores and directly high-temperature annealed hard carbon with low nitrogen BET specific surface area but isolated internal pores.
[0022] This application also discloses a battery negative electrode that uses the hard carbon material described in this application.
[0023] In some implementations, the reversible specific capacity of the negative electrode of the battery in this application is 350~500 mAh / g, and the initial coulombic efficiency is 85%~95%; preferably, the reversible specific capacity can reach 400~480 mAh / g, and the initial coulombic efficiency can reach 88%~95%.
[0024] In some implementations, the low-voltage plateau capacity of the battery negative electrode is 250~430 mAh / g; preferably, the low-voltage plateau capacity can reach 300~420 mAh / g; more preferably, the low-voltage plateau capacity can reach 350~410 mAh / g.
[0025] This application also discloses an ion battery containing the hard carbon material of this application, or the battery negative electrode of this application.
[0026] It is understood that the hard carbon material of this application and the negative electrode prepared therefrom are applicable to all existing ion batteries, including but not limited to various alkali metal ion batteries or multivalent metal ion batteries. Among them, alkali metal ion batteries include lithium-ion batteries, sodium-ion batteries, and potassium-ion batteries; multivalent metal ion batteries include magnesium-ion batteries, aluminum-ion batteries, calcium-ion batteries, and zinc-ion batteries.
[0027] In some implementations, the ion battery is a sodium-ion full cell with an operating voltage window of 1.5~4.2 V; preferably 2.0~3.8 V.
[0028] It should be noted that the key to the ion battery of this application lies in the use of the hard carbon material of this application or the negative electrode prepared therefrom. As for the specific type of ion battery and other components, existing ion batteries can be referenced. For example, a sodium-ion battery includes a conventional positive electrode, a negative electrode sheet, a separator, and an electrolyte; wherein, the negative electrode sheet is the battery negative electrode of this application or contains the hard carbon material of this application. It is understood that the hard carbon material of this application merely replaces the hard carbon material in existing negative electrode sheets, and other components in the negative electrode sheet can also refer to existing technologies. For example, the negative electrode sheet contains the hard carbon material of this application, a conductive agent, and a binder. The ratio of each component in the negative electrode sheet can also refer to existing technologies; for example, the mass ratio of hard carbon material, conductive agent, and binder is 70~98:1~20:1~20, preferably 80~95:2~10:2~10, and more preferably 90:5:5. The conductive agent can be a conventionally used conductive agent, such as at least one of Super P, acetylene black, conductive carbon black, carbon nanotubes, graphene, and conductive graphite. The binder can also be a conventional binder, such as at least one of sodium carboxymethyl cellulose, lithium carboxymethyl cellulose, polyacrylic acid, sodium polyacrylate, polyvinylidene fluoride, styrene-butadiene rubber, sodium alginate, and polyacrylonitrile. The current collector of the negative electrode includes at least one of aluminum foil, copper foil, stainless steel foil, carbon paper, or conductive carbon cloth. For sodium-ion batteries, aluminum foil is preferred as the negative electrode current collector. The positive electrode can be a conventional positive electrode, such as at least one of sodium vanadium phosphate, layered oxides, Prussian blue compounds, and polyanionic compounds; the preferred positive electrode is Na3V2(PO4)3. The electrolyte can be a conventional electrolyte, such as at least one sodium salt of NaPF6, NaClO4, NaFSI, and NaTFSI; the solvent of the electrolyte includes at least one of diethylene glycol dimethyl ether, ethylene glycol dimethyl ether, ethylene carbonate, diethyl carbonate, dimethyl carbonate, and methyl ethyl carbonate; in some implementations, for example, the electrolyte is a 1.0 mol / L diethylene glycol dimethyl ether solution of NaPF6.
[0029] This application also discloses the application of the hard carbon material of this application, the battery negative electrode of this application, or the ion battery of this application in grid energy storage, low-speed electric vehicles, backup power supplies, distributed energy storage, cryogenic energy storage, and fast-charging energy storage devices.
[0030] This application also discloses a method for preparing the hard carbon material of this application, including a controlled oxidation treatment of the hard carbon raw material to obtain an oxidized hard carbon intermediate; the oxidized hard carbon intermediate is subjected to high-temperature treatment under an inert atmosphere or vacuum conditions, and after cooling, a network structure in which diffusion channels between internal pores are interconnected is obtained; wherein, the controlled oxidation treatment includes oxidizing the hard carbon raw material in an oxygen-containing atmosphere at a temperature lower than but close to the combustion temperature of the hard carbon raw material.
[0031] The oxygen-containing atmosphere includes at least one of oxygen, air, a mixture of oxygen and an inert gas, an ozone atmosphere, a mixture of water vapor and oxygen, and a mixture of carbon dioxide and oxygen. The volume fraction of oxygen in the oxygen-containing atmosphere is 1% to 100%, preferably 5% to 100%, and more preferably 20% to 100%.
[0032] It should be noted that the hard carbon material preparation method of this application involves further processing of existing hard carbon raw materials, or further processing of the finished or semi-finished hard carbon products based on existing hard carbon raw material preparation processes to obtain the hard carbon material of this application.
[0033] It should be noted that the hard carbon material preparation method of this application, based on the existing high-temperature annealing treatment of hard carbon materials, creatively pre-treatments the materials with controlled oxidation. This involves oxidizing the hard carbon raw material in an oxygen-containing atmosphere at a temperature lower than, but close to, that of hard carbon raw material combustion. This application's research has found that oxidation under such critical temperature conditions can selectively remove disordered carbon regions in the hard carbon raw material, open blocked pores and / or connect isolated pores, forming a guiding structure for subsequent reconstruction. This allows subsequent high-temperature treatment to increase the number and volume of internal pores while maintaining an ion-accessible internal transport network, avoiding the generation of a large number of isolated closed pores or "dead pores" at high temperatures. It is understood that the high-temperature treatment in this application is the same as the existing high-temperature annealing treatment. One of the key aspects of this application is that a controlled oxidation treatment is performed before the high-temperature annealing treatment. The controlled oxidation selectively removes highly defective disordered carbon, opens the pores, and forms a subsequent reconstruction guiding structure. Through the synergistic treatment of "controlled oxidation-high-temperature reconstruction", the internal pore structure of hard carbon is transformed from an isolated state to an interconnected and accessible state, so that the hard carbon material of this application has more interconnected pores that can be entered by ions.
[0034] It should be noted that the preparation method of this application achieves the transformation of the closed pore structure inside hard carbon from an isolated state to an interconnected state through a synergistic process of "controlled oxidation-high temperature reconstruction". Controlled oxidation selectively etches disordered carbon regions in hard carbon that have low thermal stability, high defect levels, and strong reactivity, opening previously blocked micropore entrances, connecting previously isolated internal pores, and introducing defects and open channels into the carbon framework that can serve as guides for subsequent structural reconstruction. Subsequently, high-temperature reconstruction promotes the rearrangement, local ordering, pore wall closure, and pore fusion of the carbon layers in the oxidized hard carbon intermediate, transforming small-sized dispersed pores into an expanded interconnected pore network. Compared with direct high-temperature annealing, the method of this application can retain the connectivity between internal pores while closing the pore walls, avoiding excessive densification that could completely isolate the internal pores.
[0035] In this application, the interconnected pore network structure is different from conventional open pores and also different from completely inaccessible isolated closed pores. This interconnected pore network structure can serve as a nucleation and storage space for quasi-metallic sodium clusters and can also improve the electrochemical utilization rate of the internal pores, thereby significantly improving the low-voltage platform capacity and rate performance.
[0036] In this application, the oxidized hard carbon intermediate subjected to controlled oxidation treatment has a higher content of oxygen-containing functional groups compared to the hard carbon raw material; wherein, the oxygen-containing functional groups include at least one of CO, C=O, and OC=O; the oxidized hard carbon intermediate has a higher open pore content and / or a higher degree of pore connectivity compared to the hard carbon raw material.
[0037] It should be noted that the controlled oxidation process in this application is not intended to retain oxygen-containing functional groups in the long term, but rather to selectively remove highly defective disordered carbon, open pores, and form a subsequent reconstruction-guided structure through the oxidation process. The subsequent high-temperature reconstruction process can remove most of the unstable oxygen-containing functional groups, thereby reducing the oxygen content on the surface of the hard carbon material with the final interconnected porous network structure, thus reducing irreversible side reactions and maintaining a high initial coulombic efficiency.
[0038] In this application, the temperature is below but close to the combustion temperature of the hard carbon raw material, that is, the critical oxidation temperature window before obvious combustion in an oxygen-containing atmosphere; in other words, the controlled oxidation treatment of this application involves oxidizing the hard carbon raw material in an oxygen-containing atmosphere within the critical oxidation temperature window before obvious combustion. Hard carbon materials are flame-retardant carbon-based substances; no obvious combustion occurs if there is no obvious flame spread, no molten dripping, and the flame extinguishes immediately upon removal from the flame. Conversely, if there is a continuous open flame, violent exothermic temperature rise, or significant mass loss, it is determined that obvious combustion has occurred.
[0039] It should be noted that in the interconnected porous network structure of this application, the interconnected porous network is surrounded by closed or semi-closed carbon walls formed by carbon layer rearrangement, and internally forms connection channels that allow sodium ions to enter and diffuse. The hard carbon material with the interconnected porous network structure of this application has a higher degree of internal pore connectivity, higher carbon layer order, and higher electron transport capability compared to directly high-temperature annealed hard carbon materials. After selectively removing disordered carbon regions through controlled oxidation treatment, subsequent high-temperature reconstruction can promote carbon layer rearrangement, forming a continuous electron transport framework, thereby improving the electronic conductivity and rate performance of the hard carbon material.
[0040] In some implementations, the controlled oxidation treatment temperature is 250~550 ℃ and the treatment time is 0.1~24 h.
[0041] It should be noted that the controlled oxidation process temperature should not be too low or too high. If the oxidation process temperature is too low, for example below 250 °C, the selective etching effect of oxygen on the disordered carbon regions in hard carbon is insufficient, making it difficult to open blocked channels and establish a pore interconnection network. If the oxidation process temperature is too high, for example above 550 °C, the hard carbon matrix is prone to violent combustion or excessive gasification, resulting in severe loss of the carbon skeleton, structural collapse, and decreased yield. Therefore, the controlled oxidation process temperature is usually 250~550 °C. Preferably, the controlled oxidation process temperature is selected near the critical oxidation temperature before the hard carbon shows obvious combustion, so that oxygen can accurately etch high-energy disordered regions without causing uncontrolled combustion of the hard carbon matrix. For example, 250~550 °C is preferred, 300~500 °C is more preferred, 350~450 °C is even more preferred, and 380~420 °C is even more preferred.
[0042] Similarly, the controlled oxidation process time should not be too long or too short. If the controlled oxidation process time is too short, the disordered carbon etching will be insufficient, making it difficult to form continuous internal diffusion channels; if the controlled oxidation process time is too long, it may lead to excessive carbon loss, excessive opening of pore structures, and too many low-temperature oxidation defects, which will reduce the material yield or affect the first coulombic efficiency after subsequent high-temperature reconstruction. Therefore, the controlled oxidation process time is usually 0.1~24 h, preferably 1~12 h, and more preferably 3~8 h.
[0043] In some implementations, the controlled oxidation process has a heating rate of 0.5–20 °C / min. Preferably, the controlled oxidation process has a heating rate of 2–10 °C / min.
[0044] For example, in some implementations of this application, the controlled oxidation process includes heating to 400 °C at a heating rate of 5 °C / min in an oxygen atmosphere and holding at that temperature for 6 h.
[0045] In some implementations, the high-temperature treatment temperature is 1000~2200 ℃, and the treatment time is 0.1~12 h.
[0046] In some implementations, the inert atmosphere includes at least one of argon, nitrogen, helium, and neon.
[0047] For example, the high-temperature treatment time is 0.5–6 h or 1–3 h. For example, in some implementations, the high-temperature reconstruction treatment includes holding at 1600 °C for 2 h in an argon atmosphere.
[0048] It should be noted that the high-temperature treatment in this application, namely high-temperature reconstruction treatment or high-temperature annealing treatment, can promote the rearrangement of carbon layers, pore wall closure, pore fusion and / or reconstruction of closed pore structure in the hard carbon oxide intermediate; the high-temperature reconstruction treatment transforms at least partially the open pores in the hard carbon oxide intermediate into closed pores, and at least partially fuses the dispersed pores in the hard carbon oxide intermediate into an interconnected pore network; and removes at least some of the oxygen-containing functional groups in the hard carbon oxide intermediate.
[0049] It should also be noted that the high-temperature reconstruction temperature in this application should not be too low or too high. If the reconstruction temperature is too low, for example below 1000 °C, the carbon layer rearrangement, pore wall closure, and pore fusion will be insufficient, making it difficult to form a stable closed pore structure. If the reconstruction temperature is too high, for example above 2200 °C, it may lead to excessive graphitization of the carbon layer and excessive densification of the structure, causing the ion channels to be pinched back, and the internal pores to become unusable isolated closed pores, reducing sodium storage kinetics and plateau capacity. Therefore, the high-temperature reconstruction temperature is usually 1000~2200 °C, preferably 1200~2000 °C, more preferably 1400~1800 °C, even more preferably 1500~1700 °C, and in some specific implementations, the high-temperature treatment temperature is 1600 °C.
[0050] It should also be noted that, after the high-temperature reconstruction treatment in this application, the material is naturally cooled or programmed to room temperature to obtain a hard carbon material with interconnected pores. The preparation method of this application does not require the introduction of metal salt template agents, inorganic hard templates, or highly corrosive acid washing steps. Compared with traditional template methods, activation methods, or precursor engineering methods, the preparation method of this application can directly use finished or semi-finished hard carbon products as raw materials for post-processing upgrades. It has fewer process steps, controllable parameters, and strong equipment compatibility, making it more suitable for large-scale production and performance improvement of commercial hard carbon materials.
[0051] In some implementations, the hard carbon raw materials include at least one of commercial hard carbon, coal-based hard carbon, resin-based hard carbon, pitch-based hard carbon, biomass-based hard carbon, organic polymer-based hard carbon, and recycled hard carbon from waste batteries.
[0052] It should be noted that the preparation method of this application is, in principle, applicable to all existing hard carbon raw materials, including but not limited to various commercial hard carbons, coal-based hard carbons, resin-based hard carbons, pitch-based hard carbons, biomass-based hard carbons, organic polymer-based hard carbons, and hard carbons recycled from waste batteries. It is understood that the hard carbon raw material in this application is hard carbon powder that has already undergone carbonization treatment, such as commercial hard carbon powder, such as hard carbon anode materials for sodium-ion batteries. The commercial hard carbon in this application is hard carbon powder that has already been carbonized or whose graphitization degree has been controlled. It is understood that the method of this application does not rely on a specific carbon precursor, nor does it require the introduction of a template agent or metal salt before the pyrolysis of the precursor; therefore, it is particularly suitable for secondary processing of commercial hard carbon or already prepared hard carbon materials.
[0053] Due to the adoption of the above technical solutions, the beneficial effects of this application are as follows:
[0054] The hard carbon material of this application has more interconnected pores that allow ions to enter. When used as an anode material for ion batteries, it can achieve a balance between high plateau capacity, high initial coulombic efficiency, and fast ion transport kinetics, solving the problems of poor pore accessibility, low pore utilization efficiency, and limited plateau capacity in existing high-temperature treated hard carbon materials. Attached Figure Description
[0055] Figure 1 The TGA / DSC curves for the intermediate oxidation process in the embodiments of this application are shown.
[0056] Figure 2 The CO2 and H2O signals are from the in-situ TG-MS curves of the oxidation process in the embodiments of this application.
[0057] Figure 3 The typical SEM morphology of the hard carbon material in the embodiments and comparative examples of this application is shown.
[0058] Figure 4 The transmission electron microscopy (TEM) results of the hard carbon materials in the embodiments and comparative examples of this application are shown.
[0059] Figure 5 The X-ray diffraction (XRD) results of the hard carbon materials in the embodiments and comparative examples of this application are shown.
[0060] Figure 6 XPS and Raman results for hard carbon materials in the embodiments and comparative examples of this application;
[0061] Figure 7 The nitrogen adsorption isotherms of the hard carbon material in the embodiments and comparative examples of this application are shown below.
[0062] Figure 8 The X-ray small-angle scattering (SAXS) results of hard carbon materials in the embodiments and comparative examples of this application are shown.
[0063] Figure 9 The calculation results of the pore network interconnection factor fa of the hard carbon material in the embodiments and comparative examples of this application;
[0064] Figure 10 The charge-discharge curves of the coin cells assembled from hard carbon materials in the embodiments and comparative examples of this application are shown at a current density of 20 mA / g. Detailed Implementation
[0065] This application reveals that while existing direct high-temperature annealing of hard carbon can form a certain closed pore structure and improve the initial coulombic efficiency, the high-temperature-induced carbon layer densification easily interrupts ion diffusion channels, causing many internal pores to transform into isolated closed pores that cannot be effectively utilized by sodium ions, thus limiting plateau capacity and rate performance. This application introduces a controlled oxidation step before high-temperature reconstruction, utilizing the selective etching effect of oxygen on the highly defective and disordered carbon regions in hard carbon to pre-open blocked pore entrances and connect internal isolated closed pores; subsequently, high-temperature reconstruction rearranges the carbon layers and closes the pore walls, thereby forming an interconnected pore network. This structure provides both efficient low-voltage sodium storage space and maintains fast ion transport paths, thus significantly improving the sodium storage capacity, plateau capacity, and rate performance of hard carbon materials.
[0066] The preparation method and the hard carbon material prepared in this application have the following advantages compared with the prior art:
[0067] (1) The preparation method of this application transforms isolated closed or blocked pores in hard carbon into an interconnected pore network that sodium ions can enter through the synergistic effect of controlled oxidation and high-temperature reconstruction, thus solving the problems of poor pore accessibility, low pore utilization efficiency and limited platform capacity in existing direct high-temperature annealed hard carbon.
[0068] (2) The controlled oxidation process of this application can selectively remove high-defect disordered carbon regions, open blocked channels and establish a pore interconnection network; the subsequent high-temperature reconstruction process can promote the rearrangement of carbon layers and closure of pore walls, transforming open channels into stable interconnected pore structures, thereby taking into account high platform capacity, high first coulombic efficiency and fast ion transport kinetics.
[0069] (3) The method of this application does not depend on specific precursors, does not require complex template agents, metal salt activators or highly corrosive acid washing steps, and can be directly used for performance upgrades of commercial hard carbon, coal-based hard carbon, resin-based hard carbon, biomass hard carbon or recycled hard carbon. It has the advantages of simple process, controllable parameters, strong scalability and good industrial applicability.
[0070] (4) The interconnected porous network structure hard carbon material prepared in this application can provide abundant internal nucleation and storage space for quasi-metallic sodium clusters, reduce the diffusion resistance in the deep sodium intercalation / pore filling stage, and improve the low-voltage plateau capacity and rate performance. When this material is used as the anode of sodium-ion batteries, it can achieve high reversible capacity, high initial coulombic efficiency, excellent rate performance and stable cycle performance.
[0071] In summary, this application selectively removes highly defective and disordered carbon regions in hard carbon through controlled oxidation, opening previously blocked micropore channels and connecting isolated pores. Subsequently, high-temperature reconstruction promotes carbon layer rearrangement, pore wall closure, and pore fusion, thereby forming an interconnected pore network within the hard carbon that combines both closure and accessibility. This interconnected pore structure provides abundant access for sodium ions to the internal sodium storage space, reduces sodium cluster nucleation resistance, and improves pore utilization efficiency, solving the problems of closed-pore isolation, blocked ion transport paths, insufficient plateau capacity, and limited rate performance in existing high-temperature hard carbon materials. When used as an anode material for sodium-ion batteries, the hard carbon material prepared in this application exhibits high reversible specific capacity, plateau capacity, initial coulombic efficiency, rate performance, and cycle stability, making it suitable for high-energy-density sodium-ion batteries and related energy storage devices.
[0072] The present application will be further described in detail below through specific embodiments. The following embodiments are only for further illustration of the present application and should not be construed as limiting the present application.
[0073] Unless otherwise specified, the technical means used in the embodiments are conventional means well known to those skilled in the art.
[0074] Example 1
[0075] Preparation of interconnected porous hard carbon materials
[0076] 1) Controlled oxidation treatment: Commercial hard carbon powder (Kuraray Corporation, Japan, Type 2 battery-grade hard carbon) was used as the hard carbon raw material, denoted as HC. The HC powder was spread evenly in a corundum boat and placed in a tube furnace. Under continuous oxygen flow, the temperature was increased to 400 °C at a rate of 5 °C / min and held at 400 °C for 6 h to induce controlled oxidation of the hard carbon powder. After the oxidation treatment, the powder was naturally cooled to room temperature, and the resulting oxidized hard carbon intermediate was collected, denoted as O-HC.
[0077] 2) High-temperature reconstruction treatment: The O-HC obtained in step 1) was spread evenly in a corundum boat and placed in a high-temperature furnace. The temperature was raised to 1600 °C and held for 2 h under a flowing argon atmosphere, causing carbon layer rearrangement, pore wall closure, and pore structure reconstruction in the oxidized hard carbon intermediate. After the high-temperature treatment, it was naturally cooled to room temperature, and the resulting black powder was collected. This black powder is the hard carbon material with an internal network structure of interconnected pores, denoted as ICP-HC.
[0078] It should be noted that the 400 °C in step 1) is the critical oxidation temperature window before the commercial hard carbon used in this embodiment undergoes significant combustion in an oxygen atmosphere. At this temperature, oxygen can selectively etch highly defective and disordered carbon regions in the hard carbon and open blocked pores without causing severe combustion of the hard carbon matrix. The 1600 °C high-temperature reconstruction in step 2) can remove unstable oxygen-containing functional groups introduced during the oxidation process and promote carbon layer rearrangement and pore structure closure, thereby forming an interconnected porous structure that combines sealing and connectivity. Detailed preparation methods and process flow diagrams involved in this embodiment are shown below. Figure 1 and 2 As shown.
[0079] The obtained hard carbon material ICP-HC was mixed with acetylene black (Denka black Li435, Denka Corporation, Japan) and sodium carboxymethyl cellulose (CMC) (Daicel Corporation, CMC2200, Japan) in a mass ratio of 90:5:5. The mixture was ground evenly, and then deionized water was added to form a slurry. The slurry was then evenly coated onto copper foil using a coating machine and placed in a vacuum drying oven at 100 °C for 12 h. After that, it was processed into a circular electrode with a diameter of 10 mm using a die-casting machine.
[0080] The obtained circular electrode was used as the negative electrode, a glass fiber disc (Cytiva, UK, Whatman-GF / D) with a diameter of 19 mm was used as the separator, and a sodium metal sheet (Aladdin, China, S108757) with a diameter of 15.6 mm and a thickness of 0.4 mm was used as the counter electrode and reference electrode. The electrolyte was a 1 mol / L sodium hexafluorophosphate / diethylene glycol dimethyl ether solution. The sodium-ion battery was assembled in a glove box filled with high-purity argon gas according to the construction of a CR2032 standard coin cell.
[0081] After the obtained sodium-ion battery was left to stand at room temperature for 12 h, charge-discharge tests were conducted under constant current conditions and a current density of 20 mA / g.
[0082] Comparative Example 1
[0083] Preparation of hard carbon materials by direct high-temperature annealing
[0084] Commercial hard carbon powder HC, the same as in Example 1, was heated directly to 1600 °C and held for 2 h under a flowing argon atmosphere without controlled oxidation treatment. After the high-temperature treatment, it was naturally cooled to room temperature, and the resulting hard carbon material was collected and designated as ISO-HC.
[0085] The obtained hard carbon anode material ISO-HC was mixed with acetylene black and sodium carboxymethyl cellulose (CMC) in a mass ratio of 90:5:5, ground evenly, and then deionized water was added to form a slurry. The slurry was evenly coated onto copper foil using a coating machine and placed in a vacuum drying oven at 100 °C for 12 h. After that, it was prepared into a circular electrode with a diameter of 10 mm using a punching machine.
[0086] The obtained circular electrode was used as the negative electrode, a glass fiber (Whatman, GF / D) disc with a diameter of 19 mm was used as the separator, and a sodium metal sheet with a diameter of 15.6 mm and a thickness of 0.4 mm was used as the counter electrode and reference electrode. The electrolyte was a 1 mol / L sodium hexafluorophosphate / diethylene glycol dimethyl ether solution. The sodium-ion battery was assembled in a glove box filled with high-purity argon gas according to the construction of a CR2032 standard coin cell.
[0087] After the obtained sodium-ion battery was left to stand at room temperature for 12 h, charge-discharge tests were conducted under constant current conditions and a current density of 20 mA / g.
[0088] Comparative Example 2
[0089] Preparation of hard carbon oxide intermediates
[0090] Take the same commercial hard carbon powder HC as in Example 1, and perform controlled oxidation treatment at 400 °C in an oxygen atmosphere according to step 1) of Example 1. After the treatment, no high-temperature reconstruction is performed, and the resulting material is denoted as O-HC.
[0091] The obtained hard carbon anode material O-HC was mixed with acetylene black and sodium carboxymethyl cellulose (CMC) in a mass ratio of 90:5:5, ground evenly, and then deionized water was added to form a slurry. The slurry was evenly coated onto copper foil using a coating machine and placed in a vacuum drying oven at 100 °C for 12 h. After that, it was prepared into a circular electrode with a diameter of 10 mm using a die-casting machine.
[0092] The obtained circular electrode was used as the negative electrode, a glass fiber (Whatman, GF / D) disc with a diameter of 19 mm was used as the separator, and a sodium metal sheet with a diameter of 15.6 mm and a thickness of 0.4 mm was used as the counter electrode and reference electrode. The electrolyte was a 1 mol / L sodium hexafluorophosphate / diethylene glycol dimethyl ether solution. The sodium-ion battery was assembled in a glove box filled with high-purity argon gas according to the construction of a CR2032 standard coin cell.
[0093] After the obtained sodium-ion battery was left to stand at room temperature for 12 h, charge-discharge tests were conducted under constant current conditions and a current density of 20 mA / g.
[0094] Example 2
[0095] Preparation of interconnected porous hard carbon materials at different oxidation temperatures
[0096] Except for adjusting the controlled oxidation temperatures to 350 °C, 380 °C, 420 °C, and 450 °C respectively, the remaining steps were the same as in Example 1. All the resulting materials underwent subsequent high-temperature reconstruction treatment at 1600 °C in an argon atmosphere.
[0097] The obtained hard carbon material was mixed with acetylene black and sodium carboxymethyl cellulose (CMC) in a mass ratio of 90:5:5, ground evenly, and then deionized water was added to form a slurry. The slurry was then evenly coated onto copper foil using a coating machine and placed in a vacuum drying oven at 100 °C for 12 h. After that, it was prepared into a circular electrode with a diameter of 10 mm using a punching machine.
[0098] The obtained circular electrode was used as the negative electrode, a glass fiber (Whatman, GF / D) disc with a diameter of 19 mm was used as the separator, and a sodium metal sheet with a diameter of 15.6 mm and a thickness of 0.4 mm was used as the counter electrode and reference electrode. The electrolyte was a 1 mol / L sodium hexafluorophosphate / diethylene glycol dimethyl ether solution. The sodium-ion battery was assembled in a glove box filled with high-purity argon gas according to the construction of a CR2032 standard coin cell.
[0099] After the obtained sodium-ion battery was left to stand at room temperature for 12 h, charge-discharge tests were conducted under constant current conditions and a current density of 20 mA / g.
[0100] Example 3
[0101] Preparation of interconnected porous hard carbon materials at different high-temperature reconstruction temperatures
[0102] Except for adjusting the high-temperature reconstruction processing temperatures to 1400 ℃, 1500 ℃, 1700 ℃ and 1800 ℃ respectively, the remaining steps are the same as in Example 1.
[0103] The obtained hard carbon material was mixed with acetylene black and sodium carboxymethyl cellulose (CMC) in a mass ratio of 90:5:5, ground evenly, and then deionized water was added to form a slurry. The slurry was then evenly coated onto copper foil using a coating machine and placed in a vacuum drying oven at 100 °C for 12 h. After that, it was prepared into a circular electrode with a diameter of 10 mm using a punching machine.
[0104] The obtained circular electrode was used as the negative electrode, a glass fiber (Whatman, GF / D) disc with a diameter of 19 mm was used as the separator, and a sodium metal sheet with a diameter of 15.6 mm and a thickness of 0.4 mm was used as the counter electrode and reference electrode. The electrolyte was a 1 mol / L sodium hexafluorophosphate / diethylene glycol dimethyl ether solution. The sodium-ion battery was assembled in a glove box filled with high-purity argon gas according to the construction of a CR2032 standard coin cell.
[0105] After the obtained sodium-ion battery was left to stand at room temperature for 12 h, charge-discharge tests were conducted under constant current conditions and a current density of 20 mA / g.
[0106] Example 4
[0107] Upgraded processing of different hard carbon raw materials
[0108] Bamboo-based biomass hard carbon (Suzhou Yituolian International Trade Co., Ltd., ETY-B002-M), coal-based hard carbon (Suzhou Yituolian International Trade Co., Ltd., ETY-E004-M), resin-based hard carbon (Suzhou Yituolian International Trade Co., Ltd., ETY-F004-M), and waste battery recycled hard carbon (Wuxi Pangu New Energy Co., Ltd., PG-Na32140-10P) were selected as hard carbon raw materials and processed according to the controlled oxidation-high temperature reconstruction method described in Example 1.
[0109] The obtained hard carbon material was mixed with acetylene black and sodium carboxymethyl cellulose (CMC) in a mass ratio of 90:5:5, ground evenly, and then deionized water was added to form a slurry. The slurry was then evenly coated onto copper foil using a coating machine and placed in a vacuum drying oven at 100 °C for 12 h. After that, it was prepared into a circular electrode with a diameter of 10 mm using a punching machine.
[0110] The obtained circular electrode was used as the negative electrode, a glass fiber (Whatman, GF / D) disc with a diameter of 19 mm was used as the separator, and a sodium metal sheet with a diameter of 15.6 mm and a thickness of 0.4 mm was used as the counter electrode and reference electrode. The electrolyte was a 1 mol / L sodium hexafluorophosphate / diethylene glycol dimethyl ether solution. The sodium-ion battery was assembled in a glove box filled with high-purity argon gas according to the construction of a CR2032 standard coin cell.
[0111] After the obtained sodium-ion battery was left to stand at room temperature for 12 h, charge-discharge tests were conducted under constant current conditions and a current density of 20 mA / g.
[0112] The results of the reversible sodium storage capacity and first-week coulombic efficiency tests for each embodiment and comparative example are summarized in Table 1.
[0113] Table 1
[0114] Reversible sodium storage capacity First week Coulomb efficiency Example 1 437 mAh / g 91.5% Comparative Example 1 300 mAh / g 90.3% Comparative Example 2 98 mAh / g 39.8% Example 2 - Experiment 1 330 mAh / g 89.5% Example 2 - Experiment 2 388 mAh / g 90.2% Example 2 - Experiment 3 376 mAh / g 88.6% Example 2 - Experiment 4 / / Example 3 - Experiment 1 379 mAh / g 88.4% Example 3 - Experiment 2 398 mAh / g 89.1% Example 3 - Experiment 3 413 mAh / g 91.6% Example 3 - Experiment 4 392 mAh / g 92.2% Example 4 - Experiment 1 421 mAh / g 90.5% Example 4 - Experiment 2 407 mAh / g 90.1% Example 4 - Experiment 3 456 mAh / g 91.8% Example 4 - Experiment 4 392 mAh / g 88.7%
[0115] In Table 1, Examples 2-Experiment 1 to 2-Experiment 4 are sodium-ion batteries prepared using hard carbon materials prepared with controlled oxidation treatment temperatures of 350 ℃, 380 ℃, 420 ℃ and 450 ℃, respectively; Examples 3-Experiment 1 to 3-Experiment 4 are sodium-ion batteries prepared using hard carbon materials prepared with high-temperature reconstruction treatment temperatures of 1400 ℃, 1500 ℃, 1700 ℃ and 1800 ℃, respectively; Examples 4-Experiment 1 to 4-Experiment 4 are sodium-ion batteries prepared using hard carbon materials prepared with bamboo-based biomass hard carbon, coal-based hard carbon, resin-based hard carbon and recycled hard carbon from waste batteries, respectively.
[0116] Table 1 shows that the results of Example 1, Comparative Example 1 and Comparative Example 2 demonstrate that controlled oxidation treatment combined with high-temperature reconstruction treatment can effectively improve the reversible sodium storage capacity and first-cycle coulombic efficiency of sodium-ion batteries prepared from hard carbon materials.
[0117] The results of Example 2 show that, except for the controlled oxidation treatment temperature in Experiment 4 of Example 2 being too high, which caused the material to burn out and become unusable, oxygen was able to selectively etch the disordered carbon regions in the hard carbon within the above-mentioned temperature range, forming a certain degree of interconnected porous structure after subsequent high-temperature reconstruction. However, when the oxidation temperature was too low, the pore opening and pore connectivity were insufficient; when the oxidation temperature was too high, the loss of carbon skeleton and the introduction of defects increased, which may affect the material yield and final electrochemical stability. Therefore, for the commercial hard carbon used in this example, 380~420 °C is a better oxidation temperature range, and 400 °C is a further preferred condition.
[0118] It should be noted that the controlled oxidation treatment uses a temperature lower than but close to the combustion temperature of the hard carbon raw material, generally ranging from 250 to 550 °C. However, for the commercial hard carbon powder specifically used in Example 2, it has already been burned off at 450 °C. Therefore, an oxidation temperature of 380 to 420 °C is preferred, and 400 °C is more preferable. It is understood that the specific preferred controlled oxidation temperature varies for different hard carbon raw materials; however, as long as a controlled oxidation treatment is performed at a temperature lower than but close to the combustion temperature of the hard carbon raw material, the same or similar effects can be achieved.
[0119] The results of Example 3 show that the high-temperature reconstruction temperature significantly affects the ordering of the carbon layer, pore wall closure, and the formation of interconnected pore structures. At lower temperatures, the open pores and defects formed after oxidation are difficult to close and reconstruct sufficiently, resulting in limited improvements in material plateau capacity and initial coulombic efficiency. At excessively high temperatures, over-densification of the carbon layer may cause the pores to be re-interlocked, reducing the accessibility of internal pores. Therefore, for the hard carbon material used in this example, 1500–1700 °C is a preferred high-temperature reconstruction temperature range, and 1600 °C is a further preferred condition.
[0120] The results of Example 4 show that controlled oxidation-high temperature reconstruction treatment can improve the accessibility of internal pore structures and enhance low-voltage plateau capacity or rate performance of hard carbon materials from different sources to a certain extent. This indicates that the method of this application has good raw material versatility and can be used for performance upgrades of various hard carbon materials.
[0121] Furthermore, the oxidized hard carbon intermediate O-HC prepared in Example 1 was analyzed by TGA / DSC, and the results are as follows: Figure 1 As shown. Figure 1 The results showed that O-HC began to exhibit significant mass changes at approximately 450-650 °C, with a marked exothermic peak accompanied by rapid weight loss, indicating that a vigorous oxidative combustion process of hard carbon occurred. However, no significant exothermic peak or weight loss was observed below 400 °C. This result suggests that oxidation at 400 °C falls within a "selective etching window," which can prevent complete combustion of the main structure, thereby constructing the active structural basis required for subsequent reconstruction.
[0122] In-situ TG-MS analysis of the oxidation process of the oxidized hard carbon intermediate prepared in Example 1 was performed, and the results are as follows: Figure 2 As shown. Figure 2 The results show that the CO2 signal exhibits a significant peak at approximately 450-650 °C, indicating that the hard carbon components are preferentially converted into CO2 gas during oxidation. The H2O signal is weak, indicating a low H content in the hard carbon material. Below 400 °C, the CO2 signal is very weak, corresponding to the selective oxidation of the low-stability, disordered carbon components. This result further proves that at 400 °C, the controlled oxidation of hard carbon is dominated by selective etching rather than homogeneous bulk combustion, which is beneficial for forming a reconfigurable interconnected pore structure.
[0123] The morphology and structure of hard carbon raw material HC, hard carbon material ICP-HC prepared in Example 1, hard carbon material ISO-HC prepared in Comparative Example 1, and hard carbon material O-HC prepared in Comparative Example 2 were observed by SEM. The results are as follows: Figure 3 As shown. Figure 3The results showed that the original hard carbon (HC) exhibited a typical and irregular blocky / granular structure with a relatively smooth surface and sharp edges. After a low-temperature pre-oxidation treatment at 400 °C, the particle size, macroscopic shape, and overall morphology of O-HC showed almost no perceptible changes compared to the original HC, maintaining its complete blocky characteristics. After further high-temperature heat treatment, the comparative sample ISO-HC and the sample ICP-HC from the present application also perfectly inherited the macroscopic blocky framework structure of the original hard carbon, without obvious particle pulverization, melting agglomeration, or severe surface collapse. This indicates that the pre-oxidation reaction conducted at 400 °C in this application is essentially a mild micropore control process without significantly damaging the macroscopic three-dimensional framework structure of the hard carbon material. Subsequently, this stable macroscopic morphology was also successfully maintained during the high-temperature heat treatment. This demonstrates the efficiency and feasibility of this modification strategy in achieving precise microstructure construction while maintaining the integrity of the material's macroscopic structure.
[0124] Transmission electron microscopy (TEM) analysis was performed on the hard carbon material ICP-HC prepared in Example 1 and the hard carbon material ISO-HC prepared in Comparative Example 1. The results are as follows: Figure 4 As shown. Figure 4 The results show that both materials exhibit typical microstructural characteristics of hard carbon materials, namely, they are composed of short-range ordered, long-range disordered, and randomly interwoven curved graphene microcrystal layers (fullerene-like structures). For ISO-HC without special closed-pore regulation, the internal carbon layer arrangement is relatively random and loose; although a small number of micropores exist, there is a lack of obvious, large-scale pore network aggregation. In contrast, ICP-HC, after specific processing, exhibits a completely different micromorphology. Between its curved and interwoven carbon layers, a large number of enriched pore structures with more significant interconnected features can be clearly observed. These pores are encased by highly curved carbon walls and exhibit a more large-scale and continuous network distribution at the nanoscale. These results demonstrate that the processing method used in this application is extremely efficient and successful in regulating the microstructure of hard carbon. This process successfully constructs and optimizes rich pore structures with obvious interconnected features within hard carbon by guiding the rearrangement and directional evolution of carbon layers. The existence of this interconnected pore structure provides abundant internal active sites and efficient storage space for sodium / lithium storage. Furthermore, its closed-loop properties and excellent carbon wall encapsulation contribute to improving the material's first-cycle coulombic efficiency and cycling stability. This fully demonstrates the effectiveness of this treatment method in constructing the internal pore network of hard carbon materials.
[0125] X-ray diffraction (XRD) analysis was performed on the hard carbon raw material HC, the hard carbon material ICP-HC prepared in Example 1, the hard carbon material ISO-HC prepared in Comparative Example 1, and the hard carbon material O-HC prepared in Comparative Example 2. The results are as follows: Figure 5 As shown. Figure 5 The results showed that all samples exhibited two distinct broad diffraction peaks at approximately 24° and 44° 2θ, corresponding to the (002) and (100) crystal planes of amorphous carbon, respectively. This indicates that regardless of whether it was pre-oxidized at low temperature (O-HC) or subsequently subjected to high-temperature heat treatment (ISO-HC and ICP-HC), the bulk material maintained a highly long-range disordered hard carbon amorphous structure and did not undergo a transformation towards graphitization. However, compared to the original HC, the (002) peak position of O-HC pre-oxidized at 400 ℃ shifted to a higher angle (rightward), and the peak half-width at half-maximum (FWHM) narrowed. This change in the microcrystalline structure indicates that the pre-oxidation treatment caused the carbon layer structure of O-HC to exhibit a certain degree of local ordering tendency. The underlying mechanism is that the highly reactive, low-crystallinity / extremely disordered carbon components are preferentially etched or consumed during the oxidation process, thus relatively preserving the carbon layer structure with higher crystallinity and more regular arrangement. This lays the structural foundation for the subsequent construction of hard carbon with interconnected pore structures. After further high-temperature heat treatment, the (002) peak shapes of ISO-HC and ICP-HC remained good, and the peak positions were still maintained at a low angle. This indicates that the ICP-HC obtained through the process control of this application still successfully retained a large carbon interlayer spacing, which provides sufficient geometric space for the rapid insertion and extraction of sodium ions.
[0126] XPS and Raman analyses were performed on the hard carbon raw material HC, the hard carbon material ICP-HC prepared in Example 1, the hard carbon material ISO-HC prepared in Comparative Example 1, and the hard carbon material O-HC prepared in Comparative Example 2. The results are as follows: Figure 6 As shown. Figure 6The results showed that the high-resolution O 1s spectrum corresponded to two core characteristic peaks, C=O and CO bonds, respectively, in the amorphous carbon substrate. The CO bond percentage in the original HC was 37.65%. After low-temperature pre-oxidation at 400 °C, the relative percentage of CO bonds in O-HC significantly increased to 48.02%. This quantitatively confirms that the pre-oxidation process successfully introduced a high density of oxygen-containing functional groups into hard carbon, providing key chemical precursor sites for subsequent high-temperature carbon layer rearrangement and pore closure. Subsequent high-temperature heat treatments (ISO-HC and ICP-HC) induced the removal of these CO functional groups. The CO percentage in ICP-HC returned to 37.75%, while the more stable C=O bonds regained dominance (62.25%). The high-temperature removal of a large number of CO functional groups released a large number of unsaturated active sites in the microlattice, thus becoming the core driving force for the in-situ bending and closure of adjacent carbon layers to construct continuous closed pore walls. Figure 6 b shows the result of multi-peak fitting of the Raman spectrum (dissociated into peaks D, G, D1, and D2). The overall integral area ratio A is used... D / A G To quantitatively assess the overall microscopic defect level of materials. The original HC's A D / A G The value is 2.64. The pre-oxidized O-HC has an A value of... D / A G The value jumped significantly to 3.06, representing short-range SP. 3 The D2 peak area of amorphous carbon is significantly increased. This indicates that while low-temperature oxidation preferentially etches disordered carbon, the oxidized embedded CO bonds cause severe local distortion at the carbon layer edge (D1 region). At this point, the material interior is filled with highly disordered open microscopic defects. After a final high-temperature heat treatment, the A atoms of ISO-HC and ICP-HC... D / A G The ratio showed a significant decrease, and the D2 peak weakened considerably. This significant lattice repair phenomenon is directly causally related to the construction of closed pores: under high-temperature thermal drive, the high-density unsaturated defects resulting from the aforementioned pre-oxidation are extremely unstable, prompting adjacent curved graphene sheets to undergo in-situ thermal rearrangement, eliminating these high-energy defects through interweaving and self-assembly curling; in this defect elimination process, the curved carbon layers connect end to end, ultimately closing and converging at the nanoscale, evolving into a continuous porous interconnected network structure wrapped by ordered carbon walls. Because ICP-HC possesses the lowest A value in the entire series... D / A G(2.21) indicates that the transformation from disordered defects to highly continuous, well-ordered closed pore walls is the most thorough within it. These results demonstrate that the "low-temperature pre-oxidation + high-temperature heat treatment" modification strategy proposed in this application follows a complete and continuous mechanism of "pre-oxidation-induced local defects - in-situ self-assembly and closure of carbon layers - construction of interconnected closed pores." The oxygen-containing functional group defects added during the pre-oxidation stage are essentially "activation precursors" for the closed pore framework. In the subsequent heat treatment stage, with the elimination of unstable oxygen-containing functional groups and disordered carbon layer structures, the carbon framework spontaneously evolves into a lower-energy, more structurally stable topological carbon network under thermodynamic drive. This precise rearrangement process of the microscopic lattice is directly manifested in the macroscopic and microscopic morphology as the interwoven closure of carbon layers and the perfect construction of a high-density interconnected pore structure. This low-defect, highly regular closed-pore carbon wall not only blocks non-specific electrolyte penetration to suppress side reactions and improves first-cycle coulombic efficiency, but its well-developed interconnected closed-pore network also provides excellent sodium storage space, achieving a deep synergy between microstructure regulation and electrochemical performance optimization.
[0127] Nitrogen adsorption analysis was performed at 77 K on hard carbon raw material HC, hard carbon material ICP-HC prepared in Example 1, hard carbon material ISO-HC prepared in Comparative Example 1, and oxidized hard carbon intermediate O-HC prepared in Comparative Example 2. Nitrogen adsorption tests were performed using a Micromeritics ASAP 2460 gas adsorption analyzer or an instrument with equivalent testing capabilities. Vacuum degassing was performed on the samples before testing. Results are as follows: Figure 7 As shown in the figure, nitrogen adsorption results indicate that O-HC, after controlled oxidation at 400 °C, exhibits a significantly increased nitrogen adsorption capacity and nitrogen-accessible pore volume, suggesting that controlled oxidation opened previously blocked pores and improved the openness of the pore structure. After high-temperature reconstruction at 1600 °C, the nitrogen adsorption capacity and nitrogen BET specific surface area of ICP-HC significantly decreased, indicating that the open pores reclosed or significantly narrowed during carbon layer rearrangement. ISO-HC also showed a lower nitrogen adsorption capacity, but the low nitrogen BET specific surface area only indicates a lower degree of openness of the pore structure and cannot alone determine whether the internal pores are interconnected.
[0128] Furthermore, small-angle X-ray scattering (SAXS) analysis was performed on the hard carbon raw material HC, the hard carbon material ICP-HC prepared in Example 1, the hard carbon material ISO-HC prepared in Comparative Example 1, and the hard carbon material O-HC prepared in Comparative Example 2. The results are as follows: Figure 8 As shown. Figure 8 The results show that all samples have a scattering vector q of approximately 0.3–3.0 nm. -1All samples exhibited varying degrees of scattering signal enhancement or plateau characteristics, attributed to the scattering response of hard carbon's internal nanoscale pores to X-rays. The original HC showed the lowest scattering intensity in this region, indicating a lack of inherent nanoporous structures within the raw material. O-HC, after low-temperature pre-oxidation at 400 °C, showed improved scattering intensity compared to HC, consistent with previous analysis: the "local disordered carbon etching" during pre-oxidation opened or created some micro-cavities and primary open defects within the material, laying the foundation for subsequent pore formation. After final high-temperature heat treatment, the scattering behavior of the comparative ISO-HC and the example ICP-HC showed significant differentiation. ICP-HC exhibited the highest scattering intensity among all samples, with the most pronounced scattering plateau characteristics. These results demonstrate that the control method employed in this application successfully achieved large-scale, precise construction of internally interconnected closed pore structures. This allows for the successful transformation of originally loose or open micro-cavities into a high-density, highly interconnected nanoporous network at the nanoscale. This topological framework, which combines low lattice defects with abundant interconnected pores, can effectively prevent electrolyte penetration to improve the first-cycle coulombic efficiency of the battery, and also provides an extremely rich number of internal topological storage sites for sodium ions. It is the core structural guarantee for achieving high-capacity, fast-dynamic energy storage.
[0129] Furthermore, the SAXS results were fitted according to the Teubner-Strey model, specifically, the pore network interconnection factor fa was obtained by applying the small-angle X-ray scattering curve of hard carbon powder to the semi-empirical Teubner-Strey model. The model is expressed as:
[0130] (1)
[0131] Among them, I mp The scattering vector modulus is Q, representing the intensity of the small-angle X-ray scattering model generated by the microporous network inside hard carbon. The subscript "mp" indicates the scattering contribution corresponding to the microporous structure. Q represents the modulus of the scattering vector, calculated as: Q = (4πsinθ) / λ, where θ is half the scattering angle between the incident X-ray and the scattered X-ray, λ is the wavelength of the incident X-ray, and π is the mathematical constant pi. I0, C1, and C2 are represented as:
[0132] (2)
[0133] (3)
[0134] (4)
[0135] In the formula, d is the average distance between adjacent holes; ξ is the relevant length that restricts the long-range ordered range of the hole structure; π is the mathematical constant pi; ρstruc The structural density of hard carbon materials, i.e., the mass of material per unit volume of carbon skeleton, is usually expressed in g / cm³. 3 This indicates that in equation (2), it is used to normalize the density of the scattering intensity using the scale factor; ϕ(ΔSLD) 2 The term represents the effective scattering contrast of the hard carbon-porous two-phase structure, where ϕ represents the effective volume fraction factor of the porous phase, SLD represents the scattering length density (SLD), which, for X-ray scattering, is related to the electron density of the corresponding phase, and ΔSLD represents the difference in scattering length density between the hard carbon framework phase and the porous phase, i.e., ΔSLD = SLD. carbon -SLD pore For pores with internal cavities, the X-ray scattering length density of the pore phase is close to zero, therefore ϕ(ΔSLD) 2 The overall expression represents the product of the effective volume fraction of the porous phase and the square of the scattering length density difference between the hard carbon and porous phases, used to characterize the effective scattering contrast of the two-phase structure and its contribution to the SAXS intensity amplitude; the pore network interconnection factor fa is calculated by the following formula:
[0136]
[0137] fa is a dimensionless parameter. Under the same testing and fitting conditions, a larger fa indicates that the internal pore structure has a higher degree of disorder and pore network interconnection.
[0138] The fitting results are as follows Figure 9 As shown, the pore network interconnection factors (fa) of HC, O-HC, ISO-HC, and ICP-HC are 0.276, 0.563, 0.186, and 0.559, respectively. The fa of ICP-HC is approximately three times that of ISO-HC and twice that of the original HC, indicating a significantly improved degree of interconnection in the internal pore network of ICP-HC. Although O-HC has a high fa, its nitrogen adsorption capacity and nitrogen BET specific surface area are also high, indicating that its pores are still largely open to the outside. Although ISO-HC has a low nitrogen BET specific surface area, its fa is only 0.186, indicating that its internal pores are mainly isolated or in a low interconnection state. Only ICP-HC simultaneously possesses both a high fa and a low nitrogen BET specific surface area, thus achieving a balance between internal pore network interconnection and external pore network closure.
[0139] In conclusion, Figures 7 to 9 A combined quantitative criterion for interconnected pore structures was established: a higher fa (fa) is used to define the interconnection of the internal pore network, while a lower 77 K nitrogen BET specific surface area is used to define the external closure of the pore network. Simultaneously, high-resolution transmission electron microscopy (HRTEM) serves as supplementary evidence, demonstrating the simultaneous existence of internal ultramicroporous channels, pore fusion, and closed carbon walls. Therefore, the hard carbon material of this application possesses more internal pores that combine closure, internal interconnection, and sodium accessibility.
[0140] The charge-discharge curves of the coin cell using the hard carbon material ICP-HC prepared in Example 1 and the coin cell using the hard carbon material ISO-HC prepared in Comparative Example 1 at a current density of 20 mA / g are shown below. Figure 10 As shown. Figure 10 The results show that ICP-HC exhibits exceptional sodium storage capacity, with an initial reversible specific capacity of 437 mAh / g, a significant improvement over ISO-HC (300 mAh / g). A close comparison of the curve structures reveals that the capacity difference in the slope region (>0.1 V) between the two is small, and the capacity increase of ICP-HC almost entirely originates from the ultra-long, flat voltage plateau region below 0.1 V. In the hard carbon sodium storage mechanism, the low-potential plateau region directly corresponds to the filling behavior of sodium ions in the internal pores, which intuitively demonstrates the substantial increase in sodium ion filling of the internal pores of ICP-HC. Simultaneously with the significant leap in reversible capacity, the initial coulombic efficiency (ICE) of ICP-HC further improves to 91.5% (ISO-HC is 90.3%). ICP-HC achieves simultaneous improvement in capacity and ICE.
[0141] The above description, in conjunction with specific embodiments, provides a further detailed explanation of this application and should not be construed as limiting the specific implementation of this application to these descriptions. Those skilled in the art to which this application pertains can make several simple deductions or substitutions without departing from the concept of this application.
Claims
1. A hard carbon material, characterized in that: The hard carbon material has an internal network structure with interconnected pores.
2. The hard carbon material according to claim 1, characterized in that: The hard carbon material contains micropores or ultramicropores with a pore size of 0.3~2.0 nm; Preferably, the hard carbon material contains ultramicropores with a pore size of 0.3~0.8 nm.
3. The hard carbon material according to claim 1, characterized in that: The interconnected channels between the pores allow ions to enter and diffuse, and can prevent the co-intercalation of electrolyte solvent molecules or prevent direct contact between the electrolyte and the pores.
4. The hard carbon material according to any one of claims 1-3, characterized in that: The raw materials for the hard carbon material are at least one of the following: commercial hard carbon, coal-based hard carbon, resin-based hard carbon, pitch-based hard carbon, biomass-based hard carbon, organic polymer-based hard carbon, and recycled hard carbon from waste batteries.
5. A battery negative electrode, characterized in that: The hard carbon material described in any one of claims 1-4 is used.
6. An ion battery, characterized in that: It contains the hard carbon material as described in any one of claims 1-4, or the battery negative electrode as described in claim 5.
7. The ion battery according to claim 6, characterized in that: The ion battery is an alkali metal ion battery or a multivalent metal ion battery. Optionally, the alkali metal ion battery includes at least one of lithium-ion batteries, sodium-ion batteries, and potassium-ion batteries; Optionally, the multivalent metal ion battery includes at least one of magnesium ion battery, aluminum ion battery, calcium ion battery, and zinc ion battery.
8. The application of the hard carbon material according to any one of claims 1-4, the battery negative electrode according to claim 5, or the ion battery according to claim 6 or 7 in grid energy storage, low-speed electric vehicles, backup power supplies, distributed energy storage, cryogenic energy storage, and fast-charging energy storage devices.
9. The method for preparing the hard carbon material according to any one of claims 1-4, characterized in that: This includes controlled oxidation of hard carbon raw materials to obtain oxidized hard carbon intermediates; The hard carbon oxide intermediate is subjected to high-temperature treatment under an inert atmosphere or vacuum, and after cooling, a network structure in which diffusion channels between internal pores are interconnected is obtained. The controlled oxidation process involves oxidizing the hard carbon raw material in an oxygen-containing atmosphere at a temperature lower than, but close to, that of the hard carbon raw material combustion.
10. The preparation method according to claim 9, characterized in that: The controlled oxidation treatment is performed at a temperature of 250~550℃ for a duration of 0.1~24 h. Optionally, the heating rate of the controlled oxidation treatment is 0.5~20 °C / min; Optionally, the high-temperature treatment is performed at a temperature of 1000~2200 ℃ for a duration of 0.1~12 h. Optionally, the inert atmosphere includes at least one of argon, nitrogen, helium, and neon; Optionally, the hard carbon raw material includes at least one of commercial hard carbon, coal-based hard carbon, resin-based hard carbon, pitch-based hard carbon, biomass-based hard carbon, organic polymer-based hard carbon, and recycled hard carbon from waste batteries.